VINYLIDENE FLUORIDE POLYMER COMPOSITION AND PRODUCTION METHOD THEREOF, RESIN COMPOSITION, ELECTRODE MIXTURE, AND ELECTRODE CONTAINING THEM AND PRODUCTION METHOD THEREOF

The vinylidene fluoride polymer composition with a high melting point and surfactants addresses the swelling and solubility issues in NMP, achieving reduced NMP usage and improved electrode smoothness and productivity.

JP7587403B2Active Publication Date: 2024-11-20KUREHA CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020198127
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-20
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Existing vinylidene fluoride polymers used in electrode mixtures for secondary batteries swell and dissolve easily in N-methyl-2-pyrrolidone (NMP), leading to increased viscosity and difficulty in reducing NMP usage, which affects the smoothness and productivity of the electrode surface.

Method used

A vinylidene fluoride polymer composition with a melting point of 130°C or higher, combined with specific surfactants, is dispersed in water and heated below its melting point to reduce swelling and solubility in NMP, maintaining low viscosity and preventing sedimentation, allowing for a smooth electrode surface.

Benefits of technology

The composition enables reduced NMP usage, improved productivity, and enhanced surface smoothness of electrodes by minimizing swelling and sedimentation, thus optimizing electrode formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587403000001
    Figure 0007587403000001
  • Figure 0007587403000002
    Figure 0007587403000002
  • Figure 0007587403000003
    Figure 0007587403000003
Patent Text Reader

Abstract

To provide a vinylidene fluoride polymer composition which is hardly swelled and dissolved in N-methyl-2-pyrrolidone, and enables formation of an electrode having a smooth surface.SOLUTION: A vinylidene fluoride polymer composition contains a vinylidene fluoride polymer having a melting point of 130°C or higher. When the vinylidene fluoride polymer composition and N-methyl-2-pyrrolidone are mixed, and a vinylidene fluoride polymer dispersion liquid having a percentage content of the vinylidene fluoride polymer of 6 mass% is prepared, a ratio of viscosity at 30°C of the vinylidene fluoride polymer dispersion liquid to viscosity at 30°C of the N-methyl-2-pyrrolidone is 20 or less, and a change rate of the percentage content of the vinylidene fluoride polymer in a region of 40 vol.% of the upper part of the vinylidene fluoride polymer dispersion liquid before and after left for 15 minutes after the vinylidene fluoride polymer dispersion liquid is agitated is 2 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vinylidene fluoride polymer composition and a method for producing the same, a resin composition, an electrode mixture, and an electrode containing these and a method for producing the same. [Background technology]

[0002] In electrodes for secondary batteries and the like, polyvinylidene fluoride (hereinafter also referred to as "PVDF") is widely used as a binder for binding active materials to current collectors. Such electrodes are formed by applying an electrode mixture containing PVDF, active materials, and a solvent such as N-methyl-2-pyrrolidone (hereinafter also referred to as "NMP") onto a current collector and then removing the solvent. In this case, if the solvent is not sufficiently removed, the battery performance is likely to decrease. However, there is a production cost issue in that it takes time to sufficiently remove the solvent.

[0003] Therefore, it is possible to reduce costs by reducing the amount of NMP mixed with PVDF, etc., and to improve productivity by shortening the drying time. However, general PVDF is easily swollen and dissolved in NMP. Therefore, the viscosity of the electrode mixture is easily increased, and it is difficult to reduce the amount of NMP in order to ensure the applicability of the electrode mixture.

[0004] In response to this, a vinylidene fluoride polymer with reduced solubility in NMP is proposed in Patent Documents 1 and 2. In these documents, the crystallinity of the vinylidene fluoride polymer is increased to reduce the swelling and solubility in NMP, thereby suppressing the amount of NMP used in the electrode mixture. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-041065 A [Patent Document 2] International Publication No. 2020 / 054274 Summary of the Invention [Problem to be solved by the invention]

[0006] However, it has become clear that when a mixture layer is formed using a vinylidene fluoride polymer that has low swelling and solubility in NMP, the smoothness of the resulting electrode surface is likely to be low. The present invention has been made in consideration of this problem. The object of the present invention is to provide a vinylidene fluoride polymer composition, a resin composition, an electrode mixture, and a manufacturing method thereof that are unlikely to swell or dissolve in N-methyl-2-pyrrolidone and that can form an electrode with a smooth surface. [Means for solving the problem]

[0007] The present invention relates to a vinylidene fluoride polymer composition containing a vinylidene fluoride polymer having a melting point of 130° C. or more, and when the vinylidene fluoride polymer composition and N-methyl-2-pyrrolidone are mixed to prepare a vinylidene fluoride polymer dispersion having a vinylidene fluoride polymer content of 6 mass%, the vinylidene fluoride polymer dispersion has a melting point of 130° C. or more and a melting point of 130° C. or more. -1 The viscosity of N-methyl-2-pyrrolidone at 30°C measured at a shear rate of 100 s using a parallel plate rheometer. -1 the vinylidene fluoride polymer dispersion has a viscosity ratio at 30°C of 20 or less as measured at a shear rate of 100 / s, and the rate of change in the vinylidene fluoride polymer content in the upper 40% by volume region of the vinylidene fluoride polymer dispersion before and after stirring and then allowing to stand for 15 minutes is 2% by mass or less.

[0008] The present invention also provides a resin composition comprising the above-mentioned vinylidene fluoride polymer composition and another resin, wherein the other resin is at least one polymer selected from the group consisting of vinylidene fluoride-based polymers other than the above-mentioned vinylidene fluoride polymers, polyacrylonitrile, nitrile rubber, poly(meth)acrylic acid and esters thereof, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, and cellulose ether.

[0009] The present invention also provides a method for producing a vinylidene fluoride polymer composition, comprising the steps of obtaining a latex in which an untreated vinylidene fluoride polymer is dispersed in water, and heating the latex in the presence of a surfactant whose hydrophobic group is non-perfluorinated and whose hydrophilic group is ionic at a temperature lower than the melting point of the untreated vinylidene fluoride polymer and not lower than the melting point by 20°C (but not lower than 100°C).

[0010] The present invention also provides an electrode mixture comprising the vinylidene fluoride polymer composition, an active material, and a dispersion medium. The present invention further provides an electrode mixture comprising the resin composition, an active material, and a dispersion medium, in which the polymer in the resin composition is dissolved in the dispersion medium.

[0011] The present invention also provides an electrode having a mixture layer containing the vinylidene fluoride polymer composition or the resin composition and an active material.

[0012] The present invention also provides a method for producing an electrode, comprising the steps of mixing the vinylidene fluoride polymer composition or the resin composition, an active material, and a dispersion medium to obtain an electrode mixture, and applying the electrode mixture onto a current collector and drying the same, wherein the temperature of the electrode mixture is maintained at 60° C. or lower from the preparation of the electrode mixture until it is applied. Effect of the Invention

[0013] The vinylidene fluoride polymer composition of the present invention is difficult to swell or dissolve in N-methyl-2-pyrrolidone, making it possible to reduce the amount of dispersion medium (NMP) used in the electrode mixture. In addition, the vinylidene fluoride polymer composition makes it possible to form an electrode with a smooth surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1. Vinylidene fluoride polymer composition The vinylidene fluoride polymer composition of the present invention may be any composition containing at least a vinylidene fluoride polymer having a melting point of 130° C. or higher. In general, the composition is preferably solid at 25° C. In this specification, the phrase "a composition is solid at 25° C." means that the main components of the composition are solid at 25° C., and the composition may partially contain liquid components (e.g., surfactants, etc.) within the scope of not impairing the object and effect of the present invention.

[0015] The vinylidene fluoride polymer composition is particularly useful as a binder for a mixture layer of an electrode of a secondary battery, for example, although the use of the vinylidene fluoride polymer composition is not limited to a binder.

[0016] As mentioned above, in an electrode mixture containing a general vinylidene fluoride polymer and NMP, the vinylidene fluoride polymer is easily swollen and dissolved in NMP, making it difficult to obtain an electrode mixture with low viscosity using a small amount of NMP. In response to this, a technology has been proposed that makes the vinylidene fluoride polymer less likely to swell and dissolve in NMP. However, when an electrode mixture using the vinylidene fluoride polymer is applied to form a mixture layer, the smoothness of the resulting electrode surface tends to be low.

