Optical glass, preforms and optical elements
By optimizing the composition of optical glass with La2O3, TiO2, SiO2, and BaO, the high refractive index and dispersion requirements are met while minimizing production costs, resulting in stable and cost-effective optical elements.
Patent Information
- Application Number
- JP2023188630
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-12-01
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2037-11-13
AI Technical Summary
The existing optical glasses with high refractive index and high dispersion, such as those containing GeO2, Nb2O5, and Ta2O5, face high production costs due to the use of components with high unit prices, limiting their widespread application.
Optical glass compositions are formulated with specific ratios of La2O3, TiO2, SiO2, B2O3, and BaO, along with optional components, to achieve high refractive index and dispersion while reducing production costs, with adjustments to ensure a short wavelength and stable glass properties.
The solution provides optical glass with a short wavelength, low production cost, and improved stability, enabling the production of preforms and optical elements with enhanced imaging characteristics and reduced chromatic aberration.
Smart Images

Figure 0007587000000011 
Figure 0007587000000012 
Figure 0007587000000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical glass, a preform, and an optical element. [Background technology]
[0002] In recent years, there has been rapid progress in the digitization of devices that use optical systems and in the improvement of image and video definition. The improvement in image and video definition is particularly notable in optical devices such as digital cameras, video cameras, and projectors. At the same time, the optical systems built into these optical devices are being made lighter and more compact by reducing the number of optical elements such as lenses and prisms.
[0003] Among the optical glasses used to manufacture optical elements, those with a high refractive index (n d ) and has a low Abbe number (ν d ) is in high demand. As such high refractive index, low dispersion glass, glass compositions such as those shown in Patent Document 1 are known. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-178571 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the glass described in Patent Document 1 has a problem in that it contains many components with high unit prices, such as GeO2, Nb2O5, and Ta2O5, in order to achieve a high refractive index and high dispersion, resulting in high production costs.Therefore, there has been a demand for optical glass that has a high refractive index and high dispersion, a short wavelength (λ5) at which the spectral transmittance is 5%, and low production costs.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide an optical glass that has a high refractive index, a short wavelength (λ5) at which the spectral transmittance is 5%, and low production costs, and a preform and optical element using the same. [Means for solving the problem]
[0007] The inventors conducted extensive testing and research to solve the above problems, and as a result discovered that by using the La2O3 component, the TiO2 component, and the BaO component in combination and adjusting the total amount of the SiO2 component and the B2O3 component and the mass ratio of TiO2 / (TiO2+BaO), it is possible to obtain the desired high refractive index and high dispersion while suppressing production costs and shortening the wavelength (λ5) at which the spectral transmittance shows 5%, thereby completing the present invention. Specifically, the present invention provides the following:
[0008] (1) Mass percent based on oxides: La2O3 component is 0% to 45.0%, TiO2 content of 0% to 45.0%, and BaO content: 0% to 40.0% Contains The total amount of SiO2 and B2O3 components is 5.0% or more and 30.0% or less. The mass ratio of TiO2 / (TiO2+BaO) is 0.10 or more and 0.90 or less, Optical glass having a refractive index (nd) of 1.90 or more, an Abbe number (νd) of 30.0 or less, and a wavelength (λ5) showing a spectral transmittance of 5% of 400 nm or less.
[0009] (2) Mass percent based on oxides: SiO2 content 0-30.0%, and B2O3 component 0~30.0% The optical glass according to (1),
[0010] (3) Mass percent based on oxides: ZnO content: 0 to 20.0% Y2O3 component 0~15.0%, Nb2O5 content: 0-25.0% Yb2O3 content 0-15.0%, and Gd2O3 component 0~15.0% The optical glass according to (1) or (2),
[0011] (4) Mass percent based on oxides: The optical glass according to any one of (1) to (3), wherein the sum of the masses of (La2O3+Nb2O5+Gd2O3+Yb2O3) is more than 0% and not more than 60.0%.
[0012] (5) Mass percent based on oxides: The optical glass according to any one of (1) to (4), wherein the total content of Ln2O3 components (wherein Ln is one or more selected from the group consisting of La, Gd, Y, and Yb) is more than 0% and 50.0% or less.
[0013] (6) On an oxide basis The optical glass according to any one of (1) to (5), wherein TiO2 / BaO is greater than 0 and is not greater than 3.00.
[0014] (7) Mass percent based on oxides: The optical glass according to any one of (1) to (6), wherein the sum of the masses of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na and K) is 15.0% or less.
[0015] (8) Mass percent based on oxide: The optical glass according to any one of (1) to (7), wherein the sum of the masses of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, Ba, and Zn) is more than 0% and 35.0% or less.
[0016] (9) Mass percent based on oxide: ZrO2 content 0~20.0%, Nb2O5 content: 0-15.0% WO3 content 0-10.0% Ta2O5 component 0~10.0%, MgO content: 0-15.0% CaO component 0~15.0%, SrO content 0~15.0%, Li2O content 0~15.0% Na2O content 0~15.0%, K2O content 0~15.0%, P2O5 content: 0-10.0% GeO2 content 0~10.0% Al2O3 content: 0-15.0% Ga2O3 component 0~15.0%, Bi2O3 content 0~10.0%, TeO2 content 0~10.0%, SnO2 content 0-3.0%, and Sb2O3 component 0~1.0% The optical glass according to any one of (1) to (8), comprising:
[0017] (10) A preform material made of the optical glass according to any one of (1) to (9).
[0018] (11) An optical element made of the optical glass according to any one of (1) to (9).
