Communication equipment housing
A polycarbonate resin composition with controlled structural units and molecular weight addresses high dielectric loss and appearance defects in communication equipment housings, providing enhanced radio wave transparency and aesthetics for devices with built-in antennas.
Patent Information
- Application Number
- JP2020176184
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-20
AI Technical Summary
Existing communication equipment housings with built-in microwave and/or millimeter wave antennas suffer from high dielectric loss tangents and appearance defects due to shear heat generation during molding, particularly in thin-walled products made from polycarbonate resins with poor thermal stability.
A polycarbonate resin composition is developed with specific structural units, terminal hydroxyl group content, and viscosity average molecular weight ranges, incorporating compounds like 2,2-bis(4-hydroxy-3-methylphenyl)propane and 2-(4-hydroxyphenyl)-2-(3-methyl-4-hydroxyphenyl)propane, ensuring low dielectric loss tangent and minimal appearance defects.
The solution results in a thin-walled communication equipment casing with improved radio wave transparency, low dielectric loss tangent, and excellent appearance, suitable for devices like notebook computers, smartphones, and router devices, while maintaining mechanical strength and design aesthetics.
Smart Images

Figure 0007589494000001 
Figure 0007589494000002 
Figure 0007589494000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a housing for a communication device having a built-in microwave and / or millimeter wave antenna, in particular to a thin-walled housing for a communication device having a low dielectric tangent and little appearance defect. The present invention also relates to a polycarbonate resin composition from which such a housing for a communication device can be obtained, and a molded article thereof. [Background technology]
[0002] In high-frequency communication devices, there is a demand for materials with low dielectric properties to reduce transmission loss in wiring and housings and to improve signal propagation speed. In addition, there is a demand for materials with low dielectric properties in various fields, such as devices using so-called millimeter-wave radar for obstacle detection in automobiles.
[0003] Patent Document 1 proposes a cover made of a polycarbonate resin material with excellent millimeter wave transparency. However, the polycarbonate resin having the specific structure disclosed therein has relatively poor thermal stability, and there is a problem that when obtaining a thin molded body, the molded body has a poor appearance (black foreign matter) due to shear heat generated during molding. In addition, there is a demand for a further reduction in the dielectric loss tangent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-197048 A Summary of the Invention [Problem to be solved by the invention]
[0005] Under these circumstances, an object of the present invention is to provide a housing for a communication device having a built-in microwave and / or millimeter wave antenna, which is a thin-walled housing for a communication device having a lower dielectric tangent and almost no appearance defects. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that the above problems can be solved by using a polycarbonate resin containing a carbonate structural unit derived from a specific aromatic dihydroxy compound, in which the amount of terminal hydroxyl groups and viscosity average molecular weight are controlled within specific ranges, thereby completing the present invention.
[0007] That is, the gist of the present invention lies in the following [1] to [8].
[0008] [1] A housing for a communications device having a built-in microwave and / or millimeter wave antenna, obtained using a polycarbonate resin composition, the polycarbonate resin composition containing a polycarbonate resin having at least a structural unit represented by the following formula (1), an alkaline hydrolyzate obtained by alkaline hydrolysis of the polycarbonate resin contains a compound represented by the following formula (2) and a compound represented by the following formula (3), the amount of the compound represented by the following formula (3) in the alkaline hydrolyzate being 1,500 ppm by mass or more and 6,000 ppm by mass or less relative to the amount of the compound represented by the following formula (2) in the alkaline hydrolyzate, the amount of terminal hydroxyl groups in the polycarbonate resin being 200 ppm by mass or more and 400 ppm by mass or less, and the viscosity average molecular weight of the polycarbonate resin being 21,000 or more and 25,500 or less.
[0009] [ka]
[0010] (In formula (1), formula (2) and formula (3), R 1 , R 2 and R 3 each independently represents a substituted or unsubstituted alkyl group having from 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group, and X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom.
[0011] [2] A housing for a communications device according to [1], having a thickness of 1.5 mm or less.
[0012] [3] The housing for a communication device according to [1] or [2], wherein the structural unit represented by formula (1) is a structural unit represented by the following formula (1-1), the compound represented by formula (2) is a compound represented by the following formula (2-1), and the compound represented by formula (3) is a compound represented by the following formula (3-1).
[0013] [ka]
[0014] [4] The housing for a communication device according to any one of [1] to [3], wherein the antenna is used for radio waves in a frequency band of 3.5 to 30 GHz.
[0015] [5] The housing for a communications device according to any one of [1] to [4], wherein the communications device is a notebook computer, a tablet terminal, a smartphone, or a router device.
[0016] [6] A communication device having a built-in microwave and / or millimeter wave antenna, obtained by using the housing for the communication device according to any one of [1] to [5].
[0017] [7] A polycarbonate resin composition comprising a polycarbonate resin having at least a structural unit represented by the following formula (1), wherein an alkaline hydrolyzate obtained by alkaline hydrolysis of the polycarbonate resin contains a compound represented by the following formula (2) and a compound represented by the following formula (3), the amount of the compound represented by the following formula (3) in the alkaline hydrolyzate being 1,500 ppm by mass or more and 6,000 ppm by mass or less relative to the amount of the compound represented by the following formula (2) in the alkaline hydrolyzate, the amount of terminal hydroxyl groups in the polycarbonate resin being 200 ppm by mass or more and 400 ppm by mass or less, and the viscosity average molecular weight of the polycarbonate resin being 21,000 or more and 25,500 or less.
[0018] [ka]
[0019] (In formula (1), formula (2) and formula (3), R 1 , R 2 and R 3 each independently represents a substituted or unsubstituted alkyl group having from 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group, and X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom.
[0020] [8] A molded article obtained using the polycarbonate resin composition according to [7]. Effect of the Invention
[0021] The housing for a communication device having a built-in microwave and / or millimeter wave antenna of the present invention is a thin-walled housing for a communication device that has a lower dielectric tangent and almost no appearance defects, and has excellent radio wave transmittance in the microwave and / or millimeter wave bands, as well as being thin and providing excellent product appearance. In addition, the polycarbonate resin composition of the present invention has excellent low dielectric properties and thin-wall moldability, and can be widely used as a member of communication devices that require low dielectric properties, specifically, as a housing for communication devices with built-in microwave and / or millimeter wave antennas, such as notebook computers, tablet terminals, smartphones, router devices, etc. Furthermore, it can be used in a wide range of fields such as automobiles, medical and nursing care, railways, and aviation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the present invention will be described in detail with reference to embodiments and examples, but the present invention should not be construed as being limited to the embodiments and examples shown below. In this specification, unless otherwise specified, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0023] [Polycarbonate resin composition] The polycarbonate resin composition of the present invention is a polycarbonate resin composition containing a polycarbonate resin having at least a structural unit represented by the following formula (1) (hereinafter, may be referred to as "structural unit (1)") (hereinafter, may be referred to as "polycarbonate resin of the present invention"). <1> ~ <3> It meets the requirements. <1> The alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin of the present invention contains a compound represented by the following formula (2) (hereinafter may be referred to as "compound (2)") and a compound represented by the following formula (3) (hereinafter may be referred to as "compound (3)"), and the amount of compound (3) in the alkaline hydrolysate is 1500 ppm by mass or more and 6000 ppm by mass or less relative to the amount of compound (2) in the alkaline hydrolysate. <2> The amount of terminal hydroxyl groups is 200 ppm by mass or more and 400 ppm by mass or less. <3> Viscosity average molecular weight is 21,000 or more and 25,500 or less.
