Cationic electrodeposition coating composition
The cationic electrodeposition coating composition with a narrow molecular weight distribution and controlled elongation rates enhances adhesion and barrier properties, addressing the limitations of conventional paints for rust prevention.
Patent Information
- Application Number
- JP2020183783
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-02
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-11-02
AI Technical Summary
Conventional cationic electrodeposition paints lack sufficient adhesion and barrier properties, which are crucial for effective rust prevention in industrial applications.
A cationic electrodeposition coating composition is developed using an aminated epoxy resin with a molecular weight distribution of 2.7 or less, combined with a blocked polyisocyanate curing agent, and applied at a specific film thickness with controlled elongation rates to enhance adhesion and barrier properties.
The composition achieves improved corrosion resistance, adhesion, and barrier properties, ensuring effective rust prevention and film performance.
Smart Images

Figure 0007587394000001 
Figure 0007587394000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cationic electrodeposition coating composition, in particular to a cationic electrodeposition coating composition having high corrosion resistance. [Background technology]
[0002] Cationic electrocoating paints are widely used as undercoats to impart corrosion resistance to industrial products such as automobiles, and contain aminated epoxy resins and blocked polyisocyanate curing agents. In addition to high rust resistance, cationic electrocoating paints require high adhesion and high hydrophobicity (blocking properties).
[0003] The adhesion and hydrophobicity (blocking property) of cationic electrocoatings are important properties that contribute to rust prevention, and there is a constant demand for improvements. For example, JP-T-2000-501448 (Patent Document 1) discloses a cationic electrocoating composition that uses a diamine compound having a primary amino group and a tertiary amino group reacted with an epoxy resin, but further improvements are required in adhesion and blocking property. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2000-501448 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides a cationic electrodeposition coating composition which has improved adhesion and barrier properties of a coating film obtained from the cationic electrodeposition coating composition compared to conventional compositions, thereby providing an improved anti-rust property. [Means for solving the problem]
[0006] That is, the present invention provides the following aspects: [1] A cationic electrodeposition coating composition containing an aminated epoxy resin and a blocked polyisocyanate curing agent, the aminated epoxy resin is obtained by reacting an amine compound with an epoxy resin, the molecular weight distribution of the aminated epoxy resin is 2.7 or less; The cationic electrodeposition coating composition is applied onto a steel plate so that the cured film thickness is 20 μm, and after baking at 160° C. for 15 minutes, the elongation of the electrodeposition coating film is 0.1 to 4.5%. Cationic electrodeposition coating composition. [2] The amine compound is a combination of two types of amines, a primary amine and a secondary amine, The primary amine is a compound of the formula: NH2-(CH2)n-NR 1 R 2 (1) (In formula (1), R 1 and R 2 are the same or different and represent an alkyl group having 1 to 6 carbon atoms which may have a hydroxyl group at its terminal, and n represents an integer of 2 to 4. having The secondary amine has the formula: R 3 R 4 NH (2) (In formula (2), R 3 and R 4 represents an alkyl group having 1 to 4 carbon atoms and a hydroxyl group at its terminal. The cationic electrodeposition coating composition according to [1], [3] The tertiary amine ratio of the amine compound when obtaining the aminated epoxy resin is 85% or more. The cationic electrodeposition coating composition according to [1] or [2]. [4] A cationic electrodeposition coating film formed using the cationic electrodeposition coating composition according to any one of [1] to [3]. Effect of the Invention
[0007] The cationic electrodeposition coating composition of the present invention contains an aminated epoxy resin and a blocked polyisocyanate curing agent, and is characterized in that the aminated epoxy resin has a molecular weight distribution of 2.7 or less, and the cationic electrodeposition coating composition is applied to a steel plate so that the cured film thickness is 20 μm, and the elongation of the electrodeposition coating film after baking at 160 ° C for 15 minutes is 0.1 to 4.5%. The narrow molecular weight distribution of the aminated epoxy resin of 2.7 or less reduces side reactions in the reaction between the epoxy resin and the amine compound, and an aminated epoxy resin with a desired structure is obtained, which makes it possible to exhibit its performance (specifically, corrosion resistance, etc.). In addition, the elongation of the electrodeposition coating film is 0.1 to 4.5%, which is within the range of elongation required for the electrodeposition coating film to exhibit its performance, and therefore it can exhibit corrosion resistance, adhesion, and blocking properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The cationic electrodeposition coating composition of the present invention contains an aminated epoxy resin and a blocked polyisocyanate curing agent, the aminated epoxy resin being obtained by reacting an amine compound with an epoxy resin, the molecular weight distribution of the aminated epoxy resin being 2.7 or less, and the cationic electrodeposition coating composition being applied to a steel plate so that the cured film thickness is 20 μm and baked at 160° C. for 15 minutes, the elongation of the electrodeposition coating film being 0.1-4.5%. In this specification, when a numerical range is expressed as "a-b" (a and b both represent numerical values), it means a or more and b or less.
[0009] <Aminified epoxy resin> Aminated epoxy resins are film-forming resins that form electrodeposition coatings. Aminated epoxy resins are obtained by modifying the oxirane rings (also called "epoxy groups") of epoxy resins with amine compounds, i.e., by aminating them.
[0010] The starting epoxy resin is a polyphenol polyglycidyl ether type epoxy resin, which is a reaction product of a polycyclic phenol compound such as bisphenol A, bisphenol F, bisphenol S, phenol novolac, or cresol novolac with epichlorohydrin. In this specification, the term "polyphenol polyglycidyl ether type epoxy resin" includes a state in which a polyphenol polyglycidyl ether type epoxy resin and a polycyclic phenol compound have reacted (chain extension reaction). In this amine modification step, it is preferable to use an epoxy resin in which a polyphenol polyglycidyl ether type epoxy resin and a polycyclic phenol compound have reacted (chain extension reaction). The reaction conditions for the chain extension reaction of the polyphenol polyglycidyl ether type epoxy resin and the polycyclic phenol compound can be appropriately selected depending on the stirring device and reaction scale used. Examples of reaction conditions include conditions in which the reaction is performed at 85 to 180°C for 0.1 to 8 hours, and more preferably at 100 to 150°C for 2 to 8 hours. As the stirring device used, a stirring device generally used in the paint field can be used.
[0011] Other examples of starting resins include the oxazolidone ring-containing epoxy resins described in JP-A-5-306327. These epoxy resins can be prepared by reacting epichlorohydrin with a diisocyanate compound or a bis-urethane compound obtained by blocking the isocyanate group of a diisocyanate compound with a lower alcohol such as methanol or ethanol.