[0019] (12) An optical device comprising the optical element according to (11). Effect of the Invention
[0020] According to the present invention, it is possible to provide an optical glass that has a high refractive index and high dispersion while exhibiting a short wavelength (λ5) at which the spectral transmittance is 5% and that has low production costs, as well as a preform and an optical element that use the same. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a diagram showing a normal line represented on an orthogonal coordinate system with the partial dispersion ratio (θg,F) on the vertical axis and the Abbe number (νd) on the horizontal axis. [Diagram 2] FIG. 2 is a graph showing the relationship between the partial dispersion ratio (θg,F) and the Abbe number (νd) for glasses in the examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The optical glass of the present invention contains, by mass, from more than 0% to 45.0% of a La2O3 component, from more than 0% to 45.0% of a TiO2 component, and from more than 0% to 40.0% of a BaO component, the total amount of the SiO2 component and the B2O3 component is from 5.0% to 30.0%, the mass ratio of TiO2 / (TiO2+BaO) is from 0.10 to 0.90, the refractive index (nd) is 1.90 or more, the Abbe number (νd) is 30.0 or less, and the wavelength (λ5) at which the spectral transmittance shows 5% is 400 nm or less. According to the present invention, by using La2O3, TiO2 and BaO in combination and adjusting the contents of each component, it is possible to achieve a high refractive index and high dispersion in the glass while improving the stability of the glass. As a result, it is possible to provide an optical glass that has a high refractive index and high dispersion, a short wavelength (λ5) at which the spectral transmittance is 5%, and low production costs, as well as a preform and an optical element using the same.
[0023] [Glass composition] The composition range of each component constituting the optical glass of the present invention is described below. In this specification, the content of each component is expressed as mass% based on the oxide, unless otherwise specified. Here, "on the oxide basis" refers to a composition in which each component contained in the glass is expressed with the total mass of the oxide being 100 mass%, assuming that the oxides, composite salts, metal fluorides, etc. used as raw materials for the glass components of the present invention are all decomposed and converted to oxides during melting.
[0024] <Required and optional ingredients> The La2O3 component is a component that increases the refractive index of the glass and reduces dispersion. In particular, the La2O3 component is an essential component that can obtain a desired high refractive index by containing more than 0% of the La2O3 component. Therefore, the lower limit of the content of the La2O3 component is preferably more than 0%, more preferably 3.0%, even more preferably 15.0%, even more preferably 20.0%, even more preferably 25.0%, and even more preferably 27.0%. On the other hand, by setting the content of the La2O3 component to 45.0% or less, the devitrification resistance of the glass can be improved, an increase in the specific gravity of the glass can be suppressed, and production costs can be reduced. Therefore, the upper limit of the content of the La2O3 component is preferably set to 45.0%, more preferably 40.0%, even more preferably 38.0%, and still more preferably 37.0%. The La2O3 component can be prepared from raw materials such as La2O3, La(NO3)3·XH2O (X is any integer).
[0025] When the TiO2 component is contained at more than 0%, it is an essential component that can increase the refractive index of the glass, adjust the Abbe number low, increase the partial dispersion ratio, and increase the devitrification resistance. Therefore, the lower limit of the content of the TiO2 component is preferably more than 0%, preferably 5.0%, more preferably more than 10.0%, more preferably 15.0%, more preferably 18.0%, and more preferably more than 20.0%. On the other hand, by making the content of the TiO2 component 45.0% or less, the coloring of the glass can be reduced and the visible light transmittance can be increased. Also, devitrification caused by an excessive content of the TiO2 component can be suppressed. Therefore, the upper limit of the content of the TiO2 component is preferably 45.0%, more preferably 38.0%, even more preferably 32.0%, even more preferably 27.0%, and even more preferably 25.0%. The TiO2 component can use TiO2 or the like as a raw material.
[0026] The BaO component is an essential component that can increase the refractive index and devitrification resistance of the glass and can also increase the melting property of the glass raw material when it is contained at more than 0%. Therefore, the lower limit of the BaO component content is preferably more than 0%, more preferably 5.0%, even more preferably 8.0%, and even more preferably 10.0%. On the other hand, by keeping the content of the BaO component at 40.0% or less, it is possible to make it difficult for the refractive index of the glass to decrease and to reduce devitrification of the glass. Therefore, the upper limit of the content of the BaO component is preferably 40.0%, more preferably 35.0%, even more preferably 28.0%, even more preferably 23.0%, and even more preferably 20.0%. The BaO component can be obtained from raw materials such as BaCO3 and Ba(NO3)2.
[0027] The sum of the contents (sum of mass) of the B2O3 component and the SiO2 component is preferably 5.0% or more and 30.0% or less. In particular, by making this sum 5.0% or more, it is possible to suppress the deterioration of devitrification resistance due to the deficiency of the B2O3 component and the SiO2 component. Therefore, the lower limit of the mass sum (B2O3 + SiO2) is preferably 5.0%, more preferably 7.0%, and further preferably 9.0%. On the other hand, by making this sum 30.0% or less, the decrease in refractive index due to the excessive inclusion of these components is suppressed, making it easier to obtain a desired high refractive index. Therefore, the upper limit of the mass sum (B2O3+SiO2) is preferably 30.0%, more preferably 23.0%, even more preferably 18.0%, and even more preferably 16.50%.
[0028] Here, the ratio (mass ratio) of the content of the TiO2 component to the sum of the contents of the TiO2 component and the BaO component is preferably 0.1 or more. This makes it possible to obtain a high partial dispersion ratio while maintaining a high refractive index and high dispersion. Therefore, the mass ratio TiO2 / (TiO2+BaO) is preferably set to a lower limit of 0.10, more preferably 0.30, even more preferably 0.40, and even more preferably 0.45. On the other hand, by making this mass ratio 0.90 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / (TiO2+BaO) is preferably 0.90, more preferably 0.80, even more preferably 0.73, and still more preferably 0.68.
