Method and device for manufacturing peeling container
A two-step injection molding method forms a multilayer preform with altered resin flow and temperature to create a high-strength, less noticeable contraction-inducing structure, enhancing both appearance and functionality in transparent containers.
Patent Information
- Application Number
- JP2022566934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-01
- Filing Date
- 2021-11-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Existing container manufacturing methods result in structural portions for inducing contraction being noticeable, affecting the appearance of transparent containers.
A manufacturing method involving two-step injection molding to create a multilayer preform with a first recess in the outer layer and a second recess in the inner layer, using protrusions to alter resin flow and temperature, forming a high-strength region in the inner layer that is less noticeable.
The method allows for the formation of a contraction-inducing structure that is inconspicuous, maintaining the aesthetic appearance while ensuring regular and appropriate deformation during content discharge.
Smart Images

Figure 0007586927000001 
Figure 0007586927000002 
Figure 0007586927000003
Abstract
Description
[Technical field]
[0001] The present invention relates to Peeling container The present invention relates to a manufacturing method and a manufacturing apparatus for the same. [Background technology]
[0002] Conventionally, resin containers that shrink as the contents are discharged, such as the inner layer of a peelable container having a two-layer structure or a bag-in-box (BIB) container inserted into an outer box such as a cardboard box, have been manufactured by blow molding.
[0003] This type of container is known to have a structure in which the strength of the container body is varied regularly in the circumferential direction to induce appropriate and regular shrinkage deformation accompanying the discharge of the contents. The above structure can be manufactured, for example, by blow molding a preform in which the wall thickness distribution and temperature distribution are varied regularly in the circumferential direction as in Patent Documents 1 and 2, or by blow molding using a mold having irregularities in the body for inducing shrinkage as in Patent Document 3. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-142186 A [Patent Document 2] Patent No. 3255485 [Patent Document 3] Patent No. 4588200 Summary of the Invention [Problem to be solved by the invention]
[0005] When a shrinkage-inducing structure is formed in a container using the above-mentioned method, the shrinkage-inducing structural part is easily noticeable. For example, if the entire container is transparent, the noticeable shrinkage-inducing structural part affects the aesthetic appearance of the container.
[0006] The present invention has been made in view of such problems, and provides a method for forming a shrinkage-inducing structure in a container that is less noticeable. Peeling container The object of the present invention is to provide a method for producing the above-mentioned. [Means for solving the problem]
[0007] It is one aspect of the present invention. Peeling container The manufacturing method of A first injection molding process is performed by using a first injection mold to injection mold an outer layer of a bottomed cylindrical preform with a first resin material. A second injection molding process is performed by using a second injection mold to inject a second resin material different from the first resin material onto the inner periphery of the outer layer to produce a multi-layer preform in which an inner layer is laminated inside the outer layer. The preform is blow molded while retaining the heat from the injection molding process. The inner layer shrinks as the filling material in the inner layer is discharged. A blow molding process for manufacturing a container. In the first injection molding step, a first recess is formed in at least a part of the outer layer by a first protrusion provided on the first injection mold. In the second injection molding step, a second recess is formed in the preform by inserting a second protrusion provided on the second injection mold into the first recess, penetrating the outer layer and exposing the surface of the inner layer. At least one of the flow rate and temperature of the second resin material that has passed through the second protrusion is changed by contact between the second protrusion and the second resin material, and a region having a higher strength than other parts in the circumferential direction is formed in the inner layer starting from the position corresponding to the second recess. Effect of the Invention
[0008] According to one aspect of the present invention, the contraction-inducing structural portion of the container can be formed so as to be less noticeable. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2(a) is a vertical cross-sectional view of the preform of this embodiment, and FIG. 2(b) is a bottom view of the preform. [Diagram 2] FIG. 2A is a front view of the peeling container of this embodiment, and FIG. 2B is a bottom view of the peeling container of this embodiment. [Diagram 3] FIG. 2 is a vertical cross-sectional view of the peeling container of the present embodiment. [Figure 4] FIG. 2 is a cross-sectional view showing the vicinity of the bottom surface of an example of a peeling container in a state in which the inner layer has contracted. [Diagram 5] 1 is a diagram showing a schematic configuration of a blow molding device according to an embodiment of the present invention; [Figure 6] 3A to 3C are diagrams illustrating a manufacturing process of the preform according to the present embodiment. [Figure 7] FIG. 2 is a diagram showing the vicinity of the bottom of the first layer in the first injection molding part. [Figure 8] FIG. 13 is a diagram showing the vicinity of the bottom of the preform in the second injection molding section. [Figure 9] 1 is a flowchart showing steps of a method for manufacturing a peeled container. [Figure 10] 13 is a diagram showing the vicinity of the bottom of an injection molded part in a modified example of the present embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In this embodiment, a peeling container will be described as an example of a resin container (hereinafter, simply referred to as a container) that can shrink in response to the discharge of the content.
[0011] In the embodiments, in order to make the description easier to understand, structures and elements other than the main parts of the present invention will be described in a simplified or omitted manner. In addition, in the drawings, the same elements are given the same reference numerals. Note that the shapes, dimensions, etc. of each element shown in the drawings are shown only for illustrative purposes, and do not represent the actual shapes, dimensions, etc.
[0012] <Example of preform composition> First, a configuration example of a preform for a peeling container according to this embodiment will be described with reference to Fig. 1. Fig. 1(a) is a vertical cross-sectional view of a preform 10 of this embodiment, and Fig. 1(b) is a bottom view of the preform 10.
