Semiconductor device and its manufacturing method
The semiconductor device with balanced n-type and p-type carbon nanotube layers addresses the narrow noise margin issue in CNT-FETs, achieving improved signal integrity and performance in RFID tags.
Patent Information
- Application Number
- JP2021012739
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-17
- Filing Date
- 2021-01-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Existing RFID tag technologies using carbon nanotube field-effect transistors (CNT-FETs) face challenges with narrow noise margins in complementary semiconductor devices, which affect signal integrity and device performance.
A semiconductor device configuration featuring both n-type and p-type semiconductor elements, each with carbon nanotube layers of specific lengths and distances, is designed to enhance noise margin by equalizing electrical characteristics.
The configuration results in a complementary semiconductor device with a wide noise margin, ensuring stable and reliable operation by balancing the electrical properties of n-type and p-type elements.
Smart Images

Figure 0007589569000006 
Figure 0007589569000007 
Figure 0007589569000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device and a manufacturing method thereof. [Background technology]
[0002] In recent years, wireless communication systems using RFID (Radio Frequency IDentification) technology have been attracting attention as devices using field effect transistors (hereinafter referred to as FETs). RFID tags have an IC chip with a circuit composed of FETs, and an antenna for wireless communication with a reader / writer. The antenna installed in the tag receives a carrier wave transmitted from the reader / writer, and the driving circuit in the IC chip operates.
[0003] RFID tags are expected to be used for a variety of purposes, including logistics management, product management, and shoplifting prevention, and are already being introduced in some areas, such as in IC cards for transportation cards and product tags.
[0004] In order for RFID tags to be used in all kinds of products in the future, it will be necessary to reduce manufacturing costs, and the use of inexpensive processes that use coating and printing technologies in their production is being considered.
[0005] For example, in the case of transistors in drive circuits within IC chips, FETs using carbon nanotubes (CNTs) or organic semiconductors, to which inkjet technology or screen printing technology can be applied, are being actively studied.
[0006] Incidentally, the drive circuit in the IC chip is composed of at least a memory circuit for storing data, a rectifier circuit for generating a power supply voltage from an AC signal transmitted from a reader / writer, and a logic circuit for demodulating the AC signal and reading out the data stored in the memory circuit. Among them, the logic circuit is generally composed of a complementary semiconductor device consisting of a p-type FET and an n-type FET in order to reduce its power consumption.
[0007] However, it is known that FETs using CNTs (hereinafter referred to as CNT-FETs) usually exhibit the characteristics of a p-type semiconductor element in the atmosphere. Therefore, it has been considered to convert the characteristics of a CNT-FET to an n-type semiconductor element by forming an n-type modified polymer on a semiconductor layer containing CNTs or by forming a second insulating layer containing an electron donor compound having at least one selected from nitrogen atoms and phosphorus atoms (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2009 / 139339 [Patent Document 2] International Publication No. 2018 / 180146 Summary of the Invention [Problem to be solved by the invention]
[0009] However, the techniques described in Patent Documents 1 and 2 have a problem in that when a complementary semiconductor device is assembled, the noise margin of the output signal relative to the input signal is narrow.
[0010] SUMMARY OF THE PRESENT EMBODIMENT In view of the above problems, an object of the present invention is to provide a complementary semiconductor device having a wide noise margin. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention has the following configuration. That is, the present invention provides: A semiconductor device having a first semiconductor element and a second semiconductor element provided on a substrate having an insulating surface, the first semiconductor element is an n-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a first semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the first semiconductor layer from the gate electrode; Including, The second semiconductor element is A source electrode; A drain electrode; A gate electrode; a second semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the second semiconductor layer from the gate electrode; Including, the first semiconductor layer and the second semiconductor layer both contain carbon nanotubes; The first semiconductor layer 1 μm 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the second semiconductor layer is divided by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element, and the value (Cn / Ln) is 2 The semiconductor device is characterized in that the total length (Cp) of the carbon nanotubes present per unit area is different from the value (Cp / Lp) obtained by dividing the total length (Cp) of the carbon nanotubes present per unit area by the distance (Lp) between the source electrode and drain electrode of the second semiconductor element.
[0012] The semiconductor device of the present invention further comprises: A semiconductor device having a first semiconductor element and a second semiconductor element provided on a substrate having an insulating surface, the first semiconductor element is an n-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a first semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the first semiconductor layer from the gate electrode; Including, the second semiconductor element is a p-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a second semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the second semiconductor layer from the gate electrode; Including, the first semiconductor layer and the second semiconductor layer both contain carbon nanotubes; The first semiconductor layer 1 μm 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the second semiconductor layer 2 The semiconductor device is characterized in that the total length (Cp) of the carbon nanotubes present per unit area is different from the total length (Cp) of the carbon nanotubes present per unit area. Effect of the Invention
[0013] According to the present invention, it is possible to provide a complementary semiconductor device having a wide noise margin. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic cross-sectional view showing a first semiconductor element in the semiconductor device according to the first embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a second semiconductor element in the semiconductor device according to the first embodiment of the present invention; [Diagram 3] FIG. 11 is a schematic cross-sectional view showing a first semiconductor element in a semiconductor device according to a third embodiment of the present invention. [Figure 4A] FIG. 2 is a schematic diagram illustrating the function of a semiconductor device according to an embodiment of the present invention; [Figure 4B] FIG. 1 is a diagram showing an example of transfer characteristics of a semiconductor device according to an embodiment of the present invention. [Diagram 5] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a semiconductor device according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] One embodiment of the semiconductor device according to the present invention has a first semiconductor element which is an n-type semiconductor element and a second semiconductor element which is a p-type semiconductor element, the semiconductor layers of both semiconductor elements contain carbon nanotubes, and the semiconductor layer of the first semiconductor element is 1 μm thick. 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the semiconductor layer of the second semiconductor element is determined by dividing the total length (Cn) of the carbon nanotubes by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element. 2 This is different from the value (Cp / Lp) obtained by dividing the total length (Cp) of the carbon nanotubes present per unit area by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element.
[0016] In addition, one embodiment of the semiconductor device according to the present invention has a first semiconductor element which is an n-type semiconductor element and a second semiconductor element which is a p-type semiconductor element, the semiconductor layers of both semiconductor elements contain carbon nanotubes, and 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the semiconductor layer of the second semiconductor element 2 This is different from the total length (Cp) of the carbon nanotubes present per unit area.
[0017] With the configuration according to each of the above embodiments, it is possible to provide a complementary semiconductor device with a wide noise margin.
[0018] Hereinafter, preferred embodiments of the semiconductor device and the manufacturing method thereof according to the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be modified in various ways depending on the purpose and application.
[0019] (Embodiment 1) The semiconductor device according to the first embodiment of the present invention is a semiconductor device in which the first semiconductor element further includes a second insulating layer in contact with the first semiconductor layer on the side opposite to the gate insulating layer with respect to the first semiconductor layer.
[0020] <First semiconductor element> The first semiconductor element is provided on a substrate having an insulating surface, and comprises a source electrode, a drain electrode, a gate electrode, a first semiconductor layer in contact with the source electrode and the drain electrode, a gate insulating layer that insulates the first semiconductor layer from the gate electrode, and a second insulating layer in contact with the first semiconductor layer on the opposite side of the gate insulating layer with respect to the first semiconductor layer, and the first semiconductor layer contains carbon nanotubes.
[0021] 1 is a schematic cross-sectional view showing an example of a first semiconductor element. This semiconductor element 1 has a gate electrode 11 formed on a substrate 10, a gate insulating layer 12 covering it, a source electrode 13 and a drain electrode 14 provided thereon, a first semiconductor layer 15 provided between these electrodes, and a second insulating layer 16 on the upper side of the first semiconductor layer 15 to cover the first semiconductor layer. The first semiconductor layer 15 contains carbon nanotubes (hereinafter referred to as "CNTs").
[0022] The structure of the first semiconductor element 1 is a so-called bottom gate bottom contact structure in which the gate electrode 11 is disposed on the lower side (substrate 10 side) of the first semiconductor layer 15, and the source electrode 13 and the drain electrode 14 are disposed on the lower surface of the first semiconductor layer 15. However, the structure of the first semiconductor element is not limited to this, and may be, for example, a so-called top gate structure in which the gate electrode 11 is disposed on the upper side (opposite the substrate 10) of the first semiconductor layer 15, or a so-called top contact structure in which the source electrode 13 and the drain electrode 14 are disposed on the upper surface of the first semiconductor layer 15.
[0023] (Substrate having an insulating surface) The substrate having an insulating surface of the first semiconductor element may be made of any material as long as at least the surface on which the electrode system is disposed is insulating. For example, inorganic materials such as silicon wafer, glass, sapphire, and alumina sintered body, and organic materials such as polyimide, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane, polyvinylphenol (PVP), polyester, polycarbonate, polysulfone, polyethersulfone, polyethylene, polyphenylene sulfide, and polyparaxylene are preferably used. In addition, it may be a laminate of multiple materials, such as a PVP film formed on a silicon wafer or a polysiloxane film formed on polyethylene terephthalate.
