Perimeter adhesive for improved reliability and reduced stress unevenness in curved displays with cover glass

The use of a glass sheet with edge adhesives of varying moduli in curved display assemblies addresses light leakage issues by maintaining the display's cylindrical shape, thereby improving optical performance.

JP7588142B2Active Publication Date: 2024-11-21CORNING INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022521662
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-17
Filing Date
2020-09-23
Publication Date
2024-11-21
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

Existing methods for forming curved display assemblies using glass sheets suffer from optical deficiencies such as light leakage due to stress unevenness, particularly in backlit displays, as they often use polymers that lack the durability and optical performance of glass.

Method used

A curved display assembly is formed using a glass sheet with a higher modulus adhesive along the edges to maintain a cylindrical shape, reducing stress unevenness by extending these edges beyond the display area, and applying adhesives with varying moduli to manage bending moments.

Benefits of technology

This approach significantly reduces light leakage by maintaining the cylindrical shape of the display, ensuring minimal stress distribution and enhancing optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588142000004
    Figure 0007588142000004
  • Figure 0007588142000005
    Figure 0007588142000005
  • Figure 0007588142000006
    Figure 0007588142000006
Patent Text Reader

Abstract

An embodiment of a curved display assembly is disclosed. The assembly includes a glass sheet having a first major surface and a second major surface. The second major surface defines a first curvature of the glass sheet, the first curvature having a bending axis. The assembly also includes a curved display having a second thickness between the first display surface and the second display surface. The display has a display area and two overhanging edges adjacent to the display area and parallel to the bending axis. A first adhesive bonds the second display surface to the second major surface at the display area. A second adhesive is disposed between each of the two overhanging edges and the second major surface. The second adhesive has a higher modulus of elasticity than the first adhesive. Each overhanging edge extends outside the display area a distance that is at least three times the second thickness of the curved display.
Need to check novelty before this filing date? Find Prior Art

Description

Related Applications

[0001] This application claims the benefit of priority under 35 U.S.C. §119 to U.S. Provisional Application No. 62 / 916,660, filed October 17, 2019, the contents of which are relied upon and incorporated by reference in their entirety herein. [Technical field]

[0002] The present disclosure relates to curved display assemblies including glass and methods for forming the same, and more particularly to curved display assemblies and methods for forming the same that reduce stress variations associated with bending the display. [Background technology]

[0003] Vehicle interiors, equipment, and consumer electronics include curved surfaces that may incorporate displays. Materials used to form such curved surfaces are typically limited to polymers that do not exhibit the durability and optical performance of glass. As such, curved glass sheets are desirable, especially when used as covers for displays. Existing methods for forming such curved display assemblies have drawbacks, including optical defects associated with light leakage from backlit displays. Applicant has therefore recognized a need for curved display assemblies that may incorporate curved glass sheets, and curved displays that do not suffer from light leakage problems. Summary of the Invention

[0004] According to one aspect, an embodiment of the present disclosure relates to a curved display assembly. The curved display assembly includes a glass sheet having a first major surface and a second major surface opposite the first major surface. The glass sheet has a first thickness measured between the first major surface and the second major surface. The second major surface defines a first radius of curvature of the glass sheet, the first radius of curvature having a bending axis. The curved display assembly also includes a curved display having a second thickness between the first display surface and the second display surface. The display comprises a display area and two overhanging edges adjacent to the display area and parallel to the bending axis. The curved display assembly includes a first adhesive bonding the second display surface of the curved display to a second major surface of the glass sheet in the display area. The curved display assembly further includes a second adhesive bonding each of the two overhanging edges to the second major surface of the glass sheet. The second adhesive has a higher modulus of elasticity than the first adhesive. Each overhanging edge extends outside the display area a distance that is at least three times the second thickness of the curved display.

[0005] According to another aspect, an embodiment of the present disclosure relates to a method of forming a curved display assembly. In the method, a glass sheet is provided having a first major surface and a second major surface. The second major surface is opposite to the first major surface. A display is bonded to the second major surface of the glass sheet. The display includes a display area and two overhanging edges adjacent to the display area. The display area is bonded to the second major surface of the glass sheet using a first adhesive, and the two overhanging edges are bonded to the second major surface of the glass sheet using a second adhesive. The second adhesive has a higher elastic modulus than the first adhesive. The method also includes bending the glass sheet and the display at a temperature below a glass transition temperature of the glass sheet to form a curvature in the glass sheet and the display having a bending axis. The two overhanging edges are parallel to the bending axis, and each of the two overhanging edges extends beyond the display area a distance that is at least three times the thickness of the display.

[0006] According to yet another aspect, an embodiment of the present disclosure relates to a method of forming a curved glass article. In the method, a curved glass sheet is provided, the curved glass sheet includes a first major surface and a second major surface. The second major surface is opposite the first major surface and defines a curvature having a bending axis. A display is bent beyond the curvature of the glass sheet. The display includes a display area and two overhanging edges adjacent to the display area and parallel to the bending axis. In the method, the display is bonded to the second major surface of the glass sheet. The display area is bonded to the second major surface of the glass sheet using a first adhesive, and the two overhanging edges are bonded to the second major surface of the glass sheet using a second adhesive. The second adhesive has a higher modulus of elasticity than the first adhesive. Each of the two overhanging edges extends beyond the display area for a distance that is at least three times the thickness of the display.

[0007] Additional features and advantages will be set forth in the following detailed description, and in part will become readily apparent to those skilled in the art from that description, or will be learned by practicing the embodiments described herein, including the following detailed description, the claims, and the accompanying drawings.

[0008] It should be understood that both the foregoing general description and the following detailed description are merely exemplary and are intended to provide an overview or framework for understanding the nature and features of the claims. The accompanying drawings are included to provide a further understanding, and are incorporated in and constitute a part of this specification. The drawings illustrate one or more embodiments and, together with the description, serve to explain the principles and operation of the various embodiments. [Brief description of the drawings]

[0009] [Figure 1] 1 is a perspective view of a vehicle interior with a vehicle interior system according to an exemplary embodiment; [Diagram 2] FIG. 1 illustrates a curved glass assembly according to an exemplary embodiment. [Diagram 3] FIG. 2 is a close-up view of an LCD bonded to a glass sheet according to an exemplary embodiment. [Figure 4] FIG. 2 is a rear view of a curved glass assembly according to an exemplary embodiment. [Diagram 5] 1 illustrates the directional deformation of a cylindrically bent glass sheet according to an exemplary embodiment. [Figure 6] FIG. 6 illustrates the stress distribution across the cylindrically bent glass sheet of FIG. 5 according to an exemplary embodiment. [Figure 7] FIG. 1 illustrates the light leakage rate of a conventional display assembly. [Figure 8] FIG. 2 illustrates the light leakage rate of a curved display assembly according to the present disclosure. [Figure 9] FIG. 13 illustrates maximum light leakage as a function of adhesive modulus according to an exemplary embodiment. [Figure 10]FIG. 2 illustrates an exemplary dimensional glass sheet according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Reference will now be made in detail to various embodiments of the curved display assembly, with exemplary curved display assemblies illustrated in the accompanying drawings. The curved display assembly includes a cover glass sheet, an outer frame to which the cover glass is attached, a display panel coupled to the cover glass, and a backlight module attached to the outer frame. In an embodiment, both the cover glass sheet and the outer frame have a cylindrical shape within the area of ​​the display, but may have other shapes and other curvatures outside the area of ​​the display. Furthermore, the curved display assembly may include more than one display, with different radii of curvature and different axes for each display. As described herein, the display panel is bonded to the cover glass using an optically clear adhesive, and at the outer edges of the display, a second adhesive having a higher modulus of elasticity is used to bond the edges of the display to the cover glass. The second adhesive creates a bending moment at the edges of the display to reduce the appearance of stress irregularities (e.g., light leakage from the backlight module due to stress in the glass layer). Various aspects and advantages of the curved display assembly and methods of forming the curved display assembly will be described in connection with the exemplary embodiments described herein and illustrated in the drawings.

[0011] The curved display assemblies described herein are applicable in a variety of different situations, including consumer electronics (computer monitors, televisions, etc.), equipment, and various vehicle interiors. To illustrate one possible situation for using the curved display assemblies, FIG. 1 shows an exemplary vehicle interior 1000 including three different embodiments of vehicle interior systems 100, 200, 300 that can incorporate one or more curved display assemblies. The vehicle interior system 100 includes a base, shown as a center console base 110, with a curved surface 120 that includes a curved display 130. The vehicle interior system 200 includes a base, shown as a dashboard base 210, with a curved surface 220 that includes a curved display 230. The dashboard base 210 typically includes an instrument panel 215 that may also include a curved display. The vehicle interior system 300 includes a base, shown as a steering wheel base 310, with a curved surface 320 and a curved display 330. In one or more embodiments, the vehicle interior system includes a base that is any part of the vehicle interior, including an armrest, a pillar, a seat back, a floorboard, a headrest, a door panel, or a curved surface. In other embodiments, the base is part of a housing for a freestanding display (i.e., a display that is not permanently connected to any part of the vehicle). As described herein, the curved display assembly is mounted to a frame that can be coupled to any of the aforementioned bases to provide a curved display, such as within any of the aforementioned bases. Thus, the curved display assemblies described herein can be used in each of the vehicle interior systems 100, 200, 300, etc.

[0012] Additionally, the glass material of the curved display assembly may be selected based on its weight, aesthetic appearance, etc., and may be provided with a decorative coating (e.g., an ink coating or pigment coating) in a pattern (e.g., a brushed metal look, a wood grain look, a leather look, a tinted look, etc.) to visually match the glass component with adjacent non-glass components. In certain embodiments, such ink or pigment coatings may have a transparency level that provides dead-front functionality. Additionally or alternatively, the glass material may be provided with a functional coating, such as a coating that provides touch functionality.