[0017] As a result of intensive research by the present inventors, it has become clear that the vinylidene fluoride polymers described in Patent Document 1 and Patent Document 2, which have low swelling and solubility in NMP, tend to settle in NMP. The tendency to settle in NMP means that the dispersed particles of vinylidene fluoride polymer are large. Here, it is assumed that when an electrode mixture containing vinylidene fluoride polymer particles is applied to a current collector, the active material settles before the electrode mixture is solidified, and the vinylidene fluoride polymer particles tend to rise relatively. Then, when the electrode mixture applied to the current collector is heated, the vinylidene fluoride polymer particles usually swell with NMP, and then transition from the swollen state to a dissolved state. When the vinylidene fluoride polymer particles are in a dissolved state, it is believed that the vinylidene fluoride polymer is widely dispersed in the electrode mixture. However, the vinylidene fluoride polymer particles having a large particle size undergo a large volume change in the electrode mixture due to swelling in NMP when the electrode mixture is heated to solidify. Then, NMP evaporates before the electrode mixture changes from the swollen state to the dissolved state. Therefore, the electrode mixture solidifies before the vinylidene fluoride polymer that floats near the electrode surface is widely dispersed, so that voids of a size equivalent to the polymer particle size are likely to occur on the surface of the mixture layer. Therefore, the smoothness of the electrode surface is reduced.

[0018] In contrast, it has been found that a vinylidene fluoride polymer composition that satisfies the following physical properties is difficult to swell or dissolve in NMP used to form a mixture layer, and further, when the mixture layer is formed using the vinylidene fluoride polymer composition, an electrode with high surface smoothness can be obtained. Specifically, when the vinylidene fluoride polymer composition of the present invention is mixed with NMP to prepare a vinylidene fluoride polymer dispersion having a vinylidene fluoride polymer content of 6 mass% at 25°C, the ratio (X / Y) of the viscosity X of the vinylidene fluoride polymer dispersion at 30°C to the viscosity Y of NMP at 30°C is 20 or less. The viscosity ratio (X / Y) of 20 or less means that the vinylidene fluoride polymer composition is difficult to swell or dissolve in NMP at 30°C. In other words, when an electrode mixture containing the vinylidene fluoride polymer composition and NMP is prepared, the viscosity is difficult to increase at 30°C. Therefore, the amount of NMP in the electrode mixture can be reduced, the cost of NMP can be reduced, and the productivity can be improved. The viscosity ratio (X / Y) is more preferably 10 or less, and further preferably 5 or less.

[0019] The viscosity Y of the NMP at 30°C and the viscosity X of the vinylidene fluoride polymer dispersion at 30°C were measured using a parallel plate rheometer (parallel plate: 50 mm, gap distance: 0.5 mm) at a shear rate of 100 s -1 It is measured in.

[0020] Here, it is preferable that the vinylidene fluoride polymer composition of the present invention is not dissolved in NMP at 30° C., but is preferably easily swellable and soluble in NMP at temperatures exceeding 60° C., as described below. Therefore, when checking the swelling and solubility of the vinylidene fluoride polymer composition at 30° C., i.e., when measuring the viscosity, it is preferable to maintain the temperature of the vinylidene fluoride polymer dispersion at 60° C. or lower from the preparation of the vinylidene fluoride polymer dispersion to the end of the viscosity measurement. It is more preferable to maintain the temperature of the dispersion at 50° C. or lower, and even more preferable to maintain the temperature at 40° C. or lower.

[0021] In addition, when the vinylidene fluoride polymer composition of the present invention is stirred at 25°C and then allowed to stand for 15 minutes in a cylindrical container with a diameter of 1 cm, the vinylidene fluoride polymer content in the upper 40% by volume region of the vinylidene fluoride polymer dispersion before and after standing is 2% by mass or less. The change in content before and after standing represents the ease of settling of the vinylidene fluoride polymer composition in NMP, and the smaller the rate of change, the less likely the vinylidene fluoride polymer composition is to settle in NMP. In the vinylidene fluoride polymer composition of the present invention, the rate of change is 2% by mass or less, so that the vinylidene fluoride polymer composition is less likely to settle in an electrode mixture containing the vinylidene fluoride polymer composition and NMP, and the particle size of the vinylidene fluoride polymer composition is small. Therefore, when the electrode mixture containing the vinylidene fluoride polymer composition is applied and heated, the vinylidene fluoride polymer composition does not swell excessively in NMP and transitions to a dissolved state, so that the volume change of the electrode during drying is small. As a result, the surface smoothness of the obtained mixture layer and therefore the electrode is improved. The change rate of the above content is preferably 1.7% by mass or less, more preferably 1.5% by mass or less.

[0022] The change in the content of vinylidene fluoride polymer dispersion is measured as follows. A 5 cm high vinylidene fluoride polymer dispersion is placed in a cylindrical container with a diameter of 1 cm, and stirred at 25°C for 10 minutes with a magnetic stirrer. Then, a portion of the vinylidene fluoride polymer dispersion in the stirring treatment state is taken while continuing to stir, and the vinylidene fluoride polymer content in the dispersion is measured (vinylidene fluoride polymer content W1 before standing). Then, the vinylidene fluoride polymer dispersion is left to stand at 25°C for 15 minutes. Then, the vinylidene fluoride polymer dispersion in the upper 40% by volume region of the vinylidene fluoride polymer dispersion is taken to measure the vinylidene fluoride polymer content (vinylidene fluoride polymer content W2 after standing). Then, the rate of change in content is calculated by the following formula.

number

[0023] Here, the vinylidene fluoride polymer composition of the present invention may be composed of only a vinylidene fluoride polymer, but a specific surfactant may be present around the vinylidene fluoride polymer. When the vinylidene fluoride polymer composition contains a specific surfactant together with the vinylidene fluoride polymer, sedimentation is easily suppressed. The components in the vinylidene fluoride polymer composition and the preparation method thereof will be described in detail below.

[0024] (1) Vinylidene fluoride polymer The vinylidene fluoride polymer contained in the vinylidene fluoride polymer composition of the present invention is a compound that contains a structural unit derived from vinylidene fluoride and has a melting point of 130°C or higher. The vinylidene fluoride polymer may be a homopolymer of vinylidene fluoride or a copolymer of vinylidene fluoride and other monomers. However, from the viewpoint of making the melting point of the vinylidene fluoride polymer 130°C or higher, the amount of the structural unit derived from vinylidene fluoride relative to the total structural units of the vinylidene fluoride polymer is preferably 90% by mass or higher, more preferably 95% by mass or higher, and even more preferably 99% by mass or higher, and it is particularly preferably a homopolymer of vinylidene fluoride. Although it depends on the type of other monomer combined with vinylidene fluoride, the melting point is usually likely to increase as the amount of the structural unit derived from vinylidene fluoride in the vinylidene fluoride polymer increases. The mass fraction of the structural unit derived from vinylidene fluoride is 19 It can be identified by F-NMR analysis.

[0025] Examples of other monomers copolymerizable with vinylidene fluoride include fluorine-containing monomers other than vinylidene fluoride, hydrocarbon monomers such as ethylene and propylene, unsaturated dibasic acid derivatives such as (meth)acrylic acid alkyl compounds, monomethyl maleate and dimethyl maleate, and carboxylic anhydride group-containing monomers. For example, acryloyloxyethyl succinate, methacryloyloxyethyl succinate, acryloyloxypropyl succinate, methacryloyloxypropyl succinate, acryloyloxyethyl phthalate, methacryloyloxyethyl phthalate, 2-carboxyethyl (meth)acrylic acid, etc. may be used.

[0026] Examples of the fluorine-containing monomer include vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, hexafluoroethylene, fluoroalkyl vinyl ethers, and perfluoroalkyl vinyl ethers such as perfluoromethyl vinyl ether.

