Resin sheet and method for producing the same

Hot press molding of thermoplastic resin sheets with controlled conditions addresses the limitations of conventional methods, enabling high shape accuracy and reduced variations in aspherical portions for optical elements.

JP7589694B2Active Publication Date: 2024-11-26ZEON CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021550578
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-15
Publication Date
2024-11-26
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing small-diameter lenses, such as injection molding, struggle with weld line formation and birefringence, limiting high optical performance and shape accuracy, especially in aspherical portions.

Method used

A method involving hot press molding of a thermoplastic resin sheet at controlled temperature and pressure conditions, with specific parameters to achieve aspherical portions with high shape accuracy and reduced thickness variations.

Benefits of technology

The method produces resin sheets with aspherical portions having small variations in thickness accuracy and high shape accuracy, suitable for use in transmissive optical elements like lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589694000002
    Figure 0007589694000002
  • Figure 0007589694000001
    Figure 0007589694000001
Patent Text Reader

Abstract

The present invention provides a resin sheet including a plurality of aspherical portions having small variations in thickness precision and having high shape precision. A resin-sheet manufacturing method according to the present invention is a method for manufacturing a resin sheet including a plurality of separate aspherical portions by subjecting a thermoplastic resin film formed by using a thermoplastic resin to thermal press molding, wherein the thermal press molding is performed at a press temperature that is higher than the glass transition temperature of the thermoplastic resin by at least 40°C, while boosting the press pressure to a final press pressure at an average boost rate of at most 0.1 MPa / s.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet and a method for manufacturing a resin sheet, and more particularly to a resin sheet useful for manufacturing a transmission type optical element and a method for manufacturing a resin sheet. [Background technology]

[0002] In recent years, electronic and electrical devices have become lighter, smaller, and thinner, and there is an increasing need for thinner and smaller diameter camera units and the like mounted on these electronic and electrical devices. In addition, there is a need for even higher image quality in such camera units and the like, and the lenses, prisms, and other transmissive optical elements mounted on these optical devices are also required to have high performance.

[0003] Conventionally, transmissive optical elements such as lenses used in camera units and the like have generally been manufactured by injection molding. However, when lenses are formed by injection molding, it is difficult to completely prevent weld lines from being formed in the obtained lenses. In addition, lenses obtained by injection molding are prone to birefringence. For this reason, it is difficult to sufficiently increase the ratio of the area capable of exhibiting sufficiently high optical performance in the obtained lenses, and even if a small-diameter lens with a diameter of less than 1 cm is formed by injection molding, it is difficult to make it function sufficiently as a lens.

[0004] In recent years, therefore, methods for manufacturing transmission type optical elements such as small-diameter lenses by methods other than injection molding have been considered. For example, Patent Document 1 discloses a technique for manufacturing a microlens array having a large number of microlenses arranged continuously without gaps by sandwiching a lens molding material between a first mold having a plurality of first concave-convex structures forming a first lens surface and a second mold having a plurality of second concave-convex structures forming a second lens surface, and performing a heat press process. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-181515 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the above-mentioned conventional technology using press molding, when manufacturing a resin sheet having a plurality of aspherical portions that can be used, for example, as a lens, it was not possible to obtain a resin sheet having a plurality of aspherical portions with small variation in thickness accuracy and high shape accuracy.

[0007] Therefore, an object of the present invention is to provide a resin sheet having a plurality of aspheric portions with small variation in thickness accuracy and high shape accuracy. [Means for solving the problem]

[0008] The present inventors have conducted intensive research to achieve the above object. The present inventors have found that a resin sheet having a plurality of aspherical portions with small variation in thickness accuracy and high shape accuracy can be obtained by hot press molding a resin sheet under predetermined conditions. The present inventors have also found that forming a resin sheet into a predetermined shape can reduce the variation in thickness accuracy of the aspherical portions and increase the shape accuracy. The present inventors have completed the present invention based on the above-mentioned new findings.

[0009] That is, the present invention aims to advantageously solve the above-mentioned problems, and the method for producing a resin sheet of the present invention is a method for producing a resin sheet having a plurality of aspherical portions spaced apart from each other by hot-press molding a thermoplastic resin film formed using a thermoplastic resin, characterized in that the hot-press molding is carried out at a press temperature 40°C or more higher than the glass transition temperature of the thermoplastic resin, and by increasing the press pressure to a final press pressure at an average pressure increase rate of 0.1 MPa / sec or less. In this way, by keeping the average pressure increase rate of the press pressure and the press temperature within a predetermined range, a resin sheet having a plurality of aspherical portions with small variation in thickness accuracy and high shape accuracy can be easily produced. In the present invention, the "glass transition temperature of the thermoplastic resin" can be measured based on JIS K7121.

