Biodegradable paper container
A biodegradable paper container with a polylactic acid resin-containing layer on a paper base material addresses heat resistance and adhesiveness issues, ensuring stability and rapid biodegradation for disposable food containers.
Patent Information
- Application Number
- JP2020151886
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-10
- Filing Date
- 2020-09-10
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-09-10
AI Technical Summary
Existing biodegradable paper containers suffer from poor heat resistance and adhesiveness between the paper base material and biodegradable resin layer, leading to issues like peeling and delamination during heating, especially in microwave ovens.
A biodegradable paper container with a specific layer structure comprising a paper base material and a polylactic acid resin-containing layer, with a basis weight of 150-500 g/m² and a thickness of 10-55 μm, ensuring excellent adhesiveness and moldability, and high heat resistance.
The container maintains integrity during heating, preventing peeling and delamination, and ensures rapid biodegradation, making it suitable for disposable food containers.
Smart Images

Figure 0007587376000002 
Figure 0007587376000003 
Figure 0007587376000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel biodegradable paper container, and in particular to a disposable container that is heated and cooked in a microwave oven or the like. [Background technology]
[0002] In recent years, in order to reduce the environmental load, the distribution of various disposable containers made mainly of soil-degradable biodegradable plastics has been promoted. The advantage of using known biodegradable plastics is that they are decomposed into water and carbon dioxide by the self-purifying action of nature, disappear completely, and do not remain in the ground. In this respect, it is not only extremely preferable from the perspective of waste disposal, but also that even if they are incinerated, the combustion calories are about half or less compared to synthetic resins such as polyethylene, and disposal costs can be reduced.
[0003] Well-known representative examples of disposable paper containers include paper cups for beverages, whose base paper is a laminate of "plastic layer / paper" in which a plastic material is laminated on at least one side of a paper substrate, and paper cups for instant noodles that are heated and cooked in hot water. Most of the plastic materials used in the plastic layers of these base papers are non-biodegradable plastics. The reasons why these non-biodegradable plastics cannot be replaced by biodegradable plastics include not only cost and productivity, but also insufficient heat resistance. For this reason, containers made of biodegradable materials with improved heat resistance have been proposed.
[0004] For example, Patent Document 1 discloses a paper container having a bottom and a body made of a paper base material with a resin sheet on the inner surface, characterized in that the resin sheet is made of a biodegradable plastic that is uniaxially or biaxially stretched and has thermal adhesive properties.
[0005] Patent document 2 discloses a biodegradable container made by adhering a biodegradable film made primarily from plants to the inner surface of a molded food container made from non-wood fibers (reed, kenaf, sugar cane, corn). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-26143 A [Patent Document 2] JP 2008-18703 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, according to research by the present inventors, it has been confirmed that when a paper container such as that described in Patent Document 1 is filled with commercially available white sauce used in gratins and the like and heated in a microwave oven, the biodegradable resin layer peels off from the paper base material due to its poor heat resistance, and large air bubbles are generated in the biodegradable resin layer, making it difficult to withstand cooking with heat.
[0008] Furthermore, if the structure is such that a laminate with separate bottom and sides is bonded together, like a paper cup, problems such as delamination between the biodegradable resin layer and the paper base material are unlikely to occur. However, when a single laminate is processed into a single container shape by processing such as press molding, the laminate is pulled and squeezed during molding, which applies strong forces to it, and there is a risk that the biodegradable resin will peel off from the paper base material or pinholes or tears will occur due to the adhesion between the biodegradable resin layer and the paper base material, etc.
[0009] Therefore, a main object of the present invention is to provide a biodegradable paper container which has excellent adhesion between the paper base material and the biodegradable resin layer, excellent formability, and also high heat resistance. [Means for solving the problem]
[0010] As a result of extensive research into the problems of the prior art, the present inventors discovered that a container having a specific layer structure can achieve the above object, and thus completed the present invention.
