How mineral wool is produced
The use of recycled raw materials in mineral wool production with a balanced oxide composition addresses the issues of explosive fragmentation and CO2 emissions, enhancing melt stability and product quality while being environmentally friendly.
Patent Information
- Application Number
- JP2022535503
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-11
- Filing Date
- 2020-12-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Conventional mineral wool production using dolomite and magnesia as magnesium carriers leads to explosive fragmentation and CO2 emissions, affecting furnace operation and product quality, while being environmentally unfriendly.
A method for producing mineral wool with a specific chemical composition using recycled raw materials, free of dolomite and magnesia, and containing at least 8.5% recycled materials with 3.5% magnesium oxide, achieving a balanced oxide content of SiO2 30-50%, Al2O3 15-35%, CaO 5-25%, MgO 1-25%, Fe2O3 2-15%, and Na2O+K2O >10%, promoting high fluidity and fiberization temperatures.
The method enhances melt bath stability, reduces CO2 emissions, and improves product quality with improved resistance to high temperatures, ensuring environmentally friendly production.
Smart Images

Figure 0007588145000001 
Figure 0007588145000002 
Figure 0007588145000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of artificial mineral fibres. It is more particularly directed to a method for producing mineral wool, in particular intended for the manufacture of thermal and / or acoustic insulation products.
[0002] Mineral wool is conventionally obtained by melting a mixture of raw materials in a melting furnace and decanting the molten material thus obtained into a fiberizing device, where the mineral wool is subsequently formed. Usually natural raw materials are selected, and their ratios are adapted based on the desired target chemical composition of the mineral wool. Magnesium oxide may be part of the composition of the mineral wool, with the purpose of giving them certain properties or improving the processability of said mineral wool. Dolomite and magnesia are the main magnesium carriers used in the manufacture of mineral wool. However, these raw materials have certain drawbacks. In fact, they can cause the phenomenon of explosive fragmentation, i.e. "decrepitation", during the melting of the mixture of raw materials. This leads to the formation of a layer formed of decrepitation debris and dust at the top of the furnace, which can be detrimental both to the operation of the furnace and to the quality of the bath of molten material. Moreover, due to their chemical composition, these raw materials contribute significantly to the release of CO2 during the melting of the mixture of raw materials.
[0003] The object of the present invention is to overcome the aforementioned drawbacks by proposing an economical method for producing mineral wool containing magnesium oxide, while guaranteeing good processability, preserving (indeed even improving) the quality of the molten bath and the properties of the mineral wool, in particular in terms of resistance to high temperatures, and reducing the environmental impact.
[0004] Thus, a first aspect of the present invention is a composition comprising, when expressed as mass % of oxide, SiO2 30~50% Al2O3 15-35% CaO 5~25% MgO 1~25% Fe2O3 2~15% Na2O+K2O>10% A method for producing a mineral wool having a chemical composition comprising: The method further comprising: - Providing a mixture of raw materials; - melting said mixture of raw materials to obtain a molten material; - Fiberization of molten material Including, the raw material mixture comprises at least 8.5% by weight of recycled raw material containing at least 3.5% magnesium, expressed by weight of oxide, the recycled raw material being substantially free of carbonates, and the raw material mixture being free of dolomite and magnesia.
[0005] The process according to the invention relates to the production of mineral wool, the chemical composition of which results in high flowability at the fiberization temperature and high liquidus temperature associated with a high glass transition temperature.
[0006] The silica (SiO2) content is within the range of 30 to 50%, preferably 35 to 48%, and more preferably 37 to 45%.
[0007] The alumina (Al2O3) content is within the range of 15 to 35%, preferably 18 to 30%, and further preferably 20% to 28%.
[0008] The lime (CaO) content is in the range of 5 to 25%, preferably 7 to 20%, and more preferably 8% to 18%.
[0009] The magnesia (MgO) content is within the range of 1 to 25%, preferably 1 to 15%, and further preferably 1 to 10%.
[0010] Mineral wool is usually free of alkaline earth metal oxides other than CaO and MgO, but it may nevertheless contain small amounts of BaO or SrO, with contents that may range up to 2%, or even up to 1%, up to 0.20%, or up to 0.1%, which oxides may be present as impurities in certain raw materials.
[0011] The total content of alkali metal oxides (RO), in particular sodium oxide (NaO) and potassium oxide (KO), is more than 10%, preferably 10.2-20%, or even 10.5-15%. The NaO content is typically in the range of 4-20%, preferably 5-15%, or even 6-13%. The KO content, for its part, is typically at most 20%, preferably 1-15%, or even 2-10. The mineral wool preferably does not contain any alkali metal oxides apart from NaO and KO. Nevertheless, it may contain small amounts of LiO (sometimes present as an impurity in certain raw materials) with a content that may range at most 0.5%, or even at most 0.2%, or even at most 0.1%.