[0012] Before the amine modification, a part of the epoxy resin may be chain-extended with a bifunctional polyester polyol, polyether polyol (e.g., a polyol having a polyethylene oxide group, a polyol having a polypropylene oxide group, etc.), a dibasic carboxylic acid, or the like. For example, when a polyol having a polypropylene oxide group is used for the chain-extension reaction, a polypropylene oxide group-containing epoxy resin is obtained. An example of this embodiment is a state in which a polyphenol polyglycidyl ether type epoxy resin, a polycyclic phenol compound, and a polypropylene oxide group-containing epoxy resin are reacted (chain-extension reaction). When the epoxy resin to be reacted with the amine compound in the amine modification step contains a polypropylene oxide group-containing epoxy resin, the content of the polypropylene oxide group-containing epoxy resin is preferably 1 to 40 parts by mass, more preferably 15 to 25 parts by mass, relative to 100 parts by mass of the epoxy resin.
[0013] In general, the oxirane ring of the epoxy resin is reacted with an amine compound to obtain an aminated epoxy resin. As the amine compound, an amine compound generally used in producing an aminated epoxy resin is used. Examples of commonly used amine compounds include primary amines such as butylamine, octylamine, and monoethanolamine; secondary amines such as diethylamine, dibutylamine, methylbutylamine, diethanolamine, and N-methylethanolamine; and complex amines such as diethylenetriamine. The primary amines can be formed into ketimine groups using ketone compounds to control the reaction by so-called blocking. Examples of amine compounds having a ketimine group or diketimine group that can be used include ketimine of aminoethylethanolamine and diketimine of diethylenetriamine. Examples of ketone compounds that generate ketimine groups include methyl isopropyl ketone (MIPK), diisobutyl ketone (DIBK), methyl isobutyl ketone (MIBK), diethyl ketone (DEK), ethyl butyl ketone (EBK), ethyl propyl ketone (EPK), dipropyl ketone (DPK), and methyl ethyl ketone (MEK), with methyl isobutyl ketone (MIBK) being preferred. As the amine compound, a tertiary amine may be used, and specific examples thereof include, for example, triethylamine, N,N-dimethylbenzylamine, and N,N-dimethylethanolamine. These amines may be used alone or in combination of two or more.
[0014] In the present invention, the molecular weight distribution of the aminated epoxy resin must be controlled to 2.7 or less. In order to control the molecular weight distribution, the selection of a specific amine compound makes it easier to control the molecular weight distribution. Specifically, the amine compound is a combination of two types of amines, a primary amine and a secondary amine, and The primary amine is a compound of the formula: NH2-(CH2)n-NR 1 R 2 (1) (In formula (1), R 1 and R 2are the same or different and represent an alkyl group having 1 to 6 carbon atoms which may have a hydroxyl group at its terminal, and n represents an integer of 2 to 4. having The secondary amine has the formula: R 3 R 4 NH (2) (In formula (2), R 3 and R 4 represents an alkyl group having 1 to 4 carbon atoms and a hydroxyl group at its terminal. It is preferable to use those having the following structure. When these amine compounds are used, the primary amino group of the primary amine reacts with the epoxy resin and is consumed, leaving only the secondary amino group, which reacts with the epoxy group of the epoxy resin. Therefore, the reaction proceeds evenly without superiority or inferiority in reactivity, and it is believed that the molecular weight distribution can be controlled. It is also possible that the tertiary amino group present in the primary amine or the tertiary amino group generated by the reaction of the secondary amino group reacts with the epoxy group to become a quaternary ammonium group, but this reaction is thought to occur infrequently.
[0015] The primary amine has the formula (1) above, R 1 and R 2 Specifically, n is methyl, ethyl, propyl or butyl, and may have a hydroxyl group at the end. In addition, n is 2 to 4, and preferably 3. Specific examples of the primary amine include aminopropyldiethanolamine, dimethylaminopropanediamine, diethylaminopropanediamine, and dibutylaminopropanediamine. The secondary amine is a secondary amine having the above formula (2), but has R attached to a nitrogen atom. 3 and R 4 is combined, and R 3 and R 4 Both of them have a hydroxyl group-containing alkyl group having 1 to 4 carbon atoms. Specific examples of the secondary amine include dimethanolamine and diethanolamine.
[0016] In the amine modification step, the amount of the amine compound reacted with the epoxy resin is preferably 0.9 to 1.2 equivalents per equivalent of the epoxy group of the epoxy resin. When the amine compound is a primary amine and a secondary amine as described above, the amount of the primary amine is 30 to 80% by weight, more preferably 40 to 70% by weight, of the total amine compounds. If the amount of the primary amine exceeds 80% by weight of the total amine compounds, the viscosity of the resin increases, making stirring difficult, and if it is less than 30% by weight, the stability of the emulsion decreases.
[0017] The reaction conditions for reacting the epoxy resin with the amine compound to modify it with an amine can be appropriately selected depending on the reaction scale, etc. Examples of the reaction conditions include reaction at 80 to 150° C. for 0.1 to 5 hours, and more preferably reaction at 120 to 150° C. for 0.5 to 3 hours.
[0018] The number average molecular weight of the aminated epoxy resin is preferably in the range of 1,000 to 7,000. By having a number average molecular weight of 1,000 or more, the physical properties such as solvent resistance and corrosion resistance of the obtained cured electrodeposition coating film become good. On the other hand, by having a number average molecular weight of 7,000 or less, the viscosity of the aminated epoxy resin can be easily adjusted, making smooth synthesis possible, and the emulsion dispersion of the obtained aminated epoxy resin can be easily handled. The number average molecular weight of the aminated epoxy resin is more preferably in the range of 1,500 to 4,000.
[0019] In the present invention, the molecular weight distribution of the aminated epoxy resin must be 2.7 or less, preferably 2.5 or less. The molecular weight distribution means the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn), Mw / Mn. The average molecular weight and molecular weight distribution are polystyrene equivalent weight average molecular weights measured by gel permeation chromatography. If the molecular weight distribution of the aminated epoxy resin exceeds 2.7, many side reactions occur in the reaction between the epoxy resin and the amino compound, and the intended performance of the aminated epoxy resin may not be achieved.
[0020] In order to control the molecular weight distribution of the aminated epoxy resin to 2.7 or less, as described above, it is preferable to use a combination of a primary amine and a secondary amine as the amine compound, but this can also be achieved by controlling the reaction temperature, reaction time, etc. For example, when the reaction temperature is less than 120°C or exceeds 180°C, the molecular weight distribution tends to become high.