[0024] [ka]
[0025] (In formula (1), formula (2) and formula (3), R 1 , R 2 and R 3 each independently represents a substituted or unsubstituted alkyl group having from 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group, and X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom.
[0026] <Polycarbonate resin> First, the polycarbonate resin of the present invention contained in the polycarbonate resin composition of the present invention will be described.
[0027] (Structural unit (1) · Compound (2)) The structural unit (1) is a structural unit that is introduced into a polycarbonate resin by using the compound (2) as a raw dihydroxy compound in the process for producing the polycarbonate resin described below. In the formula (1) representing the structural unit (1) and the formula (2) representing the compound (2), R 1 and R 2 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or a substituted or unsubstituted aryl group.
[0028] R in Equations (1) and (2) 1 and R 2 Examples of the substituted or unsubstituted alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a sec-pentyl group, an n-hexyl group, an n-heptyl group, and an n-octyl group. Examples of the substituted or unsubstituted aryl group include a phenyl group, a benzyl group, a tolyl group, a 4-methylphenyl group, and a naphthyl group.
[0029] Among these, R 1 and R 2 is preferably a methyl group, an ethyl group, an n-propyl group, or a 4-methylphenyl group, and particularly preferably a methyl group.
[0030] In addition, R in formulas (1) and (2) 1 , R 2 The bonding position of is preferably the 3-position relative to X.
[0031] In formulae (1) and (2), X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom. The substituted or unsubstituted alkylidene group is preferably a substituted or unsubstituted alkylidene group having 1 to 20 carbon atoms, and the alkylidene group may be linear, branched, or cyclic. X is preferably a single bond or a substituted or unsubstituted alkylidene group from the viewpoint of thermal stability and heat resistance, and among these, a substituted or unsubstituted alkylidene group having 1 to 12 carbon atoms is more preferable from the viewpoint of fluidity, and particularly preferably a methylidene group, an ethylidene group, or a propylidene group, and particularly preferably a 2,2-propylidene group.
[0032] Specific examples of suitable compounds (2) include 2,2-bis(4-hydroxy-3-methylphenyl)propane (hereinafter sometimes abbreviated as "BPC") represented by the following formula (2-1), 2,2-bis(2-hydroxy-5-biphenylyl)propane represented by the following formula (2-2), 1,1-bis(4-hydroxy-3-methylphenyl)cyclododecane represented by the following formula (2-3), 4,4-ethylidenebis(2-methylphenol) represented by the following formula (2-4), 4,4-(octahydro-4,7-methano-5H-inden-5-ylidene)bis(2-methylphenol) represented by the following formula (2-5), and 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane represented by the following formula (2-6).
[0033] [ka]
[0034] From the viewpoint of thermal stability and fluidity, the structural unit (1) is preferably a structural unit represented by the following formula (1-1), and the compound (2) is preferably a compound represented by the following formula (2-1), i.e., 2,2-bis(4-hydroxy-3-methylphenyl)propane (BPC).
[0035] [ka]
[0036] The polycarbonate resin of the present invention may contain only one type of structural unit (1), or may contain two or more types. Accordingly, the alkaline hydrolyzate obtained by alkaline hydrolysis of the polycarbonate resin of the present invention may contain only one type of compound (2), or may contain two or more types.
[0037] <Compound (3)> In the formula (3) representing the compound (3), R 3 represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or a substituted or unsubstituted aryl group.
[0038] R in Equation (3) 3 Examples of the substituted or unsubstituted alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a sec-pentyl group, an n-hexyl group, an n-heptyl group, and an n-octyl group. Examples of the substituted or unsubstituted aryl group include a phenyl group, a benzyl group, a tolyl group, a 4-methylphenyl group, and a naphthyl group.
[0039] Among these, R 3 is preferably a methyl group, an ethyl group, an n-propyl group, or a 4-methylphenyl group, and particularly preferably a methyl group.
[0040] In addition, R in formula (3) 3 The bonding position of is preferably the 3-position relative to X.
[0041] In formula (3), X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom. The substituted or unsubstituted alkylidene group is preferably a substituted or unsubstituted alkylidene group having 1 to 20 carbon atoms, and the alkylidene group may be linear, branched, or cyclic. X is preferably a single bond or a substituted or unsubstituted alkylidene group from the viewpoint of thermal stability and heat resistance, and among these, a substituted or unsubstituted alkylidene group having 1 to 12 carbon atoms is more preferable from the viewpoint of fluidity, and particularly preferably a methylidene group, an ethylidene group, or a propylidene group, and particularly preferably a 2,2-propylidene group.
[0042] Suitable specific examples of the compound (3) include 2-(4-hydroxyphenyl)-2-(3-methyl-4-hydroxyphenyl)propane (hereinafter, sometimes referred to as "monomethyl BPA") represented by the following formula (3-1), 2-(4-hydroxyphenyl)-2-(3-phenyl-4-hydroxyphenyl)propane represented by the following formula (3-2), 1-(4-hydroxyphenyl)-1-(3-methyl-4-hydroxyphenyl)cyclododecane represented by the following formula (3-3), 1-(4-hydroxyphenyl)-1-(3-methyl-4-hydroxyphenyl)ethane represented by the following formula (3-4), 4-(4-hydroxyphenyl)-4-(3-methyl-4-hydroxyphenyl)(octahydro-4,7-methano-5H-inden-5-ylidene) represented by the following formula (3-5), and 1-(4-hydroxyphenyl)-1-(3-methyl-4-hydroxyphenyl)cyclohexane represented by the following formula (3-6).
[0043] [ka]
[0044] From the viewpoint of thermal stability and fluidity, compound (3) is preferably 2-(4-hydroxyphenyl)-2-(3-methyl-4-hydroxyphenyl)propane (monomethyl BPA) represented by the following formula (3-1).
[0045] [ka]
[0046] The alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin of the present invention may contain only one type of compound (3), or may contain two or more types.
[0047] In addition, R in formula (2) representing compound (2) 1 ,R 2 and R in formula (3) representing compound (3). 3 are not necessarily the same and may be different. In addition, X in formula (2) and X in formula (3) may be the same or different. However, from the viewpoint of thermal stability and fluidity, R in formula (2) 1 ,R 2 At least one of these and R in formula (3) 3 are preferably the same, and X in formula (2) and X in formula (3) are preferably the same.
[0048] <Structural unit of polycarbonate resin> The polycarbonate resin of the present invention containing the structural unit (1) produces the compound (2) upon alkaline hydrolysis. Furthermore, the presence of compound (3) in the alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin of the present invention means that the polycarbonate resin of the present invention has a structural unit derived from compound (3), specifically, a structural unit represented by the following formula (4) (hereinafter, sometimes referred to as "structural unit (4)").
[0049] [ka]
[0050] (In formula (4), R 3 , X has the same meaning as in formula (3).
[0051] That is, the polycarbonate resin of the present invention contains at least one or more types of structural units (1) and one or more types of structural units (4), but the polycarbonate resin of the present invention may contain structural units other than the structural units (1) and (4). The other structural units are not particularly limited, and examples thereof include structural units derived from the dihydroxy compounds listed below.
