Rubber composition for tread and tire

A tailored rubber composition for automobile tires, using specific ratios of styrene-butadiene rubber, butadiene rubber, carbon black, and silica, addresses the imbalance in wear resistance and fuel efficiency by controlling tan δ values, resulting in enhanced wet grip and reduced rolling resistance.

JP7587343B2Active Publication Date: 2024-11-20SUMITOMO RUBBER INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2018194578
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-10-15
Publication Date
2024-11-20
Estimated Expiration
2038-10-15

AI Technical Summary

Technical Problem

Existing rubber compositions for automobile tires improve fuel efficiency but compromise wear resistance and wet grip performance due to excessive bonding between silica and rubber, and lack balanced performance across varying temperatures.

Method used

A rubber composition for treads containing specific ratios of styrene-butadiene rubber, butadiene rubber, carbon black, and silica, along with a silane coupling agent, is formulated to achieve tan δ values within certain ranges at different temperatures, ensuring optimal wet grip, wear resistance, and fuel efficiency.

Benefits of technology

The composition achieves improved overall tire performance by balancing wet grip, wear resistance, and fuel efficiency through controlled tan δ values, reducing rolling resistance and enhancing braking performance across dry and wet road conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587343000001
    Figure 0007587343000001
  • Figure 0007587343000002
    Figure 0007587343000002
  • Figure 0007587343000003
    Figure 0007587343000003
Patent Text Reader

Abstract

To provide a rubber composition for a tread excellent in overall performance including wet grip performance, low fuel consumption performance and abrasion resistance performance, and also to provide a tire equipped with a tread composed of the rubber composition for a tread.SOLUTION: A rubber composition for a tread includes, based on 100 pts.mass of a rubber component containing 60-85 mass% of styrene-butadiene rubber and 15-40 mass% of butadiene rubber: 1-40 pts.mass of carbon black; and 50-150 pts.mass of silica. The rubber composition for a tread satisfies following equations (Equation A) to (Equation C). A tire is equipped with a tread composed of the rubber composition for a tread. (Equation A) tan δ(0°C)≤0.60; (Equation B) tan δ(15°C)≤0.20; (Equation C) |tan δ(15°C)-tan δ(30°C)|≤0.08 (In the equations, the tan δ(0°C), tan δ(15°C) and tan δ(30°C) respectively denote tan δ at 0°C, 15°C and 30°C and at a dynamic strain amplitude of 0.5%.).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for a tread and a tire having a tread formed from the rubber composition. [Background technology]

[0002] In recent years, from the standpoint of resource conservation, energy conservation, and environmental protection, there has been a growing social demand for the reduction of carbon dioxide emissions, and various countermeasures for automobiles, such as weight reduction and the use of electrical energy, are being considered. For this reason, there is a demand to reduce the rolling resistance of automobile tires and improve fuel efficiency, and there is also a demand for improving performance such as wear resistance.

[0003] For example, Patent Document 1 proposes a method for reducing rolling resistance by using a diene rubber (modified rubber) modified with an organosilicon compound containing an amino group and an alkoxy group. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-344955 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the rubber composition of Patent Document 1, the reaction efficiency between silica and rubber is improved, improving fuel economy, but the bond between silica and rubber is too dense, leaving room for improvement in wear resistance. In addition, rubber compositions for automobile tires are required to have excellent wet grip performance from the standpoint of safety.

[0006] Therefore, an object of the present invention is to provide a rubber composition for a tread that is excellent in overall performance such as wet grip performance, fuel efficiency and abrasion resistance, and a tire having a tread formed from the rubber composition for a tread. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by providing a rubber composition for treads that contains a predetermined amount of carbon black and a predetermined amount of silica in 100 parts by mass of a rubber component containing a predetermined amount of styrene butadiene rubber and a predetermined amount of BR, and that has a tan δ at a dynamic strain amplitude of 0.5% at 0°C (hereinafter also referred to as tan δ(0°C)) of 0.60 or less, a tan δ at a dynamic strain amplitude of 0.5% at 15°C (hereinafter also referred to as tan δ(15°C)) of 0.20 or less, and satisfies |tan δ(15°C)-tan δ(30°C)|≦0.08, and have completed the present invention through further research. Note that tan δ(30°C) represents tan δ at a dynamic strain amplitude of 0.5% at 30°C.

[0008] That is, the present invention provides [1] 100 parts by mass of a rubber component containing 60 to 85% by mass, preferably 65 to 80% by mass, more preferably 70 to 75% by mass or 65 to 70% by mass of a styrene-butadiene rubber and 15 to 40% by mass, preferably 20 to 35% by mass, more preferably 25 to 30% by mass or 30 to 35% by mass of a butadiene rubber, 1 to 40 parts by mass, preferably 3 to 30 parts by mass, more preferably 5 to 20 parts by mass of carbon black, and Silica: 50 to 150 parts by mass, preferably 55 to 115 parts by mass, more preferably 60 to 100 parts by mass A rubber composition for a tread comprising the above-mentioned components and satisfying the following formulae (A) to (C): (Formula A) tan δ(0°C)≦0.60 (preferably 0.25≦tan δ(0°C)≦0.45, more preferably 0.25≦tan δ(0°C)≦0.40, and even more preferably 0.30≦tan δ(0°C)≦0.40) (Formula B) tan δ(15° C.)≦0.20 (preferably 0.11≦tan δ(15° C.)≦0.19, more preferably 0.13≦tan δ(15° C.)≦0.18, even more preferably 0.14≦tan δ(15° C.)≦0.18, and particularly preferably 0.14≦tan δ(15° C.)≦0.16) (Formula C) |tan δ(15°C)-tan δ(30°C)|≦0.08 (preferably 0.01≦|tan δ(15°C)-tan δ(30°C)|≦0.07, more preferably 0.02≦|tan δ(15°C)-tan δ(30°C)|≦0.06, and even more preferably 0.03≦|tan δ(15°C)-tan δ(30°C)|≦0.05) (tan δ(0°C), tan δ(15°C) and tan δ(30°C) represent tan δ at a dynamic strain amplitude of 0.5% at 0°C, 15°C and 30°C, respectively.) [2] The rubber composition for treads according to the above [1], which contains aluminum hydroxide. [3] The rubber composition for treads according to the above [1] or [2], which contains 10 to 80 parts by mass, preferably 15 to 70 parts by mass, and more preferably 20 to 60 parts by mass of oil per 100 parts by mass of the rubber component. [4] The rubber composition for tread according to any one of the above [1] to [3], which contains a silane coupling agent having a mercapto group, which is a compound represented by the following formula (1) and / or a compound containing a bond unit A represented by the following formula (2) and a bond unit B represented by the following formula (3): [ka] (In the formula, R 101 ~R 103 is a linear or branched alkyl group having 1 to 12 carbon atoms, a linear or branched alkoxy group having 1 to 12 carbon atoms, or -O-(R 111 -O) z -R 112 (z R 111 represents a linear or branched divalent hydrocarbon group having 1 to 30 carbon atoms. 111 may be the same or different. 112represents a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. z represents an integer of 1 to 30. R 101 ~R 103 may be the same or different. 104 represents a linear or branched alkylene group having 1 to 6 carbon atoms. [ka] [ka] (In the formula, x is an integer of 0 or more, and y is an integer of 1 or more. R 201 R represents a hydrogen atom, a halogen atom, a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, a linear or branched alkynyl group having 2 to 30 carbon atoms, or an alkyl group in which the terminal hydrogen atom has been substituted with a hydroxyl group or a carboxyl group. 202 R represents a linear or branched alkylene group having 1 to 30 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, or a linear or branched alkynylene group having 2 to 30 carbon atoms. 201 and R 202 may form a ring structure with [5] A tire having a tread made of the rubber composition for tread according to any one of [1] to [4] above. Regarding. Effect of the Invention

