Film forming method

The film forming method addresses the issue of ozone-induced oxidation by using heated oxygen gas to form metal oxide films, resulting in capacitors with low leakage current and maintained conductivity.

JP7588487B2Active Publication Date: 2024-11-22TOKYO ELECTRON LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020159694
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-24
Publication Date
2024-11-22
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing film forming methods using ozone gas to create titanium oxide films on zirconium oxide films lead to oxidation of underlying conductive films, resulting in decreased conductivity and capacitance in capacitors.

Method used

A film forming method involving three steps: forming a dielectric film, a metal oxide film using organic metal compound vapor and heated oxygen gas, and a second conductive film, which avoids oxidation of the underlying conductive film by using heated oxygen gas instead of ozone.

Benefits of technology

The method results in capacitors with significantly reduced leakage current, maintaining conductivity and functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588487000001
    Figure 0007588487000001
  • Figure 0007588487000002
    Figure 0007588487000002
  • Figure 0007588487000003
    Figure 0007588487000003
Patent Text Reader

Abstract

To manufacture a capacitor with a low leakage current.SOLUTION: A deposition method includes a first film formation step, a second film formation step, and a third film formation step. In the first film formation step, a dielectric film is formed on a first conductive film. In the second film formation step, a metal oxide film is formed on the dielectric film. Further, in the second film formation step, a metal oxide film is formed by using the vapor of an organic metal compound and the heated oxygen gas. In the third film formation step, a second conductive film is formed on the metal oxide film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Various aspects and embodiments of the present disclosure relate to a film formation method. [Background technology]

[0002] For example, the following Patent Document 1 discloses a capacitor having a structure in which a zirconium oxide film and a titanium oxide film are sandwiched between electrodes made of titanium nitride. In the following Patent Document 1, TTIP (titanium tetraisopropoxide: Ti(OCHMe 2 ) 4 ), and a titanium oxide film is formed on the zirconium oxide film by ALD (Atomic Layer Deposition) using ozone gas as an oxidizing gas. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-80094 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a film formation method capable of manufacturing a capacitor with a small leakage current. [Means for solving the problem]

[0005] One aspect of the present disclosure is a film formation method including a first film formation step, a second film formation step, and a third film formation step. In the first film formation step, a dielectric film is formed on a first conductive film. In the second film formation step, a metal oxide film is formed on the dielectric film. In addition, in the second film formation step, a metal oxide film is formed using vapor of an organometallic compound and heated oxygen gas. In the third film formation step, a second conductive film is formed on the metal oxide film. Effect of the Invention

[0006] According to various aspects and embodiments of the present disclosure, a capacitor with low leakage current can be manufactured. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a flowchart illustrating an example of a film forming method according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating an example of a film forming apparatus according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a manufacturing process of a capacitor. [Figure 4] FIG. 4 is a schematic diagram showing an example of a manufacturing process of a capacitor. [Diagram 5] FIG. 5 is a schematic diagram showing an example of a manufacturing process for a capacitor. [Figure 6] FIG. 6 is a schematic diagram showing an example of a manufacturing process for a capacitor. [Figure 7] FIG. 7 is a diagram showing an example of the relationship between the temperature of the oxygen gas and the thickness of the metal oxide film. [Figure 8] FIG. 8 is a diagram showing an example of the relationship between the thickness of a metal oxide film and the leakage current. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the disclosed film forming method will be described in detail with reference to the drawings. Note that the disclosed film forming method is not limited to the following embodiment.

[0009] However, ozone gas used when forming a metal oxide film such as a titanium oxide film on a dielectric film such as a zirconium oxide film has a strong oxidizing power, and therefore the zirconium oxide film and the conductive film below the zirconium oxide film are also oxidized. When the conductive film below the zirconium oxide film is oxidized, the conductivity of the conductive film decreases, and the capacitance as a capacitor decreases or the function as a capacitor may be lost.

[0010] Therefore, the present disclosure provides a technique that can manufacture a capacitor with a small leakage current.

[0011] [Film forming method and film forming apparatus] Fig. 1 is a flowchart showing an example of a film forming method according to an embodiment of the present disclosure. The process illustrated in the flowchart of Fig. 1 is executed by, for example, a film forming apparatus 100 shown in Fig. 2. Fig. 2 is a schematic cross-sectional view showing an example of the film forming apparatus 100 according to an embodiment of the present disclosure.

