Anode active material, anode and lithium ion secondary battery

The use of silicon monoxide particles with a tailored particle size distribution and BET specific surface area, optionally coated with a carbon film, addresses the issue of electrolyte decomposition in silicon-based lithium ion batteries, enhancing their cycle performance.

JP7586774B2Active Publication Date: 2024-11-19SHIN ETSU CHEMICAL CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2021095807
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-08
Publication Date
2024-11-19
Estimated Expiration
2041-06-08

AI Technical Summary

Technical Problem

Lithium ion secondary batteries using silicon-based materials face challenges in achieving cycle characteristics comparable to carbon-based active materials due to insufficient suppression of electrolyte decomposition on the negative electrode surface during repeated charging and discharging, leading to poor long-term cycle performance.

Method used

A negative electrode active material composed of silicon monoxide particles with a specific particle size distribution (D0.1: 1.2μm≦D0.1≦3.0μm, D10: 3.5μm≦D10≦7.0μm, D50: 6.0μm≦D50≦15.0μm, D99.9: 25.0μm≦D99.9≦50.0μm) and a BET specific surface area (1.0m²/g≦S m ≦3.5m²/g) is used, optionally coated with a carbon film to suppress electrolyte reactions.

Benefits of technology

The specified particle size distribution and BET specific surface area significantly improve the battery's cycle characteristics by reducing electrolyte reactions, especially in long-term cycling tests, maintaining high discharge capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586774000003
    Figure 0007586774000003
  • Figure 0007586774000004
    Figure 0007586774000004
  • Figure 0007586774000005
    Figure 0007586774000005
Patent Text Reader

Abstract

To provide an anode active material capable of improving cycle characteristics when used as an anode active material for an anode electrode of a secondary battery.SOLUTION: The present invention relates to an anode active material containing monoxide silicon particles. In a volume-based distribution measured by a laser diffraction particle size distribution measurement device, a cumulative 0.1% particle diameter D0.1 of the monoxide silicon particle satisfies 1.2 μm≤D0.1≤3.0 μm, a cumulative 10% particle diameter D10 satisfies 3.5 μm≤D10≤7.0 μm, a cumulative 50% particle diameter D50 satisfies 6.0 μm≤D50≤15.0 μm and a cumulative 99.9% particle diameter D99.9 satisfies 25.0 μm≤D99.9≤50.0 μm. A BET specific surface area Sm of the monoxide silicon particle satisfies 1.0 m2 / g≤Sm≤3.5 m2 / g.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode active material, a negative electrode, and a lithium ion secondary battery. [Background technology]

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of obtaining high energy density has been promoted. The application of these secondary batteries is being considered not only for small electronic devices, but also for large electronic devices such as automobiles and power storage systems such as homes.

[0003] Among these, lithium-ion secondary batteries are becoming increasingly widespread because they can be easily made small and have a high capacity, and because they provide a higher energy density than lead batteries and nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have called for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material is being considered. This is because the theoretical capacity of silicon (4199mAh / g) is more than 10 times greater than that of graphite (372mAh / g), and a significant improvement in battery capacity can be expected. In the development of silicon materials as negative electrode active materials, not only silicon itself but also alloys and compounds such as oxides are being considered. In addition, the shape of the active material is being considered, ranging from the standard coating type for carbon-based active materials to an integrated type that is directly deposited on the current collector.

[0006] However, when silicon is used as the silicon-based material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, mainly near the surface layer of the negative electrode active material. In addition, ionic substances are generated inside the active material, making the negative electrode active material prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reaction area of ​​the active material. At this time, a decomposition reaction of the electrolyte occurs on the new surface, and a coating, which is a decomposition product of the electrolyte, is formed on the new surface, consuming the electrolyte. This makes the cycle characteristics more likely to deteriorate.

[0007] To date, various studies have been conducted on negative electrode active materials and electrode configurations for lithium ion secondary batteries that are primarily made of silicon-based materials in order to improve the initial efficiency and cycle characteristics of the battery.

[0008] Specifically, in order to obtain good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a gas phase method (see, for example, Patent Document 1). Also, in order to obtain high battery capacity and safety, a carbon material (electron conductive material) is provided on the surface layer of silicon oxide particles (see, for example, Patent Document 2). Furthermore, in order to improve cycle characteristics and obtain high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio is formed in the vicinity of the current collector (see, for example, Patent Document 3). Also, in order to improve cycle characteristics, oxygen is contained in the silicon active material, and the silicon active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is high in the vicinity of the current collector (see, for example, Patent Document 4).

[0009] In addition, in order to improve the initial charge / discharge efficiency, the Si phase, SiO2, and M y Nanocomposites containing metal oxides are used (see, for example, Patent Document 5). In addition, in order to improve cycle characteristics, SiO x(0.8 ≦ x ≦ 1.5, particle size range = 1 μm to 50 μm) is mixed with a carbon material and fired at a high temperature (see, for example, Patent Document 6). Further, in order to improve cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled within a range where the difference between the maximum value and the minimum value of the molar ratio near the interface between the active material and the current collector is 0.4 or less (see, for example, Patent Document 7). Further, in order to improve the battery load characteristics, a metal oxide containing lithium is used (see, for example, Patent Document 8). Further, in order to improve cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface layer of the silicon material (see, for example, Patent Document 9).