[0009] The rubber composition for treads of the present invention contains 100 parts by mass of a rubber component containing 60 to 85% by mass of styrene-butadiene rubber and 15 to 40% by mass of butadiene rubber, 1 to 40 parts by mass of carbon black and 50 to 150 parts by mass of silica, and satisfies tan δ(0°C) ≦ 0.60, tan δ(15°C) ≦ 0.20, and |tan δ(15°C) - tan δ(30°C) | ≦ 0.08. When used in a tire tread, the tire can be made to have excellent overall performance, such as wet grip performance, low fuel consumption performance, and wear resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The rubber composition for treads, which is one embodiment, is characterized in that it contains 100 parts by mass of a rubber component containing 60 to 85% by mass of styrene butadiene rubber and 15 to 40% by mass of butadiene rubber, 1 to 40 parts by mass of carbon black and 50 to 150 parts by mass of silica, and satisfies tan δ(0°C) ≦ 0.60 (formula A), tan δ(15°C) ≦ 0.20 (formula B), and |tan δ(15°C)-tan δ(30°C)| ≦ 0.08 (formula C). This characteristic allows the tire's overall performance, such as wet grip performance, fuel efficiency, and wear resistance, to be dramatically improved compared to a rubber composition using a similar blend. Specifically, it is believed that the RRC (rolling resistance coefficient) can be reduced by reducing the energy loss at a tire temperature of 30 to 40°C. In this case, it is believed that the wear resistance can be improved by lowering the glass transition temperature Tg by containing 15% by mass or more of BR. In this way, by satisfying the conditions tan δ(0°C) ≦ 0.60, tan δ(15°C) ≦ 0.20, and |tan δ(15°C) - tan δ(30°C)| ≦ 0.08, it is believed that even in a tire that uses an ultra-fuel-efficient compound, it is possible to achieve a lower RRC, i.e., lower fuel consumption, at the same level of tan δ(30°C), compared to compounds with higher tan δ values ​​or higher |tan δ(15°C) - tan δ(30°C)| values.

[0011] The tan δ(0°C) of the rubber composition for treads in one embodiment is 0.60 or less, preferably 0.45 or less, and more preferably 0.40 or less. If the tan δ(0°C) exceeds 0.60, fuel economy performance, particularly fuel economy performance in winter, may deteriorate. In addition, the tan δ(0°C) is preferably 0.25 or more, and more preferably 0.30 or more. By setting the tan δ(0°C) to 0.25 or more, there is a tendency that good wet grip performance can be obtained. Note that the tan δ(0°C) is a value obtained by the measurement method described in the examples described later.

[0012] The tan δ(15°C) of the rubber composition for treads in one embodiment is 0.20 or less, preferably 0.19 or less, more preferably 0.18 or less, and even more preferably 0.16 or less. If the tan δ(15°C) exceeds 0.20, fuel efficiency may deteriorate. In addition, the tan δ(15°C) is preferably 0.11 or more, more preferably 0.13 or more, and even more preferably 0.14 or more. By making the tan δ(15°C) 0.11 or more, there is a tendency that the necessary braking force on a dry road surface can be exerted. The tan δ(15°C) is a value obtained by the measurement method described in the examples described later.

[0013] In one embodiment, the rubber composition for treads has a value of |tan δ(15°C)-tan δ(30°C)| of 0.08 or less, preferably 0.07 or less, more preferably 0.06 or less, and even more preferably 0.05 or less. If |tan δ(15°C)-tan δ(30°C)| exceeds 0.08, the temperature dependency of energy loss increases, that is, the dependency of fuel efficiency on the temperature of the tire's operating environment may increase, and fuel efficiency tends to deteriorate in winter. In addition, |tan δ(15°C)-tan δ(30°C)| is preferably 0.01 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. By setting |tan δ(15°C)-tan δ(30°C)| to 0.01 or more, it tends to be possible to balance the braking performance on dry road surfaces and wet road surfaces. Note that |tan δ(15°C)-tan δ(30°C)| is a value obtained by a measurement method described in the examples described later.

[0014] In a rubber composition containing 100 parts by mass of a rubber component containing 60 to 85% by mass of styrene butadiene rubber and 15 to 40% by mass of butadiene rubber, 1 to 40 parts by mass of carbon black and 50 to 150 parts by mass of silica, tan δ(0°C) ≦ 0.60 (formula A), tan δ(15°C) ≦ 0.20 (formula B), and |tan δ(15°C)-tan δ(30°C)| ≦ 0.08 (formula C) can be satisfied by optimizing the Tg of the styrene butadiene rubber and butadiene rubber used, specifically, by selecting the tan δ peak temperature of the tread rubber composition compounded by combining these so that it is -9°C or less, or by adjusting the amount of other compounding agents such as oil, resin, etc., it is also possible to adjust it to -9°C or less by performing these compounding adjustments, and it can be performed by those skilled in the art without imposing an excessive burden.

[0015] (Rubber component) In one embodiment, the rubber component contains 60 to 85 mass% of styrene butadiene rubber (SBR) and 15 to 40 mass% of butadiene rubber (BR). In addition to SBR and BR, the rubber component may contain, for example, natural rubber (NR), deproteinized natural rubber (DPNR), highly purified natural rubber (HPNR), epoxidized natural rubber (ENR), isoprene rubber (IR), etc., but only SBR and BR are preferred.

[0016] (SBR) There are no particular limitations on the SBR, and examples thereof include solution-polymerized SBR (S-SBR), emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR). Modified SBRs include SBRs whose ends and / or main chains are modified, and modified SBRs (condensates, those having a branched structure, etc.) coupled with tin or silicon compounds. Of these, S-SBR is preferred. Furthermore, hydrogenated products of these SBRs (hydrogenated SBRs) and the like can also be used. These SBRs may be used alone or in combination of two or more.

[0017] Examples of S-SBR that can be used in this embodiment include S-SBR manufactured and sold by JSR Corporation, Ube Industries, Ltd., Asahi Kasei Corporation, ZS Elastomers Co., Ltd., and the like.

[0018] From the viewpoint of grip performance, the styrene content of SBR is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. If the styrene content is too high, styrene groups are adjacent to each other, the polymer becomes too hard, crosslinking is likely to be non-uniform, and blowability during high-temperature driving may deteriorate. In addition, temperature dependency increases, and performance changes due to temperature changes become large, and stable grip performance during driving and in the later stages tends not to be obtained. Therefore, the styrene content of SBR is preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. In this specification, the styrene content of SBR is 1 It is calculated by H-NMR measurement.

[0019] The vinyl bond amount of SBR is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more, from the viewpoints of ensuring reactivity with silica, rubber strength, and abrasion resistance. Also, the vinyl bond amount of SBR is preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less, from the viewpoints of preventing an increase in temperature dependency, grip performance, EB (durability), and abrasion resistance. In this specification, the vinyl bond amount of SBR (amount of 1,2-bonded butadiene units) is measured by infrared absorption spectroscopy.

