Preparation of aqueous dispersions of copolymer particles of vinyl acetate and cyclic ketene acetal monomers.

By preparing VA-CKA copolymers under controlled emulsion polymerization conditions, the method addresses the hydrolytic instability of CKA, minimizing by-products and enhancing the efficiency of CKA incorporation into polymer backbones for biodegradable packaging.

JP7586649B2Active Publication Date: 2024-11-19ROHM & HAAS CO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020046306
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-10
Filing Date
2020-03-17
Publication Date
2024-11-19
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

The hydrolytic instability of cyclic ketene acetal (CKA) monomers in water leads to the formation of undesirable hydrolysis by-products, necessitating the use of costly organic solvents and affecting the efficiency of polymer backbone incorporation, especially in applications requiring aqueous-based copolymers like degradable packaging and thin films.

Method used

Aqueous-based copolymers of vinyl acetate (VA) and CKA are prepared under emulsion polymerization conditions at 30°C to 55°C and pH 6.0 to 9.0, using 0.05 to 5 parts by weight of a monoethylenically unsaturated acid monomer or its salt, forming an aqueous dispersion of copolymer particles without volatile organic solvents.

Benefits of technology

This method significantly reduces the formation of undesirable hydrolysis by-products, enabling the production of biodegradable packaging products with efficient incorporation of CKA units into the polymer backbone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586649000001
    Figure 0007586649000001
  • Figure 0007586649000002
    Figure 0007586649000002
  • Figure 0007586649000003
    Figure 0007586649000003
Patent Text Reader

Abstract

To provide a method of preparing aqueous-based VA-CKA copolymers for significantly reducing formation of unwanted hydrolytic byproducts.SOLUTION: The method comprises the steps of contacting, under emulsion polymerization conditions, vinyl acetate, a cyclic ketene acetal monomer, and a monoethylenically unsaturated acid monomer or a salt thereof, so as to form an aqueous dispersion of copolymer particles comprising structural units of the vinyl acetate, cyclic ketene acetal and monoethylenically unsaturated acid monomer or salt thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the preparation of aqueous dispersions of polymer particles comprising structural units of vinyl acetate and cyclic ketene acetal monomers. [Background technology]

[0002] Copolymers of vinyl acetate (VA) and cyclic ketene acetal (CKA) monomers such as 2-methylene-1,3-dioxepane (MDO) are particularly useful in applications requiring degradation of the polymer backbone, such as degradable packaging, or physical erosion of polymer-based thin films and surface coatings. These copolymers have been described as being prepared in the presence of organic solvents, as disclosed, for example, in Polym. J. 2009, 41, 650-660; Polym. Chem. 2012, 3, 1260-1266; Polym. Chem. 2015, 6, 7447-7454; and US1996 / 5541275.

[0003] Because CKA is known to be hydrolytically unstable, organic solvents are used to prepare CKA-containing polymers. For example, MDO hydrolyzes in water to form 4-hydroxybutyl acetate, thereby reducing the efficiency of incorporation of MDO structural units into the copolymer backbone. Thus, the hydrolytic instability of MDO mandates the use of non-reactive organic solvents, which unfortunately are undesirable due to the high costs associated with removal, recovery, and recycling, and their contribution to residual volatile organic solvents in the final isolated product.

[0004] Summary of the Invention [Problem to be solved by the invention]

[0005] It would therefore be advantageous to find a method for preparing aqueous-based VA-CKA copolymers in a manner that significantly reduces the formation of undesirable hydrolysis by-products. [Means for solving the problem]

[0006] The present invention addresses the need in the art by providing a process comprising the steps of: a) contacting, under emulsion polymerization conditions of a temperature in the range of 30° C. to 55° C., and a pH in the range of 6.0 to 9.0, 1) 75 to 98.5 parts by weight of vinyl acetate, 2) 1 to 20 parts by weight of a cyclic ketene acetal monomer, and 3) 0.05 to 5 parts by weight of a monoethylenically unsaturated acid monomer or salt thereof to form an aqueous dispersion of copolymer particles comprising structural units of vinyl acetate, a cyclic ketene acetal, and a monoethylenically unsaturated acid monomer or salt thereof, wherein the cyclic ketene acetal monomer is characterized by the structure: [ka] where n is 0, 1, or 2; R is H or C 1 -C 6 -alkyl, R 1 and R 2 are independently H, C 1 -C 12 -alkyl, phenyl, or vinyl; or R 1 and R 2 together with the carbon atoms to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, and R 1’ and R 2’ are each independently H or C 1 -C 12 -alkyl, or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’ are independently H, C 1 -C 12-alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Furthermore, if n is 2, then Each R 3 , H, C 1 -C 12 Alkyl, or together with the carbon atom to which they are attached, a double bond, a fused benzene ring, or a fused C 3 -C 7 - an alicyclic ring.