[0013] The overall shape of the preform 10 is a cylindrical shape with one end open and the other end closed. The preform 10 includes a cylindrical body 14, a bottom 15 closing the other end of the body 14, and a neck 13 formed at the opening on one end side of the body 14.
[0014] The preform 10 has a two-layer structure in which a second layer (inner layer) 12 is laminated on the inside of a first layer (outer layer) 11. The first layer 11 and the second layer 12 are formed from different thermoplastic resin materials by two-stage injection molding as described below. As an example, the first layer 11 is made of a synthetic resin having excellent moldability and transparency. On the other hand, the second layer 12 is made of a synthetic resin having properties (e.g., moisture barrier properties, gas barrier properties, heat resistance, chemical resistance) that can stably store the contents of the container and suppress deterioration (oxidation). In addition, a resin material having a higher melting point than that of the second layer 12 is selected for the first layer 11.
[0015] The resin material of the first layer 11 does not have to satisfy the above relationship as long as it has a higher melting point than the resin material of the second layer 12. For example, the resin material of the first layer 11 may be a resin material having higher moisture barrier property, gas barrier property, heat resistance, or chemical resistance than the resin material of the second layer 12.
[0016] Hereinafter, the resin material of the first layer 11 will also be referred to as a first resin material, and the resin material of the second layer 12 will also be referred to as a second resin material. The combination of the first resin material and the second resin material can be appropriately selected according to the specifications of the peeling container.Specific types of materials include, for example, PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PCTA (polycyclohexane dimethylene terephthalate), Tritan (Tritan (registered trademark): copolyester manufactured by Eastman Chemical Co.), PP (polypropylene), PE (polyethylene), PC (polycarbonate), PES (polyethersulfone), PPSU (polyphenylsulfone), PS (polystyrene), COP / COC (cyclic olefin polymer), PMMA (polymethyl methacrylate: acrylic), and PLA (polylactic acid).
[0017] As an example, the first resin material is PET (polyethylene terephthalate), and the second resin material is PP (polypropylene). The melting point of PP is about 160 to 170°C, and the melting point of PET is higher than that of PP, about 245 to 260°C.
[0018] In addition, in the body 14 of the preform 10, the ratio (t1 / t2) of the thickness t1 of the first layer 11 to the thickness t2 of the second layer 12 is preferably 1.5 or more. From the viewpoint of ensuring the transparency of the peelable container to be molded, the thickness ratio is preferably 3.0 or less.
[0019] In the bottom 15 of the preform 10, an opening 16 is formed at the center of the bottom of the first layer 11, penetrating the first layer 11. The opening 16 of the first layer 11 is blocked from the inside by the second layer 12.
[0020] In addition, a plurality of recesses 17 for forming air introduction holes in the peeling container are formed in the bottom 15 of the preform 10 in a radial arrangement based on the center of the bottom. The recesses 17 are substantially circular and formed at intervals in the radial direction from the opening 16. For example, two or more recesses 17, preferably four recesses 17, are formed so as to be rotationally symmetrical based on the center of the bottom 15 of the preform 10. In this embodiment, an example in which four recesses 17 are formed is shown.
[0021] The depth of the recess 17 in the thickness direction of the preform 10 is set to a dimension such that the recess 17 penetrates at least the first layer 11 and the surface of the second layer 12 is exposed in the recess 17. The recess 17 formed in the two-layered preform 10 is an example of a second recess.
[0022] In addition, the second layer 12 is formed with a plurality of stripe-like first regions 19 extending radially outward from the recesses 17 as starting points. Two or more, preferably four, first regions 19 are formed in the circumferential direction so as to be rotationally symmetrical with respect to the center of the bottom 15 of the preform 10. The first regions 19 have different physical properties such as resin density and / or resin orientation compared to other regions (also referred to as second regions) in the circumferential direction of the preform 10, and have the property of being less likely to deform in the circumferential direction or in the inner diameter direction. For example, the resin density in the first regions 19 is higher than that in the second regions. In addition, in the first regions 19, the resin orientation has directionality in the longitudinal direction from the bottom 15 to the neck 13, whereas in the second regions, the resin orientation varies in a direction intersecting the longitudinal direction compared to the first regions 19. Although the first region 19 in the second layer 12 is difficult to distinguish from the second region visually, it can be distinguished by a method such as strain measurement using a photoelastic method.
[0023] <Example of peeling container configuration> Next, a configuration example of a resin peeling container 20 according to this embodiment will be described with reference to Figs. 2, 3, and 4. Figs. 2(a) and 2(b) are a front view and a bottom view of the peeling container 20 according to this embodiment. Fig. 3 is a vertical cross-sectional view of the peeling container 20 according to this embodiment. Fig. 4 is a horizontal cross-sectional view near the bottom showing an example of the peeling container 20 in a state where the inner layer is shrunk.
[0024] The peelable container 20 is a bottle-shaped resin container obtained by stretch-blow molding the preform 10, and contains, for example, seasoning liquid such as soy sauce. The peelable container 20 may also be used to contain other contents such as cosmetic liquid.
[0025] 3, the peeling container 20 has a two-layer structure in which a bag-shaped second layer 12 is laminated inside a first layer 11, similar to the preform 10. In the body portion 22 of the peeling container 20, the ratio (t11 / t12) of the thickness t11 of the first layer 11 to the thickness t12 of the second layer 12 is approximately the same as the thickness ratio (t1 / t2) in the body portion 14 of the preform 10.