[0011] That is, the present invention relates to the following biodegradable paper container. 1. A container comprising a laminate including a paper base material and a polylactic acid resin-containing layer on one or both sides of the paper base material, (1) The weight of the paper base material is 150 to 500 g / m 2 and (2) The thickness of the polylactic acid resin-containing layer is 10 to 55 μm. A biodegradable paper container characterized by the above. 2. The biodegradable paper container according to item 1, wherein the polylactic acid resin contained in the polylactic acid resin-containing layer has a biodegradability of 30 to 70%. 3. The biodegradable paper container according to item 1 or 2, wherein the polylactic acid resin content in the polylactic acid resin-containing layer is 80 to 100% by weight. 4. The biodegradable paper container according to any one of items 1 to 3, wherein the polylactic acid resin-containing layer is laminated on at least the inner surface of the container. 5. The biodegradable paper container described in any one of items 1 to 4, characterized in that the container is composed of a) a bottom portion, b) a side wall portion connected to the periphery of the bottom portion and rising upward, c) a flange portion connected to the upper end of the side wall portion and extending in a substantially horizontal direction, and d) a rolled rim portion connected to the outer periphery of the flange portion. 6. A method for producing a biodegradable paper container, comprising: (1) Weight per unit area: 150-500g / m 2 A step of laminating a polylactic acid resin-containing composition on at least one surface of the paper base material using a T-die extruder to a thickness of 10 to 55 μm to obtain a laminate; (2) A step of forming the laminate into a container shape having a recess by press molding. A method for producing a biodegradable paper container, comprising: Effect of the Invention
[0012] According to the present invention, it is possible to provide a biodegradable paper container that has excellent adhesion between a paper base material and a biodegradable resin layer, excellent formability, and also high heat resistance.
[0013] In particular, the combination of a paper base material with a specific basis weight and a specific polylactic acid resin-containing layer makes it difficult for the container itself (especially the polylactic acid resin-containing layer) to change or deteriorate even when the container is heated in a microwave oven or the like, so it is suitable for any type of content (heated or non-heated).
[0014] In addition, since the adhesion between the paper base material and the polylactic acid resin-containing layer is excellent, problems such as delamination during heating are unlikely to occur. Furthermore, since the occurrence of pinholes and the like that may occur during molding can be prevented, high reliability can be ensured as an integrally molded type container.
[0015] According to the manufacturing method of the present invention, a molten polylactic acid resin-containing composition is melt-extruded onto a specific paper substrate to produce a laminate, and then the laminate is molded, thereby making it possible to efficiently manufacture containers that have good adhesion between the paper substrate and the biodegradable resin layer, as described above.
[0016] The container of the present invention having such characteristics can be used as a container for storing various products, and can be particularly preferably used as a container in which both the container and the contents are heated (particularly by microwave oven). More specifically, the container can be particularly preferably used as tableware for cooking products (boxed lunches, side dishes, gratin, curry and rice, pasta, rice bowls, ramen, udon, soup, stew, coffee, juice, and other foods and beverages) in convenience stores, supermarkets, and the like. [Brief description of the drawings]
[0017] [Figure 1] 1 shows the layer configuration of a laminate used to manufacture the container of the present invention. [Diagram 2] 1 shows a cross-sectional configuration of a container according to an embodiment of the present invention. [Diagram 3] 1 shows a cross-sectional configuration of a container according to an embodiment of the present invention. [Figure 4] 1 shows an enlarged view of a flange portion of a container of the present invention. [Diagram 5] 1 shows an image of a paper container produced in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] 1. Biodegradable paper containers The biodegradable paper container of the present invention (container of the present invention) is a container comprising a paper base material and a laminate including a polylactic acid resin-containing layer on one or both sides of the paper base material, (1) The weight of the paper base material is 150 to 500 g / m 2 and (2) The thickness of the polylactic acid resin-containing layer is 10 to 50 μm. It is characterized by:
[0019] The laminate constituting the container of the present invention is a laminate containing a paper base material and a polylactic acid resin-containing layer on one or both sides of the paper base material. For example, FIG. 1 shows an example of a laminate. In the laminate 10 of FIG. 1A, a polylactic acid resin-containing layer 12 is laminated on one side of a paper base material 11. In the laminate 10' of FIG. 1B, polylactic acid resin-containing layers 12, 12' are laminated on both sides of a paper base material 11. In the laminate 10 or 10', other layers (e.g., adhesive layers, sealant layers, printed layers, etc.) may be appropriately formed between the paper base material and the polylactic acid resin-containing layer within a range that does not impede the effects of the present invention. Furthermore, other layers may be disposed, if necessary, on the other side of the surface of the paper base material that is not in contact with the polylactic acid resin-containing layer within a range that does not impede the effects of the present invention. Similarly, other layers may be disposed, if necessary, on the other side of the surface of the paper base material that is not in contact with the polylactic acid resin-containing layer within a range that does not impede the effects of the present invention.
