Anode active material, anode layer and fluoride ion secondary battery

The use of AlF3, Li3AlF6, and Li2ZrF6 as a negative electrode active material in fluoride ion secondary batteries addresses the insulating issue of aluminum fluoride, enhancing charge/discharge capacity and voltage stability.

JP7586735B2Active Publication Date: 2024-11-19HONDA MOTOR CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021033737
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-03
Publication Date
2024-11-19
Estimated Expiration
2041-03-03

AI Technical Summary

Technical Problem

Aluminum fluoride, used as a negative electrode active material in fluoride ion secondary batteries, has insulating properties that hinder electrochemical reactions, and existing fluoride ion secondary batteries have limited charge/discharge capacity.

Method used

A negative electrode active material comprising AlF3, Li3AlF6, and Li2ZrF6, which can be combined with other negative electrode active materials, enhances the charge/discharge capacity by facilitating electrochemical reactions through defluorination and stabilizing voltage.

Benefits of technology

The proposed material improves the charge/discharge capacity of fluoride ion secondary batteries by promoting defluorination and stabilizing voltage, resulting in higher performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586735000001
    Figure 0007586735000001
  • Figure 0007586735000002
    Figure 0007586735000002
  • Figure 0007586735000003
    Figure 0007586735000003
Patent Text Reader

Abstract

To provide a negative electrode active material which enables the increase in charge / discharge capacity of a fluoride ion secondary battery.SOLUTION: A negative electrode active material comprises AlF3, Li3AlF6 and Li2ZrF6.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode active material, a negative electrode layer, and a fluoride ion secondary battery. [Background technology]

[0002] Lithium ion secondary batteries have been widely used as secondary batteries having high energy density. A lithium ion secondary battery has a separator disposed between a positive electrode and a negative electrode, and is filled with an electrolyte.

[0003] The electrolyte solution of a lithium ion secondary battery usually contains a flammable organic solvent, and therefore, there have been cases where thermal safety has been a problem.

[0004] In view of this, fluoride ion secondary batteries have been studied as all-solid-state batteries in which a solid electrolyte layer is disposed between a positive electrode layer and a negative electrode layer (see, for example, Patent Documents 1 to 6). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-87403 A [Patent Document 2] JP 2017-50113 A [Patent Document 3] JP 2019-29206 A [Patent Document 4] JP 2018-206755 A [Patent Document 5] JP 2018-198130 A [Patent Document 6] JP 2018-92863 A Summary of the Invention [Problem to be solved by the invention]

[0006] Aluminum fluoride has been considered as a negative electrode active material for fluoride ion secondary batteries. However, aluminum fluoride has insulating properties and is therefore less susceptible to electrochemical reactions.

[0007] Therefore, the applicant has proposed to use Li3AlF6 as the negative electrode active material of the fluoride ion secondary battery, but it is desired to further improve the charge / discharge capacity of the fluoride ion secondary battery.

[0008] An object of the present invention is to provide a negative electrode active material capable of improving the charge / discharge capacity of a fluoride ion secondary battery. [Means for solving the problem]

[0009] In one embodiment of the present invention, the negative electrode active material contains AlF3, Li3AlF6, and Li2ZrF6.

[0010] The negative electrode active material may include a complex of AlF3, Li3AlF6, and Li2ZrF6.

[0011] In another embodiment of the present invention, a negative electrode layer contains the above-described negative electrode active material.

[0012] Another embodiment of the present invention is a fluoride ion secondary battery having the above-described negative electrode layer, an electrolyte, and a positive electrode layer. Effect of the Invention

[0013] According to the present invention, it is possible to provide a negative electrode active material capable of improving the charge / discharge capacity of a fluoride ion secondary battery. [Brief description of the drawings]

[0014] [Figure 1] 1 is an XRD spectrum of the AlF3-Li3AlF6-Li2ZrF6 composite of Example 1. [Diagram 2] 1 shows an SEM photograph and EPMA analysis results of the AlF3-Li3AlF6-Li2ZrF6 composite of Example 1. [Diagram 3] FIG. 2 is a diagram showing initial charge / discharge curves of the all-solid-state fluoride ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described.

[0016] <Negative electrode active material> The negative electrode active material of this embodiment contains AlF3, Li3AlF6, and Li2ZrF6, and therefore when the negative electrode active material of this embodiment is applied to a fluoride ion secondary battery, the charge / discharge capacity is improved.