[0012] The film forming apparatus 100 in this embodiment has a processing vessel 1 formed into a cylindrical or box shape, for example, from aluminum or the like. A mounting table 3 on which a substrate W is placed is provided inside the processing vessel 1. The mounting table 3 is made of a carbon material, such as a graphite plate or a graphite plate covered with silicon carbide, or ceramics having good thermal conductivity, such as aluminum nitride.

[0013] A cover member 13 made of, for example, aluminum or the like and formed in a substantially cylindrical shape to cover the mounting table 3 is provided on the outer periphery of the mounting table 3. A bent portion 14 bent horizontally into, for example, an L-shape is formed on the upper end of the cover member 13. The space surrounded by the mounting table 3 and the cover member 13 constitutes a purge chamber 15. The upper surface of the bent portion 14 is substantially on the same plane as the upper surface of the mounting table 3 and is spaced from the outer periphery of the mounting table 3. A connecting rod 12 is inserted into the gap between the mounting table 3 and the bent portion 14. The mounting table 3 is supported by three support arms 4 extending from the upper inner wall of the cover member 13. Two of the three support arms 4 are shown in FIG. 2.

[0014] A plurality of (e.g., three) L-shaped lifter pins 5 are provided below the mounting table 3 so as to protrude upward from a ring-shaped support member 6. Two of the three lifter pins 5 are shown in Fig. 2. The support member 6 can be raised and lowered by a lifting rod 7 provided to penetrate from the bottom of the processing vessel 1. The lifting rod 7 is driven up and down by an actuator 10 provided below the processing vessel 1.

[0015] Holes 8 penetrating the mounting table 3 are provided in portions of the mounting table 3 corresponding to the lifter pins 5. An actuator 10 raises the lifter pins 5 via the lifting rod 7 and the support member 6, thereby allowing the lifter pins 5 to pass through the holes 8 and lift the substrate W. The portion of the lifting rod 7 inserted into the processing vessel 1 is covered with a bellows 9 to prevent outside air from entering the processing vessel 1 through the portion of the lifting rod 7 inserted into the processing vessel 1.

[0016] A generally ring-shaped clamp ring 11 is provided on the periphery of the mounting table 3 to conform to the contour of the substrate W in order to hold the periphery of the substrate W and fix the substrate W to the mounting table 3. The clamp ring 11 is made of ceramics such as aluminum nitride. The clamp ring 11 is connected to the support member 6 via a connecting rod 12, and is adapted to rise and fall integrally with the lifter pins 5. The lifter pins 5, connecting rod 12, etc. are made of ceramics such as alumina.

[0017] A plurality of contact protrusions 16 are formed on the lower surface of the inner circumference side of the ring-shaped clamp ring 11 and are arranged at approximately equal intervals along the circumferential direction. When clamping the substrate W, the lower end surfaces of the contact protrusions 16 come into contact with the upper surface of the peripheral portion of the substrate W and press the substrate W, thereby clamping the substrate W. Gaps 17 between adjacent contact protrusions 16 communicate with a purge chamber 15 below the mounting table 3.

[0018] A gap 18 between the outer peripheral edge of the clamp ring 11 and the bent portion 14 of the cover member 13 communicates with the purge chamber 15. gas flows into the processing space through gaps 17 between adjacent contact protrusions 16 of the clamp ring 11 and through gaps 18 between the clamp ring 11 and the bent portion 14 .

[0019] A gas supply unit 19 is provided at the bottom of the processing vessel 1 to supply an inert gas into the purge chamber 15. The gas supply unit 19 includes a nozzle 20, a gas supply source 21, a pipe 22, an MFC (Mass Flow Controller) 23, a valve 24, and a valve 25. The nozzle 20 supplies an inert gas, such as argon gas, into the purge chamber 15. The gas supply source 21 is a supply source of an inert gas, such as argon gas. The pipe 22 guides the inert gas from the gas supply source 21 to the nozzle 20. The pipe 22 is provided with the MFC 23 as a flow rate controller, the valve 24, and the valve 25. As the inert gas, other rare gases, such as nitrogen gas and helium gas, may be used instead of argon gas.