[0020] The total thickness of the laminate is not particularly limited and can be appropriately set depending on the form of use, application, type of contents, etc., and can be within the range of, for example, about 160 to 700 μm, but is not limited thereto.
[0021] In addition, in the container of the present invention, when the laminate is molded, it is preferable to mold the polylactic acid resin-containing layer so as to be disposed on the inner surface of the container. A cross-sectional view of an example of the container of the present invention is shown in FIG. 2. In FIG. 2, the laminate 10 is molded into a concave shape (cup shape), and the polylactic acid resin-containing layer 12 is disposed on the inner surface (inner layer) of the container, and the paper base material 11 is disposed on the outside. That is, the contents filled in the container are disposed so as to be in direct contact with the polylactic acid resin-containing layer 12. In this case, even if the contents come into contact with the polylactic acid resin-containing layer, the polylactic acid resin-containing layer prevents the contents from touching the paper base material, so that the shape of the container can be effectively maintained at least during use.
[0022] Another embodiment of the container of the present invention is shown in Fig. 3. The container 20 in Fig. 3 is composed of a) a bottom portion B, b) a side wall portion S that is connected to the periphery of the bottom portion and rises upward, and c) a flange portion F that is connected to the upper end of the side wall portion and extends in a substantially horizontal direction. In the present invention, it is preferable that the container has a flange portion that projects outward in a horizontal direction around the entire periphery of the peripheral wall that constitutes the recess (cup). This structure not only increases the strength of the container, but also makes it easy to grasp the flange portion with the fingers even if the contents become hot after cooking, making it possible to carry the paper container.
[0023] The flange portion F of the container in FIG. 3 can be further processed to form a rolled edge portion. FIG. 4 shows an enlarged view of the flange portion F. In FIG. 4A, the flange portion F is formed to extend in a substantially horizontal direction. In contrast, as shown in FIG. 4B, the edge portion of the flange portion is processed to form the rolled edge portion R. That is, the present invention also includes a container that is composed of a) a bottom portion, b) a side wall portion that is connected to the periphery of the bottom portion and rises upward, c) a flange portion that is connected to the upper end of the side wall portion and extends in a substantially horizontal direction, and d) a rolled edge portion that is connected to the outer periphery of the flange portion. In this way, by providing the rolled edge portion, the strength of the container can be further increased.
[0024] In the container of the present invention, it is preferable that the above-mentioned a) to c) or the above-mentioned a) to d) have an integral structure. For example, it is preferable that the above-mentioned a) to c) or the above-mentioned a) to d) are not composed of separate members, but have a seamless structure. Such a structure can be produced by integrally molding the above-mentioned laminate into a container shape by a press molding method or the like.
[0025] The container of the present invention is not particularly limited as long as it has a shape capable of accommodating the contents, and is preferably a container molded in a concave shape to accommodate food (cooked food). Therefore, it can be used as, for example, a tray, a plate, a bowl, a paper cup, etc. The components of the container of the present invention (paper substrate, polylactic acid resin-containing layer, etc.) will be described below.
[0026] (1)Paper base material The paper substrate serves as a substrate for supporting the polylactic acid resin-containing layer, and at the same time, plays a role in ensuring the rigidity of the container.
[0027] The paper base material has a basis weight of 150 to 500 g / m 2 The weight is 150g / m 2 If the thickness is less than 500 g / m, the rigidity is poor when filled with foodstuffs, and the strength as a food container is insufficient. 2 If it exceeds this limit, moldability is significantly reduced, which not only increases the cost but also exceeds the specifications required for use as a food container or the like.
[0028] The paper substrate is not particularly limited as long as it has the above-mentioned basis weight, and various paper substrates used in known or commercially available paper containers can be used. For example, pure white roll paper, craft paper, parchment paper, ivory paper, Manila paper, card paper, cup paper, etc. can be used according to the desired application. In addition, recycled paper can be used as the paper.
[0029] The thickness of the paper base material is not limited as long as it satisfies the above-mentioned basis weight, and may be, for example, about 150 to 600 μm, but is not limited thereto.
[0030] (2) Polylactic acid resin-containing layer The polylactic acid resin-containing layer mainly functions to prevent or inhibit the penetration of the contents into the paper base material, and thus contributes to the shape retention of the container.