[0007] The methods of the present invention provide aqueous dispersions that are substantially free of volatile organic solvents, which are useful, for example, in the manufacture of biodegradable packaging products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention provides a method comprising the steps of: a) contacting, under emulsion polymerization conditions of a temperature in the range of 30° C. to 55° C., and a pH in the range of 6.0 to 9.0, 1) 75 to 98.5 parts by weight of vinyl acetate, 2) 1 to 20 parts by weight of a cyclic ketene acetal monomer, and 3) 0.05 to 5 parts by weight of a monoethylenically unsaturated acid monomer or salt thereof to form an aqueous dispersion of copolymer particles comprising structural units of vinyl acetate, a cyclic ketene acetal, and a monoethylenically unsaturated acid monomer or salt thereof, wherein the cyclic ketene acetal monomer is characterized by the structure: [ka] n is 0, 1, or 2; R is H or C 1 -C 6 -alkyl, R 1 and R 2 are independently H, C 1 -C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2together with the carbon atoms to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 -C 12 -alkyl, or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’ are independently H, C 1 -C 12 -alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Furthermore, if n is 2, Each R 3 , H, C 1 -C 12 Alkyl, or together with the carbon atom to which they are attached, may form a double bond, a fused benzene ring, or a fused C 3 -C 7 - Forms an alicyclic ring.

[0009] As used herein, the term "structural unit of vinyl acetate" refers to a polymer backbone containing the following repeating units: [ka] Here, the dotted lines represent points of attachment to other structural units in the polymer backbone.

[0010] The term "cyclic ketene acetal monomer structural unit" is used to refer to a polymer backbone that includes the following repeat units: [ka] Here, R, R 1 , R 2 , R 3 , R 1’ , R 2’ , R 3’ , and n is as previously defined.

[0011] Examples of cyclic ketene acetal monomers include: [ka] [ka]

[0012] A preferred cyclic ketene acetal monomer is 2-methylene-1,3-dioxepane (MDO). [ka]

[0013] The structural units of MDO are illustrated. [ka]

[0014] The ethylenically unsaturated acid monomer may be a carboxylic acid-containing monomer, a phosphoric acid-containing monomer, or a sulfur acid-containing monomer, or their salts. Examples of suitable carboxylic acid-containing monomers include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, and fumaric acid, examples of suitable phosphorus-containing monomers include phosphoethyl methacrylate and 2-(methacryloyloxy)ethylphosphonic acid, and suitable sulfur-containing monomers include 2-acrylamido-2-methyl-1-propanesulfonic acid (AMPS), vinylsulfonic acid, 2-sulfoethyl acrylate, 2-sulfoethyl methacrylate, 3-sulfopropyl acrylate, 3-sulfopropyl methacrylate, and 2-propene-1-sulfonic acid. The ethylenically unsaturated acid monomer is preferably a sulfonic acid-containing monomer, preferably a salt of a sulfonic acid-containing monomer, and the salt of 2-acrylamido-2-methylpropanesulfonic acid is particularly preferred.

[0015] Preferably, the polymer particles have a z-average particle size in the range from 50 nm, more preferably from 80 nm, most preferably from 100 nm, preferably to 500 nm, more preferably to 300 nm, more preferably to 200 nm, and most preferably to 150 nm.

[0016] Preferably, VA is used in an amount of 80 parts by weight, more preferably in the range of 85 parts by weight to 96.5 parts by weight, more preferably 95 parts by weight, based on the weight of VA, CKA, and the ethylenically unsaturated acid monomer; preferably, CKA is used in an amount of 3 parts by weight to 15 parts by weight, more preferably 12 parts by weight, and most preferably 8 parts by weight, based on the weight of VA, CKA, and the ethylenically unsaturated acid monomer; and the monoethylenically unsaturated acid monomer is preferably used in an amount of 0.1 parts by weight to 3 parts by weight, more preferably up to 1 part by weight, based on the weight of VA, CKA, and the ethylenically unsaturated acid monomer.

