Laminated packaging material, packaging containers produced therefrom, and methods for producing laminated materials - Patents.com

The laminated packaging material with a calendered corrugated base paper and transparent outer layer addresses cost and customization challenges, offering flexible appearance options and maintaining mechanical strength and print quality for liquid food containers.

JP7586644B2Active Publication Date: 2024-11-19TETRA LAVAL HOLDINGS & FINANCE SA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2019566273
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-05-31
Filing Date
2018-05-31
Publication Date
2024-11-19
Estimated Expiration
2038-05-31

AI Technical Summary

Technical Problem

Existing laminated packaging materials for liquid food containers are costly and lack flexibility in appearance customization, while modifications to reduce costs often compromise mechanical strength and barrier properties.

Method used

A laminated packaging material comprising a corrugated base paper with a calendered surface roughness and a transparent outermost thermoplastic polymer layer, allowing for customizable decorative features and reduced bulk material usage, while maintaining mechanical strength and print quality.

Benefits of technology

The solution enables cost-effective differentiation of packaging appearance with improved mechanical properties and printability, allowing for shorter production series without waste or logistics issues, and maintains packaging integrity for long-term storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586644000001
    Figure 0007586644000001
  • Figure 0007586644000002
    Figure 0007586644000002
  • Figure 0007586644000003
    Figure 0007586644000003
Patent Text Reader

Abstract

The present invention relates to a laminated liquid food packaging material comprising a layer of cellulosic bulk material and outer thermoplastic polymer layers on either side, with a decorative printed pattern disposed under one of the outer thermoplastic polymer layers. The present invention also relates to a method for manufacturing the laminated packaging material, and to a packaging container for liquid food packaging comprising the laminated packaging material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated packaging material comprising a bulk layer of paper or carton or other cellulosic material and outer layers of a thermoplastic polymer on both sides, with a printed decoration disposed under one of the outer layers of thermoplastic polymer.

[0002] Additionally, the present invention relates to packaging containers that include or are made from the laminated packaging material, as well as methods for producing the laminated material. [Background technology]

[0003] Single-use, disposable packaging containers for liquid foods are often manufactured from packaging laminates based on paperboard or carton. One such common packaging container is marketed under the name Tetra Brik Aseptic® and is mainly used for aseptic packaging of liquid foods sold for long-term ambient storage, such as milk, fruit juice, etc. The packaging material in this known packaging container is typically a laminate comprising a bulk layer of paper or paperboard and an outer liquid-tight layer of thermoplastic material. To make the packaging container airtight, in particular oxygen-tight, for example for the purpose of aseptic packaging and packaging of milk or fruit juice, the laminates in these packaging containers usually comprise at least one additional layer, most commonly aluminum foil.

[0004] On the inside of the laminate, i.e. on the side of the container produced from it that is intended to face the filled food contents, there is an innermost layer applied on the aluminum foil, this innermost inner layer may consist of one or several partial layers comprising adhesive polymers and / or heat-sealable thermoplastic polymers such as polyolefins. Outside the bulk layer there is also a heat-sealable outermost layer.

[0005] Packaging containers are generally produced by modern high-speed packaging machines of the type that form, fill and seal packages from webs of packaging material or prefabricated blanks. Thus, packaging containers can be produced by reforming a web of laminated packaging material into a tube by fusing together the innermost and outermost heat-sealable thermoplastic polymer layers, thereby uniting both longitudinal ends of the web with each other at overlapping joints. The tube is filled with the intended liquid food product and then divided into individual packages by repeating the transverse sealing of the tube at a predetermined distance from each other below the level of the contents in the tube. The packages are separated from the tube by cutting along the transverse seals and given the desired geometric configuration, usually a parallelepiped or rectangular prism, by folding and forming the packaging material along prepared fold lines.

[0006] The main advantage of this continuous canning, filling and sealing packaging concept is that the web can be continuously sterilized just before canning, thus offering the possibility of aseptic packaging, where the filled packaging containers are produced under clean conditions, where the liquid contents to be filled as well as the packaging material itself are reduced in bacteria, so that the filled packages can be stored for long periods, even at room temperature, without the risk of microbial growth in the filled products. Another important advantage of the Tetra Brik® type of packaging is that it allows continuous high speed packaging, which, as mentioned above, has a considerable impact on cost efficiency.

[0007] Typically, thousands of packages can be prepared per hour. For example, the Tetra Pak® A3 / speed can produce approximately 15,000 packages per hour (family size packages of 0.9 liters or more) and approximately 24,000 packages per hour (portion packs).

[0008] Packaging containers for sensitive liquid foods, such as milk or juice, can also be produced from sheet blanks or prefabricated blanks of the laminated packaging material of the invention. From tubular blanks of the flat-folded packaging laminate, the packaging is produced by first assembling the blanks to form an open tubular container capsule, one open end of which is closed by folding and heat-sealing an integral end panel. The container capsule thus closed is filled through its open end with the target food product, such as juice, and then the open end is closed by further folding and heat-sealing the corresponding integral end panel. An example of a packaging container produced from sheet and tubular blanks is the conventional so-called gable-top packaging. Some of this type of packaging have a molded top and / or a screw cap made of plastic.

[0009] Known packaging laminates are conventionally produced from a web of paper or paperboard unwound from a storage reel while a web of aluminum foil is unwound from a corresponding storage reel. The two unwound webs are brought together and both are guided through a nip between two adjacent rotating cylinders while a bonding layer of laminating material, usually low density polyethylene (LDPE), is extruded into a molten polymer film or curtain, thus dispensing the material between the webs and permanently bonding the aluminum foil web to the paper or paperboard web. The paper or paperboard web is then coated on both sides with a liquid-tight coating of polyethylene, usually low density polyethylene (LDPE), and then wound into a finished packaging reel for later transport and handling.

[0010] The known packaging material works extremely well and performs several important functions in the packages produced therefrom, such as protecting food against ingress of substances and microorganisms from outside the package and against deterioration by light or oxygen gas. It is the long-standing packaging structure most commonly found on retail shelves today. The bulk layer of liquid grade paperboard can be flexo or offset printed on its outer surface with high quality, highly color-controlled, high resolution, attractive printed decoration. The printable surface of the paperboard is usually coated with a white coating composition of mineral particles and binder polymers, which provides a neutral, even background for any printed color decoration pattern, as well as the required adhesion and cohesion properties within the coating and to the printed inks and any adjacent polymer layers.

[0011] Further cost reductions of today's packaging materials can be achieved by downgauging the thickness of the polymer layers or by seeking to replace the aluminum foil barrier with one or more different barrier layers. Another cost reduction method that has not been considered practical in the field of liquid carton packaging would be by downgauging the cellulosic bulk layers by the type and / or amount of cellulosic fiber material. This would usually compromise the important properties of mechanical strength and package integrity as well as the barrier properties of the material, and has not been a favorable method to pursue until now. Paperboard represents a large portion of the liquid carton packaging material, but also represents a large portion of the total packaging cost.

[0012] A further requirement for laminated packaging materials for future liquid packaging containers is that the appearance of such packaging containers must be highly differentiated, i.e. by providing new, interesting, appealing decorative or tactile features to entice consumers and retailers. Such features are, for example, printed decorative patterns, metallization, e.g. with gold or other different glossy colors, embossed and engraved features, e.g. holographic decoration, tactile or relief surface effects, background effects on matte / glossy surfaces. The increasing demand for such differentiation options is a challenge, since the addition of features and materials usually entails an increase in the cost of raw materials and / or manufacturing processes.

[0013] Any change to existing paperboard materials would entail costly developments at the paper manufacturer, as paperboard manufacturing is a highly complex process. This has not been deemed worth the effort and resources until now, since it is believed that the majority of liquid carton packaging produced will still be selected to have the state of the art, reliable and consistent white coating background. There is an increasing need for more variation and differentiation from traditional liquid cartons, which in turn places increased demands on the conformance and flexibility of the packaging materials produced. Summary of the Invention [Problem to be solved by the invention]

[0014] It is therefore a general object of the present invention to provide a laminated packaging material having good mechanical properties and meeting the needs in laminated packaging materials for liquid cartons at a lower cost.

[0015] A further general object is to provide a laminated packaging material which provides increased opportunities for differentiating the appearance of packages made from the laminated material as compared to the state of the art packaging materials and packaging containers described above.

[0016] A further object is to provide a laminated cellulosic packaging material with increased opportunities for exterior differentiation, sufficient mechanical strength and dimensional stability, and good print surface properties to meet the needs in laminated packaging materials for liquid cartons, at reduced or at least maintained cost.

[0017] A specfic objective of the present invention is to enable cost-effective differentiation of the outer layer of such laminated packaging materials, i.e. a visible decorative layer that is attractive and appealing to the consumer, allowing for later customization of the outside of the packaging container in the packaging manufacturing process and with shorter runs of pre-manufactured packaging materials.

[0018] A further object is to provide a laminated cellulosic packaging material based on a down-gauged, low cost bulk or core layer having a rough, dark or brown surface rather than a surface suitable for printed decorative patterns, yet the final packaging material has print quality and differentiation opportunities comparable to conventional such packaging laminates.