[0020] The weight average molecular weight (Mw) of SBR is preferably 200,000 or more from the viewpoint of abrasion resistance and grip performance, more preferably 300,000 or more, even more preferably 400,000 or more, and particularly preferably 500,000 or more. From the viewpoint of crosslinking uniformity, Mw is preferably 2,000,000 or less, more preferably 150 or less, and even more preferably 1,000,000 or less. Mw can be calculated based on the measured value by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTPORE HZ-M manufactured by Tosoh Corporation) in terms of standard polystyrene.

[0021] The content of SBR in the rubber component is 60% by mass or more, preferably 65% ​​by mass or more, and more preferably 70% by mass or more. If the content of SBR in the rubber component is less than 60% by mass, the grip performance on wet road surfaces tends to be insufficient. Also, the content of SBR in the rubber component is 85% by mass or less, preferably 80% by mass or less, more preferably 75% by mass or less, and more preferably 70% by mass or less. If the content of SBR in the rubber component is more than 85% by mass, the abrasion resistance tends to be insufficient.

[0022] (BR) The BR is not particularly limited, and examples of the BR that can be used include those commonly used in the tire industry, such as BR having a cis 1,4 bond content of less than 50% (low cis BR), BR having a cis 1,4 bond content of 90% or more (high cis BR), rare earth butadiene rubber synthesized using a rare earth catalyst (rare earth BR), BR containing syndiotactic polybutadiene crystals (SPB-containing BR), and modified BR (high cis modified BR, low cis modified BR).

[0023] Examples of high cis BR include BR1220 manufactured by Zeon Corporation, BR130B, BR150B, and BR150L manufactured by Ube Industries, Ltd., and BR730 manufactured by JSR Corporation. By including high cis BR, low temperature properties and wear resistance can be improved. Examples of rare earth BR include BUNA-CB25 manufactured by Lanxess Corporation.

[0024] The SPB-containing BR is not one in which 1,2-syndiotactic polybutadiene crystals are simply dispersed in the BR, but one in which the 1,2-syndiotactic polybutadiene crystals are dispersed after being chemically bonded to the BR. Examples of such SPB-containing BR include VCR-303, VCR-412, and VCR-617 manufactured by Ube Industries, Ltd.

[0025] The modified BR is obtained by polymerizing 1,3-butadiene with a lithium initiator and then adding a tin compound, and includes those in which the terminals of the modified BR molecule are bonded with tin-carbon bonds (tin-modified BR), butadiene rubber having a condensed alkoxysilane compound at the active terminal of the butadiene rubber (silica-modified BR), etc. Examples of such modified BR include BR1250H (tin-modified) and S-modified polymer (silica-modified) manufactured by ZS Elastomer Co., Ltd.

[0026] The weight average molecular weight (Mw) of BR is preferably 300,000 or more, more preferably 400,000 or more, and even more preferably 450,000 or more, from the viewpoint of abrasion resistance and grip performance. Also, from the viewpoint of crosslinking uniformity, Mw is preferably 2,000,000 or less, more preferably 1,000,000 or less. Mw can be determined by standard polystyrene conversion based on the measured value by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTPORE HZ-M manufactured by Tosoh Corporation).

[0027] The content of BR in the rubber component is 15% by mass or more, preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. If the content of BR in the rubber component is less than 15% by mass, the abrasion resistance tends to be insufficient. Also, the content of BR in the rubber component is 40% by mass or less, preferably 35% by mass or less, and more preferably 30% by mass or less. If the content of BR in the rubber component exceeds 40% by mass, the grip performance on wet road surfaces tends to be insufficient.

[0028] (Carbon Black) The carbon black is not particularly limited, and GPF, FEF, HAF, ISAF, SAF, and other carbon blacks commonly used in the tire industry can be used. Specifically, N110, N115, N120, N125, N134, N135, N219, N220, N231, N234, N293, N299, N326, N330, N339, N343, N347, N351, N356, N358, N375, N539, N550, N582, N630, N642, N650, N660, N683, N754, N762, N765, N772, N774, N787, N907, N908, N990, N991, and the like can be suitably used. In addition to these, in-house synthesized products and the like can also be suitably used. These may be used alone or in combination of two or more.

[0029] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m from the viewpoint of weather resistance and reinforcement. 2 / g or more is preferable, and 80m 2 In addition, the N2SA of carbon black is preferably 250 m / g or more from the viewpoints of fuel economy, dispersibility, breakage characteristics and durability. 2 / g or less is preferable, and 220m 2 In this specification, the N2SA of carbon black is a value measured in accordance with Method A of JIS K 6217-2 "Basic properties of carbon black for rubber use - Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method".

[0030] The carbon black content is 1 part by mass or more, preferably 3 parts by mass or more, and more preferably 5 parts by mass or more, per 100 parts by mass of the rubber component. If the carbon black content is less than 1 part by mass, weather resistance cannot be ensured, and cracks due to ultraviolet rays may occur. In addition, the carbon black content is 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 15 parts by mass or less, per 100 parts by mass of the rubber component. If the carbon black content exceeds 40 parts by mass, sufficient fuel efficiency may not be achieved.

[0031] (silica) In one embodiment, silica is used. By blending silica, fuel economy, wear resistance, and wet grip performance can be improved. The silica is not particularly limited, and for example, silica prepared by a dry method (anhydrous silica), silica prepared by a wet method (hydrated silica), and other silicas commonly used in the tire industry can be used. Among them, hydrated silica prepared by a wet method is preferred because it has a large number of silanol groups. Silica may be used alone or in combination of two or more types.

[0032] The BET specific surface area of ​​silica is 80m from the viewpoint of durability and elongation at break. 2 / g or more is preferable, and 100m 2 / g or more is more preferable, and 150m 2 / g or more is more preferable, and 180m 2 From the viewpoints of fuel economy and processability, the BET specific surface area of ​​silica is preferably 300 m 2 / g or less is preferable, and 250m 2 The BET specific surface area of ​​silica in this specification is a value measured by the BET method in accordance with ASTM D3037-93.

[0033] The content of silica is 50 parts by mass or more, preferably 55 parts by mass or more, more preferably 60 parts by mass or more, relative to 100 parts by mass of the rubber component. If the content of silica is less than 50 parts by mass, the effect of improving fuel efficiency by blending silica tends to be insufficient, the effect of improving wear resistance tends to be insufficient, and grip performance on wet roads may not be sufficiently obtained. The content of silica is 150 parts by mass or less, preferably 115 parts by mass or less, more preferably 100 parts by mass or less, relative to 100 parts by mass of the rubber component. If the content of silica exceeds 150 parts by mass, the dispersibility of silica in the rubber may deteriorate, leading to a tendency for fuel efficiency and wear resistance to decrease, and the processability of the rubber may deteriorate, especially the viscosity may become too high, making processing difficult.

[0034] The rubber composition for tread according to one embodiment may contain, in addition to the above-mentioned components, compounding agents conventionally generally used in the tire industry, such as reinforcing fillers other than carbon black and silica, silane coupling agents, oils, tackifier resins, waxes, processing aids, various antioxidants, softeners, vulcanizing agents such as zinc oxide, stearic acid and sulfur, various vulcanization accelerators, etc., as appropriate.

[0035] (Other reinforcing fillers) As reinforcing fillers other than carbon black and silica, those conventionally used in rubber compositions for treads, such as aluminum hydroxide, calcium carbonate, alumina, clay, and talc, can be compounded.