[0026] As shown in Fig. 2(a), the peeling container 20 has a neck 21 having an opening at the top, a cylindrical body 22 continuing from the neck 21, and a bottom 23 continuing from the body 22. The body 22 may have a shape including a shoulder 22a having one end connected to the neck 21 and expanding radially toward the other end, a body 22c having the other end connected to the bottom 23, and a constricted portion 22b connected to the other end of the shoulder 22a and one end of the body 22c, and connecting the shoulder 22a and the body 22c. The cross section of the peeling container 20 is substantially circular at any position in the axial direction.
[0027] In manufacturing the peeling container 20, the body 14 and bottom 15 of the preform 10 are expanded by stretch blowing, and are shaped into the body 22 and bottom 23 of the peeling container 20. During the stretch blowing, the recess 17 of the preform 10 is stretched, and as shown in FIG. 2(b), four air introduction holes 24 penetrating the first layer 11 are formed in the bottom 23 of the peeling container 20.
[0028] In addition, in the bottom 23 of the peeling container 20, an opening 25 penetrating the first layer 11 is formed in the center of the bottom of the first layer 11, similar to the preform 10. The opening 25 is filled with the material of the second layer 12, closing the opening 25, and the second layer 12 is exposed to the outside of the first layer 11 in the vicinity of the opening 25 of the bottom 23 of the peeling container 20. By exposing the second layer 12 to the outside of the first layer 11 at the opening 25 of the peeling container 20, the second layer 12 is partially fixed to the first layer 11, and positional deviation of the second layer 12 relative to the first layer 11 is suppressed.
[0029] Furthermore, in the second layer 12 of the peeling container 20, streaky high strength portions 26 are formed by stretching the first region 19 of the preform 10. The high strength portions 26 extend radially outward from the positions of the air inlet holes 24, and four high strength portions 26 are formed in the circumferential direction so as to be rotationally symmetrical with respect to the opening 25 of the bottom portion 23.
[0030] Similar to the preform 10, the high-strength portion 26 of the peeling container 20 has physical properties such as resin density and / or resin orientation different from other regions (also referred to as easily deformable portions 27) in the circumferential direction of the second layer 12, and has the property of being less likely to deform in the circumferential direction. Note that the high-strength portion 26 is difficult to distinguish from the easily deformable portion 27 by visual inspection, but can be distinguished by a method such as strain measurement using a photoelastic method.
[0031] In the peeling container 20, the contents are filled in the space inside the second layer 12. In the peeling container 20, when the contents are discharged from the second layer 12, air gradually flows between the first layer 11 and the second layer 12 from the air introduction hole 24, and the first layer 11 and the second layer 12 are peeled off. This allows the volume occupied by the contents in the container to be replaced with air without exposing the contents of the second layer 12 to air, and allows the contents filled in the second layer 12 to be discharged outside the container.
[0032] In the peelable container 20, as the contents filled in the second layer 12 are discharged, the second layer 12 shrinks inward. Since the high-strength portions 26 of the second layer 12 are less likely to deform in the circumferential direction than the easily deformed portions 27, as shown in Fig. 4, when the second layer 12 shrinks, the easily deformed portions 27 shrink inward before the high-strength portions 26. As a result, the easily deformed portions 27 are folded so as to be in close contact with the high-strength portions 26 extending in the radial direction, and the high-strength portions 26 guide the shrinkage deformation of the second layer 12 to be appropriate and regular.
[0033] In addition, when the second layer 12 shrinks due to the drainage of liquid from the container, the upper, easily deformable portion 27 close to the neck is deformed first, and the bottom side of the second layer 12 is likely to be stuck to the bottom of the first layer 11 due to the weight of the contents. As the second layer 12 shrinks, the bottom of the second layer 12 is folded at the ridge line 28 connecting the end of the striated high strength portion 26 or the center of the bottom and a part of the extension line of the air introduction hole 24 as a corner, as shown in FIG. 4. As a result, the bottom of the second layer 12 is deformed so as to approach a polygonal shape from a circular shape. For example, in the case of four air introduction holes 24 as shown in FIG. 4, the bottom shape of the second layer 12 becomes rectangular. In this way, in the second layer 12, the ridge line 28 on the bottom side and the striated high strength portion 26 are folded at the ridge line 28 connecting these corners.26 When the second layer 12 is shrunk to a columnar (beam-like) shape, the other portions become easier to fold. In the contraction caused by the drainage of liquid from the container, the easily deformable portion 27 on the lower side or body side close to the bottom of the second layer 12 may deform first due to the air being supplied from the air inlet hole 24. In addition, at least the easily deformable portion 27 on the bottom side of the second layer 12 may peel off from the bottom of the first layer 11 in the early stage of the contraction caused by the drainage of liquid.
[0034] <Description of the peeling container manufacturing equipment> 5 is a diagram showing a schematic configuration of the blow molding apparatus 30 of this embodiment. The blow molding apparatus 30 of this embodiment is an example of an apparatus for manufacturing the peelable container 20, and employs a hot parison method (also called a one-stage method) in which the preform 10 is not cooled to room temperature, but the heat (internal heat) retained during injection molding is utilized to blow mold the peelable container 20.
