Heat-shrinkable film, molded article using same, heat-shrinkable label, and container

The heat-shrinkable film with a specialized antistatic layer addresses static electricity problems, ensuring excellent transparency, gloss, and improved printing quality even in low-humidity conditions.

JP7589562B2Active Publication Date: 2024-11-26MITSUBISHI CHEM CORP
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2021006607
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-19
Publication Date
2024-11-26
Estimated Expiration
2040-03-09

AI Technical Summary

Technical Problem

Existing heat-shrinkable films face issues with static electricity generation and accumulation, especially in low-humidity environments, leading to poor printing quality and film adhesion, which conventional antistatic coatings do not adequately address.

Method used

A heat-shrinkable film with a layer containing an antistatic agent on one side, having specific surface resistivity, static friction coefficient, and heat shrinkage rate, ensuring excellent transparency, gloss, and antistatic properties even in low-humidity conditions.

Benefits of technology

The film achieves improved antistatic performance, reducing static-related issues and enhancing printing processability, with reduced film adhesion and ink transfer defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589562000001
    Figure 0007589562000001
  • Figure 0007589562000002
    Figure 0007589562000002
Patent Text Reader

Abstract

To provide a heat-shrinkable film which is excellent in transparency, glossiness, antistatic properties in particular under low-humidity environments, and printing processability.SOLUTION: A heat-shrinkable film has an anti-static agent containing layer disposed on at least one face of a layer whose main constituent is a thermoplastic resin. The heat-shrinkable film satisfies a) to d) in the following: a) the electrification voltage half-life of the anti-static agent containing layer measured according to JIS L1094 is 5 seconds or less, under an atmosphere having the temperature of 23°C and the relative humidity of 50%; b) the coefficients of static friction of one face and the other face measured according to JIS K7125 are from 0.20 to 0.50 inclusive, under an atmosphere having the temperature of 23°C and the relative humidity of 50%; c) the shrinkage rate in the main shrinkage direction is 20% or more after immersion in warm water at 80°C for 10 seconds; and d) the haze value measured according to JIS K7136 is 7% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-shrinkable film, a molded product, a heat-shrinkable label, and a container that can be suitably used as a packaging material for food, a packaging material for beverages, a packaging material for medicines and medical products, a packaging material for chemicals, a packaging material for cosmetics, a packaging material for toiletries, a packaging material for industrial use, a packaging material for agricultural materials, and the like. [Background technology]

[0002] Heat shrinkable films are used for a variety of purposes, including food packaging, beverage packaging, pharmaceutical and medical packaging, chemical packaging, cosmetic packaging, toiletry packaging, industrial packaging, and agricultural packaging, and due to their heat shrinkability, they are widely used in shrink wrapping, shrink bundling packaging, shrink labels for plastic containers (such as PET bottles), shatter-proof packaging for glass containers, cap seals, etc. As the heat-shrinkable film, films made of polyvinyl chloride resin or polystyrene resin have been mainly used in the past. In contrast, in recent years, there has been a demand for heat-shrinkable films made of polyester resin, which is excellent in safety, hygiene, and chemical resistance, and the use of stretched films made of polyester resin has been increasing.

[0003] In recent years, a wide variety of printing methods, including beautiful designs, have been applied to heat-shrinkable films in order to convey information such as product names and usage precautions, as well as to add a decorative element to the film. Printing technology has improved remarkably in recent years, allowing for faster printing speeds and the printing of sophisticated gradation patterns, and so gradation patterns have recently been used more and more frequently in gravure printing. Among them, heat shrinkable films using thermoplastic resin as a base material have a problem that static electricity is easily generated and accumulated in the film because the material is an insulator, and problems caused by static electricity are likely to occur, especially in winter environments with low humidity. Specifically, static electricity generated during roll transport of the film when printing on the heat shrinkable film causes poor transfer of the printing ink, and also causes adverse effects on the printing design due to contamination mixed into the film surface. Furthermore, with the increasing printing speed in recent years, static electricity is easily generated, and heat shrinkable films are required to have excellent antistatic properties.

[0004] As an example of the heat-shrinkable film having excellent antistatic properties, Patent Document 1 discloses a heat-shrinkable polyester film having a betaine-based amphoteric surfactant applied to one side of the film.

[0005] Furthermore, Patent Document 2 discloses a heat-shrinkable polyester film having a coating layer made of either a mixture of an anionic surfactant and glycerin or a cationic surfactant on at least one side of the film. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-265465 A [Patent Document 2] JP 2007-197527 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the technology disclosed in Patent Document 1 does not have sufficient antistatic properties, and further improvement is required. The technology disclosed in Patent Document 2 has a certain degree of antistatic properties, but does not have sufficient antistatic properties under low humidity. In addition, although the dynamic friction coefficient is in a sufficient range, during film production and secondary processing such as printing, the film becomes charged, especially under low humidity, and the films tend to adhere to each other, which makes it easy for defects such as scratches to occur, and further improvement is required. Furthermore, since the technology disclosed in Patent Document 2 does not take into account the static friction coefficient, when the heat-shrinkable film is wound into a roll-shaped original film, it is easy for the winding to slip, which makes it easy for defects to occur during secondary processing such as printing, and further improvement is required in this respect as well.

[0008] In view of the above, an object of the present invention is to provide a heat-shrinkable film having excellent transparency, gloss, antistatic properties even in a low humidity environment, and excellent printability. [Means for solving the problem]

[0009] As a result of intensive research into the above-mentioned problems, the inventors have discovered that by setting the surface resistivity, static friction coefficient, heat shrinkage rate, and haze value of a thermoplastic film having a layer containing an antistatic agent on at least one side of a layer mainly composed of a thermoplastic resin within specific ranges, a heat-shrinkable film can be obtained that is excellent in transparency, gloss, and particularly in antistatic properties even in low humidity environments, and has excellent printability, and have completed the present invention.

[0010] That is, the present invention relates to a heat-shrinkable film having a layer containing an antistatic agent on at least one side of a layer containing a thermoplastic resin as a main component, and which satisfies the following a) to d). a) The surface resistivity of the layer containing the antistatic agent is 5.0×10 in an atmosphere at a temperature of 23° C. and a relative humidity of 30%. 11 (Ω / sq) or less, and at a temperature of 23°C and a relative humidity of 50%, 1.0×10 11 (Ω / sq) or less b) The static friction coefficient between one surface and the other surface, measured in accordance with JIS K7125, is 0.20 to 0.50 in an atmosphere having a temperature of 23°C and a relative humidity of 50%. c) The shrinkage rate in the main shrinkage direction when immersed in 80°C hot water for 10 seconds is 20% or more. d) Haze value measured according to JIS K7136 is 7% or less Effect of the Invention

[0011] According to the present invention, the above film can be made into a heat-shrinkable film that has excellent transparency, gloss, and antistatic properties, particularly even in a low humidity environment, and is excellent in printability, and can be suitably used for food packaging applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The heat shrinkable film of the present invention (hereinafter, sometimes referred to as "the film of the present invention") will be described in detail below. In this specification, the term "mainly contained" means that other components are permitted to be contained within a range that does not impede the action and effect of the resin contained as the main component. Furthermore, the term "mainly contained" does not limit the specific content, but preferably means a component whose content in the total components is 50% by mass or more, more preferably a component whose content is 70% by mass or more, even more preferably a component whose content is 80% by mass or more, and further preferably a component whose content is 100% by mass or less.