[0029] The SiO2 component is an optional component that can improve devitrification resistance when contained in an amount of more than 0%. Therefore, the lower limit of the content of the SiO2 component is preferably more than 0%, more preferably more than 0.5%, even more preferably more than 1.0%, and even more preferably more than 2.0%. On the other hand, by making the content of the SiO2 component 30.0% or less, the SiO2 component can be easily dissolved in the molten glass and melting at high temperatures can be avoided. The upper limit of the content of the SiO2 component is preferably 30.0%, more preferably 23.0%, even more preferably 16.0%, even more preferably 11.0%, and even more preferably 9.0%. The SiO2 component can be made from SiO2, K2SiF6, Na2SiF6, etc. as raw materials.
[0030] The B2O3 component is an optional component that, when contained at more than 0%, forms a network structure inside the glass, promotes stable glass formation, and enhances devitrification resistance. Therefore, the lower limit of the content of the B2O3 component is preferably more than 0%, more preferably more than 0.5%, even more preferably more than 1.0%, and even more preferably more than 2.0%. On the other hand, by making the content of the B2O3 component 30.0% or less, it is possible to suppress the decrease in the refractive index, reduce the Abbe number, and suppress the deterioration of chemical durability. Therefore, the upper limit of the content of the B2O3 component is preferably 30.0% or less, more preferably 20.0%, even more preferably less than 15.0%, even more preferably 12.0%, and even more preferably less than 10.0%. The B2O3 component can be produced from H3BO3, Na2B4O7, Na2B4O7·10H2O, BPO4, etc.
[0031] The ZnO component is an optional component that can improve the meltability of glass, lower the glass transition point, and reduce devitrification when contained at more than 0%. Therefore, the lower limit of the ZnO content is preferably more than 0%, more preferably more than 0.5%, even more preferably more than 1.0%, and even more preferably more than 1.5%. On the other hand, by making the content of the ZnO component 20.0% or less, it is possible to reduce the decrease in the refractive index and devitrification. This also increases the viscosity of the molten glass, thereby reducing the occurrence of striae in the glass. Therefore, the upper limit of the content of the ZnO component is preferably 20.0%, more preferably 15.0%, even more preferably 11.0%, and even more preferably 8.0%. As the ZnO component, ZnO, ZnF2, etc. can be used as the raw material.
[0032] The Y2O3 component is an optional component that, when contained at more than 0%, can suppress an increase in the material cost of the glass. By keeping the content of the Y2O3 component at 15.0% or less, the decrease in the refractive index of the glass can be suppressed, the Abbe number can be reduced, and the devitrification resistance of the glass can be improved. Therefore, the upper limit of the content of the Y2O3 component is preferably set to 15.0%, more preferably 10.0%, and even more preferably 5.0%. As the Y2O3 component, Y2O3, YF3, etc. can be used as the raw material.
[0033] The Nb2O5 component is an optional component that can increase the refractive index of the glass and improve the devitrification resistance when it is contained at more than 0%. Therefore, the lower limit of the content of the Nb2O5 component is preferably more than 0%, more preferably 2.0%, and further preferably 4.0%. On the other hand, by keeping the content of the Nb2O5 component at 25.0% or less, it is possible to suppress the deterioration of the devitrification resistance of the glass and the deterioration of the visible light transmittance caused by the excessive content of the Nb2O5 component, and also to suppress the increase in the material cost of the glass. Therefore, the upper limit of the content of the Nb2O5 component is preferably 25.0%, more preferably 20.0%, even more preferably 16.0%, and even more preferably 13.0%. As the Nb2O5 component, Nb2O5 or the like can be used as a raw material.
[0034] The Yb2O3 component is an optional component that can increase the refractive index of the glass when it is present at more than 0%. Ingredients. On the other hand, by making the content of the Yb2O3 component 15.0% or less, the devitrification resistance of the glass can be improved and the Abbe number can be made small. Therefore, the upper limit of the content of the Yb2O3 component is preferably set to 15.0%, more preferably to 10.0%, and further preferably to 5.0%. For the Yb2O3 component, Yb2O3 or the like can be used as a raw material.
[0035] The Gd2O3 component is an optional component that, when contained at more than 0%, can increase the refractive index of the glass and increase the Abbe number. On the other hand, by reducing the content of Gd2O3, which is particularly expensive among rare earth elements, to 15.0% or less, the material cost of the glass can be reduced, making it possible to produce a cheaper optical glass. This also prevents the Abbe number of the glass from increasing more than necessary. Therefore, the upper limit of the content of the Gd2O3 component is preferably 15.0%, more preferably 10.0%, and even more preferably 5.0%. The Gd2O3 component can be prepared from Gd2O3, GdF3, etc.
[0036] In addition, in the optical glass of the present invention, the sum of the contents (mass sum) of the La2O3 component, the Nb2O5 component, the Gd2O3 component, and the Yb2O3 component is preferably 60.0% or less. This reduces the contents of these expensive components, thereby reducing the material cost of the glass and making it possible to reduce the Abbe number. Therefore, the upper limit of the mass sum (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably 60.0%, more preferably 57.0%, even more preferably 53.0%, even more preferably 49.0%, and even more preferably 47.0%. On the other hand, a desired high refractive index can be obtained by including more than 0%. Therefore, the lower limit is preferably more than 0%, more preferably 10.0%, even more preferably 20.0%, even more preferably 25.0%, even more preferably 30.0%, and even more preferably 35.0%.