[0010] Also, in order to improve cycle characteristics, silicon oxide is used, and conductivity is imparted by forming a graphite film on its surface layer (see, for example, Patent Document 10). In Patent Document 10, regarding the shift value obtained from the Raman spectrum of the graphite film, broad peaks appear at 1330 cm -1 and 1580 cm -1 and the intensity ratio I 1330 / I 1580 is such that 1.5 < I 1330 / I 1580 < 3. Also, in order to improve high battery capacity and cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). Further, in order to improve overcharge and overdischarge characteristics, silicon oxide in which the atomic ratio of silicon to oxygen is controlled to 1:y (0 < y < 2) is used (see, for example, Patent Document 12).

[0011] Also, in the lithium ion secondary battery using silicon oxide, Hitachi Maxell started shipping a rectangular secondary battery for smartphones employing a nanosilicon composite in June 2010 (see, for example, Non-Patent Document 1). The silicon oxide proposed by Hohl is Si 0+ ~Si 4+It is a composite material with various oxidation states (Non-Patent Document 2). Kapaklis has also proposed a disproportionated structure in which silicon oxide is separated into Si and SiO2 by applying a thermal load to it (Non-Patent Document 3). Miyachi et al. have focused on Si and SiO2, which contribute to charging and discharging, among silicon oxides with disproportionated structures (Non-Patent Document 4).

[0012] In addition, in order to improve cycle characteristics, silicon oxide powders are used in which the particle size distribution of mode diameter, D50, and D90 are specified (for example, Patent Document 13). In the particle size distribution, D50 indicates the cumulative 50% diameter, D90 indicates the cumulative 90% diameter, and other values ​​are similar. In addition, in order to improve cycle characteristics, D90, D90 / D10, and the amount of fine powder of 1 μm or less of silicon oxide powders that have been subjected to wet classification with water after ball milling are specified (for example, Patent Document 14). In addition, in order to improve the initial discharge capacity and cycle characteristics, silicon oxide powders are used in which D50 / D10 of silicon oxide powders before carbon film formation and BET specific surface area of ​​negative electrode active material after carbon film formation are specified (for example, Patent Document 15). In addition, in order to improve cycle characteristics, the ratio of the specific surface area calculated from the particle size distribution of the negative electrode active material, assuming that the particles are spherical, to the BET specific surface area of ​​the negative electrode active material is specified for the negative electrode active material made of silicon oxide on which a carbon film is formed (e.g., Patent Document 16). In addition, the D10 and D90 of the negative electrode active material made of silicon oxide after the formation of the carbon film are specified (e.g., Patent Document 17). [Prior art documents] [Patent documents]

[0013] [Patent Document 1] JP 2001-185127 A [Patent Document 2] JP 2002-042806 A [Patent Document 3] JP 2006-164954 A [Patent Document 4] JP 2006-114454 A [Patent Document 5] JP 2009-070825 A [Patent Document 6] JP 2008-282819 A [Patent Document 7] JP 2008-251369 A [Patent Document 8] JP 2008-177346 A [Patent Document 9] JP 2007-234255 A [Patent Document 10] JP 2009-212074 A [Patent Document 11] JP 2009-205950 A [Patent Document 12] Japanese Patent Application Publication No. 06-325765 [Patent Document 13] JP 2015-149171 A [Patent Document 14] JP 2011-65934 A [Patent Document 15] International Publication No. 2012 / 077268 [Patent Document 16] International Publication No. 2014 / 002356 [Patent Document 17] JP 2013-101770 A [Non-patent literature]

[0014] [Non-Patent Document 1] Battery Association of Japan's journal "Denchi", May 1, 2010 issue, page 10 [Non-Patent Document 2] A. Hohl, T. Wieder, PA van Aken, TE Weirich, G. Denninger, M. Vidal, S. Oswald, C. Deneke, J. Mayer, and H. Fuess: J. Non-Cryst. Solids, 320, (2003 ), 255. [Non-Patent Document 3] V. Kapaklis, J. Non-Crystalline Solids, 354 (2008) 612 [Non-Patent Document 4] Mariko Miyachi, Hironori Yamamoto, and Hidemasa Kawai, J. Electrochem. Soc. 2007 volume 154, issue 4, A376-A380 Summary of the Invention [Problem to be solved by the invention]

[0015] Lithium ion secondary batteries using silicon-based materials with high charge / discharge capacity are expected to have cycle characteristics similar to those of lithium ion secondary batteries using carbon-based active materials. Among silicon-based materials, silicon oxide has the potential to obtain higher cycle characteristics, and various improvements have been made to it. However, even with the above-mentioned various techniques for controlling the particle size of the negative electrode active material, the decomposition of the electrolyte on the surface of the negative electrode active material is insufficient during repeated charging and discharging, and cycle characteristics that can withstand a practical level have not been obtained.

[0016] The reason for this is considered to be as follows. In Patent Document 14, wet classification with water is performed to obtain SiO x Using powder, D90 / D10 and the amount of fine powder of 1 μm or less are specified, but it is not possible to make a relative evaluation of the initial efficiency, cycle characteristics, and particle size distribution.