[0021] In the amine compound of the above aminated epoxy resin, the primary amino group reacts to form a secondary amino group and then a tertiary amino group, and the tertiary amine conversion rate must be 85% or more. The tertiary amine conversion rate is calculated as tertiary amine value / total amine value x 100 and expressed as a percentage. The tertiary amine value refers to the amount of potassium hydroxide (mg) equivalent to the perchloric acid required to neutralize the tertiary amine contained in 1 g of sample. It is measured according to the following method in accordance with ASTM D2073.
[0022] Tertiary amine value test method (1) Weigh the sample into a 100 ml beaker. (2) Add 0.5g of pure water. (3) Dissolve the above sample in 50 g of THF (tetrahydrofuran). (4) Stir for 5 minutes. (5) Next, add 7.5 ml of acetic anhydride and 2.5 ml of acetic acid and stir at about 40°C for 5 minutes. (6) Using an automatic potentiometric titrator, titrate with 0.1N perchloric acid acetic acid solution. (7) Measure the tertiary amine value using the following formula. Tertiary amine value = (titer amount mL × factor × 10) / (sample amount g × solids amount)
[0023] Total Amine Number Test Method (1) Accurately weigh out 500 mg of sample into a 200 ml Erlenmeyer flask. (2) Add approximately 50 ml of glacial acetic acid and dissolve uniformly. (3) Add 5 to 6 drops of indicator methyl violet solution and mix uniformly. (4) Titrate with 0.1N perchloric acid and acetic acid solution, and the endpoint is when the solution turns bright green. (The above (3) and (4) can also be performed by potentiometric titration.)
[0024] The amine value of the aminated epoxy resin (same as the total amine value above) is preferably within the range of 20 to 100 mgKOH / g. When the amine value of the aminated epoxy resin is 20 mgKOH / g or more, the emulsion dispersion stability of the aminated epoxy resin in the electrodeposition coating composition is good. On the other hand, when the amine value is 100 mgKOH / g or less, the amount of amino groups in the cured electrodeposition coating film becomes appropriate, and there is no risk of reducing the water resistance of the coating film. The amine value of the aminated epoxy resin is more preferably within the range of 20 to 80 mgKOH / g.
[0025] The tertiary amine conversion rate of aminated epoxy resin is also related to the electrical conductivity of the electrodeposition coating composition. When the tertiary amine conversion rate decreases, the electrical conductivity increases and the gas pinning property deteriorates. The electrical conductivity of the electrodeposition coating composition is 1500 to 2000 μS / cm 2 If the electrical conductivity is less than 1500, the throwing power decreases, and if it exceeds 2000, the gas pinning property becomes poor and the appearance of the coating surface deteriorates. The electrical conductivity can be measured using a commercially available electrical conductivity meter.
[0026] The hydroxyl value of the aminated epoxy resin is preferably within the range of 150 to 650 mgKOH / g. When the hydroxyl value is 150 mgKOH / g or more, the cured electrodeposition coating film is cured well, and the coating film appearance is improved. On the other hand, when the hydroxyl value is 650 mgKOH / g or less, the amount of hydroxyl groups remaining in the cured electrodeposition coating film becomes appropriate, and there is no risk of reducing the water resistance of the coating film. The hydroxyl value of the aminated epoxy resin is more preferably within the range of 150 to 400 mgKOH / g.
[0027] In the electrodeposition coating composition of the present invention, by using an aminated epoxy resin having a number average molecular weight in the range of 1,000 to 7,000, an amine value of 20 to 100 mgKOH / g, and a hydroxyl value of 150 to 650 mgKOH / g, more preferably 150 to 400 mgKOH / g, there is an advantage in that excellent corrosion resistance can be imparted to the substrate.
[0028] As the aminated epoxy resin, aminated epoxy resins having different amine values and / or hydroxyl values may be used in combination as necessary. When two or more aminated epoxy resins having different amine values and hydroxyl values are used in combination, the average amine value and average hydroxyl value calculated based on the mass ratio of the aminated epoxy resins used are preferably in the above-mentioned numerical range. As the aminated epoxy resins to be used in combination, it is preferable to use an aminated epoxy resin having an amine value of 20 to 50 mgKOH / g and a hydroxyl value of 50 to 300 mgKOH / g in combination with an aminated epoxy resin having an amine value of 50 to 200 mgKOH / g and a hydroxyl value of 200 to 500 mgKOH / g in combination. When such a combination is used, there is an advantage that the core part of the emulsion becomes more hydrophobic and the shell part becomes hydrophilic, thereby imparting excellent corrosion resistance.
[0029] The aminated epoxy resin may contain an amino group-containing acrylic resin, an amino group-containing polyester resin, or the like, as necessary.
[0030] <Blocked polyisocyanate curing agent> A blocked polyisocyanate curing agent (hereinafter, sometimes simply referred to as a "curing agent") is a coating film-forming resin that constitutes an electrodeposition coating film. The blocked polyisocyanate curing agent can be prepared by blocking a polyisocyanate with a sealing agent.
[0031] Examples of polyisocyanates include aliphatic diisocyanates such as hexamethylene diisocyanate (including trimer), tetramethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and 4,4'-methylenebis(cyclohexylisocyanate); and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, and xylylene diisocyanate.
[0032] Examples of the sealing agent that can be preferably used include monovalent alkyl (or aromatic) alcohols such as n-butanol, n-hexyl alcohol, 2-ethylhexanol, lauryl alcohol, phenol carbinol, and methylphenyl carbinol; cellosolves such as ethylene glycol monohexyl ether and ethylene glycol mono 2-ethylhexyl ether; polyether-type both-terminal diols such as polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol phenol; polyester-type both-terminal polyols obtained from diols such as ethylene glycol, propylene glycol, and 1,4-butanediol and dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, suberic acid, and sebacic acid; phenols such as para-t-butylphenol and cresol; oximes such as dimethyl ketoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, methyl amyl ketoxime, and cyclohexanone oxime; and lactams represented by ε-caprolactam and γ-butyrolactam.
[0033] The blocking rate of the blocked polyisocyanate curing agent is preferably 100%, which has the advantage of improving the storage stability of the electrodeposition coating composition.
[0034] As the blocked polyisocyanate curing agent, it is preferable to use in combination a curing agent prepared by blocking an aliphatic diisocyanate with a blocking agent and a curing agent prepared by blocking an aromatic diisocyanate with a blocking agent.
[0035] The blocked polyisocyanate curing agent reacts preferentially with the primary amine of the aminated epoxy resin, and then reacts with the hydroxyl group to cure. As the curing agent, at least one curing agent selected from the group consisting of organic curing agents such as melamine resins or phenolic resins, silane coupling agents, and metal curing agents may be used in combination with the blocked isocyanate curing agent.