[0035] The blow molding device 30 includes a first injection molding section 31, a second injection molding section 32, a temperature adjustment section 33, a blow molding section 34, a take-out section 35, and a conveying mechanism 36. The first injection molding section 31, the second injection molding section 32, the temperature adjustment section 33, the blow molding section 34, and the take-out section 35 are arranged at positions rotated by a predetermined angle (for example, 72 degrees) around the conveying mechanism 36. Note that a temperature adjustment section may be further added between the first injection molding section 31 and the second injection molding section 32 to supplementarily heat or cool the first layer 11 of the preform 10. In addition, a core mold lifting mechanism (not shown) is provided above the conveying mechanism 36 in the first injection molding section 31 and the second injection molding section 32.
[0036] (Transport mechanism 36) The transport mechanism 36 includes a transport plate (not shown) that moves so as to rotate around an axis perpendicular to the plane of the drawing in FIG. 5. At least one neck mold 36a (not shown in FIG. 5) that holds the neck 13 of the preform 10 (or the neck 21 of the peeling container 20) is arranged at each predetermined angle on the transport plate. The transport mechanism 36 transports the preform 10 (or the peeling container 20) held by the neck mold 36a to the first injection molding section 31, the second injection molding section 32, the temperature adjustment section 33, the blow molding section 34, and the removal section 35 in that order by moving the transport plate by a predetermined angle at a time. The transport mechanism 36 can also raise and lower the transport plate, and also performs operations related to mold closing and mold opening (mold release) in the first injection molding section 31 and the second injection molding section 32.
[0037] (First injection molding section 31) The first injection molding section 31 includes a cavity mold 40, a core mold 41, and a hot runner mold 42, and manufactures the first layer 11 of the preform 10. The cavity mold 40 is composed of a first cavity mold 40A on the opening side (upper side) and a second cavity mold 40B on the bottom side (lower side). A first injection device 37 that supplies a first resin material to the hot runner mold 42 is connected to the first injection molding section 31. The cavity mold 40 and the hot runner mold 42 are fixed to the machine base of the blow molding device 30 in an integrated state. The core mold 41 is fixed to a core mold lifting mechanism.
[0038] 6(a) and (b) show a first injection molding section 31 for molding the first layer 11 of the preform 10 of this embodiment. Fig. 7 is a diagram showing the vicinity of the bottom of the first layer 11 in the first injection molding section 31.
[0039] The cavity mold 40 defines the shape of the outer periphery of the first layer 11. The first cavity mold 40A is a mold facing the opening side of the cavity mold 40 and defines the shape of the outer periphery of the body of the first layer 11. The second cavity mold 40B is a mold facing the bottom side of the cavity mold 40 and defines the shape of the outer periphery of the bottom of the first layer 11. The hot runner mold 42 has a resin supply section 42a that introduces the first resin material from the first injection device 37. The core mold 41 is a mold that defines the shape of the inner periphery of the first layer 11 and is inserted from above into the inner periphery of the cavity mold 40. The first cavity mold 40A and the second cavity mold 40B may be integrally formed.
[0040] 6(a) and (b), in the first injection molding section 31, the cavity mold 40, the core mold 41, and the neck mold 36a of the transport mechanism 36 are closed to form a mold space for the first layer 11. Then, the first resin material is poured from the bottom of the mold space through the hot runner mold 42, whereby the first layer 11 of the preform 10 is manufactured in the first injection molding section 31.
[0041] A plurality of first protrusions 44 in the form of ribs are provided in a radial arrangement on the upper surface side of the second cavity mold 40B facing the outer periphery of the bottom of the first layer 11. The first protrusions 44 are arranged at intervals in the radial direction from the center of the bottom where the resin supply unit 42a is located, and two or more, preferably four, are formed so as to be rotationally symmetrical with respect to the center of the bottom. As shown in FIG. 7(a), the protrusion amount h1 of the first protrusions 44 from the outer periphery of the bottom of the first layer 11 is approximately the same dimension as the thickness of the first layer 11. Therefore, when the first injection molding unit 31 is closed, the tip of the first protrusion 44 faces the surface of the core mold 41. As a result, during the injection molding of the first injection molding unit 31, the first protrusions 44 form a circular recess 11a in the first layer 11 at a position corresponding to the recess 17 of the preform 10. The recess 11a of the first layer 11 may penetrate the first layer 11, or may have a thin film formed between the core mold 41 and the first protrusion 44. The recess 11a of the first layer 11 formed by the first injection molding unit 31 is also referred to as a first recess.
[0042] 6(b), a resin supply section 42a of the hot runner mold 42 is provided with a valve pin 43 that is axially movable to a position close to the core mold 41. The valve pin 43 is housed inside the hot runner mold 42 until the mold space is filled with the first resin material, and protrudes to a position close to the core mold 41 after the mold space is filled with the first resin material. By such movement of the valve pin 43 during injection molding, a thin film portion 18 in which the resin material is thinner than the peripheral portion can be formed in the center of the bottom of the first layer 11.
[0043] Furthermore, even when the first injection molding section 31 is opened, the neck mold 36a of the transport mechanism 36 is not opened, but continues to hold and transport the first layer 11 of the preform 10. The number of preforms 10 simultaneously molded in the first injection molding section 31 (i.e., the number of peeling containers 20 that can be simultaneously molded by the blow molding device 30) can be set appropriately.
[0044] (Second injection molding section 32) The second injection molding section 32 includes a cavity mold 50, a core mold 51, and a hot runner mold 52, and injection molds the second layer 12 on the inner periphery side of the first layer 11. The cavity mold 50 is composed of a first cavity mold 50A on the opening side (upper side) and a second cavity mold 50B on the bottom side (lower side). A second injection device 38 that supplies a second resin material to the hot runner mold 52 is connected to the second injection molding section 32. The first cavity mold 50A and the second cavity mold 50B may be integrally formed.