[0037] The sum of the contents (sum of mass) of Ln2O3 components (wherein Ln is one or more selected from the group consisting of La, Gd, Y and Yb) is more than 0% and 50.0%. In particular, by making the mass sum exceed 0%, the refractive index of the glass can be increased, making it easier to obtain a high refractive index glass. This also reduces coloring. Therefore, the mass sum of the content of the Ln2O3 component is preferably more than 0%, more preferably 1.0%, even more preferably 3.0%, and even more preferably 5.0% as the lower limit. On the other hand, by making the mass sum 50.0% or less, it is possible to improve the devitrification resistance and reduce the Abbe number. Therefore, the mass sum of the Ln2O3 component content is preferably set to an upper limit of 50.0%, more preferably less than 40.0%, even more preferably 30.0%, and even more preferably 25.0%.
[0038] Here, the ratio (mass ratio) of the content of the TiO2 component to the sum of the contents of the La2O3 component, the Nb2O5 component, the Gd2O3 component, and the Yb2O3 component is preferably greater than 0. This makes it possible to obtain a high partial dispersion ratio while maintaining a high refractive index and high dispersion, and to reduce production costs. Therefore, the mass ratio TiO2 / (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably greater than 0, more preferably 0.10, even more preferably 0.20, and even more preferably 0.40 as the lower limit. On the other hand, by making this mass ratio 2.00 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably set to 2.00, more preferably to 1.00, even more preferably to 0.80, and even more preferably to 0.66.
[0039] Here, the ratio (mass ratio) of the content of the TiO2 component to the content of the BaO component is preferably greater than 0. This makes it possible to obtain a high partial dispersion ratio while maintaining a high refractive index and high dispersion. The mass ratio TiO2 / BaO has a lower limit of preferably greater than 0, more preferably 0.10, even more preferably 0.40, and even more preferably 0.60. On the other hand, by making this mass ratio 3.00 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / BaO is preferably 3.00, more preferably 2.00, and further preferably 1.60.
[0040] Here, the ratio (mass ratio) of the sum of the contents of the TiO2 component and the WO3 component to the sum of the contents of the BaO component is preferably greater than 0. This makes it possible to obtain a high partial dispersion ratio while maintaining a high refractive index and high dispersion, and to improve devitrification resistance. Therefore, the mass ratio (TiO2+WO3) / BaO is preferably greater than 0, more preferably 0.30, even more preferably 0.60, even more preferably 0.80, and even more preferably 1.00 as the lower limit. On the other hand, by making this mass ratio 3.00 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio (TiO2+WO3) / BaO is preferably 3.00, more preferably 2.50, and further preferably 1.90.
[0041] The sum of the contents of the TiO2 component and the Nb2O5 component (mass sum) is preferably more than 0%. This makes it possible to increase the refractive index and dispersion and to improve devitrification resistance. Therefore, the lower limit of the mass sum (TiO2 + Nb2O5) is preferably more than 0%, more preferably more than 10.0%, even more preferably more than 15.0%, even more preferably more than 20.0%, and even more preferably more than 25.0%. On the other hand, when the content is 60.0% or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit is preferably 60.0%, more preferably 50.0%, even more preferably 45.0%, even more preferably 40.0%, even more preferably 35.0%, and even more preferably 33.0%.
[0042] The total amount of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na, K, and Cs) is preferably 15.0% or less. This makes it possible to suppress a decrease in the refractive index of the glass and to improve devitrification resistance. Therefore, the upper limit of the sum of the masses of the Rn2O components is preferably 15.0%, more preferably 10.0%, even more preferably less than 5.0%, and even more preferably less than 1.0%.
[0043] The sum of the contents (mass sum) of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) is preferably 35.0% or less. This can reduce devitrification due to excessive inclusion of RO components, and suppress a decrease in the refractive index. Therefore, the upper limit of the mass sum of the contents of RO components is preferably 35.0%, more preferably 30.0%, even more preferably 27.0%, even more preferably less than 23.0%, and even more preferably 20.0%. On the other hand, by making this sum more than 0%, the meltability of the glass raw material and the stability of the glass can be improved. Therefore, the lower limit of the total content of the RO components may be preferably more than 0%, more preferably 4.0%, even more preferably 7.0%, and even more preferably more than 9.0%.
[0044] When the ZrO2 component is contained in an amount exceeding 0%, it can contribute to a high refractive index and low dispersion of the glass, and can also improve the devitrification resistance of the glass. Therefore, the lower limit of the content of the ZrO2 component may be preferably more than 0%, more preferably 0.5%, and even more preferably 1.0%. On the other hand, by keeping the ZrO2 component at 20.0% or less, it is possible to prevent a decrease in the devitrification resistance of the glass and an unnecessary increase in the Abbe number due to an excessive content of the ZrO2 component. Therefore, the upper limit of the content of the ZrO2 component is preferably 20.0%, more preferably 16.0%, even more preferably 12.0%, even more preferably 9.0%, and even more preferably less than 6.5%. As the ZrO2 component, ZrO2, ZrF4, etc. can be used as raw materials.
[0045] The WO3 component is an optional component that, when contained at more than 0%, can increase the refractive index while reducing the coloring of the glass caused by other high refractive index components, increase the partial dispersion ratio, and increase the devitrification resistance of the glass. The WO3 component is also a component that can lower the glass transition point. Therefore, the content of the WO3 component may be set at a lower limit of preferably more than 0%, more preferably 0.1%, even more preferably 0.2%, and even more preferably 0.3%. On the other hand, by keeping the content of the WO3 component at 10.0% or less, the coloring of the glass caused by the WO3 component can be reduced and the visible light transmittance can be increased. Therefore, the upper limit of the content of the WO3 component is preferably set to 10.0%, more preferably to 5.0%, and further preferably to 3.0%. As the WO3 component, WO3 or the like can be used as a raw material.