[0031] The content of the polylactic acid resin in the polylactic acid resin-containing layer is not particularly limited, but is usually 80 to 100% by mass, and preferably 90 to 98% by mass, and therefore may be, for example, 98 to 100% by mass.
[0032] In the present invention, one of the reasons for adopting polylactic acid resin as the main component in the polylactic acid resin-containing layer is its unique biodegradation mechanism. The biodegradation mechanism is thought to be that after decomposition proceeds to a molecular weight of about 10,000 by hydrolysis (more specifically, environmental factors of temperature 60°C or higher, humidity 80% or higher, and pH 8 or higher), the decomposition is accelerated by microorganisms, and finally decomposed into carbon dioxide and water. This shows that polylactic acid resin is as stable as non-biodegradable plastics unless it is exposed to high temperature and high humidity conditions for a certain period of time. Therefore, for example, when used as a food container, it is possible to obtain disposal characteristics with low environmental impact as quickly as possible while maintaining the service life or product life as long as possible in the general distribution process until the end consumer eats the food. In this respect, the container of the present invention can be suitably used as, for example, a one-way (disposable) food container, etc.
[0033] The polylactic acid resin may be either a homopolymer or copolymer formed by polymerization of lactic acid (at least one of L-lactic acid (L-form) and D-lactic acid (D-form)) via ester bonds, or a copolymer formed by polymerization of lactic acid and another copolymer component (for example, an acid component such as glycolic acid). In particular, in the present invention, a homopolymer or copolymer formed by polymerization of lactic acid (at least one of L-lactic acid and D-lactic acid) is preferred. In the present invention, one or more of these polylactic acid resins may be used.
[0034] When the polylactic acid resin is substantially composed of lactic acid, the monomer may be a) substantially only L-isomer, b) substantially only D-isomer, or c) both L- and D-isomers. In the present invention, a copolymer containing both L- and D-isomers is preferred, and a copolymer containing 1 to 10% by mass of D-isomer is more preferred. In general, L-isomer polylactic acid resins have superior mechanical properties, but if the resin is composed of only L-isomers, the structure may become brittle and the processability may become poor. Specifically, when polylactic acid is randomly copolymerized in the range of 1 to 10% by mass of D-isomer, the resin becomes soft, the crystallinity decreases, and the melting point decreases. This reduces brittleness and balances the physical properties such as processability, mechanical properties, and heat resistance as a container. Therefore, in the present invention, a copolymer composition containing 1 to 10% by mass of D-isomer and the remainder of L-isomer is preferred.
[0035] In the present invention, a polylactic acid resin having a melt flow rate (MFR: 210°C, 2.16 kg load) of 1 to 30 g / 10 min, particularly 3 to 20 g / 10 min, is preferred. This further improves processing stability when producing a laminate. If the MFR is less than 1 / 10 min, the extruder may stop due to an increase in the motor load during extrusion. If the MFR exceeds 30 g / 10 min, the processability may decrease due to an increase in neck-in and the occurrence of surging during high-temperature extrusion.
[0036] The polylactic acid resin itself having these characteristics can be a known or commercially available product, for example, Nature Works' "2003D", "2500HP", "4060D", etc.
[0037] The polylactic acid resin-containing layer may contain other components within the range that does not impair the effects of the present invention. For example, additives that improve various physical properties such as heat resistance, such as adipic acid ester mixtures, rosin-based mixtures, polyglycerin fatty acid esters, etc., may be used. In the present invention, it is preferable that the polylactic acid resin-containing layer is formed of a polylactic acid resin to which no additives are actively added, that is, a polylactic acid resin with high purity. Therefore, for example, a polylactic acid resin-containing layer having a polylactic acid resin content of 99 to 100% by mass can be preferably used.
[0038] In the present invention, the biodegradability of the polylactic acid resin contained in the polylactic acid resin-containing layer is not particularly limited, but is usually preferably about 30 to 70%, and more preferably 35 to 55%. If the biodegradability is less than 30%, the biodegradability is poor, and there is a risk that the resin will not decompose quickly even if it is disposed of in the natural environment after use as a container. On the other hand, if the biodegradability is more than 70%, the resin is easily decomposed, and there is a risk that the decomposition will proceed even during use as a container. The biodegradability of such a polylactic acid resin can be appropriately adjusted by the ratio of the linear structure and the branched structure of the polylactic acid resin in the polylactic acid resin-containing layer and the presence or absence of functional groups. Therefore, by controlling the biodegradability of the polylactic acid resin to 30% or more and 70% or less, it is possible to more reliably achieve both stability and disposal characteristics with less environmental load (i.e., rapid decomposition).