[0019] Some or all of these objects can be achieved in accordance with the present invention by the laminated packaging material, the method of manufacturing the laminated packaging material, and the packaging containers made therefrom, as defined below and in the appended claims. [Means for solving the problem]

[0020] Thus, according to a first aspect of the present invention, there is provided a laminated liquid food packaging material comprising a cellulosic bulk material layer, a transparent outermost protective layer of a thermoplastic polymer arranged on the outer side of the bulk material layer, i.e. on the side that will face the exterior of a packaging container made from the laminated material, a decorative printed pattern arranged underneath, i.e. on the inner side, and visible through the transparent outermost protective layer of the thermoplastic polymer, and an innermost layer of a heat-sealable, liquid-tight thermoplastic polymer that will be in direct contact with the liquid food in the packaging container, wherein the bulk material layer is a corrugated paperboard, which has been calendered to a Bendtsen outside surface roughness value of less than 200 ml air / min, and which meets the requirements of ISO 9895 and ISO 536, and a bending stiffness at least 30% lower than that of a liquid packaging board of comparable surface weight, excluding any printable coating (clay coat) thereof, and the laminated packaging material further comprises a cellulosic print substrate paper, the print substrate paper having an outer printing surface carrying a decorative print pattern, the print substrate paper having a dry weight of 1 to 4 g / m 2 It is bonded to the outside of the bulk material layer by an adhesive of 100 g / m 2 A laminated liquid food packaging material is provided having a surface weight (ISO 536) of 0.01 mm or less and an outer printed surface having a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min.

[0021] Such construction allows for the use of cheaper bulk material layers in place of traditional high end liquid packaging paperboard.

[0022] At the same time, because the outer layer can be easily replaced, different decorative visible and / or tactile features can be laminated into the material according to different styles and desires among customers, consumers and retailers. Such customization allows the production of separate, shorter series of differently decorated customized packaging materials without causing stoppages, waste and logistics problems in the mainstream material production line. That is, it allows the packaging material to be customized later. Furthermore, such later customization allows the selection from a list or catalog of available paper and paperboard grades to obtain a combination of bulk layer and printing base paper that provides the laminated material with the desired stiffness and mechanical dimensional stability as required for a specific packaging size and food product type, as well as the desired appearance of the printing background with good printability.

[0023] The various background features and appearances of the printing base paper could be silver and gold metallic appearance or other different metallic colors, embossed and engraved features, tactile or relief surface effects, matte / glossy surface, etc. The increasing demand for such differentiation options is a challenge, since the addition of features and materials usually entails an increase in the cost of raw materials and / or manufacturing processes. By transferring the printing surface portion of the commonly used paperboard material layer to another layer, which has complementary mechanical properties that support the remaining bulk properties of the remaining bulk material layer, while providing differentiated features and a good printable surface, the same functionality as the state of the art packaging material is achieved in the final laminated packaging material. At the same time, some of the costs spent on various high-end outer printing base papers can be compensated for by the savings in the bulk material layer.

[0024] In a second aspect of the invention, there is provided a packaging container for packaging liquid food products comprising the laminated packaging material of the invention, which may be made entirely from the laminated packaging material by folding and forming a sheet or web-like blank into a rectangular parallelepiped, another folded and formed package, or simply into a pouch package.

[0025] In a third aspect of the present invention, there is provided a method for producing a laminated cellulosic liquid food packaging material as defined above, comprising the following steps: a) providing a first web (A) of cellulosic bulk material layer which is a calendered linerboard having a Bendtsen outer surface roughness value of less than 200 ml air / min, a specific SCT in MD greater than 30 Nm / g determined according to ISO 9895 and ISO 536, and a bending stiffness at least 30% lower than that of a liquid packaging board of comparable surface mass, excluding any printable coating (clay coat) thereof, outer meaning the side which will face the exterior of a packaging container made from the laminated material; b) 100g / m 2 Providing a second web (B) of cellulosic printing base paper having a surface weight (ISO 536) of 0.1 mm or less and an outer printing surface carrying a decorative printing pattern, the outer printing surface having a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min; c) Adhesive polymer with a dry content of 1 to 4 g / m 2 applying an aqueous adhesive composition comprising an aqueous adhesive composition having an amount of 0.1 to 0.5% by weight of the aqueous adhesive composition to at least one of the outer side of the first web and the inner side of the second web, where inner side means facing the interior of the packaging container; d) delivering the first and second webs from step c) towards a pressure roller nip (22) to laminate them together with the intervening aqueous adhesive composition while passing through the nip and while the aqueous adhesive composition is partially absorbed into at least one surface of the first and second webs (A and B); e) printing a decorative printing pattern onto the printing surface of the printing base paper; f) laminating an innermost layer of heat sealable thermoplastic polymer to the inside of the web of bulk material layer, opposite the side of the printing base paper, innermost meaning the side that will come into contact with the liquid food in said packaging container; g) laminating a transparent outermost protective layer of a thermoplastic polymer to the outside of the web of printing base paper, i.e., the outer printing surface opposite the bulk material layer side; in any order.

[0026] Step e) may be carried out before steps c) and d), so that the printing base paper is first printed with the decoration on its printing side in a separate printing operation.

[0027] Usually the printing substrate paper is laminated to a bulk material layer before it is subjected to further printing operations. Suitable printing methods may be modern digital and inkjet printing methods, but also traditional flexographic and offset printing methods.

[0028] The surface roughness of the printing base paper, when laminated to the bulk material layer, will be almost the same after printing the decorative printing pattern as before the printing operation. Usually, if there is any change, the smoothness of the printed printing base paper should be increased, because the paper may pass through several printing rollers and nips before it is finally printed. Thus, the outer printing surface of the printing base paper, even when laminated to the bulk material layer, has a smoothness of less than 100 ml air / min (Bentsen).

[0029] The bulk material layer is preferably calendered to an outer surface roughness of less than 200 ml air / min (Bentsen), for example less than 150 ml air / min.

[0030] This method allows the material to be later customized by later combining bulk material layers with printing base paper for appropriate mechanical properties depending on the size and type of packaging, and also allows for later customization as to which printed decorations are provided depending on the customer's brand and type of product to be filled into the packaging container.

[0031] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. [Brief description of the drawings]

[0032] [Figure 1a] FIG. 2 shows a schematic cross-sectional view of a first laminated packaging material according to the present invention. [Figure 1b] FIG. 2 shows a schematic cross-sectional view of a further embodiment of a laminated packaging material according to the invention. [Figure 1c] FIG. 2 shows a schematic cross-sectional view of another embodiment of a laminated packaging material according to the present invention. [Figure 2a] 2A-2D are schematic diagrams illustrating the steps of a method for laminating a web of printing base paper to a web of a layer of bulk material according to the present invention; [Figure 2b] FIG. 2 shows a schematic diagram of a preferred embodiment of a method for laminating a barrier film or foil to a bulk layer according to the present invention. [Figure 2c] Figure 2c shows a schematic representation of a further method step for laminating an innermost layer of thermoplastic polymer to a web comprising a laminated bulk material layer, for example a laminated web obtained from the method step described in Figure 2a. Alternatively, Figure 2c can illustrate a further method step for laminating an outermost layer of thermoplastic polymer to the outside of a web comprising a printing base paper having a printed decoration thereon, according to the present invention. [Figure 3a] FIG. 2 shows a typical example of a packaging container produced from a laminated packaging material according to the present invention. [Figure 3b] FIG. 2 shows a typical example of a packaging container produced from a laminated packaging material according to the present invention. [Figure 3c] FIG. 2 shows a typical example of a packaging container produced from a laminated packaging material according to the present invention. [Figure 3d] FIG. 2 shows a typical example of a packaging container produced from a laminated packaging material according to the present invention. [Figure 4] FIG. 1 illustrates the principle of how packaging containers can be produced from packaging laminates in a continuous roll-fed, form, fill and seal process. [Diagram 5] FIG. 1 illustrates how the high surface roughness of the bulk material layer of the liner can be reduced to support a good print surface of the final laminated packaging material. [Figure 6] Figure 6 shows the principle of operation of metal belt calendering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The term "long term storage" in the context of the present invention means that the packaging container should be able to preserve the quality, i.e. nutritional value, hygienic safety and taste, of the packed food product at ambient conditions for at least 1 or 2 months, such as at least 3 months, preferably longer, such as 6 months, for example 12 months or longer.

[0034] The term "package integrity" in the context of the present invention generally refers to the durability of the package, i.e., the resistance of the package to leakage or breakage. It includes the resistance of the package to the ingress of microorganisms such as bacteria, dirt, and other substances that may deteriorate the food product contained therein and shorten the expected shelf life of the package.

[0035] One of the main contributors to the integrity of a package from a laminated packaging material is provided by good internal adhesion between adjacent layers of laminated material. Another contributor to the integrity of the package is the resistance of the material to defects, e.g., pinholes, punctures, etc., within each material layer itself, and yet another contributor to the integrity of the package is the strength of the seal joint where the materials are sealed together to form the package container. Thus, with respect to the laminated packaging material itself, the integrity properties are primarily focused on the adhesion of each laminate layer to its adjacent layers, as well as the quality of the individual material layers. With respect to the closure of the package, the integrity is primarily focused on the quality of the seal joint, which is ensured by a well-functioning and robust sealing operation in the filling machine, which is ensured by the heat seal properties of a properly adapted laminated packaging material.

[0036] The term "liquid food" generally refers to food products with low or high viscosity flowable contents that may optionally contain food particles. Dairy and milk, soy, rice, grain and seed drinks, juices, nectars, still drinks, energy drinks, sports drinks, coffee or tea drinks, coconut water, tea drinks, wine, soup, crushed tomatoes, sauces (such as pasta sauces), and olive oil are some non-limiting examples of contemplated food products.