[0036] Preparation of resin emulsion The resin emulsion can be prepared by dissolving the aminated epoxy resin and the blocked polyisocyanate curing agent in an organic solvent to prepare a solution, mixing these solutions, and then neutralizing the mixture with a neutralizing acid. Examples of the neutralizing acid include organic acids such as methanesulfonic acid, sulfamic acid, lactic acid, dimethylolpropionic acid, formic acid, and acetic acid. In the present invention, it is more preferable to neutralize the resin emulsion containing the aminated epoxy resin and the curing agent with one or more acids selected from the group consisting of formic acid, acetic acid, and lactic acid.
[0037] The content of the blocked polyisocyanate curing agent is required to be sufficient to react with active hydrogen-containing functional groups such as primary amino groups, secondary amino groups, or hydroxyl groups in the aminated epoxy resin during curing to give a good cured coating film. The preferred content of the curing agent is in the range of 90 / 10 to 50 / 50, more preferably 80 / 20 to 65 / 35, expressed as the solid content mass ratio of the aminated epoxy resin to the curing agent (aminated epoxy resin / curing agent). By adjusting the solid content mass ratio of the aminated epoxy resin to the blocked polyisocyanate curing agent, the fluidity and curing speed of the coating film (deposited film) during film formation are improved, and the coating appearance is improved.
[0038] The solid content of the resin emulsion is usually 25 to 50 mass %, and preferably 35 to 45 mass %, based on the total amount of the resin emulsion. Here, the "solid content of the resin emulsion" refers to the mass of all components contained in the resin emulsion that remain in a solid form even after removal of the solvent. Specifically, it refers to the total mass of the aminated epoxy resin, the curing agent, and other solid components added as necessary, contained in the resin emulsion.
[0039] The neutralizing acid is preferably used in an amount such that the equivalent ratio of the neutralizing acid to the equivalent of the amino group in the aminated epoxy resin is 10 to 100%, and more preferably 20 to 70%. In this specification, the equivalent ratio of the neutralizing acid to the equivalent of the amino group in the aminated epoxy resin is referred to as the neutralization rate. When the neutralization rate is 10% or more, affinity for water is ensured, and water dispersibility is improved.
[0040] <Pigment dispersion paste> The cationic electrodeposition coating composition of the present invention may contain a pigment dispersion paste as necessary. The pigment dispersion paste is a component that is optionally contained in the electrodeposition coating composition, and generally contains a pigment dispersing resin and a pigment.
[0041] Pigment Dispersion Resin The pigment dispersion resin is a resin for dispersing pigments, and is used by dispersing it in an aqueous medium. As the pigment dispersion resin, a pigment dispersion resin having a cationic group, such as a modified epoxy resin having at least one or more groups selected from a quaternary ammonium group, a tertiary sulfonium group, and a primary amino group, can be used. Specific examples of the pigment dispersion resin include a quaternary ammonium group-containing epoxy resin and a tertiary sulfonium group-containing epoxy resin. As the aqueous solvent, ion-exchanged water or water containing a small amount of alcohols is used.
[0042] Pigments Pigment is the pigment generally used in electrodeposition coating composition.Pigment can be, for example, commonly used inorganic pigment and organic pigment, for example, color pigment such as titanium white (titanium dioxide), carbon black and red iron oxide; extender pigment such as kaolin, talc, aluminum silicate, calcium carbonate, mica and clay; rust-preventive pigment such as iron phosphate, aluminum phosphate, calcium phosphate, aluminum tripolyphosphate, aluminum phosphomolybdate and aluminum zinc phosphomolybdate.
[0043] Manufacturing of pigment dispersion paste The pigment dispersion paste is prepared by mixing a pigment dispersion resin and a pigment. The content of the pigment dispersion resin in the pigment dispersion paste is not particularly limited, but for example, it can be used in an amount of 20 to 100 parts by mass in terms of the resin solid content ratio per 100 parts by mass of the pigment.
[0044] The solid content of the pigment dispersion paste is usually 40 to 70% by mass, and particularly preferably 50 to 60% by mass, based on the total amount of the pigment dispersion paste.
[0045] In this specification, the "solid content of the pigment dispersion paste" means the mass of all components contained in the pigment dispersion paste that remain in a solid state even after removal of the solvent, specifically, the total mass of the pigment dispersion resin, pigment, and other solid components added as necessary contained in the pigment dispersion paste.
[0046] <Other ingredients, etc.> The cationic electrodeposition coating composition of the present invention may further contain a metal nitrite salt in addition to the above components. As the metal nitrite salt, a nitrite salt of an alkali metal or a nitrite salt of an alkaline earth metal is preferable, and a nitrite salt of an alkaline earth metal is more preferable. As the metal nitrite salt, for example, calcium nitrite, sodium nitrite, potassium nitrite, magnesium nitrite, strontium nitrite, barium nitrite, zinc nitrite, etc. can be mentioned.
[0047] The cationic electrodeposition coating composition contains a metal nitrite, which has the advantage of improving corrosion resistance, particularly the corrosion resistance of edges (edge rust prevention). When the cationic electrodeposition coating composition contains a metal nitrite, the content is preferably 0.001 to 0.2 mass% of the metal component calculated as the metal element relative to the total mass of the coating film-forming resin.
[0048] The metal nitrite can be added to the cationic electrodeposition coating composition by any method. For example, an aqueous solution of the metal nitrite may be prepared in advance and added to the cationic electrodeposition coating composition. Alternatively, the metal nitrite may be mixed with the pigment in advance and dispersed in the same manner as the pigment.
[0049] <Production of cationic electrodeposition coating composition> The cationic electrodeposition coating composition of the present invention can be prepared by mixing a resin emulsion containing an aminated epoxy resin and a blocked polyisocyanate curing agent, a pigment dispersion paste, additives, etc., by a commonly used method.
[0050] In this specification, the "solid content of the electrodeposition coating composition" means the mass of all components contained in the electrodeposition coating composition that remain in the form of a solid even after removal of the solvent, specifically, the total mass of the solid content of the aminated epoxy resin, blocked polyisocyanate curing agent, and optionally the pigment dispersing resin, pigment, and other solid components contained in the electrodeposition coating composition.
[0051] The solid content of the cationic electrodeposition coating composition of the present invention is preferably 1-30% by mass based on the total amount of the electrodeposition coating composition. If the solid content of the cationic electrodeposition coating composition is less than 1% by mass, the amount of deposition of the electrodeposition coating film is small, and it may be difficult to ensure sufficient corrosion resistance. If the solid content of the cationic electrodeposition coating composition is more than 30% by mass, the throwing power or coating appearance may be deteriorated.