[0024] (Source electrode, drain electrode, gate electrode) The material used for the source electrode, drain electrode and gate electrode of the first semiconductor element may be any conductive material that can be generally used as an electrode. Examples of such conductive materials include conductive metal oxides such as tin oxide, indium oxide and indium tin oxide (ITO). In addition, examples of such conductive materials include metals such as platinum, gold, silver, copper, iron, tin, zinc, aluminum, indium, chromium, lithium, sodium, potassium, cesium, calcium, magnesium, palladium, molybdenum, amorphous silicon and polysilicon, alloys of a plurality of metals selected from these, and inorganic conductive materials such as copper iodide and copper sulfide. In addition, examples of such conductive materials include polythiophene, polypyrrole, polyaniline, a complex of polyethylenedioxythiophene and polystyrenesulfonic acid, and conductive polymers whose conductivity is improved by doping with iodine or the like. In addition, examples of such conductive materials include carbon materials and materials containing an organic component and a conductor.
[0025] A material containing an organic component and a conductor increases the flexibility of the electrode, and has good adhesion and electrical connection even when bent. The organic component is not particularly limited, but may be a monomer, an oligomer or a polymer, a photopolymerization initiator, a plasticizer, a leveling agent, a surfactant, a silane coupling agent, an antifoaming agent, a pigment, etc. From the viewpoint of improving the bending resistance of the electrode, an oligomer or a polymer is preferable. However, the conductive material of the electrode and the wiring is not limited to these. These conductive materials may be used alone, or a plurality of materials may be laminated or mixed.
[0026] The electrode can be formed using a known method, for example, as described in International Publication No. 2018 / 180146.
[0027] The distance 100 (Ln) between the source electrode and the drain electrode of the first semiconductor element is not particularly limited, but is preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 100 μm or less. By setting the distance within this range, the characteristics of the semiconductor element are further improved. The distance between the electrodes can be measured using an optical microscope, a scanning electron microscope (SEM), or the like.
[0028] In addition, wiring may be formed to electrically connect the plurality of first semiconductor elements. The material used for the wiring may be any conductive material that can be generally used as an electrode. For example, the same materials as the electrode materials described above may be used.
[0029] The method for forming the wiring and the method for forming the wiring in a pattern are not particularly limited as long as they are a method that can provide electrical continuity, and examples thereof include the same methods as those for the electrode materials described above.
[0030] (Gate insulation layer) The material used for the gate insulating layer is not particularly limited, but may include inorganic materials such as silicon oxide and alumina; organic polymer materials such as polyimide, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane, and polyvinylphenol (PVP); or a mixture of inorganic material powder and organic material. Among organic materials, those containing organic compounds containing silicon-carbon bonds are preferred from the viewpoint of adhesion to the substrate and electrodes.
[0031] An example of an organic compound containing a silicon-carbon bond is polysiloxane, etc. Polysiloxane is more preferred because it has high insulating properties and can be cured at a low temperature.
[0032] The thickness of the gate insulating layer of the first semiconductor element is preferably 0.05 to 5 μm, more preferably 0.1 to 1 μm. By setting the thickness within this range, it becomes easy to form a uniform thin film. The thickness can be measured by an atomic force microscope, an ellipsometry method, or the like.
[0033] The method for producing the gate insulating layer of the first semiconductor element is not particularly limited, but for example, a method of applying a composition containing a material for forming the gate insulating layer to a substrate, drying the composition, and heat-treating the resulting coating film as necessary can be mentioned. Examples of the application method include known application methods such as spin coating, blade coating, slit die coating, screen printing, bar coater, casting, print transfer, immersion and pulling, and inkjet. The temperature for heat-treating the coating film is preferably in the range of 100 to 300°C.
[0034] The gate insulating layer may be a single layer or multiple layers. In addition, one layer may be formed from multiple insulating materials, or multiple insulating materials may be stacked to form multiple gate insulating layers.
[0035] (First Semiconductor Layer) The first semiconductor layer contains CNTs. The CNTs may be single-walled CNTs in which one carbon film (graphene sheet) is wound in a cylindrical shape, double-walled CNTs in which two graphene sheets are wound concentrically, or multi-walled CNTs in which multiple graphene sheets are wound concentrically. However, to obtain high semiconductor properties, it is preferable to use single-walled CNTs. CNTs can be obtained by arc discharge, chemical vapor deposition (CVD), laser ablation, etc.
[0036] Moreover, it is more preferable that the CNT contains 80% by weight or more of semiconducting CNT. More preferably, it contains 95% by weight or more of semiconducting CNT. As a method for obtaining 80% by weight or more of semiconducting CNT, a known method can be used. For example, there are a method of ultracentrifugation in the presence of a density gradient agent, a method of selectively attaching a specific compound to the surface of semiconducting or metallic CNT and separating the CNT by utilizing the difference in solubility, and a method of separating the CNT by electrophoresis by utilizing the difference in electrical properties. As a method for measuring the content of semiconducting CNT, there are a method of calculating the content from the absorption area ratio of the visible-near infrared absorption spectrum, a method of calculating the content from the intensity ratio of the Raman spectrum, and the like.
[0037] The length of one CNT is preferably shorter than the distance between the source electrode and the drain electrode (hereinafter simply referred to as the "electrode distance"). The average length of the CNTs is preferably 2 μm or less, although it depends on the electrode distance.
[0038] The average length of CNTs refers to the average length of 20 randomly picked CNTs. One method for measuring the average length of CNTs is to randomly pick up 20 CNTs from an image obtained by an atomic force microscope and calculate the average length of these.
[0039] Generally, commercially available CNTs have a distribution in length and may contain CNTs longer than the distance between the electrodes, so it is preferable to add a process to make the length of the CNTs shorter than the distance between the electrodes. For example, a method of cutting the CNTs into short fibers by acid treatment with nitric acid, sulfuric acid, or the like, ultrasonic treatment, or freeze-pulverization is effective. In addition, it is more preferable to use separation by a filter in order to improve the purity of the CNTs.
[0040] The diameter of the CNT is not particularly limited, but is preferably 1 nm or more and 100 nm or less, more preferably 50 nm or less, and further preferably 5 nm or less.
[0041] In addition, it is preferable to use a CNT composite having a conjugated polymer attached to at least a part of the surface of the CNT. A conjugated polymer refers to a compound whose repeating unit has a conjugated structure and has a degree of polymerization of 2 or more.
[0042] A state in which a conjugated polymer is attached to at least a part of the surface of a CNT means that a part or the entire surface of the CNT is covered with the conjugated polymer. It is speculated that the reason why a conjugated polymer can cover a CNT is that the π-electron clouds derived from the conjugated structures of both overlap, resulting in an interaction. Whether or not a CNT is covered with a conjugated polymer can be determined by checking whether the reflected color of the covered CNT approaches that of the conjugated polymer from that of the uncovered CNT. The presence of the deposit and the weight ratio of the deposit to the CNT can be quantitatively identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS).
[0043] By attaching a conjugated polymer to at least a portion of the CNT surface, it becomes possible to uniformly disperse the CNT in a solution without impairing the high electrical properties of the CNT. It also becomes possible to form a uniformly dispersed CNT film by coating the solution in which the CNTs are uniformly dispersed. This makes it possible to achieve high semiconducting properties.
[0044] Methods for attaching a conjugated polymer to CNT include (I) a method of adding CNT to a molten conjugated polymer and mixing, (II) a method of dissolving a conjugated polymer in a solvent, adding CNT to the solution, and mixing, (III) a method of preliminarily dispersing CNT in a solvent using ultrasonic waves or the like, adding a conjugated polymer thereto, and mixing, and (IV) a method of putting a conjugated polymer and CNT in a solvent, irradiating the mixture with ultrasonic waves, and mixing them. In the present invention, any of these methods may be used, or a combination of multiple methods may be used.
[0045] Examples of conjugated polymers include, but are not limited to, polythiophene-based polymers, polypyrrole-based polymers, polyaniline-based polymers, polyacetylene-based polymers, poly-p-phenylene-based polymers, and poly-p-phenylenevinylene-based polymers. The above-mentioned polymers are preferably those in which a single monomer unit is arranged, but those in which different monomer units are block-copolymerized or random-copolymerized may also be used. Graft-polymerized polymers may also be used.
[0046] Among the above polymers, in the present invention, polythiophene-based polymers are preferably used because they are easily attached to CNTs and easily form CNT composites. More preferred are those containing a condensed heteroaryl unit having a nitrogen-containing double bond in the ring and a thiophene unit in the repeating unit.
[0047] As the condensed heteroaryl unit having a nitrogen-containing double bond in the ring, a benzothiadiazole unit or a quinoxaline unit is particularly preferable. By having these units, the adhesion between the CNT and the conjugated polymer is increased, and the CNT can be more satisfactorily dispersed in the semiconductor layer.