[0013] The heat-shrinkable film of the present invention comprises a layer containing an antistatic agent on at least one surface of a layer containing a thermoplastic resin as a main component, and satisfies specific physical properties.

[0014] [Layer containing thermoplastic resin as main component] The heat-shrinkable film used in the present invention has a layer containing a thermoplastic resin as a main component (hereinafter referred to as a "thermoplastic resin layer"). As the thermoplastic resin, a known resin generally used for a thermoplastic film can be used. Among them, a polyester-based resin is preferred from the viewpoint of shrinkage. The polyester-based resin, which is a preferred thermoplastic resin of the present invention, will be described in detail below.

[0015] [Polyester resin] The polyester resin is a thermoplastic resin obtained by polymerizing a polymerization component containing a dicarboxylic acid component and a diol component as constituent raw materials. Among them, aromatic polyester resin and polylactic acid resin are preferable.

[0016] (Aromatic polyester resin) The aromatic polyester resin contains aromatics in at least one of the dicarboxylic acid component and the diol component. In particular, it is preferable that the dicarboxylic acid component contains aromatics. The aromatic polyester resin may be used alone, but it is preferable to use two or more of them in combination.

[0017] Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2,5-dichloroterephthalic acid, 2-methylterephthalic acid, 4,4-stilbene dicarboxylic acid, 4,4-biphenyl dicarboxylic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, bisbenzoic acid, bis(p-carboxyphenyl)methane, anthracene dicarboxylic acid, 4,4-diphenyl ether dicarboxylic acid, 4,4-diphenoxyethane dicarboxylic acid, 5-Na sulfoisophthalic acid, and ethylene-bis-p-benzoic acid, aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, and dodecanedioic acid, and alicyclic dicarboxylic acids such as 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid. These dicarboxylic acid components may be used alone or in combination of two or more. Among these, aromatic dicarboxylic acids are preferred, with terephthalic acid and isophthalic acid being particularly preferred, and it is more preferred that terephthalic acid is used as the main component.

[0018] The amount of terephthalic acid in the copolymerization components is, from the viewpoint of mechanical properties such as rigidity, heat shrinkability, and breakage resistance, preferably 60 mol% or more, more preferably 65 mol% or more, and even more preferably 70 mol% or more, and is preferably 100 mol% or less, relative to 100 mol% of the total amount of the dicarboxylic acid components.

[0019] Examples of the diol component include aliphatic diols such as ethylene glycol, 1,4-butanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, and 1,3-propanediol, and alicyclic diols such as 1,1-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanediol, and 1,4-cyclohexanediol. These diol components may be used alone or in combination of two or more. Among these, ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol are preferred. It is more preferred to use ethylene glycol or 1,4-butanediol as the main component.

[0020] When ethylene glycol or 1,4-butanediol is used as the main component, the blending amount is preferably 50 mol % or more, more preferably 55 mol % or more, and even more preferably 60 mol % or more, based on 100 mol % of the total amount of the diol components.

[0021] In addition, when a diol component other than ethylene glycol or 1,4-butanediol is contained, the blending amount is preferably 1 mol % or more, more preferably 2 mol % or more, and is preferably 40 mol % or less, more preferably 35 mol % or less, and even more preferably 30 mol % or less, relative to 100 mol % of the total amount of the diol components.

[0022] The aromatic polyester resin is a copolymer polyester resin, and contains terephthalic acid and ethylene glycol as copolymerization components, and further contains at least one component having low crystallinity, such as 1,4-butanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, 1,4-cyclohexanedimethanol, 1,3-propanediol, and isophthalic acid. Among them, it is particularly preferable to contain 1,4-butanediol, 1,4-cyclohexanedimethanol, and isophthalic acid.

[0023] The aromatic polyester resin can be produced by a conventional method for producing polyester resins, such as a direct polymerization method or an ester exchange method, in a batch or continuous manner.

[0024] The aromatic polyester resin obtained by the above method is usually drawn out in the form of a strand from a draw-out port provided at the bottom of a polycondensation reaction tank, and cut into pellets with a cutter while or after water cooling. The pellets after polycondensation can be further heated to carry out solid-phase polycondensation, thereby further increasing the polymerization degree and reducing the amount of reaction by-products such as acetaldehyde and low molecular weight oligomers.

[0025] In the above-mentioned method for producing an aromatic polyester resin, the esterification reaction can be carried out using an esterification reaction catalyst such as diantimony trioxide, an organic acid salt of antimony, titanium, magnesium, calcium, etc., or an organometallic compound, if necessary. In the ester exchange reaction, an ester exchange reaction catalyst such as an organic acid salt of lithium, sodium, potassium, magnesium, calcium, manganese, titanium, zinc, etc., or an organometallic compound, if necessary, can be used.

[0026] The polycondensation reaction can be carried out in the presence of a phosphorus compound such as orthophosphoric acid, phosphorous acid, hypophosphorous acid, polyphosphoric acid, and their esters or organic acid salts, using a polycondensation catalyst such as a metal oxide such as diantimony trioxide, germanium dioxide, or germanium tetroxide, an organic acid salt of antimony, germanium, zinc, titanium, or cobalt, or an organometallic compound.

[0027] Among these polycondensation catalysts, one or more selected from tetrabutoxytitanium, diantimony trioxide, and germanium dioxide are particularly preferably used. Furthermore, in order to promote defoaming during the polymerization process, a defoaming agent such as silicone oil can also be added.

[0028] The amount of the above catalysts, including the esterification reaction catalyst, the ester exchange reaction catalyst, and the polycondensation catalyst, used is usually in the range of 5 ppm by mass or more and 2000 ppm by mass or less, preferably 10 ppm by mass or more and 500 ppm by mass or less, in terms of metal amount (atomic equivalent) relative to the theoretical yield of the obtained aromatic polyester resin.

[0029] The intrinsic viscosity of the aromatic polyester resin used in the present invention is usually 0.4 dL / g or more, preferably 0.6 dL / g or more, and 1.5 dL / g or less, preferably 1.2 dL / g or less. If the intrinsic viscosity of the aromatic polyester resin is 0.4 dL / g or more, sufficient mechanical properties are obtained, and if the intrinsic viscosity is less than 1.5 dL / g, good moldability is obtained. The intrinsic viscosity is a value measured at 30°C in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1:1).