[0052] The cationic electrodeposition coating composition of the present invention preferably has a pH of 4.5 to 7. If the pH of the cationic electrodeposition coating composition is less than 4.5, the amount of acid present in the cationic electrodeposition coating composition becomes excessive, which may result in poor coating film appearance or coating workability. On the other hand, if the pH exceeds 7, the filterability of the cationic electrodeposition coating composition may decrease, and the horizontal appearance of the cured electrodeposition coating film may decrease. The pH of the cationic electrodeposition coating composition can be set within the above range by adjusting the amount of neutralizing acid used, the amount of free acid added, etc. The pH is more preferably 5 to 7.
[0053] The pH of the cationic electrodeposition coating composition can be measured using a commercially available pH meter having a temperature compensation function.
[0054] The milligram equivalent of acid (MEQ(A)) per 100 g of solid content of the cationic electrodeposition coating composition is preferably 10 to 50. The milligram equivalent of acid (MEQ(A)) per 100 g of resin solid content of the cationic electrodeposition coating composition can be adjusted by the amount of neutralizing acid and the amount of free acid.
[0055] Here, MEQ(A) is an abbreviation for mg equivalent(acid), and is the total mg equivalent of all acids per 100 g of solid content of the paint. This MEQ(A) can be measured by quantitatively determining the amount of acid contained in the cationic electrodeposition coating composition by precisely weighing out about 10 g of the solid content of the electrodeposition coating composition, dissolving it in about 50 ml of a solvent (THF: tetrahydrofuran), and then performing potentiometric titration using a 1 / 10 N NaOH solution.
[0056] The cationic electrodeposition coating composition of the present invention may contain additives generally used in the coating field, such as organic solvents such as ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monoethylhexyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, and propylene glycol monophenyl ether, surfactants such as drying inhibitors and defoamers, viscosity modifiers such as acrylic resin fine particles, anti-repellent agents, and inorganic rust inhibitors such as vanadium salts, copper, iron, manganese, magnesium, and calcium salts, as necessary. In addition to these, known auxiliary complexing agents, buffers, smoothing agents, stress relaxation agents, gloss agents, semi-gloss agents, antioxidants, and ultraviolet absorbers may be blended according to the purpose. These additives may be added during the production of the resin emulsion, during the production of the pigment dispersion paste, or during or after the mixing of the resin emulsion and the pigment dispersion paste.
[0057] The cationic electrodeposition coating composition of the present invention may contain other film-forming resin components in addition to the above-mentioned aminated epoxy resin. Examples of other film-forming resin components include acrylic resins, polyester resins, urethane resins, butadiene resins, phenolic resins, and xylene resins. Other film-forming resin components that can be contained in the electrodeposition coating composition are preferably phenolic resins and xylene resins. Examples of phenolic resins and xylene resins include xylene resins having 2 to 10 aromatic rings.
[0058] In the cationic electrodeposition coating composition of the present invention, the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is also an index for observing the performance of the electrodeposition coating. In the present invention, the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent must be 9.9 to 11.3, preferably 9.9 to 11.2, and more preferably 9.9 to 11.1. If the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is less than 9.9, the adhesion decreases, and conversely, if it is more than 11.3, the hydrophilicity increases and the barrier properties of the coating film decrease.
[0059] The cationic electrodeposition coating composition of the present invention is preferably such that the number of remaining adhesion functional groups is 78.6 to 134.7 mgKOH / g after the cationic electrodeposition coating composition of the present invention is applied to a steel plate so as to have a dry film thickness of 15 μm and baked at 170° C. for 20 minutes. This defines the performance of the coating film after the coating composition is obtained, and the number of remaining adhesion functional groups is a theoretical value and can be calculated by subtracting the amount of isocyanate groups (mgKOH / g) of the blocked polyisocyanate curing agent from the amount of functional groups of the aminated epoxy resin, specifically the total amount of hydroxyl groups (mgKOH / g) and the amount of primary amines (mgKOH / g). The number of remaining adhesion functional groups is preferably 89.8 to 123.4 mgKOH / g, more preferably 95.4 to 117.8 mgKOH / g. If the number of remaining adhesion functional groups in the coating film applied under these conditions is less than 78.6 mgKOH / g, the coating film will not be able to have sufficient adhesion performance, and if it is more than 134.7 mgKOH / g, the coating film will have the disadvantage of increasing its hydrophilicity and decreasing its barrier properties.
[0060] <Electrodeposition painting and electrocoating film formation> An electrodeposition coating film can be formed by electrodeposition coating of a substrate using the cationic electrodeposition coating composition of the present invention. In the electrodeposition coating using the cationic electrodeposition coating composition of the present invention, the substrate is used as a cathode, and a voltage is applied between the cathode and the anode. This causes an electrodeposition coating film to be deposited on the substrate.
[0061] As the substrate to which the cationic electrodeposition coating composition of the present invention is applied, various substrates to which electricity can be applied can be used. Examples of substrates that can be used include cold-rolled steel sheets, hot-rolled steel sheets, stainless steel, electrogalvanized steel sheets, hot-dip galvanized steel sheets, zinc-aluminum alloy-plated steel sheets, zinc-iron alloy-plated steel sheets, zinc-magnesium alloy-plated steel sheets, zinc-aluminum-magnesium alloy-plated steel sheets, aluminum-plated steel sheets, aluminum-silicon alloy-plated steel sheets, and tin-plated steel sheets.
[0062] In the electrodeposition coating process, the object to be coated is immersed in the electrodeposition coating composition, and then electrodeposition coating is performed by applying a voltage of 50 to 450 V. If the applied voltage is less than 50 V, the electrodeposition may be insufficient, and if it exceeds 450 V, the appearance of the coating film may be poor. During electrodeposition coating, the bath temperature of the coating composition is usually adjusted to 10 to 45°C.
[0063] The time for applying the voltage varies depending on the electrodeposition conditions, but can generally be set to 2 to 5 minutes.
[0064] In the electrodeposition coating using the cationic electrodeposition coating composition of the present invention, the thickness of the electrodeposition coating film to be deposited is preferably such that the thickness of the electrodeposition coating film finally obtained by heat curing is preferably 5 to 60 μm, more preferably 10 to 25 μm. If the thickness of the electrodeposition coating film is less than 5 μm, the rust prevention properties may be insufficient.
[0065] The electrodeposition coating film deposited as described above can be cured by, if necessary, rinsing with water and then heating for 10 to 30 minutes at, for example, 120 to 260° C., preferably 140 to 220° C. This forms a cured electrodeposition coating film.
