Aluminum foil laminate for PTP packaging

The aluminum foil laminate for PTP packaging addresses the challenge of adding a deodorizing function without increasing manufacturing steps by using a sealing layer with inorganic porous material and resin, ensuring effective odor absorption and sealability.

JP7586478B2Active Publication Date: 2024-11-19METAL COLOR CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020205696
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-11
Publication Date
2024-11-19
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

Existing PTP packaging methods for pharmaceutical products with deodorizing functions either increase manufacturing steps or compromise heat sealability, leading to higher costs and environmental impact.

Method used

An aluminum foil laminate for PTP packaging with a sealing layer containing an inorganic porous material and heat-sealing resin, having a basis weight of 2-10 g/m² and a zeolite content of 20-40% by mass, which maintains heat sealability and provides effective deodorization without additional manufacturing steps.

Benefits of technology

The laminate achieves both excellent deodorizing performance and sufficient heat sealability, reducing manufacturing costs and environmental impact while ensuring effective odor absorption and packaging integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586478000003
    Figure 0007586478000003
  • Figure 0007586478000004
    Figure 0007586478000004
  • Figure 0007586478000001
    Figure 0007586478000001
Patent Text Reader

Abstract

To provide an aluminum foil laminate for PTP packaging, having an excellent deodorization function added without increasing any manufacturing process conventionally.SOLUTION: An aluminum foil laminate 30 for PTP packaging includes a base material 20 constituted of aluminum foil and a seal layer 10 formed at the base material 20. The seal layer 10 contains an inorganic porous body and heat-sealable resin. The basic weight of the seal layer 10 is 2 g / m2 or more and 10 g / m2 or less and the content of the inorganic porous body in the seal layer 10 is 20 mass% or more and 40 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum foil laminate for PTP packaging. [Background technology]

[0002] PTP packages, which are widely used for packaging medicines and the like, are composed of a container portion for accommodating the contents and a lid material for sealing the container portion. The container portion has a flat portion that is bonded to the lid material when sealed, and a recess for accommodating the contents. The lid material generally has a base material made of aluminum foil and a seal layer that has heat sealability and is laminated on the base material. The PTP package can protect and seal the contents by heat welding the flat portion of the container portion and the seal layer of the lid material.

[0003] Incidentally, some medicines packaged in PTP packages emit a peculiar odor, and PTP packages with a deodorizing function have been developed.

[0004] For example, Patent Document 1 discloses providing an absorbent layer made of a resin containing an absorbent that absorbs odorous components on the surface of the container that comes into contact with the contents, while Patent Document 2 discloses providing a functional layer made of a mixture of a resin material and a functional substance with a deodorizing function on a lid. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2013-199283 [Patent Document 2] Patent Publication No. 2017-1729 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been a demand for adding a deodorizing function to a covering material by a method different from that described in Patent Document 2.

[0007] An object of the present invention is to provide an aluminum foil laminate for PTP packaging to which a deodorizing function has been added without increasing the number of manufacturing steps compared to the conventional method. [Means for solving the problem]

[0008] The aluminum foil laminate for PTP packaging of the present invention is an aluminum foil laminate for PTP packaging comprising a base material made of aluminum foil and a seal layer provided on the base material, the seal layer containing an inorganic porous body and a heat sealable resin, and the basis weight of the seal layer is 2 g / m 2 More than 10g / m 2 The content of the inorganic porous body in the seal layer is 20% by mass or more and 40% by mass or less. Here, the basis weight means the mass per unit area. By adopting such a configuration, it is possible to realize an aluminum foil laminate for PTP packaging that has an excellent deodorizing function without increasing the manufacturing process compared to the conventional case.

[0009] The average particle size of the inorganic porous material is preferably 0.1 μm or more and 10 μm or less.