[0030] (Polylactic acid resin) The polylactic acid resin refers to a homopolymer of D-lactic acid or L-lactic acid, or a copolymer thereof, specifically, poly(D-lactic acid) whose structural unit is D-lactic acid, poly(L-lactic acid) whose structural unit is L-lactic acid, and poly(DL-lactic acid) which is a copolymer of L-lactic acid and D-lactic acid, and also includes a mixed resin of a plurality of the above copolymers with different copolymerization ratios of D-lactic acid and L-lactic acid. Among them, the copolymer of L-lactic acid and D-lactic acid is preferred.

[0031] The copolymer of L-lactic acid and D-lactic acid has a copolymerization ratio of D-lactic acid to L-lactic acid (hereinafter abbreviated as "D / L ratio") of preferably 1 / 99 to 10 / 90 or 90 / 10 to 99 / 1, more preferably 3 / 97 to 15 / 85 or 85 / 15 to 97 / 3, even more preferably 5 / 95 to 15 / 85 or 85 / 15 to 95 / 5, particularly preferably 8 / 92 to 15 / 85 or 85 / 15 to 92 / 8, and most preferably 10 / 90 to 15 / 85 or 85 / 15 to 90 / 10. When the copolymerization ratio of D-lactic acid is higher than 97 or less than 3, it tends to show very high crystallinity, have a high melting point, and have excellent heat resistance and mechanical properties. However, when used as a heat shrinkable film, since it usually involves printing and a bag making process using a solvent, it is necessary to moderately reduce the crystallinity of the constituent material itself in order to improve printability and solvent sealability. In addition, if the crystallinity is excessively high, orientation crystallization progresses during stretching, and the film shrinkage characteristics during heating tend to decrease. Furthermore, even if the crystallinity is suppressed by adjusting the stretching conditions, crystallization progresses before shrinkage due to heating during heat shrinkage, and as a result, there is a tendency for shrinkage unevenness and insufficient shrinkage to occur. On the other hand, if the copolymerization ratio of D-lactic acid is less than 85 or higher than 15, the crystallinity is almost completely lost, and as a result, when the labels collide with each other after heat shrinkage, problems such as heat fusion are likely to occur. Therefore, by adjusting the composition ratio of D-lactic acid and L-lactic acid in the polylactic acid resin within the above range, it is possible to obtain a heat shrinkable film with excellent shrinkage characteristics that does not cause the above-mentioned problems.

[0032] The polylactic acid resin used in the present invention can be blended with polylactic acid resins having different D / L ratios, and blending is more preferable because it is easier to adjust the D / L ratio of the polylactic acid resin. In this case, the average D / L ratio of multiple lactic acid polymers should be within the above range. By blending two or more polylactic acid resins having different D / L ratios and adjusting the crystallinity according to the intended use, it is possible to achieve a balance between heat resistance and heat shrinkage properties.

[0033] Furthermore, the polylactic acid resin may be a copolymer with other copolymerization components such as α-hydroxycarboxylic acid, aliphatic diol, and aliphatic dicarboxylic acid, so long as the effects of the present invention are not impaired.

[0034] Examples of the α-hydroxycarboxylic acid include bifunctional aliphatic hydroxycarboxylic acids such as glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxy-n-butyric acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-methyllactic acid, and 2-hydroxycaproic acid, and lactones such as caprolactone, butyrolactone, and valerolactone.

[0035] Examples of the aliphatic diol include ethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol.

[0036] Examples of the aliphatic dicarboxylic acid include succinic acid, adipic acid, suberic acid, sebacic acid, and dodecanedioic acid.

[0037] The copolymerization ratio of lactic acid to other copolymerization components is not particularly limited, but a higher ratio of lactic acid is preferable because it reduces the consumption of petroleum resources. Specifically, the copolymerization ratio (mass ratio) of lactic acid to other copolymerization components is lactic acid:other copolymerization components=95:5 to 10:90, preferably 90:10 to 20:80, and more preferably 80:20 to 30:70. If the copolymerization ratio is within the above range, a film having a good balance of physical properties such as rigidity, transparency, and impact resistance can be obtained.

[0038] As the polymerization method of the polylactic acid resin, known methods such as condensation polymerization and ring-opening polymerization can be adopted. For example, in the condensation polymerization method, D-lactic acid, L-lactic acid, or a mixture thereof can be directly dehydrated and condensed to obtain a polylactic acid resin having an arbitrary composition. In the ring-opening polymerization method, lactide, which is a cyclic dimer of lactic acid, is ring-opened and polymerized in the presence of a predetermined catalyst while using a polymerization regulator or the like as necessary to obtain a polylactic acid resin having an arbitrary composition. The lactide includes DL-lactide, which is a dimer of L-lactic acid, and these are mixed and polymerized as necessary to obtain a polylactic acid resin having an arbitrary composition and crystallinity. Furthermore, a small amount of a chain extender, such as a diisocyanate compound, a diepoxy compound, an acid anhydride, or an acid chloride, may be used for the purpose of increasing the molecular weight.

[0039] The weight (mass) average molecular weight of the polylactic acid resin is 20,000 or more, preferably 40,000 or more, more preferably 60,000 or more, and the upper limit is 400,000 or less, preferably 350,000 or less, more preferably 300,000 or less. If the weight (mass) average molecular weight is 20,000 or more, a suitable resin cohesive force can be obtained, and the film strength and elongation can be prevented from being insufficient or from becoming brittle. On the other hand, if the weight (mass) average molecular weight is 400,000 or less, the melt viscosity can be reduced, which is preferable from the viewpoint of improving production and productivity.

[0040] Commercially available products of the polylactic acid resin include, for example, "NatureWorks" manufactured by Nature Works LLC and "LACEA" manufactured by Mitsui Chemicals.

[0041] The polyester-based resin used in the present invention is preferably the above-mentioned aromatic polyester-based resin or polylactic acid-based resin, but is not limited thereto. For example, it may be composed only of polyethylene terephthalate (homopolyester) composed only of terephthalic acid and ethylene glycol, it may contain the above-mentioned homopolyester and one or more types of copolymer polyesters, it may be composed only of one type of copolymer polyester, or it may contain two or more types of copolymer polyesters having different compositions.

[0042] (Other resins) In addition to the polyester-based resins, the thermoplastic resin layer may further contain at least one other resin, such as (meth)acrylic resins such as ethylene-acrylic acid copolymer (EAA), ethylene-ethyl acrylate copolymer (EEA), ethylene-(meth)acrylic acid copolymer (EMA), and ethylene-methyl(meth)acrylic acid copolymer (EMMA), polyethylene resins, ethylene-vinyl acetate copolymer (EVA), polypropylene resins, polystyrene resins (GPPS (general-purpose polystyrene), HIPS (high-impact polystyrene), SBS (styrene-butadiene copolymer), SIS (styrene-isoprene copolymer), SEBS (styrene-ethylene-butylene-styrene copolymer), SEPS (styrene-ethylene-propylene-styrene copolymer), aliphatic polyester resins excluding polylactic acid resins, aromatic aliphatic polyester resins, copolymers of diol, dicarboxylic acid, and lactic acid resin, core-shell structure rubber, styrene-carboxylic acid copolymer, polyamide resins, and polyoxymethylene resins, within a range that does not significantly impair the effects of the present invention.