[0039] The biodegradation mechanism referred to here is generally quantified by a biodegradability test as specified in the Japanese Industrial Standards JIS K6953-1, -2. The value obtained here is also called "biodegradability" and indicates the proportion of organic matter decomposed by the action of microorganisms in a certain period of time as a percentage, and is an index of the ease of decomposition in the environment. Here, the biodegradability in the present invention complies with the above-mentioned JIS, but the test period is specified as 12 days in order to observe the tendency of early decomposition, and the biodegradability (decomposability) for that number of test days is shown.
[0040] The thickness of the polylactic acid resin-containing layer is not particularly limited, but is usually 10 to 55 μm, particularly 10 to 50 μm, and particularly preferably 15 to 45 μm. If the thickness is less than 10 μm, the heat resistance is insufficient from the viewpoint of heat capacity, and the anchoring effect to the paper is not obtained, which induces delamination during microwave cooking. If the thickness exceeds 55 μm, the processability of extrusion lamination is significantly reduced, which increases the cost, and also significantly reduces the container forming processability in press forming processing, for example, as described later.
[0041] In addition, the polylactic acid resin-containing layer may be one that is composed of one layer (single layer), or may be one that is composed of two or more layers of polylactic acid resin-containing layers laminated together. For example, when the polylactic acid resin-containing layer is composed of two or more layers by co-extrusion, different raw materials can be used for each layer, so that, for example, a polylactic acid resin-containing layer that has excellent adhesion to the paper substrate is arranged on the layer that contacts the paper substrate, and a polylactic acid resin-containing layer that has functions such as surface heat resistance and low-temperature sealability is arranged on the layer opposite to the side that contacts the paper substrate, thereby more reliably achieving both adhesion to the paper substrate and heat resistance as a container. In addition, by forming a composition of two or more layers by co-extrusion, it is possible to control the balance of melt viscosity between layers, which suppresses the increase in neck-in or the occurrence of surging, and is expected to stabilize and speed up the melt film.
[0042] The polylactic acid resin-containing layer is preferably an unstretched layer. If a stretched layer (film) is used, the desired heat resistance may not be obtained. For example, a laminate obtained by laminating a pre-stretched polylactic acid resin-containing film and a paper substrate by dry lamination may not have the desired heat resistance.
[0043] (3) Other layers The container of the present invention may appropriately contain any layer or component in addition to the above-mentioned paper substrate and polylactic acid resin-containing layer, as long as it does not completely inhibit cooking with heat or biodegradation. For example, a printed layer for providing information, patterns, illustrations, and other designs related to the contents or the paper container may be provided between the paper substrate and the polylactic acid resin-containing layer, or on the surface of the paper substrate. A sealant layer may also be provided on the flange.
[0044] In addition, as long as the polylactic acid resin-containing layer is laminated on at least one side of the paper base material, the polylactic acid resin-containing layer may be laminated on one side or both sides, and when the polylactic acid resin-containing layer is laminated on only one side of the paper base material, the surface on which the polylactic acid resin-containing layer is laminated may be the side on which the contents of the paper container are stored or the back side, but it is preferable that the polylactic acid resin-containing layer is laminated on the side on which the contents of the paper container are stored. This makes it possible to prevent a part of the contents from seeping into the paper base material even if the contents contain moisture or oil. In addition, it is possible to reduce the adhesion of the contents to the paper container and making them difficult to remove.
[0045] The container of the present invention is made of a biodegradable material and can therefore be suitably used, particularly as a disposable container (tableware).
[0046] The target contents are not particularly limited, and can be applied to various products in addition to food. Examples of food include food and beverages (prepared or processed foods such as lunch boxes, side dishes, doria, gratin, curry, pasta, udon, soba, rice bowls, ramen, soup, stew, and ice cream, and beverages such as water, coffee, tea, beer, wine, and juice). Therefore, the container can be widely used as a container for food and beverages such as fast food products and takeout products, as well as food and beverage containers used for eating and drinking in commercial facilities, hospitals, schools, outdoor activities, and the like.