[0017] Preferably, the composition is substantially free of hydrolysis by-products of CKA and VA. More specifically, when the CKA is MDO, the composition preferably contains less than 20, more preferably less than 10, more preferably less than 5, more preferably less than 2, and most preferably less than 1 undesirable ester 4-hydroxybutyl acetate (exemplified below) based on the weight of the structural units of MDO in the polymer particles. [ka]

[0018] The composition preferably further comprises less than 3000 ppm, more preferably less than 2000 ppm, of acetic acid, an undesirable by-product of VA hydrolysis.

[0019] In a preferred method of the present invention, VA, CKA, preferably MDO, and monoethylenically unsaturated acid monomer, preferably a salt of a sulfur acid-containing monomer, more preferably a salt of AMPS, are contacted together under emulsion polymerization conditions. Preferably, VA and CKA are combined together and then mixed with an aqueous solution of surfactant and monoethylenically unsaturated acid monomer under emulsion polymerization conditions. The reaction is controlled at a temperature ranging from 30° C., preferably from 35° C. to 55° C., preferably up to 50° C., more preferably up to 45° C., and a pH ranging from 6.0, preferably from 6.5, more preferably from 7.0, most preferably from 7.5 to 9.0, more preferably up to 8.5. After completion of the polymerization, a dispersion of copolymer is obtained having a solids content ranging from preferably 20 weight percent, more preferably from 25 weight percent, most preferably from 30 to 50 weight percent, more preferably up to 40 weight percent.

[0020] Surprisingly, it was discovered that aqueous dispersions of copolymers of VA and CKA can be efficiently prepared without the use of organic solvents and with minimal undesirable hydrolysis by-products of CKA and VA.

[0021] How to measure particle size Particle size was measured using a Malvern Zetasizer Nano ZS90, which was used to measure the Z-average particle size (D) using dynamic light scattering (DLS) at a scattering angle of 90° using Zetasizer software version 7.11. z ) was measured. A drop of the sample dispersion was diluted using an aqueous solution of MilliQ water (18.2 MΩ.cm at 25 °C) to achieve particle counts in the range of 200,000 to 400,000 counts per second (Kcps). Particle size measurements were performed using the particle size measurement method of the instrument, D z was calculated by the software. D z is also known as the intensity-based harmonic mean grain size and is expressed as:

number

[0022] Acetic acid determination method Analysis of acetic acid was performed using an Agilent 1100 Series High Performance Liquid Chromatography system equipped with a Phenomenex Rezex ROA-Organic Acid H+(8%) (250x4.6) mm column (part number 00G-0138-E0), a Phenomenex Security Guard Carbo-H4 element, a UV detector operating at a wavelength of 210 nm, and an autosampler. The column oven temperature was set at 35 °C, and the mobile phase was 2.5 mM phosphoric acid in MilliQ water. The instrument was operated at a flow rate of 0.4 mL / min (isocratic), and the sample injection volume was 5 μL. Data acquisition and analysis were performed using Agilent ChemStation software (version B.04.03). Samples were prepared for analysis by diluting (1:100) with MilliQ water, followed by agitation for 10 min on a horizontal reciprocating shaker. The samples were centrifuged at 100,000 rpm for 10 min at 25° C., and the supernatant was filtered through a 0.45 μm disposable syringe filter for injection.

