BiSbX(012) layers with high operating temperature for SOT and MRAM devices

By doping BiSb lamellar layers in SOT MTJ devices with cohesive carbides or ceramic materials, the devices can operate at higher temperatures with reduced Sb migration and maintained performance.

JP7588273B2Active Publication Date: 2024-11-21WESTERN DIGITAL TECHNOLOGIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024501784
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-18
Filing Date
2022-05-06
Publication Date
2024-11-21
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

Existing BiSb layers with (012) orientation in spin-orbit-torque (SOT) magnetic tunnel junction (MTJ) devices face challenges in maintaining high spin Hall angle and conductivity while suppressing antimony (Sb) migration at process temperatures required for MRAM devices.

Method used

Incorporating clusters of atoms containing highly cohesive carbides, nitrides, or composite ceramic materials into the BiSb lamellar layers with (012) crystal orientation, which have grain boundary glass forming temperatures below 400°C, thereby stabilizing the grain boundaries and reducing Sb migration.

Benefits of technology

The solution allows SOT MTJ devices to operate at higher temperatures with improved grain boundary stability, reducing Sb migration and maintaining the high spin Hall angle and conductivity of BiSb layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588273000001
    Figure 0007588273000001
  • Figure 0007588273000002
    Figure 0007588273000002
  • Figure 0007588273000003
    Figure 0007588273000003
Patent Text Reader

Abstract

The present disclosure generally relates to a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device with a topological insulator (TI) modulation layer. The TI modulation layer includes a plurality of bismuth or bismuth-rich composition modulation layers, a plurality of TI lamella layers including BiSb with a (012) crystal orientation, and a plurality of texturing layers. The TI lamella layers include dopants or clusters of atoms, and the clusters of atoms include a carbide, a nitride, an oxide, or a composite ceramic material. The clusters of atoms are configured to have a grain boundary glass formation temperature of less than about 400° C. Doping the TI lamella layers including BiSb with a (012) crystal orientation with clusters of atoms including a carbide, a nitride, an oxide, or a composite ceramic material allows the SOT MTJ device to operate at a higher temperature while suppressing migration of Sb from the BiSb in the TI lamella layers.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit of U.S. Non-provisional Application No. 17 / 405,954, filed August 18, 2021, entitled “BISBX(012)LAYERS HAVING INCREASED OPERATING TEMPERATURES FOR SOT AND MRAM DEVICES,” the entire contents of which are incorporated by reference into this application for all purposes.

[0002] FIELD OF THEINVENTION SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure generally relate to buffer and intermediate layers that inhibit antimony (Sb) migration in bismuth antimony (BiSb) layers having a (012) orientation. [Background technology]

[0003] Description of Related Art Topological insulators (Tis) are materials that behave as insulators in their interior but have surfaces that contain conducting states. BiSb is an exemplary TI, which has been proposed as a spin Hall layer for spin torque oscillators (STO) and magnetoresistive random access memory (MRAM) devices. BiSb is a narrow-gap topological insulator that possesses both a giant spin Hall effect and high electrical conductivity.

[0004] NHD Khang, Y. Ueda, and PNHai, "A conductive topological insulator with large spin Hall effect for ultralow power spin orbit torque switching," Nature Materials, v.17, 808 (2018), found that BiSb with (012) crystal orientation has a higher spin Hall angle and higher conductivity than BiSb with (001) crystal orientation. BiSb with (012) crystal orientation was formed on a MnGa film with (001) crystal orientation formed on a GaAs substrate with (001) crystal orientation.

[0005] N. Roschewsky, E.S. Walker, P. Gowtham, S. Muschinske, F. Hellman, S.R. Bank, and S. Salahuddin, "Spin-orbit torque and Nernst effect in Bi-Sb / Co heterostructures," Phys. Rev. B, vol. 99, 195103 (2 May 2019), confirmed that BiSb growth, crystal orientation, spin Hall angle, and high electrical conductivity have low consistency between experiments.

[0006] E.S. Balker, S. Muschinske, C.Brennan, S.R.Na, T.Trivedi, S.D.March, Y.Sun, T.Y.Yang, A.Yau, D.Jung, A.F.Briggs, E.M.Krivoy, M.L.Lee, K.M.Liecti, E.T.Yu, D.Akinwande, and S.R.Bank, "Composition-dependent structural transition in epitaxial Bi1-xSbx thin films on Si(111)", Phys.Rev.Materials 3, 064201 (7 June 2019), grew BiSb alloy films with (012) orientation on Si(111), as well as (012)-textured ultrathin films of pure Bi<20 Å on Si(111) substrates.

[0007] N. Eustathopoulos, "Wetting by Liquid Metals-Application in Materials Processing: The Contribution of the Grenoble Group", Metals 2015, 5(1), 350-370, recognized that liquid metals generally wet transition metal carbide, nitride, boride, and oxide materials that have low band gaps or are somewhat conductive with high covalent cohesion. This wetting behavior is expected at the interface of such low band gap or conductive ceramics with low melting point BiSbX liquid alloys near or above their melting temperature (Tm), or near the boundaries of nanoparticles of low band gap or conductive ceramic layers of oxides, carbides, and nitrides in a liquid metal BiSbX matrix near or above its Tm.

[0008] T. Frolov, D. Olmsted, M. Asta, and Y. Mishin. "Structural phase transformations in metallic grain boundaries", Nature Communications, vol. 4, 1899 (2013), used molecular dynamics simulations to find that grain boundaries (GBs) accumulate dislocations (lattice defects) as a function of annealing temperature, and that the GBs increase in width with temperature, premelting with complete wetting of the GBs well below the melting temperature. Thus, thicker or wider grain boundaries in glass-forming materials produce more grain separation and increased resistance to Sb or Bi or general metal migration across the GBs, allowing higher temperatures to be utilized.

[0009] J. Berry, KR Elder, and M. Grant, "Molecular Dynamic Simulation Literature such as: A phase field crystal study," Phys Rev. B, 77, 224114, 2008; melting at dislocations and grain boundaries, and their premelting of dislocations and other defects with complete wetting of grain boundaries, occurs at temperatures well below the bulk melting temperature Tm. O. Kogtenkova, B. Straumal, A. Korneva, T. Czeppe, A. Wierzbicka-Miernik, M. Faryna, and P Zieba, "Grain Boundary Complexions and Phase Transformations in Al-and Cu-based Alloys," Metals, 2019, 9(1), 10. showed that NiCu grain boundary premelting and wetting occurs more than 600 °C below Tm.

[0010] P. Buffat and JP. Borel, "Size effect on the melting temperature of gold particles", Phys Rev. A, Vol. 13, Num. 6, 1976, 2287-2298, were the first to show that Au nanoparticles can melt below the Tm of bulk Au (~1000°C for nanoparticle sizes of ~10 Å and ~600°C for nanoparticle sizes of ~20 Å). P. R. Cantwell, M. Tang, S. J. Dillon, J. Luo, G. S. Rohrer, and M. P. Harmer, "Grain boundary complexions", Acta Materialia, 62, (2014), 1-48, were review articles on the size dependence of surface and interface melting, nanoparticle melting and dislocation premelting, and complete grain boundary wetting, all well below the bulk temperature Tm value. Tanaka T, Hara SZ, Metallkd 2001;92:1236 showed that the solidus-liquidus of BiCu binary alloy nanoparticles is also size-dependent, melting at a temperature approximately 600°C lower than the alloy bulk Tm.

[0011] Those skilled in the art of thin film deposition can mainly co-deposit highly cohesive oxide, carbide, and nitride ceramic atom clusters with metal alloys. Such ceramic atom clusters can still retain some cohesion and be embedded in the metal matrix as atom clusters. From the above prior art, small atom clusters behave as small nanoparticles. If the ceramic clusters are from materials that exhibit low band gaps or metallic bonding or are conductive, the boundaries of these clusters can be wetted by liquid metals such as BiSbX alloys near or above the melting point of the clusters. These atom clusters coalesce into grain boundary GBs and, considering the small size of the atom clusters, can melt at temperatures well below their bulk Tm to form amorphous glass at the GBs, in some cases about 1000°C lower than the original bulk Tm of the ceramic. Temperatures near or above the melting point widen the GBs and provide better resistance to Bi and Sb migration through the GBs. Thus, a ceramic with a bulk Tm of about 1400 °C can melt at the GB and form a glass at about 400 °C, which is well above the melting temperature of BiSbX alloys but within the process temperatures required for MRAM devices.