[0047] The container of the present invention has excellent heat resistance and can be suitably used as a container for storing food to be heated. In particular, it can be advantageously used as a container to be heated in a microwave oven. Therefore, the container of the present invention can withstand heating for about 1 to 5 minutes at about 500 to 1000 W in a commercially available microwave oven.
[0048] 2. Manufacturing method of biodegradable paper containers The method for producing the container of the present invention is not particularly limited, but for example, the following method can be adopted. That is, a method for producing a biodegradable paper container, comprising the steps of: (1) Weight per unit area: 150-500g / m 2 A step of laminating a polylactic acid resin-containing composition onto at least one surface of the paper substrate using a T-die extruder to a thickness of 10 to 55 μm to obtain a laminate (lamination step); (2) A step of forming the laminate into a container shape having a recess by press molding (molding step). A method for producing a biodegradable paper container comprising the steps of:
[0049] Lamination process In the lamination process, the weight is 150 to 500 g / m 2 A polylactic acid resin-containing composition is laminated on at least one surface of the paper base material using a T-die extruder to a thickness of 10 to 55 μm (preferably 10 to 50 μm, more preferably 15 to 45 μm) to produce a laminate.
[0050] The T-die extruder may be any device capable of simultaneously extruding the molten polylactic acid resin-containing composition and the paper substrate into a sheet, and any known or commercially available device may be used. The laminate extruded by the T-die extruder is obtained as a laminate including the paper substrate and a polylactic acid resin-containing layer on one or both sides of the paper substrate.
[0051] When forming a polylactic acid resin-containing layer on both sides of a paper base material, any of the following methods can be used: a) a method in which a molten polylactic acid resin-containing composition is extruded so that it comes into contact with both sides of the paper base material; or b) a method in which a polylactic acid resin-containing layer is first formed on one side of the paper base material, and then the molten polylactic acid resin-containing composition is extruded so that it comes into contact with the other side of the paper base material.
[0052] The polylactic acid resin-containing composition contains, in addition to the polylactic acid resin, additives as necessary. Examples of the polylactic acid resin and additives include those described above in "1. Biodegradable paper containers."
[0053] Molding process In the molding step, the laminate is molded into a container shape having a recess by press molding.
[0054] The press molding method is not particularly limited, and the method and conditions used in molding publicly known or commercially available paper containers can be adopted. Also, it can be performed using a publicly known or commercially available press molding machine. For example, the laminate can be subjected to a press molding machine under heating at a temperature of 60 to 120°C and molded into a container shape.
[0055] The shape of the container is not limited as long as it is a concave shape that can accommodate the contents, and can be appropriately set depending on the type of contents, the purpose, the purpose of use, etc. For example, any shape such as a cup or a curry dish can be adopted. The size of the container is also not particularly limited, and can be appropriately set depending on the purpose, etc.
[0056] In addition, the molding process may further include a step of providing a flange portion and a rolled edge portion to the container of the present invention. These steps may also be carried out using a known or commercially available molding machine. EXAMPLES
[0057] The features of the present invention will be described in more detail below with reference to examples and comparative examples, although the scope of the present invention is not limited to the examples.
[0058] Example 1 Length 243cm x width 184cm, weight 260g / m 2 A commercially available polylactic acid resin (Nature Works "2003D", D-form content: 2-3.5% by mass, MFR: 6 (g / 10 min·210°C, 2.16 kg), biodegradability: 36%) was melt-extruded to a thickness of 30 μm onto one side of the paper using a commercially available T-die extruder to produce a base paper (laminate) in which a polylactic acid resin-containing layer was laminated on one side of the paper base.
[0059] Example 2 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin-containing layer was formed to a thickness of 10 μm.
[0060] Example 3 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin-containing layer was formed to a thickness of 20 μm.
[0061] Example 4 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin-containing layer was formed to a thickness of 40 μm.
[0062] Example 5 Paper 150g / m 2 A base paper was prepared in the same manner as in Example 1, except for the above.
[0063] Example 6 Paper 450g / m 2 A base paper was prepared in the same manner as in Example 1, except for the above.
[0064] Example 7 Paper 150g / m 2 A base paper was prepared in the same manner as in Example 1, except that the thickness of the polylactic acid resin-containing layer was 20 μm.