[0010] Here, in the method for producing a resin sheet of the present invention, it is preferable to increase the press pressure to the final press pressure at a constant increase rate of 0.1 MPa / sec or less. By keeping the increase rate of the press pressure constant, the shape precision of the aspheric portion can be further improved, and the variation in birefringence and thickness precision can be further reduced.

[0011] In the method for producing a resin sheet of the present invention, it is preferable that at least one surface of the aspherical portion has a cross-sectional shape in the thickness direction having an inflection point. An aspherical portion having such a shape can be advantageously used as a transmission optical element such as a lens.

[0012] Another object of the present invention is to solve the above-mentioned problems in an advantageous manner, and the resin sheet of the present invention is a resin sheet having a plurality of aspherical portions formed by using a thermoplastic resin, the arrangement density of the aspherical portions being 0.16 pieces / cm 2The present invention is characterized in that the minimum interval between adjacent aspherical portions is 1.0 mm or more, the diameter of the aspherical portions in a plan view is 1 mm to 15 mm, the phase difference of the aspherical portions is 50 nm or less, and the thickness of the thinnest portion is 500 μm or less. In this way, if the arrangement density, minimum interval, diameter, and phase difference of the aspherical portions, and the thickness of the thinnest portion are within a predetermined range, it is possible to reduce the variation in thickness accuracy of the aspherical portions and to increase the shape accuracy. In the present invention, the "phase difference" can be measured by the method described in the Examples.

[0013] Here, in the resin sheet of the present invention, it is preferable that the variation in thickness accuracy of the aspherical portion is 0.2 μm or less. If the variation in thickness accuracy of the aspherical portion is 0.2 μm or less, birefringence can be sufficiently reduced. In the present invention, the "variation in thickness accuracy" can be measured using the method described in the Examples.

[0014] In the resin sheet of the present invention, it is preferable that at least one surface of the aspherical portion has a cross-sectional shape in the thickness direction having an inflection point. The aspherical portion having such a shape can be advantageously used as a transmission optical element such as a lens. Effect of the Invention

[0015] According to the present invention, it is possible to provide a resin sheet having a plurality of aspheric portions with small variation in thickness accuracy and high shape accuracy. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a cross-sectional view showing a cross section along a thickness direction of an example of a resin sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail. The manufacturing method of the resin sheet of the present invention can be used, for example, when manufacturing the resin sheet of the present invention. The resin sheet according to the present invention can be suitably used for manufacturing a transmission type optical element such as an optical lens and a prism, without being particularly limited. Here, the term "optical lens" means a transparent body that exhibits a light refraction action. The term "prism" means a transparent polyhedron that exhibits a light dispersion action, a refraction action, a total reflection action, and / or a birefringence action. By using the resin sheet according to the present invention, a transmission type optical element having high shape accuracy and low birefringence can be efficiently obtained. More specifically, by using the resin sheet according to the present invention, various shapes of aspherical lenses, such as aspherical lenses having an inflection point on one side and / or both sides, can be suitably manufactured. The aspheric lens can be suitably used, for example, as a lens for a camera unit of a small electronic or electrical device.

[0018] (Resin sheet) The resin sheet of the present invention is a resin sheet 10 formed of a thermoplastic resin, the cross-sectional shape of which is taken along the thickness direction, as shown in Fig. 1, and has a plurality of aspherical portions 11. The resin sheet 10 of the present invention has an arrangement density of the aspherical portions 11 of 0.16 pieces / cm. 2 or more, the minimum distance P between the adjacent aspherical portions 11 is 1.0 mm or more, the diameter D of the aspherical portions 11 in a plan view is 1 mm or more and 15 mm or less, the phase difference of the aspherical portions 11 is 50 nm or less, and the thinnest portion H min When the arrangement density, minimum interval, diameter, and phase difference of the aspherical portions, as well as the thickness of the thinnest portion of the resin sheet, are within the above ranges, the variation in thickness accuracy of the aspherical portions can be reduced, and the shape accuracy can be improved. The shape of the aspherical portion of the resin sheet is not limited to the shape shown in Fig. 1, and may be any aspherical shape, such as a plano-convex lens, a biconvex lens, a convex meniscus lens, a plano-concave lens, a biconcave lens, and a concave meniscus lens. The aspherical portion of the resin sheet is not particularly limited, and may be suitably used as an aspherical lens, for example, by cutting it out from the resin sheet. Here, from the viewpoint of advantageous use as a transmission optical element such as a lens, it is preferable that at least one surface of the aspherical portion has a shape in which the cross-sectional shape in the thickness direction has an inflection point.