[0013] FIG 2 illustrates a curved display assembly 10, such as a cover glass for a curved display 130, 230, 330, according to an exemplary embodiment. Although FIG 2 is described in terms of forming a curved display 130, 230, 330, it should be understood that the curved display assembly 10 of FIG 2 may be used in any suitable curved glass application, including any curved glass component of the vehicle interior system of FIG 1 or other curved glass surfaces in the vehicle interior 1000. Such curved glass components may be display or non-display areas, for example, flat display areas and curved non-display areas, multiple curved displays, and curved display areas and curved non-display areas.

[0014] 2 illustrates a cross-sectional view of a curved display assembly 10 according to an exemplary embodiment. As shown in FIG. 2, the curved display assembly 10 includes a curved glass sheet 12 bonded to a frame 14 via an adhesive layer 16. The glass sheet 12 has a first major surface 18 and a second major surface 20 opposite the first major surface 18. The distance between the first major surface 18 and the second major surface 20 defines a thickness T1 between them. Furthermore, the first major surface 18 and the second major surface 20 are connected by a minor surface 22 that extends around the periphery of the glass sheet 12.

[0015] The glass sheet 12 has a curved shape such that the first major surface 18 and the second major surface 20 each include at least one curved section having a radius of curvature R1. In an embodiment, R1 is between 30 mm and 5 mm. Furthermore, in an embodiment, the glass sheet 12 has a thickness T1 (e.g., an average thickness measured between the surface 18 and the surface 20) that is between 0.05 mm and 2 mm. In a particular embodiment, T1 is equal to or less than 1.5 mm, and in a more particular embodiment, T1 is between 0.3 mm and 1.3 mm. Applicant has discovered that such thin glass sheets can be cold formed into various curved shapes utilizing cold forming without breakage, while at the same time providing a high quality covering layer for various vehicle interior applications. In addition, such thin glass sheets 12 can be more easily deformed, which includes the possibility of compensating for shape inconsistencies and gaps that may exist relative to the frame 14.

[0016] In various embodiments, the first major surface 18 and / or the second major surface 20 of the glass sheet 12 include one or more surface treatments or layers. The surface treatments may cover at least a portion of the first major surface 18 and / or the second major surface 20. Exemplary surface treatments include an anti-glare surface / anti-glare coating, an anti-reflective surface / anti-reflective coating, and an anti-soiling surface coating / anti-soiling surface treatment. In one or more embodiments, at least a portion of the first major surface 18 and / or the second major surface 20 may include any one, any two, or all three of an anti-glare surface, an anti-reflective surface, and an anti-soiling coating / anti-soiling treatment. For example, the first major surface 18 may include an anti-glare surface and the second major surface 20 may include an anti-reflective surface. In another example, the first major surface 18 includes an anti-reflective surface and the second major surface 20 includes an anti-glare surface. In yet another example, first major surface 18 includes an anti-soiling coating and second major surface 20 includes either or both of an anti-glare surface and an anti-reflective surface. In one or more embodiments, the anti-glare surface includes an etched surface. In one or more embodiments, the anti-reflective surface includes a multi-layer coating.

[0017] In embodiments, the glass sheet 12 may also include a pigment design on the first major surface 18 and / or the second major surface 20. The pigment design may include any aesthetic design formed from a pigment (e.g., ink, paint, etc.) and may include, for example, a wood grain design, a brushed metal design, a graphic design, a portrait, or a logo. The pigment design may be printed onto the glass sheet.

[0018] Generally, the glass sheet 12 can be cold formed or cold bent into a desired curved shape by applying a bending force to the glass sheet 12 while it is placed on a chuck having a curved surface. Advantageously, it is easier to apply a surface treatment to a flat glass sheet 12 before inducing a curvature in the glass sheet 12, and cold forming can bend the treated glass sheet 12 without destroying the surface treatment. In an embodiment, the cold forming process is carried out at a temperature below the glass transition temperature of the glass sheet 12. In particular, the cold forming process can be carried out at room temperature (e.g., about 20° C.) or at a slightly higher temperature, e.g., 200° C. or less, 150° C. or less, 100° C. or less, or 50° C. or less. Nevertheless, the teachings of the present disclosure regarding reducing stress unevenness in displays also apply to hot formed glass sheets 12 used in curved display assemblies 10.

[0019] As shown in FIG. 2, adhesive layer 16 is disposed on second major surface 20 of glass sheet 12. Adhesive layer 16 includes a first adhesive 24 and a second adhesive 26 that bond one or more displays 28 to second major surface 20 of glass sheet 12. Adhesive layer 16 includes a third adhesive 30 for adhering frame 14 to second major surface 20 of glass sheet 12. In one embodiment, first adhesive 24 is an optically clear adhesive and second adhesive 26 and third adhesive 30 are structural adhesives. In embodiments, second adhesive 26 and third adhesive 30 are the same adhesive, while in other embodiments, second adhesive 26 and third adhesive 30 are different adhesives.

[0020] In embodiments, the second adhesive 26 and the third adhesive 30 provide long term strength after curing over the course of, for example, about one hour at ambient temperature. In embodiments, exemplary adhesives for the second adhesive 26 and the third adhesive 30 include at least one of toughened epoxy, flexible epoxy, acrylic, silicone, urethane, polyurethane, or silane modified polymer. In certain embodiments, the second adhesive 26 and the third adhesive 30 include one or more toughened epoxies, such as EP21TDCHT-LO (available from Masterbond®, Hackensack, NJ), 3M™ Scotch-Weld™ Epoxy DP460 Off-White (available from 3M, St. Paul, MN). In other embodiments, the second adhesive 26 and the third adhesive 30 include one or more flexible epoxies such as Masterbond EP21TDC-2LO (available from Masterbond®, Hackensack, New Jersey), 3M™ Scotch-Weld™ Epoxy 2216 B / A Gray (available from 3M, St. Paul, Minnesota), and 3M™ Scotch-Weld™ Epoxy DP125. In yet other embodiments, the second adhesive 26 and the third adhesive 30 include one or more acrylics, such as LORD® Adhesive 410 / Accelerator 19 w / LORD® AP134 primer, LORD® Adhesive 852 / LORD® Accelerator 25GB (both available from LORD Corporation, Cary, North Carolina), DELO PUR SJ9356 (available from DELO Industrial Adhesives, Windach, Germany), Loctite® AA4800, Loctite® HF8000, TEROSON® MS9399, and TEROSON® MS647-2C (four of which are available from Henkel AG & Co. KGaA, Düsseldorf, Germany).In yet another embodiment, the second adhesive 26 and the third adhesive 30 include one or more urethanes, such as 3M™ Scotch-Weld™ Urethane DP640 Brown and 3M™ Scotch-Weld™ Urethane DP604, and in yet another embodiment, the second adhesive 26 and the third adhesive 30 include one or more silicones, such as Dow Corning® 995 (available from Dow Corning Corporation, Midland, Mich.). The first adhesive 24 can be any of a variety of suitable (i.e., optically clear) epoxies, urethanes, silicones, or acrylics.

[0021] In an embodiment, the first adhesive 24 has a modulus of elasticity smaller than that of the second adhesive 26. In an embodiment, the first adhesive 24 has a modulus of elasticity less than 0.5 MPa, in particular in the range of 10 kPa to 100 kPa. In an embodiment, the second adhesive 26 has a modulus of elasticity of at least 0.5 MPa, for example in the range of 0.5 MPa to 20 MPa. Furthermore, in an embodiment, the third adhesive 30 has a modulus of elasticity of at least 2.0 MPa, for example in the range of 2.0 MPa to 20 MPa.

[0022] In the illustrated embodiment, the displays 28 are curved and disposed on a curved region 32 of the glass sheet 12. In embodiments, the glass article 10 can be any of a variety of curved shapes, such as V-shaped (e.g., having flat sections on either side of the curved region 32), C-shaped (continuously curved bent region 32 between the ends of the curved display assembly 10), J-shaped (one flat section and one bent region 32), S-shaped (two bent regions 32 with opposite curvatures), and other possible configurations. Each display 28 can be any of a variety of suitable types of displays, such as a liquid crystal display (LCD), a light emitting diode (LED) display, an organic LED (OLED) display, a quantum dot LED (QLED) display, or a plasma display. Additionally, the display 28 or the glass sheet 12 can include touch functionality for interacting with the display 28 and / or the system in which the display is incorporated.

[0023] To illustrate the bonding of display 28 to glass sheet 12, Figure 3 shows LCD 28 bonded to glass sheet 12, and the following description is structured with respect to an LCD. However, this description is exemplary in nature and is not meant to imply that the concepts described therein apply only to LCDs. Instead, the concepts also apply to LED displays, OLED displays, QLED displays, plasma displays, and the like.

[0024] In conventional LCDs, mura can appear as a result of stress in the glass layers of the display (or "stress mura"). In such LCDs, stress in the glass layers can cause birefringence, which can change the polarization of the light transmitted by the glass. In conventional LCDs, this change in polarization can cause some light to be transmitted by the display even when no light is desired. When darkening is desired, the light transmitted from the display is called light leakage. There are other causes of light leakage, but stress in the glass layers of an LCD is one of the most common. However, not all stress in the glass layers of an LCD causes light leakage. If the major axes of stress in the glass layers are aligned perpendicular and parallel to the polarization of the transmitted light, there is no change in polarization and therefore no light leakage. For this reason, curved LCDs often have front and back polarizers aligned parallel and perpendicular to the axis of curvature. In that case, as long as the glass is bent into a cylindrical shape, the polarization axes will be aligned with the major axes of stress in the glass layers.