[0037] The term "sterile" with respect to packaging materials and packaging containers refers to a state in which microorganisms have been eliminated, inactivated, or killed. Examples of microorganisms are bacteria and spores. In general, aseptic processes are used when products are aseptically packed into packaging containers. In order to remain sterile during the shelf life of the package, the integrity properties of the package are of course extremely important. For the long shelf life of a filled food product, it may be even more important that the package has a barrier property against gases and vapors, for example against oxygen gas, to preserve its original taste and nutritional value, such as its vitamin C content.

[0038] The term "bulk layer" usually refers to the thickest layer or the layer containing the most material in a multi-layer laminate, i.e., the layer that contributes most to the mechanical properties and dimensional stability of the laminate and the packaging container folded from it, e.g., paperboard or carton, etc. It can also refer to the layer that provides a longer thickness distance in the sandwich structure and further interacts with stabilising facing layers (having a higher Young's modulus) on both sides of the bulk layer to achieve sufficient such mechanical properties and dimensional stability.

[0039] A "spacer layer" is a layer that creates a distance or space between significantly thinner layers of material with higher Young's modulus and density, i.e. layers that provide stiffness and stability, so-called surface layers, such as stretched films, metal foils, or high-density, high-tensile stiff paper layers, foils, or films, arranged on both sides of the spacer layer in a sandwich structure. The spacer layer can have a lower or reduced inherent bending stiffness, and therefore does not directly contribute significantly to the bending stiffness of the laminated packaging material by itself. However, indirectly, it can contribute significantly by interacting with adjacent or laminated layers on both sides, some of which have a higher Young's modulus but a smaller thickness compared to the spacer layer. In a sandwich structure, it is important that at least one such surface layer, or stiffness-reinforcing layer, is on both sides of the spacer layer. Thus, the "bulk layer" may include the "spacer layer" and further layers combined in the bulk, but may be the same as the spacer layer.

[0040] The term "heat sealing" refers to the process of fusing one surface of a thermoplastic material to the surface of another thermoplastic material. A heat-sealable material should be capable of producing a seal when pressed in contact with another suitable thermoplastic material under the right conditions, such as application of sufficient heat and pressure. Suitable heating can be achieved by induction or ultrasonic heating, or other conventional contact or convection heating means, such as hot air or impulse heating. Heating increases the mobility of polymer chains at the surfaces of the materials intended to be sealed together, thereby allowing the chains to unravel and move and reentangle with polymer chains from the opposing sealing surface. Cooling creates strong bonds of the entangled polymer chains across the sealing interface, thus bonding the two material surfaces together. The heat-sealing operation must be carried out within a fraction of a second in packaging machines that produce thousands of packages per hour, with the durations of the different phases, such as heating, partial melting, bonding, and cooling, counting in milliseconds.

[0041] The term "inner" when defining the position or side of a layer in a laminated packaging material has the meaning "facing the inside of a packaging container formed from the packaging material" and the term "outer" defines "in the direction facing the exterior or outside of a packaging container formed from the packaging material."

[0042] "Innermost" means the layer that is in contact with the product packed within the package formed from the packaging material.

[0043] "Outermost" means the layer that provides the outer, exterior surface of a packaging container formed from the packaging material.

[0044] The printing surface of the printing base paper has a density of 22 to 28, e.g. 24 to 27, e.g. 24 to 26 g / m2, measured according to ISO 535. 2The cellulose composition of the printing base paper should be sized to reduce edge wicking, i.e. to reduce water or liquid absorption at the exposed paper edge of the cut laminate structure, and to reduce excessive absorption of water from the aqueous adhesive composition during the lamination operation of laminating the printing base paper to the bulk material layer. A Cobb value above 30 would mean that the paper would absorb too much aqueous composition, resulting in weak bonds from the lamination absorbing the aqueous adhesive. The cut edge of the laminate would also absorb aqueous composition, causing the laminated material to swell and delaminate along the exposed edge area. On the other hand, if the Cobb value is too low, for example below 20, there may be problems in adhering the printed ink to the printing base paper and in further coating the printed paper with a thermoplastic polymer layer. Thus, the preferred Cobb value for the printing base paper is 24-26 g / m to balance absorption and adhesion. 2 It is water.

[0045] The size is suitably an internal, dual size, i.e. two sizes are added to the cellulose pulp when the pulp is used to make paper. A suitable such size is alkyl ketene dimer (AKD) with Rosin (Hartz). AKD may alternatively be used as the sole size. Another possible size is alkylene succinic anhydride (ASA).

[0046] The sizing is achieved by adding 1 to 4 kg / ton, for example 2 to 4 kg / ton, ie 0.1 (0.2) to 0.4 mass % of a sizing agent to the cellulose pulp.

[0047] The printing surface may have a Bendtsen surface roughness value below 80 ml air / min, such as below 60 ml air / min, for example below 70 ml air / min. The smoother it is, the better the print quality obtained. Furthermore, the printing base paper may have a surface roughness value below 80 g / m 2Less than 70g / m 2 The surface mass may be less than 100 nm.

[0048] The printing base paper may have a tensile index (GM) of at least 40 Nm / g in order to better handle the forces applied in the lamination process. Furthermore, for this purpose, it should have a GM of at least 6 mNm 2 / g.

[0049] More specifically, the printing base paper has a density of 650 kg / m 3 Higher density, 100g / m 2 Surface mass (ISO 536) of at least 40 Nm / g tensile specific strength (GM) of at least 6.0 mNm 2 % of at least one sizing agent, and the outer printed surface may have a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min, and a specific tear strength (GM) of less than 20 g / m 2 Larger than 30g / m 2 (water) has a Cobb value of less than

[0050] Thus, the printing base paper may be a paper having a smooth printable surface selected from the group consisting of MG (machine glossy) paper, MF (machine finished) paper, LWC (lightweight coated) paper, flexible wrapping paper, metallization base paper, digital printing paper, copy paper, and inkjet printing paper.

[0051] MG paper is a paper with a high gloss finish on one side and is produced by drying a web of wet paper against a highly polished metal cylinder, also called a Yankee cylinder or Yankee dryer, in a paper machine. MG paper may be MG Kraft paper or an extremely thin paper and is often used for wrapping paper and posters. The surface roughness may be 40-150 ml air / min (Bentsen). For the present invention, MG paper with a surface roughness below 100 ml / min would be selected.

[0052] MF paper has a smooth surface similar to MG paper, but achieved by a final smoothing machine roller treatment along with calendaring on the paper machine.

[0053] LWC paper is a category of paper accepted by the paper industry that has a thin white coating and is based in part on mechanical pulp and is used, for example, in magazines.

[0054] Flexible wrapping paper is another category of suitable paper approved by the paper industry, has a smooth surface and contains only chemical pulp. It is usually a thin kraft paper coated on one side, but may alternatively be uncoated. This type of paper is often used, for example, to package food. An example of a suitable product name is Lennoflex, manufactured by Feldmuehle. The term "flexible" distinguishes the paper type from inflexible cartons (bending mode). The surface roughness of flexible wrapping paper can be as low as about 15 ml air / min.

[0055] Metallized base papers are manufactured and pre-coated to provide a smooth surface for metallization. Such papers may be used in the present invention as both metallized and non-metallized printing base papers. Suitable metallized base paper products are "Lennovac" and "Metalvac".

[0056] Digital printing papers, inkjet papers, and copy papers are all surface treated on both sides to provide a smooth surface adapted to accept a variety of printing inks from different printing processes.

[0057] The surface of the printing base paper may have any color, a metallized color or pattern, or a white color to serve as a background for the subsequently printed decoration. In one embodiment, the printing base paper is a natural brown, i.e., unbleached brown paper.

[0058] In one embodiment, the printing base paper is metallized, i.e. carries a nanometer-thin metallized coating. For metallized printing base paper, the metallized surface is sensitive to being laminated to a rough surface on the back side, which will disrupt the metallic, mirror-like smooth appearance of the metallized surface, which in turn will degrade or disrupt the decorative print that is subsequently printed on the surface. Therefore, it is important that the metallized printing base paper is laminated to a sufficiently smooth surface under the printing base paper, i.e. on the opposite side of the metallized coating. In particular, for metallized printing base paper, the surface roughness of the surface of the underlying bulk material layer should be less than 150 ml air / min (Bentsen), so that the surface roughness obtained in the lamination of the printing base paper and the bulk material layer can be reduced to less than 50 ml air / min.

[0059] Typically, a white printing surface is still desirable, and a suitable printing substrate having such a surface would be a thin printing paper suitable for digital or inkjet printing, or flexographic printing.

[0060] The bulk material layer is 100-300g / m 2 , for example 100-200g / m 2 may have a surface mass of

[0061] The bulk material layer preferably has an outer surface smoothness of less than 200 ml air / min, e.g. less than 150 ml air / min (Bentsen). A linerboard with such a smooth surface cannot be found commercially and must be prepared by a calendering process. Suitable calendering processes are metal belt calendering and heated roller calendering. That a linerboard such as a linerboard has been calendered before being laminated into a laminated packaging material can be detected by the fact that the surface of the linerboard has a "flame" that varies in color and / or degree of surface texture of the linerboard. Thus, that the surface of the linerboard has been treated by some high heat and pressure can be seen when peeling away layers of such laminated material.