[0027] The melting point of the vinylidene fluoride polymer may be 130° C. or higher, more preferably 140° C. or higher and 175° C. or lower, and even more preferably 150° C. or higher and 175° C. or lower. The melting point of the vinylidene fluoride polymer depends on the crystallinity of the vinylidene fluoride polymer, and the higher the crystallinity, the higher the melting point.

[0028] The melting point of the vinylidene fluoride polymer can be determined by calorimetry using a differential scanning calorimeter (DSC). Specifically, the vinylidene fluoride polymer is heated from 30°C to 230°C at 5°C / min (first heating), cooled from 230°C to 30°C at 5°C / min (first cooling), and further heated from 30°C to 230°C at 5°C / min (second heating), and the melting peak is determined by DSC. The maximum melting peak temperature Tm1 observed in the first heating is determined as the melting point of the vinylidene fluoride polymer.

[0029] Furthermore, the vinylidene fluoride polymer preferably has a peak area ΔH of 45.0 J / g or more, more preferably 47.0 J / g or more, in a differential scanning calorimetry curve obtained in the first heating in calorimetry by DSC. When the vinylidene fluoride polymer has ΔH in the above range, the amount of crystalline components in the vinylidene fluoride polymer increases, and the vinylidene fluoride polymer composition is less likely to swell or dissolve in NMP at 25° C.

[0030] Here, the weight average molecular weight of the vinylidene fluoride polymer is preferably 100,000 to 10 million, more preferably 200,000 to 5 million, and further preferably 300,000 to 2 million. The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0031] In the vinylidene fluoride polymer composition, the vinylidene fluoride polymer is preferably particulate. When the vinylidene fluoride polymer composition is dispersed in a solvent such as NMP at 25° C., the vinylidene fluoride polymer in the dispersion is often in the form of primary particles. The average primary particle size of the vinylidene fluoride polymer particles determined by dynamic light scattering for the dispersion is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. On the other hand, the average primary particle size is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. When the average primary particle size of the vinylidene fluoride polymer particles is 5 μm or less, settling can be suppressed when dispersed in NMP, and the surface smoothness of the electrode using the particles is likely to be good.

[0032] The average primary particle size is calculated by regularization analysis of the dynamic light scattering method. For example, it can be measured using DelsaMaxCORE manufactured by BECKMAN COULTER in accordance with JIS Z8828, with water as the dispersion medium and a measurement temperature of 25°C. The largest peak obtained by regularization analysis is regarded as the average primary particle size.

[0033] The amount of vinylidene fluoride polymer in the vinylidene fluoride polymer composition is preferably 97% by mass or more and 99.9% by mass or less, and more preferably 98% by mass or more and 99.9% by mass or less. When the amount of vinylidene fluoride polymer is within this range, when the vinylidene fluoride polymer composition is used to form a mixture layer of an electrode, the adhesion between the mixture layer and a current collector can be improved.

[0034] (2) Surfactants As described above, the vinylidene fluoride polymer composition may further contain a specific surfactant. The surfactant may cover the entire periphery of the vinylidene fluoride polymer, or may cover only a part of the periphery. The surfactant may be the same as or different from the surfactant used in the polymerization of the vinylidene fluoride polymer described above.

[0035] Here, the surfactant contained in the vinylidene fluoride polymer composition is preferably a compound whose hydrophobic group is non-perfluorinated and whose hydrophilic group is ionic. When such a surfactant is present around the vinylidene fluoride polymer, the vinylidene fluoride polymer composition is less likely to settle when mixed with a solvent such as NMP, making it easier to obtain an electrode with a smooth surface.

[0036] Here, the hydrophobic group of the surfactant may be any non-perfluoro group, and includes, for example, an alkyl group, an alkylbenzene group, a polyoxyethylene alkyl ether, etc. Among these, polyoxyethylene alkyl ether, lauryl group, etc. are preferred from the viewpoints of affinity with vinylidene fluoride polymer, ease of availability, etc.

[0037] On the other hand, the hydrophilic group is not particularly limited as long as it is an ionic group, and examples thereof include anionic groups such as a carboxy group, a sulfo group, and a sulfate group, and cationic groups such as a quaternary ammonium group, and an alkylamine group. Among these, a sulfate group is preferred from the viewpoint of the stability of the latex in the heating step.

[0038] Specific examples of surfactants in which the hydrophilic group is anionic include ammonium lauryl sulfate, sodium lauryl sulfate, polyoxyethylene lauryl ether acetate, sodium polyoxyethylene lauryl ether acetate, alkylbenzenesulfonic acid, and the like.

[0039] Specific examples of surfactants having a cationic hydrophilic group include stearylamine acetate, stearyltrimethylammonium chloride, etc. The vinylidene fluoride polymer composition may contain only one type of the above surfactant, or may contain two or more types. Among these, anionic surfactants are more preferred.

[0040] The amount of surfactant contained in the vinylidene fluoride polymer composition is preferably 0.001% by mass or more and 3% by mass or less, more preferably 0.01% by mass or more and 2% by mass or less, based on the total amount of the vinylidene fluoride polymer and the surfactant. When the amount of surfactant is 3% by mass or less, when the vinylidene fluoride polymer composition is used to form a mixture layer of an electrode, the adhesion between the mixture layer and a current collector can be improved. The amount of surfactant is 1 Measured by H NMR.

[0041] (3) Physical Properties of Vinylidene Fluoride Polymer Compositions The vinylidene fluoride polymer composition of the present invention may satisfy the above-mentioned physical properties (viscosity of vinylidene fluoride polymer dispersion and change in content when left to stand), but when the vinylidene fluoride polymer composition and NMP are mixed to prepare a vinylidene fluoride polymer dispersion having a vinylidene fluoride polymer content of 6 mass%, it is preferable that the vinylidene fluoride polymer dispersion further satisfies the following shear viscosity. Specifically, the vinylidene fluoride polymer dispersion is heated from 25° C. to 80° C. at a temperature increase rate of 5° C. / min using a parallel plate rheometer (parallel plate: 50 mm, gap distance: 0.5 mm) for 100 s. -1When the shear viscosity is measured at each temperature at a shear rate of 100° C., the temperature at which the shear viscosity reaches 5 times the shear viscosity at 30° C. is preferably 35° C. or more and 60° C. or less. The temperature at which the shear viscosity reaches 5 times the shear viscosity at 30° C. is more preferably 40° C. or more and 60° C. or less, and even more preferably 45° C. or more and 60° C. or less. When the shear viscosity of the vinylidene fluoride polymer dispersion is in the above range, the vinylidene fluoride polymer composition is difficult to swell and dissolve in NMP at low temperatures (less than 35° C.), and is easily swelled and dissolved in NMP when the temperature rises. Therefore, when such a vinylidene fluoride polymer composition is used for the electrode mixture, the viscosity of the electrode mixture during preparation (less than 35° C.) can be kept low, so that the amount of NMP used can be reduced, productivity can be improved, and the vinylidene fluoride polymer composition can swell and dissolve in a solvent when the mixture is dried, thereby obtaining the desired adhesiveness.

[0042] The shear viscosity of the vinylidene fluoride polymer dispersion at 30° C. is preferably 3 mPa·s or more and 100 mPa·s or less, and more preferably 3 mPa·s or more and 20 mPa·s or less. When the shear viscosity of the vinylidene fluoride polymer dispersion at 30° C. is within the above range, the viscosity increase of the electrode mixture containing the vinylidene fluoride polymer composition at low temperatures (less than 35° C.) can be suppressed, and the amount of the dispersion medium (NMP) used can be reduced while maintaining the coatability of the electrode.

[0043] (4) Method for producing vinylidene fluoride polymer composition A vinylidene fluoride polymer composition satisfying the above-mentioned physical properties can be produced, for example, by the following method, however, the method for producing the vinylidene fluoride polymer composition is not limited to the following method.

[0044] The above-mentioned method for producing a vinylidene fluoride polymer composition includes a step of obtaining a latex in which an untreated vinylidene fluoride polymer is dispersed in water (hereinafter also referred to as a "latex preparation step"), and a step of heating the latex at a temperature lower than the melting point of the untreated vinylidene fluoride polymer and at least 20°C lower than the melting point in a state in which a surfactant whose hydrophobic group is non-perfluoro-based and whose hydrophilic group is ionic is present in the latex (hereinafter also referred to as a "heating step"). It is preferable to further include a step of removing water from the latex after heating (hereinafter also referred to as a "drying step"). It is also preferable to carry out a step of adding a surfactant whose hydrophobic group is non-perfluoro-based and whose hydrophilic group is ionic to the latex after the latex preparation step and before the heating step (hereinafter also referred to as a "surfactant addition step"). In addition, other steps may be further included as necessary.