[0025] Nevertheless, deviations from a cylindrical shape cause the glass's principal stress axis to rotate from the nominal axis of curvature. In this regard, it is difficult to force a large display panel to conform to a cylindrical shape in which the principal stress axis remains parallel and perpendicular to the polarization of the transmitted light. In accordance with the present disclosure, as described below, light leakage resulting from deviations associated with bending the display 28 into a cylindrical shape is substantially reduced by using a second adhesive 26 along the edges of the display 28 that has a higher elastic modulus than the optically clear first adhesive 24. In particular, the second adhesive 26 applies a moment along the edges of the display and maintains the cylindrical shape. Conventionally, flexible, optically clear adhesives have been used to apply the moment, and the resulting deformations have caused stress distributions in the display panel, resulting in light leakage optical defects (i.e., stress irregularities) in the display assembly. By using a second adhesive 26 with a higher elastic modulus along at least the edges of the display 28 that are parallel to the bending axis, such stress irregularity defects can be substantially reduced or eliminated.

[0026] Referring to FIG. 3, an exemplary embodiment of an LCD 28 bonded to a glass sheet 12 is shown. The LCD 28 includes multiple layers, including a first polarizer 34, a thin film transistor (TFT) substrate 36, a color filter (CF) substrate 38, and a second polarizer 40. Although not shown in FIG. 3 (due to its relatively small size compared to the other layers of the display 28), the LCD 28 also includes a liquid crystal layer and a sealant around the edges of the liquid crystal layer. The liquid crystal layer is disposed between the TFT substrate 36 and the CF substrate 38. Also not shown in the figure is a backlight for the LCD 28 disposed above the first polarizer 34 (relative to the orientation shown in FIG. 3). As can be seen, the TFT substrate 36 extends a predetermined distance D beyond at least a periphery 42 of the CF substrate 38. In the depiction of FIG. 3, the periphery 42 is not aligned with the edges of the first polarizer 34 or the second polarizer 40, and the edges of the CF substrate 38 are shown with dashed lines. In an embodiment, the overhang distance D is at least three times the thickness T2 of the display 28 (i.e., D≧3*T2), and the display 28 includes the first polarizer 34 or the second polarizer 40, the TFT substrate 36, the CF substrate 38, the liquid crystal layer, and the sealant. In an embodiment, the display 28 has a thickness T2 of 0.25 mm to 0.75 mm. Thus, in an embodiment, the overhang distance D is at least 0.75 mm, at least 1.0 mm, at least 1.5 mm, at least 2.0 mm, at least 2.5 mm, etc.

[0027] When the LCD 28 is bent to curve the display, a bending moment is applied to the TFT substrate 36 and transferred to the CF substrate 38, particularly by the sealant around the edges of the liquid crystal layer, because the sealant bonds the TFT substrate 36 to the CF substrate 38. Advantageously, extending the TFT substrate 36 beyond the peripheral edge 42 of the CF substrate 38 provides a mounting surface for the display driver electronics on the overhanging edge 44 of the TFT substrate 36. In particular, the electronic chip cannot be located on the curved edge of the display 28 because the silicon chip would add stiffness to the TFT substrate 36, which would cause unevenness from light leakage when the edge is bent.

[0028] Additionally, the second adhesive 26 is applied on the side opposite the overhanging edge 44 from the side on which the electronics are attached. That is, the second adhesive 26 is disposed between the overhanging edge 44 of the TFT substrate 36 and the second major surface 20 of the glass sheet 12. FIG. 4 shows a rear view of the glass sheet 12 with the LCD 28 attached. As can be seen, in an embodiment, the overhanging edge 44 of the TFT substrate 36 extends beyond the CF substrate 38 around the perimeter of the LCD 28, and in an embodiment, the second adhesive 26 is applied to the overhanging edge 44 around the entire perimeter of the LCD 28. However, in other embodiments, the second adhesive 26 is applied only to the lateral side 46 of the TFT substrate 36 that is parallel to the bending axis α of the glass article 10. As shown in FIG. 4, the glass article 10 has a single bending axis α about which the glass sheet 12 and the LCD 28 are bent. In other embodiments, each curved display 28 of the glass article 10 has a bending axis, and the glass sheet 12 may have multiple bending axes, including bending axes where no display 28 is located. In embodiments, the display 28 is bent only about a single axis such that the bend is cylindrical. Additionally, while the embodiment of FIG. 3 shows the overhang edge 44 having a uniform overhang distance D around the periphery of the display 28, in embodiments, the overhang distance D is only at least three times greater than the thickness T2 of the display 28 in the area where the second adhesive is applied. That is, the overhang distance D of the overhang edge 44 is, in embodiments, at least three times greater than the thickness T2 of the display 28 only along the lateral side 46 parallel to the bending axis α.

[0029] Although an LCD 28 is described, the display 28 may be another type of display, and in such other displays 28, one layer of the display 28 may be made to extend beyond other layers of the display 28 to provide the overhanging edge 44, or another layer may be added to the display 28 to provide the overhanging edge 44. Additionally, in LCD embodiments, the TFT substrate 36 provides the overhanging edge 44 because of the synergistic effect of also providing a mounting location for the electronics, although in other embodiments, another or additional layers may be used to provide the overhanging edge 44.

[0030] Applicant has performed various simulations of a curved display assembly 10 according to the LCD structure described above, including a TFT substrate 36 providing an overhanging edge 44. The curved display assembly 10 used in the simulations was given typical dimensions for a display assembly found in an automotive interior system. Table 1 provides the materials, thicknesses, and properties of each layer of the curved display assembly 10 used in the simulations. As shown in Table 1, the second adhesive 26 was varied in the simulations to determine its effect on light leakage, and details of the second adhesive 26 are provided for each simulation discussed below.

[0031] [Table 1]

[0032] The simulations and associated data described here considered curved glass assemblies made by cold bending, where a flat display is first attached to a flat glass sheet and then the flat display and glass sheet are cold formed to their final shape, however, other simulations have shown that the perimeter adhesive is equally effective in situations where the glass sheet is first hot or cold formed before bending the display onto the glass sheet. The simulations calculated the deformation and stresses of the assembly in a mechanical simulation and the light leakage of the display in an optical simulation. In the simulations, the frame was assumed to be perfectly rigid and cylindrical in shape. Furthermore, the frame was given a radius such that the first major surface 18 of the glass sheet 12 had a nominal radius of curvature R1 of 750 mm. Taking into account the thickness of the layers, the radius of curvature of the frame was calculated to be 751.7 mm. The optically active area of ​​the display was 300 mm wide and 130 mm high. Around the periphery of the display, the edge of the first adhesive 24 relative to the edge of the CF substrate 38 was 0.3 mm on all sides. The TFT substrate 36 extended 2.0 mm on all sides beyond the CF substrate 38, so that the overhanging edge 44 extended around the entire perimeter of the display 28. A gap G (shown in FIG. 3) was provided between the overhanging edge 44 of the TFT substrate 36 and the frame 14. The gap G was 5.0 mm on all sides, and the frame width was 5.0 mm. The curved glass assembly 10 was rectangular and symmetric. In the simulation, only one-quarter of the entire assembly was considered, and symmetry was imposed on both sides. In the optical calculations, only light leakage due to stress was considered. For the display, when the glass layers (i.e., the TFT substrate 36 and the CF substrate 38) are not stressed, no light passes through the display 28. The stress in the glass rotates the polarization of the light slightly, allowing some light to pass through the second polarizer 40. The fraction of the incident intensity from the backlight unit that passes through the display 28 is called the "light leakage fraction."

[0033] FIG. 5 shows the results of a simulation of the deformation of the first major surface 18 of the glass sheet 12. In the simulation, the second adhesive 26 was provided around the entire periphery of the display 28, and the second adhesive 26 had an initial modulus of elasticity of 1.0 MPa. As can be seen in FIG. 5, the curvature deviates slightly from a perfect cylinder, which is most noticeable at the top and bottom of the deformation curve shown in FIG. 5. FIG. 6 shows the stress distribution across the first major surface 18 of the glass sheet 12. From FIG. 6, it can be seen that the maximum stress occurs at the right and left edges of the glass sheet 12, where the bending moment is applied from the frame 14 to create the curvature. FIG. 7 shows the light leakage rate of a conventional display bonded to the glass sheet using only an optically clear adhesive, i.e., the display does not include the second adhesive 26 between the overhanging edge 44 and the glass sheet 12 according to the curved display assembly 10 described herein. Figure 8 shows the light leakage rate within display 28 as described above for another simulation in which second adhesive 26 was applied around the perimeter of display 28. As can be seen from a comparison of Figures 7 and 8, the display without the perimeter adhesive has at least an order of magnitude higher light leakage than display 28 according to the present disclosure.

[0034] Having demonstrated that using second adhesive 26 to bond overhanging edge 44 to glass sheet 12 reduces light leakage, the effect of display size was considered. The results are summarized below in Table 2. The simulations used to provide the data in Table 2 considered displays constructed as described above (i.e., a second adhesive having a modulus of elasticity of 1.0 MPa, a bend radius of 750 mm, and the materials disclosed in Table 1).

[0035] [Table 2]

[0036] From Table 2 it can be seen that the use of a second adhesive 26 to bond the overhanging edge 44 to the glass sheet 12 again reduces light leakage by about an order of magnitude, even as the width of the display increases from 250 mm to 350 mm.

[0037] Table 3 below considers the effect of using the second adhesive 26 only on the lateral sides 46 of the display 28, rather than around the entire perimeter of the display 28. Additionally, the extent of the adhesive was varied. As can be seen in Table 3, the maximum light leakage rate is similar in magnitude to the curved display assembly having the second adhesive 26 applied around the entire perimeter. Additionally, once the adhesive reached the full extent of the overhanging edge 44, the maximum light leakage was the same (8.66E-05) as for the curved display assembly having the second adhesive around the entire perimeter.

[0038] [Table 3]

[0039] Figure 9 considers the effect of the elastic modulus of the second adhesive 26 on light leakage. As can be seen in Figure 9, light leakage decreases rapidly as the elastic modulus approaches 0.5 MPa and remains low as the elastic modulus exceeds 0.5 MPa.