[0010] The basis weight of the sealing layer is 3 g / m 2 More than 7g / m 2 It is preferable that: Effect of the Invention

[0011] According to the present invention, the basis weight of the sealing layer is 2 g / m 2 More than 10g / m 2 By setting the content of the inorganic porous material in the sealing layer at 20% by mass or more and 40% by mass or less, it is possible to impart an excellent deodorizing function without increasing the number of manufacturing steps compared to the conventional method. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of an aluminum foil laminate for PTP packaging according to an embodiment. [Diagram 2]FIG. 1 is a schematic cross-sectional view of a PTP packaging body using an aluminum foil laminate for PTP packaging according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have studied from the viewpoint of manufacturing a PTP package having a deodorizing function for packaging medicines that generate a peculiar odor. First, when a deodorizing function is added to the container part as disclosed in Patent Document 1, the container part is generally thicker than the lid material and is formed using a large amount of resin, so that a large amount of absorbent (adsorbent) can be added. This allows an excellent deodorizing function to be added to the container part. On the other hand, in the embodiment of Patent Document 1, the thickness of the intermediate layer containing the adsorbent is 60 μm, and further, an adhesive layer for bonding the base layer and the intermediate layer, an outer skin layer, and an inner skin layer for bonding with the lid material are required. For this reason, a large amount of resin must be used to add a deodorizing function to the container part, which causes problems in terms of manufacturing costs and environmental impact.

[0014] Next, when a deodorizing function is added to a lid material that is thinner than the container part, for example, the functional layer disclosed in Patent Document 2 does not have heat sealability. On the other hand, in order to heat-seal the lid material and the container part, it is necessary to provide a heat seal layer having heat sealability in addition to the functional layer, and in Patent Document 2, the functional layer is formed on the heat seal layer provided on the entire surface of the lid material. In addition, the functional layer must be formed at a position corresponding to the recess of the container part when sealed, and a new positioning process is required to form the functional layer. Therefore, when adding a deodorizing function to a lid material, there is a problem that the number of manufacturing processes increases compared to the conventional method.

[0015] In view of the above problems, the present inventors have investigated from the viewpoint of manufacturing a PTP packaging body having an odor eliminating function, and have arrived at the aluminum foil laminate 30 for PTP packaging of the present invention.

[0016] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following preferred embodiments are merely exemplary in nature and are not intended to limit the present invention, its applications, or its uses.

[0017] Fig. 1 shows an aluminum foil laminate 30 for PTP packaging (hereinafter referred to as "aluminum foil laminate") according to an embodiment. Fig. 2 shows a PTP packaging body 100 using the aluminum foil laminate 30 according to the embodiment. The aluminum foil laminate 30 according to the embodiment is used as a lid material to be heat-sealed to a container portion 1 that contains a content 2 such as a medicine, for example. The PTP packaging body 100 can protect and seal the content 2 contained in the recess 1a by heat-sealing the container portion 1 and the aluminum foil laminate 30 of the lid material.

[0018] The aluminum foil laminate 30 according to the embodiment includes a base material 20 made of aluminum foil and a seal layer 10 laminated on the base material 20. The seal layer 10 can be obtained by applying a seal coating agent containing an inorganic porous body and a heat-sealable resin to the surface of the base material 20.

[0019] The inorganic porous body is not particularly limited, and any inorganic compound can be used as long as it has a large number of pores on its surface and has the effect of adsorbing the odorous component, which is the object of adsorption, through these pores. Examples of the inorganic porous body include zeolite, silicon dioxide, silicate, activated carbon, titania, inorganic phosphates such as calcium phosphate, alumina, aluminum hydroxide, magnesium hydroxide, and mixtures thereof. It is preferable that the inorganic porous body contains one or more of these.

[0020] From the viewpoint of safety and excellent deodorizing function, the inorganic porous body preferably contains zeolite, aluminum hydroxide, silicate, or silicon dioxide, and more preferably contains zeolite. These inorganic porous bodies have an effective porosity relative to the size of the object to be adsorbed, and therefore can adsorb odorous components.

[0021] The inorganic porous body can be selected from those with any average particle diameter, but from the viewpoint of heat sealability and forming a uniform seal layer 10, the average particle diameter of the inorganic porous body is preferably 0.1 μm or more and 10 μm or less, more preferably 1 μm or more and 3 μm or less. If the average particle diameter of the inorganic porous body is less than 0.1 μm, the inorganic porous body may aggregate and the uniform dispersibility in the seal layer 10 may be suppressed. In addition, if the average particle diameter of the inorganic porous body is larger than 10 μm, the inorganic porous body may hinder the formation of a uniform seal layer 10, and the heat sealability of the seal layer 10 may be reduced. As a result, the aluminum foil laminate 30 may not be able to obtain sufficient heat sealability, and the protective sealing property of the contents 2 may be impaired. The average particle diameter of the inorganic porous body is calculated based on the measurement using a laser diffraction particle size distribution device (water dispersion).