[0036] (Aluminum Hydroxide) As the aluminum hydroxide, aluminum hydroxide generally used in the tire industry can be used, and examples thereof include Higilite (registered trademark) manufactured by Showa Denko K.K. and Apilar (registered trademark) manufactured by Navaltec Co., Ltd. The aluminum hydroxide in the present embodiment also includes alumina hydrate.

[0037] From the perspective of wet grip performance, the nitrogen adsorption specific surface area (N2SA) of aluminum hydroxide is 4m 2 / g or more is preferable, and 5m2 / g or more is preferable, and 6m 2 From the viewpoints of dispersibility of aluminum hydroxide, prevention of re-agglomeration, and wear resistance, the N2SA of aluminum hydroxide is preferably 50m 2 / g or less is preferable, and 45m 2 / g or less is more preferable, and 40m 2 / g or less is more preferable. In this specification, the N2SA of aluminum hydroxide is a value measured by the BET method in accordance with ASTM D3037-81.

[0038] The average particle size (D50) of aluminum hydroxide is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more, from the viewpoint of dispersibility of aluminum hydroxide, prevention of re-aggregation, and wear resistance. Also, the average particle size (D50) of aluminum hydroxide is preferably 3.0 μm or less, more preferably 2.0 μm or less, from the viewpoint of wear resistance. In this specification, the average particle size (D50) is the particle size at 50% of the cumulative mass value of the particle size distribution curve obtained by a particle size distribution measuring device.

[0039] When aluminum hydroxide is contained, the content per 100 parts by mass of the rubber component is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more. By making the content of aluminum hydroxide 3 parts by mass or more, wet grip performance tends to be good. Furthermore, when aluminum hydroxide is contained, the content per 100 parts by mass of the rubber component is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. By making the content of aluminum hydroxide 30 parts by mass or less, abrasion resistance tends to be good.

[0040] (Silane coupling agent) Since the rubber composition for tread according to one embodiment contains silica, it is preferable to use a silane coupling agent in combination. The silane coupling agent is not particularly limited, and any silane coupling agent that has been conventionally used in combination with silica in the tire industry can be used. Specific examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(4-trimethoxysilylbutyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-triethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)trisulfide, silane coupling agents having a sulfide group such as bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-trimethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazolyl tetrasulfide, and 3-trimethoxysilylpropyl methacrylate monosulfide;Silane coupling agents having a mercapto group, such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, Si363 manufactured by Evonik-Degussa, and NXT-Z30, NXT-Z45, and NXT-Z60 manufactured by Momentive; thioesters, such as 3-octanoylthio-1-propyltriethoxysilane, 3-hexanoylthio-1-propyltriethoxysilane, and 3-octanoylthio-1-propyltrimethoxysilane. Examples of the silane coupling agents include silane coupling agents having a vinyl group such as vinyltriethoxysilane; silane coupling agents having an amino group such as 3-aminopropyltriethoxysilane; silane coupling agents having a glycidoxy group such as γ-glycidoxypropyltriethoxysilane; silane coupling agents having a nitro group such as 3-nitropropyltrimethoxysilane; and silane coupling agents having a chloro group such as 3-chloropropyltrimethoxysilane, among which silane coupling agents having a mercapto group are preferred. These silane coupling agents may be used alone or in combination of two or more.

[0041] The silane coupling agent having a mercapto group is preferably a compound represented by the following formula (1) and / or a compound containing a bonding unit A represented by the following formula (2) and a bonding unit B represented by the following formula (3). [ka] (In the formula, R 101 ~R 103 is a linear or branched alkyl group having 1 to 12 carbon atoms, a linear or branched alkoxy group having 1 to 12 carbon atoms, or -O-(R 111 -O) z -R 112 (z R 111 represents a linear or branched divalent hydrocarbon group having 1 to 30 carbon atoms. 111 may be the same or different. 112represents a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. z represents an integer of 1 to 30. R 101 ~R 103 may be the same or different. 104 represents a linear or branched alkylene group having 1 to 6 carbon atoms. [ka] [ka] (In the formula, x is an integer of 0 or more, and y is an integer of 1 or more. R 201 R represents a hydrogen atom, a halogen atom, a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, a linear or branched alkynyl group having 2 to 30 carbon atoms, or an alkyl group in which the terminal hydrogen atom has been substituted with a hydroxyl group or a carboxyl group. 202 R represents a linear or branched alkylene group having 1 to 30 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, or a linear or branched alkynylene group having 2 to 30 carbon atoms. 201 and R 202 may form a ring structure.)

[0042] The compound represented by the above formula (1) will be described below.

[0043] R 101 ~R 103 is a linear or branched alkyl group having 1 to 12 carbon atoms, a linear or branched alkoxy group having 1 to 12 carbon atoms, or -O-(R 111 -O) z -R 112 In view of the fact that the desired effect can be satisfactorily obtained, R 101 ~R 103 has at least one -O-(R 111 -O) z -R 112Preferably, two of the groups are represented by -O-(R 111 -O) z -R 112 and one of them is a linear or branched alkoxy group having 1 to 12 carbon atoms.

[0044] R 101 ~R 103 Examples of the linear or branched alkyl group having 1 to 12 carbon atoms (preferably 1 to 5 carbon atoms) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, and a nonyl group.

[0045] R 101 ~R 103 Examples of the straight or branched alkoxy group having 1 to 12 carbon atoms (preferably 1 to 5 carbon atoms) include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an iso-butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, a 2-ethylhexyloxy group, an octyloxy group, and a nonyloxy group.

[0046] R 101 ~R 103 -O-(R 111 -O) z -R 112 In R 111 represents a linear or branched divalent hydrocarbon group having 1 to 30 carbon atoms (preferably 1 to 15 carbon atoms, more preferably 1 to 3 carbon atoms). Examples of the hydrocarbon group include a linear or branched alkylene group having 1 to 30 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, a linear or branched alkynylene group having 2 to 30 carbon atoms, and an arylene group having 6 to 30 carbon atoms. Of these, a linear or branched alkylene group having 1 to 30 carbon atoms is preferred.

[0047] R 111Examples of the linear or branched alkylene group having 1 to 30 carbon atoms (preferably 1 to 15 carbon atoms, more preferably 1 to 3 carbon atoms) include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, and an octadecylene group.

[0048] R 111 Examples of the straight-chain or branched alkenylene group having 2 to 30 carbon atoms (preferably 2 to 15 carbon atoms, more preferably 2 or 3 carbon atoms) include a vinylene group, a 1-propenylene group, a 2-propenylene group, a 1-butenylene group, a 2-butenylene group, a 1-pentenylene group, a 2-pentenylene group, a 1-hexenylene group, a 2-hexenylene group, and a 1-octenylene group.

[0049] R 111 Examples of the straight-chain or branched-chain alkynylene group having 2 to 30 carbon atoms (preferably 2 to 15 carbon atoms, more preferably 2 or 3 carbon atoms) include an ethynylene group, a propynylene group, a butynylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, and a dodecynylene group.

[0050] R 111 Examples of the arylene group having 6 to 30 carbon atoms (preferably 6 to 15 carbon atoms) include a phenylene group, a tolylene group, a xylylene group, and a naphthylene group.

[0051] z is an integer of 1 to 30, preferably 2 to 20, more preferably 3 to 7, and further preferably 5 or 6.

[0052] R 112represents a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. Of these, a linear or branched alkyl group having 1 to 30 carbon atoms is preferred.