[0017] Here, Li2ZrF6 is defluorinated before AlF3 and Li3AlF6 during charging, and by stabilizing the voltage of the fluoride ion secondary battery, AlF3 and Li3AlF6 are easily defluorinated, thereby improving the charge / discharge capacity of the fluoride ion secondary battery.

[0018] The molar ratio of Li3AlF6 to AlF3 is preferably 0.1 or more, more preferably 0.5 or more. When the molar ratio of Li3AlF6 to AlF3 is 0.1 or more, the contact between Li3AlF6 and inactive AlF3 increases, so that defluorination of AlF3 is likely to occur.

[0019] The molar ratio of Li2ZrF6 to AlF3 is preferably 0.1 to 3, more preferably 0.3 to 1.5. When the molar ratio of Li2ZrF6 to AlF3 is 0.1 or more, the contact between Li2ZrF6 and inactive AlF3 increases, and the stability of the voltage of the fluoride ion secondary battery improves, so that defluorination of AlF3 is likely to occur. When the molar ratio of Li2ZrF6 to AlF3 is 3 or less, the capacity and voltage of the fluoride ion secondary battery improve.

[0020] The negative electrode active material of this embodiment may further contain a negative electrode active material other than AlF, Li3AlF6, and Li2ZrF6.

[0021] The negative electrode active material other than AlF, Li3AlF6, and Li2ZrF6 is not particularly limited as long as it is a negative electrode active material used in a fluoride ion secondary battery.

[0022] [Complex of AlF3, Li3AlF6, and Li2ZrF6] The negative electrode active material of this embodiment may contain a complex of AlF3, Li3AlF6, and Li2ZrF6, which improves the charge / discharge capacity when the negative electrode active material of this embodiment is applied to a fluoride ion secondary battery.

[0023] In the composite of AlF3, Li3AlF6, and Li2ZrF6, for example, at least a portion of the surface of AlF3 and Li3AlF6 is covered with Li2ZrF6.

[0024] The particle size of the composite of AlF3, Li3AlF6, and Li2ZrF6 is preferably 1 mm or less, more preferably 200 μm or less. When the particle size of the composite of AlF3, Li3AlF6, and Li2ZrF6 is 1 mm or less, it is easy to obtain a uniform powder when preparing the powder composition for the negative electrode layer.

[0025] [Method for producing a composite of AlF3, Li3AlF6, and Li2ZrF6] A composite of AlF3, Li3AlF6, and Li2ZrF6 can be obtained by crushing AlF3, LiF, and ZrF4, followed by calcination. At this time, LiF and ZrF4 react in a molar ratio of 2:1 to produce Li2ZrF6, and then the remaining LiF and AlF3 react in a molar ratio of 3:1 to produce Li3AlF6, with the remaining AlF3 remaining.

[0026] The molar ratio of LiF to AlF3 is preferably from 1 to 5. When the molar ratio of LiF to AlF3 is from 1 to 5, the ionic conductivity of the complex of AlF3, Li3AlF6, and Li2ZrF6 increases, so that defluorination of AlF3 is more likely to occur.

[0027] The molar ratio of ZrF4 to AlF3 is preferably 0.1 to 3, more preferably 0.3 to 1.5. When the molar ratio of ZrF4 to AlF3 is 0.1 or more, the ionic conductivity of the composite of AlF3, Li3AlF6, and Li2ZrF6 becomes high, so that defluorination of AlF3 is likely to occur. In addition, when the molar ratio of ZrF4 to AlF3 is 3 or less, the capacity and voltage of the fluoride ion secondary battery are improved.

[0028] As a method for pulverizing AlF3, LiF, and ZrF4, for example, a method of pulverizing them using a ball mill can be mentioned.

[0029] The firing temperature is preferably 850° C. or higher and 900° C. or lower. If the firing temperature is 850° C. or higher, the reaction proceeds sufficiently, and if the firing temperature is 900° C. or lower, evaporation of the raw materials is suppressed.

[0030] The calcination time is preferably 1 hour or more and 3 hours or less. When the calcination time is 1 hour or more, the reaction proceeds sufficiently, and when it is 3 hours or less, evaporation of the raw materials is suppressed.

[0031] <Negative electrode layer> The negative electrode layer of this embodiment contains the negative electrode active material of this embodiment, and may further contain a conductive assistant, a solid electrolyte, and the like.