[0017] In addition, in Patent Document 15, SiO before the formation of the carbon coating (obtained by wet classification with water as in Patent Document 14) is x The powder D50 and D50 / D10, and the BET specific surface area of ​​the negative electrode active material after the carbon film formation are specified, but the examples only describe the difference in initial discharge capacity when the particle size is relatively small, D50 being 4.41 to 5.35 μm, and there is no mention of D90 or D99.9. xThere is no mention of D0.1 and BET specific surface area of ​​the powder. By specifying D0.1 for the particle diameter on the small particle diameter side, more accurate particle size distribution information of the powder can be obtained. The BET specific surface area of ​​the negative electrode active material is greatly influenced not only by the surface state of the silicon oxide particles that serve as the base material, but also by the state of the carbon coating formed on the surface of the negative electrode active material, so it is insufficient as a factor to suppress the surface reaction of the essential silicon oxide particles. Furthermore, it is described that there is no difference in cycle characteristics (10 cycles) between the embodiment in which D50 is about 5 μm and the comparative example in which D50 is 9.36 μm, but in general, in coin battery evaluation, the Li positive electrode deteriorates due to repeated charge and discharge cycles, so it is not suitable for long-term cycle tests of more than 50 cycles. Therefore, in order to evaluate the deterioration of the negative electrode due to the reaction between the electrolyte and the negative electrode active material, charge and discharge cycles of more than 100 cycles are required, and it is necessary to perform the test in a full cell using LCO (lithium cobalt oxide) or the like as the positive electrode active material for the positive electrode.

[0018] In addition, in Patent Documents 16 and 17, SiO before the formation of the carbon coating x Furthermore, in Patent Document 17, the particle size distribution and BET surface area are not mentioned, and D90 is small, at 5 μm or less.

[0019] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a negative electrode active material that can improve cycle characteristics when used as a negative electrode active material in a negative electrode of a secondary battery. [Means for solving the problem]

[0020] In order to achieve the above object, the present invention provides a negative electrode active material containing silicon monoxide particles, wherein the silicon monoxide particles satisfy the following volume-based distributions measured with a laser diffraction particle size distribution measuring device: a cumulative 0.1% particle diameter D0.1 is 1.2 μm≦D0.1≦3.0 μm, a cumulative 10% particle diameter D10 is 3.5 μm≦D10≦7.0 μm, a cumulative 50% particle diameter D50 is 6.0 μm≦D50≦15.0 μm, and a cumulative 99.9% particle diameter D99.9 is 25.0 μm≦D99.9≦50.0 μm; and the silicon monoxide particles have a BET specific surface area S mis 1.0m 2 / g≦S m ≦3.5m 2 / g.

[0021] By providing the negative electrode active material of the present invention with such particle size distribution and BET specific surface area, the reaction between the particle surfaces of the negative electrode active material and the electrolyte can be suppressed in a long-term cycle test in which charging and discharging are repeated, and the cycle characteristics of the battery can be significantly improved.

[0022] In this case, it is preferable that the cumulative 0.1% particle size D0.1 satisfies 2.0 μm≦D0.1≦3.0 μm.

[0023] It is also preferable that the cumulative 10% particle size D10 satisfies 4.8 μm≦D10≦7.0 μm.

[0024] It is also preferable that the cumulative 50% particle size D50 satisfies 8.0 μm≦D50≦15.0 μm.

[0025] According to the negative electrode active material containing silicon monoxide having such a particle size distribution, the reaction with the electrolyte on the particle surface can be more effectively suppressed, and the cycle characteristics of the battery can be significantly improved.

[0026] In the negative electrode active material of the present invention, the BET specific surface area S m But, 1.0m 2 / g≦S m ≦2.2m 2 It is preferable that the molecular weight is 1 / g.

[0027] If the material has such a BET specific surface area, the reaction area between the electrolyte and the silicon monoxide particles becomes more appropriate, and the cycle characteristics of the battery can be significantly improved.

[0028] In the negative electrode active material of the present invention, the silicon monoxide particles are preferably coated with a carbon film.

[0029] If the silicon monoxide particles are coated with such a carbon film, the surfaces of the silicon monoxide particles can be made conductive.

[0030] The present invention also provides a negative electrode comprising the above-mentioned negative electrode active material.

[0031] When such a negative electrode is incorporated into a secondary battery, reaction between the particle surface of the negative electrode active material and the electrolyte is suppressed in a long-term cycle test involving repeated charging and discharging, thereby significantly improving the cycle characteristics of the battery.

[0032] The present invention also provides a lithium ion secondary battery comprising the above-mentioned negative electrode, a positive electrode, a separator, and an electrolyte.

[0033] In such a lithium ion secondary battery, in a long-term cycle test in which charging and discharging are repeated, the reaction between the particle surface of the negative electrode active material and the electrolyte is suppressed, and the cycle characteristics of the battery can be significantly improved. Effect of the Invention

[0034] The negative electrode active material of the present invention has a specific particle size distribution and BET specific surface area, and therefore, in a long-term cycle test involving repeated charging and discharging, the reaction between the particle surfaces of the negative electrode active material and the electrolyte is suppressed, and the cycle characteristics of the battery, particularly the cycle characteristics in a long-term cycle test, can be significantly improved. [Brief description of the drawings]