[0040] The curved glass assembly 10 described herein can be assembled in a variety of ways. In particular, the glass sheet 12 of the curved glass assembly can be hot formed or cold formed. For example, according to a first method, a flat display 28 is bonded to the flat glass sheet 12 using a first adhesive 24 and a second adhesive 26. The glass sheet 12 with the display 28 bonded thereon is then cold formed on a chuck (such as a vacuum chuck) to provide the glass sheet 12 and the display 28 with the desired curvature. While on the chuck, a frame 14 is bonded to the glass sheet 12 using a third adhesive 30, and a backlight is attached to the display 28. The adhesives 24, 26, 30 are allowed to cure, and the completed curved glass assembly is removed from the chuck.

[0041] In the second method, the glass sheet 12 is first cold formed on a chuck. The display 28 is cold bent and bonded to the glass sheet 12 using a first adhesive 24 and a second adhesive 26. The frame 14 is then bonded to the glass sheet 12 using a third adhesive 30, a backlight unit is attached to the display 28, and after curing, the completed curved display assembly 10 is removed from the chuck.

[0042] According to a third method, the glass sheet 12 is permanently bent using a hot forming technique. The display 28 is cold bent onto the glass sheet 12 and bonded to the glass sheet 12 using a first adhesive 24 and a second adhesive 26. The frame 14 is then bonded to the glass sheet 12 using a third adhesive 30, a backlight unit is attached to the display 28, and after curing, the completed curved display assembly 10 is removed from the chuck.

[0043] In various embodiments, glass sheet 12 is formed from a strengthened glass sheet (e.g., a thermally strengthened glass material, a chemically strengthened glass sheet, etc.). In such embodiments, when glass sheet 12 is formed from a strengthened glass material, first major surface 18 and second major surface 20 are under compressive stress, and thus second major surface 20 can undergo greater tensile stress when bent into a convex shape without risk of breaking. This allows strengthened glass sheet 12 to more closely conform to the curved surface.

[0044] A feature of the cold-formed glass sheet 12 is that as the glass sheet 12 is bent into a curved shape, an asymmetric surface is compressed between the first major surface 18 and the second major surface 20. In such an embodiment, prior to the cold-forming process or being cold-formed, the compressive stresses in each of the first major surface 18 and the second major surface 20 of the glass sheet 12 are substantially equal. After cold-forming, the compressive stress in the concave first major surface 18 increases, such that the compressive stress in the first major surface 18 is greater after cold-forming than it was before cold-forming. In contrast, the convex second major surface 20 is subjected to tensile stress during bending, causing a net reduction in the surface compressive stress of the second major surface 20, such that the compressive stress in the second major surface 20 after bending is less than the compressive stress in the second major surface 20 when the glass sheet is flat.

[0045] In addition to providing processing advantages such as the elimination of expensive and / or slow heating steps as described above, the cold forming processes described herein are believed to produce curved display assemblies with a variety of properties that are superior to hot formed glass articles, particularly in vehicle interior or display cover glass applications. For example, Applicants believe that for at least some glass materials, heating during the hot forming process degrades the optical properties of the curved glass sheet, and thus, curved glass sheets formed utilizing the cold bending processes / systems described herein provide both a curved glass shape along with improved optical qualities that are believed to be unattainable by hot bending processes.

[0046] Furthermore, many glass surface treatments (e.g., anti-glare coatings, anti-reflective coatings, anti-soiling coatings, etc.) are applied via deposition processes such as sputtering processes that are typically not suitable for coating curved glass articles. In addition, many surface treatments (e.g., anti-glare coatings, anti-reflective coatings, anti-soiling coatings, etc.) also cannot withstand the high temperatures associated with hot bending processes. Thus, in certain embodiments described herein, one or more surface treatments are applied to the first major surface 18 and / or second major surface 20 of the glass sheet 12 prior to cold bending, and the glass sheet 12 including the surface treatments is bent into the curved shape described herein. Thus, applicants believe that the processes and systems described herein can bend glass after one or more coating materials have been applied to the glass, as opposed to typical hot forming processes.

[0047] With reference to FIG. 10, additional structural details of the glass sheet 12 are shown and described. As noted above, the glass sheet 12 has a thickness T1 that is substantially constant and is defined as the distance between the first major surface 18 and the second major surface 20. In various embodiments, T1 may refer to the average thickness or maximum thickness of the glass sheet. In addition, the glass sheet 12 includes a width W1, defined as a first maximum dimension of one of the first major surface 18 or the second major surface 20 that is perpendicular to the thickness T1, and a length L1, defined as a second maximum dimension of one of the first major surface 18 or the second major surface 20 that is perpendicular to both the thickness and the width. In other embodiments, W1 and L1 may be the average width and average length of the glass sheet 12, respectively.

[0048] In various embodiments, the thickness T1 is 2 mm or less, specifically 0.3 mm to 1.5 mm. For example, the thickness T1 is about 0.1 mm to about 1.5 mm, about 0.15 mm to about 1.5 mm, about 0.2 mm to about 1.5 mm, about 0.25 mm to about 1.5 mm, about 0.3 mm to about 1.5 mm, about 0.35 mm to about 1.5 mm, about 0.4 mm to about 1.5 mm, about 0.45 mm to about 1.5 mm, about 0.5 mm to about 1.5 mm, about 0.55 mm to about 1.5 mm, about 0.6 mm to about 1.5 mm, about 0.65 mm to about 1.5 mm, about 0.7 mm to about 1.5 mm, about 0.1 mm to about 1.4 mm, about 0.1 mm to about 1.3 mm, about 0.1 mm to about 1.5 ... T1 may be in the range of about 1.2 mm, about 0.1 mm to about 1.1 mm, about 0.1 mm to about 1.05 mm, about 0.1 mm to about 1 mm, about 0.1 mm to about 0.95 mm, about 0.1 mm to about 0.9 mm, about 0.1 mm to about 0.85 mm, about 0.1 mm to about 0.8 mm, about 0.1 mm to about 0.75 mm, about 0.1 mm to about 0.7 mm, about 0.1 mm to about 0.65 mm, about 0.1 mm to about 0.6 mm, about 0.1 mm to about 0.55 mm, about 0.1 mm to about 0.5 mm, about 0.1 mm to about 0.4 mm, or about 0.3 mm to about 0.7 mm. In other embodiments, T1 is within any one of the exact numerical ranges described in this paragraph.

[0049] In various embodiments, the width W1 is 5 cm to about 250 cm, about 10 cm to about 250 cm, about 15 cm to about 250 cm, about 20 cm to about 250 cm, about 25 cm to about 250 cm, about 30 cm to about 250 cm, about 35 cm to about 250 cm, about 40 cm to about 250 cm, about 45 cm to about 250 cm, about 50 cm to about 250 cm, about 55 cm to about 250 cm, about 60 cm to about 250 cm, about 65 cm to about 250 cm, about 70 cm to about 250 cm, about 75 cm to about 250 cm, about 80 cm to about 250 cm, about 85 cm to about 250 cm, about 90 cm to about 250 cm, about 95 cm to about 250 cm, about 100 cm to about 250 cm, about 110 cm to about 250 cm, about The range is from 120cm to about 250cm, from about 130cm to about 250cm, from about 140cm to about 250cm, from about 150cm to about 250cm, from about 5cm to about 240cm, from about 5cm to about 230cm, from about 5cm to about 220cm, from about 5cm to about 210cm, from about 5cm to about 200cm, from about 5cm to about 190cm, from about 5cm to about 180cm, from about 5cm to about 170cm, from about 5cm to about 160cm, from about 5cm to about 150cm, from about 5cm to about 140cm, from about 5cm to about 130cm, from about 5cm to about 120cm, from about 5cm to about 110cm, from about 5cm to about 110cm, from about 5cm to about 100cm, from about 5cm to about 90cm, from about 5cm to about 80cm, or from about 5cm to about 75cm. In other embodiments, W1 falls within any one of the exact numerical ranges described in this paragraph.

[0050] In various embodiments, the length L1 is about 5 cm to about 1500 cm, about 50 cm to about 1500 cm, about 100 cm to about 1500 cm, about 150 cm to about 1500 cm, about 200 cm to about 1500 cm, about 250 cm to about 1500 cm, about 300 cm to about 1500 cm, about 350 cm to about 1500 cm, about 400 cm to about 1500 cm, about 450 cm to about 1500 cm, about 500 cm to about 1500 cm, about 550 cm to about 1500 cm, about 600 cm to about 1500 cm, about 650 cm to about 1500 cm, about 650 cm to about 1500 cm, about 700 cm to about 1500 cm, about 800 cm to about 1500 cm, about 900 cm to about 1500 cm, about 1000 cm to about 1500 cm, about 1100 cm to about 1500 cm, about 1200 cm to about 1500 cm, about 1300 cm to about 1500 cm, about 1400 cm to about 1500 cm, about 1600 cm to about 1500 cm, about 1700 cm to about 1500 cm, about 1800 cm to about 1500 cm, about 1900 cm to about 1500 cm, about 2000 cm to about 1500 cm, about 2100 cm to about 1500 cm, about 2200 cm to about 1500 cm, about 2300 cm to about 1500 cm, about 2400 cm to about 1500 cm, about 2500 cm to about 1 00 cm, about 750 cm to about 1500 cm, about 800 cm to about 1500 cm, about 850 cm to about 1500 cm, about 900 cm to about 1500 cm, about 950 cm to about 1500 cm, about 1000 cm to about 1500 cm, about 1050 cm to about 1500 cm, about 1100 cm to about 1500 cm, about 1150 cm to about 1500 cm, about 1200 cm to about 1500 cm, about 1250 cm to about 1500 cm, about 1300 cm to about 1500 cm, about 1350 cm to about 1500 cm, about 1400 cm to about 1500 cm, or about 1450 cm to about 1500 cm. In other embodiments, L1 is within any one of the exact numerical ranges described in this paragraph.