[0012] Therefore, there is a need for improved processing temperatures of low melting point topological insulators (TIs), such as BiSbX alloys, that have high spin Hall angles and high electrical conductivity, and improved devices having TI layers with high spin Hall angles and high electrical conductivity. Summary of the Invention

[0013] The present disclosure generally relates to a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device with a topological insulator (TI) modulation layer. The TI modulation layer includes a plurality of bismuth or bismuth-rich composition modulation layers, a plurality of TI lamella layers including BiSb with a (012) crystal orientation, and a plurality of texturing layers. The TI lamella layers include dopants or clusters of atoms, the clusters of atoms including a highly cohesive carbide, nitride, oxide, or composite ceramic material. The clusters of atoms are configured to have a grain boundary glass formation temperature of less than about 400° C. (bulk melting temperature is greater than about 1400° C.) at the grain boundaries. Doping the TI lamella layers including BiSb with a (012) crystal orientation with clusters of atoms including a highly cohesive carbide, nitride, oxide, or composite ceramic material allows the SOT MTJ device to operate at higher temperatures while suppressing migration of Sb from the BiSb in the TI lamella layers.

[0014] In one embodiment, a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device comprises a topological insulator (TI) modulation layer, the TI modulation layer comprising a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) composition modulation layers comprising bismuth at an atomic percent between about 96% and about 100%, a plurality of TI lamella layers, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, nitride, oxide, or composite ceramic material, the clusters of atoms configured to have a grain boundary glass formation temperature less than about 400° C. at grain boundaries having a bulk melting temperature less than about 1400° C., and a plurality of texturing layers.

[0015] In another embodiment, a SOT MTJ device comprises a TI modulation layer comprising: a plurality of bismuth or bismuth-rich composition modulation layers comprising bismuth at about 96% to about 100% atomic percent; a plurality of TI lamella layers comprising bismuth antimony (BiSb) having a (012) crystal orientation, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, a nitride, an oxide, or a composite ceramic material; and a plurality of texturing layers, each texturing layer alternately stacked between the TI lamella layers.

[0016] In yet another embodiment, a SOT MTJ device comprises a buffer layer, an intermediate layer disposed on the buffer layer, and a TI modulation layer disposed between the buffer layer and the intermediate layer, the TI modulation layer including: a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) composition modulation layers comprising bismuth at about 96% to about 100% atomic percent; a plurality of TI lamella layers comprising BiSb having a (012) crystal orientation, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, nitride, oxide, or composite ceramic material, each TI lamella layer being disposed in contact with two of the bismuth or bismuth-rich BiSb composition modulation layers; and a plurality of texturing layers, each texturing layer being disposed in contact with two of the bismuth-rich composition modulation layers. [Brief description of the drawings]

[0017] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure briefly summarized above can be made by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and therefore should not be considered as limiting its scope, as the present disclosure may admit of other equally effective embodiments. [Figure 1]FIG. 1 is a schematic diagram of a particular embodiment of a magnetic media drive including a MAMR write head having a SOT MTJ device. [Diagram 2] FIG. 2 is a partial cross-sectional side view of a particular embodiment of a read / write head having a SOT MTJ device. [Figure 3A] FIG. 1 illustrates a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device according to various embodiments. [Figure 3B] FIG. 1 illustrates a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device according to various embodiments. [Figure 4A] FIG. 4 illustrates an exemplary multi-layer structure of a TI modulation layer that may be utilized with the SOT MTJ device of FIGS. 3A and 3B, according to various embodiments. [Figure 4B] FIG. 4 illustrates an exemplary multi-layer structure of a TI modulation layer that may be utilized with the SOT MTJ device of FIGS. 3A and 3B, according to various embodiments. [Figure 5A] FIG. 13 illustrates an example stack structure of TI lamella layers of a TI modulation layer and a texturing layer as a function of depth. [Figure 5B] FIG. 13 illustrates an example stack structure of TI lamella layers of a TI modulation layer and a texturing layer as a function of depth. [Figure 5C] FIG. 13 illustrates an example stack structure of TI lamella layers of a TI modulation layer and a texturing layer as a function of depth. [Figure 6A] FIG. 1 illustrates the ability to modify the grain structure of a TI stack before and after melting. [Figure 6B] FIG. 1 illustrates the ability to modify the grain structure of a TI stack before and after melting. [Figure 7] FIG. 1 is a graph showing the melting temperature in K versus the diameter of nanocrystals of Au particles, taken from the reference, P. Buffat and JP Borel, Phys Rev. A, Vol. 13, Num. 6, 1976, showing that the melting point of nanocrystals of Au melt is well below the bulk melting temperature (Tm). [Figure 8A]13 is a graph showing the use of a 3x fcc(111) texturing layer to improve BiSb(012) epitaxy and interface roughness. [Figure 8B] 1 is a graph showing the use of various 4x texturing layers of bcc(100)Cr, Ta, W, B2(100)NiAl, and fcc(100)MgO, which can be used to create a BiSb(012) texture in a BiSb layer. [Figure 8C] 1 is a graph showing the use of various 4x texturing layers of bcc(100)Cr, Ta, W, B2(100)NiAl, and fcc(100)MgO, which can be used to create a BiSb(012) texture in a BiSb layer. [Figure 8D] 1 is a graph showing the use of four (100) texturing layers to produce a highly textured (012) BiSb layer. [Figure 8E] FIG. 8E is a blown-up view of the graph in FIG. 8D, which shows a MgO(100) film with a (100) texture. Because the grain size of the MgO film is small, a broad peak appears around 42 degrees in the out-of-plane 2θ XRD plot. [Figure 9A] FIG. 1 is a schematic cross-sectional view of a SOT device for use in a microwave assisted magnetic recording (MAMR) write head. [Figure 9B] FIG. 9B is a schematic MFS diagram of a particular embodiment of a portion of a MAMR write head with the SOT device of FIG. 9A. [Figure 9C] FIG. 9B is a schematic MFS diagram of a particular embodiment of a portion of a MAMR write head with the SOT device of FIG. 9A. [Figure 10] FIG. 1 is a schematic cross-sectional view of a SOT MTJ used as a magnetoresistive random access memory (MRAM) device.

[0018] To facilitate understanding, the same reference numbers have been used, whenever possible, to designate identical elements common to the figures. It is contemplated that elements disclosed in one embodiment may be beneficially utilized on other embodiments without specific mention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In the following, reference will be made to embodiments of the present disclosure. However, it should be understood that the present disclosure is not limited to the specifically described embodiments. Instead, any combination of the following features and elements, whether associated with different embodiments or not, is contemplated to implement and practice the present disclosure. Furthermore, although embodiments of the present disclosure may achieve advantages over other possible solutions and / or over the prior art, whether or not a particular advantage is achieved by a given embodiment does not limit the present disclosure. Thus, the following aspects, features, embodiments, and advantages are merely illustrative and are not considered elements or limitations of the appended claims unless expressly recited in the claim(s). Similarly, references to "the present disclosure" are not to be construed as a generalization of any inventive subject matter disclosed herein, and should not be considered elements or limitations of the appended claims unless expressly recited in the claims.

[0020] The present disclosure generally relates to a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device with a topological insulator (TI) modulation layer. The TI modulation layer includes a plurality of bismuth or bismuth-rich BiSb composition modulation layers, a plurality of TI lamella layers including BiSb with a (012) crystal orientation, and a plurality of texturing layers. The TI lamella layers include dopants or clusters of atoms, the clusters of atoms including high cohesion and high chemical affinity to form carbides, high cohesion and high chemical affinity to form nitrides, high cohesion and high chemical affinity to form oxides, or composite ceramic materials. The clusters of atoms are configured to have a grain boundary glass formation temperature of less than about 400° C. at the grain boundaries (bulk melting temperature is greater than about 1400° C.). Doping a TI lamella layer containing BiSb with (012) crystal orientation with clusters of atoms containing high cohesion and high chemical affinity to form carbides, high cohesion and high chemical affinity to form nitrides, high cohesion and high chemical affinity to form oxides, or composite ceramic materials allows SOT MTJ devices to operate at higher temperatures while suppressing migration of Sb or Bi from the BiSb in the TI lamella layer.