[0045] (Latex preparation process) In the latex preparation step, a latex in which an untreated vinylidene fluoride polymer is dispersed in water is prepared. In this specification, the untreated vinylidene fluoride polymer refers to a vinylidene fluoride polymer prepared by a general method, which is not subjected to a heat treatment without the intention of drying after preparation of the vinylidene fluoride polymer, and is not mixed with other components. The untreated vinylidene fluoride polymer has substantially the same composition as the vinylidene fluoride polymer described above. However, the untreated vinylidene fluoride polymer is heated in a heating step described below, and the crystal state, etc. of the untreated vinylidene fluoride polymer changes, so that the physical properties, etc. of the untreated vinylidene fluoride polymer are different from those of the vinylidene fluoride polymer described above.

[0046] The untreated vinylidene fluoride polymer may be a homopolymer of vinylidene fluoride or a copolymer of vinylidene fluoride and another monomer. The melting point (hereinafter also referred to as "Tm") of the untreated vinylidene fluoride polymer is preferably 130°C or higher, more preferably 140°C or higher and 175°C or lower, and even more preferably 150°C or higher and 175°C or lower. The melting point of the untreated vinylidene fluoride polymer can be measured in the same manner as the above-mentioned method for measuring the melting point of the vinylidene fluoride polymer.

[0047] As a method for preparing a latex containing untreated vinylidene fluoride and water, a commercially available untreated vinylidene fluoride polymer may be dispersed in water by a known dispersion method. Alternatively, an untreated vinylidene fluoride polymer prepared by a suspension polymerization method, an emulsion polymerization method, a solution polymerization method, a microsuspension polymerization method, or the like may be dispersed in water by a known dispersion method. The untreated vinylidene fluoride polymer may be finely pulverized by freeze-pulverization, classification, or the like, and then mixed with water.

[0048] On the other hand, vinylidene fluoride and, if necessary, other monomers may be polymerized in water by emulsion polymerization, and the resulting polymer may be used as a latex. In the emulsion polymerization method, vinylidene fluoride and, if necessary, other monomers, water, and an emulsifier are mixed, and a water-soluble polymerization initiator is added to the mixture to polymerize vinylidene fluoride and other monomers, etc. Known compounds can be used as the emulsifier and polymerization initiator.

[0049] The emulsion polymerization method may be a soap-free emulsion polymerization method, a mini-emulsion polymerization method, or the like. The soap-free emulsion polymerization method is a method of emulsion polymerization without using a normal emulsifier as described above. The mini-emulsion polymerization method is a method of applying a strong shearing force using an ultrasonic oscillator or the like to finely divide oil droplets of a monomer such as vinylidene fluoride to a submicron size, and then polymerizing the resulting mixture. At this time, a known hydrophobe is added to the mixture in order to stabilize the finely divided oil droplets of the monomer.

[0050] In any of the above emulsion polymerization methods, a chain transfer agent may be used to adjust the degree of polymerization of the resulting untreated vinylidene fluoride polymer, and a pH adjuster may be used as necessary.

[0051] If necessary, other optional components such as an antisettling agent, a dispersion stabilizer, a corrosion inhibitor, a mildew inhibitor, a wetting agent, etc. The amount of these optional components added is preferably 5 ppm to 10 parts by mass, more preferably 10 ppm to 7 parts by mass, based on 100 parts by mass of the total amount of all monomers used in the polymerization.

[0052] Here, the content of untreated vinylidene fluoride polymer in the latex is preferably 5% by mass or more and 70% by mass or less, more preferably 10% by mass or more and 60% by mass or less. When the content of untreated vinylidene fluoride polymer is 5% by mass or more, the drying step described below can be efficiently carried out. On the other hand, when it is 70% by mass or less, the latex tends to be stable.

[0053] The average primary particle size of the untreated vinylidene fluoride polymer in the latex determined by dynamic light scattering is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. On the other hand, the average primary particle size is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. The average primary particle size of the untreated vinylidene fluoride polymer in the latex can be specified in the same manner as the average primary particle size of the vinylidene fluoride polymer described above.

[0054] (Surfactant addition process) A surfactant addition step may be carried out to add a surfactant to the latex prepared in the above-mentioned latex preparation step. The surfactant to be added is a compound whose hydrophobic group is non-perfluoro and whose hydrophilic group is ionic. Only one type of surfactant may be added, or two or more types may be added. If the latex prepared by the emulsion polymerization method contains a sufficient amount of a surfactant whose hydrophobic group is non-perfluoro and whose hydrophilic group is ionic, and the above surfactant is present in the latex before the heat treatment step, the surfactant addition step is not necessarily required. If the above surfactant is present in the latex, the stability in the subsequent heating step is improved, making appropriate treatment possible, and when the vinylidene fluoride polymer composition obtained is dispersed in NMP, it is less likely to settle.

[0055] The amount of surfactant added is preferably 0.001 to 3 parts by mass, more preferably 0.01 to 2 parts by mass, based on 100 parts by mass of the total amount of untreated vinylidene fluoride polymer in the latex. If the amount of surfactant is excessively large, when the vinylidene fluoride polymer composition obtained is used in the mixture layer, the adhesion between the mixture layer and the current collector may decrease, but if the amount is 3 parts by mass or less, the effect on the adhesion is small. On the other hand, if the amount is 0.1 parts by mass or more, the latex becomes more stable during heat treatment. Incidentally, the excess components of the surfactant added in this step may be removed by dialysis or the like after the heat treatment step described below.

[0056] When the surfactant is added, the temperature of the latex is preferably 15°C or higher and 120°C or lower, more preferably 15°C or higher and 100°C or lower. Furthermore, it is preferable to thoroughly stir the latex during and after the addition of the surfactant. When the temperature of the latex is 15°C or higher, the workability is improved. Furthermore, when the temperature of the latex is 120°C or lower, there is an advantage that the latex is easily stabilized and the surfactant to be added does not need to be pressurized.

[0057] (Heating process) In the heating step, the latex is heated to a temperature lower than the melting point (Tm) of the untreated vinylidene fluoride polymer and not lower than Tm-20°C (but not lower than 100°C) in the presence of the surfactant. The heating temperature is preferably not higher than Tm-5°C and not lower than Tm-15°C, and more preferably not higher than Tm-8°C and not lower than Tm-12°C.

[0058] Heating at the above temperatures causes a part of the surface of the untreated vinylidene fluoride polymer to crystallize, decreasing the swelling and solubility in NMP, i.e., when the vinylidene fluoride polymer composition is dispersed in NMP as described above, the viscosity is less likely to increase.

[0059] The heating time is preferably from 10 seconds to 20 hours, more preferably from 1 minute to 10 hours, and even more preferably from 10 minutes to 5 hours. When the heating time is within this range, the crystal state of the untreated vinylidene fluoride polymer is easily changed sufficiently, and a vinylidene fluoride polymer satisfying the above-mentioned physical properties can be obtained.

[0060] The heating method is not particularly limited, and the latex may be heated without stirring or with stirring. The heating device is also not particularly limited. The latex may be heated under pressure using an autoclave or the like.

[0061] After the heat treatment, excess surfactant contained in the latex may be removed by dialysis, salting out, acid precipitation, etc. For example, dialysis can be performed by injecting the heat-treated latex into a cellulose dialysis membrane, immersing the dialysis membrane together with the latex in a water tank filled with pure water, and replacing the pure water in the tank at regular intervals.

[0062] (drying process) In the drying step, water is removed from the latex after the heating. The method for removing water is not particularly limited, but it is preferable to dry at a temperature that does not affect the physical properties of the vinylidene fluoride polymer composition in the latex. The drying step may be performed under atmospheric pressure or under reduced pressure. The vinylidene fluoride polymer composition described above is obtained by the drying. In addition, the device for removing water is not particularly limited, and a tray dryer, a conical dryer, a fluidized bed dryer, a flash dryer, a spray dryer, a freeze dryer, etc. can be used.