[0022] The shape of the inorganic porous body is not particularly limited, and may be any shape such as a sphere, a rod, or an ellipse. The form of the inorganic porous body is not particularly limited, and may be, for example, a powder, a lump, or a granule. The form of the inorganic porous body is preferably a powder or a granule from the viewpoints of uniform kneading characteristics with a heat-sealable resin, ease of application of a seal coating agent, ease of formation of the seal layer 10, and the like.

[0023] The content of the inorganic porous material in the seal layer 10 is preferably 20% by mass or more and 40% by mass or less from the viewpoint of maintaining heat sealability and obtaining an excellent deodorizing function. If the content of the inorganic porous material in the seal layer 10 is less than 20% by mass, a sufficient deodorizing effect may not be obtained. On the other hand, if the content of the inorganic porous material in the seal layer 10 is more than 40% by mass, a sufficient heat sealability may not be obtained.

[0024] Examples of heat-sealable resins include vinyl chloride-vinyl acetate copolymer resins, polyolefin resins, acrylic resins, polyester resins, and the like. The heat-sealable resin preferably contains one or more of these. In addition, from the viewpoint of facilitating thermal welding between the aluminum foil laminate 30 and the container portion 1, the heat-sealable resin is preferably a resin material of the same family as the resin material forming the container portion 1. The heat-sealable resin can be selected from these depending on the resin material of the container portion 1.

[0025] The content of the heat sealable resin in the seal layer 10 is preferably 60% by mass or more and 80% by mass or less from the viewpoint of maintaining heat sealability.

[0026] The basis weight (mass per unit area) of the seal layer 10 is 2 g / m2 from the viewpoint of maintaining heat sealability and obtaining an excellent deodorizing function. 2 More than 10g / m 2 In addition, when the aluminum foil laminate 30 is used as a lid material for the PTP package 100, the basis weight of the seal layer 10 is preferably 3 g / m or less from the viewpoint of maintaining the function as a lid material and reducing costs. 2 More than 7g / m 2 From the same viewpoint as above, the thickness of the sealing layer 10 is preferably 2 μm or more and 10 μm or less, more preferably 3 μm or more and 7 μm or less. 2 If the basis weight of the seal layer 10 is less than 10 g / m, there is a risk that sufficient sealing performance cannot be ensured when the seal layer 10 and the container portion 1 are heat-sealed. 2 If it is more than this amount, the appearance of the sealing layer 10 may be impaired.

[0027] It is believed that a large amount of adsorbent is necessary to sufficiently adsorb odorous components generated from the contents 2 sealed in the PTP package 100. For this reason, in Patent Document 1, the middle layer of the absorption layer to which the adsorbent is added is set to 60 μm. On the other hand, the thickness of the sealing layer 10 of the lid material is limited to about 10 μm in order to reduce costs and ensure clear visibility of the printing on the aluminum foil. For this reason, it was previously believed that it was not possible to add enough adsorbent to the sealing layer 10 to sufficiently adsorb odorous components.

[0028] Furthermore, adding a large amount of adsorbent to the seal layer 10 reduces the heat sealability to the container portion 1, so adding an adsorbent to the seal layer 10 has not been considered so far. Instead, as in Patent Document 2, a configuration has been considered in which an adsorbent is provided only in a portion of the lid material facing the recess 1a that contains the content 2, and only a layer that does not contain an adsorbent and has heat sealability is provided in the other portion that is heat-sealed to the flat portion 1b of the lid material.

[0029] The inventors of the present application have questioned such conventional thinking and conducted various studies, and have found that only when the content of the inorganic porous body of the adsorbent in the seal layer 10 and the basis weight of the seal layer 10 satisfy the above conditions, it is possible to achieve both a sufficient deodorizing effect and a large seal strength, and to reduce costs. Furthermore, when the above conditions are satisfied, the visibility of the printing applied to the aluminum foil can be sufficiently ensured.

[0030] The method of applying the seal coating agent to the surface of the substrate 20 is not particularly limited, but from the viewpoint of workability, for example, gravure coating is preferred. Moreover, from the viewpoint of forming a uniform seal layer 10 that maintains heat sealability and has excellent deodorizing function, it is preferred that the seal coating agent be prepared using an organic solvent. The seal coating agent can be prepared by dispersing an inorganic porous material in an organic solvent and dissolving a heat sealable resin.