[0048] The semiconductor layer may further contain an organic semiconductor or an insulating material as long as the electrical properties are not impaired. The thickness of the semiconductor layer is preferably 1 nm or more and 100 nm or less. Within this range, it is easy to form a uniform thin film. More preferably, it is 1 nm or more and 50 nm or less, and even more preferably, it is 1 nm or more and 20 nm or less. The thickness can be measured by an atomic force microscope.
[0049] As a method for forming the semiconductor layer, a dry method such as resistance heating deposition, electron beam, sputtering, and CVD can be used, but a coating method is preferably used from the viewpoint of manufacturing cost and suitability for large areas. Specifically, a spin coating method, a blade coating method, a slit die coating method, a screen printing method, a bar coater method, a mold method, a print transfer method, a dip and pull method, an inkjet method, and the like can be preferably used, and a coating method can be selected according to the coating film properties to be obtained, such as coating film thickness control and orientation control. In addition, the formed coating film may be annealed in air, under reduced pressure, or in an inert gas atmosphere such as nitrogen or argon.
[0050] (Second insulating layer) The second insulating layer is formed on the side of the semiconductor layer opposite to the side on which the gate insulating layer is formed. The side opposite to the side on which the gate insulating layer is formed on the semiconductor layer refers to the upper side of the semiconductor layer, for example, when the gate insulating layer is formed on the lower side of the semiconductor layer. By forming the second insulating layer, a CNT-FET that normally exhibits p-type semiconductor characteristics can be converted into a semiconductor element that exhibits n-type semiconductor characteristics.
[0051] The second insulating layer preferably contains an organic compound containing a bond between a carbon atom and a nitrogen atom. Any organic compound may be used as such an organic compound, and examples of such an organic compound include amide-based compounds, imide-based compounds, urea-based compounds, amine-based compounds, imine-based compounds, aniline-based compounds, and nitrile-based compounds. In particular, the second insulating layer preferably contains (a) a compound having a structure in which at least one group represented by general formula (1) and at least one group represented by general formula (2) are bonded to one carbon-carbon double bond or one conjugated system, and (b) a polymer.
[0052] In compound (a), at least one group represented by general formula (1) and at least one group represented by general formula (2) are bonded to one carbon-carbon double bond or one conjugated system, so that the electron density of the π orbital of one carbon-carbon double bond or one conjugated system is high. Furthermore, since a structure such as one carbon-carbon double bond or one conjugated system is prone to π-π interaction or charge transfer interaction with CNT, compound (a) strongly interacts electronically with CNT, and it is presumed that CNT-FETs that normally exhibit p-type semiconductor properties can be converted into semiconductor elements that exhibit stable n-type semiconductor properties.
[0053] Furthermore, since the second insulating layer contains the (b) polymer, it is believed that the field where the (a) compound interacts with the CNT can be kept stable, which is likely to result in more stable n-type semiconductor characteristics.
[0054] [ka]
[0055] In the general formulas (1) and (2), R 1 R represents a structure selected from a hydrogen atom, an alkyl group, and a cycloalkyl group. 2 ~R 4 each independently represents a structure selected from a hydrogen atom, an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, and a heteroaryl group. 1 ~R 4 Any two of the groups represented by general formula (1) and (2) may form a ring structure. 1 ~R 4 may be the same or different from each other.
[0056] The alkyl group refers to a saturated aliphatic hydrocarbon group, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, etc., which may or may not have a substituent. The number of carbon atoms in the alkyl group is not particularly limited, but from the viewpoints of availability and cost, it is preferably 1 to 20, more preferably 1 to 8.
[0057] The cycloalkyl group refers to a saturated alicyclic hydrocarbon group such as a cyclopropyl group, a cyclohexyl group, a norbornyl group, or an adamantyl group. The cycloalkyl group may or may not have a substituent. The number of carbon atoms in the cycloalkyl group is not particularly limited, but is preferably in the range of 3 to 20.
[0058] The alkenyl group refers to an unsaturated aliphatic hydrocarbon group containing a double bond, such as a vinyl group, an allyl group, or a butadienyl group, which may or may not have a substituent. The number of carbon atoms in the alkenyl group is not particularly limited, but is preferably in the range of 2 to 20.
[0059] The cycloalkenyl group refers to an unsaturated alicyclic hydrocarbon group containing a double bond, such as a cyclopentenyl group, a cyclopentadienyl group, or a cyclohexenyl group. The cycloalkenyl group may or may not have a substituent. The number of carbon atoms in the cycloalkenyl group is not particularly limited, but is preferably in the range of 3 to 20.
[0060] The alkynyl group refers to an unsaturated aliphatic hydrocarbon group containing a triple bond, such as an ethynyl group. The alkynyl group may or may not have a substituent. The number of carbon atoms in the alkynyl group is not particularly limited, but is preferably in the range of 2 to 20.
[0061] The aryl group refers to an aromatic hydrocarbon group such as a phenyl group, a naphthyl group, a biphenyl group, an anthracenyl group, a phenanthryl group, a terphenyl group, or a pyrenyl group. The aryl group may or may not have a substituent. The number of carbon atoms in the aryl group is not particularly limited, but is preferably in the range of 6 to 40.
[0062] The heteroaryl group refers to an aromatic group having one or more atoms other than carbon in the ring, such as a furanyl group, a thiophenyl group, a benzofuranyl group, a dibenzofuranyl group, a pyridyl group, a quinolinyl group, etc. The heteroaryl group may or may not have a substituent. The number of carbon atoms in the heteroaryl group is not particularly limited, but is preferably in the range of 2 to 30.
[0063] R 1 ~R 4 The case where any two of the groups form a ring structure is, for example, R 1 and R 2 Or, R 1 and R 3 and are bonded to each other to form a conjugated or non-conjugated ring structure. The ring structure may contain, in addition to carbon atoms, nitrogen, oxygen, sulfur, phosphorus, and silicon atoms. The ring structure may also be condensed with another ring.
[0064] A conjugated system is a system in which two or more multiple bonds are conjugated, and the π electrons of the multiple bonds interact with each other through single bonds and are delocalized. For example, it is a structure in which double bonds and / or triple bonds are connected by atoms having single bonds, unshared electron pairs, or empty p orbitals, and specific examples are shown in general formulas (3) to (5).
[0065] [ka]
[0066] Examples of compounds in which at least one group represented by general formula (1) and at least one group represented by general formula (2) are bonded to one conjugated system include compounds represented by general formulas (6) to (9). Note that the structure corresponding to one conjugated system is covered with a dotted line.
[0067] [ka]
[0068] Examples of the (a) compound include tetrakis(dimethylamino)ethylene, 4-((2-dimethylamino)vinyl)-N,N-dimethylaniline, 1,2-phenylenediamine, 1,4-phenylenediamine, 2,3,5,6-tetramethyl-1,4-phenylenediamine, N,N-dimethyl-1,4-phenylenediamine, N,N-dimethyl-N',N'-diphenyl-1,4-phenylenediamine, N,N,N'-trimethyl-N'-phenyl-1,4-phenylenediamine, N,N,N'-trimethyl-1,4-phenylenediamine, N,N,N',N'-tetramethyl ethyl-1,4-phenylenediamine, N,N-bis(methoxymethyl)-N',N'-dimethyl-1,4-phenylenediamine, 5,10-dihydro-5,10-dimethylphenazine, benzidine, 3,3',5,5'-tetramethylbenzidine, N,N,N',N'-tetramethylbenzidine, 4-(pyrrolidin-1-yl)aniline, 4-(4-methylpiperidin-1-yl)aniline, 2,4-dipiperidin-1-yl-phenylamine, tris[4-(diethylamino)phenyl]amine, N,N,N',N'-tetrakis[4-(diisobutylamino)phenyl]-1,4-phenylenediamine, 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, etc. The compounds may be used alone or in combination.
[0069] Methods for analyzing the (a) compound or (b) polymer in the second insulating layer include a method in which a sample obtained by extracting the composition of the second insulating layer from a semiconductor element is analyzed using nuclear magnetic resonance (NMR) or a method in which the second insulating layer is analyzed using XPS or the like.
[0070] The thickness of the second insulating layer is preferably 500 nm or more, more preferably 1.0 μm or more, even more preferably 3.0 μm or more, and particularly preferably 10 μm or more. By setting the thickness within this range, the stability of the characteristics of the semiconductor element is further improved. The upper limit is not particularly limited, but is preferably 500 μm or less.
[0071] The film thickness of the second insulating layer is determined by measuring a cross section of the second insulating layer using a scanning electron microscope, calculating the film thickness at 10 points randomly selected from the portion of the second insulating layer located on the semiconductor layer in the obtained image, and calculating the arithmetic average value.