[0063] 2.Resin composition The vinylidene fluoride polymer composition may be used as it is in the electrode mixture for forming the mixture layer described below. On the other hand, a resin composition containing the vinylidene fluoride polymer composition and another resin that dissolves during the preparation of the mixture layer described below may be prepared and used in the electrode mixture for forming the mixture layer. By using a resin composition containing the vinylidene fluoride polymer composition and another resin in the electrode mixture, the viscosity of the electrode mixture can be easily adjusted to a desired range.

[0064] The other resin may be any resin that is different from the vinylidene fluoride polymer composition and dissolves in a solvent used in preparing the mixture layer described below. Examples include vinylidene fluoride polymers other than the vinylidene fluoride polymers, polyacrylonitrile, nitrile rubber, poly(meth)acrylic acid and its esters, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, and cellulose ether. The other resin may contain only one of these, or may contain two or more of them.

[0065] The other resin is preferably particulate, and the median diameter determined by the laser diffraction scattering method is preferably 0.1 μm to 500 μm, more preferably 0.5 μm to 200 μm. The median diameter can be measured by the laser diffraction scattering method. For example, it can be measured using Microtrack MT3300EXII (measurement range 0.02 to 2000 μm) manufactured by Microtrack Bell and an automatic sample circulator, using water as a dispersion medium. In addition, when measuring, the other resin particles may be wetted with ethanol and then dispersed in water.

[0066] Furthermore, the amount of the other resin is preferably 5 parts by mass or more and 2000 parts by mass or less, and more preferably 30 parts by mass or more and 300 parts by mass or less, per 100 parts by mass of the vinylidene fluoride polymer composition.

[0067] The method of mixing the vinylidene fluoride polymer composition with the other resin is not particularly limited, and may be, for example, dry mixing or wet mixing. After mixing the vinylidene fluoride polymer composition with the other resin, the mixture may be processed into particles of a desired size by a roller compactor, a pharmapacter, a chilsonator, a spray dryer, a fluidized bed granulator, or the like.

[0068] 3. Electrode The vinylidene fluoride polymer composition or resin composition described above can be used as a binder for a mixture layer of an electrode of a secondary battery or the like. The electrode includes, for example, a current collector and a mixture layer disposed on the current collector. In this case, the vinylidene fluoride polymer composition or resin composition described above can be used to form the mixture layer. The electrode may be for a positive electrode or a negative electrode. (1) Current collector The negative and positive electrode current collectors are terminals for taking out electricity. The material of the current collector is not particularly limited, and metal foil or metal mesh of aluminum, copper, iron, stainless steel, steel, nickel, titanium, etc. can be used. In addition, the above metal foil or metal mesh may be applied to the surface of another medium.

[0069] (2) Electrode mixture and mixture layer On the other hand, the mixture layer can be a layer obtained by mixing the vinylidene fluoride polymer composition or resin composition, an active material, and a solvent to prepare an electrode mixture, applying the electrode mixture onto a current collector, and drying the electrode mixture. The mixture layer may be formed on only one surface of the current collector, or may be disposed on both surfaces.

[0070] The mixture layer may contain, for example, the vinylidene fluoride polymer composition (or a resin composition containing the same) and an active material, and may contain other components as necessary. Examples of the other components include a conductive assistant and various additives.

[0071] The amount of the vinylidene fluoride polymer composition relative to the total amount of the mixture layer is preferably 0.2% by mass to 20% by mass, more preferably 0.4% by mass to 10% by mass, and even more preferably 0.6% by mass to 4% by mass. When the amount of the vinylidene fluoride polymer composition is within this range, for example, the adhesion between the mixture layer and the current collector tends to be good.

[0072] The active material contained in the mixture layer is not particularly limited, and for example, a conventionally known active material for a negative electrode (negative electrode active material) or active material for a positive electrode (positive electrode active material) can be used.

[0073] Examples of the negative electrode active material include carbon materials such as artificial graphite, natural graphite, graphitization-resistant carbon, graphitization-prone carbon, activated carbon, or those obtained by firing and carbonizing phenolic resins, pitch, etc.; metal and alloy materials such as Cu, Li, Mg, B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Cd, Ag, Zn, Hf, Zr, and Y; and metal oxides such as GeO, GeO2, SnO, SnO2, PbO, PbO2, etc.

[0074] On the other hand, examples of the positive electrode active material include lithium-containing lithium-based positive electrode active materials. Examples of the lithium-based positive electrode active material include composite metal chalcogen compounds represented by the general formula LiMY2 (M is one or more of transition metals such as Co, Ni, Fe, Mn, Cr, and V, Y is a chalcogen element such as O and S) such as LiCoO2, LiNi x Co 1-x O2 (0 < x ≦ 1); composite metal oxides having a spinel structure such as LiMn2O4; and olivine-type lithium compounds such as LiFePO4; etc.

[0075] The amount of the active material relative to the total amount of the binder layer is preferably 90% by mass or more and 99.9% by mass or less, more preferably 92% by mass or more and 99% by mass or less, and even more preferably 94% by mass or more and 99% by mass or less. When the amount of the active material is within this range, for example, a sufficient charge-discharge capacity can be obtained, and the battery performance is likely to be good.

[0076] Also, the conductive assistant is not particularly limited as long as it is a compound that can further enhance the conductivity between the active materials or between the active material and the current collector. Examples of the conductive assistant include acetylene black, ketjen black, carbon black, graphite powder, carbon nanofiber, carbon nanotube, and carbon fiber, etc.

[0077] The amount of the conductive assistant can be arbitrarily set according to the type of the conductive assistant and the type of the battery. In order to improve both the conductivity and the dispersibility of the conductive assistant, in one example, the amount is preferably 0.1% by mass to 15% by mass or less, more preferably 0.1% by mass to 7% by mass or less, and even more preferably 0.1% by mass to 5% by mass, based on the total amount of the active material, the vinylidene fluoride polymer composition, and the conductive assistant.

[0078] Examples of the additives include phosphorus compounds, sulfur compounds, organic acids, amine compounds, nitrogen compounds such as ammonium compounds, organic esters, various silane-based, titanium-based and aluminum-based coupling agents, etc. These are used in amounts that do not impair the object and effect of the present invention.

[0079] Here, the thickness of the mixture layer is not particularly limited and can be any thickness. Usually, the thickness is preferably 30 to 600 μm per side, more preferably 50 to 500 μm, and even more preferably 70 to 350 μm. The weight per unit area of ​​the electrode mixture layer is usually 50 to 1000 g / m 2 is preferable, and 100 to 500 g / m 2 is more preferred.

[0080] (Method of forming mixture layer) The mixture layer can be formed by carrying out the steps of preparing an electrode mixture by mixing the vinylidene fluoride polymer composition or resin composition, an active material, a solvent (dispersion medium), and, if necessary, a conductive assistant and various additives, applying the electrode mixture onto a current collector, and drying the applied mixture.

[0081] The electrode mixture may be prepared by mixing the vinylidene fluoride polymer composition or resin composition, the active material, the solvent (dispersion medium), and, if necessary, the conductive assistant and various additives at once, or by mixing some of the components first and then mixing the remaining components. In this case, it is preferable to mix the components using a mixer equipped with a temperature control device so that the temperature of the mixture layer composition does not rise excessively.

[0082] In addition, the solvent (dispersion medium) may disperse the vinylidene fluoride polymer composition or the vinylidene fluoride polymer composition in the resin composition and the active material, and may dissolve the vinylidene fluoride polymer composition when the vinylidene fluoride polymer composition or the vinylidene fluoride polymer composition in the resin composition is heated below the melting point. Usually, aprotic polar solvents such as NMP are preferred, and NMP is preferred. The amount of the solvent is preferably 20 parts by mass or more and 150 parts by mass or less, more preferably 20 parts by mass or more and 100 parts by mass or less, even more preferably 20 parts by mass or more and 45 parts by mass or less, and particularly preferably 20 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the active material. The vinylidene fluoride polymer composition has low swelling and solubility in NMP. Therefore, even if the amount of the solvent is 150 parts by mass or less, the viscosity of the electrode mixture can be kept within the desired range. When the above-mentioned resin composition is used as an electrode mixture, the polymers other than the vinylidene fluoride polymer composition in the electrode mixture dissolve in the solvent and function as a dispersion stabilizer.