[0052] Biphenols such as 2,2,6,6-tetramethyl-4,4-biphenol, 4,4-biphenol, 2,5-biphenol, and 2,2-biphenol; dihydroxydiaryl ethers such as 2,2'-dihydroxydiphenyl ether, 3,3'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 1,4-bis(3-hydroxyphenoxy)benzene, and 1,3-bis(4-hydroxyphenoxy)benzene; 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methoxy-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-methoxy-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3,5-dimethylphenyl)methane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)(4-propenylphenyl)methane, bis(4-hydroxyphenyl)diphenylmethane, bis(4-hydroxyphenyl)naphthylmethane, 1,1-bis(4-hydroxyphenyl)ethane bis(hydroxyaryl)alkanes such as ethane, 2-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)-1-naphthylethan, 1-bis(4-hydroxyphenyl)butane, 2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)hexane, 2,2-bis(4-hydroxyphenyl)hexane, 1-bis(4-hydroxyphenyl)octane, 2-bis(4-hydroxyphenyl)octane, 1-bis(4-hydroxyphenyl)hexane, 2-bis(4-hydroxyphenyl)hexane, 4,4-bis(4-hydroxyphenyl)heptane, 2,2-bis(4-hydroxyphenyl)nonane, 10-bis(4-hydroxyphenyl)decane, and 1-bis(4-hydroxyphenyl)dodecane; 1-bis(4-hydroxyphenyl)cyclopentane, 1-bis(4-hydroxyphenyl)cyclohexane, 4-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3-dimethylcyclohexane, 1-bis(4-hydroxyphenyl)-3,4-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,5-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-3,5 -dimethylphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-propyl-5-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-tert-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-tert-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-phenylcyclohexane, 1,1-bis(4-hydroxyphenyl)-4-phenylcyclohexane and other bis(hydroxyaryl)cycloalkanes; Cardo structure-containing bisphenols such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene; Dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide; Dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; Dihydroxydiarylsulfones such as 4,4'-dihydroxydiphenylsulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone:
[0053] The polycarbonate resin of the present invention may contain only one type of structural unit other than the structural units (1) and (4), or may contain two or more types.
[0054] From the viewpoint of effectively obtaining the effects of the present invention due to the inclusion of the structural unit (1), the polycarbonate resin of the present invention preferably contains 20 mol % or more, particularly 50 mol % or more of the structural unit (1) among all the structural units derived from dihydroxy compounds in the polycarbonate resin of the present invention, and it is particularly preferable that the polycarbonate resin of the present invention contains only the structural unit (1) and the structural unit (4) as all the structural units derived from dihydroxy compounds.
[0055] (Requirements <1> ) Requirements for the polycarbonate resin of the present invention <1> means that the amount of compound (3) in the alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin of the present invention is in the range of 1500 to 6000 mass ppm relative to the amount of compound (2). Hereinafter, the amount of compound (3) relative to the amount of compound (2) in the alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin is referred to as "amount of compound (3) / compound (2)".
[0056] If the amount of compound (3) / compound (2) is 1500 mass ppm or more, a lower dielectric property can be achieved. The dielectric property can be improved by satisfying other requirements. <2> , <3> Although it depends on the composition, the larger the compound (3) / compound (2) amount, the lower the concentration tends to be. However, if the compound (3) / compound (2) amount is too large, the appearance of a thin-walled molded article deteriorates, so the compound (3) / compound (2) amount is 6000 mass ppm or less. From these viewpoints, the compound (3) / compound (2) amount of the polycarbonate resin of the present invention is preferably 1700 to 5500 mass ppm, more preferably 2000 to 5200 mass ppm.
[0057] The amount of compound (3) / compound (2) in the polycarbonate resin can be determined according to the alkaline hydrolysis of the polycarbonate resin and the quantitative determination of the alkaline hydrolyzate described in the Examples section below.
[0058] (Requirements <2> ) Requirements for the polycarbonate resin of the present invention <2> The amount of terminal hydroxyl groups is 200 to 400 ppm by mass. By limiting the amount of terminal hydroxyl groups to a very limited range of 200 to 400 ppm by mass, it is possible to achieve both low dielectric properties and good appearance. The amount of terminal hydroxyl groups in the polycarbonate resin of the present invention is preferably 210 to 370 ppm by mass, more preferably 220 to 350 ppm by mass.
[0059] The amount of terminal hydroxyl groups in a polycarbonate resin refers to the total amount M of terminal hydroxyl groups represented by the following formula (5), and the unit of the amount of terminal hydroxyl groups is the mass of terminal hydroxyl groups relative to the mass of the polycarbonate resin, expressed in ppm. The measurement method is colorimetric determination by the titanium tetrachloride / acetic acid method (the method described in Macromol. Chem. 88 215 (1965)).
[0060] [ka]
[0061] (In formula (5), R 4 are each independently a halogen atom, a nitro group, a cyano group, an alkyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, a cycloalkyl group having 4 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and r represents an integer of 0 to 2.
[0062] The amount of terminal hydroxyl groups in the polycarbonate resin can be adjusted to a preferred value by controlling the molar ratio of the raw materials and the amount of catalyst during the production of the polycarbonate resin, as well as the temperature and degree of vacuum during the reaction.
[0063] As the polycarbonate resin of the present invention, two or more types of polycarbonate resins having different amounts of terminal hydroxyl groups may be mixed and used. In this case, polycarbonate resins having an amount of terminal hydroxyl groups outside the above-mentioned preferable range may be used and mixed to control the amount of terminal hydroxyl groups within the above-mentioned range.
[0064] (Requirements <3> ) Requirements for the polycarbonate resin of the present invention <3> The viscosity average molecular weight is 21,000 to 25,500. By limiting the viscosity average molecular weight to a very limited range of 21000 to 25500, it is possible to achieve both low dielectric properties and good appearance. If the viscosity average molecular weight is less than the lower limit, low dielectric properties cannot be obtained, and if it exceeds the upper limit, good appearance cannot be obtained in thin-walled molded products. The viscosity average molecular weight of the polycarbonate resin of the present invention is preferably 21500 to 25000, more preferably 22000 to 24500.
[0065] The viscosity average molecular weight (Mv) of polycarbonate resin was calculated by using methylene chloride as a solvent and an Ubbelohde viscometer to determine the intrinsic viscosity (limiting viscosity) [η] (unit: dL / g) at a temperature of 20°C, and then calculating it using the Schnell viscosity formula, i.e., η = 1.23 × 10 -4 Mv 0.83 The intrinsic viscosity (limiting viscosity) [η] is calculated by measuring the specific viscosity [ηsp] at each solution concentration [C] (g / dL) and using the following formula:
[0066]
number
[0067] The polycarbonate resin of the present invention may be a mixture of two or more polycarbonate resins having different viscosity average molecular weights. In this case, polycarbonate resins having a viscosity average molecular weight outside the above-mentioned preferred range may be used to control the viscosity average molecular weight within the above-mentioned range.
[0068] <Production method of polycarbonate resin> The polycarbonate resin of the present invention can be produced by a conventionally known polymerization method using the raw material dihydroxy compound described below, and the polymerization method is not particularly limited.Examples of the polymerization method include interfacial polymerization method, melt transesterification method, pyridine method, ring-opening polymerization method of cyclic carbonate compound, solid-phase transesterification method of prepolymer, etc.The following will specifically explain the particularly suitable method among these methods.