[0020] A transmission window 30 made of quartz or the like is provided airtightly at a position directly below the mounting table 3 at the bottom of the processing vessel 1. A box-shaped heating chamber 31 is provided below the transmission window 30 so as to surround the transmission window 30. In the heating chamber 31, a plurality of lamps 32 are attached to a rotation table 33 that also serves as a reflecting mirror. The rotation table 33 is rotated by a motor 34 provided at the bottom of the heating chamber 31. As a result, heat rays emitted from the lamps 32 pass through the transmission window 30 and are irradiated onto the lower surface of the mounting table 3, thereby heating the mounting table 3.

[0021] Further, an exhaust port 36 is provided on the periphery of the bottom of the processing vessel 1, and an exhaust pipe 37 is connected to the exhaust port 36. An exhaust device such as a vacuum pump (not shown) is connected to the exhaust pipe 37. By exhausting gas inside the processing vessel 1 through the exhaust port 36 and the exhaust pipe 37, the inside of the processing vessel 1 can be maintained at a predetermined vacuum level. Further, an opening 39 is formed in the sidewall of the processing vessel 1 for loading and unloading the substrate W. The opening 39 is opened and closed by a gate valve 38.

[0022] A shower head 40 is provided on the ceiling of the processing vessel 1 facing the mounting table 3 to introduce gas into the processing vessel 1. The shower head 40 is made of, for example, aluminum, and has a body 41 having an internal space 41a. A gas inlet 42 is provided on the ceiling of the body 41. A gas supply unit 50 that supplies gas used in the film formation process is connected to the gas inlet 42 via a pipe 51.

[0023] A number of gas holes 43 are arranged over the entire bottom of the main body 41 to discharge the gas supplied into the main body 41 into the processing space in the processing vessel 1, so that the gas can be discharged over the entire surface of the substrate W. A diffusion plate 44 having a number of through holes 45 formed therein is provided in the space 41a of the main body 41, so that the gas can be supplied more evenly to the surface of the substrate W. Furthermore, heaters 46 and 47 for adjusting temperature are provided in the sidewall of the processing vessel 1 and in the sidewall of the shower head 40. The heaters 46 and 47 make it possible to maintain the wall surface in contact with the gas supplied into the processing vessel 1 at a predetermined temperature.

[0024] The gas supply unit 50 includes a storage unit 53, a storage unit 54, a gas supply source 55, and a gas supply source 56. The storage unit 53 stores a nickel (Ni) raw material. In this embodiment, the nickel raw material is, for example, (EtCp) 2 Ni (Bis(ethylcyclopentadienyl)nickel). (EtCp) 2 Ni includes nickel, a transition metal. Also, (EtCp) 2 Ni contains a cyclopentadienyl group (EtCp). 2 Ni is an example of an organometallic compound. The storage unit 54 stores a zirconium (Zr) raw material. In this embodiment, the zirconium raw material is, for example, TEMAZ (tetrakisethylmethylaminozirconium). The gas supply source 55 is a supply source of an inert gas such as argon gas used for diluting the gas supplied into the processing vessel 1. The gas supply source 56 is a supply source of oxygen gas for oxidizing the metal.

[0025] Gas supply source 55 is connected to pipe 51 via valve 62, MFC 61, and valve 63. In addition, reservoir 53 is connected to pipe 51 via pipe 58. In addition, reservoir 54 is connected to pipe 51 via pipe 59. In addition, gas supply source 56 is connected to pipe 51 via pipe 60. Pipe 60 is provided with MFC 82, valve 83, valve 84, and heating unit 88. Heating unit 88 heats the oxygen gas supplied from gas supply source 56 to a temperature in the range of, for example, 150°C to 350°C.

[0026] Furthermore, a pipe 68 is provided between the pipe 51 and the pipe 60 between the MFC 82 and the heating unit 88. A valve 65, an ozonizer 66, and a valve 67 are provided in the pipe 68. The ozonizer 66 generates ozone gas from oxygen gas supplied from the gas supply source 56. The ozone gas generated by the ozonizer 66 is supplied into the processing vessel 1 via the valve 67 and the pipe 51.