[0083] The viscosity of the electrode mixture is preferably 0.5 Pa·s or more and 50 Pa·s or less, and more preferably 2 Pa·s or more and 30 Pa·s or less. The viscosity of the electrode mixture is measured using an E-type viscometer or the like. If the viscosity of the electrode mixture is 0.5 Pa·s or more, dripping when applying the electrode mixture to obtain an electrode, uneven electrode application, and delayed drying after application can be prevented, and the workability of electrode preparation tends to be good. In addition, if the viscosity of the electrode mixture is 50 Pa·s or less, the applicability of the electrode tends to be good.

[0084] The method for applying the electrode mixture is not particularly limited, and methods such as a doctor blade method, a reverse roll method, a comma bar method, a gravure method, an air knife method, a die coating method, and a dip coating method can be used.

[0085] Here, it is preferable to maintain the temperature of the electrode mixture at 60° C. or less from preparation to application. It is more preferable to maintain the temperature of the electrode mixture at 0° C. or more and 50° C. or less, and even more preferable to maintain the temperature at 5° C. or more and 40° C. or less. As described above, the vinylidene fluoride polymer composition is difficult to swell and dissolve in a solvent (dispersion medium) such as NMP at 25° C., but becomes more soluble as the temperature rises. Therefore, by maintaining the temperature of the electrode mixture at 60° C. or less from preparation to application, the viscosity of the electrode mixture can be maintained within a desired range.

[0086] After the electrode mixture is applied, it is heated at an arbitrary temperature to dry the solvent (dispersion medium). Drying may be performed multiple times at different temperatures. Pressure may be applied during drying. The heating temperature is preferably 60°C or higher and 200°C or lower, more preferably 80°C or higher and 150°C or lower. When the heating temperature is within this range, the vinylidene fluoride polymer composition in the electrode mixture dissolves in the solvent (dispersion medium), increasing the fluidity. Then, an electrode having the desired adhesiveness can be obtained. The heating time is preferably 30 seconds or higher and 200 minutes or lower, more preferably 60 seconds or higher and 150 minutes or lower.

[0087] After the electrode mixture is applied and dried, a pressing process may be further carried out, which can improve the electrode density. EXAMPLES

[0088] The present invention will be described in more detail below with reference to examples, which should not be construed as limiting the scope of the present invention.

[0089] 1. Preparation of vinylidene fluoride polymer composition [Examples 1, 3, 5, 7, and 9, and Comparative Examples 2 and 4] A vinylidene fluoride polymer composition was obtained by carrying out the following latex preparation step, surfactant addition step, heat treatment step, and drying step. The type of surfactant added in the surfactant treatment step and the temperature in the heat treatment step in each Example or Comparative Example are shown in Table 1.

[0090] [Examples 2, 4, 6, 8, and 10, and Comparative Examples 3 and 5] A vinylidene fluoride polymer composition was obtained by carrying out the following latex preparation step, surfactant addition step, heat treatment step, dialysis step, and drying step. The type of surfactant added in the surfactant treatment step and the temperature in the heat treatment step in each Example or Comparative Example are shown in Table 1.

[0091] [Comparative Example 1] After the latex preparation process described below, a drying process was carried out without carrying out a surfactant addition process or a heat treatment process, to obtain a vinylidene fluoride polymer composition.

[0092] [Comparative Examples 6 to 8] After the latex preparation process described below, a drying process was carried out without carrying out a surfactant addition process or a heat treatment process, and then a powder heat treatment process was further carried out to obtain a vinylidene fluoride polymer composition.

[0093] [Comparative Example 9] After the latex preparation step and surfactant addition step described below, a drying step was carried out without carrying out a heat treatment step to obtain a vinylidene fluoride polymer composition.

[0094] [Comparative Example 10] After the latex preparation step described below, a heat treatment step and a drying step were carried out without carrying out a surfactant treatment step, to obtain a vinylidene fluoride polymer composition.

[0095] Latex preparation process 330 parts by mass of ion-exchanged water was placed in the autoclave, and degassed by bubbling with nitrogen for 30 minutes. Next, 0.1 parts by mass of disodium hydrogen phosphate and 0.8 parts by mass of ammonium perfluorooctanoate (PFOA) were charged, and the pressure was increased to 4.5 MPa, and nitrogen replacement was performed three times. Then, 0.05 parts by mass of ethyl acetate and 30 parts by mass of vinylidene fluoride (VDF) were added to the autoclave. The temperature was raised to 80°C while stirring. A 5% by mass aqueous solution of ammonium persulfate (APS) was added so that the amount of APS was 0.05 parts by mass, and polymerization was started. The pressure inside the autoclave at this time was 2.5 MPa. 70 parts by mass of VDF were continuously added immediately after the start of polymerization so that the pressure inside the autoclave was maintained at 2.5 MPa at the start of polymerization. After the addition was completed, the polymerization was completed when the pressure dropped to 1.5 MPa, and a latex containing vinylidene fluoride polymer A was obtained. The solid content of the obtained latex (content of vinylidene fluoride polymer A) was 21.5% by mass. The solid content was calculated by putting about 5 g of the latex into an aluminum cup, drying it at 80° C. for 3 hours, and measuring the weight before and after drying.

[0096] Surfactant addition process At 25°C, 800 g of vinylidene fluoride polymer A latex was dispensed into an autoclave, and the surfactants shown in Table 1 were weighed out and added in the amounts shown in Table 1 (amounts relative to the vinylidene fluoride polymer). 70 g of pure water was used to wash away the sample adhering to the weighed wall of the container. Regarding the types of surfactants in Table 1, ALS (ammonium lauryl sulfate) represents Kao Corporation's Latemul (registered trademark) AD-25, SLS (sodium lauryl sulfate) represents Kao Corporation's Emal (registered trademark) 0, and POELEA (polyoxyethylene lauryl ether acetic acid) represents Kao Corporation's AKYPO (registered trademark) RLM45.

[0097] Heat treatment process The latex containing the surfactant was placed in an autoclave, sealed, and heated to the temperature shown in Table 1 with a jacketed temperature controller while stirring at 500 rpm. The treatment temperature was then maintained for 1 hour. After the treatment was completed, the jacketed temperature controller was removed, and the temperature was lowered to 30°C by air cooling while still sealed. When the temperature fell below 30°C, the autoclave was opened, and the heat-treated latex was collected.

[0098] ·Dialysis process The latex after heat treatment was poured into a cellulose dialysis membrane (manufactured by Sekisui Medical Co., Ltd., model number: 521737, molecular weight cutoff: 12000-14000) and immersed together with the dialysis membrane in a water tank filled with pure water. The pure water inside was replaced at regular intervals (1-6 hours) and the membrane was left to stand for 2 days. The latex inside the membrane was then collected.

[0099] ·Drying process Approximately 70 mL of the latex obtained (after the latex preparation process, surfactant addition process, heat treatment process, or dialysis process) was placed in a 300 mL eggplant flask, and the content liquid was frozen using liquid nitrogen. Next, the frozen eggplant flask was attached to a freeze dryer (Tokyo Rikakikai FDU-2110) and left for approximately 8 hours with the inside in a reduced pressure state. After that, the eggplant flask was removed from the freeze dryer, and the powder was collected.

[0100] Powder heat treatment process After the latex preparation process, the PVDF powder obtained only through the drying process was thinly spread on a SUS tray (30cm x 21cm x 2cm) by about 8g. After that, it was covered with aluminum foil, placed in a hot air circulation oven (HT210 constant temperature bath with explosion vent, manufactured by ETAC) set at the processing temperature, and left to stand for 1 hour while circulating with nitrogen. After that, the temperature holding function was stopped and the temperature was lowered to 100°C, and then it was taken out and cooled to room temperature to collect the powder.