[0062] When using a printing base paper with a given surface weight, laminated materials for different packaging container sizes and for different requirements regarding mechanical properties can be obtained by simply exchanging the bulk material layers, which can then be selected from different commercial grades of liquid packaging paperboard. 2When using a printing base paper of 1000 mm, a packaging laminate suitable for the smaller so-called portion packs of sizes up to 250 or 300 ml can be obtained by laminating it to a 30 mN liquid packaging board (LPB). The resulting paper laminate acquires a bending stiffness of 80 mN, i.e. at the same level as the LPB grades currently on the market aimed at the smaller portion packs of the same type. If the same printing base paper is instead laminated to an 80 mN LPB, the resulting laminated material may be suitable for slightly larger packaging containers that would normally require a 150 mN LPB, or for some packages where a 260 mN type LPB is required. Instead, when the same printing base paper is laminated to a 150mN liquid packaging board (LPB), the resulting laminated material may be suitable for packaging containers where a 260mN liquid packaging board (LPB) is usually required, i.e. for so-called family packs with a volume of 750ml to 1000ml. By such construction, the desired mechanical properties, in particular the desired bending stiffness etc., can be achieved in the final laminated packaging material to suit different sizes and types of packaging by combining only a few possible paper types with a few liquid packaging boards. In addition, the advantage of being able to replace between different outer printing base papers, i.e. being able to replace between different appearances of the packaging, can be achieved. The white printing surface can be easily replaced with a metallized printing surface, or a natural brown printing surface, or a surface of any color, of a similar type of printing base paper, i.e. with the same density, surface mass and other mechanical properties (tensile strength, tear strength) and Cobb value.

[0063] Another example of a suitable material for the bulk material layer is so-called corrugated paperboard, which is usually quite dense but has an inherent lower bending stiffness compared to conventional liquid packaging paperboard, together with other different mechanical properties, which, when produced as a packaging laminate for a conventional carton, would result in a deterioration of the dimensional and mechanical stability of the package from a laminate with a bulk layer of such material, and thereby the integrity and barrier properties of the package.

[0064] Thus, linerboard has a substantially lower inherent bending stiffness compared to liquid packaging board, or LPB, or laminated packaging materials suitable for liquid packaging.

[0065] The bending stiffness is generally not measured on linerboard materials, since they were intended for the manufacture of corrugated boxes anyway. However, such materials have been measured to have a bending stiffness that is at least 30%, such as at least 40%, such as at least 50% lower than that of liquid carton paperboard at a corresponding surface mass when the surface mass of the printable coating (clay coat) is excluded. However, the linerboard still contributes to the overall mechanical properties and bending stiffness of the laminated packaging material by also providing spacer layers, i.e. spacing layers, between the surface layers with a higher Young's modulus in the sandwich structure, and by having higher compressive strength properties in the plane (xy) of the layers than conventional liquid packaging board (LPB). Suitable such surface layers may be tissue paper (such as printing base paper) and, for example, aluminum metal foil.

[0066] Corrugated board is also known as corrugated case material (CCM) and the material required for corrugated board or case material is corrugated medium (or fluted medium) which is fluted (welled) in use and arranged in its corrugated state by being applied between two flat liners or intermediate liners. Such corrugated structures increase the bending stiffness of the sandwich structure due to the corrugated intermediate layer acting as a spacing or spacer layer between the two relatively thinner liner layers. Thus, the two types of papers that make up corrugated board are liner material, also commonly called kraft liner or certified liner, and corrugated paper (or corrugated medium) material.

[0067] Generally, corrugated paper materials have a higher bending stiffness per surface mass than liner materials.

[0068] Because linerboard is made primarily from natural unbleached cellulose fibers, it is generally brown or beige in color, although the color can vary depending on the type of cellulose, but white top liners also exist, which have a white top layer on one surface and are usually a more expensive material.

[0069] The liner is usually 850kg / m 3 Less than, for example, 835 kg / m 3 It has a density less than 100 nm, is brown or beige in color, and contains primarily softwood fibers, such as spruce and pine fibers. The fiber pulp from which the liner is made is a chemical pulp.

[0070] Corrugated paper is a paper product that is usually used as the core paper in corrugated container board, and has a strength of 600 to 750 kg / m 3 , e.g. 600-700kg / m 3 , usually about 650kg / m 3Corrugated paper has a density of 100%. Corrugated paper is brown or beige in color, contains mostly short fibers, and is generally a very cheap, low quality paper, as a liner, which is not suitable in itself for the manufacture of liquid carton packaging. However, when used as a spacer layer in a sandwich construction, if it is of the approved type and combined in the right manner with the right layers in such a packaging laminate, it can work well for this purpose at a substantially lower price.

[0071] However, the corrugated core paper is expected to form a non-corrugated spacer layer in the present invention, since it is a less stiff and cheaper fibrous material and can provide sufficient distance in the sandwich structure for the laminated liquid carton packaging material. A corrugated spacer layer, i.e. a spacer layer formed into a corrugation, is not within the scope of the present invention. Corrugated box material is excluded, since it poses completely different technical meanings and requirements for the laminated packaging material for liquid cartons.

[0072] Fibers commonly used in the manufacture of linerboard materials can be broadly categorized into two main types: recycled fibers and new, or virgin fibers. The properties of the paper depend on the structural properties of the various fibers that make up the sheet. In general, the higher the virgin fiber content, the stronger and stiffer (more resistant to compression) the corrugated paper or liner material will be. Birch is the optimal corrugated paper raw material. Its structure contains a high concentration of lignin and hemicellulose. The pulping process preserves the originally highly hydrophobic lignin and modifies the remaining hemicellulose so that the soft, flexible cellulose core of the fiber is protected. This results in higher stiffness and increased resistance to creep. When used for liquid packaging, commercially available corrugated paper materials need to be supplemented with one or more additional sizing agents during pulping or cellulosic web production to handle the liquid and high moisture conditions for this new use and application. Traditional sizing techniques and chemicals (AKD, ASA, rosin, etc.) can be used in corrugated paper materials to meet the requirements needed for a particular product.

[0073] Liners made from virgin fibers are called kraft liners, whereas liners from recycled fibers are known as certified liners. For liquid food packaging purposes, virgin fibers are preferred. A mixture of virgin and recycled fibers may also be possible. Kraft linerboard should have at least 80 wt.%, preferably 100 wt.%, virgin fibers. The fibers used for liners are longer than those used for corrugated paper materials, and since the liners are originally intended for the outer liner layer of carton materials, they are already sized to withstand different degrees of moisture and wet conditions.

[0074] Corrugated board materials have a bending stiffness at least 30% lower than comparable liquid packaging paperboards (when excluding the surface mass of the printable coating (clay coat)). On the other hand, they have a higher specific SCT in the machine direction (MD), i.e. a higher SCT value per unit of surface mass, than conventional liquid packaging board materials or than other paper or cellulosic materials that may be suitable in this situation. In general, corrugated paper materials have a higher bending stiffness per unit of surface mass than liner materials.

[0075] The SCT value is a property measured by the international standard ISO 9895 and is reliable for comparing different linerboard materials with each other. SCT, or Short compression Test, measures the internal compression resistance of paper fibers, i.e. the in-plane compressive strength of the paper in the CD and MD. This property varies depending on the surface weight of the particular paper being measured. The surface weight of paper products is measured according to ISO 536.

[0076] Packaging made from materials with higher specific SCT has better stackability, and thus specific SCT is a measure of the compressive strength per surface mass in the plane (xy plane) of the carton material. Since baseboard materials usually have a specific SCT of more than 30 Nm / g in MD, they should provide, among other things, the compressive strength and stackability properties required for liquid board laminates. They do not need to be optimized with respect to stiffness properties, since they are expected to be used only as (non-corrugated) spacer layers in laminated materials for liquid carton packaging. Thus, while liner materials are originally intended as surface layers in the sandwich structure of the corrugated box, in the present case the liquid carton will be used as spacer layers in a laminated structure with further surface layers laminated on both sides to provide the stiffness properties required for the laminated material.

[0077] In comparison, today's liquid board materials have a lower specific SCT of about 25 Nm / g, but are then optimized with respect to all other properties, because they are the primary ones relied upon to provide dimensional stability to the packaging material to which the liquid carton is laminated. When today's optimized liquid boards are replaced in the laminate with inexpensive spacer layers in a sandwich structure, such spacer layers need to have a higher specific SCT of over 30 Nm / g to compensate for the properties lost when the state of the art board is removed.

[0078] In terms of moisture resistance, these materials are recommended to be used with a thickness of 35 g / m to perform better in liquid carton packaging laminates. 2 The Cobb water adsorption value may be less than 0.05%. The Cobb value is measured according to ISO 535 and is already met by most liner materials, but some corrugated paper materials may require additional sizing for use as a non-corrugated spacer layer in a liquid carton packaging laminate. Therefore, the linerboard material in the bulk layer includes at least one sizing additive.

[0079] Since the new spacer layer will be laminated to the further surface layer in a sandwich configuration in the laminate structure, it is not necessary to provide a white or smooth (e.g. clay coated) printed surface on the spacer layer itself, so again, linerboard material is a suitable material for such a spacer layer.

[0080] On the other hand, linerboard material has a very rough surface characteristic, having a Bendtsen Surface Roughness Value of at least 500 ml air / min (Bentsen).

[0081] When a rough cellulose fiber layer such as a linerboard is laminated to a thin printing base paper, the surface roughness of the linerboard, specifically the liner, is transferred through the printing base paper, and even if the printing base paper itself is smooth, the printable outer surface of the printing base paper also becomes too rough for high-quality printing of exterior decorations onto packaging materials. Thus, it is difficult to produce a smooth, well-functioning printing surface with a printing base paper of reasonable thickness if the bulk layer material is a linerboard such as a linerboard. High surface roughness results in poor print quality both when printing on the printing base paper first in a separate operation and then laminating it to the liner, and when printing after laminating the printing base paper to the bulk material of the liner.