[0031] Examples of the organic solvent include, but are not limited to, ketone-based organic solvents such as methyl ethyl ketone, acetone, and methyl isobutyl ketone, aromatic hydrocarbon solvents such as toluene, xylene, and benzene, and mixtures thereof. The seal coating agent can also be prepared by dispersing the inorganic porous material directly in the heat-sealable resin without dispersing the inorganic porous material in the organic solvent in advance.

[0032] The seal layer 10 can be formed by gravure-coating the seal coating agent on the surface of the substrate 20 and then drying it. This makes it possible to obtain an aluminum foil laminate 30 in which the seal layer 10 is formed on the substrate 20. In addition, by applying heat and pressure from the surface of the substrate 20 opposite to the surface on which the seal layer 10 is provided, while the seal layer 10 of the aluminum foil laminate 30 is in contact with the container portion 1, the seal layer 10 and the flat portion 1b of the container portion 1 are thermally welded together. This makes it possible to obtain a PTP package 100 using the aluminum foil laminate 30 as a lid material.

[0033] The aluminum foil laminate 30 according to the embodiment of the above configuration can obtain an excellent deodorizing function because the inorganic porous body contained in the sealing layer 10 adsorbs odorous components generated from the contents 2. Furthermore, even though the sealing layer 10 contains an inorganic porous body, it has heat sealability, so that it is possible to realize an aluminum foil laminate 30 to which an excellent deodorizing function has been added without increasing the number of manufacturing steps compared to the conventional method.

[0034] Furthermore, since the aluminum foil laminate 30 according to the embodiment can be heat-sealed to an existing container part 1, when packaging odor-generating contents 2, it is possible to obtain a PTP package 100 having a deodorizing function by simply using the existing container part 1 and equipment and changing the lid material to the aluminum foil laminate 30. This makes it possible to reduce the cost of manufacturing the PTP package 100 having a deodorizing function.

[0035] In the above embodiment, the seal layer 10 is provided directly on the substrate 20, but this is not particularly limited, and an arbitrary layer may be interposed between the substrate 20 and the seal layer 10 as necessary. An example of the arbitrary layer is a printed layer. When a printed layer is provided, the seal coat agent forming the seal layer 10 is transparent, so that the visibility of the printed layer can be ensured. The printing ink used to form the printed layer may be a conventional one.

[0036] A printed layer can also be provided on the surface of the base material 20 opposite to the seal layer 10. When the aluminum foil laminate 30 and the container portion 1 are heat-welded to each other, heat and pressure are applied from the surface of the base material 20 opposite to the seal layer 10, so that a heat-resistant coating layer can also be provided on the printed layer. EXAMPLES

[0037] [Evaluation test 1] The following aluminum foil laminates were produced in Example 1-1 and Comparative Example 1-1. The configurations of each are also shown in Table 1.

[0038] <Example 1-1> A seal coat agent was prepared by adding 63 parts by mass of vinyl chloride-vinyl acetate copolymer resin and 37 parts by mass of powdered zeolite (average particle size 2 μm) to a mixture of organic solvents, methyl ethyl ketone and toluene, and stirring the mixture. The basis weight of the seal layer was 4.5 g / m2. 2 The seal coating agent was gravure coated on the surface of the aluminum foil substrate so that the seal coating agent was applied to the surface of the aluminum foil substrate, and then the substrate was dried. This resulted in an aluminum foil laminate having a seal layer formed on the substrate. This aluminum foil laminate was designated as Example 1-1.

[0039] <Comparative Example 1-1> An aluminum foil laminate was prepared as Comparative Example 1-1 in the same manner as in Example 1-1, except that the seal coating agent did not contain zeolite and was composed only of vinyl chloride-vinyl acetate copolymer resin.

[0040] [Table 1]

[0041] (Test Method) <Diacetyl reduction rate> The aluminum foil laminate of Example 1-1 was placed in a sampling bag (Smart Bag PA AF-5, manufactured by GL Sciences), and 3 L of clean air was injected. Then, diacetyl was injected so that the initial concentration was 400 ppm, and the diacetyl concentration was measured at predetermined time intervals. The diacetyl concentration was measured using a gas detector tube (Acetaldehyde No. 92, manufactured by Gastec Corporation). Note that, since the lower measurement limit of the gas detector tube is 25 ppm, diacetyl concentrations of 25 ppm or less (gas detector tube memory 0 to 10) were not measurable.