[0101] 2. Evaluation of vinylidene fluoride polymer compositions The vinylidene fluoride polymer compositions prepared as above were subjected to the following evaluations.

[0102] (1) Rate of change in content of vinylidene fluoride polymer dispersion 0.9 g of the vinylidene fluoride polymer composition obtained in each Example or Comparative Example was mixed with 14.1 g of N-methyl-2-pyrrolidone (NMP) to prepare a vinylidene fluoride polymer dispersion having a vinylidene fluoride polymer content of 6 mass %. At this time, mixing was performed so that the temperature of the vinylidene fluoride polymer dispersion was always in the range of 20 to 30°C.

[0103] Thereafter, the vinylidene fluoride polymer dispersion was stirred at 25°C for 10 minutes using a magnetic stirrer. A portion of the vinylidene fluoride polymer dispersion in the stirring treatment state was collected while continuing to stir, and the vinylidene fluoride polymer content in the dispersion was measured (vinylidene fluoride polymer content W1 before standing). Thereafter, the vinylidene fluoride polymer dispersion with a height of 5 cm was left standing for 15 minutes in a cylindrical container with a diameter of 1 cm at 25°C. Then, the vinylidene fluoride polymer dispersion in the upper 40% by volume region of the vinylidene fluoride polymer dispersion was separated, and the vinylidene fluoride polymer content was measured (vinylidene fluoride polymer content W2 after standing). The rate of change in content was calculated using the following formula. The vinylidene fluoride polymer content in the dispersion was calculated from the ratio of the weight before and after drying when the collected dispersion was left to stand for 2 hours in a thermostatic chamber at 130°C with nitrogen circulation. The results are shown in Table 2.

number

[0104] (2) Ratio of viscosity of vinylidene fluoride polymer dispersion to viscosity of NMP (X / Y) Similarly to the measurement of the rate of change in content, a vinylidene fluoride polymer dispersion with a vinylidene fluoride polymer content of 6 mass% was prepared. Then, the viscosity Y of NMP at 30°C and the viscosity X of the vinylidene fluoride polymer dispersion at 30°C were measured using a TA Instruments G2 rheometer (parallel plate: 50 mm, gap distance: 0.5 mm) at a shear rate of 100 s -1The viscosity was measured at 100° C. for 30 seconds. The value of X / Y was then calculated. The results are shown in Table 2. Table 2 also shows the viscosity X of the vinylidene fluoride polymer dispersion at 30° C.

[0105] (3) The temperature at which the shear viscosity becomes five times the shear viscosity at 30°C (thickening temperature) Similarly to the measurement of the rate of change in content, a vinylidene fluoride polymer dispersion with a vinylidene fluoride polymer content of 6 mass% was prepared. The temperature of the vinylidene fluoride polymer dispersion was then raised from 25°C to 80°C at a rate of 5°C per minute, and the viscosity at each temperature was measured at a shear rate of 100 s using a TA Instruments G2 rheometer (parallel plate: 50 mm, gap distance: 0.5 mm). -1 The viscosity at each temperature was then divided by the viscosity at 30°C to determine the temperature at which the shear viscosity reached five times the viscosity at 30°C. The results are shown in Table 2.

[0106] (4) Differential scanning calorimetry (DSC) The vinylidene fluoride polymer composition was subjected to differential scanning calorimetry in accordance with JIS K7122-1987 using a DSC1 manufactured by Mettler Toledo Co., Ltd. Specifically, about 10 mg of a sample was precisely weighed out in an aluminum sample pan, and nitrogen was supplied at a flow rate of 50 mL / min, and the measurement was performed under the following conditions. First temperature rise: From 30°C to 230°C at a rate of 5°C per minute First cooling: From 230℃ to 30℃ at a rate of 5℃ per minute Second temperature rise: From 30°C to 230°C at a rate of 5°C per minute The maximum melting peak temperature in the first heating was designated as Tm1, and the maximum melting peak temperature in the second heating was designated as Tm2. The peak area in the differential scanning calorimetry curve obtained in the first heating was designated as ΔH. The results are shown in Table 3.

[0107] (5) Measurement of residual surfactant amount The amount of residual surfactant in the vinylidene fluoride polymer composition was measured by the following method ( 1 The results are shown in Table 3. (1 H NMR measurement) ·Device Bruker AVANCE AC 400FT NMR Spectrometer Measurement conditions Frequency: 400MHz Measurement solvent: DMSO-d6 Measurement temperature: 25℃ 1 The amount of each component present was calculated based on the integrated intensity of a signal observed at 0.85 ppm, which was mainly attributable to the alkyl chain end of the surfactant, and signals observed at 2.24 ppm and 2.87 ppm, which were mainly attributable to vinylidene fluoride, in the H NMR spectrum, and the ratio of the amount of the residual surfactant to the total amount of the vinylidene fluoride polymer composition was calculated.

[0108] 3. Formation of Electrodes (1) Preparation of Polymer B In a 2-liter autoclave, 925 g of ion-exchanged water, 0.65 g of Metolose (registered trademark) SM-100 (manufactured by Shin-Etsu Chemical Co., Ltd.), 4.0 g of 50 wt% diisopropyl peroxydicarbonate-Flon 225cb solution, 421 g of vinylidene fluoride, and 0.22 g of acryloyloxypropyl succinic acid were charged, and the temperature was raised to 26°C in 1 hour. Thereafter, while maintaining the temperature at 26°C, a 3 wt% aqueous solution of acryloyloxypropyl succinic acid was gradually added at a rate of 0.19 g per minute. A total of 2.92 g of acryloyloxypropyl succinic acid was added, including the amount added at the beginning. The polymerization was stopped at the same time as the addition of the aqueous solution of acryloyloxypropyl succinic acid was completed. The obtained polymer slurry was dehydrated, washed with water, and further dried at 80°C for 20 hours to obtain polymer B. The weight average molecular weight was 800,000, the median diameter (D50) was 180 μm, and the melting point was 169.3°C.

[0109] (2) Preparation of Binder Composition 85 parts by mass of NMP at 25° C. was weighed into an Erlenmeyer flask. For the vinylidene fluoride polymer compositions of Examples 1 to 10 and Comparative Examples 7, 8, and 10, 15 parts by mass of NMP was added while stirring with a magnetic stirrer, and stirred at 25° C. for 30 minutes to prepare a 15% by mass binder composition.

[0110] On the other hand, each of the vinylidene fluoride polymer compositions of Comparative Examples 1 to 6 and 9 was added to NMP so as to give a concentration of 6 mass %, and the mixture was stirred in the same manner as above to prepare a binder composition.

[0111] (3) Preparation of Polymer B Solution 94 parts by mass of NMP at 25° C. was weighed into an Erlenmeyer flask, and 6 parts by mass of the above-mentioned polymer B was added thereto while stirring with a magnetic stirrer. The mixture was heated and stirred at 50° C. for 5 hours to prepare a solution of polymer B.

[0112] (4) Preparation of electrode mixture A dispersion liquid containing the active material was prepared using lithium cobalt oxide (CH) manufactured by Nippon Chemical Industry Co., Ltd. as the positive electrode active material, carbon black (SUPER P) manufactured by Imerys Graphite & Carbon Co., Ltd. as the conductive assistant, and N-methyl-2-pyrrolidone (NMP) with a purity of 99.8% as the dispersion medium. The solid content ratio in the electrode mixture was CH:SUPER P:vinylidene fluoride polymer composition (PVDF):polymer B=100:2:1:1. The binder composition described above was used for PVDF.