[0021] Embodiments of the present disclosure generally relate to the introduction of clusters of atoms into topological insulator (TI) layers having a (012) orientation. The introduction of clusters of atoms during deposition can enhance grain boundary volume and improve TI grain separation, such that grain boundaries (GBs) can provide additional energy barriers for the migration of reactive TI components.

[0022] In the example where the TI is bismuth antimonide (BiSb), the GBs can prevent the antimony (Sb) from migrating. Antimony (Sb) is highly reactive, and the highly cohesive ceramic GBs provide a low-reactivity medium that reduces chemical interaction between the BiSb layer and external materials while promoting the growth of BiSb in the (012) orientation.

[0023] Conventional BiSb layers with (012) orientation have a large spin Hall angle effect and high electrical conductivity. BiSb layers with (012) orientation can be used to form spin-orbit torque (SOT) magnetic tunnel junction (MTJ) devices. For example, BiSb layers with (012) orientation can be used as spin Hall layers in spin-orbit torque devices in magnetic recording heads, for example as part of a read head and / or microwave assisted magnetic recording (MAMR) write head. In another example, BiSb layers with (012) orientation can be used as spin Hall electrode layers in magnetoresistive random access memory (MRAM) devices. SOT MTJ devices can be vertically stacked or in-plane stacked. SOT MTJ devices can be utilized in, for example, MAMR write heads, MRAMs, artificial intelligence chips, and other applications. Topological insulator (TI) modulation layer composites 304 with (012) orientation have higher spin Hall angles and higher performance in SOT MTJ devices than BiSb layers with (001) orientation.

[0024] 1 is a schematic diagram of a particular embodiment of a magnetic media drive 100 including a MAMR write head with a SOT MTJ device. Such a magnetic media drive may be a single drive or may include multiple drives. For ease of explanation, a single disk drive 100 according to a particular embodiment is shown. As shown, at least one rotatable magnetic medium 112 is supported on a spindle 114 and rotated by a disk drive motor 118. The magnetic recording on each magnetic disk 112 is in the form of any suitable pattern of data tracks, such as an annular pattern of concentric data tracks (not shown) on the magnetic disk 112.

[0025] At least one slider 113 is positioned near the magnetic medium 112, and each slider 113 supports one or more magnetic head assemblies 121 that include a SOT device. As the magnetic disk 112 rotates, the slider 113 moves radially in and out above the disk surface 122 so that the magnetic head assemblies 121 can access different tracks of the magnetic disk 112 on which desired data is written. Each slider 113 is attached to an actuator arm 119 by a suspension 115. The suspension 115 provides a slight spring force that biases the slider 113 toward the disk surface 122. Each actuator arm 119 is attached to an actuator means 127. The actuator means 127 as shown in FIG. 2 can be a voice coil motor (VCM). The VCM includes a coil movable within a fixed magnetic field, and the direction and speed of the coil movement are controlled by motor current signals provided by a control unit 129.

[0026] During operation of disk drive 100, the rotation of magnetic disk 112 creates an air bearing between slider 113 and disk surface 122, which exerts an upward force, or lift, on slider 113. The air bearing thus counteracts the slight spring force of suspension 115 and supports slider 113 a small, substantially constant distance away from and slightly above disk surface 122 during normal operation.

[0027] The various components of disk drive 100 are controlled by control signals generated by control unit 129, such as access control signals and internal clock signals. Typically, control unit 129 includes logic control circuits, storage means, and a microprocessor. Control unit 129 generates control signals for controlling various system operations, such as drive motor control signals on line 123 and head position and seek control signals on line 128. The control signals on line 128 provide the desired current profiles to optimally move and position slider 113 to the desired data track on medium 112. Write and read signals are communicated to and from the write and read heads on assembly 121 by recording channel 125.

[0028] The above description of a typical magnetic media drive, and its illustration in Figure 1, are for illustrative purposes only. It will be apparent that a magnetic media drive may include multiple media or disks and actuators, and each actuator may support multiple sliders.

[0029] 2 is a partial cross-sectional side view of a particular embodiment of a read / write head 200 having a SOT MTJ device. The read / write head 200 faces the magnetic medium 112. The read / write head 200 may correspond to the magnetic head assembly 121 shown in FIG. 1. The read / write head 200 includes a medium facing surface (MFS) 212, such as a gas bearing surface, that faces the disk 112, a MAMR write head 210, and a magnetic read head 211. As shown in FIG. 2, the magnetic medium 112 moves past the MAMR write head 210 in the direction indicated by arrow 232, and the read / write head 200 moves in the direction indicated by arrow 234.

[0030] In some embodiments, the magnetic read head 211 is a magnetoresistive (MR) read head and includes an MR sensing element 204 positioned between MR shields S1 and S2. In other embodiments, the magnetic read head 211 is a magnetic tunnel junction (MTJ) read head and includes an MTJ sensing device 204 positioned between MR shields S1 and S2. The magnetic fields of adjacent magnetized regions in the magnetic medium 112 are detectable by the MR (or MTJ) sensing element 204 as recorded bits. The SOT MTJ devices of various embodiments can be incorporated into the read head 211.

[0031] The MAMR write head 210 includes a main pole 220, a leading shield 206, a trailing shield 240, a spin-orbit torque (SOT) device 250, and a coil 218 that excites the main pole 220. The coil 218 may have a "pancake" configuration that wraps around the rear contact between the main pole 220 and the trailing shield 240 instead of the "spiral" configuration shown in FIG. 2. The SOT device 250 is formed in a gap 254 between the main pole 220 and the trailing shield 240. The main pole 220 includes a trailing taper 242 and a leading taper 244. The trailing taper 242 extends from a recessed position to the MFS 212. The leading taper 244 extends from a recessed position to the MFS 212. The trailing taper 242 and the leading taper 244 may have the same degree of taper, where the degree of taper is measured relative to the longitudinal axis 260 of the main pole 220 .

[0032] In some embodiments, the main pole 220 does not include a trailing taper 242 and a leading taper 244. Instead, the main pole 220 includes a trailing side (not shown) and a leading side (not shown), where the trailing side and the leading side are substantially parallel. The main pole 220 can be a magnetic material, such as an FeCo alloy. The leading shield 206 and the trailing shield 240 can be a magnetic material, such as a NiFe alloy. In certain embodiments, the trailing shield 240 can include a trailing shield hot seed layer 241. The trailing shield hot seed layer 241 can include a high moment sputter material, such as CoFeN or FeXN, where X includes at least one of Rh, Al, Ta, Zr, and Ti. In certain embodiments, the trailing shield 240 does not include a trailing shield hot seed layer.

[0033] 3A and 3B show spin-orbit torque (SOT) magnetic tunnel junction (MTJ) devices 300, 301 according to various embodiments. Each of the SOT MTJ devices 300, 301 may be used individually in the MAMR write head of the drive 100 of FIG. 1, the read / write head 200 of FIG. 2, or other suitable magnetic media drive.

[0034] 3A illustrates an SOT MTJ device 300 according to one embodiment. The SOT MTJ device 300 includes a substrate 302, a buffer layer 310 disposed on the substrate 302, a TI modulation layer 304 including bismuth antimonide (BiSb) having a (012) crystal orientation disposed on the buffer layer 310, an intermediate layer 320 disposed on the TI modulation layer 304, a tunnel magnetoresistance (TMR)-like free layer 322 disposed on the intermediate layer 320, and an MgO layer 324 disposed on the TMR-like free layer 322.

[0035] 3B shows an inverted SOT MTJ device 301 according to one embodiment. The SOT MTJ device 301 includes a substrate 302, a MgO layer 324 disposed on the substrate 302, a TMR-like free layer 322 disposed on the MgO layer 324, a buffer layer 310 disposed on the TMR-like free layer 322, a TI modulation layer 304 including BiSb with a (012) crystal orientation disposed on the buffer layer 310, and an intermediate layer 320 disposed on the TI modulation layer 304. The SOT MTJ devices 300, 301 include the same layers 302, 304, 310, 320, 322, and 324 in different arrangements.

[0036] The substrate 302 can be a silicon substrate or an alumina substrate. The silicon substrate 302 has a cubic crystal structure with a (111), (100), (100), or other crystal orientation. The alumina substrate 302 has a hexagonal crystal structure with a (001) orientation or other crystal orientation, or has an amorphous structure. The substrate 302 can be a bare substrate or can have one or more layers formed thereon, such as a thermally grown or deposited oxide layer thereon.