[0046] The Ta2O5 component is an optional component that, when contained in an amount exceeding 0%, increases the refractive index of the glass and improves the devitrification resistance. On the other hand, by reducing the expensive Ta2O5 component to 10.0% or less, the material cost of the glass is reduced, and therefore a cheaper optical glass can be produced. In addition, by reducing the content of the Ta2O5 component to 10.0% or less, the melting temperature of the raw material is lowered, and the energy required for melting the raw material is reduced, and therefore the manufacturing cost of the optical glass can be reduced. Therefore, the content of the Ta2O5 component is preferably set to an upper limit of 10.0%, more preferably 8.0%, and even more preferably 5.0%. In particular, from the viewpoint of producing a cheaper optical glass, the content of the Ta2O5 component is preferably set to an upper limit of 4.0%, more preferably 3.0%, and even more preferably less than 1.0%, and most preferably not contained. The Ta2O5 component can use Ta2O5 or the like as a raw material.
[0047] The MgO component is an optional component that, when contained in an amount exceeding 0%, can improve the meltability of the glass raw material and the devitrification resistance of the glass. On the other hand, by limiting the content of the MgO component to 15.0% or less, it is possible to suppress the decrease in refractive index and the decrease in devitrification resistance caused by the excessive content of these components. Therefore, the upper limit of the content of the MgO component is preferably set to 15.0%, more preferably 10.0%, and further preferably 5.0%. The MgO component can be made from raw materials such as MgCO3 and MgF2.
[0048] The CaO component is an optional component that, when contained at more than 0%, can increase the refractive index and devitrification resistance of the glass and can also increase the melting property of the glass raw material. Therefore, the lower limit of the CaO content is preferably more than 0%, more preferably 0.5%, even more preferably 1.5%, and even more preferably 3.0%. On the other hand, by making the content of the CaO component 15.0% or less, it is possible to make it difficult for the refractive index of the glass to decrease and to reduce devitrification of the glass. Therefore, the upper limit of the content of the CaO component is preferably set to 15.0%, more preferably 10.0%, and further preferably 5.0%. The CaO component can be obtained from raw materials such as CaCO3 and CaF2.
[0049] The SrO component is an optional component that, when contained at more than 0%, can increase the refractive index and devitrification resistance of the glass and can also increase the melting property of the glass raw material. Therefore, the lower limit of the SrO component content is preferably more than 0%, more preferably 0.5%, even more preferably 1.5%, and even more preferably 3.0%. On the other hand, by keeping the content of the SrO component at 15.0% or less, it is possible to make it difficult for the refractive index of the glass to decrease and to reduce devitrification of the glass. Therefore, the upper limit of the content of the SrO component is preferably set to 15.0%, more preferably 10.0%, and further preferably 5.0%. As the SrO component, SrCO3, SrF2, etc. can be used as the raw material.
[0050] The Li2O, Na2O and K2O components are optional components that can improve the meltability of glass when at least any of them is contained in an amount exceeding 0%. In particular, the K2O component is a component that further increases the partial dispersion ratio of glass. On the other hand, by reducing the content of the Li2O component, the Na2O component, or the K2O component, the decrease in the refractive index of the glass can be suppressed and devitrification can be reduced. In particular, by reducing the content of the Li2O component, the decrease in the partial dispersion ratio of the glass can be suppressed. Therefore, the upper limit of the content of at least any one of the Li2O component, the Na2O component, and the K2O component is preferably 15.0%, more preferably less than 10.0%, even more preferably less than 5.0%, and even more preferably less than 1.0%. The Li2O component, Na2O component and K2O component can use Li2CO3, LiNO3, LiF, Na2CO3, NaNO3, NaF, Na2SiF6, K2CO3, KNO3, KF, KHF2, K2SiF6, etc. as raw materials.
[0051] The P2O5 component is an optional component that can improve the devitrification resistance of glass when it is contained in an amount exceeding 0%. In particular, by keeping the content of the P2O5 component at 10.0% or less, the deterioration of the chemical durability of the glass, particularly the water resistance, can be suppressed. Therefore, the upper limit of the content of the P2O5 component is preferably set to 10.0%, more preferably 5.0%, and even more preferably 3.0%. The P2O5 component can be made from raw materials such as Al(PO3)3, Ca(PO3)2, Ba(PO3)2, BPO4, and H3PO4.
[0052] The GeO2 component is an optional component that can increase the refractive index of the glass and improve the devitrification resistance when it is contained at more than 0%. However, since the raw material price of GeO2 is high, if the amount is large, the material cost increases, and the effect of reducing the cost by reducing the Gd2O3 component and the Ta2O5 component is reduced. Therefore, the content of the GeO2 component is preferably set to an upper limit of 10.0%, more preferably 5.0%, and even more preferably 1.0%, and most preferably is not contained. The GeO2 component can use GeO2 or the like as a raw material.
[0053] The Al2O3 component and the Ga2O3 component are optional components that, when contained by more than 0%, can increase the chemical durability of the glass and can also increase the devitrification resistance of the glass. On the other hand, by limiting the content of each of the Al2O3 component and the Ga2O3 component to 15.0% or less, it is possible to prevent a decrease in the devitrification resistance of the glass due to their excessive content. Therefore, the upper limit of each of the Al2O3 component and the Ga2O3 component contents is preferably set to 15.0%, more preferably 8.0%, and further preferably 3.0%. The Al2O3 component and the Ga2O3 component can use Al2O3, Al(OH)3, AlF3, Ga2O3, Ga(OH)3, etc. as raw materials.