[0051] In various embodiments, one or more radii of curvature of the glass sheet 12 (e.g., R1 shown in FIG. 2) are about 30 mm or more. For example, R1 can be about 30 mm to about 5000 mm, about 50 mm to about 5000 mm, about 70 mm to about 5000 mm, about 90 mm to about 5000 mm, about 110 mm to about 5000 mm, about 150 mm to about 5000 mm, about 200 mm to about 5000 mm, about 250 mm to about 5000 mm, about 300 mm to about 5000 mm, about 350 mm to about 5000 mm, about 400 mm to about 5000 mm, about 450 mm to about 5000 mm, about 500mm~5000mm, 550mm~5000mm, 600mm~5000mm, 650mm~5000mm, 700mm~5000mm, 750mm~5000mm, 800mm~5000mm, 850mm~5000mm, 900mm~5000mm, 950mm~5000mm, 1000mm~5000mm, 1500mm~5000mm, 2000mm mm~about 5000mm, about 2500mm~about 5000mm, about 3000mm~about 5000mm, about 3500mm~about 5000mm, about 4000mm~about 5000mm, about 4500mm~about 5000mm, about 30mm to about 4500mm, about 30mm to about 4000mm, about 30mm to about 3500mm, about 30mm to about 3000mm, about 30mm to about 2500mm, about 30mm to about 2000mm, about 30mm to about 150 0 mm, about 30 mm to about 1000 mm, about 30 mm to about 950 mm, about 30 mm to about 900 mm, about 30 mm to about 850 mm, about 30 mm to about 800 mm, about 30 mm to about 750 mm, about 30 mm to about 700 mm, about 30 mm to about 650 mm, about 30 mm to about 600 mm, about 30 mm to about 550 mm, about 30 mm to about 500 mm, about 30 mm to about 450 mm, or about 30 mm to about 400 mm. In other embodiments, R1 is within any one of the exact numerical ranges described in this paragraph.

[0052] Various embodiments of the in-vehicle system may be incorporated into vehicles, such as trains, automobiles (e.g., cars, trucks, buses, etc.), marine vessels (boats, ships, submarines, etc.), and aircraft (e.g., drones, planes, jets, helicopters, etc.).

[0053] Characteristics of tempered glass As described above, the glass sheet 12 may be strengthened. In one or more embodiments, the glass sheet 12 may be strengthened to include compressive stresses that extend from the surface to a depth of compression (DOC). The compressive stress areas are balanced by a central portion that exhibits tensile stress. At the DOC, the stresses cross over from positive (compressive) to negative (tensile).

[0054] In various embodiments, the glass sheet 12 can be mechanically strengthened by taking advantage of the mismatch in thermal expansion coefficients between portions of the article to create areas of compressive stress and a central area that exhibits tensile stress. In some embodiments, the glass sheet can be thermally strengthened by heating the glass to a temperature above the glass transition temperature and then rapidly quenching it.

[0055] In various embodiments, the glass sheet 12 can be chemically strengthened by ion exchange. In the ion exchange process, ions at or near the surface of the glass sheet are replaced (or exchanged) with larger ions having the same valence or oxidation state. In those embodiments in which the glass sheet comprises an alkali aluminosilicate glass, the ions at the surface layer of the article and the larger ions are Li + , Na + , K + , Rb + , and Cs + Alternatively, the monovalent cation in the surface layer is Ag + In such embodiments, the exchanged monovalent ions (or cations) in the glass sheet create stress.

[0056] The ion exchange process is typically carried out by immersing the glass sheet in a molten salt bath (or two or more molten salt baths) containing larger ions that are to be exchanged for smaller ions in the glass sheet. Note that aqueous salt baths can also be utilized. In addition, the composition of the bath can be modified to contain more than one type of larger ion (e.g., Na + and K. + ) or one of the larger ions. Those skilled in the art will appreciate that the parameters for the ion exchange process, including but not limited to the bath composition and temperature, immersion time, number of immersions of the glass sheet in the salt bath (or salt baths), use of multiple salt baths, additional steps such as annealing, washing, etc., are generally determined by the composition of the glass sheet (including the structure of the article and any crystalline phases present) and the desired DOC and CS of the glass sheet resulting from the strengthening. Exemplary molten bath compositions may include nitrates, sulfates, and chlorides of the larger alkali metal ions. Typical nitrates include KNO3, NaNO3, LiNO3, NaSO4, and combinations thereof. The temperature of the molten salt bath typically ranges from about 380°C up to about 450°C, while the immersion time ranges from about 15 minutes up to about 100 hours, depending on the thickness of the glass sheet, the bath temperature, and the diffusivity of the glass (or monovalent ions). However, temperatures and immersion times other than those mentioned above may also be used.

[0057] In one or more embodiments, the glass sheet can be immersed in a molten salt bath of 100% NaNO3, 100% KNO3, or a combination of NaNO3 and KNO3 having a temperature of about 370°C to about 480°C. In some embodiments, the glass sheet can be immersed in a molten mixed salt bath including about 5% to about 90% KNO3 and about 10% to about 95% NaNO3. In one or more embodiments, the glass sheet can be immersed in a first bath and then in a second bath. The first and second baths can have different compositions and / or temperatures. The immersion time in the first bath and the immersion time in the second bath can vary. For example, the immersion in the first bath can be longer than the immersion in the second bath.

[0058] In one or more embodiments, the glass sheet may be immersed in a molten mixed salt bath including NaNO3 and KNO3 (e.g., 49% / 51%, 50% / 50%, 51% / 49%) having a temperature of less than about 420°C (e.g., about 400°C or about 380°C) for less than about 5 hours, or even up to about 4 hours.

[0059] The ion exchange conditions can be tailored to provide a "spike" or increase the gradient of the stress profile at or near the surface of the resulting glass sheet. The spike can result in a larger surface CS value. This spike can be achieved by a single bath or multiple baths, using baths with single or mixed compositions, due to the unique properties of the glass compositions used in the glass sheets described herein.

[0060] In one or more embodiments in which more than one monovalent ion is exchanged within the glass sheet, the different monovalent ions can exchange to different depths within the glass sheet (and generate different amounts of stress within the glass sheet at different depths), and the relative depths of the resulting stress-generating ions can be determined, giving rise to different characteristics of the stress profile.

[0061] CS is measured using means known in the art, such as by commercially available equipment, such as a surface stress meter (FSM), such as the FSM-6000 manufactured by Orihara Industrial Co., Ltd. (Japan). Surface stress measurement relies on accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. SOC is then measured by methods known in the art, such as the fiber and four-point bending methods and the bulk cylinder method described in ASTM standard C770-98 (2013) "Standard Test Method for Measurement of Glass Stress-Optical Coefficient," the contents of which are incorporated herein by reference in their entirety. As used herein, CS may be the "maximum compressive stress," which is the highest compressive stress value measured within the compressive stress layer. In some embodiments, the maximum compressive stress is located at the surface of the glass sheet. In other embodiments, the maximum compressive stress may occur at a depth below the surface, giving the compressive profile the appearance of a "buried peak."

[0062] DOC can be measured by FSM or Scattered Light Polariscope (SCALP) (such as SCALP-04 Scattered Light Polariscope available from Glasstress Ltd., Tallinn, Estonia) depending on the strengthening method and conditions. If the glass sheet is chemically strengthened by an ion exchange process, then either FSM or SCALP can be used depending on the ions exchanged in the glass sheet. If the stress in the glass sheet is developed by exchanging potassium ions in the glass sheet, then FSM is used to measure the DOC. If the stress in the glass sheet is developed by exchanging sodium ions in the glass sheet, then SCALP is used to measure the DOC. If the stress in the glass sheet is developed by exchanging both potassium and sodium ions in the glass, then DOC is measured by SCALP since it is believed that the sodium exchange depth indicates the DOC and the potassium ion exchange depth indicates the change in the magnitude of the compressive stress (but not the change in stress from compression to tension). The potassium ion exchange depth of such glass sheets is measured by FSM. The central tension or CT is the maximum tensile stress and is measured by SCALP.

[0063] In one or more embodiments, the glass sheet can be strengthened to exhibit a DOC, expressed as a percentage of the thickness T1 of the glass sheet (as described herein). For example, in one or more embodiments, the DOC can be about 0.05T1 or more, about 0.1T1 or more, about 0.11T1 or more, about 0.12T1 or more, about 0.13T1 or more, about 0.14T1 or more, about 0.15T1 or more, about 0.16T1 or more, about 0.17T1 or more, about 0.18T1 or more, about 0.19T1 or more, about 0.2T1 or more, or about 0.21T1 or more. In some embodiments, the DOC is from about 0.08T1 to about 0.25T1, from about 0.09T1 to about 0.25T1, from about 0.18T1 to about 0.25T1, from about 0.11T1 to about 0.25T1, from about 0.12T1 to about 0.25T1, from about 0.13T1 to about 0.25T1, from about 0.14T1 to about 0.25T1, from about 0.15T1 to about 0.25T1, from about 0.08T1 to about 0.24 T1, about 0.08T1 to about 0.23T1, about 0.08T1 to about 0.22T1, about 0.08T1 to about 0.21T1, about 0.08T1 to about 0.2T1, about 0.08T1 to about 0.19T1, about 0.08T1 to about 0.18T1, about 0.08T1 to about 0.17T1, about 0.08T1 to about 0.16T1, or about 0.08T1 to about 0.15T1. In some cases, the DOC may be about 20 μm or less. In one or more embodiments, the DOC may be about 40 μm or more, for example, about 40 μm to about 300 μm, about 50 μm to about 300 μm, about 60 μm to about 300 μm, about 70 μm to about 300 μm, about 80 μm to about 300 μm, about 90 μm to about 300 μm, about 100 μm to about 300 μm, about 110 μm to about 300 μm, about 120 μm to about 300 μm, about 140 μm to about 300 μm, about 150 μm to about 300 μm, about 40 μm to about 290 μm, about 40 μm to about 280 μm, or the like. μm, about 40 μm to about 260 μm, about 40 μm to about 250 μm, about 40 μm to about 240 μm, about 40 μm to about 230 μm, about 40 μm to about 220 μm, about 40 μm to about 210 μm, about 40 μm to about 200 μm, about 40 μm to about 180 μm, about 40 μm to about 160 μm, about 40 μm to about 150 μm, about 40 μm to about 140 μm, about 40 μm to about 130 μm, about 40 μm to about 120 μm, about 40 μm to about 110 μm, or about 40 μm to about 100 μm.In other embodiments, the DOC falls within any one of the exact numerical ranges recited in this paragraph.