[0042] The diacetyl concentration in the sampling bag immediately after diacetyl injection was taken as 100%, and the rate of diacetyl reduction in the sampling bag after being left for 24 and 48 hours was confirmed.

[0043] For the aluminum foil laminate of Comparative Example 1-1, the diacetyl reduction rate was confirmed in the same manner as for the aluminum foil laminate of Example 1-1.

[0044] <Seal strength> The seal layer in each of the aluminum foil laminates of Example 1-1 and Comparative Example 1-1 was heat-welded to a polyvinyl chloride resin film having a thickness of 200 μm, and the seal strength (N / 15 mm) was measured. The welding conditions were a welding temperature of 150° C., a welding time of 1 second, and a welding pressure of 0.29 MPa. If the seal strength is 10 N / 15 mm or more, it is considered that the contents are sufficiently protected and sealed.

[0045] (Test Results) The test results are shown in Table 1. According to Table 1, in Example 1-1 containing zeolite, the diacetyl reduction rate after 48 hours was 90% or more, and the odor of diacetyl was not confirmed. It can also be seen that Example 1-1 has the same level of seal strength as Comparative Example 1-1 containing no zeolite.

[0046] This shows that the aluminum foil laminate of Example 1-1 has an excellent deodorizing function and also maintains the seal strength required for protecting and sealing the contents.

[0047] [Evaluation test 2] The aluminum foil laminates of the following Examples 2-1 to 2-19 and Comparative Examples 2-1 to 2-4 were produced.

[0048] <Examples 2-1 to 2-7> A seal coat agent was prepared by adding 80 parts by mass of vinyl chloride-vinyl acetate copolymer resin and 20 parts by mass of powdered zeolite (average particle size 2 μm) to a mixture of organic solvents, methyl ethyl ketone and toluene, and stirring the mixture. The basis weight of the seal layer was 2.0 g / m2. 2 The seal coating agent was gravure coated on the surface of a substrate made of aluminum foil (thickness 20 μm) so that the seal coating agent was formed on the substrate, and then the substrate was dried. This resulted in an aluminum foil laminate having a seal layer formed on the substrate. This aluminum foil laminate was designated as Example 2-1.

[0049] In addition, in Examples 2-2 to 2-7, the basis weight of the sealing layer was 3.0 g / m 2 , 4.0g / m 2 , 5.0g / m 2 , 6.0g / m 2 , 7.0g / m 2 and 10.0 g / m 2 This aluminum foil laminate was obtained in the same manner as in Example 2-1, except that:

[0050] <Examples 2-8 to 2-13> The vinyl chloride-vinyl acetate copolymer resin was 70 parts by mass, the zeolite was 30 parts by mass, and the basis weight of the seal layer was 3.0 g / m 2 An aluminum foil laminate obtained in the same manner as in Example 2-1 except for the above was designated as Example 2-8.

[0051] In addition, in Examples 2-9 to 2-13, the basis weight of the sealing layer was 4.0 g / m 2 , 5.0g / m 2 , 6.0g / m 2 , 7.0g / m 2 and 10.0 g / m 2 This aluminum foil laminate was obtained in the same manner as in Example 2-8, except that:

[0052] <Examples 2-14 to 2-19> The vinyl chloride-vinyl acetate copolymer resin was 60 parts by mass, the zeolite was 40 parts by mass, and the basis weight of the seal layer was 3.0 g / m 2 An aluminum foil laminate obtained in the same manner as in Example 2-1, except for the above, was designated as Example 2-14.

[0053] In addition, in Examples 2-15 to 2-19, the basis weight of the sealing layer was 4.0 g / m 2 , 5.0g / m 2 , 6.0g / m 2 , 7.0g / m 2 and 10.0 g / m 2 This aluminum foil laminate was obtained in the same manner as in Example 2-14, except that:

[0054] <Comparative Example 2-1> An aluminum foil laminate was prepared as Comparative Example 2-1 in the same manner as in Example 2-1, except that the seal coating agent did not contain zeolite and was composed only of vinyl chloride-vinyl acetate copolymer resin.

[0055] <Comparative Example 2-2> An aluminum foil laminate was prepared in the same manner as in Example 2-1, except that the amount of vinyl chloride-vinyl acetate copolymer resin was 90 parts by mass and the amount of zeolite was 10 parts by mass, and was designated Comparative Example 2-2.