[0072] The second insulating layer may contain other compounds in addition to the compound (a) and the polymer (b), such as a thickener or a thixotropic agent for adjusting the viscosity or rheology of the solution when the second insulating layer is formed by coating.
[0073] The second insulating layer may be a single layer or multiple layers. In the case of multiple layers, as long as at least the layer containing the compound (a) is in contact with the semiconductor layer, at least one layer may contain the compound (a) and the polymer (b), or the compound (a) and the polymer (b) may be contained in separate layers. For example, a configuration in which a first layer containing the compound (a) is formed on the semiconductor layer, and a second layer containing the polymer (b) is formed thereon can be mentioned.
[0074] The method for forming the second insulating layer is not particularly limited, and dry methods such as resistance heating deposition, electron beam, sputtering, and CVD can be used, but it is preferable to use a coating method from the viewpoint of manufacturing costs and suitability for large areas. Specific examples of coating methods that can be preferably used include spin coating, blade coating, slit die coating, screen printing, bar coater, mold method, print transfer method, immersion and pulling method, inkjet method, and drop casting method. The coating method can be selected depending on the coating film properties to be obtained, such as coating film thickness control and orientation control.
[0075] (protective layer) The first semiconductor element may further have a protective layer on the second insulating layer, the role of which is to protect the semiconductor element from physical damage such as rubbing and from moisture and oxygen in the air.
[0076] Examples of materials for the protective layer include inorganic materials such as silicon wafer, glass, sapphire, and sintered alumina, and organic materials such as polyimide, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane, polyvinylphenol, polyester, polycarbonate, polysulfone, polyethersulfone, polyethylene, polyphenylene sulfide, polyparaxylene, polyacrylonitrile, and cycloolefin polymer. Also, the protective layer may be a laminate of a plurality of materials, such as a polyvinylphenol film formed on a silicon wafer or an aluminum oxide film formed on polyethylene terephthalate.
[0077] In a semiconductor device, the current flowing between the source electrode and the drain electrode (source-drain current) can be controlled by changing the gate voltage. The mobility μ (cm 2 / V s) can be calculated using the following formula:
[0078] μ=(δId / δVg)L·D / (W·εr·ε·Vsd) where Id is the source-drain current (A), Vsd is the source-drain voltage (V), Vg is the gate voltage (V), D is the thickness of the gate insulating layer (m), L is the channel length (m), W is the channel width (m), εr is the relative dielectric constant of the gate insulating layer (F / m), and ε is the dielectric constant of vacuum (8.85×10 -12 F / m), and δ indicates the change in the corresponding physical quantity.
[0079] Moreover, the threshold voltage of the semiconductor element can be obtained from the intersection point between the extension line of the linear portion of the Id-Vg graph and the Vg axis.
[0080] A semiconductor element having a small absolute value of the threshold voltage and high mobility is highly functional and has good characteristics.
[0081] <Second semiconductor element> The second semiconductor element is provided on a substrate having an insulating surface, and includes a source electrode, a drain electrode, a gate electrode, a second semiconductor layer in contact with the source electrode and the drain electrode, and a gate insulating layer that insulates the second semiconductor layer from the gate electrode, and the second semiconductor layer contains CNTs.
[0082] 2 is a schematic cross-sectional view showing an example of a second semiconductor element. This semiconductor element 2 has a gate electrode 21 formed on a substrate 20, a gate insulating layer 22 covering it, a source electrode 23 and a drain electrode 24 provided thereon, and a second semiconductor layer 25 provided between these electrodes. The second semiconductor layer 25 contains CNTs.
[0083] The structure of the second semiconductor element 2 is a bottom-gate / bottom-contact structure, similar to the semiconductor element 1 shown in Fig. 1. However, the structure of the second semiconductor element 2 is not limited to this, and may be a top-gate structure or a top-contact structure.
[0084] (Substrate having an insulating surface) The substrate having an insulating surface of the second semiconductor element may be, for example, the same as the substrate having an insulating surface of the first semiconductor element described above.
[0085] From the viewpoints of manufacturing costs and process simplicity, it is preferable to form the above-mentioned first semiconductor element and second semiconductor element on the same substrate having an insulating surface, rather than on separate substrates.
[0086] (Source electrode, drain electrode, gate electrode) Materials used for the source electrode, drain electrode, and gate electrode of the second semiconductor element may be, for example, the same as the materials used for the electrodes of the first semiconductor element described above.
[0087] From the viewpoint of manufacturing costs, it is preferable that the electrodes of the second semiconductor element and the electrodes of the first semiconductor element are formed from the same material, rather than from different materials. The electrodes being formed from the same material means that the elements contained in each electrode have the same highest molar ratio. The types and content ratios of the elements in the electrodes can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) and secondary ion mass spectrometry (SIMS).
[0088] Furthermore, from the viewpoint of process simplicity, it is preferable that the electrodes of the second semiconductor element are formed in the same process as the electrodes of the above-mentioned semiconductor element.
[0089] The distance 200 (Ln) between the source electrode and the drain electrode of the second semiconductor element is not particularly limited, but is preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 100 μm or less. By setting the distance within this range, the characteristics of the semiconductor element are further improved. The distance between the electrodes can be measured using an optical microscope, a scanning electron microscope (SEM), or the like.
[0090] Also, wiring may be formed to electrically connect between the second semiconductor elements or between the first semiconductor element and the second semiconductor element. The material used for the wiring may be any conductive material that can be generally used as an electrode. For example, the same material as the wiring electrically connecting between the first semiconductor elements described above may be used.
[0091] (Gate insulation layer) The material used for the gate insulating layer of the second semiconductor element is not particularly limited, but examples thereof include the same materials as those used for the gate insulating layer of the first semiconductor element described above.
[0092] From the viewpoint of manufacturing cost, it is preferable that the gate insulating layer of the second semiconductor element is formed of the same material as the gate insulating layer of the first semiconductor element, rather than being formed of different materials. These gate insulating layers are made of the same material means that the types and composition ratios of elements contained in the composition constituting each gate insulating layer at 1 mol % or more are the same. Whether the types and composition ratios of elements are the same or not can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) or secondary ion mass spectrometry (SIMS).
[0093] Furthermore, from the viewpoint of process simplicity, it is preferable that the gate insulating layer of the second semiconductor element is formed in the same process as the gate insulating layer of the above-mentioned first semiconductor element.
[0094] (Second Semiconductor Layer) The second semiconductor layer contains CNTs, which are the same as those in the first semiconductor layer described above.
[0095] From the viewpoint of manufacturing cost, the second semiconductor layer is preferably formed of the same material as the first semiconductor layer, not a different material. Moreover, from the viewpoint of process simplicity, the second semiconductor layer is preferably formed in the same process as the first semiconductor layer.
[0096] In the semiconductor device according to the first embodiment, the first semiconductor layer is 1 μm 2 The total length of the CNTs (Cn) per 1 μm of the second semiconductor layer is 2This is different from the total length (Cp) of the CNTs present per unit area. This makes the electrical characteristics of the first and second semiconductor elements, such as the on-current, off-current, and threshold voltage, equivalent, resulting in a semiconductor device with a wide noise margin.
[0097] Among them, the second semiconductor layer is 1 μm 2 The total length of CNTs (Cp) per 1 μm of the first semiconductor layer 2 It is preferable that the total length (Cn) of the CNTs present per unit area is shorter than that of the CNTs present per unit area. This is preferable because the electrical characteristics of the first semiconductor element and the second semiconductor element are more equal. This is presumed to be due to the following reason. As can be seen from the fact that CNT-TFTs usually exhibit p-type semiconductor characteristics, in CNTs, the mobility of holes, which are carriers responsible for the electrical conductivity of p-type semiconductors, is greater than the mobility of electrons, which are carriers responsible for the electrical conductivity of n-type semiconductors. For this reason, in order to equalize the electrical characteristics of the p-type semiconductor element and the n-type semiconductor element, it is preferable to make the carrier density of the n-type semiconductor element denser than the carrier density of the p-type semiconductor element. Furthermore, in order to equalize the electrical characteristics of the p-type semiconductor element and the n-type semiconductor element, it is also preferable to make the distance between the source electrode and the drain electrode of the n-type semiconductor element shorter than the distance between the source electrode and the drain electrode of the p-type semiconductor element.
[0098] More preferably, the second semiconductor layer is 1 μm 2 The total length of CNTs (Cp) per 1 μm of the first semiconductor layer 2 The length is 0.2 to 0.8 times the total length of the CNTs (Cn) present per unit area. The above numerical range is obtained by rounding off the last significant digit of the limit value. That is, 0.8 times or less means 0.84 times or less, and 0.2 times or more means 0.15 times or more. By being in this range, the mobility of the first semiconductor element and the second semiconductor element is increased, the electrical characteristics become more equivalent, and the semiconductor device has a wider noise margin.