[0082] Therefore, the baseboard or liner should be modified to obtain a smoother surface on the outside facing the laminated packaging material. A suitable modification is to calender the baseboard, such as the liner, by applying high pressure to a hot surface. Typically, calendering is performed by metal belt calendering or heated roll calendering. A suitable nip pressure for smoothing a liner material having a surface roughness of more than 600 ml air / min, e.g. about 650 ml air / min, to a surface roughness below 200 ml air / min, e.g. below 150 ml air / min (Bentsen), is 80-120 kN / m, e.g. about 100 kN / m, and a suitable surface temperature for smoothing at a calendering operating speed of 500-1200, e.g. about 1000 m / min, is about 200° C. The nip area and operating speed are adjusted so that sufficient pressure is applied to the baseboard for a sufficient time to make its surface smoother.

[0083] Generally, the higher the pressure and / or temperature within a given time (calendering speed), the smoother the surface and the more glossy it becomes.

[0084] An alternative way to modify the liner would be to coat it with a printable coating (clay coat) to give it a smooth, printable surface. Such white coated liners with a surface roughness of 150-250 ml air / min (Bentsen) are commercially available, but are necessarily more expensive.

[0085] The thermoplastic polymer of the innermost heat-sealable layer may be a polyolefin, such as polyethylene.

[0086] Suitable thermoplastic polymers for the outermost and innermost heat-sealable liquid-tight layers in the laminated packaging material of the present invention are polyolefins, such as homopolymers or copolymers of polyethylene and polypropylene, preferably polyethylene, more preferably polyethylene selected from the group consisting of low density polyethylene (LDPE), linear LDPE (LLDPE), single-site catalyst metallocene polyethylene (m-LLDPE), and blends or copolymers thereof. According to a preferred embodiment, for optimal lamination and heat-sealing properties, the outermost heat-sealable liquid-tight layer is LDPE, while the innermost heat-sealable liquid-tight layer is a blend composition of m-LLDPE and LDPE. The outermost and innermost thermoplastic polymer layers can be applied to the desired thickness by (co)extrusion coating of molten polymers. The outermost and / or innermost liquid-tight heat-sealable layers can alternatively be applied in the form of prefabricated oriented or unoriented films. According to another embodiment, an outermost protective layer of a heat-sealable, liquid-tight thermoplastic polymer may be applied by aqueous dispersion coating of a thermoplastic polymer, for example when such an outermost layer is desired only in small thicknesses or when such a process is preferred for other reasons.

[0087] A gas barrier film or foil, including an oxygen barrier layer or coating, may be laminated to the inside of the bulk material layer, between the bulk material layer and the innermost layer of thermoplastic polymer.

[0088] It may be laminated by melt extrusion laminating an intermediate tie layer of a thermoplastic polymer between a web of the bulk material layer and a web of a gas barrier film or foil and pressing them together in a lamination roller nip. Alternatively, an aqueous composition of an adhesive polymer may be applied to one of the webs and then pressed together in a lamination roller nip such that the adhesive composition partially migrates into the cellulosic surface of the bulk material layer and adheres the two web surfaces together, thereby laminating the gas barrier film or foil.

[0089] A typical barrier foil in the field of laminated liquid carton packaging materials is aluminum foil, which may have a thickness of 5 to 9 μm, for example 5 to 6.5 μm.

[0090] Alternatively, a polymeric film substrate having a barrier coating, such as a dispersion or liquid coated barrier coating, or a vapor deposited barrier coating, may be laminated therebetween.

[0091] Thus, the oxygen barrier properties may be provided by a thin liquid film coating, e.g. a barrier polymer, which is coated on a substrate such as a paper or polymeric film substrate in the form of a dispersion or solution in a liquid medium or solvent and subsequently dried into a thin barrier coating. It is important that the dispersion or solution is homogeneous and stable so that a flat coating with uniform barrier properties results. Examples of polymers suitable for such aqueous liquid film compositions with barrier properties are polyvinyl alcohol (PVOH), water-dispersible ethylene vinyl alcohol (EVOH) or water-dispersible or water-soluble polymers based on polysaccharides. Such dispersion-coated or so-called liquid film coated (LFC) layers can be applied to substrates up to 1 m thick. 2It can be made extremely thin, up to a few tenths of a gram per unit area, and can provide a high quality, homogeneous layer if the dispersion or solution is homogeneous and stable, i.e., well prepared and mixed. PVOH has excellent oxygen barrier properties under dry conditions and provides very good odor barrier properties, i.e., the ability to prevent odorous substances from entering the packaging container from the surrounding environment, e.g., the refrigerator or storage room. This ability is important for long-term storage of the packaging. Furthermore, such liquid film coated polymer layers from water-dispersible or water-soluble polymers often provide good internal adhesion to adjacent layers, which contributes to good integrity of the final packaging container.

[0092] Suitably, the polymer is selected from the group consisting of vinyl alcohol based polymers, such as PVOH or water-dispersible EVOH, acrylic or methacrylic acid based polymers (PAA, PMAA), polysaccharides, such as starch or starch derivatives, cellulose nanofibrils (CNF), nanocrystalline cellulose (NCC), chitosan, hemicellulose or other cellulose derivatives, water-dispersible polyvinylidene chloride (PVDC) or water-dispersible polyesters, or a combination of two or more thereof.

[0093] More preferably, the polymeric binder is selected from the group consisting of PVOH, water dispersible EVOH, polysaccharides such as starch or starch derivatives, chitosan, or other cellulose derivatives, or a combination of two or more thereof.

[0094] Such barrier polymers are suitably applied in this manner using a liquid film coating process, i.e. in the form of an aqueous or solvent-based dispersion or solution which, when applied, spreads in a thin, uniform layer on the substrate and is then dried.

[0095] The liquid composition may additionally contain an inorganic component in order to further improve the oxygen gas barrier property.

[0096] The polymeric binder material may be mixed with, for example, lamellar or flaky inorganic compounds. The layered organization of the flaky inorganic particles forces oxygen gas molecules to travel a tortuous path through the oxygen barrier layer, a longer path than the normal straight path across the barrier layer.

[0097] The inorganic lamellar compound may be dispersed in an exfoliated state, i.e., the lamellar inorganic compound is separated from one another by a liquid medium, so-called nanoparticle compounds. Thus, the lamellar compound may preferably be expanded or cleaved by a polymer dispersion or solution that disperses and penetrates the lamellar structure of the inorganic material. It may also be expanded by a solvent before being added to the polymer solution or dispersion, or may be exfoliated by physical methods such as ultrasound. Thus, the inorganic lamellar compound is dispersed in the liquid gas barrier composition and in the dried barrier layer in an exfoliated state. Although there are many chemically suitable nanoclay minerals, the preferred nanoparticles are those of montmorillonite, e.g. purified montmorillonite or sodium-exchanged montmorillonite (Na-MMT). The nano-sized inorganic lamellar compound or clay mineral preferably has an aspect ratio of 50 to 5000 in an exfoliated state and a particle size of up to about 5 μm.

[0098] Preferably, the barrier layer comprises about 1 to about 40% by weight, more preferably about 1 to about 30% by weight, and most preferably about 5 to about 20% by weight of inorganic lamellar compound based on the dry coating weight. Preferably, the barrier layer comprises about 99 to about 60% by weight, more preferably about 99 to about 70% by weight, and most preferably about 95 to about 80% by weight of polymer based on the dry coating weight. Additives such as dispersion stabilizers may be included in the gas barrier composition, preferably in an amount of about 1% by weight or less based on the dry coating weight. The total dry content of the composition is preferably 5 to 15% by weight, more preferably 7 to 12% by weight.

[0099] According to different preferred embodiments, the inorganic particles may mainly consist of lamellar talc particles having an aspect ratio of 10 to 500. Preferably, the composition comprises talc particles in an amount of 10 to 50% by weight, more preferably 20 to 40% by weight, based on the dry weight. Below 20% by weight there is no significant increase in gas barrier properties, whereas above 50% by weight there is less internal cohesion between the particles in the layer, so that the coated layer may become more brittle and prone to breakage. The amount of polymer binder appears to be too small to surround and disperse the particles in the layer and laminate them to each other. The total dry content of such liquid barrier composition from PVOH and talc particles may be between 5 and 25% by weight.

[0100] Preferably, the oxygen gas barrier layer has a dry mass of 0.1 to 5 g / m 2 , preferably 0.5 to 3.5 g / m 2 , more preferably 0.5 to 2 g / m 2 The total amount is 0.1g / m 2 If the thickness is less than 5 g / m, the gas barrier properties will not be achieved at all. 2 Above this level, the generally high cost of the barrier polymer and the high energy costs of evaporating the liquid mean that the coated layer does not provide a cost-effective solution for packaging laminates. An acceptable level of oxygen barrier is 0.5 g / m2. 2 A good balance between barrier properties and cost is achieved with PVOH of 0.5 to 3.5 g / m 2 This is achieved between

[0101] The oxygen gas barrier layer may be applied as two part-layers in two successive steps with intermediate drying. When applied as two part-layers, each layer has a thickness of 0.1 to 2.5 g / m 2 , preferably 0.5 to 1 g / m 2 Preferably, the two layers are applied in amounts of 0.5 to 2 g / m2 each, resulting in a higher overall quality layer from a smaller amount of liquid gas barrier composition. 2 , preferably 0.5 to 1 g / m2 is administered in an amount of

[0102] According to different embodiments, the barrier coating may be applied onto the substrate surface of the film material using physical vapor deposition (PVD) or chemical vapor deposition (CVD). Although the substrate material itself may contribute some properties, the substrate material should first and foremost have the right surface properties and be suitable to receive the vapor deposition coating and function efficiently in the vapor deposition process.