[0053] R 112 Examples of the linear or branched alkyl group having 1 to 30 carbon atoms (preferably 3 to 25 carbon atoms, and more preferably 10 to 15 carbon atoms) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, and an octadecyl group.

[0054] R 112 Examples of the straight or branched alkenyl group having 2 to 30 carbon atoms (preferably 3 to 25 carbon atoms, more preferably 10 to 15 carbon atoms) include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-octenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, a tetradecenyl group, a pentadecenyl group, and an octadecenyl group.

[0055] R 112 Examples of the aryl group having 6 to 30 carbon atoms (preferably 10 to 20 carbon atoms) include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenyl group.

[0056] R 112 Examples of the aralkyl group having 7 to 30 carbon atoms (preferably 10 to 20 carbon atoms) include a benzyl group and a phenethyl group.

[0057] -O-(R 111 -O) z -R 112Specific examples of the group represented by the formula are, for example, -O-(C2H4-O)5-C 11 H 23 , -O-(C2H4-O)5-C 12 H 25 , -O-(C2H4-O)5-C 13 H 27 , -O-(C2H4-O)5-C 14 H 29 , -O-(C2H4-O)5-C 15 H 31 , -O-(C2H4-O)3-C 13 H 27 , -O-(C2H4-O)4-C 13 H 27 , -O-(C2H4-O)6-C 13 H 27 , -O-(C2H4-O)7-C 13 H 27 Among them, -O-(C2H4-O)5-C 11 H 23 , -O-(C2H4-O)5-C 13 H 27 , -O-(C2H4-O)5-C 15 H 31 , -O-(C2H4-O)6-C 13 H 27 is preferred.

[0058] R 104 Examples of the linear or branched alkylene group having 1 to 6 carbon atoms (preferably 1 to 5 carbon atoms) include R 111 Examples of the linear or branched alkylene group having 1 to 30 carbon atoms include the linear or branched alkylene group having 1 to 30 carbon atoms.

[0059] Examples of the compound represented by the above formula (1) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and the compound represented by the following formula (Si363 manufactured by Evonik-Degussa), and the compound represented by the following formula can be preferably used. These may be used alone or in combination of two or more kinds. [ka]

[0060] Next, a compound containing the linking unit A represented by the above formula (2) and the linking unit B represented by the above formula (3) will be described.

[0061] The compound containing the bond unit A represented by the above formula (2) and the bond unit B represented by the above formula (3) shows less increase in viscosity during processing than polysulfide silanes such as bis-(3-triethoxysilylpropyl)tetrasulfide. This is thought to be because the sulfide portion of the bond unit A is a CSC bond, which is more thermally stable than tetrasulfides and disulfides, and therefore the increase in Mooney viscosity is smaller.

[0062] In addition, the scorch time is suppressed compared to mercaptosilanes such as 3-mercaptopropyltrimethoxysilane. This is because the bond unit B has a mercaptosilane structure, but the -CH of the bond unit A is 15 This is thought to be because the -SH group of the bonding unit B is covered by this moiety, making it less likely to react with the polymer and less likely to cause scorch.

[0063] In terms of being able to enhance the effect of suppressing the increase in viscosity during processing and the effect of suppressing the shortening of the scorch time, in the silane coupling agent of the above structure, the content of the bond unit A is preferably 30 mol% or more, more preferably 50 mol% or more, preferably 99 mol% or less, and more preferably 90 mol% or less. The content of the bond unit B is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 10 mol% or more, preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 55 mol% or less. The total content of the bond units A and B is preferably 95 mol% or more, more preferably 98 mol% or more, and particularly preferably 100 mol%. The content of the bond units A and B includes the case where the bond units A and B are located at the ends of the silane coupling agent. When the bond units A and B are located at the ends of the silane coupling agent, the form is not particularly limited, and it is sufficient to form units corresponding to the formulas (2) and (3) representing the bond units A and B.

[0064] R 201 Examples of the halogen atom include a chlorine atom, a bromine atom, and a fluorine atom.

[0065] R 201 Examples of the linear or branched alkyl group having 1 to 30 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, etc. The number of carbon atoms of the alkyl group is preferably 1 to 12.

[0066] R 201 Examples of the linear or branched alkenyl group having 2 to 30 carbon atoms include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, and a 1-octenyl group. The number of carbon atoms of the alkenyl group is preferably 2 to 12.

[0067] R 201Examples of the linear or branched alkynyl group having 2 to 30 carbon atoms include an ethynyl group, a propynyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, an octynyl group, a nonynyl group, a decynyl group, an undecynyl group, a dodecynyl group, etc. The number of carbon atoms of the alkynyl group is preferably 2 to 12.

[0068] R 202 Examples of the linear or branched alkylene group having 1 to 30 carbon atoms include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, an octadecylene group, etc. The number of carbon atoms of the alkylene group is preferably 1 to 12.

[0069] R 202 Examples of the linear or branched alkenylene group having 2 to 30 carbon atoms include a vinylene group, a 1-propenylene group, a 2-propenylene group, a 1-butenylene group, a 2-butenylene group, a 1-pentenylene group, a 2-pentenylene group, a 1-hexenylene group, a 2-hexenylene group, and a 1-octenylene group. The number of carbon atoms of the alkenylene group is preferably 2 to 12.

[0070] R 202 Examples of the linear or branched alkynylene group having 2 to 30 carbon atoms include an ethynylene group, a propynylene group, a butynylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, a dodecynylene group, etc. The number of carbon atoms of the alkynylene group is preferably 2 to 12.

[0071] In the compound containing the bonding unit A represented by the above formula (2) and the bonding unit B represented by the above formula (3), the total number of repetitions (x+y) of the bonding unit A and the bonding unit B is preferably in the range of 3 to 300. Within this range, the mercaptosilane of the bonding unit B can be bonded to the -CH of the bonding unit A. 15Since the rubber component is covered with the silica, the scorch time can be prevented from being shortened and good reactivity with the silica and rubber components can be ensured.

[0072] Examples of compounds that can be used that contain the bond unit A represented by the above formula (2) and the bond unit B represented by the above formula (3) include NXT-Z30, NXT-Z45, and NXT-Z60 manufactured by Momentive Corp. These may be used alone or in combination of two or more kinds.

[0073] When the silane coupling agent is contained, the content relative to 100 parts by mass of silica is preferably 6 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more. By making the content of the silane coupling agent relative to 100 parts by mass of silica 6 parts by mass or more, there is a tendency that the improvement effect such as fuel efficiency is easily obtained, and the dispersibility of silica in rubber can be secured. In addition, when the silane coupling agent is contained, the content relative to 100 parts by mass of silica is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 15 parts by mass or less. By making the content of the silane coupling agent relative to 100 parts by mass of silica 20 parts by mass or less, there is a tendency that the decrease in rubber strength and abrasion resistance can be suppressed.

[0074] (oil) Examples of the oil include aromatic oil, process oil, mineral oil such as paraffin oil, etc. Among them, it is preferable to use process oil because of the reduction of the burden on the environment.

[0075] When oil is contained, the content per 100 parts by mass of the rubber component is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more. By making the content of oil 10 parts by mass or more, there is a tendency that the hardness required for a tire can be ensured and processability can be guaranteed. Furthermore, when oil is contained, the content per 100 parts by mass of the rubber component is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less. By making the content of oil 80 parts by mass or less, there is a tendency that the processability can be ensured.