[0099] Semiconductor layer 1μm 2The total length of CNTs per unit area is calculated by dividing the total length of CNTs per unit area by the number of randomly selected 1 μm 2 The total length of the CNTs is the sum of the lengths of the CNTs present in the semiconductor layer of a semiconductor element. 2 One method is to select a region, measure the lengths of all the CNTs contained in that region, and then add them up. The total length of the CNTs is a value obtained by rounding off any figures less than 1 μm. In other words, a total length of 1 μm of CNTs is 0.5 μm or more and 1.4 μm or less.
[0100] In addition, the distance between the source electrode and the drain electrode of a semiconductor element refers to the shortest distance between the source electrode and the drain electrode. One method for measuring the distance between the source electrode and the drain electrode is to measure the shortest distance between the source electrode and the drain electrode from an image of the semiconductor element obtained by an optical microscope or a scanning electron microscope (SEM), etc.
[0101] (Third insulating layer) The second semiconductor element may further include a third insulating layer formed on the side opposite to the side on which the gate insulating layer is formed with respect to the second semiconductor layer. The side opposite to the side on which the gate insulating layer is formed with respect to the second semiconductor layer refers to the upper side of the semiconductor layer, for example, when the gate insulating layer is formed on the lower side of the second semiconductor layer. By further forming the third insulating layer of the present invention, the second semiconductor layer can be protected from external environments such as oxygen and moisture, and physical impacts. In addition, by forming the third insulating layer, the characteristics of the second semiconductor element can be adjusted.
[0102] The formation of the third insulating layer does not convert a CNT-FET that normally exhibits p-type semiconductor characteristics into a semiconductor element that exhibits n-type semiconductor characteristics, and in this respect, the third insulating layer differs from the second insulating layer provided in the first semiconductor element.
[0103] The third insulating layer and the second insulating layer being different means that the types and composition ratios of elements contained at 1 mol % or more in the compositions constituting the third insulating layer and the second insulating layer are different. The types and content ratios of elements in the third insulating layer and the second insulating layer can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) or secondary ion mass spectrometry (SIMS) of samples obtained by, for example, extracting the compositions of the third insulating layer and the second insulating layer from a semiconductor element.
[0104] The material used for the third insulating layer is not particularly limited, but specifically includes inorganic materials such as silicon oxide and alumina; organic polymer materials such as polyimide and its derivatives, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane and its derivatives, polyvinylphenol and its derivatives; or a mixture of inorganic material powder and organic polymer material, or a mixture of organic low molecular weight material and organic polymer material. Among these, it is preferable to use an organic polymer material that can be prepared by a coating method. In particular, it is preferable to use an organic polymer material selected from the group consisting of polyfluoroethylene, polynorbornene, polysiloxane, polyimide, polystyrene, polycarbonate and their derivatives, polyacrylic acid derivatives, polymethacrylic acid derivatives, and copolymers containing these, from the viewpoint of uniformity of the insulating layer. By using an organic polymer material selected from the group consisting of polysiloxane, polystyrene, polyvinylphenol, and polymethyl methacrylate, it is possible to protect the second semiconductor layer without deteriorating the electrical characteristics of the second semiconductor element, so it is particularly preferable.
[0105] The thickness of the third insulating layer is preferably 50 nm to 10 μm, and more preferably 100 nm to 3 μm. The third insulating layer may be a single layer or multiple layers. Furthermore, one layer may be formed from multiple insulating materials, or multiple insulating materials may be laminated.
[0106] The method for forming the third insulating layer is not particularly limited, and dry methods such as resistance heating deposition, electron beam, sputtering, and CVD can be used, but it is preferable to use a coating method from the viewpoint of manufacturing costs and suitability for large areas. Specific examples of coating methods that can be preferably used include spin coating, blade coating, slit die coating, screen printing, bar coater, mold method, print transfer method, immersion and pulling method, inkjet method, and drop casting method. The coating method can be selected depending on the coating film properties to be obtained, such as coating film thickness control and orientation control.
[0107] (Embodiment 2) A semiconductor device according to a second embodiment of the present invention is the semiconductor device according to the first embodiment, further comprising: 2 The total length of the carbon nanotubes (Cn) per 1 μm of the second semiconductor layer 2 Instead of the feature that the total length (Cp) of the carbon nanotubes present per 1 μm of the first semiconductor layer is different, 2 The total length (Cn) of the carbon nanotubes present per unit area of the second semiconductor layer is divided by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element, and the value (Cn / Ln) is determined as 2 The characteristic of this embodiment is that the total length (Cp) of the carbon nanotubes present per unit area is different from the value (Cp / Lp) obtained by dividing the total length (Cp) of the carbon nanotubes present per unit area by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element. Except for this point, the semiconductor device has the same configuration as the semiconductor device according to the first embodiment.
[0108] The semiconductor device of the second embodiment has the above-mentioned characteristics, and therefore the electrical characteristics, such as the on-current, off-current, and threshold voltage, of the first semiconductor element and the second semiconductor element are equivalent, resulting in a semiconductor device with a wide noise margin.
[0109] Among them, the second semiconductor layer is 1 μm 2 The total length (Cp) of the CNTs present per unit area is divided by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element, and the value (Cp / Lp) is determined to be equal to or smaller than the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element per unit area of the first semiconductor layer.2 It is preferable that the total length (Cn) of the CNTs present per unit area is smaller than the value (Cn / Ln) obtained by dividing the total length (Cn) of the CNTs present per unit area by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element. This is preferable because the electrical characteristics of the first semiconductor element and the second semiconductor element are more equal. This is presumed to be due to the following reason. As can be seen from the fact that CNT-TFTs usually exhibit p-type semiconductor characteristics, in CNTs, the mobility of holes, which are carriers responsible for the electrical conductivity of p-type semiconductors, is greater than the mobility of electrons, which are carriers responsible for the electrical conductivity of n-type semiconductors. For this reason, in order to equalize the electrical characteristics of the p-type semiconductor element and the n-type semiconductor element, it is preferable to make the carrier density of the n-type semiconductor element denser than the carrier density of the p-type semiconductor element. Furthermore, in order to equalize the electrical characteristics of the p-type semiconductor element and the n-type semiconductor element, it is also preferable to make the distance between the source electrode and the drain electrode of the n-type semiconductor element shorter than the distance between the source electrode and the drain electrode of the p-type semiconductor element.
[0110] More preferably, the second semiconductor layer is 1 μm 2 The total length (Cp) of the CNTs present per unit area of the first semiconductor layer divided by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element (Cp / Lp) is 2 The value (Cn / Ln) is 0.2 to 0.8 times the total length (Cn) of CNTs present per unit area divided by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element. The above numerical range is obtained by rounding off the last significant digit of the limit value. In other words, 0.8 times or less means 0.84 times or less, and 0.2 times or more means 0.15 times or more. By being within this range, the mobility of the first semiconductor element and the second semiconductor element is increased, the electrical characteristics become more equivalent, and the semiconductor device has a wider noise margin.
[0111] In addition, the semiconductor device according to the second embodiment further includes a first semiconductor layer having a thickness of 1 μm. 2 The total length of the carbon nanotubes (Cn) per 1 μm of the second semiconductor layer 2It may have a feature different from the total length (Cp) of the carbon nanotubes present per hit. Also, the second semiconductor layer is 1 μm 2 The total length (Cp) of the carbon nanotubes present per hit is 1 μm of the first semiconductor layer 2 It may have a feature that the total length (Cp) of the carbon nanotubes present per hit is shorter than the total length (Cn) of the carbon nanotubes present per hit in the first semiconductor layer. Further, the second semiconductor layer is 1 μm 2 The total length (Cp) of the carbon nanotubes present per hit is 1 μm of the first semiconductor layer 2 It may have a feature that the total length (Cp) of the carbon nanotubes present per hit is 0.2 times or more and 0.8 times or less of the total length (Cn) of the carbon nanotubes present per hit.
[0112] (Embodiment 3) The semiconductor device according to Embodiment 3 of the present invention is a semiconductor device in which the first semiconductor layer in the first semiconductor element further contains an n-type modifier.
[0113] FIG. 3 shows a schematic cross-sectional view showing an example of the first semiconductor element in the semiconductor device according to Embodiment 3 of the present invention. This semiconductor element 3 has a gate electrode 31 formed on a substrate 30, a gate insulating layer 32 covering it, a source electrode 33 and a drain electrode 34 provided thereon, and a first semiconductor layer 35 provided between those electrodes. The first semiconductor layer 35 contains CNT and an n-type modifier.
[0114] <n-type modifier> The n-type modifier is a material for converting a CNT-FET that usually exhibits p-type semiconductor characteristics into a semiconductor element that exhibits n-type semiconductor characteristics. By including CNT and an n-type modifier in the first semiconductor layer, the first semiconductor element becomes an n-type semiconductor element.
[0115] As a method of incorporating an n-type modifier into the first semiconductor layer, there are a method of doping, a method of adsorbing, a method of coating, etc. an n-type modifier to the CNT in the first semiconductor layer.