[0043] Among them, when a polylactic acid resin is used, it is preferable that the thermoplastic resin layer contains a core-shell structure type rubber, and it is particularly preferable that the core-shell structure type rubber is an acrylic rubber. The core-shell structure type rubber has a double structure formed of a core and a shell, the core part is a soft rubber, and the shell part on the surface is in a hard resin state, and the rubber itself is an elastic body in a powder (particle) state. This core-shell structure type rubber has excellent dispersibility in a polylactic acid resin, for example, because the particle state of the rubber mostly maintains its original shape even after melt-kneading with a polylactic acid resin.

[0044] Commercially available examples of the acrylic core-shell structure rubber include Kane Ace FM-40 and Kane Ace M-570 manufactured by Kaneka Corporation, and Metablen SX-005, Metablen SRK200, Metablen W600A, and Metablen C-223A manufactured by Mitsubishi Chemical Corporation.

[0045] The content of the core-shell structure type rubber is preferably 1% by mass or more, more preferably 5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, based on 100% by mass of the total amount of the thermoplastic resin layer.

[0046] Furthermore, the thermoplastic resin layer may contain recycled resin generated from trimming losses such as edges of a film, within the range that does not significantly impair the effects of the present invention.

[0047] (Additives) Furthermore, the thermoplastic resin layer may contain additives such as hindered phenol-based, phosphite-based, and thioether-based antioxidants, benzotriazole-based, benzophenone-based, benzoate-based, hindered amine-based, and cyanoacrylate-based light stabilizers, inorganic or organic crystal nucleating agents, molecular weight regulators, hydrolysis stabilizers, weather resistance stabilizers, heat resistance stabilizers, melt viscosity improvers, crosslinking agents, antioxidants, antistatic agents, lubricants, release agents, plasticizers, flame retardants, flame retardant assistants, foaming agents, colorants, and dispersing assistants, provided that the effects of the present invention are not impaired.

[0048] The plasticizer is preferable because it can improve the impact resistance, transparency, moldability, and various properties of the heat-shrinkable film. Examples of the plasticizer include fatty acid ester plasticizers, phthalate ester plasticizers, and trimellitate ester plasticizers.

[0049] Specific examples of the fatty acid ester plasticizer include dibutyl adipate, diisobutyl adipate, diisononyl adipate, diisodecyl adipate, di(2-ethylhexyl) adipate, di(n-octyl) adipate, di(n-decyl) adipate, dibutyl diglycol adipate, dibutyl sebacate, di(2-ethylhexyl) sebacate, di(n-hexyl) azelate, di(2-ethylhexyl) azelate, and di(2-ethylhexyl) dodecanedionate.

[0050] Specific examples of the phthalate ester plasticizer include diisononyl phthalate, diisodecyl phthalate, di(2-ethylhexyl) phthalate, etc. Specific examples of the trimellitate ester plasticizer include tri(2-ethylhexyl) trimellitate, etc.

[0051] The method for mixing the additives is not particularly limited, and the additives may be added during the polymerization process of the polyester resin, or may be mixed during the production process of the thermoplastic resin layer.

[0052] The thermoplastic resin layer (film) can be produced by a conventionally known method and is not particularly limited. For example, the thermoplastic resin can be melt-extruded at a temperature of 200°C or higher and 300°C or lower, cut into pellets, and then melt-extruded at a temperature of 200°C or higher and 300°C or lower; or the thermoplastic resin can be melt-extruded at a temperature of 200°C or higher and 300°C or lower.

[0053] The extrusion method is not particularly limited, and a T-die method, a tubular method, etc. can be used. In the case of the T-die method, for example, after extrusion, the film is quenched on a casting drum with a surface temperature of 15°C to 80°C to form an unstretched film. Next, the unstretched film is stretched in a uniaxial direction using a tenter under conditions of a stretching temperature of 60°C to 120°C, preferably 70°C to 100°C, and a stretching ratio of 1.7 times to 7.0 times, preferably 3.0 times to 6.0 times, and then heat-treated at a temperature of 55°C to 100°C, preferably 70°C to 95°C. The film after the heat treatment is usually wound up to form a film roll. In addition, a heated longitudinal stretching roll may be used to stretch the film in the longitudinal direction under conditions of a roll temperature of 60°C to 120°C, preferably 60°C to 100°C, and a stretching ratio of 1.0 times to 1.3 times, preferably 1.0 times to 1.1 times.

[0054] The thickness of the thermoplastic resin layer is 10 μm or more, preferably 20 μm or more, and 100 μm or less, preferably 80 μm or less. If the thickness of the thermoplastic resin layer is the above-mentioned numerical value or more, there is an advantage that secondary processing is easy, and if the thickness of the thermoplastic resin layer is the above-mentioned numerical value or less, good processability of the film can be maintained.

[0055] In addition, the thermoplastic resin layer may be subjected to a surface treatment such as a chemical treatment, a corona discharge treatment, a plasma treatment, an ozone treatment, a chemical treatment, a solvent treatment, etc., in order to improve the coatability and adhesiveness of a coating liquid containing an antistatic agent described below.

[0056] [Antistatic Agent] The film of the present invention has a layer containing an antistatic agent disposed on at least one surface of the thermoplastic resin layer. In particular, it is preferable to have a layer containing an antistatic agent disposed on one surface of the thermoplastic resin layer.

[0057] The antistatic agent may be a cationic antistatic agent, an anionic antistatic agent, an amphoteric antistatic agent, or a nonionic antistatic agent. These antistatic agents may be used alone or in combination of two or more kinds.

[0058] Examples of the cationic antistatic agent include primary amine salts, secondary amine salts, tertiary amine salts, fatty acid amide amine salts, quaternary ammonium salts, alkyl trialkylene glycol ammonium salts, alkyl ether ammonium salts, benzalkonium salts, benzethonium salts, pyridinium salts, imidazolinium salts, etc. Among these, quaternary ammonium salts are preferred, and polyoxyethylene trialkyl ammonium nitrate is particularly preferred.

[0059] Examples of the nonionic antistatic agent include esters having 5 to 25 carbon atoms, such as propylene glycol mono fatty acid esters, ethylene glycol mono fatty acid esters, glycerin mono fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, methyl glycoside fatty acid esters, alkyl polyglucosides, polyoxyethylene mono fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene sorbitol fatty acid esters; ethers having 5 to 25 carbon atoms, such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene cholesterol, polyoxyethylene cholestanol, polyoxyethylene polyoxypropylene alkyl ethers, and polyoxyethylene polyoxypropylene glycol; and amides such as polyoxyethylene fatty acid amides, alkyl diethanol amides, and alkyl amine oxides. Among these, esters having 5 to 25 carbon atoms are preferred, and polyoxyethylene mono fatty acid esters are particularly preferred.