[0054] The Bi2O3 component is an optional component that, when contained at more than 0%, can increase the refractive index and lower the glass transition point. On the other hand, by keeping the content of the Bi2O3 component at 10.0% or less, the devitrification resistance of the glass can be improved, and the coloring of the glass can be reduced to increase the visible light transmittance. Therefore, the upper limit of the content of the Bi2O3 component is preferably set to 10.0%, more preferably 5.0%, and further preferably 3.0%. The Bi2O3 component can use Bi2O3 or the like as a raw material.
[0055] The TeO2 component is an optional component that, when contained at more than 0%, can increase the refractive index and lower the glass transition point. However, when glass raw materials are melted in a platinum crucible or a melting tank in which the part in contact with the molten glass is made of platinum, TeO2 may form an alloy with platinum. Therefore, the content of TeO2 component is preferably set to 10.0%, more preferably 5.0%, and even more preferably 3.0% as the upper limit, and even more preferably none is contained. The TeO2 component can use TeO2 or the like as a raw material.
[0056] The SnO2 component is an optional component that, when contained in an amount exceeding 0%, can reduce the oxidation of the molten glass to clarify the molten glass and can also prevent the light transmittance of the glass from deteriorating. On the other hand, by making the content of the SnO2 component 3.0% or less, it is possible to prevent the coloring of the glass due to the reduction of the molten glass and the devitrification of the glass. In addition, since the alloying of the SnO2 component with the melting equipment (especially precious metals such as Pt) is reduced, the life of the melting equipment can be extended. Therefore, the content of the SnO2 component is preferably 3.0% or less, more preferably less than 2.0%, even more preferably less than 1.0%, and even more preferably not contained. As the SnO2 component, SnO, SnO2, SnF2, SnF4, etc. can be used as raw materials.
[0057] The Sb2O3 component is an optional component that can degas the molten glass when its content exceeds 0%. On the other hand, by making the content of Sb2O3 component 1.0% or less, it is possible to make it difficult for excessive foaming to occur and to reduce alloying with the melting equipment (especially precious metals such as Pt). Therefore, the content of Sb2O3 component is preferably 1.0% or less, more preferably less than 0.5%, even more preferably less than 0.3%, and even more preferably less than 0.1%. The Sb2O3 component can be made from Sb2O3, Sb2O5, Na2H2Sb2O7·5H2O, etc. as raw materials.
[0058] The component for clarifying and defoaming the glass is not limited to the above Sb2O3 component, and any fining agent, defoaming agent or combination thereof known in the field of glass manufacturing can be used.
[0059] The F component is an optional component which, when contained by more than 0%, can increase the Abbe number of the glass, lower the glass transition point, and improve the resistance to devitrification. However, when the content of the F component, i.e., the total amount of F in the fluorides which have substituted a part or all of one or more oxides of the above-mentioned metal elements, exceeds 10.0%, the amount of volatilization of the F component increases, making it difficult to obtain stable optical constants and homogeneous glass, and the Abbe number increases more than necessary. Therefore, the content of the F component is preferably 10.0%, more preferably less than 5.0%, even more preferably less than 3.0%, even more preferably less than 1.0%, and even more preferably none is contained. <Ingredients that should not be included> Next, components that should not be contained in the optical glass of the present invention and components whose inclusion is undesirable will be described.
[0060] Other components can be added to the optical glass of the present invention as necessary within the limits that do not impair the properties of the glass of the present invention, however, it is preferable that the GeO2 component is substantially not included since it increases the dispersibility of the glass.
[0061] Furthermore, transition metal components other than Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, such as Hf, V, Cr, Mn, Fe, Co, Ni, Cu, Ag, Mo, Ce, and Nd, have the property of coloring the glass and absorbing light of specific wavelengths in the visible range even when contained in small amounts alone or in combination, and therefore are preferably substantially free of these elements, particularly in optical glasses that use wavelengths in the visible range.
[0062] Furthermore, in recent years, there has been a trend to refrain from using lead compounds such as PbO, arsenic compounds such as As2O3, and the components Th, Cd, Tl, Os, Be, and Se as harmful chemical substances, and environmental measures are required not only in the glass manufacturing process but also in the processing process and disposal after commercialization. Therefore, when the environmental impact is important, it is preferable that the glass does not substantially contain these substances, except for unavoidable contamination. This means that the optical glass does not substantially contain substances that pollute the environment. Therefore, the optical glass can be manufactured, processed, and disposed of without taking special environmental measures.
[0063] [Manufacturing method] The optical glass of the present invention is produced, for example, as follows. That is, the above-mentioned raw materials are mixed uniformly so that each component falls within a predetermined content range, the mixture thus produced is put into a platinum crucible, a quartz crucible or an alumina crucible to be roughly melted, and then put into a gold crucible, a platinum crucible, a platinum alloy crucible or an iridium crucible to be melted at a temperature range of 900 to 1400°C for 1 to 5 hours, stirred and homogenized, and bubble-removing, etc. are performed, and then the temperature is lowered to 1300°C or less, and then finish stirring is performed to remove striae, and the glass is molded using a mold. Here, the means for obtaining the glass molded using a mold include a means for allowing the molten glass to flow down one end of the mold and simultaneously drawing out the molded glass from the other end of the mold, and a means for casting the molten glass into a metal mold and slowly cooling it.
[0064] [Physical Properties] The optical glass of the present invention preferably has a high refractive index and high dispersion. In particular, the refractive index (nd) of the optical glass of the present invention is preferably 1.90, more preferably 1.95, and even more preferably 1.98 as the lower limit. The upper limit of this refractive index may be preferably 2.20, more preferably 2.15, and even more preferably 2.10. The Abbe number (νd) of the optical glass of the present invention is preferably 15.0, more preferably 18.0, and even more preferably 20.0 as the lower limit, and preferably 30.0, more preferably 28.0, and even more preferably 27.0 as the upper limit. Such a high refractive index allows a large amount of light refraction to be obtained even when the optical element is made thin. Also, such a high dispersion allows for excellent imaging characteristics, for example, when combined with an optical element having low dispersion (high Abbe number). Therefore, the optical glass of the present invention is useful in optical design, and in particular, it allows the optical system to be made compact while still achieving high imaging characteristics, thereby expanding the degree of freedom in optical design.