[0064] In one or more embodiments, the strengthened glass sheet may have a CS (which may be found at the surface or at a depth within the glass sheet) of about 200 MPa or more, 300 MPa or more, 400 MPa or more, about 500 MPa or more, about 600 MPa or more, about 700 MPa or more, about 800 MPa or more, about 900 MPa or more, about 930 MPa or more, about 1000 MPa or more, or about 1050 MPa or more.

[0065] In one or more embodiments, the strengthened glass sheet may have a maximum tensile stress or central tension (CT) of about 20 MPa or more, about 30 MPa or more, about 40 MPa or more, about 45 MPa or more, about 50 MPa or more, about 60 MPa or more, about 70 MPa or more, about 75 MPa or more, about 80 MPa or more, or about 85 MPa or more. In some embodiments, the maximum tensile stress or central tension (CT) may range from about 40 MPa to about 100 MPa. In other embodiments, CS falls within the exact numerical ranges described in this paragraph.

[0066] Glass composition Glass compositions suitable for use in glass sheet 12 include soda-lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, alkali-containing borosilicate glass, and alkali-containing boroaluminosilicate glass.

[0067] Unless otherwise stated, the glass compositions disclosed herein are described in mole percent (mol %) analyzed on an oxide basis.

[0068] In one or more embodiments, the glass composition can include SiO in an amount ranging from about 66 mol% to about 80 mol%, about 67 mol% to about 80 mol%, about 68 mol% to about 80 mol%, about 69 mol% to about 80 mol%, about 70 mol% to about 80 mol%, about 72 mol% to about 80 mol%, about 65 mol% to about 78 mol%, about 65 mol% to about 76 mol%, about 65 mol% to about 75 mol%, about 65 mol% to about 74 mol%, about 65 mol% to about 72 mol%, or about 65 mol% to about 70 mol%, and all ranges and subranges therebetween.

[0069] In one or more embodiments, the glass composition includes Al2O3 in an amount greater than about 4 mol%, or greater than about 5 mol%. In one or more embodiments, the glass composition can include Al2O3 in an amount greater than about 7 mol% to about 15 mol%, greater than about 7 mol% to about 14 mol%, about 7 mol% to about 13 mol%, about 4 mol% to about 12 mol%, about 7 mol% to about 11 mol%, about 8 mol% to about 15 mol%, about 9 mol% to about 15 mol%, about 10 mol% to about 15 mol%, about 11 mol% to about 15 mol%, or about 12 mol% to about 15 mol%, and all ranges and subranges therebetween. In one or more embodiments, the upper limit of Al2O3 can be about 14 mol%, 14.2 mol%, 14.4 mol%, 14.6 mol%, or 14.8 mol%.

[0070] In one or more embodiments, the glass article is described as an aluminosilicate glass article or as including an aluminosilicate glass composition. In such embodiments, the glass composition, or article formed therefrom, includes SiO2 and Al2O3 and is not a soda-lime-silicate glass. In this regard, the glass composition, or article formed therefrom, includes Al2O3 in an amount of about 2 mol% or more, 2.25 mol% or more, 2.5 mol% or more, about 2.75 mol% or more, or about 3 mol% or more.

[0071] In one or more embodiments, the glass composition includes B2O3 (e.g., about 0.01 mol% or more). In one or more embodiments, the glass composition can include B2O3 in an amount ranging from about 0 mol% to about 5 mol%, from about 0 mol% to about 4 mol%, from about 0 mol% to about 3 mol%, from about 0 mol% to about 2 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.5 mol%, from about 0.1 mol% to about 5 mol%, from about 0.1 mol% to about 4 mol%, from about 0.1 mol% to about 3 mol%, from about 0.1 mol% to about 2 mol%, from about 0.1 mol% to about 1 mol%, from about 0.1 mol% to about 0.5 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition is substantially free of B2O3.

[0072] As used herein, the phrase "substantially free" with respect to a component of a composition means that the component is not actively or intentionally added to the composition during initial batch processing, but may be present as an impurity in an amount less than about 0.001 mole percent.

[0073] In one or more embodiments, the glass composition optionally includes P2O5 (e.g., about 0.01 mol% or more). In one or more embodiments, the glass composition includes a non-zero amount of P2O5 of 2 mol% or less, 1.5 mol% or less, 1 mol% or less, or 0.5 mol% or less. In one or more embodiments, the glass composition is substantially free of P2O5.

[0074] In one or more embodiments, the glass composition may include a total amount of RO (which is the sum of alkali metal oxides, such as LiO, NaO, KO, RbO, and CsO) of about 8 mol% or more, about 10 mol% or more, or about 12 mol% or more. In some embodiments, the glass composition may include RO in an amount ranging from about 8 mol% to about 20 mol%, about 8 mol% to about 18 mol%, about 8 mol% to about 16 mol%, about 8 mol% to about 14 mol%, about 8 mol% to about 12 mol%, about 9 mol% to about 20 mol%, about 10 mol% to about 20 mol%, about 11 mol% to about 20 mol%, about 12 mol% to about 20 mol%, about 13 mol% to about 20 mol%, about 10 mol% to about 14 mol%, or 11 mol% to about 13 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition may be substantially free of Rb2O, Cs2O, or both Rb2O and Cs2O. In one or more embodiments, R2O may include a total amount of only Li2O, Na2O, and K2O. In one or more embodiments, the glass composition may include at least one alkali metal oxide selected from Li2O, Na2O, and K2O, where the alkali metal oxide is present in an amount of about 8 mol% or greater.

[0075] In one or more embodiments, the glass composition includes Na2O in an amount of about 8 mol% or more, about 10 mol% or more, or about 12 mol% or more. In one or more embodiments, the composition can include Na2O in an amount ranging from about 8 mol% to about 20 mol%, from about 8 mol% to about 18 mol%, from about 8 mol% to about 16 mol%, from about 8 mol% to about 14 mol%, from about 8 mol% to about 12 mol%, from about 9 mol% to about 20 mol%, from about 10 mol% to about 20 mol%, from about 11 mol% to about 20 mol%, from about 12 mol% to about 20 mol%, from about 13 mol% to about 20 mol%, from about 10 mol% to about 14 mol%, or from 11 mol% to about 16 mol%, and all ranges and subranges therebetween.

[0076] In one or more embodiments, the glass composition includes less than about 4 mol% K2O, less than about 3 mol% K2O, or less than about 1 mol% K2O. In some cases, the glass composition can include K2O in an amount ranging from about 0 mol% to about 4 mol%, about 0 mol% to about 3.5 mol%, about 0 mol% to about 3 mol%, about 0 mol% to about 2.5 mol%, about 0 mol% to about 2 mol%, about 0 mol% to about 1.5 mol%, about 0 mol% to about 1 mol%, about 0 mol% to about 0.5 mol%, about 0 mol% to about 0.2 mol%, about 0 mol% to about 0.1 mol%, about 0.5 mol% to about 4 mol%, about 0.5 mol% to about 3.5 mol%, about 0.5 mol% to about 3 mol%, about 0.5 mol% to about 2.5 mol%, about 0.5 mol% to about 2 mol%, about 0.5 mol% to about 1.5 mol%, or about 0.5 mol% to about 1 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition can be substantially free of K2O.

[0077] In one or more embodiments, the glass composition is substantially free of Li2O.

[0078] In one or more embodiments, the amount of Na2O in the composition may be greater than the amount of Li2O. In some cases, the amount of Na2O may be greater than the combined amount of Li2O and K2O. In one or more alternative embodiments, the amount of Li2O in the composition may be greater than the amount of Na2O or the combined amount of Na2O and K2O.

[0079] In one or more embodiments, the glass composition may include RO (which is the sum of alkaline earth metal oxides such as CaO, MgO, BaO, ZnO, and SrO) in a total amount ranging from about 0 mol% to about 2 mol%. In some embodiments, the glass composition includes a non-zero amount of RO up to about 2 mol%. In one or more embodiments, the glass composition includes RO in an amount ranging from about 0 mol% to about 1.8 mol%, from about 0 mol% to about 1.6 mol%, from about 0 mol% to about 1.5 mol%, from about 0 mol% to about 1.4 mol%, from about 0 mol% to about 1.2 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.8 mol%, from about 0 mol% to about 0.5 mol%, and all ranges and subranges therebetween.

[0080] In one or more embodiments, the glass composition comprises CaO in an amount less than about 1 mol%, less than about 0.8 mol%, or less than about 0.5 mol%. In one or more embodiments, the glass composition is substantially free of CaO.

[0081] In some embodiments, the glass composition includes MgO in an amount in the range from about 0 mol% to about 7 mol%, from about 0 mol% to about 6 mol%, from about 0 mol% to about 5 mol%, from about 0 mol% to about 4 mol%, from about 0.1 mol% to about 7 mol%, from about 0.1 mol% to about 6 mol%, from about 0.1 mol% to about 5 mol%, from about 0.1 mol% to about 4 mol%, from about 1 mol% to about 7 mol%, from about 2 mol% to about 6 mol%, or from about 3 mol% to about 6 mol%, and all ranges and subranges therebetween.