[0116] The n-type modifier is not particularly limited as long as it can convert the CNT-FET into a semiconductor element exhibiting n-type semiconductor characteristics. Examples of the n-type modifier include substances containing electron donor atoms that provide electrons to the CNT, such as alkali metals such as potassium and phosphorus, and substances having functional groups that act as electron-donating groups, such as amines, alkyl halides, and alcohols.
[0117] The semiconductor device of the second embodiment has the same configuration and manufacturing method as the first embodiment, except that the first semiconductor element does not include the second insulating layer as an essential component, and instead the first semiconductor layer includes the above-mentioned n-type modifier.
[0118] In the semiconductor device according to the third embodiment, the first semiconductor layer is 1 μm thick. 2 The total length of the CNTs (Cn) per 1 μm of the second semiconductor layer is 2 The total length of the CNTs (Cp) per 1 μm of the first semiconductor layer is different from the total length of the CNTs (Cp) per 1 μm of the first semiconductor layer. 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the second semiconductor layer is divided by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element, and the value (Cn / Ln) is 2 The distance (Lp) between the source electrode and drain electrode of the second semiconductor element is different from the total length (Cp) of the carbon nanotubes present per unit area (Cp) divided by the distance (Lp) between the source electrode and drain electrode of the second semiconductor element (Cp / Lp). This makes the electrical characteristics of the first semiconductor element and the second semiconductor element equivalent, such as the on-current, off-current, and threshold voltage, resulting in a semiconductor device with a wide noise margin.
[0119] <Semiconductor device> The semiconductor device of the present invention includes both a first semiconductor element and a second semiconductor element. An example of a semiconductor device according to an embodiment of the present invention is shown in FIG. 4A. Here, the first semiconductor element 41 is an n-type semiconductor element, and the second semiconductor element 42 is a p-type semiconductor element. The operation of the semiconductor device shown in FIG. 3A will be described below.
[0120] First, the input signal (V in) is the difference between low “L” (ground potential GND) and high “H” (V DD When the input signal is "L", the p-type semiconductor element is conductive and the n-type semiconductor element is cut off, causing the output signal (V out ) becomes "H". Conversely, when the input signal is "H", n-type semiconductor element 41 becomes conductive and p-type semiconductor element 42 becomes cut off, causing the output signal to become "L". An example of the transfer characteristics of this semiconductor device is shown in FIG. 4B.
[0121] For example, if the threshold voltage of the n-type semiconductor element is different from that of the p-type semiconductor element, the timing of conduction and cutoff of the n-type semiconductor element and the p-type semiconductor element will differ, and the output signal will not be inverted relative to the input signal, which may result in malfunction. For this reason, if the electrical characteristics of the n-type semiconductor element and the p-type semiconductor element are equivalent, a semiconductor device with good characteristics will be obtained. For example, if the electrical characteristics of the n-type semiconductor element and the p-type semiconductor element are equivalent, the input signal that changes the output signal (V in Figure 3B: the output signal is V DD / 2) is V DD / 2, resulting in a semiconductor device with a wide noise margin and high performance. In addition, in the curve (transfer characteristic curve) showing the output signal relative to the input signal shown in Figure 4B, the slope (gain) of the tangent line at Vin = V correlates with the mobility of each semiconductor element, and a semiconductor device with a large gain has high performance. In addition to the above-mentioned threshold voltage, examples of electrical characteristics include on-current, off-current, and mobility.
[0122] (Applicability of semiconductor devices) The semiconductor device according to the embodiment of the present invention can be applied to ICs for various electronic devices, wireless communication devices such as RFID tags, wireless power supply devices, TFT arrays for displays such as active matrix driven liquid crystal displays and electronic paper, sensors, and opening detection systems.
[0123] <Method of Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device according to an embodiment of the present invention preferably includes at least a step of applying and drying a semiconductor layer to an area between a source electrode and a drain electrode of a first semiconductor element and a second semiconductor element. In this manufacturing method, the electrodes, gate insulating layer, semiconductor layer, second insulating layer, and third insulating layer constituting the first semiconductor element and the second semiconductor element to be manufactured are formed as described above. By appropriately selecting the order of these forming methods, the semiconductor device according to the present invention can be manufactured.
[0124] From the viewpoint of manufacturing cost and process simplicity, it is preferable to form the first semiconductor element and the second semiconductor element simultaneously, rather than separately. Therefore, it is preferable that they have the same structure. In particular, it is preferable to form the first semiconductor layer and the second semiconductor layer by coating and drying in the same process.
[0125] Here, "simultaneously forming" refers to forming two electrodes or layers by performing the processes required for forming the electrodes or layers once, while "forming by coating and drying in the same process" refers to forming the target layers by performing the coating and drying processes for forming those layers once.
[0126] Although any of these steps can be applied even when the first and second semiconductor elements have different structures, it is easier to apply them when they have the same structure.
[0127] An example of a method for manufacturing a semiconductor device according to an embodiment of the present invention will be specifically described below. First, as shown in Fig. 5(a), a gate electrode 510 is formed in a first semiconductor element region 500 on a substrate 50, and a gate electrode 511 is formed in a second semiconductor element region 501 by the above-mentioned method.
[0128] Next, as shown in FIG. 5(b), gate insulating layers 520 and 521 for the first semiconductor element 500 and the second semiconductor element 501 are formed.
[0129] Next, as shown in FIG. 5(c), source electrodes 540, 541 and drain electrodes 550, 551 are simultaneously formed on the gate insulating layers 520, 521 of the first semiconductor element 500 and the second semiconductor element 501 using the same material by the method described above.
[0130] Next, as shown in FIG. 5(d), first semiconductor layers 560, 460 and a second semiconductor layer 561 are formed between the source electrodes 540, 541 and the drain electrodes 550, 551 of the first semiconductor element 500 and the second semiconductor element 501, respectively, by the method described above.
[0131] Next, as shown in FIG. 5(e), a second insulating layer 5848 is formed by the above-mentioned method so as to cover the first semiconductor layer 560 of the first semiconductor element 500, thereby completing the semiconductor device.
[0132] In addition, in order to improve the efficiency of material use and reduce the number of types of materials, it is preferable that the gate electrodes 510, 511 of the first semiconductor element 400 and the second semiconductor element 501 are made of the same material. For the same reason, it is preferable that the composition used to form the first semiconductor layer 560 and the composition used to form the second semiconductor layer 561 are the same composition. The composition being the same means that the types and composition ratios of elements contained in each composition at 1 mol % or more are the same. Whether the types and composition ratios of elements are the same or not can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) or secondary ion mass spectrometry (SIMS).
[0133] In addition, it is preferable that the concentration of the composition used to form the first semiconductor layer 560 is different from the concentration of the composition used to form the second semiconductor layer 561. Alternatively, it is preferable that the coating amount of the composition used to form the first semiconductor layer 560 is different from the coating amount of the composition used to form the second semiconductor layer 561. By using any of these methods, a semiconductor device in which the first semiconductor element and the second semiconductor element have equivalent electrical characteristics can be easily manufactured, which is preferable.
[0134] The coating method in the coating process of the first semiconductor layer 560 and the second semiconductor layer 561 is not particularly limited, but is preferably any one selected from the group consisting of an inkjet method, a dispenser method, and a spray method. Among them, the inkjet method is more preferable as the coating method from the viewpoint of raw material usage efficiency. In that case, it is considered to adjust the coating amount by adjusting, for example, the number of shots or the solution extrusion pressure. EXAMPLES
[0135] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0136] Preparation example of semiconductor solution 1: Semiconductor solution A1, Semiconductor solution A2 First, 1.0 mg of CNT1 (CNI, single-walled CNT, purity 95%) was added to a 10 ml solution of 2.0 mg of poly(3-hexylthiophene) (P3HT) (Aldrich), and the mixture was stirred ultrasonically for 4 hours at 20% output using an ultrasonic homogenizer (Tokyo Rikakikai VCX-500) while cooling on ice to obtain CNT dispersion A (CNT composite concentration relative to solvent: 0.96 g / l). Next, a semiconductor solution for forming a semiconductor layer was prepared. The CNT dispersion A was filtered using a membrane filter (pore size 10 μm, diameter 25 mm, Millipore Omnipore membrane) to remove CNT composites with a length of 10 μm or more. 5 ml of o-DCB (Wako Pure Chemical Industries, Ltd.) was added to the obtained filtrate, and then the low boiling point solvent chloroform was distilled off using a rotary evaporator, and the solvent was replaced with o-DCB to obtain CNT dispersion A'. 3 mL of o-DCB was added to 1 mL of CNT dispersion A' to prepare semiconductor solution A1 (CNT composite concentration relative to solvent: 0.033 g / L). Also, 1.5 mL of o-DCB was added to 1 mL of CNT dispersion A' to prepare semiconductor solution A2 (CNT composite concentration relative to solvent: 0.061 g / L).