[0065] Example 8 Paper 150g / m 2A base paper was prepared in the same manner as in Example 1, except that the thickness of the polylactic acid resin-containing layer was 40 μm.
[0066] Example 9 Paper 450g / m 2 A base paper was prepared in the same manner as in Example 1, except that the thickness of the polylactic acid resin-containing layer was 20 μm.
[0067] Example 10 Paper 450g / m 2 A base paper was prepared in the same manner as in Example 1, except that the thickness of the polylactic acid resin-containing layer was 40 μm.
[0068] Example 11 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin was "4060D" (Nature Works, D-form content: 3 to 5% by mass), MFR: 10 (g / 10 min·210°C, 2.16 kg), biodegradability: 53%).
[0069] Example 12 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin was Total Corbion L175 (D-form content: 1% by mass or less), MFR: 8 (g / 10 min·210°C, 2.16 kg), and biodegradability: 11%).
[0070] Example 13 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin was Total Corbion's LX175 (D-form content: 4% by mass or less), MFR: 6 (g / 10 min 210°C, 2.16 kg), and biodegradability: 21%).
[0071] Comparative Example 1 A base paper was prepared in the same manner as in Example 1, except that the thickness of the polylactic acid resin-containing layer was set to 5 μm.
[0072] Comparative Example 2 A base paper was prepared in the same manner as in Example 1, except that the polylactic acid resin-containing layer was formed to a thickness of 60 μm.
[0073] Comparative Example 3 Paper 100g / m 2 A base paper was prepared in the same manner as in Example 1, except for the above.
[0074] Comparative Example 4 Paper 550g / m 2 A base paper was prepared in the same manner as in Example 1, except for the above.
[0075] Comparative Example 5 Length 243cm x width 184cm, weight 260g / m 2 The biodegradability of the paper alone was 78%.
[0076] Test Example 1 A blank sheet was obtained by punching the base paper of each Example and Comparative Example with a Thomson blade. This blank sheet was used to produce a paper container for curry dishes as shown in Figure 5 by a press molding method. Figure 5A is a photograph of the entire container, Figure 5B is a photograph of the container viewed from directly above, and Figure 5C is a photograph of the container viewed from directly to the side.
[0077] The containers were designed to be large enough to accommodate 150 g of commercially available white sauce to be used in the heat resistance evaluation test described below. In each case, the containers were molded so that the polylactic acid resin-containing layer was disposed on the inner surface (content-filled side) of the container. The base paper or its containers of each Example and Comparative Example were evaluated for (1) heat resistance, (2) adhesive strength, (3) moldability, and (4) stability and decomposability. The evaluation results are shown in Table 1. The evaluation methods are as follows.
[0078] (1) Heat resistance The container was filled with 150 g of commercially available white sauce (made by Heinz) and heated in a Sharp microwave oven (model number: RE-MA1-N) at 600 W for 3 minutes. After heating, the white sauce was removed from the container and visually checked for the presence or absence of boiling of the polylactic acid resin-containing layer of the container or peeling from the paper substrate. Those that did not show boiling or peeling from the paper substrate were marked with "○", and those that showed boiling or peeling from the paper substrate were marked with "×". Here, "boiling" refers to the phenomenon in which the polylactic acid resin-containing layer cannot withstand the heat generated by the white sauce when heated in the microwave oven, melts, and locally swells.
[0079] (2) Adhesive strength The base paper was cut into a width of 50 mm and a length of 150 mm, and a 180° peel test was performed with an autograph (R2KN-B) manufactured by Japan Measurement Systems Co., Ltd., with a gauge length of 200 mm and a peel speed of 100 mm / min. Those that did not peel between the paper layers in the paper substrate were marked with "X", and those that peeled between the paper layers were marked with "O". That is, the "X" means that the polylactic acid resin-containing layer and the paper substrate peeled between before the paper substrate itself peeled (broke), and the adhesion between the polylactic acid resin-containing layer and the paper substrate was low. On the other hand, the "O" means that the paper substrate itself peeled (broke) before the polylactic acid resin-containing layer and the paper substrate peeled between, and the adhesion between the polylactic acid resin-containing layer and the paper substrate was high.
[0080] (3) Formability The presence or absence of pinholes or tears was confirmed by spraying the inside of the container with Ageless Seal Check Liquid manufactured by Mitsubishi Gas Chemical Company, Inc. Three minutes after spraying the Ageless Check Liquid, the back of the container was visually inspected and those that had not been permeated with the Ageless Check Liquid were marked with an "O" and those that had been permeated with the Ageless Check Liquid were marked with an "X".