[0027] A carrier gas supply source 69 that supplies a carrier gas such as argon gas is connected to storage unit 53 via piping 70. Pipe 70 is provided with an MFC 71, a valve 72, and a valve 73. A carrier gas supply source 74 that supplies a carrier gas via piping 75 is connected to storage unit 54. Pipe 75 is provided with an MFC 76, a valve 77, and a valve 78.

[0028] Storage unit 53 is provided with a heater 80, and the nickel raw material stored in storage unit 53 is supplied to processing vessel 1 by bubbling while being heated by heater 80. Storage unit 54 is provided with a heater 81, and the zirconium raw material stored in storage unit 54 is supplied to processing vessel 1 by bubbling while being heated by heater 81. Note that piping, MFC, valves, etc. through which the vaporized nickel raw material and zirconium raw material flow are also heated by heaters (not shown).

[0029] In addition, in this embodiment, the nickel raw material and the zirconium raw material are vaporized by bubbling and then the flow rates are controlled by the MFC, but the disclosed technology is not limited to this. For example, the nickel raw material and the zirconium raw material may be in a liquid state and the flow rates of the nickel raw material and the zirconium raw material may be vaporized by bubbling and supplied into the processing vessel 1. In addition, in this embodiment, the nickel raw material, the zirconium raw material, and the oxygen gas are supplied into the processing vessel 1 through the pipe 51, but the disclosed technology is not limited to this. For example, the nickel raw material, the zirconium raw material, and the oxygen gas may be supplied into the processing vessel 1 through separate pipes.

[0030] The upper side wall of the processing vessel 1 is provided with NF 3 Gas and ClF 3 A gas inlet 85 is provided for introducing a cleaning gas such as a gas. A pipe 86 for supplying a cleaning gas is connected to the gas inlet 85. A remote plasma generator 87 is provided to the pipe 86. The cleaning gas supplied via the pipe 86 is converted into plasma by the remote plasma generator 87, and the plasma of the cleaning gas is supplied into the processing vessel 1 via the gas inlet 85. This cleans the inside of the processing vessel 1. Alternatively, the gas inlet 85 may be connected to the pipe 51, and the plasma of the cleaning gas may be supplied into the processing vessel 1 via the shower head 40. As the cleaning gas, NF 3 Gas and ClF 3 In addition to gas, F 2 A gas such as ClF can also be used as a cleaning gas. 3 When a gas is used, plasma-less thermal cleaning may be performed without using remote plasma.

[0031] The film forming apparatus 100 has a process controller 90 having a microprocessor or the like, and each component of the film forming apparatus 100 is controlled by the process controller 90. A user interface 91 including a keyboard for an operator to input commands for managing each component of the film forming apparatus 100 and a display for visualizing and displaying the operating status of each component of the film forming apparatus 100 is connected to the process controller 90. In addition, a storage unit 92 is connected to the process controller 90, which stores control programs, process recipes, etc. for implementing various processes executed in the film forming apparatus 100 under the control of the process controller 90.

[0032] The process controller 90 reads out a process recipe and the like stored in advance in a storage unit 92 in response to an instruction and the like inputted via a user interface 91. Then, the process controller 90 controls each unit of the film forming apparatus 100 in response to the read out process recipe and the like, thereby causing the film forming apparatus 100 to execute a predetermined process.

[0033] Returning to FIG. 1, the description will be continued. First, the gate valve 38 is opened, and a substrate W having a first conductive film 200, for example, as shown in FIG. 3, is carried into the processing chamber 1 and placed on the mounting table 3. In this embodiment, the first conductive film 200 is, for example, titanium nitride. The first conductive film 200 may be tungsten, tungsten nitride, tantalum nitride, vanadium nitride, metal ruthenium, or the like. Then, the gate valve 38 is closed. Then, vapor of a zirconium raw material used to form a zirconium oxide film is supplied into the processing chamber 1 (S10).

[0034] In step S10, valves 77 and 78 are opened, and carrier gas at a flow rate determined in advance by MFC 76 is supplied into reservoir 54. As a result, the zirconium source material is vaporized, and the vapor of the zirconium source material at a flow rate corresponding to the carrier gas whose flow rate is controlled by MFC 76 is supplied into processing chamber 1 via pipe 51. As a result, molecules of the zirconium source material are adsorbed onto the surface of first conductive film 200. Then, valves 77 and 78 are closed.