[0082] In one or more embodiments, the glass composition includes ZrO2 in an amount of about 0.2 mol% or less, about 0.18 mol% or less, about 0.16 mol% or less, about 0.15 mol% or less, about 0.14 mol% or less, about 0.12 mol% or less. In one or more embodiments, the glass composition includes ZrO2 in an amount ranging from about 0.01 mol% to about 0.2 mol%, from about 0.01 mol% to about 0.18 mol%, from about 0.01 mol% to about 0.16 mol%, from about 0.01 mol% to about 0.15 mol%, from about 0.01 mol% to about 0.14 mol%, from about 0.01 mol% to about 0.12 mol%, or from about 0.01 mol% to about 0.10 mol%, and all ranges and subranges therebetween.

[0083] In one or more embodiments, the glass composition includes SnO2 in an amount of about 0.2 mol% or less, about 0.18 mol% or less, about 0.16 mol% or less, about 0.15 mol% or less, about 0.14 mol% or less, about 0.12 mol% or less. In one or more embodiments, the glass composition includes SnO2 in an amount ranging from about 0.01 mol% to about 0.2 mol%, from about 0.01 mol% to about 0.18 mol%, from about 0.01 mol% to about 0.16 mol%, from about 0.01 mol% to about 0.15 mol%, from about 0.01 mol% to about 0.14 mol%, from about 0.01 mol% to about 0.12 mol%, or from about 0.01 mol% to about 0.10 mol%, and all ranges and subranges therebetween.

[0084] In one or more embodiments, the glass composition may include oxides that impart color or tint to the glass article. In some embodiments, the glass composition includes oxides that prevent discoloration of the glass article when the glass article is exposed to ultraviolet light. Examples of such oxides include, but are not limited to, oxides of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ce, W, and Mo.

[0085] In one or more embodiments, the glass composition includes Fe, expressed as Fe2O3, where Fe is present in an amount up to (and including) about 1 mol%. In some embodiments, the glass composition is substantially free of Fe. In one or more embodiments, the glass composition includes Fe2O3 in an amount of about 0.2 mol% or less, about 0.18 mol% or less, about 0.16 mol% or less, about 0.15 mol% or less, about 0.14 mol% or less, or about 0.12 mol% or less. In one or more embodiments, the glass composition includes Fe2O3 in an amount in the range from about 0.01 mol% to about 0.2 mol%, from about 0.01 mol% to about 0.18 mol%, from about 0.01 mol% to about 0.16 mol%, from about 0.01 mol% to about 0.15 mol%, from about 0.01 mol% to about 0.14 mol%, from about 0.01 mol% to about 0.12 mol%, or from about 0.01 mol% to about 0.10 mol%, and all ranges and subranges therebetween.

[0086] When the glass composition includes TiO2, TiO2 may be present in an amount of about 5 mol% or less, about 2.5 mol% or less, about 2 mol% or less, or about 1 mol% or less. In one or more embodiments, the glass composition may be substantially free of TiO2.

[0087] Exemplary glass compositions include SiO2 in an amount ranging from about 65 mol% to about 75 mol%, Al2O3 in an amount ranging from about 8 mol% to about 14 mol%, Na2O in an amount ranging from about 12 mol% to about 17 mol%, K2O in an amount ranging from about 0 mol% to about 0.2 mol%, and MgO in an amount ranging from about 1.5 mol% to about 6 mol%. Optionally, SnO2 may be included in amounts as otherwise disclosed herein. It should be understood that while the preceding glass composition paragraphs represent approximate ranges, in other embodiments, the glass sheet 12 can be made from any glass composition falling into any one of the exact numerical ranges listed above.

[0088] Aspect (1) of the present disclosure relates to a curved display assembly comprising: a glass sheet having a first major surface and a second major surface opposite the first major surface, the glass sheet having a first thickness measured between the first and second major surfaces, the second major surface defining a first radius of curvature of the glass sheet, the first radius of curvature having a bending axis; a curved display having a second thickness between a first display surface and a second display surface, the curved display comprising a display area and two overhanging edges adjacent the display area and parallel to the bending axis; a first adhesive bonding the second display surface of the curved display to a second major surface of the glass sheet in the display area; and a second adhesive bonding each of the two overhanging edges to the second major surface of the glass sheet, the second adhesive having a higher modulus of elasticity than the first adhesive, each of the overhanging edges extending outside the display area a distance that is at least three times the second thickness of the curved display.

[0089] Aspect (2) of the present disclosure relates to a curved display assembly according to aspect (1), wherein the curved display is at least one of a liquid crystal display (LCD), a light emitting diode (LED) display, an organic LED (OLED) display, a quantum dot LED (QLED) display, or a plasma display.

[0090] Aspect (3) of the present disclosure relates to the curved display assembly of aspect (1) or aspect (2), further comprising a backlight disposed on the second display surface, whereby the curved display is disposed between the backlight and the glass sheet.

[0091] Aspect (4) of the present disclosure relates to a curved display assembly according to any one of aspects (1) to (3), further comprising a frame, the frame being bonded to the second major surface of the glass sheet around the curved display.

[0092] Aspect (5) of the present disclosure relates to a curved display assembly according to any one of aspects (1) to (4), wherein the curved display is an LCD comprising a first polarizer defining a first display surface, a thin film transistor (TFT) substrate disposed on the first polarizer, a liquid crystal layer disposed on the TFT substrate, a color filter (CF) substrate disposed on the liquid crystal layer, and a second polarizer disposed on the CF substrate, the second polarizer defining a second display surface.

[0093] An aspect (6) of the present disclosure relates to the curved display assembly according to aspect (5), wherein the TFT substrate has two overhanging edges.

[0094] A seventh aspect of the present disclosure relates to the curved display assembly according to the fifth or sixth aspect, wherein the TFT substrate and the CF substrate each comprise a glass material.

[0095] An embodiment (8) of the present disclosure relates to the curved display assembly according to any one of embodiments (1) to (7), wherein the elastic modulus of the second adhesive is at least 0.5 MPa.

[0096] An embodiment (9) of the present disclosure relates to the curved display assembly according to any one of embodiments (1) to (8), wherein the elastic modulus of the first adhesive is 10 kPa to 100 kPa.

[0097] In the embodiment (10) of the present disclosure, the display area is 1×10 -4 The curved display assembly according to any one of aspects (1) to (9), having the following light leakage rate:

[0098] An embodiment (11) of the present disclosure relates to the curved display assembly of any one of embodiments (1) to (10), wherein the glass sheet comprises at least one of soda-lime-silicate glass, aluminosilicate glass, borosilicate glass, aluminoborosilicate glass, or alkali aluminosilicate glass.

[0099] An aspect (12) of the present disclosure relates to a curved display assembly according to any one of aspects (1) to (11), wherein the glass sheet has a thickness between the first major surface and the second major surface that is up to 2 mm.

[0100] An aspect (13) of the present disclosure relates to the curved display assembly according to any one of aspects (1) to (12), wherein the first radius of curvature is between 30 mm and 5 m.

[0101] Aspect (14) of the present disclosure relates to an in-vehicle system comprising a curved display assembly according to any one of aspects (1) to (13), the in-vehicle system being at least one of a center console, an instrument panel, or a dashboard.

[0102] A fifteenth aspect of the present disclosure relates to a vehicle including the vehicle interior system according to the fourteenth aspect.

[0103] Aspect (16) of the present disclosure relates to the vehicle according to aspect (15), wherein the vehicle is an automobile, an aircraft, a ship, or a train.

[0104] Aspect (17) of the present disclosure relates to a method of forming a curved glass article, the method including providing a glass sheet having a first major surface and a second major surface opposite the first major surface; bonding a display to the second major surface of the glass sheet, the display having a display area and two overhanging edges adjacent the display area, the display area being bonded to the second major surface of the glass sheet using a first adhesive and the two overhanging edges being bonded to the second major surface of the glass sheet using a second adhesive, the second adhesive having a higher elastic modulus than the first adhesive; and bending the glass sheet and the display at a temperature below a glass transition temperature of the glass sheet to form a curvature in the glass sheet and the display having a bend axis, the two overhanging edges being parallel to the bend axis, and each of the two overhanging edges extending beyond the display area a distance that is at least three times a thickness of the display.

[0105] Aspect (18) of the present disclosure relates to a method of forming a curved glass article, the method including providing a curved glass sheet having a first major surface and a second major surface opposite the first major surface and defining a curvature with a bend axis; bending a display across the curvature of the glass sheet, the display comprising a display area and two overhanging edges adjacent the display area and parallel to the bend axis; and bonding the display to the second major surface of the glass sheet, the display area being bonded to the second major surface of the glass sheet using a first adhesive and the two overhanging edges being bonded to the second major surface of the glass sheet using a second adhesive, the second adhesive having a higher modulus of elasticity than the first adhesive, each of the two overhanging edges extending beyond the display area a distance that is at least three times a thickness of the display.

[0106] Aspect (19) of the present disclosure relates to the method of aspect (18), wherein providing the curved glass sheet comprises hot forming the flat glass sheet to introduce a permanent curvature into the flat glass sheet.

[0107] Aspect (20) of the present disclosure relates to the method of aspect (18), wherein providing the curved glass sheet comprises cold forming the flat glass sheet by bending the flat glass sheet on a chuck at a temperature below the glass transition temperature of the flat glass sheet.

[0108] Unless otherwise expressly stated, any method described herein is in no way intended to be construed as requiring that its steps be performed in a particular order. Thus, unless a method claim actually recites an order in which its steps should be followed, or unless otherwise expressly stated in the claim or description that the steps are limited to a particular order, no particular order is intended to be inferred. Additionally, as used herein, the article "a" is intended to include one or more than one component or element, and is not intended to be construed to mean only one.