[0066] In the present invention, the elongation of the cured coating film is controlled. The elongation is obtained by applying a cationic electrodeposition coating composition to a steel plate so that the cured film thickness is 20 μm, baking at 160° C. for 15 minutes, and then measuring the elongation of the electrodeposition coating film. Specifically, the elongation is calculated as the ratio (%) of the length elongated until the coating film breaks to the length of the coating film before measurement. The elongation measured is 0.1 to 4.5%, preferably 2.0 to 4.5%. If the elongation is less than 0.1%, there is a drawback in that the impact resistance test is deteriorated, and if it exceeds 4.5%, there is a drawback in that the coating film blistered greatly during the corrosion resistance test.
[0067] The cationic electrodeposition coating composition of the present invention has the advantage that, even when a cured electrodeposition coating film is provided on a substrate having edges, a cured electrodeposition coating film having excellent edge rust prevention properties can be provided. The cationic electrodeposition coating composition of the present invention has a function of retaining the deposited electrodeposition coating film, and therefore can be suitably used in cases where a cured electrodeposition coating film is provided on a substrate having edges.
[0068] In this specification, the corrosion resistance of a cured electrodeposition coating formed on a substrate having edges is evaluated by a salt spray test (35°C x 72 hours) in accordance with JIS Z 2371 (2000). When a high-thickness cured electrodeposition coating, for example, a thickness of 25 to 50 μm, is subjected to a salt spray test, the number of rust spots occurring in the edge coating of the cured electrodeposition coating formed on a substrate having edges is 1 cm or less. 2 For example, 3 pieces / cm 2 If the number of rust spots is less than 1 cm, the coating has excellent corrosion resistance (rust prevention) at the edge. 2 1 piece per cm 2 If it is less than this, it can be said that the coating film has extremely excellent edge corrosion resistance. EXAMPLES
[0069] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0070] Production Example 1-A Production of aminated epoxy resin (resin A) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 4.2 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 600 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 110 parts of diethanolamine (DETA) and 80 parts of aminopropyldiethanolamine (APDEA) was added, and the reaction was continued for 1 hour at 140°C to obtain an aminated epoxy resin (cation-modified epoxy resin: resin A).
[0071] Production Example 1-B Production of aminated epoxy resin (resin B) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 4.2 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 620 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 110 parts of diethanolamine (DETA) and 70 parts of diethylaminopropanediamine (DEAPA) was added, and the reaction was continued for 1 hour at 140°C to obtain an aminated epoxy resin (cation-modified epoxy resin: resin B).
[0072] Production Example 1-C Production of aminated epoxy resin (resin C) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 4.2 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 620 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 110 parts of diethanolamine (DETA) and 100 parts of dibutylaminopropanediamine (DBAPA) was added, and the reaction was continued for 1 hour at 140°C to obtain an aminated epoxy resin (cation-modified epoxy resin: resin C).
[0073] Production Example 1-D Production of aminated epoxy resin (resin D) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 23 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 650 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 50 parts of dimethylaminopropylamine (DMAPA) and 100 parts of diethanolamine (DETA) was added, and the reaction was continued for 1 hour at 160°C to obtain an aminated epoxy resin (cation-modified epoxy resin: resin D).
[0074] Production Example 1-E Production of aminated epoxy resin (resin E) 25 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 380 parts of bisphenol A, 58 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 1100 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. 110 parts of diethanolamine (DETA) and 10 parts of N-methylethanolamine (MMA) were added, and the reaction was continued at 140°C for 1 hour to obtain an aminated epoxy resin (cation-modified epoxy resin: resin E).
[0075] Production Example 1-F Production of aminated epoxy resin (Resin F) 26 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 380 parts of bisphenol A, 58 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 1100 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. 60 parts of diethanolamine (DETA), 20 parts of N-methylethanolamine (MMA), and 85 parts of diethylenetriamine diketimine (diketimine: methyl isobutyl ketone solution with a solid content of 73%) were added, and the reaction was continued for 1 hour at 140°C to obtain an aminated epoxy resin (cationically modified epoxy resin: resin F).
[0076] Production Example 1-G Production of aminated epoxy resin (resin G) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 4.2 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 620 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 110 parts of diethanolamine (DETA) and 70 parts of diethylaminopropanediamine (DEAPA) was added, and the reaction was continued at 90°C for 1 hour to obtain an aminated epoxy resin (cation-modified epoxy resin: resin G).
[0077] Production Example 1-H Production of aminated epoxy resin (Resin H) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 325 parts of bisphenol A, 4.2 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was allowed to proceed until the epoxy equivalent reached 600 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 110 parts of diethanolamine (DETA) and 80 parts of aminopropyldiethanolamine (APDEA) was added, and the reaction was allowed to proceed for 1 hour at 220°C, yielding an aminated epoxy resin (cationically modified epoxy resin: resin H).
[0078] The type and amount of the amine compound used, the amination temperature (°C), molecular weight distribution, and the tertiary amine conversion rate of the amine compound of the aminated epoxy resin obtained in the above Production Examples are shown in Table 1. The molecular weight distribution and the tertiary amine conversion rate were measured as follows.
[0079] The molecular weight distribution was measured by gel permeation chromatography. Specifically, the number average molecular weight was measured under the following GPC system measurement conditions. Equipment: alliance2695S eparations Module Column: Tosoh TSKgel ALPHA-M Flow rate: 0.05ml / min Detector: alliance2414 Refractive Index Detector Mobile phase: N,N'-dimethylformamide Standard samples: TSK STANDARD POLYSTYRENE (manufactured by Tosoh), A-500, A-2500, F-1, F-4, F-20, F-80, F-700, 1-phenylhexane (manufactured by Aldrich)
[0080] Tertiary amine conversion rate Tertiary amine conversion rate (%) = Tertiary amine value / Total amine value Tertiary amine value test method (1) Weigh the sample into a 100 ml beaker. (2) Add 0.5g of pure water. (3) Dissolve the above sample in 50 g of THF (tetrahydrofuran). (4) Stir for 5 minutes. (5) Next, add 7.5 ml of acetic anhydride and 2.5 ml of acetic acid and stir at about 40°C for 5 minutes. (6) Using an automatic potentiometric titrator, titrate with 0.1N perchloric acid acetic acid solution. (7) Measure the tertiary amine value using the following formula. Tertiary amine value = (titer amount mL × factor × 10) / (sample amount g × solids amount)
[0081] Total Amine Number Test Method (1) Accurately weigh out 500 mg of sample into a 200 ml Erlenmeyer flask. (2) Add approximately 50 ml of glacial acetic acid and dissolve uniformly. (3) Add 5 to 6 drops of indicator methyl violet solution and mix uniformly. (4) Titrate with 0.1N perchloric acid and acetic acid solution, and the endpoint is when the solution turns bright green. (The above (3) and (4) can also be performed by potentiometric titration.)