[0035] The main conditions of step S10 are as follows: Pressure in processing vessel 1: 1 Torr Temperature of substrate W: 250°C Processing time: 5 seconds

[0036] Next, the surface of the substrate W is purged (S11). In step S11, the valves 62 and 63 are opened, and an inert gas at a predetermined flow rate is supplied into the processing chamber 1 through the pipe 51 by the MFC 61. This removes excess molecules of the zirconium source material adsorbed on the surface of the first conductive film 200. Then, the valves 62 and 63 are closed.

[0037] The main conditions of step S11 are as follows. Pressure in processing vessel 1: 1 Torr Temperature of substrate W: 250°C Inert gas flow rate: 500sccm Processing time: 10 seconds

[0038] Next, an oxidizing gas is supplied to the surface of the substrate W (S12). In step S12, the valves 83, 65, and 67 are opened, and oxygen gas is supplied to the ozonizer 66 at a flow rate determined in advance by the MFC 82. The ozonizer 66 generates ozone gas from the supplied oxygen gas, and supplies the generated ozone gas into the processing chamber 1 via the pipe 51. As a result, the molecules of the zirconium raw material adsorbed on the surface of the first conductive film 200 are oxidized, and a zirconium oxide film is formed on the surface of the first conductive film 200. Then, the valves 83, 65, and 67 are closed.

[0039] The main conditions of step S12 are as follows: Pressure in processing vessel 1: 1 Torr Temperature of substrate W: 250°C Oxygen gas flow rate: 500sccm Ozone gas concentration: 100g / m 3 Processing time: 10 seconds

[0040] Next, the surface of the substrate W is purged again (S13). In step S13, the valves 62 and 63 are opened, and an inert gas at a predetermined flow rate is supplied into the processing chamber 1 via the pipe 51 by the MFC 61. This removes the excess zirconium oxide film deposited on the surface of the first conductive film 200. Then, the valves 62 and 63 are closed. The main conditions of step S13 are similar to the main conditions of step S11.

[0041] Next, it is determined whether steps S10 to S13 have been performed a predetermined number of times (S14). The predetermined number of times in step S14 refers to the number of times a zirconium oxide film with a predetermined thickness is formed on the first conductive film 200. If steps S10 to S13 have not been performed the predetermined number of times (S14: No), the process shown in step S10 is performed again. The processes of steps S10 to S14 are an example of a first film forming process.

[0042] On the other hand, if steps S10 to S13 have been performed a predetermined number of times (S14: Yes), a dielectric film 201 having a predetermined thickness is formed on the first conductive film 200, as shown in Fig. 4 for example. In this embodiment, the dielectric film 201 is, for example, a zirconium oxide film. Then, vapor of a nickel raw material used to form a nickel oxide film is supplied into the processing vessel 1 (S15).

[0043] In step S15, valves 72 and 73 are opened, and carrier gas at a flow rate determined in advance by MFC 71 is supplied into reservoir 53. As a result, the nickel raw material is vaporized, and the vapor of the nickel raw material at a flow rate corresponding to the carrier gas whose flow rate is controlled by MFC 71 is supplied into processing vessel 1 via pipe 51. As a result, molecules of the nickel raw material are adsorbed onto the surface of dielectric film 201. Step S15 is an example of an adsorption process. Then, valves 72 and 73 are closed.

[0044] The main conditions of step S15 are as follows. Pressure in processing vessel 1: 5 Torr Temperature of substrate W: 245℃ Processing time: 30 seconds

[0045] Next, the surface of the substrate W is purged (S16). In step S16, the valves 62 and 63 are opened, and an inert gas at a predetermined flow rate is supplied into the processing chamber 1 via the pipe 51 by the MFC 61. This removes excess molecules of the nickel raw material adsorbed on the surface of the dielectric film 201. Step S16 is an example of a first purging step. Then, the valves 62 and 63 are closed.