[0037] In one embodiment, the intermediate layer 320 may be the same material as the buffer layer 310. For example, as shown in Figures 3A and 3B, the intermediate layer 320 and the buffer layer 310 can each individually include a single layer of a crystalline or amorphous material. In another example, the intermediate layer 320 and the buffer layer 310 can each individually include multiple layers of crystalline and / or amorphous material. In another embodiment, the intermediate layer 320 and the buffer layer 310 each individually include one or more different materials.

[0038] The buffer layer 310 and the intermediate layer 320 may each individually be a multi-layer structure, as further described below in FIG. 4A and FIG. 4B. In one embodiment, the buffer layer 310 and / or the intermediate layer 320 are amorphous metal layers or covalently bonded amorphous layers. The covalently bonded amorphous material may include one of a covalently bonded carbide, a covalently bonded oxide, or a covalently bonded nitride, or a composite ceramic. The covalently bonded amorphous material or the metallic amorphous layer has a lattice constant (a) of about 3.5 Å to 3.8 Å. fcc ) should have a nearest neighbor XRD diffraction peak of about 2.0 Å to 2.2 Å, corresponding to the (111) d spacing of a cubic fcc lattice with a fcc The covalently bonded amorphous material should have a low band gap, exhibit metallic bonding, or be somewhat electrically conductive.

[0039] In some embodiments, the buffer layer 310 and the intermediate layer 320 each individually include one or more highly cohesive bonding materials such that the materials are less likely to interact with the TI modulation layer 304 than ionic chemicals. As further described below in Figures 4A and 4B, the buffer layer 310 and the intermediate layer 320 each individually can include one or more materials selected from the group consisting of highly cohesive covalent amorphous materials, tetragonal (001) materials, tetragonal (110) materials, body-centered cubic (bcc) or ordered B2 cubic (100) materials, face-centered cubic (fcc) (100) materials, textured bcc (100) materials, textured fcc (100) materials, textured (100) materials, amorphous metal materials, fcc (111) textured materials, hexagonal close packed (hcp) (002) textured materials, and layered combinations of any one or more of the foregoing materials. Each of the fcc(100), bcc(100), tetragonal(001), and tetragonal(110) materials should have a low bandgap, exhibit metallic bonding, or be somewhat conductive.

[0040] The amorphous metallic material may be selected from the group consisting of NiTa, NiFeTa, NiNb, NiW, NiFeW, NiFeHf, CoHfB, CoZrTa, CoFeB, NiFeB, CoB, FeB, and combinations of alloys thereof having one or more elements selected from the group consisting of Ni, Fe, Co, Zr, W, Ta, Hf, Ag, Pt, Pd, Si, Ge, Mn, Al, and Ti.

[0041] The textured (100) layer is made of (1) RuAl, and (2) several alternatives: (2a) deposited at temperatures above 250° C.; (2b) in heated CrX alloys, where X=Ru, Mo, W, Ti<10 atomic percent (at.%); (2c) CrMo, where n is from about 20 at.% to about 50 at.%. n or (2d) heated Cr / CrMo n In the laminate of CrMo n / Cr / CrMo n (e.g., heated to about 200° C. or less), and (2e) Cr incorporated according to combination with other B2 phase materials such as NiAl and RhAl.

[0042] The tetragonal (001) or (110) material may have an a-axis in the range of about 4.4 Å to about 4.75 Å and a c-axis in the range of about 2.86 Å to about 3.19 Å. The tetragonal (001) or (110) material may have an a-axis lattice parameter in the range of about 4.20 Å to about 4.75 Å. The tetragonal (001) or (110) material may be selected from the group consisting of SbO2, TiO2, IrO2, RuO2, CrO2, VO2, OsO2, RhO2, PdO2, WVO4, CrNbO4, SnO2, GeO2, ZnNb, and ZnTa, composites thereof, and alloys thereof having one or more elements selected from the group consisting of W, Ta, and Nb.

[0043] The fcc(100) material may have a lattice parameter in the range of about 4.08 Å to about 4.75 Å. The fcc(100) material may be selected from (1) rock salt cubic, (2) fcc(100) materials selected from the group consisting of FeO, CoO, NiO, ZrO, MgO, TiO, ScN, TiN, NbN, ZrN, HfN, TaN, ScC, TiC, NbC, ZrC, HfC, TaC, and WC, (3) zinc blende cubic fcc(100) materials selected from the group consisting of CoO, SiC, GaN, FeN, and ZnO, and (4) composite combinations of (1), (2), and / or (3) with one or more elements selected from the group consisting of W, Al, and Si. In other words, the fcc(100) material is selected from the group consisting of FeO, CoO, NiO, ZrO, MgO, TiO, ScN, TiN, NbN, ZrN, HfN, TaN, ScC, TiC, NbC, ZrC, HfC, TaC, WC, CoO, SiC, GaN, FeN, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si.

[0044] The bcc(100) materials are V, Nb, Mo, W, Ta, and WTi. 50 , Al 10 Nb 40 Ti 50 , Cr, CrMo, RuAl in B2 phase, NiAl in B2 phase, and combinations of these alloys having one or more elements selected from the group consisting of Ti, Al, Pd, Pt, Ni, Fe, and Cr.

[0045] The covalently bonded amorphous material may include one of a covalently bonded carbide, a covalently bonded oxide, a covalently bonded nitride, or a ceramic composite thereof. The covalently bonded amorphous material has an a of about 3.5 Å to 3.8 Å. fcc have a fcc It should have a nearest neighbor XRD diffraction peak with a d-spacing of about 2.0 Å to about 2.2 Å, which may correspond to the (111) d-spacing from the crystal structure. Highly cohesive covalently bonded amorphous materials should have a low band gap, exhibit metallic bonding, or be somewhat conductive.

[0046] The fcc(111) texturing material is 3.49 Å fcc Any material may be selected having an a-axis in the range of 2.47 Å < 3.71 Å, or a hcp(002) texturing material may be selected having an a-axis in the range of 2.47 Å < ahcp Any material with an a-axis in the range <2.63 Å can be selected.

[0047] 4A and 4B show an example multi-layer structure of a TI modulation layer 304 that may be utilized with the SOT MTJ device 300, 301 of FIG. 3A and FIG. 3B, according to various embodiments. Although FIG. 4A and FIG. 4B show the TI modulation layer 304 utilized in the SOT MTJ device 300 of FIG. 3A, the TI modulation layers 304a, 304b of FIG. 4A and FIG. 4B may also be utilized in the SOT MTJ device 301 of FIG. 3B. Both the TI modulation layer 304a and the TI modulation layer 304b may be the TI modulation layer 304 of FIG. 3A and / or FIG. 3B. 4A and 4B, the TI modulation layer 304a, 304b may include one or more Bi or Bi-rich BiSb composition modulation layers 402, one or more texturing layers 408, and one or more TI lamella layers 404 co-deposited with atomic clusters 406 that include carbides, nitrides, oxides, or composite ceramic materials that have a low bandgap, exhibit metallic bonding, or are somewhat conductive. The one or more Bi or Bi-rich BiSb composition modulation layers 402 include an atomic percent of Bi between about 96% and about 100%.

[0048] As described further below, the TI lamella layer 404 includes BiSb having a (012) crystallographic orientation 412 and dopants or atomic clusters 406 that include carbides, nitrides, oxides, or composite ceramic materials. The TI lamella layer 404 may be a layered structure including BiSb lamellae 412 and dopant lamellae 406, as described further below in Figures 5A-5C.

[0049] ​As illustrated in Fig. 4A, the TI lamella layers 404 may be alternated with the texturing layers 408 and may be disposed between the Bi or Bi-rich BiSb composition modulation layers 402. Thus, in one embodiment shown in Fig. 4A, the TI modulation layer 304a includes a first Bi-rich composition layer 402 disposed on the buffer layer 310, a first TI lamella layer 404 disposed on the first Bi-rich composition layer 402, a first texturing layer 408 disposed on the first TI lamella layer 404, a second TI lamella layer 404 disposed on the first texturing layer 408, a second texturing layer 408 disposed on the second TI lamella layer 404, a third TI lamella layer 404 disposed on the second texturing layer 408, and a second Bi or Bi-rich BiSb composition layer 402 disposed on the third TI lamella layer 404. Although three TI lamella layers 404, two texturing layers 408, and two Bi-rich composition layers 402 are shown in FIG. 4A, the TI modulation layer 304a may include fewer or additional TI lamella layers 404, texturing layers 408, and Bi or Bi-rich BiSb composition layers 402.