[0035] [Figure 1] 1 is a graph showing the number of cycles at which 70% of the discharge capacity is maintained versus D0.1 for silicon monoxide particles. [Diagram 2] 1 is a graph showing the number of cycles at which 70% of the discharge capacity is maintained versus D10 of silicon monoxide particles. [Diagram 3] 1 is a graph showing the number of cycles at which 70% of the discharge capacity is maintained versus D50 of silicon monoxide particles. [Figure 4] 1 is a graph showing the number of cycles at which 70% of the discharge capacity is maintained versus D99.9 of silicon monoxide particles. [Diagram 5] 1 is a graph showing the number of cycles at which 70% discharge capacity is maintained versus the BET specific surface area of ​​silicon monoxide particles. [Figure 6] 1 is a graph showing the number of cycles at which 70% of the discharge capacity is maintained versus the BET specific surface area of ​​silicon monoxide particles coated with a carbon film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Considering that the deterioration of the negative electrode in long-term cycle characteristics is largely due to the decomposition of the electrolyte on the surface of silicon monoxide particles, the inventors conducted extensive research into controlling the particle size of the silicon monoxide particles that constitute the negative electrode active material. As a result, they discovered that it is possible to significantly improve the cycle characteristics while maintaining the initial charge / discharge characteristics by adjusting not only the particle size distribution of the silicon monoxide particles that serve as the base material, but also the BET specific surface area of ​​the silicon monoxide particles to an appropriate range, and thus arrived at the present invention.

[0037] Hereinafter, the present invention will be described in detail with reference to the preferred embodiments, but the present invention is not limited thereto.

[0038] <Negative electrode active material> The negative electrode active material of the present invention is a negative electrode active material containing silicon monoxide particles. Furthermore, the silicon monoxide particles satisfy the following conditions in a volume-based distribution measured by a laser diffraction particle size distribution measuring device. - Cumulative 0.1% particle size D0.1 is 1.2μm≦D0.1≦3.0μm, - Cumulative 10% particle size D10 is 3.5μm≦D10≦7.0μm, - Cumulative 50% particle size D50 is 6.0μm≦D50≦15.0μm, Cumulative 99.9% particle size D99.9 is 25.0μm≦D99.9≦50.0μm Furthermore, the silicon monoxide particles contained in the negative electrode active material of the present invention have a BET specific surface area S m is 1.0m 2 / g≦S m ≦3.5m2 / g is satisfied.

[0039] In the description of the present invention, the BET specific surface area is a value measured by the BET single point method based on the amount of N2 gas adsorption.

[0040] More preferably, the silicon monoxide particles contained in the negative electrode active material of the present invention have a BET specific surface area S m is 1.0m 2 / g≦S m ≦2.2m 2 / g.

[0041] Silicon oxide is a general term for amorphous silicon oxide, and silicon oxide before disproportionation is expressed by the general formula SiOx (0.5≦x≦1.6). This silicon oxide can be obtained, for example, by heating a mixture of silicon dioxide and metallic silicon to produce silicon monoxide gas, which is then cooled and precipitated to obtain silicon monoxide (SiO) where x is 1 or close to 1. For example, 0.9≦x≦1.1.

[0042] In order to make the silicon monoxide particles fall within the specific particle size range of the present invention, the silicon monoxide particles can be appropriately adjusted by processing such as pulverization and classification. Well-known devices can be used for pulverization. For example, a ball mill, a media stirring mill, or a roller mill, which pulverizes the material to be pulverized by moving a pulverization medium such as balls or beads and utilizing the impact force, friction force, or compression force due to the kinetic energy of the pulverization medium, a jet mill, which pulverizes the material to be pulverized by colliding the material to be pulverized with a lining material or with each other at high speed and utilizing the impact force due to the impact, a hammer mill, a pin mill, or a disk mill, which pulverize the material to be pulverized by utilizing the impact force due to the rotation of a rotor to which a hammer, blade, pin, or the like is fixed, a colloid mill, which utilizes shear force, or a high-pressure wet opposed collision type dispersing machine "Altimizer", etc., can be used. Both wet and dry pulverization can be used. Note that the particle size distribution becomes broad when pulverization is performed alone, but in order to further adjust the particle size distribution after pulverization, dry classification, wet classification, or sieving classification can be used. Dry classification mainly uses airflow, and the processes of dispersion, separation (separation of fine particles and coarse particles), collection (separation of solids and gas), and discharge are performed sequentially or simultaneously. In order to prevent the classification efficiency from being reduced due to the interference between particles, particle shape, turbulence of the airflow, velocity distribution, static electricity, etc., pretreatment (adjustment of moisture, dispersibility, humidity, etc.) is performed before classification, and the moisture and oxygen concentration of the airflow used are adjusted. In addition, in a dry type such as a cyclone that has a classifier integrated therein, pulverization and classification are performed at the same time, making it possible to obtain a desired particle size distribution. In order to obtain the particle size distribution and BET specific surface area of ​​the silicon monoxide particles of the present invention, it is effective to perform jet mill pulverization so that the BET specific surface area does not become large, and to cut off the small particle side by airflow classification using a classifier.

[0043] As described above, the silicon monoxide particles have a cumulative 0.1% diameter D0.1 of 1.2 to 3.0 μm, preferably 2.0 to 3.0 μm. The silicon monoxide particles have a cumulative 10% diameter D10 of 3.5 to 7.0 μm, preferably 4.8 to 7.0 μm. The silicon monoxide particles have a cumulative 50% diameter D50 of 6.0 to 15.0 μm, preferably 8.0 to 15.0 μm.