[0065] It is preferable that the optical glass of the present invention has a high visible light transmittance, particularly a high transmittance for light on the short wavelength side of visible light, and thus has little coloring. In particular, the optical glass of the present invention, when expressed in terms of glass transmittance, has a wavelength (λ ) at which a sample having a thickness of 10 mm exhibits a spectral transmittance of 70%. 70 ) is preferably limited to an upper limit of 500 nm, more preferably 490 nm, and even more preferably 480 nm. Furthermore, in the optical glass of the present invention, the shortest wavelength (λ5) at which a sample with a thickness of 10 mm exhibits a spectral transmittance of 5% is preferably set to an upper limit of 400 nm, more preferably 390 nm. This brings the absorption edge of the glass into the vicinity of the ultraviolet region, and increases the transparency of the glass to visible light, so that this optical glass can be preferably used in optical elements that transmit light, such as lenses.
[0066] The optical glass of the present invention preferably has a high partial dispersion ratio (θg,F). More specifically, the partial dispersion ratio (θg,F) of the optical glass of the present invention preferably has a lower limit of 0.570, more preferably 0.580, even more preferably 0.595, even more preferably 0.605, and even more preferably 0.612. The partial dispersion ratio (θg,F) of the optical glass of the present invention is d ), it is preferable to satisfy the relationship (-0.00162νd+0.645)≦(θg,F)≦(-0.00162νd+0.680). This makes it possible to obtain an optical glass with a small partial dispersion ratio (θg,F), which can be used to reduce chromatic aberration in optical elements. Therefore, the lower limit of the partial dispersion ratio (θg,F) of the optical glass of the present invention is preferably (−0.00162νd+0.645), and more preferably (−0.00162νd+0.650). On the other hand, the upper limit of the partial dispersion ratio (θg,F) of the optical glass of the present invention is preferably (−0.00162νd+0.675), and more preferably (−0.00162νd+0.670).
[0067] The partial dispersion ratio (θg,F) and Abbe number (ν dThe relational equation is expressed by using a straight line parallel to the normal line in an orthogonal coordinate system with the partial dispersion ratio on the vertical axis and the Abbe number on the horizontal axis. The normal line is a relationship between the partial dispersion ratio (θg,F) and Abbe number (ν d ) and the partial dispersion ratio (θg,F) is plotted on the vertical axis, while the Abbe number (ν d ) on the horizontal axis, a straight line connecting two plotted points of the partial dispersion ratios and Abbe numbers of NSL7 and PBM2 (see Figure 1). The relationship between the partial dispersion ratios and Abbe numbers of conventionally known glasses generally overlaps with the normal line. Here, NSL7 and PBM2 are optical glasses manufactured by Ohara Co., Ltd., and the Abbe number (ν d ) is 36.3, the partial dispersion ratio (θg,F) is 0.5828, and the Abbe number of NSL7 (ν d ) is 60.5, and the partial dispersion ratio (θg,F) is 0.5436.
[0068] [Preforms and optical elements] From the produced optical glass, a glass molded body can be produced, for example, by using a polishing means or a mold press molding means such as reheat press molding or precision press molding. That is, a glass molded body can be produced by performing mechanical processing such as grinding and polishing on the optical glass, a glass molded body can be produced by performing reheat press molding on a preform produced from the optical glass and then polishing, or a glass molded body can be produced by performing precision press molding on a preform produced by polishing or a preform molded by known floating molding or the like. The means for producing the glass molded body are not limited to these means.
[0069] Thus, the glass molded body formed from the optical glass of the present invention is useful for various optical elements and optical designs, and is particularly preferably used for optical elements such as lenses, prisms, etc. The increased stability of the glass makes it possible to form a glass molded body with a large diameter, and therefore, even when the optical element is made large, high-definition and high-precision imaging and projection characteristics can be achieved when used in optical instruments such as cameras and projectors. EXAMPLES
[0070] The glass compositions of the examples (No. 1 to No. 52) of the present invention and the refractive index (n d ), Abbe number (ν d ), transmittance (λ5, λ 70 The values of the dispersion ratio (θg,F) and partial dispersion ratio (θg,F) are shown in Tables 1 to 10. Note that the following examples are merely for illustrative purposes, and the present invention is not limited to these examples.
[0071] For the glasses of the examples, high purity raw materials used in ordinary optical glass, such as the corresponding oxides, hydroxides, carbonates, nitrates, fluorides, hydroxides, and metaphosphate compounds, were selected as the raw materials for each component, weighed out and mixed uniformly, and then placed in a platinum crucible. The glass raw materials were melted in an electric furnace at a temperature range of 1280 to 1340°C for 2.5 hours, and the molten glass raw materials were stirred to remove bubbles. The temperature was then lowered to 1180 to 1250°C, and the mixture was further stirred and homogenized, before being poured into a mold and slowly cooled to produce the glass.
[0072] The refractive index (n d ) and Abbe number (ν d ) is shown as a measurement value for the d line (587.56 nm) of a helium lamp. d ) is the refractive index of the d line and the refractive index of the F line (486.13 nm) of a hydrogen lamp (n F ), and the refractive index for the C line (656.27 nm) (n C ) value, the Abbe number (ν d )=[(n d -1) / (n F -nC )] was calculated using the formula: The partial dispersion ratio is the refractive index n C , the refractive index n at F line (wavelength 486.13 nm) F , the refractive index n at g line (wavelength 435.835 nm) g Measure (θg, F) = (n g -n F ) / (n F -n C ) was calculated using the formula: The glass used in this measurement was treated in an annealing furnace at an annealing rate of -25°C / hr.