[0069] (interfacial polymerization method) In the interfacial polymerization method, a dihydroxy compound as a raw material is reacted with a carbonate-forming compound in the presence of an organic solvent and an alkaline aqueous solution that are inert to the reaction, usually at a pH of 9 or higher, and then interfacial polymerization is carried out in the presence of a polymerization catalyst to obtain a polycarbonate resin. Note that a molecular weight regulator (terminal terminator) may be present in the reaction system as necessary, and an antioxidant may be present to prevent oxidation of the dihydroxy compound as a raw material.
[0070] The organic solvent inert to the reaction is not particularly limited, and examples thereof include chlorinated hydrocarbons such as dichloromethane, 1,2-dichloroethane, chloroform, monochlorobenzene, dichlorobenzene, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc. Note that the organic solvent may be used alone or in any combination and ratio of two or more kinds.
[0071] The alkaline compound contained in the alkaline aqueous solution is not particularly limited, but examples thereof include alkali metal compounds and alkaline earth metal compounds such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and sodium hydrogen carbonate. Among them, sodium hydroxide and potassium hydroxide are preferred. The alkaline compounds may be used alone or in any combination and ratio of two or more.
[0072] Although there is no limitation on the concentration of the alkali compound in the alkaline aqueous solution, the alkali compound concentration is usually 5 to 10 mass % in order to control the pH of the alkaline aqueous solution to 10 to 12. Furthermore, for example, when blowing in phosgene, in order to control the pH of the aqueous phase to 10 to 12, preferably 10 to 11, it is preferable that the molar ratio of the raw material dihydroxy compound to the alkali compound is usually 1:1.9 or more, preferably 1:2.0 or more, and usually 1:3.2 or less, preferably 1:2.5 or less.
[0073] As the starting dihydroxy compound, at least compound (2) is used. <1> If necessary, compound (3) may be used as a starting dihydroxy compound so as to satisfy the above condition. However, the compound (2) used in the production of the polycarbonate resin is usually produced by condensation of a ketone or aldehyde with an aromatic alcohol according to the following reaction formula.
[0074] [ka]
[0075] (In the above formula, R a is R in Eq. (2) 1 ,R 2 is equivalent to R b ,R c -R b -CR c which is a linking group corresponding to X in formula (2).
[0076] In such a condensation reaction between a ketone or aldehyde and an aromatic alcohol, the substituent R of the aromatic alcohol is converted into an aromatic alcohol during the reaction. a is dropped and only one benzene ring has a substituent R a In addition, the aromatic alcohol used as a raw material for the production of compound (2) may contain the substituent R as an impurity in the product. a In some cases, a phenol having no substituent R is included. In this case, only one of the benzene rings has the substituent R. a A compound (3) having the formula:
[0077] Therefore, since the compound (2) produced by the above-mentioned condensation reaction may contain the compound (3) as an impurity, the compound (3) contained as an impurity in the compound (2) may be purified as necessary to obtain the required compound. <1> By adjusting the amount of compound (3) so that a polycarbonate resin satisfying the above requirement can be obtained, a necessary amount of compound (3) can be used as the raw material dihydroxy compound.
[0078] As the carbonate-forming compound, a carbonyl halide is preferably used, and among these, it is preferable to use phosgene. The method using phosgene is particularly called the phosgene method.
[0079] The polymerization catalyst is not particularly limited, but examples thereof include aliphatic tertiary amines such as trimethylamine, triethylamine, tributylamine, tripropylamine, and trihexylamine; alicyclic tertiary amines such as N,N'-dimethylcyclohexylamine and N,N'-diethylcyclohexylamine; aromatic tertiary amines such as N,N'-dimethylaniline and N,N'-diethylaniline; quaternary ammonium salts such as trimethylbenzylammonium chloride, tetramethylammonium chloride, and triethylbenzylammonium chloride; pyridine; guanine; salts of guanidine; etc. The polymerization catalyst may be used alone or in any combination and ratio of two or more.
[0080] The molecular weight regulator is not particularly limited, and examples thereof include aromatic phenols having a monovalent phenolic hydroxyl group, aliphatic alcohols such as methanol and butanol, mercaptans, and phthalic acid imides, among which aromatic phenols are preferred. Specific examples of such aromatic phenols include phenol, on-butylphenol, mn-butylphenol, pn-butylphenol, o-isobutylphenol, m-isobutylphenol, p-isobutylphenol, ot-butylphenol, mt-butylphenol, pt-butylphenol, on-pentylphenol, mn-pentylphenol, pn-pentylphenol, on-hexylphenol, mn-hexylphenol, pn-hexylphenol, pt-octylphenol, o-cyclohexylphenol, m-cyclohexylphenol, p-cyclohexylphenol, o-phenylphenol, m-phenylphenol, p-phenylphenol, on-nonylphenol, mn-nonylphenol, and pn-nonylphenol. Examples of the phenol include phenol, o-cumylphenol, m-cumylphenol, p-cumylphenol, o-naphthylphenol, m-naphthylphenol, p-naphthylphenol, 2,5-di-t-butylphenol, 2,4-di-t-butylphenol, 3,5-di-t-butylphenol, 2,5-dicumylphenol, 3,5-dicumylphenol, p-cresol, bromophenol, tribromophenol, monoalkylphenol having a linear or branched alkyl group having an average carbon number of 12 to 35 at the ortho, meta or para position, 9-(4-hydroxyphenyl)-9-(4-methoxyphenyl)fluorene, 9-(4-hydroxy-3-methylphenyl)-9-(4-methoxy-3-methylphenyl)fluorene, 4-(1-adamantyl)phenol, etc. Among these, pt-butylphenol, p-phenylphenol and p-cumylphenol are preferably used. The molecular weight regulator may be used alone or in any combination of two or more in any ratio.
[0081] The amount of the molecular weight modifier used is not particularly limited, but is, for example, usually 0.5 mol or more, preferably 1 mol or more, and usually 50 mol or less, preferably 30 mol or less, per 100 mol of the raw material dihydroxy compound.
[0082] The antioxidant is not particularly limited, but examples thereof include hindered phenol-based antioxidants. Specific examples thereof include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4, 6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0083] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Commercially available products of such phenolic antioxidants include "Irganox 1010" and "Irganox 1076" manufactured by BASF, and "Adeka STAB AO-50" and "Adeka STAB AO-60" manufactured by ADEKA.
[0084] The antioxidants may be used alone or in any combination of two or more in any ratio.
[0085] The amount of the antioxidant used is not particularly limited, but is, for example, usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, relative to 100 parts by mass of the raw material dihydroxy compound. If the amount of the antioxidant used is less than the lower limit of the above range, the antioxidant effect may be insufficient, and if the amount of the antioxidant used exceeds the upper limit of the above range, gas may be easily generated during injection molding.
[0086] In the reaction, the order of mixing the reaction substrate (reaction raw material), reaction solvent (organic solvent), catalyst, additives, etc. is arbitrary as long as the desired polycarbonate resin is obtained, and an appropriate order may be set arbitrarily. For example, when phosgene is used as the carbonate-forming compound, the molecular weight modifier can be mixed at any time between the reaction of the raw material dihydroxy compound with phosgene (phosgenation) and the start of the polymerization reaction. The reaction temperature is not particularly limited, but is preferably 0 to 40° C., and the reaction time is not particularly limited, but is preferably several minutes (for example, 10 minutes) to several hours (for example, 6 hours).