[0045] Fig. 6(c) shows the second injection molding section 32 for molding the second layer 12 of the preform 10. Figs. 8(a) and 8(b) are diagrams showing the vicinity of the bottom of the preform 10 in the second injection molding section 32.
[0046] The cavity mold 50 is a mold that houses the first layer 11. The first cavity mold 50A is a mold facing the opening side of the cavity mold 50 and houses the body part of the first layer 11. The second cavity mold 50B is a mold facing the bottom side of the cavity mold 50 and houses the bottom part of the first layer 11. The hot runner mold 52 has a resin supply part 52a that introduces the second resin material from the second injection device 38. The core mold 51 is a mold that determines the shape of the inner circumference side of the second layer 12 and is inserted from above into the inner circumference side of the cavity mold 50.
[0047] As shown in Fig. 6(c), the second injection molding section 32 accommodates the first layer 11 of the preform 10 injection molded in the first injection molding section 31. When the second injection molding section 32 is in a closed state, a mold space is formed between the inner periphery of the first layer 11 and the surface of the core mold 51. In the second injection molding section 32, a second resin material is poured from the bottom of the mold space through a hot runner mold 52, thereby forming a preform 10 in which the second layer 12 is laminated on the inner periphery of the first layer 11.
[0048] Furthermore, on the upper surface side of the second cavity mold 50B facing the outer periphery of the bottom of the first layer 11, a circular second protrusion 54 corresponding to the shape of the recess 17 of the preform 10 is provided at a predetermined position corresponding to the first protrusion 44 of the first injection molding section 31. The second protrusion 54 is inserted into the recess 11a of the first layer 11 when the first layer 11 is accommodated in the second injection molding section 32.
[0049] Here, Fig. 8(a) shows a vertical cross section at the position of the second protrusion 54 in the circumferential direction, and Fig. 8(b) shows a vertical cross section at a position where there is no second protrusion in the circumferential direction.
[0050] As shown in FIG. 8(a), the projection amount h2 of the second projection 54 from the bottom outer peripheral surface of the first layer 11 is a dimension larger than the thickness of the first layer 11. In other words, the projection amount h2 of the second projection 54 is larger than the projection amount h1 of the first projection 44 (h2>h1). Therefore, when the second injection molding section 32 is closed, the tip of the second projection 54 penetrates the recess 11a of the first layer 11 and projects to the inner peripheral side of the first layer 11. By providing the second projection 54 on the second cavity mold 50B of the second injection molding section 32, the recess 17 can be formed in the bottom 15 of the preform 10. Although not particularly limited, it is preferable that the difference between the protrusion amount h1 of the first protrusion portion 44 and the protrusion amount h2 of the second protrusion portion 54 (the protrusion amount of the second protrusion portion 54 from the first layer) be less than 1 / 4 to 1 / 5 of the bottom thickness of the preform 10.
[0051] The protrusion amount h2 of the second protrusion 54 is set to be smaller than the thickness of the preform 10. That is, in the injection molding in the second injection molding section 32, the second resin material flows between the core mold 51 and the second protrusion 54, so that the second protrusion 54 does not form a hole penetrating the second layer 12.
[0052] In the second injection molding section 32, the second resin material is filled between the first layer 11 and the core mold 51, but at the position of the second protrusion 54 shown in Fig. 8(a), the second resin material also comes into contact with the second protrusion 54 that penetrates the recess 11a of the first layer 11. Also, in the second injection molding section 32, the distance L1 between the second protrusion 54 and the surface of the core mold 51 shown in Fig. 8(a) is smaller than the distance L2 between the inner circumferential surface of the first layer 11 and the surface of the core mold 51 shown in Fig. 8(b).
[0053] (Temperature adjustment section 33) The temperature adjustment section 33 includes a mold unit (temperature adjustment pot and temperature adjustment core) for temperature adjustment (not shown). The temperature adjustment section 33 accommodates the preforms 10 transferred from the second injection molding section 32 in a mold unit maintained at a predetermined temperature, thereby equalizing the temperature and removing temperature deviation, and adjusts the temperature of the preforms 10 to a temperature suitable for the final blow (for example, about 90°C to 105°C). The temperature adjustment section 33 also has the function of cooling the preforms 10 in a high temperature state after injection molding.
[0054] (Blow molding section 34) The blow molding section 34 performs blow molding on the preform 10 whose temperature has been adjusted in the temperature adjustment section 33 , and produces the peeled container 20 . The blow molding section 34 includes a blow cavity mold, which is a pair of split molds corresponding to the shape of the peeling container 20, a bottom mold, a stretching rod, and an air introduction member (none of which are shown). The blow molding section 34 blow molds the preform 10 while stretching it. This allows the preform 10 to be shaped into the shape of the blow cavity mold, thereby manufacturing the peeling container 20.
[0055] (Removal part 35) The removal section 35 is configured to release the neck section 21 of the peelable container 20 manufactured in the blow molding section 34 from the neck mold 36 a , and remove the peelable container 20 to the outside of the blow molding apparatus 30 .
[0056] <Explanation of container manufacturing method> Next, a method for manufacturing the peelable container 20 by the blow molding apparatus 30 of this embodiment will be described. Fig. 9 is a flow chart showing steps of the method for manufacturing the peelable container 20.