[0113] Specifically, 20 g of C5H and 0.4 g of SUPER P were precisely weighed into a polypropylene container, and mixed at 800 rpm for 1 minute using a Thinky mixer (Awatori Rentaro). After cooling the sample temperature to 25°C, 3.33 g of polymer B solution and 1.09 g of NMP were added as dispersion stabilizers to adjust the non-volatile content of the electrode mixture to 83% by mass. After mixing with a spatula, the mixture was kneaded at 2000 rpm for 3 minutes using Awatori Rentaro (primary kneading process). After cooling the sample temperature to 25°C again, the binder composition was added to the stirred liquid. The amount of the binder composition added was 1.33 g for the binder composition with a vinylidene fluoride polymer composition content of 15% by mass, and 3.33 g for the binder composition with a vinylidene fluoride polymer composition content of 6% by mass. The amount of NMP was further adjusted so that the non-volatile content of the electrode mixture was the value shown in Table 3. After mixing with a spatula, the mixture was kneaded for 2 minutes at 800 rpm using a foaming mixer to obtain an electrode mixture (secondary kneading process). The sample temperature after kneading was 28°C. After preparation of the mixture, the electrode mixture was stored at 25°C. The electrode mixture was measured using an E-type viscometer (Toki Sangyo Co., Ltd., "RE-215 model") at 25°C and a shear rate of 2 s -1 The viscosity was measured for 300 seconds at 100°C, and it was confirmed that the viscosity after 300 seconds was approximately 4 to 9 Pa·s.

[0114] (5) Electrode manufacturing The obtained electrode mixture was applied to an aluminum foil having a thickness of 15 μm by a bar coater and dried to obtain an electrode. The electrode was dried at 110° C. for 30 minutes in a nitrogen circulating thermostatic chamber. The weight of each electrode was 200±20 g / m 2 The electrode was used as an evaluation electrode.

[0115] 4. Electrode Evaluation The peel strength of the mixture layer and the surface smoothness of the obtained electrode were evaluated by the following methods. The results are shown in Table 3.

[0116] (1) Peel strength of the mixture layer The peel strength of the mixture layer was measured by attaching the surface on which the mixture layer was formed to a thick plastic plate (made of acrylic resin, 5 mm thick) with double-sided tape and performing a 90° peel strength test in accordance with JIS K6854-1. The test speed was 10 mm per minute.

[0117] (2) Arithmetic mean roughness of electrode surface The arithmetic mean roughness Ra was measured using a FORMTRACER SV-C3200 (manufactured by Mitutoyo Corporation) in accordance with JIS B 0601:2013. Reference length: 2.5 mm Measurement speed: 1.0mm / s Cutoff: λc=2.5mm, λs=8μm

[0118] [Table 1]

[0119] [Table 2]

[0120] [Table 3]

[0121] As shown in Tables 1 to 3 above, when the ratio of the viscosity X of the vinylidene fluoride polymer dispersion (vinylidene fluoride polymer content 6% by mass) at 30°C to the viscosity Y of N-methyl-2-pyrrolidone at 30°C was 20 or less, and when the vinylidene fluoride polymer dispersion (vinylidene fluoride polymer content 6% by mass) was allowed to stand for 15 minutes, the rate of change in the content of the upper 40% by volume before and after standing was 2% by mass or less, the peel strength was high and the arithmetic mean roughness of the electrode surface was low even when the non-volatile component amount of the composite layer composition was 75% by mass or more (Examples 1 to 10).

[0122] On the other hand, when the vinylidene fluoride polymer composition was dissolved in NMP (Comparative Examples 1 to 6, and 9), the smoothness of the electrode surface was likely to be good, but the viscosity of the mixture composition increased, and the non-volatile content of the mixture composition could not be increased to 75% by mass or more. Furthermore, even when the vinylidene fluoride polymer composition was dispersed in NMP, when the vinylidene fluoride polymer dispersion (vinylidene fluoride polymer content of 6% by mass) was allowed to stand for 15 minutes, if the change in the content of the upper 40% by volume before and after standing was more than 2% by mass, the smoothness of the electrode surface was likely to decrease (Comparative Examples 7, 8, and 10). [Industrial Applicability]

[0123] The vinylidene fluoride polymer composition of the present invention is difficult to swell or dissolve in N-methyl-2-pyrrolidone. In addition, the vinylidene fluoride polymer composition can form an electrode having a smooth surface. Therefore, the vinylidene fluoride polymer composition is very useful for producing electrodes for secondary batteries.

Claims

1. A vinylidene fluoride polymer composition comprising a vinylidene fluoride polymer having a melting point of 130° C. or higher and a surfactant, When the vinylidene fluoride polymer composition and N-methyl-2-pyrrolidone are mixed to prepare a vinylidene fluoride polymer dispersion having a vinylidene fluoride polymer content of 6 mass%, A parallel plate rheometer was used to measure the shear rate of 100 s -1 The viscosity of N-methyl-2-pyrrolidone at 30°C measured by a parallel plate rheometer at a shear rate of 100 s -1 the ratio of the viscosity of the vinylidene fluoride polymer dispersion at 30° C. measured by a change rate of the vinylidene fluoride polymer content in an upper 40% by volume region of the vinylidene fluoride polymer dispersion before and after stirring the vinylidene fluoride polymer dispersion and allowing it to stand for 15 minutes is 2% by mass or less; Vinylidene fluoride polymer compositions.

2. The vinylidene fluoride polymer contains 90 mass% or more of structural units derived from vinylidene fluoride. The vinylidene fluoride polymer composition of claim 1.

3. The surfactant is a surfactant in which the hydrophobic group is non-perfluorinated and the hydrophilic group is ionic. The vinylidene fluoride polymer composition according to claim 1 or 2.

4. the amount of the surfactant is 0.001 parts by mass or more and 3 parts by mass or less with respect to 100 parts by mass of the total amount of the vinylidene fluoride polymer and the surfactant; The vinylidene fluoride polymer composition of claim 1.

5. The vinylidene fluoride polymer dispersion was heated from 25° C. to 80° C. at a temperature increase rate of 5° C. / min, and the shear viscosity of the vinylidene fluoride polymer dispersion was measured at a shear rate of 100 s -1 When measured at The temperature at which the shear viscosity becomes 5 times the shear viscosity at 30° C. is 35° C. or higher and 60° C. or lower. The vinylidene fluoride polymer composition according to any one of claims 1 to 4.

6. The vinylidene fluoride polymer composition according to any one of claims 1 to 5, With other resins, Including, the other resin is at least one polymer selected from the group consisting of vinylidene fluoride polymers other than the vinylidene fluoride polymers, polyacrylonitrile, nitrile rubber, poly(meth)acrylic acid and its esters, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, and cellulose ether; Resin composition.

7. Obtaining a latex in which an untreated vinylidene fluoride polymer is dispersed in water; heating the latex at a temperature lower than the melting point of the untreated vinylidene fluoride polymer and equal to or higher than the melting point minus 20° C. (but equal to or higher than 100° C.) in the presence of a surfactant having a hydrophobic group that is non-perfluorinated and a hydrophilic group that is ionic in the latex; Including, The untreated vinylidene fluoride polymer is one which has not been subjected to a heat treatment without the intention of drying after preparation of the vinylidene fluoride polymer, and has not been mixed with any other component. A method for producing a vinylidene fluoride polymer composition.

8. The method further comprises the step of adding the surfactant after the step of obtaining the latex and before the step of heating. A method for producing the vinylidene fluoride polymer composition according to claim 7.

9. The vinylidene fluoride polymer composition according to any one of claims 1 to 5, An active material; A dispersion medium; An electrode mixture comprising:

10. The resin composition according to claim 6, An active material; A dispersion medium; Including, The electrode mixture, wherein the polymer in the resin composition is dissolved in the dispersion medium.

11. A vinylidene fluoride polymer composition according to any one of claims 1 to 5 or a resin composition according to claim 6, An active material; An electrode having a mixture layer comprising:

12. A step of mixing the vinylidene fluoride polymer composition according to any one of claims 1 to 5 or the resin composition according to claim 6, an active material, and a dispersion medium to obtain an electrode mixture; A step of applying the electrode mixture onto a current collector and drying the same; Including, The temperature of the electrode mixture is maintained at 60° C. or less from the preparation to application of the electrode mixture. A method for manufacturing an electrode.

Citation Information

Patent Citations

  • Semiconductive polyvinylidene fluoride resin composition, semiconductive resin molded product and process for production of the molded product

    JP2005350621A

  • Vinylidene fluoride / 2,3,3,3-tetrafluoropropene copolymer

    JP2011527375A

  • Secondary battery separator and secondary battery

    JP2016033913A

  • Vinylidene fluoride-based polymer powder, binder composition, electrode mixture, and manufacturing method of electrode