[0046] The main conditions in step S16 are as follows: Pressure in processing vessel 1: 5 Torr Temperature of substrate W: 245℃ Inert gas flow rate: 500sccm Processing time: 30 seconds

[0047] Next, an oxidation gas is supplied to the surface of the substrate W (S17). In step S17, the valves 83 and 84 are opened, and oxygen gas at a predetermined flow rate is supplied to the heating unit 88 by the MFC 82. The oxygen gas supplied to the heating unit 88 is heated to a predetermined temperature by the heating unit 88. The heated oxygen gas is then supplied into the processing vessel 1 via the pipes 60 and 51. As a result, the molecules of the nickel raw material adsorbed on the surface of the dielectric film 201 are oxidized, and a nickel oxide film is formed on the surface of the dielectric film 201. Step S17 is an example of a reaction process. Then, the valves 83 and 84 are closed.

[0048] The main conditions of step S17 are as follows. Pressure in processing vessel 1: 5 Torr Temperature of substrate W: 245℃ Oxygen gas flow rate: 500sccm Oxygen gas temperature: 150℃~350℃ Processing time: 60 seconds

[0049] If the molecules of the nickel raw material adsorbed on the surface of the dielectric film 201 are oxidized using ozone gas, the ozone gas has a stronger oxidizing power than oxygen gas, and may therefore also oxidize the first conductive film 200 below the dielectric film 201. If the first conductive film 200 is oxidized, the conductivity of the first conductive film 200 may decrease, and the capacitance of the capacitor may decrease or the capacitor may lose its function.

[0050] In contrast to this, in this embodiment, in step S17, heated oxygen gas, rather than ozone gas, is used to oxidize the molecules of the nickel raw material adsorbed on the surface of the dielectric film 201. This makes it possible to oxidize the molecules of the nickel raw material adsorbed on the surface of the dielectric film 201 without oxidizing the first conductive film 200 below the dielectric film 201. Note that by heating the oxygen gas, the oxidizing power can be increased, and the molecules of the nickel raw material adsorbed on the surface of the dielectric film 201 can be oxidized in a shorter time.

[0051] In addition, ozone gas is used in step S12 in forming the dielectric film 201, but since the processing time of step S12 is short, the first conductive film 200 is hardly oxidized.

[0052] Next, the surface of the substrate W is purged again (S18). In step S18, the valves 62 and 63 are opened, and an inert gas at a predetermined flow rate is supplied into the processing chamber 1 via the pipe 51 by the MFC 61. This removes the nickel oxide film that is excessively deposited on the surface of the dielectric film 201. Step S18 is an example of a second purging process. Then, the valves 62 and 63 are closed. The main conditions of step S18 are similar to the main conditions of step S16.

[0053] Next, it is determined whether steps S15 to S18 have been performed a predetermined number of times (S19). If steps S15 to S18 have not been performed a predetermined number of times (S19: No), the process shown in step S15 is executed again. The processes of steps S15 to S19 are an example of a second film forming process.

[0054] On the other hand, if steps S15 to S18 have been performed the predetermined number of times (S19: Yes), a metal oxide film 202 having a predetermined thickness is formed on the dielectric film 201, as shown in Fig. 5 for example. In this embodiment, the metal oxide film 202 is, for example, a nickel oxide film. Then, the gate valve 38 is opened, and the substrate W is unloaded from the processing chamber 1.

[0055] Next, the substrate W is carried into a film forming apparatus (not shown) for forming a conductive film, and a second conductive film 203 is formed on the metal oxide film 202 (S20), for example, as shown in FIG. 6. Step S20 is an example of a third film forming process. In this embodiment, the second conductive film 203 is, for example, titanium nitride. The second conductive film 203 may be tungsten, tungsten nitride, tantalum nitride, vanadium nitride, metal ruthenium, or the like. Then, the film forming method shown in this flowchart is completed.

[0056] [Deposition rate] Fig. 7 is a diagram showing an example of the relationship between the temperature of oxygen gas and the thickness of a metal oxide film. The horizontal axis of Fig. 7 indicates the number of repetitions (cycles) of the processes of steps S15 to S18 in Fig. 1, and the vertical axis indicates the thickness of the metal oxide film 202. For example, as shown in Fig. 7, the metal oxide film 202 can be formed even using oxygen gas by heating the oxygen gas to 120°C or higher.