[0012] The iron oxide content (total iron expressed in the form of F2O3) is in the range of 2-15%, preferably 2-12% or even 2.5-10%.
[0013] The sum of the contents of SiO2, Al2O3, CaO, MgO, R2O and Fe2O3 is preferably at least 95% by weight, in particular at least 97% by weight, or even at least 98% by weight of the composition of the mineral fibres.
[0014] The chemical composition of the mineral wool may further contain P2O5, in particular the content of which may range up to 3%, or even up to 1.2%, however it is preferably free of P2O5.
[0015] The composition of the mineral wool may further include other elements, especially those present as unavoidable impurities, such as titanium oxide (TiO2) and zirconia (ZrO2) with a content of up to 3%, especially in the range of 0.1-2.0%, or even 1.0%.
[0016] The chemical composition of mineral wool typically contains less than 0.1% by weight of halogens, especially fluorine.
[0017] It is evident that the various preferred ranges above can be freely combined with one another, and for the sake of conciseness it is not possible to list all the different combinations.
[0018] Due to its composition, mineral wool can have the advantage of both being biosoluble, in other words having the ability to dissolve quickly in physiological media, and having good resistance to very high temperatures, with a view to preventing any potential pathogenic risks associated with the potential accumulation of extremely fine fibers in the human body by inhalation. The fire resistance of a structural element corresponds to the period during which the element retains its structural function, guarantees fire retardancy and retains its insulating role. Generally, standard fire tests consist of an increase in temperature according to standard ISO 834, based on the curve of the temperature of cellulose fires.
[0019] Conventionally, the mineral wool composition as described above is obtained by preparing and melting a mixture of raw materials. The method according to the invention comprises a step of providing a mixture of raw materials comprising at least 8.5% by weight of recycled raw materials, containing at least 3.5%, preferably at least 4% or even at least 5% magnesium, expressed by the weight of oxide. The use of such raw materials makes it possible to dispense with dolomite and magnesia, allowing a better melting quality. The other raw materials can be selected from the raw materials conventionally used in the manufacture of mineral wool, such as limestone, phonolite, nepheline syenite, feldspar, basalt, sodium carbonate, iron oxide, etc. Their respective proportions in the mixture of raw materials are determined by the skilled person based on its chemical composition and the target chemical composition of the mineral wool to be obtained. In particular, the mixture of raw materials comprises, as an aluminum carrier, preferably at least 1% by weight, more preferentially at least 2% by weight or even at least 3% by weight of bauxite.
[0020] The recycled raw material can be a by-product from the treatment of aluminum dross (also called salt slag, black dross, white dross or salt cake) from the production and / or recycling of aluminum metal. In the production of aluminum, the first smelting dross that forms on the surface of the tank contains a high proportion of aluminum metal. This dross is therefore generally treated, for example in a rotary kiln, to recover the aluminum it contains. In particular, in some techniques process salts can be added during this second smelting. The second smelting dross, which contains a lower proportion of aluminum metal, can then be treated to extract the remaining aluminum metal therefrom and to reuse the process salt. Some by-products of this treatment, consisting mainly of a mixture of oxides and substantially free of metal residues, can be used as recycled raw material in the process according to the invention. Before being used in the process according to the invention, these by-products can then be subjected to certain treatments (granulation, drying, calcination, etc.). Calcination, for example in a rotary tubular kiln, makes it possible to improve the particle size distribution, in addition to reducing the amount of residual water and other volatile elements such as halogens, ammonia, etc. However, recycled materials are not limited to these examples.
[0021] Recycled raw materials typically contain Al2O3 50-80%, preferably 60-75%; SiO2 2-25%, preferably 5-50%; MgO 3-20%, preferably 5-15%; Fe2O3 0.5-10%, preferably 1-8% The chemical composition includes:
[0022] It typically contains less than 0.9% by weight, preferably less than 0.6% by weight, of halogens, especially fluorine and chlorine. This is because the presence of halogens requires expensive facilities for treating fumes. In certain embodiments, the recycled raw material is specifically fluorine-free, i.e. it contains less than 0.1% by weight of fluorine.
[0023] The recycled raw materials preferably have a composition such that the Al2O3 / MgO mass ratio is greater than 8. Such a ratio is particularly advantageous for obtaining mineral wool according to the invention without requiring the addition of dolomite.