[0087] (Melt transesterification method) In the melt transesterification method, for example, a transesterification reaction is carried out between a carbonate ester and a raw material dihydroxy compound. The starting dihydroxy compound is the same as that in the interfacial polymerization method.
[0088] The carbonate ester may be, for example, a compound represented by the following general formula (6), and examples thereof include aryl carbonates, dialkyl carbonates, biscarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and carbonates of dihydroxy compounds such as cyclic carbonates.
[0089] [ka]
[0090] In the above general formula (6), R 21 and R 22 each independently represents an alkyl group, an aryl group, or an arylalkyl group having 1 to 30 carbon atoms. 21 and R 22 However, when the group is an alkyl or arylalkyl group, it is called a dialkyl carbonate, and when the group is an aryl group, it is called a diaryl carbonate. 21 and R 22 and are preferably both aryl groups, and more preferably diaryl carbonate represented by the following general formula (7).
[0091] [ka]
[0092] In the above general formula (7), R 23 and R 24 each independently represents a halogen atom, a nitro group, a cyano group, an alkyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, a cycloalkyl group having 4 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and p and q each independently represent an integer of 0 to 5.
[0093] Specific examples of such carbonate esters include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and di-t-butyl carbonate, diphenyl carbonate (hereinafter sometimes abbreviated as "DPC"), bis(4-methylphenyl) carbonate, bis(4-chlorophenyl) carbonate, bis(4-fluorophenyl) carbonate, bis(2-chlorophenyl) carbonate, bis(2,4-difluorophenyl) carbonate, bis(4-nitrophenyl) carbonate, bis(2-nitrophenyl) carbonate, bis(methylsalicylphenyl) carbonate, and diaryl carbonates (which may have a substituent) such as ditolyl carbonate, with diphenyl carbonate being preferred. These carbonate esters may be used alone or in combination of two or more.
[0094] The carbonate ester may be substituted with a dicarboxylic acid or a dicarboxylic acid ester, preferably in an amount of 50 mol % or less, more preferably 30 mol % or less. Representative dicarboxylic acids or dicarboxylic acid esters include terephthalic acid, isophthalic acid, diphenyl terephthalate, diphenyl isophthalate, etc. When substituted with such a dicarboxylic acid or dicarboxylic acid ester, a polyester carbonate is obtained.
[0095] The ratio of the raw material dihydroxy compound and the carbonate ester is arbitrary as long as the desired polycarbonate resin can be obtained, but it is preferable to use these carbonate esters in excess of the raw material dihydroxy compound when polymerizing with the dihydroxy compound. That is, the carbonate ester is preferably 1.01 times (molar ratio) or more relative to the dihydroxy compound, more preferably 1.02 or more. By setting the molar ratio within the above range, the thermal stability of the obtained polycarbonate resin is good. In addition, the carbonate ester is preferably 1.30 times (molar ratio) or less relative to the dihydroxy compound, more preferably 1.20 times or less. By setting the molar ratio within the above range, the reactivity is improved, the productivity of the polycarbonate resin having the desired molecular weight is good, and the amount of residual carbonate ester in the resin is reduced, so that odor generation can be suppressed during molding processing or when the molded product is formed, which is preferable.
[0096] When producing a polycarbonate resin by the melt transesterification method, a transesterification catalyst is usually used. The transesterification catalyst is not particularly limited, and a conventionally known catalyst can be used. For example, it is preferable to use an alkali metal compound and / or an alkaline earth metal compound. In addition, a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound may be used in combination as an auxiliary. The transesterification catalyst may be one type, or two or more types may be used in any combination and ratio.
[0097] In the melt transesterification method, the reaction temperature is not particularly limited, but is preferably 100 to 320° C. The pressure during the reaction is not particularly limited, but is preferably reduced pressure of 2 mmHg or less. As a specific operation, the melt polycondensation reaction may be carried out under the above conditions while removing by-products.
[0098] In the presence of an alkali catalyst, the polycarbonate resin of the present invention is significantly affected by heat history and oxidation, which leads to deterioration of the color tone. Therefore, it is preferable to select a reaction temperature of 320° C. or less and a reduced pressure condition with a lower limit of about 0.05 mmHg to prevent oxygen from leaking from the equipment due to excessive reduced pressure.
[0099] The reaction can be carried out in either a batch or continuous manner. In the case of a batch reaction, the order of mixing the reaction substrate, reaction solvent, catalyst, additives, etc. is arbitrary as long as the desired polycarbonate resin can be obtained, and an appropriate order may be arbitrarily set.
[0100] In the melt transesterification method, a catalyst deactivator may be used as necessary. As the catalyst deactivator, any compound that neutralizes the transesterification catalyst may be used. Examples of the catalyst deactivator include sulfur-containing acidic compounds and their derivatives, phosphorus-containing acidic compounds and their derivatives, etc. In addition, the catalyst deactivator may be used alone or in any combination and ratio of two or more.
[0101] The amount of the catalyst deactivator used is not particularly limited, but is usually 0.5 equivalents or more, preferably 1 equivalent or more, more preferably 3 equivalents or more, and usually 50 equivalents or less, preferably 10 equivalents or less, more preferably 8 equivalents or less, relative to the transesterification catalyst. The amount of the catalyst deactivator used is usually 1 ppm by mass or more, 100 ppm by mass or less, and preferably 50 ppm by mass or less, relative to the polycarbonate resin.
[0102] <Other ingredients> The polycarbonate resin composition of the present invention may contain other components in addition to the polycarbonate resin of the present invention, as necessary, as long as the desired physical properties are not significantly impaired. Examples of other components include polycarbonate resins other than the polycarbonate resin of the present invention (i.e., polycarbonate resins that do not meet the requirements for the polycarbonate resin of the present invention). <1> ~ <3> Examples of the polycarbonate resin include polycarbonate resins that do not satisfy the above requirements, resins other than polycarbonate resins, and various resin additives.
[0103] However, in order to reliably obtain the effects of the present invention by including the polycarbonate resin of the present invention, the polycarbonate resin composition of the present invention preferably contains the polycarbonate resin of the present invention in a total amount of 65 mass % or more, particularly 70 mass % or more, and especially 75 mass % or more, based on 100 mass % of the polycarbonate resin composition. In addition, the content of the polycarbonate resin in the polycarbonate resin composition of the present invention is preferably 80 mass% or more, more preferably 85 mass% or more, and particularly preferably 90 mass% or more, relative to 100 mass% of the polycarbonate resin composition of the present invention, in order to effectively bring out the features of the present invention.
[0104] Examples of resin additives include heat stabilizers, antioxidants, release agents, light resistance agents (HALS), flame retardants, antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, dyes, pigments, etc. One type of resin additive may be contained, or two or more types may be contained in any combination and ratio.
[0105] Other resins include, for example, thermoplastic polyester resins such as polyethylene terephthalate resin, polytrimethylene terephthalate, and polybutylene terephthalate resin; styrene-based resins such as polystyrene resin, high impact polystyrene resin (HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-styrene-acrylic rubber copolymer (ASA resin), and acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin); polyolefin resins such as polyethylene resin and polypropylene resin; polyamide resins; polyimide resins; polyetherimide resins; polyurethane resins; polyphenylene ether resins; polyphenylene sulfide resins; polysulfone resins; and polymethacrylate resins. Incidentally, one type of the other resin may be contained, or two or more types may be contained in any combination and ratio.