[0057] (Step S101: First injection molding process) First, as shown in Fig. 6(a), in the first injection molding section 31, a first resin material is injected from a first injection device 37 into a mold space formed by a cavity mold 40, a core mold 41, and a neck mold 36a to mold a first layer 11 of a preform 10. At this time, a recess 11a is formed in the bottom of the first layer 11 by a first protrusion 44, as shown in Fig. 7.
[0058] In the first injection molding section 31, after the first layer 11 of the preform 10 is molded as shown in Fig. 6(b), a step is carried out in which the valve pin 43 is protruded to a position close to the core mold 41. As a result, as shown in Fig. 7, a thin film section 18 having a thickness thinner than that of the peripheral section is formed in the center of the bottom of the first layer 11.
[0059] Thereafter, the first injection molding section 31 is opened, and the first layer 11 is released. When the first injection molding section 31 is opened, the transfer plate of the transport mechanism 36 moves so as to rotate by a predetermined angle, and the first layer 11 of the preform 10 held in the neck mold 36a is transported to the second injection molding section 32 while retaining the heat retained during injection molding.
[0060] (Step S102: Second injection molding process) Next, the first layer 11 of the preform 10 is placed in the second injection molding section 32, and the second layer 12 is injection molded.
[0061] 6(c), in the second injection molding section 32, a mold space is formed between the inner periphery of the first layer 11 and the surface of the core mold 51 facing the inner periphery of the first layer 11, and the above mold space is filled with the second resin material from the hot runner mold 52. Note that a thin film portion 18 is formed at the bottom of the first layer 11, but the thin film portion 18 is broken by the injection pressure of the second resin material to form an opening 16 at the bottom, and the second resin material is introduced from the above opening 16 to the inner periphery of the first layer 11.
[0062] Here, the temperature of the second resin material filled in the second injection molding section 32 is set to a temperature lower than the melting point of the first resin material. In addition, the surface temperature of the first layer 11 when the second resin material is filled in the second injection molding section 32 is cooled to a temperature equal to or lower than the melting point of the second resin material.
[0063] In the second injection molding section 32, the cavity mold 50 faces the outer periphery of the first layer 11, and the shape of the first layer 11 is maintained from the outer periphery by the cavity mold 50. Therefore, even if the second resin material comes into contact with the first layer 11, thermal deformation of the first layer 11 can be suppressed.
[0064] In the second injection molding section 32, the second protrusions 54 penetrate and close the recesses 11a of the first layer 11, so that the recesses 17 of the preform 10 are not closed with the second resin material. In addition, the tip of the second protrusions 54 in the second injection molding section 32 protrudes to the inner periphery side of the first layer, so that the recesses 17 of the preform 10 formed by the second protrusions 54 penetrate the first layer 11 and have a shape in which the surface of the second layer 12 is exposed in the recesses 17.
[0065] In the second injection molding section 32, the second resin material flows radially outward through the gap between the core mold 51 and the second protrusion 54, thereby forming a streaky first region 19 in the second layer 12.
[0066] First, in the second injection molding section 32, as shown in Fig. 8(b), the second resin material is filled between the first layer 11 and the surface of the core mold 51, and the second resin material is cooled by contact with the core mold 51. In contrast, at the position of the second protrusion 54 shown in Fig. 8(a), the second resin material flows between the core mold 51 and the second protrusion 54, and is cooled by contact with the core mold 51 and the second protrusion 54. Therefore, at the position of the second protrusion 54, the second resin material is cooled more strongly by the second protrusion 54 than at other positions, so that the viscosity of the second resin material increases and the density of the resin in the first region 19 becomes higher.
[0067] In the second injection molding section 32, the distance L1 between the second protrusion 54 and the surface of the core mold 51 shown in FIG. 8(a) is smaller than the distance L2 between the first layer 11 and the surface of the core mold 51 shown in FIG. 8(b). Therefore, the flow rate of the resin passing between the second protrusion 54 and the core mold 51 is faster than the flow rate of the resin passing between the first layer 11 and the core mold 51. As a result, the second resin material is filled from the position of the second protrusion 54 in the circumferential direction of the second injection molding section 32, and the flow of the resin in the first region 19 is along the longitudinal direction from the bottom 15 to the neck 13. Therefore, the orientation of the resin in the first region 19 has a directionality along the longitudinal direction.
[0068] In contrast, in the second region of the second layer 12, the resin flows in later than in the first region 19, so the flow of resin in the second region is supplemented by a flow of resin spreading in the circumferential direction from the first region 19. Therefore, the orientation of the resin in the second region varies more than in the first region 19.
[0069] In this way, the first region 19 of the second layer 12 has a higher resin density than the second region, and the resin is oriented directional along the longitudinal direction of the preform 10, so that the first region 19 has the property of being less susceptible to deformation in the circumferential direction.
[0070] In this manner, the preform 10 in which the second layer 12 is laminated on the inner peripheral side of the first layer 11 is manufactured by the first injection molding step and the second injection molding step. After that, when the second injection molding section 32 is opened, the transfer plate of the transfer mechanism 36 moves so as to rotate by a predetermined angle. , Ne The preform 10 held in the mold 36a is transported to the temperature adjustment section 33 while still containing the heat retained during injection molding.
[0071] (Step S103: Temperature adjustment process) Next, in the temperature adjustment section 33, the preform 10 is accommodated in a mold unit for temperature adjustment, and temperature adjustment is performed to bring the temperature of the preform 10 close to a temperature suitable for the final blow. After that, the transfer plate of the conveying mechanism 36 moves so as to rotate by a predetermined angle, and the preform 10 after temperature adjustment held in the neck mold 36a is conveyed to the blow molding section 34.