[0032] The total content of AlF3, Li3AlF6 and Li2ZrF6 in the negative electrode layer of this embodiment is preferably 50 mass% or less, more preferably 30 mass% or less. When the total content of AlF3, Li3AlF6 and Li2ZrF6 in the negative electrode layer of this embodiment is 50 mass% or less, the charge / discharge capacity is improved when the negative electrode layer of this embodiment is applied to a fluoride ion secondary battery.

[0033] [Conductive additive] The conductive assistant may be, for example, a carbon material.

[0034] The carbon material may be carbon black.

[0035] Examples of carbon black include furnace black, ketjen black, and acetylene black, and two or more of these may be used in combination.

[0036] [Solid electrolyte] Examples of the solid electrolyte include lanthanide fluorides doped with alkaline earth metal fluorides, alkaline earth metal fluorides, etc. Among these, lanthanide fluorides doped with alkaline earth metal fluorides are preferred in terms of ion conductivity.

[0037] The lanthanoid fluoride is not particularly limited, but examples thereof include LaF3, CeF3, SmF3, and NdF3, and two or more of them may be used in combination.

[0038] The alkaline earth metal fluoride with which the lanthanoid fluoride is doped is not particularly limited as long as it has ion conductivity. Examples of the alkaline earth metal fluoride include CaF2, SrF2, BaF2, etc., and two or more of them may be used in combination.

[0039] Examples of lanthanide fluorides doped with alkaline earth metal fluorides include La 0.9 Ba 0.1 F 2.9 , Ce 0.95 Ba 0.05 F 2.95 , Ce 0.95 Sr 0.05 F 2.95 , Ce 0.95 Ca 0.05 F 2.95 and the like, and two or more of them may be used in combination.

[0040] When the negative electrode layer of the present embodiment contains a carbon material as a conductive assistant, the lanthanoid fluoride doped with the alkaline earth metal fluoride may be composited with the carbon material, that is, the negative electrode layer of the present embodiment may contain a composite of the lanthanoid fluoride doped with the alkaline earth metal fluoride and a carbon material (hereinafter, also referred to as a composite of the lanthanoid fluoride and a carbon material).

[0041] [Lanthanoid fluoride-carbon composite] In the composite of a lanthanoid fluoride and a carbon material, for example, at least a part of the surface of a lanthanoid fluoride particle is coated with a carbon material.

[0042] The particle size of the composite of the lanthanoid fluoride and the carbon material is preferably 10 μm or less, and more preferably 5 μm or less. When the particle size of the composite of the lanthanoid fluoride and the carbon material is 10 μm or less, the ionic conductivity and the electronic conductivity are improved.

[0043] The mass ratio of the carbon material to the lanthanoid fluoride doped with the alkaline earth metal fluoride is preferably 3% by mass or more and 20% by mass or less, from the viewpoint of the balance between ionic conductivity and electronic conductivity.

[0044] The content of the composite of lanthanoid fluoride and carbon material in the negative electrode layer of this embodiment is preferably 60% by mass or more and 70% by mass or less. When the content of the composite of lanthanoid fluoride and carbon material in the negative electrode layer of this embodiment is 60% by mass or more and 70% by mass or less, the discharge capacity is improved when the negative electrode layer of this embodiment is applied to a fluoride ion secondary battery.

[0045] [Method for producing a composite of lanthanide fluoride and carbon material] A method for producing a composite of a lanthanoid fluoride and a carbon material (hereinafter also referred to as the composite) includes a first step of obtaining a lanthanoid fluoride-alkaline earth metal fluoride mixed powder, a second step of mixing the lanthanoid fluoride-alkaline earth metal fluoride mixed powder with a carbon material to obtain a composite precursor, and a third step of calcining the composite precursor to obtain the composite.

[0046] The first step is to mix a lanthanoid fluoride with an alkaline earth metal fluoride to obtain a lanthanoid fluoride-alkaline earth metal fluoride mixed powder. That is, by mixing a lanthanoid fluoride with an alkaline earth metal fluoride, the solid-phase diffusion distance of elements derived from the lanthanoid fluoride and the alkaline earth metal fluoride can be shortened during firing. In addition, after firing, a lanthanoid fluoride-alkaline earth metal fluoride mixed powder is obtained in which the crystal structure of the lanthanoid fluoride and the alkaline earth metal fluoride does not remain.