[0076] (tackifier resin) Examples of tackifying resins include cyclopentadiene resins, coumarone resins, petroleum resins (aliphatic petroleum resins, aromatic petroleum resins, alicyclic petroleum resins, etc.), phenolic resins, rosin derivatives, etc., with aromatic petroleum resins being preferred.

[0077] Examples of aromatic petroleum resins include the following aromatic vinyl resins and C9 petroleum resins other than aromatic vinyl resins, with aromatic vinyl resins being preferred.

[0078] In the aromatic vinyl resin, for example, styrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene, 2,4,6-trimethylstyrene, etc. are used as the aromatic vinyl monomer (unit), and the resin may be either a homopolymer of each monomer or a copolymer of two or more monomers. In addition, the resin may be a modified one of these.

[0079] As the aromatic vinyl resin, α-methylstyrene or styrene homopolymer or α-methylstyrene and styrene copolymer is preferred, and α-methylstyrene and styrene copolymer is more preferred, because it is economical, easy to process, and has excellent wet grip performance.As the aromatic vinyl resin, for example, commercially available products such as SYLVARES SA85, SA100, SA120, SA140 manufactured by Arizona Chemical Company, and R2336 manufactured by Eastman Chemical Company are preferably used.As the copolymer of α-methylstyrene and styrene, for example, SYLVATRAXX4401 manufactured by Arizona Chemical Company are preferably used.

[0080] The softening point of the tackifier resin is preferably 40°C or higher, more preferably 60°C or higher. By setting the softening point to 40°C or higher, sufficient grip performance tends to be obtained. Moreover, the softening point is preferably 120°C or lower, more preferably 100°C or lower. By setting the softening point to 120°C or lower, sufficient grip performance tends to be obtained. In this specification, the softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point measuring device.

[0081] When a tackifier resin, particularly an aromatic vinyl resin, is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and particularly preferably 4 parts by mass or more, from the viewpoints of wet grip performance and dry grip performance. Also, when a tackifier resin, particularly an aromatic vinyl resin, is contained, the content per 100 parts by mass of the rubber component is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 35 parts by mass or less, and particularly preferably 10 parts by mass or less, from the viewpoints of abrasion resistance, fuel economy, and embrittlement fracture at low temperatures.

[0082] (Processing aids) Examples of processing aids include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, fatty acid esters, mixtures of fatty acid metal salts and amide esters, mixtures of fatty acid metal salts and fatty acid amides, etc. These may be used alone or in combination of two or more. Among them, fatty acid metal salts, amide esters, mixtures of fatty acid metal salts and amide esters or fatty acid amides are preferred, and mixtures of fatty acid metal salts and fatty acid amides are particularly preferred. Specifically, examples include fatty acid soap-based processing aids such as EF44 and WB16 manufactured by Struktol.

[0083] When a processing aid is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of improving processability, and when a processing aid is contained, the content per 100 parts by mass of the rubber component is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, from the viewpoints of abrasion resistance and breaking strength.

[0084] (Anti-aging agent) The antiaging agent is not particularly limited, and may be appropriately selected and blended from, for example, amine-based, quinoline-based, phenol-based, imidazole-based compounds, carbamic acid metal salts, etc., and these antiaging agents may be used alone or in combination of two or more. Among them, amine-based antiaging agents are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, N,N'-bis(1-methylheptyl)-p-phenylenediamine, N,N'-bis(1,4-dimethylpentyl)-p-phenylenediamine, More preferred are p-phenylenediamines such as N,N'-bis(1-ethyl-3-methylpentyl)-p-phenylenediamine, N-4-methyl-2-pentyl-N'-phenyl-p-phenylenediamine, N,N'-diaryl-p-phenylenediamine, hindered diaryl-p-phenylenediamine, phenylhexyl-p-phenylenediamine, and phenyloctyl-p-phenylenediamine, and among these, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine is particularly preferred.

[0085] When an antioxidant is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, and more preferably 0.8 parts by mass or more, from the viewpoint of exerting an antiaging effect. Also, when an antioxidant is contained, the content per 100 parts by mass of the rubber component is preferably 2.0 parts by mass or less, and more preferably 1.5 parts by mass or less, from the viewpoint of preventing browning of the rubber caused by the antioxidant.

[0086] (Softener) Examples of the softening agent include liquid polymers and low-temperature plasticizers. The plasticizer components may be used alone or in combination of two or more. Among them, it is preferable to use liquid polymers because they can improve abrasion resistance and grip performance in a well-balanced manner.

[0087] Examples of the liquid polymer include liquid SBR, liquid BR, liquid IR, liquid SIR, etc. Among them, it is preferable to use liquid SBR, since it can improve durability and grip performance in a well-balanced manner.

[0088] Examples of low-temperature plasticizers include liquid components such as dioctyl phthalate (DOP), dibutyl phthalate (DBP), tris(2-ethylhexyl) phosphate (TOP), and bis(2-ethylhexyl) sebacate (DOS).

[0089] When a softener is contained, the content thereof per 100 parts by mass of the rubber component is preferably 15 to 250 parts by mass, and more preferably 20 to 200 parts by mass, because a sufficient effect as a softener can be obtained.

[0090] In addition, the wax, zinc oxide, and stearic acid may be those conventionally used in the tire industry.

[0091] (Vulcanizing agent) The vulcanizing agent is not particularly limited, and any vulcanizing agent commonly used in the tire industry can be used. However, vulcanizing agents containing sulfur atoms are preferred, such as powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur, and insoluble sulfur.

[0092] The content of the vulcanizing agent per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.0 part by mass or more. Also, the content of the vulcanizing agent per 100 parts by mass of the rubber component is 3.0 parts by mass or less, preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less.

[0093] (Vulcanization accelerator) The vulcanization accelerator is not particularly limited, but examples thereof include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based or aldehyde-ammonia-based, imidazoline-based, and xanthate-based vulcanization accelerators. Among these, sulfenamide-based and thiuram-based vulcanization accelerators are preferred because they more suitably achieve the desired effects, and it is more preferable to use two of these accelerators in combination.

[0094] Examples of sulfenamide vulcanization accelerators include CBS (N-cyclohexyl-2-benzothiazylsulfenamide), TBBS (Nt-butyl-2-benzothiazylsulfenamide), N-oxyethylene-2-benzothiazylsulfenamide, N,N'-diisopropyl-2-benzothiazylsulfenamide, and N,N-dicyclohexyl-2-benzothiazylsulfenamide. Examples of thiazole vulcanization accelerators include 2-mercaptobenzothiazole and dibenzothiazolyl disulfide. Examples of thiuram vulcanization accelerators include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, and tetrabenzylthiuram disulfide (TBzTD). Examples of guanidine vulcanization accelerators include diphenylguanidine (DPG), di-orthotolylguanidine, and orthotolylbiguanidine. These may be used alone or in combination of two or more. Among these, the combination of CBS and TBzTD is particularly preferred since the desired effect can be more suitably obtained.

[0095] When a vulcanization accelerator is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more. The content per 100 parts by mass of the rubber component is preferably 8 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 6 parts by mass or less. By setting the content of the vulcanization accelerator within the above range, breaking strength and elongation tend to be secured.

[0096] (Method of manufacturing rubber composition for tread) The method for producing the rubber composition for tread is not particularly limited, and a known method can be used. For example, the rubber composition for tread can be produced by a method in which the components other than the vulcanizing agent and the vulcanization accelerator among the above-mentioned components are kneaded using a rubber kneading device such as an open roll, a Banbury mixer, a kneader, or an internal kneader (kneading step 1), and then the vulcanizing agent and the vulcanization accelerator are added and further kneaded (kneading step 2) to obtain an unvulcanized rubber composition for tread, which is then vulcanized (vulcanization step).