[0109] It is apparent to those skilled in the art that various modifications and variations can be made without departing from the spirit or scope of the disclosed embodiments. Since modifications, combinations, partial combinations and variations of the disclosed embodiments that encompass the spirit and essence of the embodiments can be conceived by those skilled in the art, the disclosed embodiments should be interpreted as including all within the scope of the appended claims and their equivalents.

[0110] Preferred embodiments of the present invention will be described below in detail.

[0111] EMBODIMENT 1 1. A curved display assembly, comprising: a glass sheet having a first major surface and a second major surface opposite the first major surface, the glass sheet having a first thickness measured between the first major surface and the second major surface, the second major surface defining a first radius of curvature of the glass sheet, the first radius of curvature having a bend axis; a curved display having a second thickness between a first display surface and a second display surface, the curved display comprising a display area and two overhanging edges adjacent to the display area and parallel to the bending axis; a first adhesive bonding the second display surface of the curved display to the second major surface of the glass sheet within the display area; a second adhesive bonding each of the two overhanging edges to the second major surface of the glass sheet, the second adhesive having a higher modulus of elasticity than the first adhesive; Equipped with each of the overhanging edges extends outside the display area a distance that is at least three times the second thickness of the curved display; Curved display assembly.

[0112] EMBODIMENT 2 2. The curved display assembly of embodiment 1, wherein the curved display is at least one of a liquid crystal display (LCD), a light emitting diode (LED) display, an organic LED (OLED) display, a quantum dot LED (QLED) display, or a plasma display.

[0113] EMBODIMENT 3 3. The curved display assembly of claim 1 or 2, further comprising a backlight disposed on the second display surface, whereby the curved display is disposed between the backlight and the glass sheet.

[0114] EMBODIMENT 4 4. The curved display assembly of any one of claims 1 to 3, further comprising a frame, the frame being bonded to the second major surface of the glass sheet around the curved display.

[0115] EMBODIMENT 5 5. The curved display assembly of any one of claims 1 to 4, wherein the curved display is an LCD comprising a first polarizer defining the first display surface, a thin film transistor (TFT) substrate disposed on the first polarizer, a liquid crystal layer disposed on the TFT substrate, a color filter (CF) substrate disposed on the liquid crystal layer, and a second polarizer disposed on the CF substrate, the second polarizer defining the second display surface.

[0116] EMBODIMENT 6 6. The curved display assembly of embodiment 5, wherein the TFT substrate comprises the two overhanging edges.

[0117] EMBODIMENT 7 7. The curved display assembly of embodiment 5 or 6, wherein the TFT substrate and the CF substrate each comprise a glass material.

[0118] EMBODIMENT 8 8. The curved display assembly of any one of embodiments 1 to 7, wherein the elastic modulus of the second adhesive is at least 0.5 MPa.

[0119] EMBODIMENT 9 9. The curved display assembly of any one of embodiments 1 to 8, wherein the elastic modulus of the first adhesive is 10 kPa to 100 kPa.

[0120] EMBODIMENT 10 The display area is 1×10 -4 10. The curved display assembly of any one of embodiments 1 to 9, having the following light leakage rate:

[0121] EMBODIMENT 11 11. The curved display assembly of any one of the preceding claims, wherein the glass sheet comprises at least one of soda-lime silicate glass, aluminosilicate glass, borosilicate glass, aluminoborosilicate glass, or alkali aluminosilicate glass.

[0122] EMBODIMENT 12 12. The curved display assembly of any one of the preceding claims, wherein the glass sheet has a thickness between the first major surface and the second major surface that is up to 2 mm.

[0123] EMBODIMENT 13 13. The curved display assembly of any one of embodiments 1 to 12, wherein the first radius of curvature is between 30 mm and 5 m.

[0124] EMBODIMENT 14 A vehicle interior system comprising a curved display assembly according to any one of embodiments 1 to 13, the vehicle interior system being at least one of a center console, an instrument panel, or a dashboard.

[0125] EMBODIMENT 15 A vehicle comprising the vehicle interior system according to embodiment 14.

[0126] EMBODIMENT 16 16. The vehicle of embodiment 15, wherein the vehicle is an automobile, an aircraft, a ship, or a train.

[0127] EMBODIMENT 17 1. A method of forming a curved glass article, comprising: providing a glass sheet having a first major surface and a second major surface opposite the first major surface; bonding a display to the second major surface of the glass sheet, the display comprising a display area and two overhanging edges adjacent to the display area, the display area being bonded to the second major surface of the glass sheet using a first adhesive and the two overhanging edges being bonded to the second major surface of the glass sheet using a second adhesive, the second adhesive having a higher modulus of elasticity than the first adhesive; bending the glass sheet and the display at a temperature below the glass transition temperature of the glass sheet to form a curvature in the glass sheet and the display having a bending axis; Including, the two overhanging edges are parallel to the bending axis; each of the two overhanging edges extends beyond the display area a distance that is at least three times the thickness of the display; method.

[0128] EMBODIMENT 18 1. A method of forming a curved glass article, comprising: providing a curved glass sheet having a first major surface and a second major surface opposite the first major surface and defining a curvature having a bend axis; bending a display through the curvature of the glass sheet, the display comprising a display area and two overhanging edges adjacent the display area and parallel to the bending axis; bonding the display to the second major surface of the glass sheet, the display area being bonded to the second major surface of the glass sheet using a first adhesive and the two overhanging edges being bonded to the second major surface of the glass sheet using a second adhesive, the second adhesive having a higher modulus of elasticity than the first adhesive; Including, each of the two overhanging edges extends beyond the display area a distance that is at least three times the thickness of the display; method.

[0129] EMBODIMENT 19 19. The method of claim 18, wherein providing the curved glass sheet comprises hot forming the flat glass sheet to introduce a permanent curvature into the flat glass sheet.

[0130] EMBODIMENT 20 19. The method of claim 18, wherein providing the curved glass sheet comprises cold-forming the flat glass sheet by bending the flat glass sheet on a chuck at a temperature below the glass transition temperature of the flat glass sheet.

Claims

1. 1. A curved display assembly, comprising: a glass sheet having a first major surface and a second major surface opposite the first major surface, the glass sheet having a first thickness measured between the first major surface and the second major surface, the glass sheet being bent into a cylindrical shape about a bend axis in at least one region of the glass sheet; a curved display having a second thickness between a first display surface and a second display surface, the curved display comprising a display area and two overhanging edges adjacent to the display area and parallel to the bending axis; a first adhesive bonding the second display surface of the curved display to the second major surface of the glass sheet within the display area; a second adhesive bonding each of the two overhanging edges to the second major surface of the glass sheet, the second adhesive having a higher modulus of elasticity than the first adhesive; Equipped with each of the overhanging edges extends outside the display area a distance that is at least three times the second thickness of the curved display; the second adhesive exerts a bending moment along the two overhanging edges to maintain the display in the cylindrical shape. Curved display assembly.

2. 10. The curved display assembly of claim 1, wherein the curved display is at least one of a liquid crystal display (LCD), a light emitting diode (LED) display, an organic LED (OLED) display, a quantum dot LED (QLED) display, or a plasma display.

3. 3. The curved display assembly of claim 1 or 2, wherein the curved display is an LCD comprising a first polarizer defining the first display surface, a thin film transistor (TFT) substrate disposed on the first polarizer, a liquid crystal layer disposed on the TFT substrate, a color filter (CF) substrate disposed on the liquid crystal layer, and a second polarizer disposed on the CF substrate, the second polarizer defining the second display surface.

4. the TFT substrate extends beyond the periphery of the CF substrate to form the two overhanging edges; the two overhanging edges are disposed on opposite sides of the bending axis; The curved display assembly of claim 3.

5. The curved display assembly of claim 3 or 4, wherein the TFT substrate and the CF substrate each comprise a glass material.

6. The curved display assembly of any one of claims 1 to 5, wherein the elastic modulus of the second adhesive is at least 0.5 MPa and the elastic modulus of the first adhesive is between 10 kPa and 100 kPa.

7. 7. The curved display assembly of claim 1, further comprising a frame bonded to the second major surface of the glass sheet around the curved display via a third adhesive.

8. The first adhesive has an elastic modulus of 10 kPa or more and 100 kPa or less, The second adhesive has an elastic modulus of 0.5 MPa or more and 20 MPa or less, The third adhesive has an elastic modulus of 2.0 MPa or more and 20 MPa or less. The curved display assembly of claim 7.

9. 8. The curved display assembly of claim 7, wherein the frame has the cylindrical shape, and the glass sheet is attached to the frame after being cold formed.

10. 1. A method of forming a curved glass article, comprising: providing a glass sheet having a first major surface and a second major surface opposite the first major surface; bonding a display to the second major surface of the glass sheet, the display comprising a display area and two overhanging edges adjacent to the display area, the display area being bonded to the second major surface of the glass sheet using a first adhesive and the two overhanging edges being bonded to the second major surface of the glass sheet using a second adhesive, the second adhesive having a higher modulus of elasticity than the first adhesive; bending at least one of the glass sheet and the display at a temperature below a glass transition temperature of the glass sheet to form a curvature in the glass sheet and the display having a bending axis, the glass sheet and the display being bent into a cylindrical shape about the bending axis; Including, the two overhanging edges are parallel to the bending axis; each of the two overhanging edges extends beyond the display area a distance that is at least three times the thickness of the display; the second adhesive exerts a bending moment along the two overhanging edges to maintain the display in the cylindrical shape; method.

Citation Information

Patent Citations

  • Display device

    CN106548712A

  • Electrooptical device, and electronic apparatus

    JP2011047976A

  • Flexible display panel and display apparatus including the flexible display panel

    JP2013015836A

  • A thin glass laminate that is photosensitive

    JP2018526302A

  • Panel module and display device

    JP2019086564A