[0103] Thin deposited layers are usually only nanometers thick, ie have a thickness of the order of nanometers, for example 1 to 500 nm (50 to 5000 Å), preferably 1 to 200 nm, more preferably 1 to 100 nm, most preferably 1 to 50 nm.

[0104] One common type of vapor-deposited coating that often has some barrier properties, such as water vapor barrier properties, is the so-called metallized layer, such as a metallic aluminum physical vapor deposition (PVD) coating.

[0105] Such vapour-deposited layers consisting essentially of metallic aluminium may have a thickness of 5-50 nm, which corresponds to less than 1% of the metallic aluminium material present in aluminium foil of conventional thickness for packaging, i.e. 6.3 μm. Vapour-deposited metal coatings require significantly less metal material and usually result in a lower level of oxygen barrier properties.

[0106] Other examples of vapor deposition coatings are aluminum oxide (AlOx) and silicon oxide (SiOx) coatings. Generally, such coatings are more brittle and less suitable for incorporation into packaging materials by lamination.

[0107] Other coatings for laminated packaging materials may be applied by plasma enhanced chemical vapor deposition (PECVD), in which vapors of compounds are deposited on a substrate under oxidizing conditions. PECVD coatings of silicon oxide (SiOx), for example, can achieve very good barrier properties under certain coating conditions and gas formulations.

[0108] The deposition coating may alternatively be a hydrogenated amorphous carbon barrier layer applied by plasma enhanced chemical vapor deposition, PECVD, so-called diamond-like carbon (DLC). DLC defines a class of amorphous carbon materials that exhibit some of the typical properties of diamond. Preferably, a hydrocarbon gas, e.g. acetylene or methane, is used as process gas in the plasma to produce the coating.

[0109] The same thermoplastic polyolefin-based materials, particularly polyethylene, listed above for the outermost and innermost layers may also be suitable in the interior of the laminated material, for example as a tie layer between a bulk material layer and a barrier film or foil.

[0110] Other adhesive polymers suitable for extrusion lamination of a tie layer as an intermediate tie layer between the innermost heat-sealable layer and a barrier film or foil, for example, may be so-called adhesive thermoplastic polymers, such as modified polyolefins, which are mostly based on copolymers or graft copolymers of LDPE or LLDPE, with monomer units containing functional groups such as carboxylic acid or glycidyl functional groups, for example (meth)acrylic acid or maleic anhydride (MAH) monomers (i.e. ethylene acrylic acid copolymer (EAA) or ethylene methacrylic acid copolymer (EMAA)), ethylene-glycidyl (meth)acrylate copolymer (EG(M)A), or MAH-grafted polyethylene (MAH-g-PE). Another example of such modified or adhesive polymers are the so-called ionomers or ionomeric polymers.

[0111] Depending on the requirements of the finished package, corresponding modified polypropylene-based thermoplastic adhesives or tie layers are also useful.

[0112] Such adhesive polymer layers or "tie" layers may be applied in a co-extrusion coating operation together with the respective heat-sealable outer layer, e.g. an innermost layer of a thermoplastic polymer, or together with an additional intermediate tie layer between the bulk material layer and the metallic aluminium foil.

[0113] EAA or EMAA adhesive polymers provide the best possible adhesion, for example as adhesive polymer layers bonding adjacent polyethylene layers to aluminum foil.

[0114] Thus, the gas barrier film or foil may be laminated to the bulk material layer by at least one intermediate tie layer of polyolefin (such as polyethylene, such as low density polyethylene (LDPE)), or adhesive polymer (such as polyolefin-based polymers modified with hydroxyl or carboxylic acid functional groups), or blends thereof.

[0115] Gas barrier films or foils have a dry content of 0.5 to 4 g / m 2 , for example 1 to 2 g / m 2 The barrier film or foil may be laminated to the bulk layer with an adhesive of acrylic modified polyethylene copolymer applied in an amount of 0.1 to 0.5 wt. %. Thus, the barrier film or foil can be laminated to the bulk material layer with only a small amount of the aqueous adhesive composition (20-50 wt. % dry content, e.g. 30-50 wt. %). The aqueous adhesive composition is partially absorbed into the network of fibers on the cellulose surface of the bulk material, so that even though a small amount of adhesive polymer is applied, it still laminates the surfaces together. EXAMPLES

[0116] Test Method: Basis weight, i.e. surface mass (units: g / m 2 ) is determined according to ISO 536.

[0117] Bendtsen surface roughness can be measured by clamping a test specimen between a flat glass plate and a circular metal head and measuring the airflow velocity between the paper and the head in mL / min. The Bendtsen technique is designed to work in the range of 30-1500 mL / min. Applicable test methods are BS 4420, ISO 8791 / 2, DIN 53108, and SCAN P21.

[0118] The Cobb test is used to determine the water absorption rate of paper, cardboard, and corrugated board. The Cobb test is performed according to the following standards: ISO 535, EN 20535, and TAPPI T 441. One Cobb unit is 1 g / m2 of water adsorbed on a surface during 60 seconds of exposure to water. 2 The Cobb value of a paper or paperboard depends heavily on its degree of sizing. Other factors such as the degree of beating of the fibers in the pulp may also play a role. For printing base papers suitable for the present invention, the Cobb value mainly reflects the degree of sizing of the paper. A shortened version of the Cobb test can be performed with half the absorption time above, i.e. 30 seconds. The values ​​must then be adjusted, i.e. doubled, to be comparable, but otherwise the test is essentially the same.

[0119] The tensile strength is measured according to ISO 1924-3, the unit of measurement is kN / m and is expressed as the geometric mean (GM) value between the values ​​in the machine direction (MD) and the cross direction (CD). The tensile specific strength of a cellulose material is its tensile strength normalized by its surface mass. The tensile specific strength is therefore expressed in units of Nm / g (GM).

[0120] Tear strength is measured according to ISO 1974:2012, in kN, and is also indicated as GM value. Specific tear strength is a value normalized by the surface mass of the test sample, in mNm 2 / g.

[0121] In Fig. 1a a first embodiment of the laminated packaging material of the invention, 10a, is thus shown. It has a weight of about 220 g / m 2 Surface mass, 780kg / m 3 The bulk material layer 11a of the liner has a density of 1000 nm, a specific SCT in MD of 34 Nm / g, and a Bendtsen value of 900 ml air / min when not yet calendered. The surface roughness was reduced to 200 mL / min by metal belt calendering at a surface temperature of about 200° C. in the metal belt nip and high pressure.

[0122] Outside the bulk material layer 11a, the packaging material comprises another layer of print base paper 12a. The print base paper has an outer surface for receiving and carrying the printed ink decoration 12a-1, which results in the decoration of the final package made from the packaging material. In this embodiment, the print side paper is 40 g / m 2 Surface mass, 650kg / m 3 Density of water: 27 g / m 2 Cobb value of 49 Nm / g, tensile specific strength (GM) of 6 mNm 2 The paper is a natural brown (unbleached) MG (machine gloss finish) paper with a specific tear strength of 1.0 MPa / g.

[0123] The printed decoration is protected against the external environment of the packaging by a liquid-tight, transparent outermost layer 13a of LDPE which is extrusion coated onto the printed printing base paper 12a (i.e. the printing base paper is provided with a printed decorative pattern 12a-1).

[0124] The printing base paper 12a has a density of 1 to 4 g / m 2 16. The paper is laminated to the bulk paperboard with a small amount of starch adhesive 16a between the paper.

[0125] On the inside of the bulk material layer 11a, which will face the inside of the packaging container formed from the laminated material, the laminated material comprises a metallic aluminium foil 14a having a thickness of 6.3 μm. The metallic aluminium foil is in contact with the bulk material paperboard by adhering it to a 20 g / m2 LDPE tie layer 17a is laminated to the bulk material layer.

[0126] The bulk material layer, or liner, is a layer that is cheap, bulkier than conventional LPB paperboard, and provides reduced dimensional support to the packaging material, but when laminated between the outer printing base paper and the inner aluminum foil, it can serve as a sandwich layer such that the resulting laminate has high and reliable bending stiffness, as well as high compressive strength.

[0127] On the opposite side, inside the metallic aluminum foil, is the innermost heat-sealable thermoplastic layer 15a, which is also the layer of the packaging laminate that will be in direct contact with the filled food product in the final package. The innermost layer 15a of heat-sealable polymer is melt co-extrusion coated onto the aluminum foil along with an intermediate adhesive polymer layer 18a of EAA.

[0128] Lamination of the bulk material layer 11a and the metallic aluminum foil 14a by extrusion lamination of an LDPE tie layer 17a was performed prior to co-extrusion coating an innermost layer of thermoplastic polymer 15a and an adhesive polymer layer 18a onto the metallic aluminum foil.

[0129] The innermost layer of thermoplastic polymer is a heat-sealable polymer selected from a composition comprising a blend of a polyolefin, such as polyethylene, in this case, a metallocene-catalyzed linear low density polyethylene (m-LLDPE) and a low density polyethylene (LDPE). Alternatively, or in addition, the heat-sealable material at the innermost part of the laminated packaging material may be divided into two part-layers of different types of polyethylene, for example there may be a first intermediate layer of LDPE in contact with the adhesive polymer layer, and a second innermost layer of a blend of mLLDPE and LDPE as described above.