[0072] (Step S104: Blow molding process) Next, in the blow molding section 34, the peeling container 20 is blow molded. First, the blow cavity mold is closed to accommodate the preform 10 in the mold space, and an air introduction member (blow core) is lowered to bring the air introduction member into contact with the neck 13 of the preform 10. Then, a stretching rod is lowered to hold down the bottom 15 of the preform 10 from the inside, and while vertical axis stretching is performed as necessary, blow air is supplied from the air introduction member to horizontally stretch the preform 10. As a result, the preform 10 is bulged and shaped so as to fit closely into the mold space of the blow cavity mold, and is blow molded into the peeling container 20. During the blow molding, the first region 19 of the preform 10 is stretched, so that streaky high strength portions 26 are formed in the second layer 12 of the peelable container 20 .
[0073] (Step S105: container removal process) When the blow molding is completed, the blow cavity mold is opened, which allows the peeling container 20 to be removed from the blow molding section 34. Next, the transfer plate of the conveying mechanism 36 moves so as to rotate by a predetermined angle, and the peeled container 20 is conveyed to the removal section 35. In the removal section 35, the neck section 21 of the peeled container 20 is released from the neck mold 36a, and the peeled container 20 is removed to the outside of the blow molding apparatus 30.
[0074] This completes one cycle in the method for manufacturing peeled containers. After that, the transfer plate of the conveying mechanism 36 is rotated by a predetermined angle to repeat the above steps S101 to S105. During operation of the blow molding device 30, five sets of peeled containers 20 are manufactured in parallel, with a time difference between each step.
[0075] In addition, due to the structure of the blow molding apparatus 30, the waiting times for the first injection molding process, the second injection molding process, the temperature adjustment process, the blow molding process, and the container removal process are all the same. Similarly, the transport times between each process are also the same.
[0076] The effects of the method for manufacturing a container according to this embodiment will be described below. In this embodiment, the first layer 11 (outer layer) of the preform 10 is molded in the first injection molding process, and the second layer 12 (inner layer) is injection molded inside the first layer 11 from the opening 16 of the first layer 11 in the second injection molding process to manufacture the two-layered preform 10. According to this embodiment, the outer layer is formed first with a resin material having a high melting point, and then the inner layer can be formed with a resin material having a lower melting point than the outer layer. In other words, the inner layer is continuously injection molded while the outer layer has the heat retained during injection molding, and the two-layered preform 10 suitable for the specifications of the peeling container 20 can be manufactured. In this embodiment, the two-layered preform 10 is released while both the outer layer and the inner layer have the heat retained during injection molding, so that a preform 10 suitable for manufacturing the peeling container 20 by a hot parison type blow molding method can be obtained.
[0077] In this embodiment, in the first injection molding step, the first protrusions 44 form the recesses 11a in the first layer 11. Then, in the second injection molding step, the second protrusions 54, which protrude more than the first protrusions 44, are caused to penetrate the recesses 11a in the first layer 11, to form the recesses 17 in the bottom 15 of the preform 10. This ensures that the air introduction holes 24 are formed in the peeling container 20, penetrating the first layer 11 and reaching the surface of the second layer 12.
[0078] In the second injection molding step, an injection mold in which second protrusions 54 are partially formed in the circumferential direction of the bottom is used to change the flow rate and temperature of the resin passing through the second protrusions 54. As a result, a first region 19 having a higher strength than other parts in the circumferential direction is formed in the second layer 12 of the preform 10, starting from the recess 17 formed by the second protrusions 54.
[0079] In this embodiment, the above-mentioned two-layered preform 10 is stretch-blow molded while retaining the heat from the injection molding to manufacture the peelable container 20. At this time, the first region 19 of the preform 10 is stretched, so that a streaky high-strength portion 26 is formed in the second layer 12 of the peelable container 20. When the second layer 12 of the peelable container 20 shrinks, the easily deformable portion 27 is folded so as to be in close contact with the high-strength portion 26 extending in the radial direction, and the high-strength portion 26 induces the shrinkage deformation of the second layer 12 to be appropriate and regular.
[0080] In addition, the first region 19 of the preform 10 is formed by changing the flow rate and temperature of the resin by the second protrusions 54, so there is almost no difference in appearance between the first region 19 and the second region. The same is true for the high-strength portion 26 in the second layer 12 of the peeling container 20. Therefore, in this embodiment, the structural portion for inducing shrinkage can be formed to be less noticeable, and the aesthetics and functionality of the peeling container 20 can be improved.
[0081] In this embodiment, the second protrusion 54 for forming the air introduction hole 24 is used to form the first region 19, which is the basis of the structural portion for inducing shrinkage of the container, in the second layer 12. This makes it possible to create the structural portion for inducing shrinkage in the second layer 12 while keeping the inner surface side of the second layer 12, where the contents are filled, flat, thereby improving the drainage property when the remaining amount in the blow-molded peelable container 20 is small.
[0082] The present invention is not limited to the above-described embodiment, and various improvements and design changes may be made without departing from the spirit of the present invention.
[0083] In the above embodiment, an example has been described in which a circular recess 17 is formed in the bottom 15 of the preform 10 by forming a rib-like protrusion on the bottom of the cavity mold. However, the shape of the protrusion formed on the bottom of the cavity mold is not limited to the above and may be any shape. In addition, the number of protrusions formed on the bottom of the cavity mold may be, for example, one, or a multiple other than four.