[0047] The method for mixing the lanthanoid fluoride and the alkaline earth metal fluoride is not particularly limited, and either a dry method or a wet method may be used. For example, a method in which the mixture is mixed using a mortar may be used.

[0048] The conditions, such as temperature and time, for mixing the lanthanoid fluoride and the alkaline earth metal fluoride can be appropriately set.

[0049] In the first step, the lanthanoid fluoride-alkaline earth metal fluoride mixed powder may be pulverized.

[0050] The lanthanide fluoride-alkaline earth metal fluoride mixed powder may be pulverized, for example, by using a ball mill.

[0051] The second step is a step of mixing the lanthanoid fluoride-alkaline earth metal fluoride mixed powder obtained in the first step with a carbon material to obtain a composite precursor.

[0052] In the method for producing the composite, the second step is carried out prior to the third step, in which the lanthanide fluoride-alkaline earth metal fluoride mixed powder is mixed with the carbon material in advance, thereby obtaining a composite precursor in which the carbon material is disposed on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder.

[0053] Therefore, by calcining the composite precursor in the third step, a composite is obtained in which at least a part of the surface of the lanthanoid fluoride particles doped with the alkaline earth metal fluoride is coated with the carbon material.

[0054] Furthermore, by disposing a carbon material on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder in the second step, coarsening of the particle size due to grain growth of the lanthanide fluoride-alkaline earth metal fluoride mixed powder and fusion of particle interfaces during the crystallization process in the third step can be suppressed, and a composite can be obtained that roughly maintains the particle size of the lanthanide fluoride-alkaline earth metal fluoride mixed powder.

[0055] In the second step, the method for mixing the lanthanide fluoride-alkaline earth metal fluoride mixed powder with the carbon material is not particularly limited, and either a dry method or a wet method may be used. For example, a method of mixing using a mortar may be used.

[0056] When the lanthanoid fluoride-alkaline earth metal fluoride mixed powder and the carbon material are mixed, it is preferable to apply shear.

[0057] The conditions such as the temperature for mixing the lanthanoid fluoride-alkaline earth metal fluoride mixed powder with the carbon material can be appropriately set.

[0058] Furthermore, in the second step, the composite precursor may be pulverized.

[0059] Examples of the method for pulverizing the composite precursor include a method for pulverizing using a ball mill and a method for pulverizing using a mortar.

[0060] The third step is a step of calcining the composite precursor obtained in the second step to obtain a composite.

[0061] In the second step, a composite precursor in which a carbon material is disposed on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder is obtained, and by doing so, the grain growth of the lanthanide fluoride-alkaline earth metal fluoride mixed powder and coarsening of the grain size due to fusion of the grain interfaces during the crystallization process in the third step are suppressed, resulting in a composite that roughly maintains the grain size of the composite precursor.

[0062] The conditions for firing the composite precursor can be appropriately set.

[0063] In the third step, the complex may be pulverized.

[0064] The method for pulverizing the complex may be, for example, a method in which the complex is pulverized using a mortar.

[0065] <Fluoride ion secondary battery>

[0066] The fluoride ion secondary battery of this embodiment has the negative electrode layer of this embodiment, an electrolyte, and a positive electrode layer.

[0067] [Electrolyte] The electrolyte may be an electrolytic solution, a solid electrolyte, or a gel electrolyte. The solid electrolyte or gel electrolyte may be either organic or inorganic.

[0068] As the solid electrolyte, a known solid electrolyte can be used. For example, the solid electrolyte contained in the negative electrode layer of the present embodiment may be used as the solid electrolyte.

[0069] When a solid electrolyte is used as the electrolyte, the fluoride ion secondary battery of this embodiment is an all-solid-state fluoride ion secondary battery, which includes, for example, a positive electrode collector, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode collector, which are arranged in this order.

[0070] [Positive electrode layer] The positive electrode layer includes, for example, a positive electrode active material, a solid electrolyte, and a conductive additive. In this case, it is preferable to use a positive electrode layer that can obtain a sufficiently high standard electrode potential compared to the standard electrode potential of the negative electrode layer of this embodiment.

[0071] Examples of the positive electrode active material include Pb, Cu, Sn, Bi, and Ag.

[0072] Examples of solid electrolytes include PbSnF4 and Ce. 1-x Ba x F 3-x etc.

[0073] The conductive assistant may be, for example, a carbon material.