[0082] [Table 1]
[0083] Production Example 2 Production of blocked polyisocyanate curing agent (1) 1370 parts of polymethylene polyphenyl polyisocyanate (MDI) and 732 parts of MIBK were charged into a reaction vessel and heated to 60° C. 300 parts of butyl diglycol ether and 1330 parts of butyl cellosolve were added dropwise to the vessel over 2 hours at 60° C. After further heating at 75° C. for 4 hours, it was confirmed that the absorption due to the isocyanate group had disappeared in the measurement of the IR spectrum, and after cooling, 27 parts of MIBK were added to obtain a blocked polyisocyanate curing agent (1).
[0084] Production Example 3 Preparation of pigment dispersing resin In a reaction vessel equipped with a stirrer, a cooling tube, a nitrogen inlet tube and a thermometer, 2220 parts of isophorone diisocyanate and 342.1 parts of methyl isobutyl ketone were charged, and the temperature was raised to 50°C, 2.2 parts of dibutyltin laurate were charged, and 878.7 parts of methyl ethyl ketone oxime were charged at 60°C. After that, the mixture was kept at 60°C for 1 hour, and it was confirmed that the NCO equivalent was 348, and 890 parts of dimethylethanolamine were charged. After keeping the mixture at 60°C for 1 hour and confirming that the NCO peak had disappeared by IR, 1872.6 parts of 50% lactic acid and 495 parts of deionized water were charged while cooling so as not to exceed 60°C to obtain a quaternizing agent. Next, 870 parts of tolylene diisocyanate and 49.5 parts of methyl isobutyl ketone were charged in a different reaction vessel, and 667.2 parts of 2-ethylhexanol were dropped over 2.5 hours so as not to exceed 50°C. After the dropwise addition, 35.5 parts of methyl isobutyl ketone was added and the mixture was kept warm for 30 minutes. After that, it was confirmed that the NCO equivalent was 330 to 370, and a half-blocked polyisocyanate was obtained.
[0085] In a reaction vessel equipped with a stirrer, a cooling tube, a nitrogen inlet tube and a thermometer, 940.0 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Co.) was diluted with 38.5 parts of methanol, and 0.1 parts of dibutyltin dilaurate was added thereto. After heating this to 50°C, 87.1 parts of tolylene diisocyanate was added and the temperature was further raised. At 100°C, 1.4 parts of N,N-dimethylbenzylamine was added and the mixture was kept at 130°C for 2 hours. At this time, methanol was fractionated using a fractionating tube. This was cooled to 115°C, and methyl isobutyl ketone was added until the solid content concentration reached 90%, and then 270.3 parts of bisphenol A and 39.2 parts of 2-ethylhexanoic acid were added and heated and stirred at 125°C for 2 hours, after which 516.4 parts of the half-blocked polyisocyanate was added dropwise over 30 minutes, and then heated and stirred for 30 minutes. 1506 parts of polyoxyethylene bisphenol A ether was gradually added and dissolved. After cooling to 90°C, the above quaternizing agent was added, and the mixture was kept at 70 to 80°C, and the acid value was confirmed to be 2 or less, to obtain a pigment dispersion resin (resin solid content 30%).
[0086] Production Example 4 Preparation of pigment dispersion paste A sand grinding mill was charged with 106.9 parts of the pigment dispersion resin obtained in Production Example 3, 1.6 parts of carbon black, 40 parts of kaolin, 55.4 parts of titanium dioxide, 3 parts of aluminum phosphomolybdate, and 13 parts of deionized water, and the mixture was dispersed until the particle size reached 10 μm or less, thereby obtaining a pigment dispersion paste (solid content 60%).
[0087] Production Example 5-A: Production of electrocoating resin emulsion (EmA) 400 g (solid content) of the resin (Resin A) obtained in Production Example 1-A and 160 g (solid content) of the blocked polyisocyanate curing agent (1) obtained in Production Example 2 were mixed, and ethylene glycol mono-2-ethylhexyl ether was added so that the amount was 3% (15 g) based on the solid content. Next, formic acid was added to achieve a neutralization rate of 40% for neutralization, and ion-exchanged water was added to slowly dilute the mixture to obtain an electrodeposition paint resin emulsion (EmA).
[0088] Production Example 5-B~H Production of electrodeposition paint resin emulsion (EmB~H) The aminated epoxy resins (Resins BH) obtained in Production Examples 1-B to 1-H were also used to obtain electrodeposition paint resin emulsions (EmB to EmH) in the same manner as in Production Example 5-A.
[0089] Example 1 1,394 g of ion-exchanged water, 560 g of resin emulsion (EmA) and 41 g of the pigment dispersion paste obtained in Production Example 4 were added to a stainless steel container, and the mixture was then aged at 40° C. for 16 hours to form an electrodeposition coating composition.
[0090] Examples 2 to 4 and Comparative Examples 1 to 4 In the same manner as in Example 1, electrodeposition coating compositions were obtained for Examples 2, 3 and 4 (EmB, EmC and EmD) and Comparative Examples 1, 2, 3 and 4 (EmE, EmF, EmG and EmH).
[0091] <Conductivity> In an electrodeposition bath containing 200 ml of the cationic electrodeposition coating composition obtained in each of the Examples and Comparative Examples, the electrical conductivity was measured at 25° C. using a conductivity meter (CM-305, manufactured by Toa Denpa Kogyo Co., Ltd.). The measured electrical conductivity is shown in Table 2. The unit is μS / cm.2 It is.
[0092] Electrochemical Painting A cold-rolled steel sheet (JISG3141, SPCC-SD) was degreased by immersing it in Surf Cleaner EC90 (manufactured by Nippon Paint Surf Chemicals) at 50°C for 2 minutes. Then, the sheet was immersed in a zirconium conversion treatment solution containing 0.005% ZrF and adjusted to pH 4 with NaOH at 40°C for 90 seconds to perform zirconium conversion treatment. Next, the electrodeposition coating composition obtained in the examples or comparative examples was added with a necessary amount of 2-ethylhexyl glycol so that the film thickness of the electrodeposition coating film after curing was 20 μm, and then the steel sheet was immersed in the composition. A voltage was applied under the conditions of increasing the voltage for 30 seconds to 180 V and then maintaining the voltage for 150 seconds to deposit an uncured electrodeposition coating film on the substrate.