[0084] The blow molding apparatus 30 and the blow molding method of the present invention may be implemented as a six-station blow molding apparatus and blow molding method, in which a temperature adjustment section (temperature adjustment process) may be additionally provided between the first injection molding section 31 and the second injection molding section 32 (between the first injection molding process and the second injection molding process).
[0085] In the above embodiment, a high-strength portion for inducing shrinkage is formed in the inner layer of a two-layered peelable container. However, the present invention can also be applied to the manufacture of a single-layered container (such as a BIB container) that can shrink as the contents are discharged. In this case, the blow molding device has one injection molding section (a so-called four-station type).
[0086] A preform 10A corresponding to a single-layer container is manufactured as follows. For example, as shown in Fig. 10, protrusions 44 of a height that does not contact the core mold 41 are partially formed in the circumferential direction at the bottom of the second cavity mold 40B of the injection molding part. In the case of Fig. 10, the resin contacts the core mold 41 and the second cavity mold 40B over the entire circumferential direction, but the flow speed of the resin increases in the portion passing through the protrusions 44. This allows the orientation of the resin to have directionality as described above at the position of the preform 10A corresponding to the protrusions 44.
[0087] In this manner, in the single-layer preform 10A as well, similar to the above embodiment, it is possible to form the stripe-like first regions 19 extending from the positions corresponding to the protrusions 44. By blowing such a preform 10A, it is possible to form the high-strength portions 26 similar to the second layer 12 of the peeled container 20 described above in the single-layer container as well.
[0088] The high strength portion 26 of the peeling container 20 in the above embodiment may be partially formed in the bottom 23 of the container (or from the bottom 23 to the lower region of the body 22 of the container). For example, the high strength portion 26 may not be formed in the upper region of the body 22 of the container (such as the shoulder 22a of the container). In the above embodiment, the easily deformable portion 27 is divided in the circumferential direction by the high strength portion 26 on the bottom side of the container, while the second layer 12 becomes the easily deformable portion 27 over the entire circumference in the upper region of the body 22 of the container without the high strength portion 26. In the above embodiment, the first region 19 formed in the second layer 12 of the preform 10 is also partially formed from the bottom side toward the body and is not formed on the neck side.
[0089] In addition, the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0090] 10, 10A...preform, 11...first layer, 11a...recess, 12...second layer, 16...opening, 17...recess, 19...first region, 20...peeling container, 24...air inlet hole, 26...high strength portion, 27...easily deformable portion, 30...blow molding device, 31...first injection molding portion, 32...second injection molding portion, 34...blow molding portion, 37...first injection device, 38...second injection device, 40B, 50B...cavity mold, 44...first protrusion, 54...second protrusion
Claims
1. A first injection molding process for applying a first injection mold to injection mold an outer layer of a bottomed cylindrical preform with a first resin material; a second injection molding step of using a second injection mold to inject a second resin material different from the first resin material onto the inner periphery side of the outer layer to manufacture a multi-layer preform in which an inner layer is laminated on the inner side of the outer layer; A blow molding process for blow molding the multi-layer preform in a state in which the preform has heat retained during injection molding, and producing a peelable container in which the inner layer shrinks as the filling material of the inner layer is discharged, In the first injection molding step, a first recess is formed in at least a part of the outer layer by a first protrusion provided in the first injection mold, In the second injection molding step, a second protrusion provided on the second injection mold is inserted into the first recess to form a second recess in the preform, the second recess penetrating the outer layer and exposing a surface of the inner layer; At least one of a flow rate and a temperature of the second resin material passing through the second protrusion is changed by contact between the second protrusion and the second resin material, thereby forming a region in the inner layer having a strength higher than other portions in a circumferential direction starting from a position corresponding to the second recess. A method for manufacturing a peelable container.
2. The region extends from a corresponding position of the second recess toward a radially outer side of the inner layer. The method for producing the peeled container according to claim 1 .
3. In the blow molding step, air inlet holes are formed in the outer layer at positions corresponding to the second recesses. The method for producing the peeled container according to claim 1 or 2.
4. A first injection molding section that uses a first injection mold to injection mold an outer layer of a bottomed cylindrical preform with a first resin material; A second injection molding section that uses a second injection mold and injects a second resin material different from the first resin material into the inner peripheral side of the outer layer to manufacture a multi-layer preform in which an inner layer is laminated inside the outer layer; a blow molding section for blow molding the multi-layer preform in a state in which the preform has heat retained during injection molding, and producing a peelable container in which the inner layer shrinks as the filling of the inner layer is discharged; In the first injection molding section, a first recess is formed in at least a part of the outer layer by a first protrusion provided in the first injection mold, In the second injection molding section, a second protrusion provided on the second injection mold is inserted into the first recess to form a second recess in the preform, the second recess penetrating the outer layer and exposing a surface of the inner layer; At least one of a flow rate and a temperature of the second resin material passing through the second protrusion is changed by contact between the second protrusion and the second resin material, thereby forming a region in the inner layer having a strength higher than other portions in a circumferential direction starting from a position corresponding to the second recess. Peeling container manufacturing equipment.
Citation Information
Patent Citations
Plastic bottle
JP1998338220A
Plastic bottle
JP2007326586A
Double structure vessel having excellent regular contractility of inner bag vessel
JP2019142186A
blow molding machine
JP3255485B2
Foldable blow-molded bottle
JP4588200B2