[0074] [Positive and negative electrode current collectors] Examples of the positive electrode current collector include a lead plate, an aluminum foil, etc. Examples of the negative electrode current collector include a gold foil, etc. EXAMPLES

[0075] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0076] [Example 1] An all-solid-state fluoride ion secondary battery was fabricated by the following method. Unless otherwise specified, each step was carried out in a purged glove box DBO-1.5B (manufactured by Miwa Manufacturing Co., Ltd.) equipped with an argon gas circulation purification device.

[0077] [Preparation of AlF3-Li3AlF6-Li2ZrF6 composite] 4.7 g of AlF3 powder, 4.4 g of LiF powder, 0.9 g of ZrF4 powder, and 20 silicon nitride mill balls (manufactured by Fritsch) with a diameter of 10 mm were placed in an 80 cc silicon nitride ball mill pot (manufactured by Fritsch) made of Premium Line PL-7, and then sealed. Here, the molar ratio of AlF3, LiF, and ZrF4 was 1:3:0.5.

[0078] The sealed ball mill pot was taken out of the glove box, and then the powder was ground using a ball mill under the following conditions:

[0079] Rotational speed: 400 rpm Grinding time: 15 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0080] After the ball mill pot was carried into the glove box, the AlF3-Li3AlF6-Li2ZrF6 mixed powder was collected from inside the ball mill pot.

[0081] The AlF3-Li3AlF6-Li2ZrF6 mixed powder was transferred to an alumina crucible and then fired in a small electric furnace KSL-1100X (manufactured by MTI) to obtain an AlF3-Li3AlF6-Li2ZrF6 composite. The firing conditions were as follows:

[0082] Argon gas flow rate: 300cc / min Heating rate: 184℃ / h Maximum temperature reached: 900℃ Hold time at maximum temperature: 1 hour Temperature drop rate: Uncontrolled Cooling method: natural cooling

[0083] The AlF3-Li3AlF6-Li2ZrF6 composite was collected from inside the alumina crucible and then ground for 5-10 minutes using an agate mortar and pestle.

[0084] XRD was used to analyze the AlF3-Li3AlF6-Li2ZrF6 composites.

[0085] The XRD spectrum of the AlF3-Li3AlF6-Li2ZrF6 composite is shown in Figure 1. In addition, the XRD spectra of AlF3, LiF, ZrF4, Li3AlF6 and Li2ZrF6 are also shown in Figure 1.

[0086] From FIG. 1, it can be seen that in the XRD spectrum of the AlF3-Li3AlF6-Li2ZrF6 composite, the peaks derived from the raw materials LiF and ZrF4 disappear, and the peaks derived from the products Li3AlF6 and Li2ZrF6 appear.

[0087] The AlF3-Li3AlF6-Li2ZrF6 composite was observed using SEM-EPMA, and the mapping elements were Al and Zr.

[0088] Figure 2 shows the SEM photograph and EPMA analysis results of the AlF3-Li3AlF6-Li2ZrF6 composite.

[0089] From FIG. 2, it can be seen that in the AlF3-Li3AlF6-Li2ZrF6 composite, the surfaces of AlF3 and Li3AlF6 are covered with Li2ZrF6.

[0090] [Ce 0.95 Ba 0.05 F 2.95 -Preparation of AB complex] (1st step) 8.598 g of CeF3 powder (Sigma-Aldrich; purity 99.99%) and 0.402 g of BaF2 powder (High Purity Chemical Laboratory; purity 99.9%) were weighed out and mixed for 5 to 10 minutes using an agate mortar and pestle to obtain a CeF3-BaF2 mixed powder.

[0091] The CeF3-BaF2 mixed powder and 20 silicon nitride grinding balls (manufactured by Fritsch) with a diameter of 10 mm were placed in an 80 cc silicon nitride ball mill pot, a Premium Line PL-7 dedicated container (manufactured by Fritsch), and then sealed.

[0092] The sealed ball mill pot was taken out of the glove box, and then the powder was ground using a ball mill under the following conditions:

[0093] Rotational speed: 800 rpm Grinding time: 60 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0094] After the ball mill pot was carried into the glove box, the CeF3-BaF2 mixed powder was collected from inside the ball mill pot.

[0095] (2nd process) Using an agate mortar and pestle, 700 mg of CeF3-BaF2 mixed powder was mixed with 50 mg of Denka Black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as acetylene black (AB). 0.95 Ba 0.05 F 2.95 -AB complex precursor was obtained.