[0060] Examples of the anionic antistatic agent include carboxylates, sulfonates, sulfates, and phosphates, and specifically, metal salts of alkali metals or alkaline earth metals such as alkyl ether carboxylates, fatty acid amide ether carboxylates, acyl lactates, N-acyl glutamates, N-acyl methyl alanines, N-acyl sarcosines, N-acyl-ω-amino acids, alkanesulfonates, α-olefin sulfonates, α-sulfo fatty acid methyl esters, acyl isethionates, alkyl sulfosuccinates, alkyl sulfonates, alkyl benzene sulfonates, alkyl naphthalene sulfonates, N-acyl methyl taurates, formalin condensation sulfates, alkyl sulfates, alkyl ether sulfates, alkyl aryl ether sulfates, fatty acid alkanolamide sulfates, fatty acid monoglyceride sulfates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, alkyl aryl ether phosphates, and fatty acid amide ether phosphates. Among these, alkyl sulfonates are preferred.

[0061] Examples of the amphoteric antistatic agent include aminopropionic acid, carboxybetaine having 5 to 20 carbon atoms, and sulfobetaine.

[0062] The antistatic agent preferably contains at least one of a cationic antistatic agent and an anionic antistatic agent from the viewpoints of antistatic properties and printability.

[0063] When the total amount of the antistatic agent is taken as 100 mass%, the content of at least one of the cationic antistatic agent and the anionic antistatic agent is preferably 35 mass% or more, more preferably 40 mass% or more, and particularly preferably 45 mass% or more, relative to the total amount of the antistatic agent. If the content of at least one of the cationic antistatic agent and the anionic antistatic agent relative to the total amount of the antistatic agent is too small, the antistatic property and printability tend to decrease. Note that the upper limit of the content of at least one of the cationic antistatic agent and the anionic antistatic agent in the total amount of the antistatic agent is usually 100 mass%.

[0064] When the total amount of the antistatic agent is taken as 100 mass %, it is more preferable that the above-mentioned antistatic agent contains a cationic antistatic agent as a main component relative to the total amount of the antistatic agent, and it is particularly preferable that the antistatic agent consists solely of a cationic antistatic agent.

[0065] As described above, the film of the present invention has a layer containing an antistatic agent disposed on at least one surface of the thermoplastic resin layer. From the viewpoint of antistatic properties, it is preferable that the layer containing the antistatic agent is a coating layer.

[0066] The coating layer may be formed by in-line coating or off-line coating, and is preferably formed by in-line coating from the viewpoint of ease of processing.

[0067] The in-line coating is a method of forming a coating layer by applying a coating liquid in which an antistatic agent is dissolved or dispersed in a solvent during the manufacturing process of a thermoplastic resin layer, specifically, a coating liquid is applied to form a coating layer at any stage from melt extrusion of a thermoplastic resin to stretching, heat setting and winding up. Usually, a coating liquid is applied to a thermoplastic resin layer of any of the following: an unstretched sheet obtained by melting and quenching, a stretched film that has been stretched, a stretched film before heat setting, and a film after heat setting and before winding up, to form a coating layer.

[0068] Examples of the method for applying the coating liquid include air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, extrusion coating, and other conventionally known coating methods. Among these, kiss roll coating is preferred.

[0069] The solvent for dissolving or dispersing the antistatic agent is not particularly limited, but is preferably water. By using water as the solvent, an aqueous coating liquid can be prepared.

[0070] The aqueous coating liquid may contain a small amount of an organic solvent. Examples of the organic solvent include alcohols such as ethanol, isopropanol, ethylene glycol, and glycerin, ethers such as ethyl cellosolve, t-butyl cellosolve, propylene glycol monomethyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, esters such as ethyl acetate, and amines such as dimethylethanolamine. These can be used alone or in combination. By appropriately selecting and adding these organic solvents to the aqueous coating liquid as necessary, the stability and coatability of the coating liquid may be improved.

[0071] The content (coating amount) of the active ingredient of the antistatic agent in the coating layer is 0.0012 g / m 2 It is preferable that the content is equal to or more than 0.0015 g / m 2 More preferably, 0.0018 g / m 2 More than 0.015 g / m 2 It is preferable that the content is 0.012 g / m or less, and more preferable that the content is 0.012 g / m or less. 2 Less than 0.010 g / m 2 When the content of the active ingredient of the antistatic agent is equal to or higher than the lower limit, sufficient antistatic performance tends to be obtained, whereas when the content of the active ingredient of the antistatic agent is equal to or lower than the upper limit, the static friction coefficient described below becomes appropriate, and slippage tends to be less likely to occur when the film is rolled.

[0072] The method for producing the film of the present invention is not limited to the following, but for example, a method is preferred in which a coating liquid is applied to an unstretched sheet of a thermoplastic resin layer obtained by quenching, a coating layer is formed, and then the coating layer is stretched in a transverse uniaxial direction. According to this method, since stretching is performed after the coating layer is formed, the thickness of the coating layer can be changed by the stretching ratio, and thin film coating can be performed more easily than offline coating. In addition, the thickness of the coating layer can be made more uniform than offline coating. Furthermore, by providing a coating layer on the thermoplastic resin layer before stretching, the coating layer can be stretched together with the thermoplastic resin layer, thereby allowing the coating layer to adhere firmly to the thermoplastic resin layer.

[0073] [Layer structure of film] The layer structure of the film of the present invention can be appropriately selected as necessary from the viewpoint of required quality, application, etc., and may be a single-layer film of a thermoplastic resin layer, or a multi-layer laminate film in which another resin layer is laminated on a thermoplastic resin layer. In the case of the laminate film, it is necessary that the thermoplastic resin layer is at least one of the outermost layers.

[0074] Examples of methods for forming the laminated film include a co-extrusion method, a method in which films of each layer are formed and then superimposed and heat-sealed, and a method in which the films are joined with an adhesive or the like.

[0075] It is also preferred that the outermost layer of the film of the present invention contains fine particles, since this will provide excellent blocking resistance and lubricity when made into a heat-shrinkable film.

[0076] The fine particles include inorganic fine particles and organic fine particles. Examples of the inorganic fine particles include silica, alumina, titania, kaolin, clay, calcium carbonate, calcium phosphate, lithium fluoride, carbon black, and precipitates resulting from catalysts such as alkali metals, alkaline earth metals, and phosphorus compounds during polyester polymerization. Examples of the organic fine particles include various crosslinked polymers. These fine particles may be used alone or in combination of two or more kinds.