[0056] <Comparative Example 2-3> The vinyl chloride-vinyl acetate copolymer resin was 50 parts by mass, the zeolite was 50 parts by mass, and the basis weight of the seal layer was 3.0 g / m 2 An aluminum foil laminate obtained in the same manner as in Example 2-1 except for the above was designated as Comparative Example 2-3.

[0057] <Comparative Example 2-4> The vinyl chloride-vinyl acetate copolymer resin was 40 parts by mass, the zeolite was 60 parts by mass, and the basis weight of the seal layer was 5.0 g / m 2 An aluminum foil laminate obtained in the same manner as in Example 2-1 except for the above was designated as Comparative Example 2-4.

[0058] [Table 2]

[0059] (Test Method) <Deodorizing performance> Four sheets of the aluminum foil laminate (10 cm square) of Example 2-1 were placed in a vial (capacity 100 ml). Diacetyl (100 ppm) diluted with distilled water was poured into the vial, and the vial was placed in a thermo-hygrostat and left for 16 hours. Thereafter, the deodorizing performance was confirmed by sensory evaluation.

[0060] For each of the aluminum foil laminates of Examples 2-2 to 2-19 and Comparative Examples 2-1 to 2-4, the deodorizing performance was confirmed by sensory evaluation in the same manner as in Example 2-1.

[0061] If a significant deodorizing effect was confirmed, it was rated as A; if it was confirmed that the deodorizing effect was sufficient but not significant, it was rated as B; and if no deodorizing effect was confirmed, it was rated as C.

[0062] <Sealing performance> For each of the aluminum foil laminates of Examples 2-1 to 2-19 and Comparative Examples 2-1 to 2-4, the seal strength (N / 15 mm) was measured in the same manner as in Test Evaluation 1. If the seal strength was 10 N / 15 mm or more, the contents were sufficiently protected and sealed, and it was judged to have sufficient sealing performance and to be A, and if it was less than 10 N / 15 mm, the contents were not sufficiently protected and sealed, and it was judged to have insufficient sealing performance and to be B.

[0063] (Test Results) The test results are shown in Table 2. It is considered that a lid material having a deodorizing function is preferably one for which the deodorizing performance is rated as A or B and the sealing performance is rated as A.

[0064] According to Table 2, the deodorizing performance of all of Examples 2-1 to 2-19 was judged to be A or B, and the sealing performance was judged to be A. Therefore, it can be seen that all of Examples 2-1 to 2-19 have not only remarkable or sufficient deodorizing performance, but also the sealing performance required for protecting and sealing the contents.

[0065] In Comparative Examples 2-1 and 2-2, the sealing performance was rated as A, while the deodorizing performance was rated as C. This shows that when the zeolite content is less than 20 mass %, the deodorizing performance is not obtained.

[0066] In Comparative Examples 2-3 and 2-4, the deodorizing performance was rated as A, while the sealing performance was rated as B. This shows that when the zeolite content is more than 40 mass%, the sealing performance required for protecting and sealing the contents is not obtained.

[0067] From the above evaluation test 2, in the aluminum foil laminate, the content of zeolite is set to 20 mass% to 40 mass%, and the basis weight of the seal layer is set to 2.0 g / m 2 ~10.0g / m 2 This makes it possible to achieve both excellent deodorizing performance and sealing performance. [Explanation of symbols]

[0068] 1 Container part 1a Recess 1b Plane part 2 Contents 10 Sealing layer 20 Base material 30 PTP packaging aluminum foil laminate 100 PTP packaging

Claims

1. A PTP packaging aluminum foil laminate comprising a base material made of aluminum foil and a seal layer provided on the base material, The seal layer contains an inorganic porous material and a heat-sealable resin, The basis weight of the sealing layer is 2 g / m 2 10g / m or more 2 is as follows: The content of the inorganic porous material in the sealing layer is 20% by mass or more and 40% by mass or less, The average particle size of the inorganic porous body is 1 μm or more and 3 μm or less.

2. The basis weight of the sealing layer is 3 g / m 2 7g / m or more 2 The PTP packaging aluminum foil laminate according to claim 1, which is as follows:

Citation Information

Patent Citations

  • Container for packaging medicine

    EP0370755A1

  • packaging container

    JP1993094167U

  • Laminate for PTP or blister pack, and PTP or blister pack which is molded by using the same

    JP2013199283A

  • Heat seal sheet and press through packaging body

    JP2016204047A

  • Elastic crawler

    JP2017001429A