[0096] Ce 0.95 Ba 0.05 F 2.95 The -AB composite precursor, 20 zirconia grinding balls (manufactured by Fritsch) having a diameter of 10 mm, and 20 silicon nitride grinding balls (manufactured by Fritsch) having a diameter of 10 mm were placed in a Premium Line PL-7 dedicated container (manufactured by Fritsch) as an 80 cc silicon nitride ball mill pot, and then the container was sealed.

[0097] The sealed ball mill pot was taken out of the glove box, and then the powder was ground using a ball mill under the following conditions:

[0098] Rotational speed: 800 rpm Grinding time: 60 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0099] After the ball mill pot was brought into the glove box, Ce was extracted from inside the ball mill pot. 0.95 Ba 0.05 F 2.95 The Ce-AB complex precursor was recovered. 0.95 Ba 0.05 F 2.95 The -AB complex precursor was ground for 5-10 minutes using an agate mortar and pestle.

[0100] (3rd step) Ce 0.95 Ba 0.05 F 2.95 The -AB composite precursor was transferred to an alumina crucible and then fired in a small electric furnace KSL-1100X (manufactured by MTI) to obtain Ce. 0.95 Ba 0.05 F 2.95 The sintering conditions were as follows:

[0101] Argon gas flow rate: 300cc / min Heating rate: 184℃ / h Maximum temperature reached: 1100℃ Hold time at maximum temperature: 1 hour Temperature drop rate: Uncontrolled Cooling method: natural cooling

[0102] From inside the alumina crucible, Ce 0.95 Ba 0.05 F 2.95The -AB complex was collected and then ground for 5 to 10 minutes using an agate mortar and pestle.

[0103] [Preparation of powder composition for negative electrode layer] 250 mg of AlF3-Li3AlF6-Li2ZrF6 composite and Ce 0.95 Ba 0.05 F 2.95 750 mg of the -AB complex and 40 g of silicon nitride grinding balls (manufactured by Fritsch) having a diameter of 2 mm were placed in a 45 cc silicon nitride ball mill pot (manufactured by Fritsch), a container exclusively for the Premium Line PL-7, and then sealed.

[0104] The sealed ball mill pot was taken out of the glove box, and then the powder was ground using a ball mill under the following conditions:

[0105] Rotation speed: 300 rpm Grinding time: 15 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0106] The ball mill pot was carried into the glove box, and then the powder composition for the negative electrode layer was collected from inside the ball mill pot.

[0107] [Preparation of powder for positive electrode layer (PbSnF4-AB composite)] 63.7% by mass of lead fluoride powder (manufactured by Kojundo Chemical Co., Ltd.), 29.6% by mass of tin fluoride powder (manufactured by Kojundo Chemical Co., Ltd.), and 6.7% by mass of Denka Black (manufactured by Denka Co., Ltd.) as AB were mixed in a ball mill and then fired at 400°C for 1 hour in an argon atmosphere to obtain a PbSnF4-AB composite.

[0108] [Powder for solid electrolyte layer (Ce 0.95 Ba 0.05 F 2.95 ) (1st step) 8.598 g of CeF3 powder (Sigma-Aldrich; purity 99.99%) and 0.402 g of BaF2 powder (High Purity Chemical Laboratory; purity 99.9%) were weighed out and mixed for 5 to 10 minutes using an agate mortar and pestle to obtain a CeF3-BaF2 mixed powder.

[0109] The CeF3-BaF2 mixed powder and 20 silicon nitride grinding balls (manufactured by Fritsch) with a diameter of 10 mm were placed in an 80 cc silicon nitride ball mill pot, a Premium Line PL-7 dedicated container (manufactured by Fritsch), and then sealed.

[0110] The sealed ball mill pot was taken out of the glove box, and then the powder was ground using a ball mill under the following conditions:

[0111] Rotational speed: 800 rpm Grinding time: 60 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0112] After the ball mill pot was carried into the glove box, the CeF3-BaF2 mixed powder was collected from inside the ball mill pot.

[0113] (2nd process) The CeF3-BaF2 mixed powder was transferred to an alumina crucible and then fired in a small electric furnace KSL-1100X (manufactured by MTI) to obtain Ce. 0.95 Ba 0.05 F 2.95 The firing conditions were as follows:

[0114] Argon gas flow rate: 300cc / min Heating rate: 184℃ / h Maximum temperature reached: 1100℃ Hold time at maximum temperature: 1 hour Temperature drop rate: Uncontrolled Cooling method: natural cooling

[0115] From inside the alumina crucible, Ce 0.95 Ba 0.05 F 2.95 After collection, it was ground for 5 to 10 minutes using an agate mortar and pestle.