[0093] The uncured electrodeposition coating thus obtained was baked and cured at 160°C for 15 minutes to obtain an electrodeposition coated plate having a cured electrodeposition coating. The resulting cured electrodeposition coating was subjected to the following evaluations. The results are shown in Table 2. Table 2 also lists the characteristics of each electrodeposition coating composition (curability (rubbing ability), elongation, cyclic corrosion test (CCT), edge rust prevention, paint workability, and paint stability). The evaluation methods and evaluation criteria for each are described below.
[0094] The electrodeposition coating compositions and coated plates obtained in the above examples were used to carry out the following evaluation tests.
[0095] Curing property (rubbing property) The coating was rubbed 50 times with gauze soaked in methyl isobutyl ketone (MIBK), and the curing property was judged based on the surface condition of the coating. The evaluation criteria are as follows. ○: No change in the coating film. △: Streaks in the coating. ×: The gauze is discolored.
[0096] Elongation rate (%) A stress-strain curve of the coating is created, and the ratio (%) of the length elongated until the sample breaks to the initial sample length is calculated.
[0097] Cycle Corrosion Test (CCT) A cross-cut was made with a knife on the coating of the electrocoated cold-rolled steel plate after hardening, reaching the base material, and JASOM609-91 "Corrosion Test Method for Automotive Materials" was run for 100 cycles. The cross-cut area was then observed for rust and blisters, and the corrosion resistance was evaluated in accordance with an actual corrosive environment. The evaluation criteria were as follows: Evaluation criteria ◎: The maximum width of rust or blister is less than 5 mm from the cut part (on both sides) ○: The maximum width of rust or swelling is 5mm to less than 7.5mm from the cut part (both sides). No blisters other than the cut part. ○△: The maximum width of rust or blister is 5mm to less than 7.5mm from the cut part (both sides). Blisters are present in areas other than the cut part. △: The maximum width of rust or blister is 7.5mm or more but less than 10mm from the cut part (both sides) △×: The maximum width of rust or blister is 10mm or more and less than 12.5mm from the cut part (both sides) ×: The maximum width of rust or blister is 12.5 mm or more from the cut part (on both sides) The passing grade is ○△ or above.
[0098] Edge rust prevention (edge corrosion test) For the evaluation of this test, instead of the above cold-rolled steel plate, an L-type dedicated replacement blade (LB10K: manufactured by Olfa Corporation) was used, which was degreased by immersing it in Surf Cleaner EC90 (manufactured by Nippon Paint Surf Chemicals) at 50 ° C for 2 minutes, surface-conditioned with Surf Fine GL-1 (manufactured by Nippon Paint Surf Chemicals), and then immersed in Surf Dyne SD-5000 (manufactured by Nippon Paint Surf Chemicals, zinc phosphate conversion treatment liquid) at 40 ° C for 2 minutes to perform zinc phosphate conversion treatment. The paints of Examples 1 to 4 and Comparative Examples 1 to 4 were electrocoated on this under the same conditions as the above electrocoating to form a cured electrocoated coating film, and the number of rust spots on the tip of the L-type dedicated replacement blade after the salt spray test at 35 ° C x 168 h test was examined. Evaluation criteria ◎: Less than 10 ○: 10 or more but less than 20 ○△: 20 to less than 50 △: 50 to less than 100 ×: 100 or more pieces The passing grade is ○△ or above.
[0099] Painting workability (GP: uneven grinding) Steel plates were ground with a grindstone and then electrocoated, and the appearance of the ground area was visually inspected for roughness. ○: The coating film has a uniform appearance. ○△: Some areas are visually recognized as being slightly uneven, but the overall appearance of the coating is almost uniform △: Unevenness is visible ×: Appearance of the coating film is obviously non-uniform
[0100] Stability of electrodeposition coating composition (paint stability) The electrodeposition coating composition was left to stand or stirred, and the state of the coating composition was visually judged to evaluate the coating stability. The evaluation criteria were as follows. Stable here means that the pigment does not settle within 15 minutes after stirring is stopped. Evaluation criteria ○: The electrodeposition coating composition is stable when left standing. ○△: The electrodeposition coating composition is not stable when left to stand, but is quickly stabilized by stirring again. △: The electrodeposition coating composition is stable when it is continuously stirred. ×: The electrodeposition coating composition is not stabilized even when continuously stirred.
[0101] [Table 2]
[0102] As is clear from Table 2 above, when the molecular weight distribution of the aminated epoxy resin is 2.7 or less and the elongation rate is in the range of 0.1 to 4.5%, good results are obtained in corrosion resistance (cyclic corrosion test and edge rust prevention) and other performance properties (paintability and paint stability) are also excellent. On the other hand, in the comparative examples, when the molecular weight distribution of the aminated epoxy resin and the elongation rate of the electrodeposition coating film are outside these ranges, the corrosion resistance results are insufficient and the paintability is also insufficient.
Claims
1. A cationic electrodeposition coating composition comprising an aminated epoxy resin and a blocked polyisocyanate curing agent, the aminated epoxy resin is obtained by reacting an amine compound with an epoxy resin, the amine compound is a combination of two types of amines, a primary amine and a secondary amine, The primary amine has the formula: NH 2 -(CH 2 )n-NR 1 R 2 (1) In formula (1), R 1 and R 2 may be the same or different and each represents an alkyl group having 1 to 6 carbon atoms which may have a hydroxyl group at its terminal, and n represents an integer of 2 to 4. having The secondary amine has the formula: R 3 R 4 NH (2) (In formula (2), R 3 and R 4 represent an alkyl group having 1 to 4 carbon atoms and a hydroxyl group at its terminal.) having the tertiary amine conversion rate of the amine compound in obtaining the aminated epoxy resin is 85% or more, the molecular weight distribution of the aminated epoxy resin is 2.7 or less, The cationic electrodeposition coating composition is applied onto a steel plate so that the cured film thickness is 20 μm, and after baking at 160° C. for 15 minutes, the elongation of the electrodeposition coating film is 0.1 to 4.5%. Cationic electrodeposition coating composition.
2. A cationic electrodeposition coating film formed by applying the cationic electrodeposition coating composition according to claim 1.
Citation Information
Patent Citations
Water-base coating resin composition
JP1994009920A
Cationic electrodeposition coating epoxy resin and cationic electrodeposition coating
JP2000169548A
Cationic electrocoating composition, method of making and use thereof
JP2000501448A
Coating composition and coated object
JP2009149867A
Method for improving deposition property of cationic electrodeposition coating
JP2010280787A