[0073] The transmittance of the glass in the examples was measured in accordance with the Japan Optical Glass Industry Association standard JOGIS02-2003. In the present invention, the presence and degree of coloration of the glass was determined by measuring the transmittance of the glass. Specifically, the spectral transmittance of a 10±0.1 mm thick parallel polished face-to-face product was measured in accordance with JIS Z8722 from 200 to 800 nm, and λ5 (wavelength at transmittance of 5%) and λ 70 (Wavelength at 70% transmittance) was calculated. The glass used in this measurement was treated in an annealing furnace at an annealing rate of -25°C / hr.
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3]
[0077] [Table 4]
[0078] [Table 5]
[0079] [Table 6]
[0080] [Table 7]
[0081] [Table 8]
[0082] [Table 9]
[0083] [Table 10]
[0084] As shown in the table, the optical glasses of the examples of the present invention all have a refractive index (n d ) is 1.90 or more, and the refractive index (n d ) was 2.20 or less, more specifically 2.10 or less, which was within the desired range. In addition, the optical glasses according to the embodiments of the present invention all have an Abbe number (ν d ) is 30.0 or less, more specifically 28.0 or less, and this Abbe number (ν d ) was 15.0 or more, more specifically 20.0 or more, which was within the desired range.
[0085] In addition, the optical glass according to the embodiment of the present invention has a λ 70(wavelength at 70% transmittance) was 500 nm or less, more specifically 490 nm or less. In addition, the optical glasses of the examples of the present invention all had λ5 (wavelength at 5% transmittance) of 400 nm or less, more specifically 390 nm or less.
[0086] In addition, the optical glasses of the examples of the present invention all had partial dispersion ratios (θg,F) of (-0.00162νd+0.645) or more, more specifically (-0.00162νd+0.650) or more. On the other hand, the optical glasses of the examples of the present invention had partial dispersion ratios of (-0.00162νd+0.680) or less, more specifically (-0.00162νd+0.670) or less. Therefore, it was found that these partial dispersion ratios (θg,F) were within the desired range.
[0087] It was therefore apparent that the optical glasses of the examples of the present invention had refractive indices and Abbe numbers within the desired ranges, could be produced at low cost, and were less colored.
[0088] Furthermore, the optical glass obtained in the examples of the present invention was used to carry out reheat press molding, followed by grinding and polishing to process into the shapes of lenses and prisms. Also, the optical glass in the examples of the present invention was used to form a preform for precision press molding, and this preform for precision press molding was processed by precision press molding. In either case, the glass after heat softening did not suffer from problems such as opalescence and devitrification, and could be stably processed into various lens and prism shapes.
[0089] Although the present invention has been described in detail for purposes of illustration, it will be understood that the present embodiments are for illustrative purposes only and that numerous modifications may be made by those skilled in the art without departing from the spirit and scope of the invention.
Claims
1. In mass% based on oxide, La 2 O 3 Ingredients: 32.53% to 38.0%, WO 3 Ingredients: 0 to 0.77% TiO 2 Ingredients: 20.0% to 45.0% BaO content: 5.0% to 40.0% SiO 2 Ingredients: 0-6.21%, B 2 O 3 Ingredients: 6.95% to less than 15.0% ZnO content is 0 to 2.27%, and Nb 2 O 5 Ingredients: 0 to 7.31% or less Contains SiO 2 Ingredients and B 2 O 3 The total amount of components is 7.0% or more and 16.50% or less, Ln 2 O 3 The total content of components (wherein Ln is one or more selected from the group consisting of La, Gd, Y, and Yb) is 32.53% or more and less than 40.0%, TiO 2 / (La 2 O 3 +Nb 2 O 5 +Gd 2 O 3 +Yb 2 O 3 ) is 0.501 or more and 0.80 or less in mass ratio, TiO 2 / (TiO 2 +BaO) is 0.40 or more and 0.90 or less in mass ratio, The refractive index (nd) is 1.998 or more, the Abbe number (νd) is 30.0 or less, the partial dispersion ratio (θg, F) is 0.605 or more, and the wavelength (λ) at which the spectral transmittance is 5% is 5 ) is 375 nm or less.
2. In mass% based on oxide, Y 2 O 3 Ingredient 0~5.0%, Yb 2 O 3 Ingredients 0 to 5.0%, and G.D. 2 O 3 Ingredients 0-5.0% 2. The optical glass according to claim 1,
3. In mass% based on oxide, (La 2 O 3 +Nb 2 O 5 +Gd 2 O 3 +Yb 2 O 3 3. The optical glass according to claim 1, wherein the sum of the masses of said elements is 35.0% or more and 47.0% or less.
4. In mass% based on oxide, Rn 2 4. The optical glass according to claim 1, wherein the sum of the masses of O components (wherein Rn is one or more selected from the group consisting of Li, Na and K) is 15.0% or less.
5. In mass% based on oxide, 5. The optical glass according to claim 1, wherein the sum of the masses of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr and Ba) is from 7.0% to 35.0%.
6. A preform material made of the optical glass according to any one of claims 1 to 5.
7. 6. An optical element comprising the optical glass according to claim 1.
8. An optical instrument comprising the optical element according to claim 7.
Citation Information
Patent Citations
Optical glass, glass gob for press forming and optical element
JP2007022846A
Optical glass
JP2011178571A
Cullet, optical glass and method for producing them
JP2014084235A
glass
JP2015127281A
An optical glass and optical element
US20140287906A1