[0024] The recycled raw materials preferably do not contain metal particles, especially aluminum metal. Small amounts of aluminum metal (typically at most 2% by weight, preferably at most 1% by weight, preferentially at most 0.5% by weight) may nevertheless be present, especially when the recycled raw materials are by-products of aluminum dross processing. Similarly, small amounts of aluminum nitride (typically at most 3% by weight, preferably at most 2% by weight, preferentially at most 1% by weight) may also be present, especially when the recycled raw materials are by-products of aluminum dross processing.
[0025] From a mineralogy point of view, the recycled raw material is substantially free of carbonates, i.e., the recycled raw material contains at most 5%, preferably at most 2%, more preferentially at most 1% or even at most 0.5% by weight of carbonates. The recycled raw material preferably contains at least 20%, even at least 30%, and usually at most 80%, or even at most 60%, by weight of amorphous phase. A large proportion of the amorphous phase promotes melting. The recycled raw material contains at least 10%, even at least 20%, and usually at most 50%, by weight of magnesium-containing spinel-type crystalline phase (Mg 1-x M x Al 2-y M' y O4, M and M' are transition metals.
[0026] The raw material mixture is typically in the form of a powder. In particular, the raw material mixture preferably does not include briquettes.
[0027] The melting process can be carried out by various known methods, in particular melting in a fuel-fired furnace or by electric melting. It is not usually carried out in a cupola-type furnace. The compositions of the mineral fibers targeted by the present invention are not particularly compatible with this type of melting, in particular because of their relatively high content of alkali metals. In fact, the mixtures of materials necessary to achieve these compositions tend to pass quickly from the solid state into a low-viscosity liquid, which can coat the coke grains and prevent them from burning. Cupola-type furnaces further promote the evaporation of alkali metals, which creates environmental or safety problems, as well as material losses, due to the high reactivity of said alkali metals with other substances emitted, such as sulfur.
[0028] A fuel-fired furnace includes at least one burner, either aerial (a flame is positioned above a bath of molten material and heats it by radiation) or immersed (a flame is produced directly within the bath of molten material). The or each burner can be supplied with a variety of fuels, such as natural gas or fuel oil.
[0029] "Electric melting" is understood to mean that the vitrifiable mixture is melted by the Joule effect by an electrode immersed in the bath of molten material, excluding any use of other heating means such as a flame. The vitrifiable mixture is usually distributed homogeneously over the surface of the bath of molten material, usually by means of a mechanical device, thus constituting a heat shield limiting the temperature above the bath of molten material, so that the presence of a superstructure is not necessarily necessary. The electrode can be suspended so as to be immersed in the bath of molten material through the top, or installed at the bottom or installed on the side wall of the tank. The first two options are usually preferred for large tanks in order to achieve the best possible distribution of the heating of the bath of molten material. The electrode is preferably made of molybdenum, and also optionally made of tin oxide. The molybdenum electrode passes through the bottom via a water-cooled electrode holder, preferably made of steel.
[0030] The melting process may also use both fuel-fired melting and electrical melting, for example, by using a fuel-fired furnace further equipped with electrodes on the side walls that are used to accelerate the melting of the vitrifiable mixture.
[0031] Conventionally, the mineral wool types targeted by the method according to the invention are fiberized by a centrifugal method called "external", for example of the type described in particular in patents EP 0465310 or EP 0439385, which uses a cascade of centrifugal wheels to which the molten material is fed by a static distribution device. However, the mineral wool compositions described above can also be fiberized by a centrifugation called "internal", i.e. using a centrifuge rotating at high speed and perforated with holes, which significantly reduces the amount of non-fiberized material. This method is described in particular in patents EP 0189354 or EP 0519797. The fiberization step is therefore preferably carried out by internal centrifugation.
[0032] The present invention further comprises, when expressed as mass % of oxide, SiO2 30~50% Al2O3 15-35% CaO 5~25% MgO 1~25% Fe2O3 2~15% Na2O+K2O>10% The present invention relates to the use of recycled raw materials or a mixture of raw materials comprising at least 8.5% by mass of recycled raw materials for the manufacture of mineral wool having a chemical composition comprising: wherein the recycled raw materials comprise at least 3.5% magnesium, expressed by mass of oxide, and are substantially free of carbonates. Furthermore, the mixture of raw materials is preferably free of dolomite and magnesia. The use of the above described recycled raw materials, and more generally the use of a mixture of raw materials comprising it, makes it possible to significantly reduce the carbon dioxide emissions resulting from the melting of the raw materials.