[0050] FIG. 4B illustrates another exemplary configuration of the TI modulation layer 304b according to another embodiment. In FIG. 4B, the TI lamella layer 404 is sandwiched between Bi or Bi-rich BiSb composition layers 402 (i.e., containing Bi at about 96% to about 100% atomic percent) and then alternately stacked with the texturing layers 408. In other words, the TI modulation layer 304 in FIG. 4B is similar to the TI modulation layer 304a in FIG. 4A. However, each of the texturing layers 408 is disposed between and in contact with two Bi-rich composition layers 402. Although FIGS. 4A and 4B are examples of possible TI modulation layer 304 structures, the arrangement of the layers 402, 404, 408 in the TI modulation layer 304 is not limited to the examples in FIGS. 4A and 4B.

[0051] The texturing layer 408 may be selected from the group consisting of amorphous materials with high cohesion and high chemical affinity to form covalent carbides, high cohesion and high chemical affinity to form covalent oxides, high cohesion and high chemical affinity to form covalent nitrides, face-centered cubic (fcc)(100) texturing materials, tetragonal (001) texturing materials, tetragonal (110) texturing materials, body-centered cubic (bcc)(100) texturing materials, fcc(111) texturing materials, and hcp(002) texturing metals. Texturing layer 408, which includes an amorphous material with high cohesion and high chemical affinity to form covalently bonded carbides, high cohesion and high chemical affinity to form covalently bonded oxides, or high cohesion and high chemical affinity to form covalently bonded nitrides, forms strong ionic or covalent chemical bonds with the BiSbX alloy, such that the carbides, nitrides, and / or oxides remain bound and are energetically more favorable to subsequently dissociate and react with the BiSbX alloy.

[0052] The amorphous material used in the texturing layer 408 may include a covalent carbide, a covalent oxide, a covalent nitride, or an amorphous metal layer, and may have an a-layer thickness of about 3.5 Å to 3.8 Å. fcc have a fcc It has a nearest neighbor XRD diffraction peak with d-spacing of about 2.0 Å to about 2.2 Å, which may correspond to the (111) d-spacing from the crystal structure. It should be highly cohesive with high chemical affinity (for carbon, oxygen, or nitrogen) to form covalently bonded amorphous materials, have a low band gap, or exhibit metallic bonding, or be somewhat conductive.

[0053] The fcc(100) textured material used in the texturing layer 408 may be selected from the group consisting of: (1) zinc blende cubic fcc(100) materials selected from the group consisting of FeO, CoO, NiO, ZrO, MgO, TiO, ScN, TiN, NbN, ZrN, HfN, TaN, ScC, TiC, NbC, ZrC, HfC, TaC, and WC; CoO, SiC, GaN, FeN, and ZnO; and (3) composite combinations of (1) and (2) thereof with one or more elements selected from the group consisting of W, Al, and Si. In other words, the fcc(100) texturing material is selected from the group consisting of FeO, CoO, NiO, ZrO, MgO, TiO, ScN, TiN, NbN, ZrN, HfN, TaN, ScC, TiC, NbC, ZrC, HfC, TaC, WC, CoO, SiC, GaN, FeN, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si.

[0054] The fcc(111) texturing material is 3.49 Å fcc Any material with an a-axis in the range <3.71 Å may be selected, or a hcp(002) texturing material may be selected from any material with an a-axis in the range <2.47 Å. hcp Any material with an a-axis in the range <2.63 Å can be selected.

[0055] ​​The tetragonal (001) and (110) texturing materials used in the texturing layer 408 may be selected from the group consisting of SbO2, TiO2, IrO2, RuO2, CrO2, VO2, OsO2, RhO2, RhO2, PdO2, WVO4, CrVO4, CrNbO4, SnO2, GeO2, combinations thereof with the elements Zn, Ti, Nb, and Ta, and combinations of composite materials thereof. In some embodiments, the dopants or atomic clusters 406 in the TI lamella layer 404 include tetragonal materials or any highly cohesive materials with high chemical affinity to carbon, oxygen, or nitrogen to form ceramic materials with low band gaps, materials that exhibit strong or covalent chemical bonds with BiSb, metallic bonds, or materials that are somewhat electrically conductive and have a melting temperature above about 1400° C.

[0056] The TI lamella layer 404 includes BiSb with a (012) orientation 412 co-sputtered with a dopant or atomic cluster 406 including a carbide, nitride, oxide, or composite ceramic material. When the dopant or atomic cluster 406 includes a composite ceramic material, the composite ceramic material can be selected from the group consisting of Bi, Pb, Ga, Sc, Si, Ti, V, Cr, Mn, Fe, Zr, Nb, Mo, In, Ir, Ru, V, Os, Rh, Pd, WV, CrV, CrNb, Ge, Zn, ZnNbTi, ZnTiTa, Co, Mg, Sn, Sb, Te, Hf, Ta, W, oxides thereof, nitrides thereof, carbides thereof, and composite ceramic combinations thereof.

[0057] The dopant or atom clusters 406 may be low melting ceramics such as oxides of Bi, Sn, Sb, Pd, In, such bulk ceramics have low melting points, form cohesive covalent structures with high oxygen affinity with either low band gaps, or exhibit metallic bonding properties, or are somewhat conductive with high resistivity. These clusters generally prefer to stay as clusters, not dissociate, do not react with BiSbX metals, and easily coalesce and form oxide glasses at grain boundaries. The above mentioned clusters of low melting ceramic atoms are wetted by low melting TI metals such as BiSbX alloys and their alloys, and coalesce and form ceramic glasses at grain boundaries which should increase the processing temperature of BiSbX alloys and improve the thermal transport of Sb and / or Bi. The ceramic clusters do not tend to bond with BiSbX alloys, and form cohesive high chemical affinities for carbon, oxygen, or nitrogen to form strong ionic or covalent structures that act as thermal transport grain boundary barriers. Lower melting intergranular ceramic glasses may offer some engineering advantages when high temperatures are required in the manufacturing process, or may offer a better compromise of material properties, or ease of construction of SOT devices.

[0058] The dopant or atomic clusters 406 may have a melting temperature of less than about 1400° C. Due to the small size of the atomic clusters and the alloying interactions, the melting point of the atomic clusters may be substantially reduced. The atomic clusters may be configured to have a grain boundary glass formation temperature of less than about 400° C. Doping the TI lamella layer 404 with the atomic clusters 406 reduces BiSbX grain growth in the TI lamella layer 404 and provides epitaxial growth with a BiSb(012) texturing layer. Due to the high degree of cohesion, high chemical affinity to carbon, oxygen, or nitrogen, and ionic or covalent chemical bonding nature of the dopant or atomic clusters 406, the dopant or atomic clusters 406 tend to remain as clusters and have minimal chemical interaction with the BiSbX alloy of the TI lamella layer 404, thereby providing an interface layer barrier against Sb migration while reducing grain growth and improving roughness in the MTJ SOT device 300, 301.

[0059] Each of the TI lamella layers 404 may be treated with low energy and glancing angle plasma treatment (PT) to improve the growth roughness and overall stack roughness of the SOT MTJ device. The atomic clusters 406 may be a low melting point alloy with high thermal mobility, and at least some of the atomic clusters are oxidized during co-sputtering. The method of forming the SOT MTJ device 300, 301 may include post-annealing. The annealing process melts the atomic clusters to form a glass boundary around the TI grains.

[0060] 5A-5C show an example stack structure of the TI lamella layer 404 of the TI modulation and texturing layer 304 as a function of depth. In FIG. 5A-5C, the dopant or atom clusters 406 (i.e., dopant X lamellae) comprise carbides, nitrides, oxides, or composite ceramic materials as described above, and the BiSb lamellae 412 comprise BiSbX with a (012) crystal orientation. FIG. 5A shows a modulated structure where each cluster of atoms 406 is doped between two BiSb lamellae 412. FIG. 5B shows an edge structure, where for every two clusters of atoms 406, there are three BiSb lamellae 412. FIG. 5C shows a uniform structure where the BiSb lamellae 412 and atom clusters 406 are uniformly distributed. 5A-5C are examples of doping of atomic clusters 406 in BiSb lamellae 412, the TI modulation layer 304 can include any method of non-uniform distribution of doping of atomic clusters 406 in the BiSb lamellae 412.