[0044] As described above, the cumulative 99.9% diameter D99.9 of the silicon monoxide particles is set to 25.0 to 50.0 μm. On the other hand, if D99.9 is larger than 50.0 μm, the coarse particles may expand and contract due to charging and discharging, and the conductive path may be lost in the negative electrode active material layer. Even after the electrode is produced, the coarse particles may damage the separator due to pressing or the like. Therefore, by setting D0.1 to 3.0 μm or less, D10 to 7.0 μm or less, and D50 to 15.0 μm or less as described above, D99.9 can be prevented from exceeding 50 μm.

[0045] The BET specific surface area of ​​the silicon monoxide particles contained in the negative electrode active material of the present invention is 1.0 to 3.5 m as described above. 2 / g, preferably 1.0 to 2.2m 2 / g. The BET specific surface area is 3.5m 2 By making the BET specific surface area 1.0 m or less, the reaction area between the electrolyte and the silicon monoxide particles is reduced, so that the cycle characteristics can be significantly improved when the silicon monoxide particles are used as a negative electrode active material for lithium ion secondary batteries. 2 The reason for the requirement of 1.0 m / g or more is that the BET specific surface area of ​​silicon monoxide particles satisfies the D50 requirement of 6.0 μm≦D50≦15.0 μm. 2 This is because it is industrially difficult to produce silicon monoxide particles having a particle size of less than 1 / g.

[0046] Methods for imparting electrical conductivity to the silicon monoxide particles and improving battery characteristics include mixing the silicon monoxide particles with electrically conductive particles such as graphite, coating the surface of the composite particles with a carbon film, and combining both of these methods. Among these, it is preferable to use coated particles in which the surface of the silicon monoxide particles is coated with a carbon film. As a method for coating with a carbon film, a chemical vapor deposition (CVD) method is suitable.

[0047] An example of the chemical vapor deposition (CVD) method is a method in which carbon is chemically vapor deposited on silicon monoxide particles in an organic gas and / or steam atmosphere capable of generating carbon upon thermal decomposition in a temperature range of 600 to 1,200°C to form a carbon coating.

[0048] Chemical vapor deposition (CVD) can be applied under both normal pressure and reduced pressure, and the reduced pressure can be 50 to 30,000 Pa. In addition, the apparatus used in the carbon coating formation process can be a batch furnace, a continuous furnace such as a rotary kiln or a roller hearth kiln, or a fluidized bed, which are generally known apparatuses. In particular, when the deposition apparatus is a batch furnace in which particles are left stationary, carbon can be coated more uniformly by performing the deposition under reduced pressure, and the battery characteristics can be improved.

[0049] The carbon coating formed by chemical vapor deposition can be achieved using various organic substances as carbon sources, such as those listed below. However, the pyrolysis temperature, deposition rate, and the properties of the carbon coating formed after deposition can vary greatly depending on the substance used. Substances with high deposition rates often have insufficient uniformity in the carbon coating on the surface, and on the other hand, when high temperatures are required for decomposition, silicon crystals in the silicon monoxide particles to be coated may grow too large during deposition at high temperatures, resulting in a decrease in discharge efficiency and cycle characteristics. In general, the crystallite size of silicon is determined by the Scherrer method from the half-width of the Si(111) peak in powder XRD measurement, and is preferably 50 nm or less, and more preferably 10 nm or less. The smaller the crystallite size, the more the disproportionation of silicon oxide accompanying charge and discharge is suppressed, and higher cycle characteristics can be obtained.

[0050] The Si crystallite size of the silicon monoxide particles in the negative electrode active material can be confirmed, for example, by using the following XRD apparatus. XRD: Bruker D8 ADVANCE The X-ray source is Cu Kα radiation, and a Ni filter is used. Measurements are made from 10 to 40° with an output of 40 kV / 40 mA, a slit width of 0.3°, a step width of 0.008°, and a counting time of 0.15 seconds per step.

[0051] Examples of the raw material of the organic gas that can generate carbon by pyrolysis include hydrocarbons such as methane, ethane, ethylene, acetylene, propane, butane, butene, pentane, isobutane, and hexane, aromatic hydrocarbons having one to three rings such as benzene, toluene, xylene, styrene, ethylbenzene, diphenylmethane, naphthalene, phenol, cresol, nitrobenzene, chlorobenzene, indene, coumarone, pyridine, anthracene, and phenanthrene, and gas light oil obtained in the tar distillation process, creosote oil, anthracene oil, and naphtha cracked tar oil. These can be used alone or in combination of two or more. From an economical point of view, it is preferable to use a hydrocarbon gas having a composition of CxHy.

[0052] The amount of carbon coating is preferably 1.0% by mass or more and 5.0% by mass or less based on the total amount of the carbon-coated particles. Although it depends on the particles to be coated, by setting the amount of carbon coating to 1.0% by mass or more, it is possible to generally maintain sufficient conductivity. In addition, by setting the amount of carbon coating to 5.0% by mass or less, the proportion of carbon in the negative electrode active material can be kept appropriate without being too high, and when used as a negative electrode active material for a lithium ion secondary battery, the charge / discharge capacity can be ensured.

[0053] According to the present invention, a negative electrode can be produced by using the above-mentioned negative electrode active material in which silicon monoxide particles are coated with a carbon film, and a lithium ion secondary battery can be produced.