[0023] Example 1 - Preparation of an Aqueous Dispersion of VA / MDO Polymer Particles A monomer mixture was prepared in a vessel by combining vinyl acetate (VA, 205.95 g) and 2-methylene-1,3-dioxepane (MDO, 10.88 g). Separately, an aqueous mixture was prepared in a vessel by combining deionized water (46.18 g), 2-acrylamido-2-methyl-1-propanesulfonic acid sodium salt (AMPS salt, 1.40 g, 50% active in water), Tergitol-15-S-40 secondary alcohol ethoxylate (15-S-40, 1.51 g, 70% active in water), and Disponil® FES-32, sodium lauryl ether sulfonate (FES-32, 6.15 g, 31% active in water). Separately, deionized water (285.0 g) was added to a four-neck, 1-L round-bottom reactor equipped with an overhead stirrer, condenser, and thermocouple. The reactor was heated to 40 °C, then FES-32 (16.4 g, 31% active in water), AMPS salt (3.95 g, 50% active in water), FeSO 4 7H 20 (16.2 g, 0.15 active in water) and ethylenediaminetetraacetic acid (EDTA, 3.45 g, 1.0 wt % in water) were added to the reactor with the aid of additional deionized water (51.6 g). The monomer mixture and the aqueous mixture were fed simultaneously to the reactor over 60 minutes while maintaining the reactor temperature at 40° C. Concurrently, a separately prepared solution of ammonium persulfate / t-butyl hydroperoxide (1.38 g APS and 0.58 g t-BHP in 37.0 g water) and Bruggolite FF6 (2.62 g in 37.6 g water) were fed to the reactor over 70 minutes. The reaction was measured to be pH=6.5-7 throughout the feed process. Once the feed addition was complete, the reactor temperature was maintained at 40° C. for 15 minutes and then cooled to 30° C. The resulting dispersion was adjusted to pH=7 by addition of ammonium hydroxide (28% active in water) and filtered through a 38 μm screen. The filtrate was analyzed for percent solids (32.9%) and the z-average particle size was determined to be 116 nm, as measured using dynamic light scattering (DLS). The uptake of 2-methylene-1,3-dioxepane (MDO) was determined by diffusion editing. 1 It was determined to be (84.3 ± 4.3)% by 1 H NMR spectroscopy. A 5% error was assumed in all integrals and propagated through the calculation of MDO incorporation.

[0024] Example 2 Example 1 was repeated, but the reaction was maintained at pH=8 throughout the feed by dropwise addition of ammonium hydroxide (28% active in water). The filtrate was analyzed for percent solids (31.3%) and the z-average particle size was determined to be 122 nm, as measured by DLS. The uptake of MDO was determined by diffusion spectroscopy. 1 It was determined to be essentially quantitative (~100%) by 1 H NMR spectroscopy.

[0025] Example 3 Example 2 was repeated, but a monomer mixture was prepared by combining VA (183.95 g) and MDO (32.88 g). The filtrate was analyzed for percent solids (29.7%) and the z-average particle size was determined to be 92 nm, as measured by DLS. The uptake of MDO was determined by diffusion editing. 1 It was determined to be 97.8±6.6% by 1 H NMR spectroscopy.

[0026] Comparative Example 1 Example 1 was repeated, except that the reaction temperature was maintained at 60° C. throughout the feed. The filtrate was analyzed for percent solids (29.8%) and the z-average particle size, as measured by DLS, was determined to be 177 nm. The uptake of MDO was determined by diffusion editing. 1 It was determined to be 55.1±3.9% by 1 H NMR spectroscopy.

[0027] Comparative Example 2 Example 1 was repeated, but the reaction temperature was maintained at 80° C. throughout the feeds. The filtrate was analyzed for percent solids (29.4%) and the z-average particle size, as measured by DLS, was determined to be 217 nm. The uptake of MDO was determined by diffusion editing. 1 It was determined to be 37.8±2.7% by 1 H NMR spectroscopy.

[0028] Comparative Example 3 Example 1 was repeated, except that the reaction was maintained at pH=5 throughout the feed by dropwise addition of acetic acid (10% active in water). The filtrate was analyzed for percent solids (31.0%) and the z-average particle size was determined to be 248 nm, as measured by DLS. The uptake of MDO was determined by diffusion spectroscopy. 1 It was determined to be 29.0±2.0% by 1 H NMR spectroscopy.

[0029] Comparative Example 4 Example 1 was repeated, but the reaction was maintained at pH=9.5 throughout the feed by dropwise addition of ammonium hydroxide (28% active in water). The filtrate was analyzed for percent solids (29.6%) and the z-average particle size, as measured by DLS, was determined to be 283 nm. The uptake of MDO was determined by diffusion editing. 1 The colloidal stability of the sample was nevertheless low, yielding a gel of 7850 ppm, determined by H NMR spectroscopy to be 90.3 ± 6.3%. The sample turned dark brown on standing, and unusually high concentrations of acetic acid and acetaldehyde were observed.