[0106] <Polycarbonate resin molding method> For producing a polycarbonate resin molded article from the polycarbonate resin composition of the present invention, a conventional extruder or injection molding machine is used.
[0107] The molding temperature when molding the polycarbonate resin composition of the present invention is preferably 200°C or higher, more preferably 250°C or higher, and most preferably 280°C or higher. By setting the molding temperature to the above lower limit or higher, the flowability is improved and moldability is improved. In addition, the molding temperature when molding the polycarbonate resin composition of the present invention is preferably 350°C or lower, particularly preferably 320°C or lower. By setting the molding temperature to the above upper limit or lower, the color tone of the polycarbonate resin composition can be made good.
[0108] When injection molding or extrusion molding is carried out, pigments, dyes, mold release agents, heat stabilizers, etc. may be added to the polycarbonate resin composition of the present invention as appropriate within the limits not impairing the object of the present invention.
[0109] <Polycarbonate resin molded products> The polycarbonate resin composition of the present invention can be suitably used as a molded product by thermal processing such as injection molding and extrusion molding. There is no limitation on the shape, pattern, color, size, etc. of such a polycarbonate resin molded product, and it can be appropriately selected according to the application of the molded product, and examples thereof include various shapes such as plate-like, plate-like, rod-like, sheet-like, film-like, cylindrical, annular, circular, elliptical, polygonal, irregular, hollow, frame-like, box-like, panel-like, and special shapes. In addition, it may be a three-dimensional shape having, for example, an uneven surface or a three-dimensional curved surface.
[0110] (Injection molded product) The polycarbonate resin composition of the present invention can be suitably used as an injection molded product by injection molding. The injection molding method is not particularly limited, and any molding method generally used for thermoplastic resins can be used. Examples include ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted and other hollow molding methods, molding methods using a heat-insulating mold, molding methods using a rapidly heated mold, foam molding (including supercritical fluid), insert molding, and IMC (in-mold coating molding) molding. A molding method using a hot runner system can also be used.
[0111] When an injection molding machine or the like is used, the mold temperature is preferably 150°C or less, more preferably 120°C or less, and most preferably 100°C or less. By setting the mold temperature to the above upper limit or less, the cooling time during molding can be shortened, and the manufacturing cycle of molded products can be shortened, thereby improving productivity. Furthermore, when an injection molding machine or the like is used, the mold temperature is preferably 30°C or more, and particularly preferably 50°C or more. Setting the mold temperature to the above lower limit or more is preferable because a uniform molded product can be obtained.
[0112] (Extrusion molding) The polycarbonate resin composition of the present invention can be suitably used as an extrusion molded product by extrusion molding. To produce an extrusion molded product from the polycarbonate resin composition of the present invention, an extrusion molding machine is usually used, although there is no particular limitation. The extrusion molding machine is generally equipped with a T-die or a round die, and extrusion molded products of various shapes can be obtained. Examples of the extrusion molded product include a sheet, a film, a plate, a tube, a pipe, and the like. Among these, a sheet or a film is preferred.
[0113] The extrusion molded product of the polycarbonate resin composition of the present invention may be laminated on both sides or one side of the extrusion molded product with a hard coat layer for improving adhesion, paintability, and printability, or may be heat-laminated on both sides or one side of the extrusion molded product with a film for improving weather resistance and / or scratch resistance. In addition, the surface may be subjected to a graining process, a semi-transparent or opaque process, or the like.
[0114] (Application) Molded articles of the polycarbonate resin composition of the present invention can be used, for example, as various automobile parts, electric and electronic devices, information terminal devices, office automation equipment, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods and miscellaneous goods, lighting equipment and the like, in particular, housings for electronic devices such as smartphones and computers, antenna covers, covers for wired communication devices such as routers and switches, covers for millimeter wave radars, etc.
[0115] Among these, the polycarbonate resin composition of the present invention can be effectively used as a molding material for housings for communication devices having built-in microwave and / or millimeter wave antennas, particularly because of its low dielectric properties and good appearance in thin-walled molded articles.
[0116] (Molded product thickness) The thickness of a molded article using the polycarbonate resin composition of the present invention, particularly a housing for a communication device incorporating a microwave and / or millimeter wave antenna described below, is preferably 1.5 mm or less, more preferably 1.2 mm or less, and most preferably 1.0 mm or less. Here, the thickness of the molded article refers to the thickness of a portion occupying 50% or more of the area of the entire molded article, for example, the thickness of the main plate surface. If the thickness of the molded article is equal to or less than the upper limit, the transmission loss can be reduced. If the thickness of the molded article is equal to or more than the lower limit, the mechanical strength and the like required to maintain the structure of the molded article can be made sufficient. When the thickness of the molded article is greater than 1.5 mm, the occurrence of defective appearance is rare, but when the thickness is 1.5 mm or less, shear heat during injection molding increases, and black foreign matter is particularly likely to occur. The polycarbonate resin composition of the present invention can provide a good appearance in thin-walled molded articles that are prone to such defective appearance.
[0117] [Housing for communication devices] Molded articles obtained using the polycarbonate resin composition of the present invention have a low dielectric tangent, are thin, have good appearance, and have excellent radio wave transmittance in the microwave and / or millimeter wave bands, and are therefore useful as housings for communication devices with built-in microwave and / or millimeter wave antennas for which these properties are strictly required.
[0118] There are no restrictions on the shape, pattern, color, dimensions, etc. of the housing for a communications device incorporating such a microwave and / or millimeter wave antenna, and these can be appropriately selected depending on the application of the housing for a communications device incorporating a microwave and / or millimeter wave antenna.
[0119] In the present invention, microwaves are radio waves with a frequency of 3.0 to 30 GHz, and millimeter waves are radio waves with a frequency of 30 to 300 GHz. Thus, microwaves and / or millimeter waves are radio waves with a frequency of 3.0 to 300 GHz. That is, a communication device with a built-in antenna for microwaves and / or millimeter waves is a communication device with a built-in antenna for transmitting and receiving radio waves with a frequency of 3.0 to 300 GHz. Specific examples of the communication device include a notebook computer, a tablet terminal, a smartphone, or a router device that transmits and receives radio waves with a frequency of 3.0 to 300 GHz.
[0120] The frequency at which the microwave and / or millimeter wave antenna of the communication device housing of the present invention transmits and receives is not particularly limited as long as it is 3.0 to 300 GHz, but is more suitable for radio waves in the frequency band of 3.2 to 250 GHz, and even more suitable for radio waves in the frequency band of 3.4 to 200 GHz.
[0121] In particular, the communications device housing having a built-in microwave and / or millimeter wave antenna of the present invention can be suitably used for radio waves in the frequency band of 3.5 to 30 GHz used in 5G (fifth generation mobile communications system).
[0122] Radio waves in the microwave and / or millimeter wave bands tend to have poor radio wave permeability, and from this perspective, a housing for a communication device incorporating an antenna for transmitting and receiving radio waves in the microwave and / or millimeter wave bands is required to have high radio wave permeability. Furthermore, housings for communication devices that incorporate microwave and / or millimeter wave antennas are required to be thin and have a good appearance in order to make them compact and to improve the design of the product.