[0054] [Negative electrode] When the negative electrode is prepared using the above-mentioned negative electrode active material, a conductive agent such as carbon or graphite can be further added. In this case, the type of conductive agent is not particularly limited, and it is sufficient if it is an electronically conductive material that does not decompose or deteriorate in the constructed battery. Specifically, metal particles or metal fibers such as Al, Ti, Fe, Ni, Cu, Zn, Ag, Sn, Si, etc., or graphite such as natural graphite, artificial graphite, various coke particles, mesophase carbon, vapor-grown carbon fiber, pitch-based carbon fiber, PAN-based carbon fiber, and various resin baked bodies can be used.

[0055] The following method is an example of a method for preparing the negative electrode. The above-mentioned negative electrode active material, if necessary, a conductive agent, other additives such as a binder such as carboxymethyl cellulose (hereinafter referred to as CMC), and a solvent such as an organic solvent or water are kneaded to form a paste-like mixture, and this mixture is applied to a sheet of a current collector. In this case, as the current collector, any material that is usually used as a current collector for a negative electrode, such as copper foil or nickel foil, can be used without any particular restrictions on thickness or surface treatment. The method for forming the mixture into a sheet is not particularly limited, and a known method can be used.

[0056] [Lithium-ion secondary battery] The lithium ion secondary battery is a lithium ion secondary battery having at least a positive electrode, a negative electrode, and a lithium ion conductive non-aqueous electrolyte, and the negative electrode is made of the negative electrode active material according to the present invention. The lithium ion secondary battery of the present invention is characterized in that it is made of a negative electrode using the negative electrode active material made of the coated particles, and other materials such as the positive electrode, electrolyte, separator, etc., and the battery shape, etc., can be known and are not particularly limited. As described above, the negative electrode active material of the present invention has good battery characteristics (charge and discharge capacity and cycle characteristics) when used as a negative electrode active material for a lithium ion secondary battery, and is particularly excellent in cycle durability.

[0057] As the positive electrode active material, oxides of transition metals such as LiCoO2, LiNiO2, LiMn2O4, V2O5, MnO2, TiS2, and MoS2, lithium, and chalcogen compounds are used.

[0058] As the electrolyte, for example, a non-aqueous solution containing a lithium salt such as lithium hexafluorophosphate or lithium perchlorate is used. As the non-aqueous solvent, one or more of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethoxyethane, γ-butyrolactone, 2-methyltetrahydrofuran, etc. are used in combination. In addition, various other non-aqueous electrolytes and solid electrolytes can also be used. EXAMPLES

[0059] The present invention will be described in more detail below by showing examples and comparative examples of the present invention, but the present invention is not limited to these examples.

[0060] [Example 1] First, a mixture of silicon dioxide and metallic silicon was heated to generate silicon monoxide gas, which was then cooled and precipitated to obtain silicon monoxide (SiOx) with x being approximately 1.0. Next, this SiOx (x=1.0) was roughly crushed using a jaw crusher (Maekawa Industries Co., Ltd.), and further pulverized for 15 minutes using a ball mill (Makino Co., Ltd.) to obtain silicon monoxide particles with a D50 of 100 μm. These particles were then finely pulverized using a jet mill (KJ800, Kurimoto Iron Works Co., Ltd.) under conditions of a compressed air pressure of 0.52 MPa and a classifier rotation speed of 4,500 rpm, and were then collected using a cyclone. When these particles were measured using a laser diffraction particle size distribution analyzer (Shimadzu SALD-3100) under the condition of a refractive index of 2.05-0.00i, the results were: D0.1 was 1.2 μm, D10 was 3.5 μm, D50 was 7.9 μm, D99.9 was 28.1 μm, and the BET specific surface area was 2.9 m 2 / g of silicon monoxide particles.

[0061] These particles were placed on a tray so that the powder layer was 10 mm thick, and then placed in a batch-type heating furnace. The pressure inside the furnace was reduced using an oil rotary vacuum pump, while the temperature inside the furnace was raised to 1,000°C at a heating rate of 200°C / hr. After reaching 1,000°C, methane was passed through the furnace at 0.3 L / min, and carbon coating treatment was carried out for 10 hours. After methane was stopped, the temperature inside the furnace was lowered and cooled, and the collected agglomerates were crushed to obtain black particles.

[0062] The obtained black particles had a D50 of 7.9 μm and a BET specific surface area of ​​2.2 m 2 The carbon coating amount relative to the black particles was 2.8 mass %, and the silicon crystallite size was 5.0 nm.

[0063] <Battery evaluation> Next, a battery using the obtained carbon-coated particles as a negative electrode active material was evaluated by the following method.

[0064] First, the negative electrode active material, graphite, conductive additive 1 (carbon nanotubes, CNT), conductive additive 2 (carbon particles with a median diameter of approximately 50 nm), sodium polyacrylate, and CMC were mixed in a dry mass ratio of 9.3:83.7:1:1:4:1, and then diluted with pure water to prepare a negative electrode mixture slurry.

[0065] This slurry was applied to a copper foil having a thickness of 15 μm and dried in a vacuum atmosphere at 100° C. for 1 hour. After drying, the deposition amount of the negative electrode active material layer per unit area on one side of the negative electrode (also called the area density) was 7.0 mg / cm 2 It was.

[0066] Next, the solvents ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed, and then an electrolyte salt (lithium hexafluorophosphate: LiPF6) was dissolved to prepare an electrolyte solution. In this case, the solvent composition was EC:DMC=30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. As additives, vinylene carbonate (VC) and fluoroethylene carbonate (FEC) were added in amounts of 1.0 mass% and 2.0 mass%, respectively.