[0077] From the viewpoint of obtaining the effects of blocking resistance and slipperiness, it is desirable that the average particle size of the above-mentioned fine particles is in the range of 0.5 μm or more, preferably 1.0 μm or more, and 10 μm or less, preferably 8 μm or less, and more preferably 5 μm or less. The term "average particle size" used herein refers to the 50% volume average particle size (d50) measured by a method such as laser diffraction, electromagnetic scattering such as dynamic light scattering, or light transmission such as centrifugal sedimentation. When differences arise depending on the measurement method, the value measured by the laser diffraction method is used.

[0078] The content of the above-mentioned fine particles is desirably in the range of 0.005% by mass or more, preferably 0.01% by mass or more, and more preferably 0.02% by mass or more, and 1% by mass or less, preferably 0.6% by mass or less, and more preferably 0.5% by mass or less, when the total mass of the resin layer constituting the outermost layer is taken as 100% by mass.

[0079] The film of the present invention may be subjected to surface treatment or surface processing such as corona treatment, printing, deposition, etc., as well as bag making processing using various solvents or heat sealing, perforation, etc., if necessary. Furthermore, a deposition layer or various coating layers may be provided, if necessary.

[0080] The film of the present invention obtained as described above satisfies the following a) to d). a) The surface resistivity of the layer containing the antistatic agent is 5.0×10 in an atmosphere at a temperature of 23° C. and a relative humidity of 30%. 11 (Ω / sq) or less, and at a temperature of 23°C and a relative humidity of 50%, 1.0×10 11 (Ω / sq) or less b) The static friction coefficient between one surface and the other surface, measured in accordance with JIS K7125, is 0.20 to 0.50 in an atmosphere having a temperature of 23°C and a relative humidity of 50%. c) The shrinkage rate in the main shrinkage direction when immersed in 80°C hot water for 10 seconds is 20% or more. d) Haze value measured according to JIS K7136 is 7% or less

[0081] <Surface resistivity> The surface resistivity of the layer containing the antistatic agent of the film of the present invention is 5.0×10 11 (Ω / sq) or less, preferably 4.7×10 11 (Ω / sq) or less, more preferably 4.5×10 11 If the surface resistivity in an atmosphere of 23°C and 30% relative humidity is the above-mentioned value or less, the antistatic performance is sufficient and the printability is improved.

[0082] The surface resistivity of the layer containing the antistatic agent of the film of the present invention is 1.0×10 11 (Ω / sq) or less, preferably 8.0×10 10 (Ω / sq) or less, and more preferably 5.0×10 10 If the surface resistivity in an atmosphere of a temperature of 23° C. and a relative humidity of 50% is the above-mentioned value or less, the antistatic performance is sufficient and the printability is improved.

[0083] <Static friction coefficient> The film of the present invention has a static friction coefficient between one surface and the other surface of the film in an atmosphere at a temperature of 23° C. and a relative humidity of 50%, according to JIS K7125, of 0.20 or more, preferably 0.22 or more, particularly preferably 0.23 or more, and 0.50 or less, preferably 0.45 or less, particularly preferably 0.40 or less. If the static friction coefficient is the above-mentioned value or more, the film tends to be less likely to slip when rolled, and if the static friction coefficient is the above-mentioned value or less, the film is less likely to have wrinkles or unevenness when rolled, making it easier to unroll the film roll and improving workability.

[0084] <Heat shrinkage rate> The heat shrinkage rate of the film of the present invention in the main shrinkage direction when immersed in 80°C warm water for 10 seconds is 20% or more. The lower limit of the shrinkage rate is preferably 25% or more, more preferably 30% or more. The upper limit is not particularly limited, but is generally preferably 70% or less, more preferably 65% ​​or less, and even more preferably 60% or less. If the heat shrinkage rate in the main shrinkage direction at 80°C is less than 20%, the heat shrinkage may be insufficient at the neck or top surface of the container when the film is heat-shrunk. The above-mentioned "main shrinkage direction" refers to the direction in which the heat shrinkage rate is high when the film is shrunk by applying heat, that is, the direction in which the stretching direction is larger among the vertical and horizontal directions, and is usually the horizontal direction (the direction perpendicular to the vertical direction and the direction in which the film is taken up). In addition, when the film is attached to a bottle, it is, for example, the direction corresponding to the outer circumferential direction.

[0085] <Haze value> The transparency of the film of the present invention is evaluated by the haze value measured in accordance with JIS K7136, and the haze value is 7% or less. It is preferably 6.5% or less, and particularly preferably 6% or less. If the haze value is the above value or less, good transparency can be obtained, and beautiful printing and the like can be achieved.

[0086] Furthermore, it is preferable that the film of the present invention further satisfies the following electrostatic voltage half-life. <Charged voltage half-life> The electrostatic potential half-life of the layer containing the antistatic agent in the film of the present invention is preferably 5 seconds or less, more preferably 3.5 seconds or less, in an atmosphere of a temperature of 23° C. and a relative humidity of 50%, according to JIS L 1094. When the electrostatic potential half-life is the above-mentioned value or less, it tends to be possible to prevent the occurrence of so-called printing whiskers, particularly in the printing process, and winding around a roll in the printing and tubing process.

[0087] The film of the present invention having such physical properties has an antistatic agent having an effective ingredient coating amount of 0.0012 g / m 2 More than 0.015g / m 2or less, and further, when producing the thermoplastic resin layer, the stretching ratio can be set to 1.7 times or more and 7.0 times or less.

[0088] [Molded products, heat-shrinkable labels, containers] The film of the present invention can be processed from a flat shape to a cylindrical shape or the like depending on the packaged item and used for packaging. In the case of cylindrical containers such as PET bottles that require printing, first, a required image is printed on one side of a wide flat film wound on a roll, and then, while cutting it to the required width, it is folded so that the printed side faces inward and center-sealed (the shape of the sealed portion is a so-called envelope-paste) to form a cylindrical shape. Possible center-sealing methods include an organic solvent adhesion method, a heat sealing method, an adhesive method, and an impulse sealer method. Among these, an organic solvent adhesion method is preferably used from the viewpoints of productivity and appearance.

[0089] In addition, since the film of the present invention has excellent transparency, glossiness, and particularly excellent power outage prevention properties even in a low humidity environment, and excellent printability, its uses are not particularly limited, but by laminating a printed layer, a vapor deposition layer, or other functional layers as necessary, it can be used as a base material for various molded products such as bottles (blow bottles), trays, lunch boxes, containers for prepared foods, and containers for dairy products. The obtained molded products can be used as containers, etc.

[0090] Furthermore, the film of the present invention can be used as a substrate for heat-shrinkable labels for food containers (e.g., PET bottles for soft drinks or food, glass bottles, preferably PET bottles). In this case, it is possible to adhere even to containers with complex shapes (e.g., cylinders with a narrowed center, square prisms with corners, pentagonal prisms, hexagonal prisms, etc.), and a beautiful label without wrinkles or pockmarks can be obtained. The above molded products and containers can be produced by using ordinary molding methods.