[0137] Composition Preparation Example 1: Gate Insulating Layer Solution A 61.29g (0.45 mol) of methyltrimethoxysilane, 12.31g (0.05 mol) of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 99.15g (0.5 mol) of phenyltrimethoxysilane were dissolved in 203.36g of propylene glycol monobutyl ether (boiling point 170°C), and 54.90g of water and 0.864g of phosphoric acid were added thereto while stirring. The resulting solution was heated at a bath temperature of 105°C for 2 hours, and the internal temperature was raised to 90°C to distill off components mainly consisting of by-produced methanol. The solution was then heated at a bath temperature of 130°C for 2.0 hours, and the internal temperature was raised to 118°C to distill off components mainly consisting of water and propylene glycol monobutyl ether, and then cooled to room temperature to obtain polysiloxane solution A with a solid content concentration of 26.0% by weight. The weight average molecular weight of the resulting polysiloxane was 6000. 10 g of the obtained polysiloxane solution A was weighed out, and 54.4 g of propylene glycol monoethyl ether acetate (hereinafter referred to as PGMEA) was mixed therewith, followed by stirring at room temperature for 2 hours to obtain a gate insulating layer solution A.
[0138] Composition Preparation Example 2: Solution A for preparing the second insulating layer 2.5 g of polymethyl methacrylate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was dissolved in 7.5 g of N,N-dimethylformamide to prepare polymer solution A. Next, 1 g of N,N,N',N'-tetramethyl-1,4-phenylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 9.0 g of N,N-dimethylformamide to prepare compound solution A. 0.30 g of compound solution A was added to 0.68 g of polymer solution A to obtain solution A for producing a second insulating layer.
[0139] Composition Preparation Example 3: Solution B for preparing the second insulating layer Solution B for preparing the second insulating layer was obtained in the same manner as in composition preparation example 2, except that N,N,N',N'-tetramethylbenzidine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of N,N,N',N'-tetramethyl-1,4-phenylenediamine.
[0140] Composition Preparation Example 4: Third Insulating Layer Solution A A third insulating layer solution A was prepared by dissolving 1.485 g of polymethyl methacrylate in 8.5 g of cyclohexanone.
[0141] Composition Preparation Example 5: Third Insulating Layer Solution B A third insulating layer solution B was obtained in the same manner as in Composition Preparation Example 4, except that an acrylic resin having a hydroxyl group (manufactured by Kyoeisha Chemical Co., Ltd., product number "Oricox KC-7000") was used instead of polymethyl methacrylate.
[0142] Composition Preparation Example 6: Third Insulating Layer Solution C A third insulating layer solution C was obtained in the same manner as in Composition Preparation Example 4, except that ethyl cellulose (manufactured by The Dow Chemical Company, product number "Ethocel STD-100CPS") was used instead of polymethyl methacrylate.
[0143] (Evaluation of semiconductor device) The semiconductor devices shown in FIG. 3A, which are composed of the first semiconductor element and the second semiconductor element, fabricated in each of the examples and comparative examples, were evaluated. DD The input signal (V in ) to a 0 to 10 V change in output signal (V out The slope (gain) of the tangent of the transfer characteristic of V out V changes in (V out V DD V = / 2 in ) was measured. The higher the gain, the higher the performance of the semiconductor device. DD / 2), the more equivalent and better the semiconductor characteristics of the n-type and p-type semiconductor elements are.
[0144] Example 1 First, 5 nm of chromium and 50 nm of gold were vacuum-deposited through a mask on a glass substrate (film thickness 0.7 mm) using a resistance heating method, thereby forming a gate electrode 510 of the first semiconductor element and a gate electrode 511 of the second semiconductor element shown in Figure 5.
[0145] Next, the gate insulating layer solution A was spin-coated (2000 rpm×30 seconds) onto the substrate, and heat-treated at 200° C. for 1 hour in a nitrogen stream to form gate insulating layers 520 and 521 with a thickness of 600 nm.
[0146] Next, gold was vacuum-deposited to a film thickness of 50 nm by resistance heating, and photoresist (product name "LC100-10cP", manufactured by Rohm and Haas Co., Ltd.) was applied thereon by spin coating (1000 rpm x 20 seconds), and dried by heating at 100°C for 10 minutes. Next, the photoresist film prepared as described above was pattern-exposed through a mask using a parallel light mask aligner (manufactured by Canon Inc., PLA-501F), and then shower-developed with a 2.38 wt% aqueous solution of tetramethylammonium hydroxide (product name "ELM-D", manufactured by Mitsubishi Gas Chemical Co., Ltd.) for 70 seconds using an automatic developing device (manufactured by Takizawa Sangyo Co., Ltd., AD-2000), followed by washing with water for 30 seconds. Thereafter, the film was etched for 5 minutes with an etching solution (product name "AURUM-302", manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. Next, the resist was removed by immersing the substrate in a stripping solution (product name "AZ Remover 100", manufactured by AZ Electronic Materials Co., Ltd.) for 5 minutes, followed by washing with water for 30 seconds and then drying by heating at 120°C for 20 minutes to form source electrode 540 and drain electrode 550 of the first semiconductor element, and source electrode 541 and drain electrode 551 of the second semiconductor element.
[0147] The width of the source electrode 540 and the drain electrode 550 of the first semiconductor element, and the source electrode 541 and the drain electrode 551 of the second semiconductor element were 100 μm, and the distance between these electrodes was 30 μm. On the substrate 1 on which each electrode was formed as described above, 200 pl of the semiconductor solution A1 was applied to the first semiconductor element by the inkjet method, and 100 pl of the semiconductor solution A1 was applied to the second semiconductor element by the inkjet method, and then a heat treatment was performed for 30 minutes at 150° C. under a nitrogen gas flow on a hot plate to form a first semiconductor layer 560 and a second semiconductor layer 561. Next, 5 μL of the solution A for forming the second insulating layer was dropped on the first semiconductor layer 560 so as to cover the first semiconductor layer, and a heat treatment was performed for 30 minutes at 110° C. under a nitrogen gas flow to form a second insulating layer 58.
[0148] In this way, the semiconductor device of Example 1 was obtained. Next, an image of the first semiconductor layer was obtained using an atomic force microscope Dimension Icon (manufactured by Bruker AXS K.K.). 2 The total length of all the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 16 μm. 2 The total length of the CNT complex per unit area was measured and found to be 11 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 29, V out V changes in was 5.9V.
[0149] Example 2 A semiconductor device was fabricated in the same manner as in Example 1, except that 10 μL of a 5% by mass propylene glycol 1-monomethyl ether 2-acetate solution of polystyrene (manufactured by Aldrich, weight average molecular weight (Mw): 192,000, hereinafter referred to as PS) was drop-cast onto the second semiconductor layer 561 of the second semiconductor element, and the resultant was air-dried at 30° C. for 5 minutes, and then heat-treated at 120° C. for 30 minutes under a nitrogen gas flow on a hot plate to form a second semiconductor element having a third insulating layer. 2The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 16 μm. 2 The total length of the CNT complex per unit area was measured and found to be 11 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 30, V out V changes in was 5.7V.
[0150] Example 3 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 250 pl of the semiconductor solution A1, and the second semiconductor layer of the second semiconductor element was formed by dropping 200 pl of the semiconductor solution A1. 2 The total length of the CNT complexes per unit area was measured and found to be 18 μm. 2 The total length of the CNT complex per unit area was measured and found to be 16 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 7, V out V changes in was 7.9V.
[0151] Example 4 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 100 pl of the semiconductor solution A2, and the second semiconductor layer of the second semiconductor element was formed by dropping 250 pl of the semiconductor solution A1. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 24 μm. 2 The total length of the CNT complex per unit area was measured and found to be 18 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 19, V out V changes in was 6.1V.
[0152] Example 5 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 100 pl of the semiconductor solution A2, and the second semiconductor layer of the second semiconductor element was formed by dropping 100 pl of the semiconductor solution A1. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 24 μm. 2 The total length of the CNT complex per unit area was measured and found to be 11 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 38, V out V changes in was 4.8V.
[0153] Example 6 A semiconductor device was fabricated in the same manner as in Example 5, except that the solution B for forming the second insulating layer was used instead of the solution A for forming the second insulating layer. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 24 μm. 2 The total length of the CNT complex per unit area was measured and found to be 11 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 34, V out V changes in was 4.5V.
[0154] Example 7 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 3000 pl of the semiconductor solution A1, and the second semiconductor layer of the second semiconductor element was formed by dropping 100 pl of the semiconductor solution A2. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 80 μm. 2 The total length of the CNT complex per unit area was measured and found to be 24 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 18, V out V changes inwas 3.8V.
[0155] Example 8 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 1000 pl of the semiconductor solution A1, and the second semiconductor layer of the second semiconductor element was formed by dropping 70 pl of the semiconductor solution A1. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 53 μm. 2 The total length of the CNT complex per unit area was measured and found to be 7 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 5, V out V changes in was 1.9V.