[0067] Next, a coin battery was assembled as follows.

[0068] First, a 1 mm thick Li foil was punched out to a diameter of 16 mm and attached to an aluminum clad. The obtained electrode was punched out to a diameter of 15 mm, and placed opposite a Li counter electrode via a separator. After injecting an electrolyte, a 2032 coin battery was fabricated.

[0069] The initial efficiency was measured under the following conditions. First, the charge rate was equivalent to 0.03C. Charging was performed in CCCV mode. CV was 0V and the final current was 0.04mA. The discharge rate was also 0.03C, the discharge voltage was 1.2V, and CC discharge was performed.

[0070] When investigating the initial charge / discharge characteristics, the initial efficiency (hereinafter sometimes referred to as initial efficiency) was calculated using the formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) x 100.

[0071] Based on the initial data obtained, a counter cathode was designed and a battery was evaluated. Lithium cobalt oxide (LCO) was used as the cathode active material.

[0072] The cycle characteristics were investigated as follows. First, to stabilize the battery, two cycles of charge and discharge were performed at 0.2C in an atmosphere of 25°C, and the discharge capacity of the second cycle was measured. The battery cycle characteristics were calculated from the discharge capacity of the third cycle, and the battery test was stopped when the discharge capacity retention rate reached 70%. Charge and discharge were performed at 0.7C and 0.5C. The charge voltage was 4.3V, the discharge cut-off voltage was 2.5V, and the charge cut-off rate was 0.07C.

[0073] [Examples 2 to 10] The same SiOx (x=1.0) as in Example 1 was similarly ball milled to have a D50 of 100 μm. In the subsequent jet mill process, the classifier rotation speed, grinding pressure, and atmosphere were controlled to produce silicon monoxide particles having the powder properties shown in Table 1. In the same manner as in Example 1, silicon monoxide particles were coated with a carbon film to produce conductive particles, and the obtained conductive particles were used to produce a negative electrode, which was then subjected to battery evaluation.

[0074] [Comparative Example 1] The same SiOx (x=1.0) as in Example 1 was similarly milled to 100 μm using a ball mill. In the next jet mill process, the particles were finely pulverized under conditions of a compressed air pressure of 0.52 MPa and a rotation speed of 5000 rpm in the classifier, and then collected in a cyclone. The particles collected in the cyclone had a D0.1 of 1.8 μm, a D10 of 4.5 μm, a D50 of 6.6 μm, a D99.9 of 18.9 μm, and a BET specific surface area of ​​3.3 m 2 The silicon monoxide particles had a carbon film coating thereon in the same manner as in Example 1 to prepare conductive particles, and the obtained conductive particles were used to prepare a negative electrode, which was then subjected to battery evaluation.

[0075] [Comparative Example 2] The same SiOx (x=1.0) as in Example 1 was used and pulverized in a ball mill for 30 minutes to a D50 of 20 μm. In the subsequent jet mill process, the particles were finely pulverized under conditions of a compressed air pressure of 0.45 MPa and a rotation speed of 5500 rpm in the classifier and collected in a cyclone. The particles collected in the cyclone had a D0.1 of 0.4 μm, a D10 of 2.5 μm, a D50 of 5.8 μm, a D99.9 of 18.5 μm, and a BET specific surface area of ​​3.7 m 2 The silicon monoxide particles thus obtained were coated with a carbon film, and the D50 was 6.1 μm and the BET specific surface area was 3.2 m. 2 Conductive particles having a carbon coating amount of 3.5 mass % relative to the black particles were obtained. Using the obtained conductive particles, a negative electrode was produced in the same manner as in Example 1, and a battery evaluation was performed.

[0076] [Comparative Example 3] Conductive particles were produced in the same manner as in Example 1, except that the silicon monoxide particles obtained in Comparative Example 2 were used and the methane aeration time was changed to 7 hours. 2 The conductive particles had a carbon coating amount of 2.7 mass % relative to the black particles and a carbon coating amount of 2.7 mass % relative to the black particles. Using the conductive particles obtained, a negative electrode was produced in the same manner as in Example 1, and a battery evaluation was performed.

[0077] [Comparative Example 4] The ball mill powder with a D50 of 100 μm obtained in Example 1 was finely pulverized in a jet mill under conditions of a classifier compressed air pressure of 0.40 MPa and a rotation speed of 2200 rpm, and then collected in a cyclone. The particles collected in the cyclone had a D0.1 of 3.5 μm, a D10 of 7.2 μm, a D50 of 18.9 μm, a D99.9 of 53.4 μm, and a BET specific surface area of ​​1.3 m 2 The silicon monoxide particles thus obtained were coated with a carbon film, and the D50 was 19.0 μm and the BET specific surface area was 1.2 m. 2 Conductive particles having a carbon coating amount of 2.0 mass % relative to the black particles were obtained. Using the obtained conductive particles, a negative electrode was produced in the same manner as in Example 1, and a battery evaluation was performed.