[0130] A second embodiment of a similar laminated packaging material, 10b, is shown in Figure 1b. The laminated material is almost the same as that in Figure 1a. It is bleached white MG paper, 785 kg / m 3 Density: 70g / m 2 Surface mass of 24g / m 2 Cobb value of 100ml air / min (Bentsen) and outer surface roughness of 7mNm 2 The printing base paper 12b on which the print decoration 12b-1 is to be printed has a tear strength (GM) of 1 to 4 g / m2 on the outside of the bulk material layer 11b. 2 The laminate is made of starch adhesive.

[0131] The bulk material layer was the same as the liner used for FIG. 1a, with the surface roughness of its surface reduced by calendaring to 200 mL / min.

[0132] The gas barrier layer 14b is a substrate film 14b-1 of biaxially oriented polyethylene terephthalate (BOPET) that is coated with a nanometer-thick continuous coating 14b-2 of amorphous diamond-like carbon coating (DLC) by plasma-enhanced chemical vapor deposition. The DLC coating is oriented on the outside of the BOPET film and is bonded to the bulk material layer by an intermediate tie layer 17b of polyethylene. The BOPET film has a primer or adhesion-promoting coating (not shown) on its inside that further complies with the extrusion-coated polyolefin-based layer. The thus-primed or treated BOPET film is coextrusion-coated on its inside with an innermost layer 15b of a blend of mLLDPE and LDPE and an intermediate adhesion layer 18b of EAA.

[0133] The bulk material layer, or liner, is a layer that is cheap, bulkier than conventional LPB paperboard, and provides reduced dimensional support to the packaging material, but when laminated between the outer printing base paper and the inner layer, can contribute as a sandwich layer so that the resulting laminate achieves in any event a large and reliable bending stiffness, as well as a large compressive strength.

[0134] Figure 1c shows a third embodiment, 10c, of a laminated packaging material according to the present invention, which has the same bulk layer of liner 11c as in Figure 1a, and the same outer and innermost layers of thermoplastic polymer 13c and 15c as described in Figures 1a and 1b, but does not have an additional gas barrier layer inside the bulk material layer.

[0135] Such laminates are suitable, for example, for refrigerated dairy products, which do not require extremely high gas barrier properties of the packaging material.

[0136] Thus, the laminated packaging materials 10a, 10b, and 10c provide dairy and food fillers with the opportunity to easily differentiate and highlight their food products from one another with the interchangeable appearance of different printing base papers with different printing background effects.

[0137] FIG. 2a shows how a first web A of bulk material layers, which is liquid food grade paperboard, is laminated to a second web B of printing base paper by absorption lamination of an aqueous adhesive at low temperature. In an adhesive application operation 21, a small amount of aqueous adhesive solution is applied onto the non-printing side of the printing base paper web B. The wet-coated printing base paper web is laminated to the first web A of paperboard in a lamination operation 22 in the nip of two lamination rollers, and then the aqueous adhesive solution is absorbed into one or both of the surfaces of the two papers by simultaneously feeding the webs through the lamination nip 22 while they are pressed together and bonded.

[0138] In Fig. 2b it is shown how the web AB of laminated layers obtained in Fig. 2a is subsequently fed into a further lamination roller nip and laminated 25 with a third web C comprising a gas barrier layer such as an aluminum foil in Fig. 1a, 14a or a DLC coated film in Fig. 1b, 14b. Thus, the semi-laminate web AB and the web C comprising the gas barrier layer are fed into the lamination roller nip, while at the same time a molten curtain 23 of thermoplastic bonding polymer is extruded 24 downwards into the lamination roller nip and cooled, during which the two webs are pressed together in such a way that sufficient adhesion is obtained between the surfaces of the two webs AB and C, i.e. between the inner surface of the bulk material layer and the outer surface of the barrier foil or film, to form a laminated web 26.

[0139] Alternatively, when laminating the bulk material layer AB to the web C, a low temperature water-based adhesive absorption lamination method as described in FIG. 2a may be used.

[0140] The method steps of FIG. 2b are not necessary in the case of the packaging material of FIG. 1c, which is instead then wound onto a reel for intermediate storage or transportation to another time or location where final lamination and finishing steps can be performed.

[0141] In Fig. 2c it is mainly shown how the web AB of laminated printing base paper and bulk layer or the web ABC of bulk material layer, printing base paper and gas barrier film or foil obtained from Fig. 2a or 2b respectively is sent to a further lamination operation 27 in a roller nip, where a molten curtain 28 of the inner polymer layers, i.e. adhesive polymer layers 18a; 18b; optionally 18c, and the innermost layers 15a; 15b; 15c are co-extruded 29 downwards into the lamination roller nip, cooled and coated on the inside of the web AB or ABC as a multi-layer film coating by pressing and solidifying the polymer layers 18, 19 against the inner surface. The resulting laminate 30 may be sent for further similar lamination operations to extrusion coat laminate the outer layers of LDPE 13a, 13b, 13c to the opposite, outer side of the printing base papers 12a, 12b, 12c, or if this has already been done prior to the above lamination steps, it may be sent to a winding station to be wound up onto a reel for further transport and storage of the packaging laminate.

[0142] FIG. 3a shows an embodiment of a packaging container 30a produced from a packaging laminate 10a; 10b; 10c according to the invention. The packaging container is particularly suitable for beverages, sauces, soups, etc. Typically, the volume of such a package is about 100-1000 ml. It may be of any configuration, but is preferably brick-shaped, and it has longitudinal and transverse seals, 31a and 32a, respectively, and optionally an opening 33. In another embodiment (not shown), the package may be shaped like a wedge. To obtain such a "wedge shape", only the bottom part of the package is folded and formed such that the transverse heat seals of the bottom are hidden under triangular corner flaps, which are then folded and sealed against the bottom of the package. The transverse seals of the top section are left unfolded. The package half-folded in this way is easy to handle and dimensionally stable, even when placed on a shelf in a grocery store, on a desk, etc.

[0143] Figure 3b shows an alternative preferred embodiment of a packaging container 30b produced from an alternative packaging laminate according to the present invention. The alternative packaging laminate is thinner by having a thinner bulk layer of cellulose, and therefore is not dimensionally stable enough to form a rectangular, parallelepiped or wedge-shaped packaging container and is not folded and formed after the lateral closure 32b. It therefore remains a pillow-like pouch-type container and is distributed and sold in this form.

[0144] Figure 3c shows a gable-top package 30c that is folded and formed from a pre-cut sheet or blank from a laminated packaging material including a bulk layer of the paperboard of the present invention and a durable barrier film. Flat-top packages can also be formed from blanks of similar material.

[0145] Figure 3d shows a bottle-type package 30d, which combines a sleeve 34 formed from a pre-cut blank of the laminated packaging material of the invention with a top 35 formed from injection-molded plastic in combination with an opening such as a screw cap. Packages of this type are commercially available, for example, under the trade names Tetra Top® and Tetra Evero®. These particular packages are formed by attaching a molded top 35 having an opening attached in a closed position to a tubular sleeve 34 of laminated packaging material, sterilizing the bottle-top capsule thus formed, filling it with a food product, and finally folding and forming the bottom of the package and sealing it.

[0146] Figure 4 shows the principle as described in the introduction of this application: a web of packaging material is formed into a tube 41 by integrating the longitudinal ends 42 of the web together at overlapping joints 43. The tube is filled 44 with the intended liquid food product and divided into individual packages by repeating transverse sealing 45 of the tube at a predetermined distance from each other below the level of the contents filled in the tube. The packages 46 are separated by incising at the transverse sealings and given the desired geometric configuration by folding along fold lines prepared in the material.

[0147] FIG. 5 shows the surface roughness values ​​(Bentsen ml air / min) of the different cellulosic materials used in the present invention. 2 A typical liner (SCA Kraftliner) with a surface mass of 70 g / m2 and an SR value of 640 ml air / min was 2 The laminate was applied to a printing base paper that was a flexible wrapping paper (Lennoflex from Feldmuehle) with a surface weight of about 1.5 g / m2 and an initially measured surface roughness of the print side of about 15 (commercially available as 20) ml air / min. The lamination was performed using a water-based adhesive composition containing starch and was applied wet to a thickness of about 1.4 g / m2. 2 The dry weight of the aqueous composition was 16 wt%. The surface roughness of the printed surface of the laminated printing base paper obtained after lamination was then reduced to 146 ml air / min, which was considered too high to be acceptable.

[0148] In further experiments, the above liner was calendered in a metal belt calender with a nip load of 100 kN / m and a surface temperature of about 200° C. The surface roughness obtained on the metal belt side was 141 ml air / min, i.e., approximately the same as the liner laminate described previously. This calendered liner (which lost some surface mass due to moisture loss during calendering, i.e., 125 g / m instead) was obtained. 2When a rough liner having a surface mass of 100 ml / min was instead laminated in the same way to the same printing base paper, the resulting surface acquired a roughness value of only 42 ml air / min, i.e., much lower than half the maximum allowable value of the printing base paper (i.e., 100 ml air / min), even though the initial surface roughness value of the printing base paper was the same in both experiments. Thus, by calendering the rough liner before laminating it to the printing base paper, it is possible to obtain a printing surface similar to or even smoother than that of a conventional liquid packaging paperboard, such as a clay-coated Duplex LPB. Furthermore, it is possible to obtain a sufficiently smooth printing surface of the laminate of the printing base paper and the bulk material layer of the liner, such that it is possible to ensure that the metallized surface can maintain its mirror-like smooth appearance and is not negatively affected by the roughness of the various bulk material layers.

[0149] Figure 6 shows the principle of operation of metal belt calendering. A corrugated board sheet 61, such as a liner, is fed into a nip 62 between a metal belt 63 and a metal roller 64 while heat is supplied to the nip and the surface of the liner by the heated metal roller 64 and a pressure force is simultaneously applied by a pressure roller 65. In heated roller calendering, which is usually applied directly in-line after the paper making line (not shown here), the liner is simply passed through a series of heated, hard pressure roller nips.