[0061] 6A and 6B show the ability to modify the grain structure before and after melting of the TI stack 304. The TI modulation layer 304 may melt during use of the MTJ SOT device 300, 301, for example. FIG. 6A shows the deposition of a BiSb lamella 412 followed by a thin uniform deposition of atomic clusters 406. As shown in FIG. 6A, the atomic clusters 406 are randomly located on the BiSb lamella 412. FIG. 6B shows the distribution of atomic clusters 406 after growth and annealing of the BiSb lamella 412. As shown in FIG. 6B, the atomic clusters 406 migrate to the grain boundaries 614 of the BiSb lamella 412, thereby strengthening the grain boundaries 614 against thermal migration while providing an additional barrier against Sb migration. The dopants or atomic clusters 406 reduce the as-deposited grain size of the BiSbX lamellae 412 and allow thermal transport to the grain boundaries 614 due to grain coarsening upon post-annealing.

[0062] FIG. 7 is a graph 700 showing the melting temperature of Au nanoparticles in K versus the diameter of the Au nanoparticles. This behavior is generally true for all materials when the feature size, grain size, or cluster size is reduced and the melting of the materials used to form these features is also reduced. For Au, the melting temperature is 1000° C. for a grain size of 10 Å, or 600° C. for a grain size of 20 Å. Literature shows that this is also true for thin surface or interface layers, as well as grain boundaries where premelting and complete wetting of the grain boundaries can be achieved at temperatures well below the bulk melting temperature of the material. The dopants or atomic clusters 406 can reduce the grain size of the as-deposited BiSbX lamellae 412. However, upon melting, the TI modulation layer 304 reverts to a large grain size at room temperature, and with the appropriate buffer 310, texture 408, and intermediate layer 320, the TI modulation layer 304 retains most of its crystal structure and its (012) texture after melting.

[0063] 8A is a graph 800 illustrating the use of a (111) textured texturing layer to improve interfacial roughness to improve epitaxy during growth. The highest texture, with a full width at half maximum (FWHM) of about 8 degrees, has the lowest interfacial roughness, less than about 8 Å. Layers 310, 320, and 408 have a roughness of 3.49 Å. fcc Triple fcc(111) textured materials with lattice spacings in the range of <3.71 Å, or 2.47 Å hcp It can be a hcp(002) textured material with an a-axis in the range of <2.63 Å.

[0064] Figures 8B and 8C are graphs 801, 803, respectively, showing an example of a quadruple texturing layer that can be used to produce a BiSb(012) texture. Figure 8D is graph 805 showing an example of a quadruple texturing layer that produces a highly textured BiSb(012) film. Figure 8E is graph 807 showing a stretched portion of graph 805 of Figure 8D, showing that a 25 Å thick MgO texturing film has a (100) texture. ​​

[0065] FIG. 9A is a schematic cross-sectional view of a SOT device 900 for use in a microwave assisted magnetic recording (MAMR) write head, such as the MAMR write head of the drive 100 of FIG. 1 or other suitable magnetic media drive. The SOT device 900 includes a TI modulation layer 304 including BiSb with a (012) crystal orientation and a dopant or cluster of atoms including a carbide, nitride, oxide, or composite ceramic material disposed and formed on a buffer layer 310 formed on a substrate 302, such as the TI modulation layer 304 and buffer layer 310 of FIGS. 3A-6B. A spin torque layer (STL) 970 is formed on the TI modulation layer 304. The STL 970 includes a ferromagnetic material, such as a layer of one or more of CoFe, CoIr, NiFe, and CoFeX alloys, where X=B, Ta, Re, or Ir.

[0066] In certain embodiments, a current shunt blocking layer 960 is disposed between the TI modulation layer 304 and the STL 970. The current shunt blocking layer 960 reduces current flow from the TI modulation layer 304 to the STL 970, but allows spin-orbit coupling between the TI modulation layer 304 and the STL 970. In certain embodiments, the current shunt blocking layer 960 includes a magnetic material that provides greater spin-orbit coupling between the TI modulation layer 304 and the STL 970 than a non-magnetic material. In certain embodiments, the current shunt blocking layer 960 includes a magnetic material of FeCo, FeCoM, FeCoMO, FeCoMMeO, FeCoM / MeO stack, FeCoMNiMnMgZnFeO, FeCoM / NiMnMgZnFeO stack, multiple layers / stacks thereof, or combinations thereof, where M is one or more of B, Si, P, Al, Hf, Zr, Nb, Ti, Ta, Mo, Mg, Y, Cu, Cr, and Ni, and Me is Si, Al, Hf, Zr, Nb, Ti, Ta, Mg, Y, or Cr. In certain embodiments, the current shunt blocking layer 960 is formed to a thickness of about 10 Å to about 100 Å. In certain aspects, the current shunt blocking layer 960 having a thickness of more than 100 Å can reduce spin-orbit coupling between the TI modulation layer 304 and the STL 970. In certain embodiments, a current shunt blocking layer having a thickness less than 10 Å may not sufficiently reduce current flow from the TI modulation layer 304 to the STL970.

[0067] In certain embodiments, additional layers are formed over the STL 970, such as a spacer layer 980 and a pinning layer 990. The pinning layer 990 can partially pin the STL 970. The pinning layer 990 includes a single or multiple layers of PtMn, NiMn, IrMn, IrMnCr, CrMnPt, FeMn, other antiferromagnetic materials, or combinations thereof. The spacer layer 980 includes a single or multiple layers of magnesium oxide, aluminum oxide, other nonmagnetic materials, or combinations thereof.

[0068] 9B and 9C are schematic MFS diagrams of a particular embodiment of a portion of a MAMR write head 210 having the SOT device 900 of FIG. 9A. The MAMR write head 210 can be the write head of FIG. 2 or any other suitable write head in the drive 100 of FIG. 1 or any other suitable magnetic media drive, such as a tape drive. The MAMR write head 210 includes a main pole 220 and a trailing shield 240 in the tracking direction. The SOT device 900 is disposed in the gap between the main pole and the trailing shield 240.

[0069] In operation, a charging current through the TI modulation layer 304 acting as a spin Hall layer generates a spin current in the BiSb layer. Spin-orbit coupling between the BiSb layer and the spin torque layer (STL) 970 causes switching or precession of the magnetization of the STL 970 due to spin-orbit coupling of the spin current from the TI modulation layer 304. The switching or precession of the magnetization of the STL 970 can generate an auxiliary AC magnetic field to the write magnetic field. Energy-assisted write heads based on SOT have several times greater power efficiency compared to MAMR write heads based on spin transfer torque. As shown in FIG. 9B, the easy axis of the magnetization direction of the STL 970 is perpendicular to the MFS from the shape anisotropy of the STL 970, from the pinning layer 990 of FIG. 9A, and / or from the hard bias element close to the STL 970. As shown in FIG. 9C, the easy axis of magnetization of the STL 970 is parallel to the MFS from the shape anisotropy of the STL 970, from the pinning layer 990 of FIG. 9A, and / or from hard bias elements proximate to the STL 970.

[0070] 10 is a schematic cross-sectional view of a SOT MTJ 1001 used as a magnetoresistive random access memory (MRAM) device 1000. The MRAM device 1000 includes a reference layer (RL) 1010, a spacer layer 1020 disposed on the RL 1010, a recording layer 1030 disposed on the spacer layer 1020, a buffer layer 310 on a current shunt blocking layer 1040 disposed on the recording layer 1030, and a TI modulation layer 304 including BiSb with a (012) crystal orientation, a dopant or cluster of atoms including a carbide, nitride, oxide, or composite ceramic material disposed on the buffer layer 310. The TI modulation layer 304 and buffer layer 310 may be the TI modulation layer 304 and buffer layer 310 of FIGS. 3A-6B.

[0071] The RL 1010 includes single or multiple layers of CoFe, other ferromagnetic materials, or combinations thereof. The spacer layer 1020 includes single or multiple layers of magnesium oxide, aluminum oxide, other dielectric materials, or combinations thereof. The recording layer 1030 includes single or multiple layers of CoFe, NiFe, other ferromagnetic materials, or combinations thereof.