[0078] [Comparative Example 5] The same SiOx (x = 1.0) as in Example 1 was used and ground in a ball mill for 1 hour. The silicon monoxide particles had a D0.1 of 0.3 μm, a D10 of 1.5 μm, a D50 of 9.1 μm, a D99.9 of 57.0 μm, and a BET specific surface area of ​​2.8 m 2 The carbon film was coated in the same manner as in Example 1 without performing fine pulverization and classification using a jet mill, and the D50 was 9.3 μm and the BET specific surface area was 2.5 m 2 The conductive particles had a carbon coating amount of 3.1 mass % relative to the black particles and a carbon coating amount of 3.1 mass % relative to the black particles. Using the conductive particles obtained, a negative electrode was produced in the same manner as in Example 1, and a battery evaluation was performed.

[0079] The conditions of the examples and comparative examples are shown in Table 1. The powder properties and battery characteristics are shown in Table 2. FIG. 1 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for silicon monoxide particles D0.1 in a state where the silicon monoxide particles are not coated with carbon, FIG. 2 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for silicon monoxide particles D10 in a state where the silicon monoxide particles are not coated with carbon, FIG. 3 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for silicon monoxide particles D50 in a state where the silicon monoxide particles are not coated with carbon, FIG. 4 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for silicon monoxide particles D99.9 in a state where the silicon monoxide particles are not coated with carbon, FIG. 5 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for the BET specific surface area of ​​the silicon monoxide particles in a state where the silicon monoxide particles are not coated with carbon, and FIG. 6 shows the number of cycles at which the discharge capacity of the negative electrode active material in a carbon-coated state is maintained at 70% for the BET specific surface area of ​​the negative electrode active material in a state where the carbon is coated.

[0080] From FIG. 1, it can be seen that the number of cycles is 800 or more when the cumulative 0.1% particle diameter D0.1 of the silicon monoxide particles is in the range of 1.2 μm≦D0.1≦3.0 μm. Also, from FIG. 2, it can be seen that the number of cycles is 800 or more when the cumulative 10% particle diameter D10 of the silicon monoxide particles is in the range of 3.5 μm≦D10≦7.0 μm. Also, from FIG. 3, it can be seen that the number of cycles is 800 or more when the cumulative 50% particle diameter D50 of the silicon monoxide particles is in the range of 6.0 μm≦D50≦15.0 μm. Also, from FIG. 4, it can be seen that the number of cycles is 800 or more when the cumulative 99.9% particle diameter D99.9 of the silicon monoxide particles is in the range of 25.0 μm≦D99.9≦50.0 μm. Also, from FIG. 5, it can be seen that the BET specific surface area S m is 1.0m 2 / g≦S m ≦3.5m 2 It can be seen that in the range of 0.1 μm / g, the number of cycles is 800 or more.

[0081] [Table 1]

[0082] [Table 2]

[0083] It was confirmed that the lithium ion secondary batteries of Examples 1 to 10 had significantly improved cycle characteristics while maintaining the initial charge / discharge characteristics, compared to Comparative Examples 1 to 5. In Comparative Examples 1 to 3, the particle size distribution of the silicon monoxide particles did not satisfy the optimal conditions, and the BET specific surface area was high, so that cycle characteristics comparable to those of the Examples were not obtained. In Comparative Examples 4 and 5, it was confirmed that the cycle characteristics were reduced due to the negative electrode active material made of silicon monoxide particles having a particle size distribution in which D99.9 exceeds 50 μm. It is presumed that the coarse particles expanded and contracted due to charge and discharge, causing the conductive path to be lost.

[0084] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention.

Claims

1. A negative electrode active material for a secondary battery containing silicon monoxide particles and using an electrolyte solution, The silicon monoxide particles have a volume-based distribution measured by a laser diffraction particle size distribution measuring device, The cumulative 0.1% particle size D0.1 is 1.2 μm≦D0.1≦3.0 μm, The cumulative 10% particle size D10 is 3.5 μm≦D10≦7.0 μm, The cumulative 50% particle diameter D50 is 6.0 μm≦D50≦15.0 μm, Cumulative 99.9% particle size D99.9 is 25.0 μm≦D99.9≦50.0 μm Fulfilling The silicon monoxide particles have a BET specific surface area S m is 1.0m 2 / g≦S m ≦3.5m 2 / g.

2. 2. The negative electrode active material according to claim 1, wherein the cumulative 0.1% particle size D0.1 satisfies 2.0 μm≦D0.1≦3.0 μm.

3. 3. The negative electrode active material according to claim 1, wherein the cumulative 10% particle diameter D10 satisfies 4.8 μm≦D10≦7.0 μm.

4. 4. The negative electrode active material according to claim 1, wherein the cumulative 50% particle diameter D50 satisfies 8.0 μm≦D50≦15.0 μm.

5. The BET specific surface area S m But, 1.0m 2 / g≦S m ≦2.2m 2 The negative electrode active material according to claim 1 , wherein the molecular weight of the negative electrode active material is 1 / g.

6. 6. The negative electrode active material according to claim 1, wherein the silicon monoxide particles are coated with a carbon film.

7. A negative electrode comprising the negative electrode active material according to claim 1 .

8. A lithium ion secondary battery comprising the negative electrode according to claim 7, a positive electrode, a separator, and the electrolyte.

Citation Information

Patent Citations

  • Nanosheet-shaped silicon oxide and composite negative electrode material thereof

    CN111969196A

  • Nonaqueous electrolytic secondary battery and its manufacture

    JP1994325765A

  • Lithium secondary battery

    JP2001185127A

  • Non-aqueous electrolyte secondary battery

    JP2002042806A

  • Battery

    JP2006114454A