[0097] For example, in the kneading step 1, the mixture is kneaded at a discharge temperature of 150 to 160°C for 1 to 10 minutes, and then in the kneading step 2, a vulcanizing agent and a vulcanization accelerator are added and kneaded using an open roll or the like. In the vulcanization step, the mixture can be vulcanized at 150 to 170°C for 10 to 35 minutes, for example.

[0098] (tire) A tire according to one embodiment has a tread constituted by the above-mentioned rubber composition for a tread, and can be used for tires in general, such as tires for passenger cars, high-performance tires for passenger cars, heavy-duty tires for trucks and buses, tires for motorcycles, racing tires, etc. In this specification, the high-performance tire is a tire that is particularly excellent in grip performance, and is a concept that also includes racing tires used for racing vehicles.

[0099] (Tire manufacturing method) A tire having a tread made of the rubber composition for a tread can be manufactured by a normal method using the rubber composition for a tread. That is, an unvulcanized rubber composition obtained by blending the above-mentioned components with a rubber component as necessary is extruded according to the shape of the tread, laminated together with other tire components on a tire building machine, and molded by a normal method to form an unvulcanized tire, and the unvulcanized tire is heated and pressurized in a vulcanizer to manufacture a tire. EXAMPLES

[0100] The present invention will be described below based on examples, but the present invention is not limited to these examples.

[0101] The various chemicals used in the examples and comparative examples are listed below. SBR1: TRINSEO's SLR6430 (S-SBR, styrene content: 40% by mass, vinyl bond content: 18 mol%, Mw: 1.46 million, Tg: -39°C, oil-extended product containing 37.5 parts by weight of oil per 100 parts by weight of rubber component) SBR2: Modified SBR synthesized in Production Example 1 described later (styrene content: 38 mass%, vinyl bond content: 39 mol%, Mw: 800,000, Tg: -25°C) SBR3: Modified solution-polymerized SBR produced in Production Example 2 described below (styrene content: 42% by mass, vinyl bond content: 36% by mole, Mw: 800,000, Tg: -21°C) SBR4: Modified solution-polymerized SBR produced in Production Example 3 described later (styrene content: 30 mass%, vinyl bond content: 52 mol%, Mw: 250,000, Tg: -23°C) BR1: Modified BR produced in Production Example 4 described later (vinyl bond amount: 12 mol%, cis 1,4-content: 38%, Mw: 500,000) BR2: UBEPOL BR (registered trademark) 150B manufactured by Ube Industries, Ltd. (vinyl bond content: 1.5 mol%, cis-1,4-content: 97%, Mw: 440,000) Carbon black: Show Black N220 (N2SA:111m) manufactured by Cabot Japan Co., Ltd. 2 / g) Silica: Evonik Degussa Ultrasil 9000GR (BET: 240m 2 / g, CTAB: 200m 2 / g, pH: 6.9) Silane coupling agent: NXT-Z45 manufactured by Momentive (a copolymer of bond unit A and bond unit B (bond unit A: 55 mol %, bond unit B: 45 mol %)) Aluminum hydroxide: H-43 (N2SA: 6.7m) manufactured by Showa Denko K.K. 2 / g, average primary particle diameter: 800nm) Oil: VivaTec400 (TDAE oil, Tg: -58°C) manufactured by H&R Corporation Tackifying resin: Sylvares SA85 (α-methylstyrene / styrene resin, softening point: 85°C) manufactured by Arizona Chemical Co. Wax: Ozoace 0355 (paraffin-based) manufactured by Nippon Seiro Co., Ltd. Processing aid: Struktol WB16 (mixture of calcium salts of fatty acids, fatty acid monoethanolamides and esters of fatty acid monoethanolamides) from Schill & Seilacher Anti-aging agent: Antigen 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Sumitomo Chemical Co., Ltd. Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Stearic acid: Beads of stearic acid camellia manufactured by NOF Corporation Sulfur: HK-200-5 (powdered sulfur containing 5% oil) manufactured by Hosoi Chemical Industry Co., Ltd. Vulcanization accelerator (1): Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator (2): Sancerer TBZTD (Tetrabenzyl thiuram disulfide (TBzTD)) manufactured by Sanshin Chemical Industry Co., Ltd.

[0102] Production Example 1: Synthesis of SBR2 Two autoclaves with an internal volume of 10 liters, an inlet at the bottom and an outlet at the top, and an agitator and a jacket were connected in series as reactors, and butadiene, styrene, and cyclohexane were mixed in a predetermined ratio. This mixed solution was passed through a dehydration column filled with activated alumina, and after mixing with n-butyllithium in a static mixer to remove impurities, it was continuously fed from the bottom of the first reactor, and further 2,2-bis(2-oxolanyl)propane as a polar substance and n-butyllithium as a polymerization initiator were continuously fed from the bottom of the first reactor at a predetermined rate, respectively, and the temperature inside the reactor was maintained at 95°C. The polymer solution was continuously withdrawn from the top of the reactor and fed to the second reactor. The temperature of the second reactor was kept at 95°C, and a mixture of tetraglycidyl-1,3-bisaminomethylcyclohexane (monomer) and its oligomer component (hereinafter referred to as "modifier A") was added continuously at a specified rate as a 1000-fold diluted solution of cyclohexane to carry out a modification reaction. This polymer solution was continuously extracted from the reactor, and an antioxidant was continuously added using a static mixer. Furthermore, 25 parts by mass of Japan Energy extender oil NC140 per 100 parts by mass of the polymer was added to this polymer solution and mixed, and the solvent was then removed to obtain SBR2.

[0103] Production Example 2: Synthesis of SBR3 Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyl lithium was added to start polymerization. Polymerization was performed under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, 10 parts by mass of extender oil was added to 100 parts by mass of the polymer, and the solvent was removed by steam stripping. After drying with a hot roll adjusted to 110°C, SBR3 was obtained.

[0104] Production Example 3: Synthesis of SBR4 Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyllithium was added to initiate polymerization. Polymerization was carried out under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR4.

[0105] Preparation Example 4: Synthesis of BR1 <Preparation of Terminal Modifier B> In a nitrogen atmosphere, 23.6 g of 3-(N,N-dimethylamino)propyltrimethoxysilane (manufactured by Azmax Corporation) was placed in a 100 mL measuring flask, and anhydrous hexane (manufactured by Kanto Chemical Co., Ltd.) was added to make the total volume 100 mL to prepare modifier B.

[0106] <Preparation of modified BR> 18 L of n-hexane, 2000 g of butadiene, and 2 mmol of tetramethylethylenediamine (TMEDA) were added to a 30 L pressure vessel that had been thoroughly substituted with nitrogen, and the temperature was raised to 60°C. Next, 10.3 mL of butyl lithium was added, and the temperature was raised to 50°C and stirred for 3 hours. Next, 11.5 mL of modifier B was added and stirred for 30 minutes. After adding 15 mL of methanol and 0.1 g of 2,6-tert-butyl-p-cresol to the reaction solution, the reaction solution was placed in a stainless steel vessel containing 18 L of methanol to recover the aggregates. The obtained aggregates were dried under reduced pressure for 24 hours to obtain BR1.