[0072] As mentioned above, in certain embodiments, the current shunt blocking layer 1040 is disposed between the buffer layer 310 and the recording layer 1030. The current shunt blocking layer 1040 reduces current flow from the TI modulation layer 304 to the recording layer 1030, but allows spin-orbit coupling between the TI modulation layer 304 and the recording layer 1030. For example, writing to an MRAM device can be enabled by spin-orbit coupling between the BiSb layer and the recording layer 1030, which allows switching of the magnetization of the recording layer 1030 by spin-orbit coupling of the spin current from the TI modulation layer 304. In certain embodiments, the current shunt blocking layer 1040 includes a magnetic material that provides greater spin-orbit coupling between the TI modulation layer 304 and the recording layer 1030 than a non-magnetic material. In certain embodiments, the current shunt blocking layer 1040 comprises a magnetic material of FeCoM, FeCoMO, FeCoMMeO, FeCoM / MeO stack, FeCoMNiMnMgZnFeO, FeCoM / NiMnMgZnFeO stack, multiple layers / stacks thereof, or combinations thereof, where M is one or more of B, Si, P, Al, Hf, Zr, Nb, Ti, Ta, Mo, Mg, Y, Cu, Cr, and Ni, and Me is Si, Al, Hf, Zr, Nb, Ti, Ta, Mg, Y, or Cr.

[0073] The MRAM device 1000 of Figure 10 can include other layers such as pinning layers, pinning structures (e.g., synthetic antiferromagnetic (SAF) pinned structures), electrodes, gates, and other structures. Other MRAM devices than the structure of Figure 10 can be formed using a TI modulation layer 304 with a (012) orientation on a buffer layer 310 to form a SOT MTJ 1001.

[0074] By doping a TI lamella layer containing BiSb with a (012) crystal orientation with a carbide, nitride, oxide, or composite ceramic material, the melting point of the dopant or atomic clusters can be substantially lowered, further reducing the migration of Sb in the TI lamella layer while allowing the MTJ SOT device to operate at higher temperatures. The atomic clusters migrate to the grain boundaries of the BiSb lamella in the TI lamella layer, thereby providing an additional barrier to Sb migration while the grain boundaries are strengthened against thermal migration. Doping the TI lamella layer with a carbide, nitride, oxide, or composite ceramic material reduces BiSbX grain growth in the TI lamella layer and provides epitaxial growth with a BiSb(012) texturing layer. Due to the nature of high or strong ionic or covalent chemical bonds of the dopants or atom clusters, the dopants or atom clusters have minimal chemical interaction with the BiSbX alloy of the TI lamella layer, thereby providing an interfacial layer barrier against Sb migration while reducing grain growth and improving roughness in the MTJ SOT device.

[0075] Furthermore, to maintain the growth and (012) texture of the TI material to match the MRAM or SOT device intermediate or buffer layers, higher process temperatures can be reached using low-melting TI materials such as BiSbX by using low band gap or conductive ceramics, or ceramics with metallic bonds, since the glass-forming grain boundaries separate at wide grain boundaries, along with the ceramic-TI stack, composition modulation layer, and growth texturing layer defined later.

[0076] In one embodiment, a spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device comprises a topological insulator (TI) modulation layer, the TI modulation layer comprising a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) composition modulation layers comprising bismuth at an atomic percent between about 96% and about 100%, a plurality of TI lamella layers, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, nitride, oxide, or composite ceramic material, the clusters of atoms configured to have a grain boundary glass formation temperature less than about 400° C. at grain boundaries having a bulk melting temperature less than about 1400° C., and a plurality of texturing layers.

[0077] The TI lamella layer includes bismuth antimony (BiSb) having a (012) crystal orientation. The composite ceramic material has a melting temperature of less than about 1400° C. The texturing layer is selected from the group consisting of amorphous materials including covalently bonded carbides, oxides, or nitrides, face-centered cubic (fcc) materials, tetragonal materials, and body-centered cubic (bcc) materials. The SOT MTJ device further includes a buffer layer, the TI modulation layer being disposed on the buffer layer, and an intermediate layer disposed on the TI modulation layer. A first bismuth or bismuth-rich BiSb composition modulation layer of the plurality of bismuth or bismuth-rich BiSb composition modulation layers is disposed in contact with the buffer layer, and a second bismuth or bismuth-rich BiSb composition modulation layer of the plurality of bismuth or bismuth-rich BiSb composition modulation layers is disposed in contact with the intermediate layer.

[0078] The carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The oxide material is selected from the group consisting of FeO, CoC, ZrO, MgO, TiO, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The composite ceramic material is selected from the group consisting of Bi, Pb, Ga, Sc, Ti, V, Cr, Mn, Fe, Zr, Nb, Mo, In, Ir, Ru, V, Os, Rh, Pd, WV, CrV, CrNb, Ge, ZnNb, ZnTa, Co, Mg, Sn, Sb, Te, Hf, Ta, W, oxides thereof, nitrides thereof, carbides thereof, and alloys thereof. The magnetoresistive random access memory device comprises a SOT MTJ.

[0079] In another embodiment, a SOT MTJ device comprises a TI modulation layer comprising: a plurality of bismuth or bismuth-rich composition modulation layers comprising bismuth at about 96% to about 100% atomic percent; a plurality of TI lamella layers comprising bismuth antimony (BiSb) having a (012) crystal orientation, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, a nitride, an oxide, or a composite ceramic material; and a plurality of texturing layers, each texturing layer alternately stacked between the TI lamella layers.

[0080] The TI lamella layer is co-deposited with clusters of atoms in a modulated orientation. The TI lamella layer is co-deposited with clusters of atoms in an edge orientation. The TI lamella layer is co-deposited with clusters of atoms in a uniform or non-uniformly distributed orientation. The carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The oxide material is selected from the group consisting of FeO, CoC, ZrO, MgO, TiO, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The magnetoresistive random access memory device comprises a SOT MTJ.

[0081] In yet another embodiment, a SOT MTJ device comprises a buffer layer, an intermediate layer disposed on the buffer layer, and a TI modulation layer disposed between the buffer layer and the intermediate layer, the TI modulation layer including: a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) composition modulation layers comprising bismuth at about 96% to about 100% atomic percent; a plurality of TI lamella layers comprising BiSb having a (012) crystal orientation, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, nitride, oxide, or composite ceramic material, each TI lamella layer being disposed in contact with two of the bismuth or bismuth-rich BiSb composition modulation layers; and a plurality of texturing layers, each texturing layer being disposed in contact with two of the bismuth-rich composition modulation layers.

[0082] The carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The oxide material is selected from the group consisting of FeO, CoC, ZrO, MgO, TiO, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si. The composite ceramic material is selected from the group consisting of Bi, Pb, Ga, Sc, Ti, V, Cr, Mn, Fe, Zr, Nb, Mo, In, Ir, Ru, V, Os, Rh, Pd, WV, CrV, CrNb, Ge, ZnNb, ZnTa, Co, Mg, Sn, Sb, Te, Hf, Ta, W, oxides thereof, nitrides thereof, carbides thereof, and alloys thereof. A first bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the buffer layer, and a second bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the intermediate layer.

[0083] The intermediate layer comprises one or more materials selected from the group consisting of a tetragonal (001) material, a tetragonal (110) material, a body-centered cubic (bcc) (100) material, a face-centered cubic (fcc) (100) material, a textured bcc (100) material, a textured fcc (100) material, a textured (100) material, a textured fcc (111) material, a textured hcp (002) material, an amorphous material comprising covalently bonded carbides, oxides, or nitrides, an amorphous metallic material, and layered combinations of any one or more of the foregoing materials. The buffer layer includes one or more sublayers including one or more materials selected from the group consisting of tetragonal (001) material, tetragonal (110) material, body-centered cubic (bcc) (100) material, face-centered cubic (fcc) (100) material, textured bcc (100) material, textured fcc (100) material, textured (100) material, textured fcc (111) material, textured hcp (002) material, amorphous metal material, amorphous material including covalently bonded carbides, oxides, or nitrides, and layered combinations of any one or more of the foregoing materials. The magnetoresistive random access memory device comprises a SOT MTJ.

[0084] While the above is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, which scope is determined by the following claims.