[0091] Furthermore, the film of the present invention can be suitably used as a heat-shrinkable label material for plastic molded products that deform when heated to high temperatures, as well as a heat-shrinkable label material for plastic packaging (containers) that uses as its constituent material at least one material selected from the group consisting of polyolefin resins such as polyethylene, polypropylene, and polybutene, polymethacrylate resins, polycarbonate resins, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, and polyamide resins, whose thermal expansion coefficients and water absorption properties are extremely different from those of the heat-shrinkable film of the present invention, for example, metal, porcelain, glass, paper, and at least one material selected from the group consisting of polyolefin resins such as polyethylene, polypropylene, and polybutene, polymethacrylate resins, polycarbonate resins, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, and polyamide resins.

[0092] In addition to the above resins, examples of materials constituting the above plastic packaging include polystyrene, rubber-modified impact-resistant polystyrene (HIPS), styrene-butyl acrylate copolymer, styrene-acrylonitrile copolymer, styrene-maleic anhydride copolymer, acrylonitrile-butadiene-styrene copolymer (ABS), (meth)acrylic acid-butadiene-styrene copolymer (MBS), polyvinyl chloride resin, phenol resin, urea resin, melamine resin, epoxy resin, unsaturated polyester resin, silicone resin, etc. These plastic packaging materials may be mixtures or laminates of two or more resins. EXAMPLES

[0093] Examples of the film of the present invention will be shown below, but the present invention is not limited to these examples in any way. The measurements and evaluations shown in the examples were performed as follows: In the examples, the direction in which the film is taken up (flow) is referred to as "MD", and the direction perpendicular thereto is referred to as "TD".

[0094] <Measurement and evaluation methods> (1)Surface resistivity The surface resistivity of the layer containing the antistatic agent of the film obtained in the examples was measured using a digital ultra-high resistance microammeter manufactured by ADC Corporation under conditions of an applied voltage of 500 V, under an atmosphere of temperature 23°C and relative humidity 30% and an atmosphere of temperature 23°C and relative humidity 50%, and was evaluated according to the following criteria. [Atmosphere temperature 23℃, relative humidity 30%] ◎:2.0×10 11 (Ω / sq) or less ○:2.0×10 11 (Ω / sq) exceeds 5.0×10 11 (Ω / sq) or less ×:5.0×10 11 Exceeds (Ω / sq) [Atmosphere temperature 23℃, relative humidity 50%] ◎:5.0×10 10 (Ω / sq) or less ○:5.0×10 10 (Ω / sq) exceeds 1.0×10 11 (Ω / sq) or less ×:1.0×10 11 Exceeds (Ω / sq)

[0095] (2) Coefficient of static friction The static friction coefficient between one surface of the film obtained in the examples and the other surface of the film was measured in accordance with JIS K7125 at a temperature of 23°C and a relative humidity of 50%, and was evaluated according to the following criteria: ◯: Static friction coefficient is 0.20 or more and 0.50 or less. ×: The static friction coefficient is less than 0.20 or more than 0.50.

[0096] (3) Heat shrinkage rate The films obtained in the examples were cut into pieces measuring 20 mm in MD and 100 mm in TD, and the amount of shrinkage in the TD was measured by immersing the pieces in a hot water bath at 80° C. for 10 seconds. The thermal shrinkage rate was expressed as a percentage value, which is the ratio of the amount of shrinkage to the original size before shrinkage.

[0097] (4) Haze value The haze value of the films obtained in the examples was measured in accordance with JIS K7136, and the transparency was evaluated according to the following criteria. ◎: Haze value is 5% or less ○: Haze value is more than 5% and 7% or less ×: Haze value exceeds 7%

[0098] (5) Charge voltage half-life The electrostatic potential half-life of the layer containing the antistatic agent of the film obtained in the examples was measured in accordance with JIS L1094 using a static honest meter manufactured by Shishido Electrostatic Corporation under an atmosphere of temperature 23°C and relative humidity 50%, and was evaluated according to the following criteria. ◎: 3.5 seconds or less ○: More than 3.5 seconds, 5 seconds or less ×: More than 5 seconds

[0099] (6) Overall film rating In the above evaluations (1) to (5), if all the evaluations were "good" or better, the film was evaluated as "good" overall. In addition, if even one of the evaluations (1) to (5) was "bad", the film was evaluated as "bad".

[0100] (7) Printing evaluation (ink loss) After performing solid printing on 1000 m of each film obtained in the examples, a defect detector was used to measure the defect density of 100 m. 2 The number of ink voids measuring 0.5 mm or more that occurred in each test was counted. ○: 5 or less ×:6 or more

[0101] The raw materials and antistatic agents used in the examples and comparative examples are as follows.

[0102] <Thermoplastic resin layer> (Aromatic polyester resin) Polyester resin A (acid component: 100 mol% terephthalic acid, glycol component: 65 mol% ethylene glycol, 3 mol% diethylene glycol, 32 mol% cyclohexanedimethanol) Polyester resin B (acid component: terephthalic acid 70 mol%, isophthalic acid 30 mol%, glycol component: ethylene glycol 100 mol%) Polyester resin C (acid component: terephthalic acid 90 mol%, isophthalic acid 10 mol%, glycol component: 1,4 butanediol 100 mol%) Polyester resin D (acid components: terephthalic acid 95 mol%, isophthalic acid 5 mol%, glycol components: 1,4 butanediol 97 mol%, tetramethylene glycol 3 mol%) (Polylactic acid resin) Polylactic acid resin A (Nature Works LLC, product name: Ingeo biopolymer 4060D, D-form / L-form ratio = 12 / 88) Polylactic acid resin B (Nature Works LLC, product name: Ingeo biopolymer 4043D, D-form / L-form ratio = 4.25 / 95.75) (acrylic rubber) Acrylic rubber (Kaneka Corporation, product name: Kane Ace FM-40, methyl methacrylate copolymer)

[0103] <Antistatic agent> (cationic surfactant) Antistatic agent a (manufactured by Toho Chemical Industry Co., Ltd., product name: Anstex C-200X, active ingredient: polyoxyethylene trialkylammonium nitrate 50% by mass) (Nonionic surfactant) Antistatic agent B (Marubishi Yuka Kogyo Co., Ltd., product name: Denon 733, active ingredient: alkyl alkanolamide-polyoxyethylene polyhydric alcohol fatty acid ester 40% by mass) (Anionic surfactants) Antistatic agent c (Marubishi Yuka Kogyo Co., Ltd., product name: Denon 1895, active ingredient: alkyl sulfonate 30% by weight) (Amphoteric surfactant) Antistatic agent d (Kao Corporation, product name: Electrostripper AC, active ingredients: imidazoline amphoteric surfactant / linear alkylbenzene sulfonic acid sodium salt 25% by mass)

[0104] <Examples 1 and 2, Comparative Examples 1 to 3 and 5> After mixing the raw materials in the formulations shown in Table 1, the materials were melt-kneaded at a set temperature of 270°C using an extruder and a die, and then taken up by a cast roll at 35°C and cooled and solidified to obtain an unstretched sheet. Each antistatic agent was applied to one side of the obtained sheet using a kiss-type roll coater, and then the sheet was stretched 5.0 times in the transverse uniaxial direction using a film tenter at a preheating temperature of 95°C and a stretching temperature of 75°C, and then heat-treated at 75°C to obtain a polyester-based heat-shrinkable film having a thickness of 40 μm. The evaluation results of the obtained film are shown in Table 1. In addition, the films of Examples 1 and 2 and Comparative Examples 1, 3 and 5 were subjected to a printing evaluation. The results of the printing evaluation are shown in Table 2.