[0123] The polycarbonate resin of the present invention contained in the polycarbonate resin composition of the present invention used for a housing for a communication device having a built-in antenna for transmitting and receiving microwave and / or millimeter wave band radio waves of the present invention has a low dielectric tangent, high thin-wall moldability, and good appearance. Therefore, the polycarbonate resin composition of the present invention containing such a polycarbonate resin of the present invention has a low relative dielectric constant, high thin-wall moldability, and good appearance, and is suitable for use in the housing of a communication device that transmits and receives microwave and / or millimeter wave band radio waves.
[0124] Specific examples of the housing for communication devices having a built-in microwave and / or millimeter wave antenna include the housings for notebook computers, tablet terminals, smartphones, router devices, etc. The molded article of the present invention made of the polycarbonate resin composition of the present invention is particularly suitable for these applications. EXAMPLES
[0125] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0126] The physical properties of the polycarbonate resins obtained in the following Examples and Comparative Examples were evaluated by the following methods.
[0127] (1) Viscosity average molecular weight (Mv) The polycarbonate resin was dissolved in methylene chloride (concentration: 6.0 g / L), and the intrinsic viscosity (limiting viscosity) [η] (unit: dL / g) at 20°C was determined using an Ubbelohde viscosity tube (manufactured by Moritomo Rika Kogyo Co., Ltd.), and the viscosity average molecular weight (Mv) was calculated using Schnell's viscosity formula (formula below). η = 1.23 × 10 -4 Mv 0.83
[0128] (2) Terminal hydroxyl group content The amount of terminal hydroxyl groups in the polycarbonate resin was measured by colorimetry in accordance with the titanium tetrachloride / acetic acid method (the method described in Macromol. Chem. 88, 215 (1965)). In the case of a polycarbonate resin copolymer consisting of a plurality of dihydroxy compounds, samples are prepared by mixing the corresponding dihydroxy compounds according to the copolymerization ratio at least at three levels of concentration, and a calibration curve is drawn from the data of the three or more points before measuring the amount of terminal hydroxyl groups of the polycarbonate resin. The detection wavelength is 546 nm.
[0129] (3) Alkaline hydrolysis and quantification of alkaline hydrolysate 0.5 g of polycarbonate resin was dissolved in 5 mL of methylene chloride to obtain a solution. Then, 45 mL of methanol and 5 mL of 25% by mass aqueous sodium hydroxide solution were added to the solution, and the mixture was stirred at 70° C. for 30 minutes. The obtained solution was analyzed by liquid chromatography under the following measurement conditions, and the hydrolyzate was quantified to calculate the amount of compound (3) / compound (2) (ratio of monomethyl BPA to BPC). Equipment: Shimadzu Corporation System controller: CBM-20A Pump: LC-10AD Column oven: CTO-10ASvp Detector: SPD-M20A Analytical column: YMC-Pack ODS-AM 75mm×φ4.6mm Oven temperature: 40℃ Detection wavelength: 280nm Eluent: Solution A: 0.1% trifluoroacetic acid aqueous solution, Solution B: acetonitrile From A / B=60 / 40(vol%) to A / B=95 / 5(vol%) Gradient in 50 minutes Flow rate: 1mL / min Sample injection volume: 20 μL Each hydrolyzate was identified by the peaks observed at the above retention times. Fractionated samples were collected and 1 HNMR, 13 CNMR, two-dimensional NMR method, mass spectrometry (MS) and infrared absorption spectroscopy (IR spectroscopy).
[0130] (4) Number of plates with black foreign matter The polycarbonate resin pellets were dried at 100°C for 5 hours using a hot air dryer, and then injection molded using a Japan Steel Works J75EII injection molding machine under conditions of a cylinder temperature of 290°C, a mold temperature of 70°C, and a molding cycle of 40 seconds, to obtain 10 polycarbonate resin plate-shaped molded bodies measuring 0.8 mm in thickness, 100 mm in length, and 100 mm in width. The appearance of the 10 plate-like molded products was visually observed, and plates on which one or more black foreign matter of 30 μm or more was confirmed were regarded as plates with black foreign matter, and the number of such plates was counted.
[0131] (5) Specific permittivity (ε r ) · Dielectric tangent (tan δ) Polycarbonate resin that had been vacuum dried at 80°C for 5 hours was molded into a film shape using a heat press molding machine to produce a film with a thickness of 80 to 120 μm. The molding conditions for the heat press molding machine were appropriately adjusted within the range of a temperature of 150 to 250°C and a pressure of 10 to 15 MPa. From this film, a strip of film with a length of 70 mm and a width of 2 mm was cut out and conditioned for 48 hours under conditions of a room temperature of 23°C and a humidity of 50%. After that, the relative dielectric constant (ε r) and dielectric tangent (tan δ) were measured.
[0132] [Raw material dihydroxy compound] The raw dihydroxy compound used was BPC: 2,2-bis(4-hydroxy-3-methylphenyl)propane (manufactured by Honshu Chemical Industry Co., Ltd.), which contained monomethyl BPA as an impurity in the amounts shown in Table 1 below.
[0133] [Table 1]
[0134] [Example 1] 6.6 kg of BPC-a and 5.8 kg of diphenyl carbonate (DPC) were added to a first reactor having an internal volume of 40 L and equipped with a stirrer, a heat medium jacket, a vacuum pump, and a reflux condenser. Then, an aqueous solution of cesium carbonate was added so that the amount of cesium carbonate was 1.5 μmol per 1 mol of the dihydroxy compound (BPC-a) to prepare a mixture.
[0135] Next, the inside of the first reactor was depressurized to 1.33 kPa (10 Torr), and then the operation of returning the pressure to atmospheric pressure with nitrogen was repeated five times, and the inside of the first reactor was replaced with nitrogen. After the nitrogen replacement, the inside temperature of the first reactor was gradually increased by passing a heat medium at a temperature of 230°C through the heat medium jacket, and the mixture was dissolved. Then, the stirrer was rotated at 330 rpm, and the temperature in the heat medium jacket was controlled to keep the inside temperature of the first reactor at 220°C. Then, the pressure in the first reactor was reduced from 101.3 kPa (760 Torr) to 13.3 kPa (100 Torr) in absolute pressure over 40 minutes, while distilling off phenol by-produced by the oligomerization reaction of BPC-a and DPC carried out inside the first reactor.
[0136] Next, the pressure in the first reactor was kept at 13.3 kPa, and the transesterification reaction was carried out for 80 minutes while further distilling off phenol. The system was restored to 101.3 kPa absolute pressure with nitrogen, and the gauge pressure was increased to 0.2 MPa, and the oligomer in the first reactor was pumped to the second reactor via a transfer pipe previously heated to 200°C or higher. The second reactor had an internal volume of 30 L, and was equipped with a stirrer, a heat medium jacket, a vacuum pump, and a reflux condenser, and the internal pressure was controlled to atmospheric pressure and the internal temperature to 240°C.