[0057] However, when the temperature of the oxygen gas is 120° C., even if the processes of steps S15 to S18 are repeated 200 cycles, the metal oxide film 202 is only formed to a thickness of 4 Å. Therefore, from the viewpoint of improving the throughput in forming the metal oxide film 202, it is preferable to heat the oxygen gas to a temperature of 150° C. or higher.

[0058] 7, the higher the temperature of the oxygen gas, the higher the deposition rate of the metal oxide film 202. However, the nickel raw material decomposes at temperatures higher than 350°C, and is less likely to be adsorbed onto the surface of the dielectric film 201. As a result, when the oxygen gas is heated to a temperature higher than 350°C, the deposition rate of the metal oxide film 202 decreases. Therefore, it is preferable to heat the oxygen gas to a temperature within the range of 150°C or higher and 350°C or lower.

[0059] [Leakage current] Fig. 8 is a diagram showing an example of the relationship between the film thickness of the metal oxide film 202 and the leakage current. Fig. 8 shows the value of the leakage current of a capacitor in which the metal oxide film 202 is formed using oxygen gas heated to 150°C by the film forming method of this embodiment. Fig. 8 also shows, as a comparative example, the value of the leakage current of a capacitor in which only the dielectric film 201 is laminated between the first conductive film 200 and the second conductive film 203 and which does not have the metal oxide film 202 (NiO layer). Fig. 8 also shows, as a comparative example, the value of the leakage current of a capacitor in which the metal oxide film 202 is formed using ozone gas.

[0060] 8, the leakage current value of the capacitor formed by the film forming method of this embodiment is lower than the leakage current value of the capacitor not having the metal oxide film 202. Also, the leakage current value of the capacitor formed by the film forming method of this embodiment is about two orders of magnitude lower than the leakage current value of the capacitor having the metal oxide film 202 formed by using ozone gas. Therefore, by forming the metal oxide film 202 between the dielectric film 201 and the second conductive film 203 by using heated oxygen gas, the leakage current of the capacitor can be suppressed.

[0061] The embodiment has been described above. As described above, the film formation method in the present embodiment includes a first film formation process, a second film formation process, and a third film formation process. In the first film formation process, a dielectric film 201 is formed on a first conductive film 200. In the second film formation process, a metal oxide film 202 is formed on the dielectric film 201. In the second film formation process, the metal oxide film 202 is formed using vapor of an organometallic compound and heated oxygen gas. In the third film formation process, a second conductive film 203 is formed on the metal oxide film 202. This makes it possible to manufacture a capacitor with a small leakage current.

[0062] Moreover, the second film forming process in the above embodiment includes an adsorption process, a first purge process, a reaction process, and a second purge process. In the adsorption process, the vapor of the organometallic compound is supplied to the surface of the dielectric film 201, so that the molecules of the organometallic compound are adsorbed on the surface of the dielectric film 201. In the first purge process, the surface of the dielectric film 201 on which the molecules of the organometallic compound are adsorbed is purged with an inert gas. In the reaction process, the molecules of the organometallic compound adsorbed on the surface of the dielectric film 201 are oxidized by supplying heated oxygen gas to the surface of the dielectric film 201 on which the molecules of the organometallic compound are adsorbed. In the second purge process, the surface of the dielectric film 201 on which the molecules of the organometallic compound are oxidized is purged with an inert gas. This allows the metal oxide film 202 to be formed on the dielectric film 201.

[0063] In the second film formation step in the above embodiment, the oxygen gas is heated to a temperature in the range of 150° C. to 350° C. This makes it possible to oxidize the molecules of the organometallic compound adsorbed on the surface of the dielectric film 201 without oxidizing the first conductive film 200 below the dielectric film 201.

[0064] In the above embodiment, the organometallic compound contains a cyclopentadienyl group. Although organometallic compounds containing a cyclopentadienyl group are generally difficult to decompose, the decomposition can be promoted by heating the oxygen gas used for oxidation, so that the metal oxide film 202 can be sufficiently oxidized.

[0065] In the above-described embodiment, the first conductive film 200 and the second conductive film 203 are made of titanium nitride, tungsten, tungsten nitride, tantalum nitride, vanadium nitride, or metal ruthenium, thereby making it possible to manufacture a capacitor with a small leakage current.