[0081] (4) Stability and decomposition Using a biodegradation measuring device (model: MODA-CS, manufactured by Yawata Bussan), the amount of CO2 generated (g), which indicates decomposition, was measured over a 12-day test period in accordance with the biodegradability test stipulated in the Japanese Industrial Standards JIS K6953-1, -2. The measurement sample used was a film (30 μm) of polylactic acid resin alone. The measurement procedure was to mix 10 g of polylactic acid resin cut to 3.5 mm x 3.5 mm into 500 g of compost, and conduct the test according to the method compliant with the above JIS standard. (4-1) Stability: After five days of testing, the CO2 emissions (120 hours) of 10g or less were marked as "Good," while those exceeding 10g were marked as "Poor." This is because, since the maximum expiration date of food stored in a container is generally about five days, those that generate more than 10g of CO2 may decompose too quickly and may not be suitable for practical use as food containers. (4-2) Degradability: The product with CO2 generation of 10g to 20g after 12 days of testing was marked as "Good", while the product with CO2 generation of less than 10g and the product with CO2 generation of more than 20g were marked as "Poor". If the product generated CO2 of less than 10g, the degradability was impaired, and if the product generated CO2 of more than 20g, as mentioned above, it may not be suitable for practical use as a food container.
[0082] [Table 1]
[0083] As is clear from the results in Table 1, the biodegradable paper container of the present invention has good heat resistance and good adhesion between the paper substrate and the polylactic acid resin-containing layer, even though the base paper is a laminate of a polylactic acid resin-containing layer / paper substrate. It is also clear that excellent containers such as those in each Example can be efficiently manufactured by press molding. In particular, Examples 1 to 11, which use a relatively high polylactic acid resin with a biodegradability of about 30 to 60%, show good results in terms of stability and degradability. That is, it is clear that the biodegradability test specified in JIS K6953-1, -2 shows that the amount of CO2 generated over 5 days is 10g or less, and the amount of CO2 generated over 12 days is 10 to 20g, which is suitable for disposable containers.
Claims
1. A container comprising a laminate including a paper base material and a polylactic acid resin-containing layer on one or both sides of the paper base material, (1) The weight of the paper base material is 150 to 500 g / m 2 and (2) The thickness of the polylactic acid resin-containing layer is 10 to 55 μm, (3) The polylactic acid resin contained in the polylactic acid resin-containing layer has a biodegradability of 30 to 70%; (4) The content of the polylactic acid resin in the polylactic acid resin-containing layer is 98 to 100% by mass. A biodegradable paper container characterized by the above.
2. 2. The biodegradable paper container according to claim 1, wherein the polylactic acid resin has a copolymer composition containing 1 to 10% by weight of D-lactic acid and the remainder being L-lactic acid.
3. A biodegradable paper container as described in claim 1 or 2, which is subjected to heating in a microwave oven.
4. The biodegradable paper container according to any one of claims 1 to 3, wherein the polylactic acid resin-containing layer is laminated on at least the inner surface of the container.
5. A biodegradable paper container according to any one of claims 1 to 4, characterized in that the container is composed of: a) a bottom portion; b) a side wall portion connected to the peripheral edge of the bottom portion and rising upward; c) a flange portion connected to the upper end of the side wall portion and extending in an approximately horizontal direction; and d) a rolled rim portion connected to the outer peripheral end of the flange portion.
6. A method for producing a biodegradable paper container, comprising the steps of: (1) Weight per unit area: 150 to 500 g / m 2 A step of laminating a composition containing 98 to 100% by mass of a polylactic acid resin having a biodegradability of 30 to 70% on at least one surface of the paper base material using a T-die extruder to a thickness of 10 to 55 μm to obtain a laminate; (2) A step of forming the laminate into a container shape having a recess by press molding. A method for producing a biodegradable paper container, comprising:
Citation Information
Patent Citations
Compostable coated paper or paperboard, process for making the same and products obtained therefrom
JP2002519222A
Paper container
JP2003026143A
Drawing-molded paper container and manufacturing method for the same
JP2004115054A
Wrap film
JP2006225043A
Biodegradability non-lumber fiber receptacle
JP2008018703A