[0150] The present invention is not limited by the embodiments shown and described above, which may vary within the scope of the claims. In general terms, the ratios between the thicknesses of the layers, the ratios between the distances of the layers, and the sizes of other features and their relative sizes compared to each other should not be taken as shown in the figures. They merely describe the order and type of layers relative to each other, and all other features that should be understood as described in the text specification. [Explanation of symbols]

[0151] 10a packaging material 10b Packaging materials 10c packaging material 11a Cellulosic bulk material layer 11b Cellulosic bulk material layer 11c Cellulosic bulk material layer 12a Cellulosic printing base paper 12a-1 Outer printing surface 12b Cellulosic printing base paper 12b-1 Outer printing surface 12c Cellulosic printing base paper 12c-1 Outer printing surface 13a Transparent outer protective layer of thermoplastic polymer 13b Transparent outer protective layer of thermoplastic polymer 13c Transparent outer protective layer of thermoplastic polymer 14a Gas barrier film or foil 14b Gas barrier film or foil 14b-1 Base film 14b-2 DLC coated film 15a Innermost layer of heat sealable, liquid tight thermoplastic polymer 15b Innermost layer of heat sealable, liquid tight thermoplastic polymer 15c Innermost layer of heat sealable, liquid tight thermoplastic polymer 16a Starch adhesive 16b Starch adhesive 16c Starch adhesive 17a bonding layer 17b Bonding layer 18a Adhesive polymer layer 18b Intermediate adhesive layer, adhesive polymer layer 18c Adhesive polymer layer 21 Step of applying the water-based adhesive composition 22 Pressure Roller Nip 23 Melt curtains of thermoplastic polymers 24 Extrusion 25 Lamination 26 Laminated Web 27 Laminating process 27' Laminating process 28 Melting Curtain 29 Coextrusion 30 Lamination 30a packaging container 30b Packaging container 30c Gable Top Packaging 30d Bottle Packaging 31a Vertical Seal 31b Vertical sealing 32a Horizontal sealing 32b Horizontal sealing 33 Mouth opening 34 Sleeve 35 Top 41 Tubes 42 Vertical edge 42' Vertical End 43 Joint 44 Filling 45 Horizontal sealing 46 Packaging 61 Corrugated cardboard 62 Nip 63 Metal Belt 64 Metal Roller 65 Pressure Roller A. A first web of cellulosic bulk material layer AB: A web of layers in which a printing base paper and a bulk layer are laminated together ABC Bulk material layer, printing base paper, and gas barrier film or foil web B. A second web of cellulosic printing base paper C. Web containing a gas barrier layer

Claims

1. A laminated packaging material (10a; 10b; 10c) for packaging liquid food, comprising a cellulosic bulk material layer (11a; 11b; 11c), a transparent outermost protective layer of a thermoplastic polymer (13a; 13b; 13c) arranged on the outer side of the bulk material layer, i.e., on the side that will face the outside of a packaging container made from the laminated material, a decorative printed pattern arranged under, i.e., on the inner side, the transparent outermost protective layer of the thermoplastic polymer and visible through said transparent outermost protective layer of the thermoplastic polymer, and an innermost layer (15a; 15b; 15c) of a heat-sealable, liquid-tight thermoplastic polymer that will be in direct contact with the liquid food in the packaging container, wherein the bulk material layer is a corrugated paperboard, said corrugated paperboard being calendered to a Bendtsen outer surface roughness value of less than 200 ml air / min, and wherein the innermost layer (15a; 15b; 15c) of a heat-sealable, liquid-tight thermoplastic polymer that will be in direct contact with the liquid food in the packaging container, 536, and a bending stiffness that is at least 30% lower than the bending stiffness of the liquid packaging board at the corresponding surface weight when the surface weight of the printable coating (clay coat) is excluded, the laminated packaging material further comprising a cellulose-based printing base paper (12a; 12b; 12c), said printing base paper having an outer printing surface (12a-1; 12b-1; 12c-1) carrying a decorative printing pattern, said printing base paper having a dry weight of 1 to 4 g / m 2 and is adhered to the outside of the bulk material layer by an adhesive of 100 g / m 2 and the outer printed surface has a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min. Laminated packaging materials.

2. 2. The laminated packaging material of claim 1, wherein a gas barrier film or foil (14a; 14b) comprising an oxygen barrier layer or coating is laminated on the inside of the bulk material layer, between the bulk material layer and the innermost layer of thermoplastic polymer.

3. 3. The laminated packaging material according to claim 1 or 2, wherein the bulk material layer (11a; 11b; 11c) is calendered to an outer surface roughness of less than 150 ml air / min (Bentsen) before being laminated to the printing base paper.

4. 4. The laminated packaging material according to claim 1, wherein the outer printed surface (12a-1; 12b-1; 12c-1) has a Bendtsen surface roughness value below 80 ml air / min, below 70 ml air / min, below 60 ml air / min, or below 50 ml air / min.

5. The printing base paper (12a; 12b; 12c) is 80 g / m 2 Less than 70 g / m 2 5. The laminated packaging material of claim 1 having a surface mass of less than 1000 nm.

6. The outer printing surface (12a-1; 12b-1; 12c-1) is 20 to 30, or 22 to 28, or 24 to 27, or 24 to 26 g / m 2 2. The laminated packaging material of claim 1 having a Cobb value of (water).

7. The printing base paper (12a; 12b; 12c) is 650 kg / m 3 Higher density, 100 g / m 2 Surface mass (ISO 536) of at least 40 Nm / g, tensile index (GM) of at least 6.0 mNm 2 / g, and comprising 0.1 to 0.4 wt. % of at least one sizing agent, and the outer printing surface (12a-1; 12b-1; 12c-1) has a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min, and a specific tear strength (GM) of less than 20 g / m 2 (Water) 30 g / m 2 7. The laminated packaging material of claim 1 having a Cobb value less than (water).

8. 8. The laminated packaging material according to any one of claims 1 to 7, wherein the printing base paper (12a; 12b; 12c) is a paper selected from the group consisting of MG (machine glossy) paper, MF (machine finished) paper, LWC (lightweight coated) paper, flexible wrapping paper, digital printing paper and inkjet printing paper.

9. 9. The laminated packaging material according to any one of claims 1 to 8, wherein the outer printing surface (12a-1; 12b-1; 12c-1) of the printing base paper (12a; 12b; 12c) is metallized and has a surface roughness of less than 100 ml air / min (Bentsen), or less than 50 ml air / min.

10. 10. The laminated packaging material according to any one of claims 1 to 9, wherein the outer printing surface (12a-1; 12b-1; 12c-1) of the printing base paper (12a; 12b; 12c) is naturally brown in colour.

11. A liquid food packaging container (30a; 30b; 30c; 30d) comprising a laminated packaging material according to any one of claims 1 to 10.

12. 1. A method for producing a laminated packaging material for packaging liquid food products, comprising the steps of: a) providing a first web (A) of cellulosic bulk material layer which is a calendered linerboard having a Bendtsen outer surface roughness value of less than 200 ml air / min, a specific SCT in MD greater than 30 Nm / g determined according to ISO 9895 and ISO 536, and a bending stiffness at least 30% lower than that of a liquid packaging board at its corresponding surface weight excluding the surface weight of the printable coating (clay coat), where outer means the side which will face the exterior of a packaging container made from the laminated material; b) 100 g / m 2 Providing a second web (B) of cellulosic printing base paper having a surface weight (ISO 536) of 0.1 mm or less and an outer printing surface carrying a decorative printing pattern, said outer printing surface having a Bendtsen surface roughness value (ISO 8791-2) of less than 100 ml air / min; c) Adhesive polymer in a dry content of 1 to 4 g / m 2 on at least one of the outer side of the first web and the inner side of the second web, where inner side means facing the interior of the packaging container; d) delivering the first and second webs from step c) towards a pressure roller nip (22) to laminate them together with the intervening aqueous adhesive composition while passing through the nip and while the aqueous adhesive composition is partially absorbed into at least one surface of the first and second webs (A and B); e) printing a decorative printing pattern onto the printing surface of the printing base paper; f) laminating an innermost layer of a heat sealable thermoplastic polymer to the inside of the web of bulk material layer, opposite the print base paper side, innermost meaning the side that will come into contact with the liquid food in said packaging container (27); g) laminating a transparent outermost protective layer of a thermoplastic polymer to the outer side of the web of printing base paper, i.e., the outer printing side opposite the bulk material layer side (27'); The method includes:

13. 13. The method according to claim 12, wherein step e) is carried out before steps c) and d), in which the printing base paper is first printed with a decorative print on its printing side (12a-1; 12b-1; 12c-1) in a separate printing operation.

14. 14. The method according to claim 12 or 13, wherein a gas barrier film or foil (14a; 14b) comprising an oxygen barrier layer or coating is laminated on the inside of the bulk material layer, between the bulk material layer and the innermost layer of thermoplastic polymer.

15. 15. The method according to any one of claims 12 to 14, wherein the bulk material layer (11a; 11b; 11c) has been calendered in a separate step prior to step a) to an outer surface roughness of less than 200 ml air / min (Bentsen), or less than 150 ml air / min (Bentsen), at a nip load of 80-120 kN / m and a surface temperature above 200°C, at a calendering speed of 500-1200 m / min.

Citation Information

Patent Citations

  • Laminate packaging material, packaging container made therefrom, and method for producing the laminate material

    JP2018537314A