[0105] <Examples 3 to 5, Comparative Example 4> After mixing the raw materials in the proportions shown in Table 1, the materials were melt-kneaded using an extruder and die at a set temperature of 200°C, then taken up by a cast roll at 60°C and cooled to solidify, to obtain an unstretched sheet. Each antistatic agent was applied to one side of the obtained sheet using a kiss-type roll coater, and the sheet was then stretched 5.0 times in the transverse uniaxial direction using a film tenter at a preheating temperature of 85°C and a stretching temperature of 85°C, and then heat-treated at 80-85°C to obtain a polylactic acid-based heat-shrinkable film with a thickness of 30 μm. The evaluation results of the obtained film are shown in Table 1.

[0106] [Table 1]

[0107] [Table 2]

[0108] From the results in Table 1 above, it can be seen that the heat shrinkable films obtained according to the present invention (Examples 1 to 5) exhibited sufficient heat shrinkage, had low haze values ​​and excellent transparency, were endowed with appropriate slipperiness, and had excellent antistatic properties, and thus satisfied the required quality required when the heat shrinkable film is processed. On the other hand, the polyester heat-shrinkable film using an amphoteric surfactant (Comparative Example 1), the polyester heat-shrinkable film coated with a specific blend ratio of nonionic and anionic surfactants (Comparative Example 2), the polyester heat-shrinkable film not coated with an antistatic agent (Comparative Example 3), and the polylactic acid heat-shrinkable film coated with a small amount of antistatic agent (Comparative Example 4) showed insufficient antistatic properties such as surface resistivity and half-life of charged voltage. Also, the polyester heat-shrinkable film coated with a large amount of antistatic agent (Comparative Example 5) resulted in a friction coefficient outside the range of the present invention.

[0109] Furthermore, from the results in Table 2, the films of Examples 1 and 2 had excellent antistatic properties, and the films were less likely to become charged during the printing process. This prevented dirt, dust, and the like from adhering to the film surface and being wound up in the rolled film, and reduced the resulting ink loss (number of pieces). In contrast, the films of Comparative Examples 1 and 3 did not have sufficient antistatic properties, and the films were more likely to become charged during the printing process, which increased the adhesion of dirt, dust, and the like to the film surface and the winding up of the rolled film, resulting in a large number of ink loss (number of pieces). In addition, in the case of the film of Comparative Example 5, the static friction coefficient was too low in the printing process, so that the film in roll form shifted when handled, and handling was poor during printing processing, making it impossible to print. The films of Examples 3 to 5, for which no printing evaluation was performed, are also presumed to have the same printability as those of Examples 1 and 2, since they have the physical properties specified in the present invention.

[0110] The present invention has been described above in relation to the embodiment that is considered to be the most practical and preferable at present. However, the present invention is not limited to the embodiment disclosed in the specification of this application, and can be modified as appropriate within the scope of the claims and the gist or concept of the invention that can be read from the specification as a whole, and films with such modifications should also be understood to be included within the technical scope of the present invention. [Industrial Applicability]

[0111] The heat-shrinkable film of the present invention can be suitably used as a heat-shrinkable film having excellent transparency, gloss, antistatic properties even in a low humidity environment, and excellent printability.

Claims

1. A heat-shrinkable film comprising a layer containing 70% by mass or more of a polyester resin and a coating layer containing an antistatic agent on at least one surface of the layer, the film satisfying the following a) and c), and the content of the active ingredient of the antistatic agent in the coating layer is 0.0012 g / m 2 0.015g / m or more 2 A heat shrinkable film that is: a) The surface resistivity of the coating layer is 5.0×10 at a temperature of 23° C. and a relative humidity of 30%. 11 (Ω / sq) or less, and at a temperature of 23° C. and a relative humidity of 50% in an atmosphere, 11 (Ω / sq) or less c) The shrinkage rate in the main shrinkage direction when immersed in 80°C warm water for 10 seconds is 20% or more.

2. 2. The heat shrinkable film according to claim 1, wherein at least one of a cationic antistatic agent and an anionic antistatic agent is present in an amount of 35% by mass or more relative to the total amount of the antistatic agents, where the total amount of the antistatic agents is taken as 100% by mass.

3. 3. The heat-shrinkable film according to claim 1, wherein the static friction coefficient between one surface and the other surface of the heat-shrinkable film, as measured in accordance with JIS K7125, is 0.20 or more and 0.50 or less in an atmosphere having a temperature of 23°C and a relative humidity of 50%.

4. The heat shrinkable film according to any one of claims 1 to 3, which has a haze value of 7% or less as measured in accordance with JIS K7136.

5. The heat shrinkable film according to any one of claims 1 to 4, wherein the coating layer has a half-life of electrostatic potential measured in accordance with JIS L1094 of 5 seconds or less in an atmosphere having a temperature of 23°C and a relative humidity of 50%.

6. The heat-shrinkable film according to any one of claims 1 to 5, wherein the polyester-based resin is an aromatic polyester-based resin or a polylactic acid-based resin.

7. The heat-shrinkable film according to claim 6, wherein the aromatic polyester-based resin is a copolymer polyester-based resin and contains, as a copolymer component, at least one selected from the group consisting of 1,4-butanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, 1,4-cyclohexanedimethanol, 1,3-propanediol, and isophthalic acid.

8. The heat-shrinkable film according to claim 6, wherein the polylactic acid-based resin is a copolymer of D-lactic acid and L-lactic acid, and the D / L ratio of D-lactic acid to L-lactic acid is D / L = 1 / 99 to 10 / 90, or 90 / 10 to 99 / 1.

9. A molded product using the heat shrinkable film according to any one of claims 1 to 8 as a substrate.

10. A heat-shrinkable label using the heat-shrinkable film according to any one of claims 1 to 8 as a substrate.

11. A container having attached thereto the molded article according to claim 9 or the heat-shrinkable label according to claim 10.

Citation Information

Patent Citations

  • Transmission type screen and back projection type display device using same

    JP1992018534A

  • Packing material for group packaging of small boxes

    JP1995005733U

  • Shrinkable Anti-static resin film and its production

    JP2001131317A

  • Polylactic acid-based biaxially oriented film with excellent antistaticity and method for producing the same

    JP2002012687A