[0107] Examples 1 to 15 and Comparative Examples 1 to 8 According to the compounding recipe shown in Table 1 or 2, the chemicals other than sulfur and vulcanization accelerator were kneaded for 1 to 10 minutes using a 1.7 L closed Banbury mixer until the discharge temperature reached 150 to 160 ° C., and a kneaded product was obtained. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained using a two-axis open roll, and the mixture was kneaded for 4 minutes until the temperature reached 105 ° C., and an unvulcanized rubber composition was obtained. The unvulcanized rubber composition obtained was press-vulcanized at 170 ° C. for 12 minutes to prepare a test rubber composition. In Tables 1 and 2, when the rubber component is oil-extended rubber, the amount of the rubber component excluding the oil content is described as the compounding amount of the rubber component such as "SBR1", and the oil content is listed as the compounding amount of "oil" by adding the TDAE oil content separately compounded.

[0108] In addition, the unvulcanized rubber composition was extruded into the shape of a tire tread using an extruder equipped with a nozzle of a predetermined shape, and then laminated together with other tire components to form an unvulcanized tire. A test tire (size: 195 / 65R15) was manufactured by press-vulcanizing the tire at 170°C for 12 minutes.

[0109] The vulcanized rubber compositions and test tires obtained in the respective Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Tables 1 and 2.

[0110] <tanδ> Using a spectrometer manufactured by Ueshima Seisakusho Co., Ltd., the tan δ of the vulcanized rubber composition was measured at a dynamic strain amplitude of 0.5%, a frequency of 10 Hz, and measurement temperatures of 0°C, 15°C, and 30°C.

[0111] <Wet grip performance> Wet grip performance was evaluated using a flat belt abrasion tester (FR5010 type) manufactured by Ueshima Seisakusho Co., Ltd. A cylindrical rubber test piece of each vulcanized rubber composition having a width of 20 mm and a diameter of 100 mm was used as a sample, and the slip ratio of the sample against the road surface was changed from 0 to 70% under the conditions of a speed of 20 km / h, a load of 4 kgf, and a road surface temperature of 20°C, and the maximum value of the friction coefficient detected at that time was read. The measurement results were expressed as an index using the following calculation formula. The higher the index, the better the wet grip performance. (Wet grip performance index) = (maximum value of friction coefficient of each formulation) / (maximum value of friction coefficient of Comparative Example 1)×100

[0112] <Wear resistance> The test tires were fitted to a 2000cc domestically produced FR vehicle and driven on a test course with a dry asphalt surface. The tire tread depth was measured after 10,000km of driving, and the distance traveled when the tire tread depth was reduced by 1mm was calculated and expressed as an index using the following formula. The higher the index, the better the wear resistance. (Wear resistance index) = (mileage for each formulation) / (mileage for Comparative Example 1) x 100

[0113] <Fuel efficiency index> A rectangular test piece measuring 4 mm in width, 50 mm in length and 2 mm in thickness was punched out from the sheet-like vulcanized rubber composition and used for testing. Using a spectrometer manufactured by Ueshima Seisakusho Co., Ltd., the loss tangent (tan δ) of the vulcanized rubber sheet was measured at a dynamic strain amplitude of 1%, a frequency of 10 Hz, and temperatures of 50°C and 22.5°C, and the reciprocal value of tan δ was expressed as an index (fuel economy index) with Comparative Example 1 being set at 100. The results obtained at 50°C and 22.5°C were designated fuel economy index A and B, respectively. The larger the value, the smaller the rolling resistance and the more excellent the fuel economy. (Fuel economy index) = (tan δ of Comparative Example 1) / (tan δ of each formulation) × 100

[0114] [Table 1]

[0115] [Table 2]

[0116] From the results of Tables 1 and 2, in Examples 1 to 15, which contain 100 parts by mass of a rubber component containing 60 to 85% by mass of SBR and 15 to 40% by mass of butadiene rubber, 1 to 40 parts by mass of carbon black, and 50 to 150 parts by mass of silica, and satisfy tan δ (0 ° C) ≦ 0.60, tan δ (15 ° C) ≦ 0.20, and | tan δ (15 ° C) - tan δ (30 ° C) | ≦ 0.08, the overall performance such as wet grip performance, wear resistance, and fuel economy is improved compared to Comparative Example 5, which has a high BR content, Comparative Example 6, which has a low BR content, Comparative Example 7, which has a low silica content, Comparative Example 8, which does not contain carbon black, and Comparative Examples 1 to 4, which do not satisfy at least any of tan δ (0 ° C) ≦ 0.60, tan δ (15 ° C) ≦ 0.20, and | tan δ (15 ° C) - tan δ (30 ° C) | ≦ 0.08 in the same formulation.

Claims

1. 100 parts by mass of a rubber component containing 60 to 85% by mass of styrene-butadiene rubber and 15 to 40% by mass of butadiene rubber, 1 to 40 parts by weight of carbon black, and Silica: 50 to 150 parts by weight A rubber composition for a tread containing the above-mentioned compound and satisfying the following formulae (A) to (C): The silica has a BET specific surface area of ​​180 m 2 / g or more. (Formula A) tan δ (0°C)≦0.60 (Formula B) tan δ (15°C)≦0.20 (Formula C) |tanδ(15℃)−tanδ(30℃)|≦0.08 (Tan δ (0° C.), tan δ (15° C.) and tan δ (30° C.) represent tan δ at a dynamic strain amplitude of 0.5% at 0° C., 15° C. and 30° C., respectively.)

2. The rubber composition for treads according to claim 1, which contains aluminum hydroxide.

3. 3. The rubber composition for treads according to claim 1, which contains 10 to 80 parts by mass of oil per 100 parts by mass of the rubber component.

4. The rubber composition for tread according to any one of claims 1 to 3, comprising a silane coupling agent having a mercapto group, which is a compound represented by the following formula (1) and / or a compound containing a bond unit A represented by the following formula (2) and a bond unit B represented by the following formula (3): 【Chemistry 1】 (In the formula, R 101 ~R 103 is a linear or branched alkyl group having 1 to 12 carbon atoms, a linear or branched alkoxy group having 1 to 12 carbon atoms, or -O-(R 111 -O) z -R 112 (z R 111 represents a linear or branched divalent hydrocarbon group having 1 to 30 carbon atoms. 111 may be the same or different. 112 represents a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms. z represents an integer of 1 to 30. 101 ~R 103 may be the same or different. 104 represents a linear or branched alkylene group having 1 to 6 carbon atoms. 【Chemistry 2】 【Chemistry 3】 (In the formula, x is an integer of 0 or more, and y is an integer of 1 or more. R 201 R represents a hydrogen atom, a halogen atom, a linear or branched alkyl group having 1 to 30 carbon atoms, a linear or branched alkenyl group having 2 to 30 carbon atoms, a linear or branched alkynyl group having 2 to 30 carbon atoms, or an alkyl group in which the terminal hydrogen atom has been substituted with a hydroxyl group or a carboxyl group. 202 R represents a linear or branched alkylene group having 1 to 30 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, or a linear or branched alkynylene group having 2 to 30 carbon atoms. 201 and R 202 may form a ring structure.)

5. A tire having a tread made of the rubber composition for a tread according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Modified diene-based rubber composition

    JP2000344955A

  • Rubber composition for use in tire, and pneumatic tire

    JP2011144349A

  • Rubber composition for tire, and pneumatic tire

    JP2011231303A

  • Pneumatic tire

    JP2016113051A

  • Rubber composition for tire outer layer and pneumatic tire

    JP2016204504A