[0116] [Fabrication of all-solid-state fluoride-ion secondary batteries] A cylindrical pellet-type cell was produced by pressing under a pressure of 40 MPa using a tablet press. Specifically, a 20 μm thick gold foil (manufactured by Nilaco; purity 99.99%) as a negative electrode current collector, 10 mg of a powder composition for a negative electrode layer, 150 mg of powder for a solid electrolyte layer, 20 mg of powder for a positive electrode layer, a 200 μm thick lead plate (manufactured by Nilaco; purity 99.99%) as a positive electrode active material and positive electrode current collector, and a 20 μm thick aluminum foil (manufactured by Nilaco; purity 99+%) as a positive electrode current collector were put into the tablet press in this order to produce a pellet-type cell.

[0117] [Example 2] An all-solid-state fluoride ion secondary battery was produced in the same manner as in Example 1, except that when preparing the powder composition for the negative electrode layer, a mixture of 28 mg of AlF3 powder, 110 mg of Li3AlF6 powder, and 112 mg of Li2ZrF6 powder (molar ratio 0.5:1:0.8) was used instead of 250 mg of the AlF3-Li3AlF6-Li2ZrF6 composite, and the grinding treatment conditions were changed as follows.

[0118] Rotation speed: 300 rpm Grinding time: 15 minutes Number of grinding processes: 40 Rest time between grinding processes: 5 minutes Rotation reverse: ON

[0119] [Comparative Example 1] An all-solid-state fluoride ion secondary battery was produced in the same manner as in Example 2, except that Li3AlF6 powder was used instead of the mixture of AlF3 powder, Li3AlF6 powder and Li2ZrF6 powder when producing the powder composition for the negative electrode layer.

[0120] [Comparative Example 2] An all-solid-state fluoride ion secondary battery was produced in the same manner as in Example 2, except that Li2ZrF6 powder was used instead of the mixture of AlF3 powder, Li3AlF6 powder and Li2ZrF6 powder when producing the powder composition for the negative electrode layer.

[0121] [AlF3-Li3AlF6-Li2ZrF6 complex and Ce 0.95 Ba 0.05 F 2.95 -AB complex particle size] The powder was photographed using a scanning electron microscope SU-6600 (Hitachi High-Technologies Corporation), and the length of the powder in the SEM images of multiple fields of view was measured and used as the particle size.

[0122] As a result, AlF3-Li3AlF6-Li2ZrF6 composite and Ce 0.95 Ba 0.05 F 2.95 The particle sizes of the -AB complexes were 200 μm and 50 μm, respectively.

[0123] [Charge / discharge test] A constant current charge / discharge test was carried out on the all-solid-state fluoride ion secondary battery. Specifically, a potentiogalvanostat SI1287 / 1255B (manufactured by Solartron) was used to carry out a constant current charge / discharge test in a vacuum environment at 140°C, with a charge current of 0.04mA, a discharge current of 0.02mA, a lower limit voltage of -2.44V, and an upper limit voltage of -0.1V. The constant current charge / discharge test was carried out starting with charging.

[0124] FIG. 3 shows the initial charge / discharge curves of the all-solid-state fluoride ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2.

[0125] It can be seen from FIG. 3 that the all solid state fluoride ion secondary batteries of Examples 1 and 2 have higher charge / discharge capacities than the all solid state fluoride ion secondary batteries of Comparative Examples 1 and 2.

Claims

1. AlF 3 And, Li 3 AlF 6 And, Li 2 ZrF 6 and a negative electrode active material comprising:

2. AlF 3 And, Li 3 AlF 6 And, Li 2 ZrF 6 The negative electrode active material of claim 1 , comprising a composite of

3. A negative electrode layer comprising the negative electrode active material according to claim 1 or 2.

4. A fluoride ion secondary battery comprising the anode layer according to claim 3, an electrolyte, and a cathode layer.

Citation Information

Patent Citations

  • Fluoride ion battery

    JP2017050113A

  • Fluoride ion all solid state battery

    JP2018092863A

  • Fluoride ion battery

    JP2018198130A

  • Positive electrode active material and fluoride ion battery

    JP2018206755A

  • Fluoride ion battery

    JP2019029206A