[0033] Another subject of the invention is a mineral wool obtainable by the process described above, comprising at least 8.5% by weight of recycled raw materials, containing at least 3% magnesium, expressed as a percentage by weight of oxide, and SiO2 30~50% Al2O3 15-35% CaO 5~25% MgO 1~25% Fe2O3 2~15% Na2O+K2O>10% and the recycled feedstock is substantially free of carbonates.
[0034] Another subject of the invention is an insulation (thermal barrier) product comprising mineral wool as described above. Such a product is provided in particular in the form of rolls or panels. It can be used, for example, in buildings, industry or transport means, in particular railways or ships. It is particularly suitable for applications where there may be exposure to high temperatures, either continuously (insulating domestic or industrial ovens or stoves, or insulating pipes for the transport of fluids) or exceptionally in fire protection roles (insulating fire doors, ships, tunnels or offshore platforms, etc.). More generally, the product according to the invention can be used to insulate any kind of building, tertiary sector building or dwelling (multiple units or individual). It can be used, for example, in systems for insulation via the outside, for insulation of wooden houses, sandwich panels, ventilation ducts, etc.
[0035] The features described above in relation to the method according to the invention, in particular with regard to the mineral wool composition, the raw material mixture and the recycled raw material, also apply to other aspects of the invention (the use of recycled raw materials or raw material mixtures comprising same, the mineral wool or the insulation product) although they are not repeated for the sake of brevity.
[0036] The following examples illustrate the invention in a non-limiting manner. EXAMPLES
[0037] example The production of mineral wool with the target chemical composition as shown in Table 1 was carried out starting from different material mixtures. The raw material mixture of Comparative Example C1 is a conventional mixture with dolomite as magnesium carrier. In the inventive example I1, the dolomite was completely replaced by the recycled material according to the invention. The composition of the raw material mixture is detailed in Table 2. Table 3 shows the chemical composition of the recycled material. [Table 1] [Table 2] [Table 3]
[0038] During various production runs, no decrepitation was observed during melting of the raw material mixture of Example I1. This significantly reduces the amount of emitted material and the risk of blocking the heat exchanger compared to the use of the raw material mixture of Example C1. The stability of the composition of the molten bath is also improved compared to Example C1. Finally, a reduction of 2-5% in CO2 emissions during melting of the raw material mixture of Example I1 was observed compared to that of Example C1.
Claims
1. When expressed as mass percent of oxide Yes 2 30-50% <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 155~355% CaO 5-25% MgO 1-25% Fe 2 O 3 2~15% Na 2 O+K 2 2nd A method for producing a mineral wool having a chemical composition comprising: The method further comprising: - providing a mixture of raw materials; - melting said mixture of raw materials to obtain a molten material; - Fiberization of the molten material Including, the raw material mixture is in the form of a powder and comprises at least 8.5% by weight of recycled raw material containing at least 3% magnesium expressed by weight of oxide, the recycled raw material is substantially free of carbonate, and the raw material mixture is free of dolomite and magnesia. method.
2. 2. The method according to claim 1, characterized in that the chemical composition of the mineral wool contains less than 0.1% by weight of halogens.
3. 2. The method according to claim 1, characterized in that the recycled raw material contains less than 0.9% by weight, preferably less than 0.6% by weight, of halogens.
4. The method according to any one of claims 1 to 3, characterized in that the recycled raw materials are fluorine-free.
5. 5. The method according to any one of claims 1 to 4, characterized in that the recycled raw material contains up to 2% by weight of aluminium metal.
6. When the recycled raw material is expressed by mass of oxide, <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 550~80%; Yes 2 2~25%; MgO 3-20%; Fe 2 O 3 0.5~10% 6. The method according to claim 1, characterized in that the compound has a chemical composition comprising:
7. The recycled raw material is its Al 2 O 3 7. The method according to claim 1, characterized in that the SiO2 / MgO mass ratio is greater than 8.
8. The method according to any one of claims 1 to 7, characterized in that the mixture of raw materials does not contain briquettes.
9. 9. The method according to any one of claims 1 to 8, characterized in that the mixture of raw materials comprises at least 1% by weight of bauxite.
10. 10. The method according to any one of the preceding claims, characterized in that the mixture of raw materials is melted in a fuel-fired furnace, in particular a submerged-fired furnace, and / or by electric melting.
11. The method according to any one of claims 1 to 10, characterized in that the fiberization is carried out by internal centrifugation.
Citation Information
Patent Citations
JP1972035324B1
Briquettes for the production of mineral fibers and their use
JP2001524447A
mineral wool composition
JP2002526364A
mineral wool composition
JP2003527287A
Glass manufacturing method using electric melting
JP2016501822A