[0066] [others] It should be noted that the technology disclosed in the present application is not limited to the above-described embodiment, and various modifications are possible within the scope of the gist thereof.

[0067] For example, in the embodiment described above, the organometallic compound supplied in step S15 contains nickel as a transition metal, but the disclosed technology is not limited to this. The organometallic compound supplied in step S15 may contain other transition metals, such as cobalt, manganese, or iridium.

[0068] In the above embodiment, in step S15, the organometallic compound is (EtCp) 2 Ni vapor is supplied, but the disclosed technology is not limited to this. In step S15, for example, (EtCp) 2 Vapor of other organometallic compounds having functional groups that are difficult to decompose, such as cyclopentadienyl groups, may also be supplied, such as Co vapor.

[0069] In the above embodiment, the dielectric film 201 is a zirconium oxide film, but the disclosed technology is not limited to this. For example, the dielectric film 201 may be an oxide film containing at least one of zirconium, hafnium, aluminum, and titanium. The dielectric film 201 may be a multilayer film containing at least one layer of zirconium oxide, hafnium oxide, aluminum oxide, and titanium oxide.

[0070] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be construed as limiting. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0071] W substrate 100 Film deposition equipment 40 Shower Head 50 Gas supply section 51 Piping 53 Storage section 54 Storage section 55 Gas supply source 56 Gas supply source 58 Piping 59 Piping 60 Piping 61 MFC 62 Valve 63 Valve 65 Valve 66 Ozonizer 67 Valve 68 Piping 69 Carrier Gas Supply Source 70 Piping 71 M.F.C. 72 Valve 73 Valve 74 Carrier gas supply source 75 Piping 76 MFC 77 Valve 78 Valve 80 Heater 81 Heater 82 MFC 83 Valve 84 Valve 85 Gas inlet 86 Piping 87 Remote Plasma Generator 88 Heating section 200 First conductive film 201 Dielectric film 202 Metal oxide film 203 Second conductive film

Claims

1. a first film formation step of forming a dielectric film on the first conductive film; a second deposition step of depositing a metal oxide film on the dielectric film; a third film formation step of forming a second conductive film on the metal oxide film; Including, In the second film forming step, The film forming method includes forming the metal oxide film by using vapor of an organometallic compound containing a cyclopentadienyl group and heated oxygen gas.

2. The second film formation step includes: an adsorption step of adsorbing molecules of the organometallic compound on the surface of the dielectric film by supplying vapor of the organometallic compound to the surface of the dielectric film; a first purging step of purging the surface of the dielectric film on which the molecules of the organometallic compound are adsorbed with an inert gas; a reaction step of supplying heated oxygen gas to the surface of the dielectric film on which the molecules of the organometallic compound are adsorbed, thereby oxidizing the molecules of the organometallic compound adsorbed on the surface of the dielectric film; a second purge step of purging the surface of the dielectric film where the molecules of the organometallic compound have been oxidized with an inert gas; The method of forming a film according to claim 1 , further comprising:

3. In the second film forming step, 3. The film forming method according to claim 1, wherein the oxygen gas is heated to a temperature in the range of 150° C. to 350° C.

4. The film forming method according to claim 1 , wherein the organometallic compound contains a transition metal.

5. 5. The film forming method according to claim 4, wherein the transition metal is nickel.

6. 6. The film forming method according to claim 1, wherein the dielectric film is an oxide film containing at least one of zirconium, hafnium, aluminum, and titanium.

7. 7. The film forming method according to claim 6, wherein the dielectric film is a multi-layer film including at least one layer of zirconium oxide, hafnium oxide, aluminum oxide, and titanium oxide.

8. 8. The film forming method according to claim 1, wherein the first conductive film and the second conductive film are made of titanium nitride, tungsten, tungsten nitride, tantalum nitride, vanadium nitride, or metallic ruthenium.

Citation Information

Patent Citations

  • Atomic layer deposition onto fibrous materials

    JP2010510392A

  • Liquid composition containing aminoether for developing metal-containing film

    JP2011080144A

  • Semiconductor memory device and method for manufacturing the same

    JP2012080094A

  • Method for manufacturing semiconductor device

    WO2020066819A1

  • Film-forming method, film-forming apparatus, and oxidation method

    WO2020158079A1