[0030] These examples demonstrate the important role that temperature and pH play in optimizing the incorporation of water-sensitive monomers into the polymer backbone and reducing the formation of undesirable hydrolysis products arising from these monomers.

Claims

1. 1. A method comprising: a) under emulsion polymerization conditions at a temperature in the range of 30° C. to 55° C. and a pH in the range of 6.0 to 9.0; 1) 75 to 98.5 parts by weight of vinyl acetate, 2) 1 to 20 parts by weight of a cyclic ketene acetal monomer, and 3) contacting 0.05 to 5 parts by weight of a monoethylenically unsaturated acid monomer or salt thereof to form an aqueous dispersion of copolymer particles comprising vinyl acetate, cyclic ketene acetal, and monoethylenically unsaturated acid monomer or salt thereof structural units; The cyclic ketene acetal monomer is characterized by the structure: [Case 1] n is 0, 1, or 2; R is H or C 1 -C 6 - alkyl, R 1 and R 2 are each independently H, C 1 -C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 -C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 -C 12 -alkyl, or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, when n is 1, R 3 and R 3’ are each independently H, C 1 -C 12 - alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, with the proviso that when n is 2, Each R 3 is H, C 1 -C 12 Alkyl, together with the carbon atom to which they are attached, may form a double bond, a fused benzene ring, or a fused C 3 -C 7 - forming an alicyclic ring.

2. 2. The method of claim 1, wherein the cyclic ketene acetal monomer, the vinyl acetate, and the monoethylenically unsaturated acid monomer or salt thereof are contacted under emulsion polymerization conditions, at a temperature in the range of from 35° C. to 55° C., and at a pH in the range of from 6.5 to 8.

5.

3. 3. The method of claim 2, wherein the cyclic ketene acetal monomer is selected from the group consisting of: [chemical 2-1] [Case 2-2]

4. 4. The method of claim 3, wherein the cyclic ketene acetal monomer is 2-methylene-1,3-dioxepane, the monoethylenically unsaturated acid monomer is a sulfur acid containing monomer or salt thereof, and the 2-methylene-1,3-dioxepane, the vinyl acetate, and the sulfur acid containing monomer or salt thereof are contacted under emulsion polymerization conditions at a temperature in the range of from 35° C. to 50° C., and a pH in the range of from 7.5 to 8.

5.

5. 5. The method of claim 4, wherein the sulfur acid-containing monomer or salt thereof is selected from the group consisting of 2-acrylamido-2-methyl-1-propanesulfonic acid, salts of 2-acrylamido-2-methyl-1-propanesulfonic acid, vinyl sulfonic acid, salts of vinyl sulfonic acid, 2-sulfoethyl acrylate, 2-sulfoethyl methacrylate, 3-sulfopropyl acrylate, 3-sulfopropyl methacrylate, sodium styrenesulfonate, 2-propene-1-sulfonic acid, and salts of 2-propene-1-sulfonic acid.

6. The method of claim 5, wherein the sulfur acid-containing monomer or salt thereof is a salt of 2-acrylamido-2-methyl-1-propanesulfonic acid.

7. The method of claim 4, wherein the aqueous dispersion of copolymer particles further comprises less than 20 weight percent of 4-hydroxybutyl acetate based on the weight of 2-methylene-1,3-dioxepane structural units in the copolymer particles, and the 2-methylene-1,3-dioxepane, vinyl acetate, and sulfur acid-containing monomer or salt thereof are contacted under emulsion polymerization conditions at a temperature in the range of 35°C to 45°C.

8. The method of claim 7, wherein the aqueous dispersion of copolymer particles further comprises less than 10 weight percent of 4-hydroxybutyl acetate, based on the weight of 2-methylene-1,3-dioxepane structural units in the copolymer particles.

9. The method of claim 8, wherein the aqueous dispersion of copolymer particles further comprises less than 2 weight percent of 4-hydroxybutyl acetate based on the weight of 2-methylene-1,3-dioxepane structural units in the copolymer particles.

Citation Information

Patent Citations

  • Polymer latex from vinyl acetate and vinyl ester of branched carboxylic acid

    JP1993222131A

  • Biodegradable vinyl ester copolymer

    JP1994322104A

  • Methacrylate copolymer and molding

    JP2017210503A

  • Aqueous adhesive compositions and methods for making same

    JP2020530058A

  • Biodegradable vinyl ester copolymers

    US5541275A