[0137] Next, the oligomer pumped into the second reactor was stirred at 33 rpm, the internal temperature was raised by a heat medium jacket, and the pressure in the second reactor was reduced from 101.3 kPa to 13.3 kPa in absolute pressure over 40 minutes. After that, the temperature was continued to be raised, and the internal pressure was reduced from 13.3 kPa to 399 Pa (3 Torr) in absolute pressure over another 40 minutes, and the distilled phenol was removed from the system. Furthermore, the temperature was continued to be raised, and after the absolute pressure in the second reactor reached 70 Pa (about 0.5 Torr), 70 Pa was maintained and a polycondensation reaction was carried out. When the agitator of the second reactor reached a predetermined stirring power (corresponding to a viscosity average molecular weight of 23,000 to 25,000), the polycondensation reaction was terminated, and then the mixture was pelletized. The polymerization reaction time in the second reactor was about 194 minutes. The maximum temperature of the second reactor was 286°C. The polycarbonate resin thus obtained was subjected to the various evaluations according to the above procedures. The results are shown in Table 2.
[0138] [Example 2] Except for using BPC-b instead of BPC-a, the same procedure as in Example 1 was carried out. The evaluation results are shown in Table 2.
[0139] [Example 3] The same procedure as in Example 1 was repeated except that BPC-c was used instead of BPC-a. The evaluation results are shown in Table 2.
[0140] [Example 4] The same procedure as in Example 1 was repeated, except that 3.3 kg of BPC-a and 3.3 kg of BPC-d were used instead of 6.6 kg of BPC-a. The evaluation results are shown in Table 2.
[0141] [Comparative Example 1] The same procedure as in Example 1 was repeated except that BPC-d was used instead of BPC-a. The evaluation results are shown in Table 2.
[0142] [Comparative Example 2] The same procedure as in Example 1 was repeated except that BPC-e was used instead of BPC-a. The evaluation results are shown in Table 2.
[0143] [Comparative Example 3] The same procedure as in Example 1 was repeated except that 6.5 kg of BPC-a was used. The evaluation results are shown in Table 2.
[0144] [Comparative Example 4] The same procedure as in Example 1 was repeated except that 6.7 kg of BPC-a was used. The evaluation results are shown in Table 2.
[0145] [Comparative Example 5] The same procedure as in Example 1 was carried out, except that 6.7 kg of BPC-a was used and the reaction was stopped when the predetermined stirring power target in the stirrer of the second reactor corresponded to a viscosity average molecular weight of 20,000. The evaluation results are shown in Table 2.
[0146] [Comparative Example 6] The same procedure as in Example 1 was carried out, except that the reaction was stopped when the predetermined stirring power target in the stirrer of the second reactor corresponded to a viscosity average molecular weight of 26,000. The evaluation results are shown in Table 2.
[0147] [Comparative Example 7] The same procedure as in Example 1 was repeated, except that 6.8 kg of BPC-e was used instead of BPC-a, and the reaction was stopped when the predetermined stirring power target in the stirrer of the second reactor corresponded to a viscosity average molecular weight of 26,500. The evaluation results are shown in Table 2.
[0148] In Table 2 below, the polycarbonate resin produced in each example meets the requirements. <1> Requirements <3> In the remarks column, it is also noted whether or not the above conditions are met (○) or not (×).
[0149] [Table 2]
[0150] [Consideration] From the above results, the following can be seen: Requirements <1> or <2> In Comparative Examples 1 to 4, which do not satisfy the above requirement, a low dielectric tangent cannot be achieved. <1> and requirements <2> Even if it meets the requirements, the molecular weight is small. <3> In Comparative Example 5, which does not satisfy the above requirement, the dielectric tangent is high, but the molecular weight is large. <3> In Comparative Example 6, which does not satisfy the above requirements, black foreign matter is generated in a relatively thin molded product having a thickness of 0.8 mm. <1> Requirements <3> Comparative Example 7, which does not satisfy all of the above, is significantly inferior in both dielectric properties and appearance. In contrast, the requirements <1> Requirements <3> In Examples 1 to 4 which satisfy the above, the dielectric tangent is low, and even with a thin plate of 0.8 mm, the generation of black foreign matter is suppressed, and a molded product with excellent appearance can be obtained.
Claims
1. A housing for a communication device having a built-in microwave and / or millimeter wave antenna, the housing being obtained using a polycarbonate resin composition, The polycarbonate resin composition contains at least a polycarbonate resin having a structural unit represented by the following formula (1): An alkaline hydrolysate obtained by alkaline hydrolysis of the polycarbonate resin contains a compound represented by the following formula (2) and a compound represented by the following formula (3), and the amount of the compound represented by the following formula (3) in the alkaline hydrolysate is 1,500 ppm by mass or more and 6,000 ppm by mass or less relative to the amount of the compound represented by the following formula (2) in the alkaline hydrolysate, The amount of terminal hydroxyl groups in the polycarbonate resin is 200 ppm by mass or more and 400 ppm by mass or less, The polycarbonate resin has a viscosity average molecular weight of 21,000 or more and 25,500 or less. 【Chemistry 1】 (In formula (1), formula (2) and formula (3), R 1 , R 2 and R 3 each independently represents a substituted or unsubstituted alkyl group having from 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group, and X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom.
2. 2. The housing for communication device according to claim 1, which has a thickness of 1.5 mm or less.
3. The housing for a communication device according to claim 1 or 2, wherein the structural unit represented by formula (1) is a structural unit represented by the following formula (1-1), the compound represented by formula (2) is a compound represented by the following formula (2-1), and the compound represented by formula (3) is a compound represented by the following formula (3-1). 【Chemistry 2】
4. 4. The housing for a communications device according to claim 1, wherein the antenna is used for radio waves in a frequency band of 3.5 to 30 GHz.
5. The housing for a communication device according to any one of claims 1 to 4, wherein the communication device is a notebook computer, a tablet terminal, a smartphone, or a router device.
6. A communication device having a built-in microwave and / or millimeter wave antenna, obtained by using the housing for communication device according to any one of claims 1 to 5.
7. A polycarbonate resin composition for a housing of a communication device having a built-in microwave and / or millimeter wave antenna, comprising a polycarbonate resin having at least a structural unit represented by the following formula (1): The alkaline hydrolyzate obtained by alkaline hydrolysis of the polycarbonate resin contains a compound represented by the following formula (2) and a compound represented by the following formula (3), the amount of the compound represented by the following formula (3) in the alkaline hydrolysate is 1500 ppm by mass or more and 6000 ppm by mass or less relative to the amount of the compound represented by the following formula (2) in the alkaline hydrolysate, The amount of terminal hydroxyl groups in the polycarbonate resin is 200 ppm by mass or more and 400 ppm by mass or less, The viscosity average molecular weight of the polycarbonate resin composition for use in housings of communication devices is 21,000 or more and 25,500 or less. 【Chemistry 3】 (In formula (1), formula (2) and formula (3), R 1 , R 2 and R 3 each independently represents a substituted or unsubstituted alkyl group having from 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group, and X represents a single bond, a carbonyl group, a substituted or unsubstituted alkylidene group, a substituted or unsubstituted sulfur atom, or an oxygen atom.
8. A molded article for a housing of a communication device, obtained by using the polycarbonate resin composition for a housing of a communication device according to claim 7.
Citation Information
Patent Citations
Method for producing polycarbonate resin, and polycarbonate resin
JP2011219636A
Method for producing polycarbonate resin
JP2013072077A
Polycarbonate resin and composition thereof
JP2013227508A
Polycarbonate resin and polycarbonate resin composition
JP2015030835A
Millimeter wave radar-purpose cover and millimeter wave radar module including the same
JP2019197048A