[0156] Example 9 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element was formed by dropping 3000 pl of the semiconductor solution A1, and the second semiconductor layer of the second semiconductor element was formed by dropping 200 pl of the semiconductor solution A1. 2 The total length of the CNT complexes per 1 μm in the second semiconductor layer was measured and found to be 80 μm. 2 The total length of the CNT complex per unit area was measured and found to be 16 μm. In addition, when the above evaluation was performed on this semiconductor device, the gain was 15, V out V changes in was 3.2V.
[0157] Examples 10 to 12 A semiconductor device was fabricated in the same manner as in Example 2, except that the third insulating layer solutions A, B, and C were used, respectively, as shown in Table 1, instead of the 5 mass % propylene glycol 1-monomethyl ether 2-acetate solution of PS. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0158] Example 13 A semiconductor device was fabricated in the same manner as in Example 1, except that the distance between the source electrode 541 and the drain electrode 551 of the second semiconductor element was set to 35 μm. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0159] Example 14 The second semiconductor layer of the second semiconductor element was formed by depositing 200 pl of the semiconductor solution A1, and the distance between the source electrode 541 and the drain electrode 551 of the second semiconductor element was set to 60 μm. A semiconductor device was fabricated in the same manner as in Example 1. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0160] Example 15 A semiconductor device was fabricated in the same manner as in Example 14, except that the distance between the source electrode 541 and the drain electrode 551 of the second semiconductor element was set to 130 μm. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0161] Example 16 A semiconductor device was fabricated in the same manner as in Example 14, except that the distance between the source electrode 540 and the drain electrode 550 of the first semiconductor element was 10 μm, and the distance between the source electrode 541 and the drain electrode 551 of the second semiconductor element was 100 μm. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0162] Example 17 A semiconductor device was fabricated in the same manner as in Example 14, except that the distance between the source electrode 540 and the drain electrode 550 of the first semiconductor element was 30 μm, and the distance between the source electrode 541 and the drain electrode 551 of the second semiconductor element was 35 μm. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0163] Example 18 A semiconductor device was fabricated in the same manner as in Example 14, except that the second semiconductor layer of the second semiconductor element was formed by depositing 100 pl of the semiconductor solution A2. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0164] Example 19 A semiconductor device was fabricated in the same manner as in Example 14, except that 10 μL of the third insulating layer solution A was drop-cast onto the second semiconductor layer 561 of the second semiconductor element, and the solution was air-dried at 30° C. for 5 minutes, and then heat-treated on a hot plate under a nitrogen stream at 120° C. for 30 minutes to form a second semiconductor element having a third insulating layer. 2 The total length of the CNT complexes present per unit area was measured, and the above evaluation was performed for each semiconductor device.
[0165] Comparative Example 1 A semiconductor device was fabricated in the same manner as in Example 1, except that the first semiconductor layer of the first semiconductor element and the second semiconductor layer of the second semiconductor element were both formed by dropping 100 pl of the semiconductor solution A1. 2 The total length of the CNT composites per unit area was measured and found to be 11 μm for both. in V for a change of 0 to 10 V outThe voltage only changed from 10V to 4V, and the semiconductor device did not operate normally.
[0166] [Table 1]
[0167] [Table 2] [Explanation of symbols]
[0168] 10, 20, 30, 50 boards 11, 21, 31, 510, 511 Gate electrode 12, 22, 32, 520, 521 Gate insulating layer 13, 23, 33, 540, 541 Source electrode 14, 24, 34, 550, 551 Drain electrode 15, 35, 560 First semiconductor layer 16, 58 Second insulating layer 100, 200 Distance between source and drain electrodes of semiconductor element 25, 561 Second semiconductor layer 41,500 First semiconductor element 42, 501 Second semiconductor element
Claims
1. A semiconductor device including a first semiconductor element and a second semiconductor element provided on a substrate having an insulating surface, the first semiconductor element is an n-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a first semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the first semiconductor layer from the gate electrode; Including, the second semiconductor element is a p-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a second semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the second semiconductor layer from the gate electrode; Including, the semiconductor device is a complementary semiconductor device including the n-type semiconductor element and the p-type semiconductor element, the first semiconductor layer and the second semiconductor layer both contain carbon nanotubes; The first semiconductor layer 1 μm 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the second semiconductor layer is divided by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element (Cn / Ln). 2 the total length (Cp) of the carbon nanotubes present per unit area is different from the value (Cp / Lp) obtained by dividing the total length (Cp) of the carbon nanotubes present per unit area by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element.
2. The second semiconductor layer 1 μm 2 The total length (Cp) of the carbon nanotubes present per 1 μm of the first semiconductor layer is divided by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element (Cp / Lp). 22. The semiconductor device according to claim 1, wherein the total length (Cn) of the carbon nanotubes present per unit area is smaller than a value (Cn / Ln) obtained by dividing the total length (Cn) of the carbon nanotubes present per unit area by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element.
3. The second semiconductor layer 1 μm 2 The total length (Cp) of the carbon nanotubes present per 1 μm of the first semiconductor layer is divided by the distance (Lp) between the source electrode and the drain electrode of the second semiconductor element (Cp / Lp). 2 3. The semiconductor device according to claim 1, wherein the total length (Cn) of the carbon nanotubes present per unit area is 0.2 to 0.8 times the value (Cn / Ln) obtained by dividing the total length (Cn) of the carbon nanotubes present per unit area by the distance (Ln) between the source electrode and the drain electrode of the first semiconductor element.
4. A semiconductor device including a first semiconductor element and a second semiconductor element provided on a substrate having an insulating surface, the first semiconductor element is an n-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a first semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the first semiconductor layer from the gate electrode; Including, the second semiconductor element is a p-type semiconductor element, A source electrode; A drain electrode; A gate electrode; a second semiconductor layer in contact with the source electrode and the drain electrode; a gate insulating layer insulating the second semiconductor layer from the gate electrode; Including, the semiconductor device is a complementary semiconductor device including the n-type semiconductor element and the p-type semiconductor element, the first semiconductor layer and the second semiconductor layer both contain carbon nanotubes; The first semiconductor layer 1 μm 2 The total length (Cn) of the carbon nanotubes present per 1 μm of the second semiconductor layer 2 a total length (Cp) of the carbon nanotubes present per unit area is different from the total length (Cp) of the carbon nanotubes present per unit area.
5. The second semiconductor layer 1 μm 2 The total length (Cp) of the carbon nanotubes present per 1 μm of the first semiconductor layer 2 5. The semiconductor device according to claim 4, wherein the length (Cn) of the carbon nanotubes is shorter than the total length (Cn) of the carbon nanotubes present per unit area.
6. The second semiconductor layer 1 μm 2 The total length (Cp) of the carbon nanotubes present per 1 μm of the first semiconductor layer 2 6. The semiconductor device according to claim 4, wherein the length of said first carbon nanotube is 0.2 to 0.8 times the total length (Cn) of said carbon nanotubes present per unit area.
7. 7. The semiconductor device according to claim 1, wherein the first semiconductor element further includes a second insulating layer in contact with the first semiconductor layer on a side opposite to the gate insulating layer with respect to the first semiconductor layer.
8. 7. The semiconductor device according to claim 1, wherein the first semiconductor layer further comprises an n-type modifier.
9. 8. The semiconductor device according to claim 7, wherein the second semiconductor element has a third insulating layer different from the second insulating layer, and the third insulating layer contacts the second semiconductor layer on a side opposite to the gate insulating layer with respect to the second semiconductor layer.
10. 10. The method for manufacturing a semiconductor device according to claim 1, comprising the steps of applying and drying the first semiconductor layer and the second semiconductor layer.
11. 11. The method for manufacturing a semiconductor device according to claim 10, wherein the first semiconductor layer and the second semiconductor layer are formed by coating and drying in the same process.
12. 12. The method for manufacturing a semiconductor device according to claim 10, wherein a composition used to form the first semiconductor layer and a composition used to form the second semiconductor layer are the same composition.
13. 13. The method for manufacturing a semiconductor device according to claim 10, wherein a concentration of a composition used to form the first semiconductor layer is different from a concentration of a composition used to form the second semiconductor layer.
14. The method for manufacturing a semiconductor device according to any one of claims 10 to 13, wherein an application amount of a composition used to form the first semiconductor layer is different from an application amount of a composition used to form the second semiconductor layer.
Citation Information
Patent Citations
Elements containing carbon nanotubes, and circuits, battery charging circuits, automobile systems, computer systems, or electronic devices comprising such elements
JP2008514008A
Method of manufacturing semiconductor device
JP2011166070A
Carbon nanotube composite, organic semiconductor composite, and field-effect transistor
WO2009139339A1
Semiconductor device, complementary semiconductor device, manufacturing method of semiconductor device, wireless communication device and product tag
WO2018180146A1
Packing material, method for producing packing material, reading device, stored-article management system, disconnection detection device, unsealing detection label, and unsealing detection system
WO2019069772A1