Claims

1. 1. A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device, comprising: A topological insulator (TI) modulation layer, comprising: a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) compositionally modulated layers comprising bismuth at an atomic percent of about 96% to about 100%; and a plurality of TI lamella layers, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, a nitride, an oxide, or a composite ceramic material, the clusters of atoms being configured to have a grain boundary glass formation temperature of less than about 400° C. at grain boundaries having a bulk melting temperature of less than about 1400° C.; a TI modulation layer comprising: Multiple texturing layers; A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device comprising:

2. The SOT MTJ device of claim 1 , wherein the TI lamella layer comprises BiSb having a (012) crystal orientation.

3. The SOT MTJ device of claim 1 , wherein the composite ceramic material has a melting temperature less than about 1400° C.

4. 2. The SOT MTJ device of claim 1, wherein the texturing layer is selected from the group consisting of amorphous materials containing covalently bonded carbides, oxides, or nitrides, face-centered cubic (fcc) materials, tetragonal materials, body-centered cubic (bcc) materials, and metallic amorphous materials.

5. a buffer layer, the TI modulation layer being disposed on the buffer layer; an intermediate layer disposed on the TI modulation layer; The SOT MTJ device of claim 1 further comprising:

6. 6. The SOT MTJ device of claim 5, wherein a first bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the buffer layer, and a second bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the intermediate layer.

7. 2. The SOT MTJ device of claim 1, wherein the carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si, and the oxide material is selected from the group consisting of FeO, ZrO, MgO, TiO, ZnO, and combinations of these composite materials with one or more elements selected from the group consisting of W, Al, and Si.

8. the nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of these composite ceramic materials having one or more elements selected from the group consisting of W, Al, and Si; The composite ceramic material is selected from the group consisting of Bi, Pb, Ga, Sc, Ti, V, Cr, Mn, Fe, Zr, Nb, Mo, In, Ir, Ru, V, Os, Rh, Pd, WV, CrV, CrNb, Ge, ZnNb, ZnTa, Co, Mg, Sn, Sb, Te, Hf, Ta, W, oxides thereof, nitrides thereof, carbides thereof, and alloys thereof. The SOT MTJ device of claim 1 .

9. A magnetoresistive random access memory device comprising the SOT MTJ device of claim 1.

10. A magnetic recording device comprising a magnetic recording head comprising the SOT MTJ device of claim 1.

11. A magnetoresistive memory comprising the SOT MTJ device of claim 1.

12. 1. A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device, comprising: A topological insulator (TI) modulation layer, comprising: a plurality of bismuth or bismuth-rich compositionally modulated layers comprising bismuth at an atomic percent of about 96% to about 100%; a plurality of TI lamella layers comprising bismuth antimony (BiSb) having a (012) crystallographic orientation, the TI lamella layers being co-deposited with a cluster of atoms, the cluster of atoms comprising a carbide, a nitride, an oxide, or a composite ceramic material; a plurality of texturing layers, each texturing layer being alternately stacked between TI lamella layers; A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device with a TI modulation layer comprising:

13. The SOT MTJ device of claim 12 , wherein the TI lamella layer is co-deposited with the clusters of atoms in a modulated orientation.

14. The SOT MTJ device of claim 12 , wherein the TI lamella layer is co-deposited with the clusters of atoms in an edge orientation.

15. The SOT MTJ device of claim 12 , wherein the TI lamella layer is co-deposited with the clusters of atoms in a uniform or non-uniform distributed orientation.

16. 13. The SOT MTJ device of claim 12, wherein the carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of composites thereof having one or more elements selected from the group consisting of W, Al, and Si.

17. 13. The SOT MTJ device of claim 12, wherein the nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of composite materials thereof with one or more elements selected from the group consisting of W, Al, and Si.

18. 13. The SOT MTJ device of claim 12, wherein the oxide material is selected from the group consisting of FeO, ZrO, MgO, TiO, ZnO, and combinations of composite materials thereof with one or more elements selected from the group consisting of W, Al, and Si.

19. A magnetoresistive random access memory device comprising the SOT MTJ device of claim 12.

20. A magnetic recording device comprising a magnetic recording head comprising the SOT MTJ device of claim 12.

21. A magnetoresistive memory comprising the SOT MTJ device of claim 12.

22. 1. A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device, comprising: A buffer layer; an intermediate layer disposed on the buffer layer; a topological insulator (TI) modulation layer disposed between the buffer layer and the intermediate layer, the topological insulator (TI) modulation layer comprising: a plurality of bismuth or bismuth-rich bismuth antimony (BiSb) compositionally modulated layers comprising bismuth at an atomic percent of about 96% to about 100%; and a plurality of TI lamella layers comprising BiSb having a (012) crystallographic orientation, the TI lamella layers being co-deposited with clusters of atoms, the clusters of atoms comprising a carbide, a nitride, an oxide, or a composite ceramic material, each TI lamella layer being disposed in contact with two bismuth or bismuth-rich BiSb compositionally modulated layers; a plurality of texturing layers, each texturing layer being disposed in contact with two bismuth or bismuth-rich BiSb composition modulation layers; A topological insulator (TI) modulation layer comprising: A spin-orbit torque (SOT) magnetic tunnel junction (MTJ) device comprising:

23. 23. The SOT MTJ device of claim 22, wherein the carbide material is selected from the group consisting of ScC, TiC, NbC, ZrC, HfC, TaC, WC, SiC, and combinations of composites thereof with one or more elements selected from the group consisting of W, Al, and Si.

24. 23. The SOT MTJ device of claim 22, wherein the nitride material is selected from the group consisting of ScN, TiN, NbN, ZrN, HfN, TaN, GaN, FeN, and combinations of composite materials thereof with one or more elements selected from the group consisting of W, Al, and Si.

25. 23. The SOT MTJ device of claim 22, wherein the oxide material is selected from the group consisting of FeO, ZrO, MgO, TiO, ZnO, and composite combinations thereof with one or more elements selected from the group consisting of W, Al, and Si.

26. 23. The SOT MTJ device of claim 22, wherein the composite ceramic material is selected from the group consisting of Bi, Pb, Ga, Sc, Ti, V, Cr, Mn, Fe, Zr, Nb, Mo, In, Ir, Ru, V, Os, Rh, Pd, WV, CrV, CrNb, Ge, ZnNb, ZnTa, Co, Mg, Sn, Sb, Te, Hf, Ta, W, oxides thereof, nitrides thereof, carbides thereof, and alloys thereof.

27. 23. The SOT MTJ device of claim 22, wherein a first bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the buffer layer, and a second bismuth or bismuth-rich BiSb composition modulated layer of the plurality of bismuth or bismuth-rich BiSb composition modulated layers is disposed in contact with the intermediate layer.

28. 23. The SOT MTJ device of claim 22, wherein the intermediate layer comprises one or more materials selected from the group consisting of tetragonal (001) material, tetragonal (110) material, body-centered cubic (bcc) (100) material, face-centered cubic (fcc) (100) material, textured bcc (100) material, textured fcc (100) material, textured (100) material, textured fcc (111) material, textured hcp (002) material, amorphous material comprising covalently bonded carbides, oxides, or nitrides, amorphous metallic material, and layered combinations of any one or more of the preceding materials.

29. 23. The SOT MTJ device of claim 22, wherein the buffer layer comprises one or more sublayers comprising one or more materials selected from the group consisting of tetragonal (001) material, tetragonal (110) material, body-centered cubic (bcc) (100) material, face-centered cubic (fcc) (100) material, textured bcc (100) material, textured fcc (100) material, textured (100) material, textured fcc (111) material, textured hcp (002) material, amorphous metal material, amorphous material comprising covalently bonded carbides, oxides, or nitrides, and layered combinations of any one or more of the foregoing materials.

30. 23. A magnetoresistive random access memory device comprising the SOT MTJ device of claim 22.

31. 23. A magnetic recording device comprising a magnetic recording head comprising the SOT MTJ device of claim 22.

32. 23. A magnetoresistive memory comprising the SOT MTJ device of claim 22.

Citation Information

Patent Citations

  • Magnetoresistive memory

    JP2021057357A

  • Magnetic device with a hybrid free layer stack

    US20210104344A1

  • BiSb Topological Insulator with Novel Buffer Layer that Promotes a BiSb (012) Orientation

    US20210249038A1

  • METHOD FOR MANUFACTURING LAYERED STRUCTURE OF MAGNETIC BODY AND BiSb, MAGNETORESISTIVE MEMORY, AND PURE SPIN INJECTION SOURCE

    WO2019054484A1