[0019] <Thermoplastic resin> Examples of the thermoplastic resin include (meth)acrylic resin, alicyclic structure-containing resin, styrene resin, polycarbonate resin, polyester resin, polyether resin, urethane resin, olefin resin, and thiourethane resin. Note that "(meth)acrylic" refers to acrylic and / or methacrylic. The above-mentioned thermoplastic resins may be used alone or in combination of two or more. Among these, the thermoplastic resin preferably contains an alicyclic structure-containing resin because of its excellent transparency.

[0020] The alicyclic structure-containing resin is a polymer having an alicyclic structure such as a saturated cyclic hydrocarbon structure and an unsaturated cyclic hydrocarbon structure in the main chain and / or side chain. Among them, those having a cycloalkane structure in the main chain are preferred because they are easy to obtain a resin sheet with excellent mechanical strength and heat resistance. The proportion of repeating units having an alicyclic structure in the polymer constituting the alicyclic structure-containing resin (hereinafter also referred to as "alicyclic structure-containing polymer") is not particularly limited, but is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total repeating units contained in the polymer. By using an alicyclic structure-containing polymer having a proportion of repeating units having an alicyclic structure of 50% by mass or more, a resin sheet with excellent transparency and heat resistance can be easily obtained.

[0021] Specific examples of the alicyclic structure-containing polymer include norbornene-based polymers, monocyclic cyclic olefin-based polymers, cyclic conjugated diene-based polymers, vinyl alicyclic hydrocarbon-based polymers, etc. Among these, norbornene-based polymers are preferred from the viewpoint of improving the transparency, heat resistance, and mechanical strength of the resulting resin sheet. In this specification, these polymers refer not only to polymerization reaction products but also to hydrogenated products thereof.

[0022] The norbornene polymer is a polymer of a norbornene monomer or a hydrogenated product thereof. Examples of the norbornene polymer include a ring-opening polymer of a norbornene monomer, a ring-opening polymer of a norbornene monomer and another monomer capable of ring-opening copolymerization with the norbornene monomer, an addition polymer of a norbornene monomer, an addition polymer of a norbornene monomer and another monomer capable of copolymerization with the norbornene monomer, and a hydrogenated product of these polymers. Among these, a hydrogenated ring-opening polymer of a norbornene monomer (i.e., a hydrogenated ring-opening polymer of a norbornene monomer) is preferred. By using a hydrogenated ring-opening polymer of a norbornene, the transparency, heat resistance, mechanical strength, etc. of the resin sheet can be further improved, and the mold releasability and transferability can be improved when manufacturing a resin sheet using hot press molding.

[0023] Norbornene monomers include bicyclo[2.2.1]hept-2-ene (common name: norbornene) and its derivatives, tricyclo[4.3.0 1,6 .1 2,5 ]Deca-3,7-diene (commonly known as dicyclopentadiene) and its derivatives, 7,8-benzotricyclo[4.3.0.1 2,5 ]dec-3-ene (commonly known as methanotetrahydrofluorene: 1,4-methano-1,4,4a,9a-tetrahydrofluorene) and its derivatives, tetracyclo[4.4.0.1 2,5 .1 7,10]dodec-3-ene (common name: tetracyclododecene) and its derivatives. Substituents that may be contained in the derivatives include alkyl groups, alkylene groups, vinyl groups, alkoxycarbonyl groups, and alkylidene groups. For example, derivatives as norbornene-based monomers include 8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methyl-8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, etc. These norbornene-based monomers may be used alone or in combination of two or more.

[0024] Other monomers capable of ring-opening copolymerization with norbornene-based monomers include monocyclic olefin monomers such as cyclohexene, cycloheptene, and cyclooctene. Other monomers capable of addition copolymerization with norbornene-based monomers include α-olefins having 2 to 20 carbon atoms such as ethylene, propylene, 1-butene, 1-pentene, and 1-hexene, and derivatives thereof; cycloolefins such as cyclobutene, cyclopentene, cyclohexene, cyclooctene, and 3a,5,6,7a-tetrahydro-4,7-methano-1H-indene, and derivatives thereof; non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene; and the like.

[0025] The ring-opening polymers and addition polymers containing norbornene-based monomers as described above can be synthesized by polymerization in the presence of a known catalyst, and their hydrogenated products can be obtained by hydrogenation using a known hydrogenation catalyst.

[0026] Examples of the monocyclic olefin polymer, cyclic conjugated diene polymer, and vinyl alicyclic hydrocarbon polymer include those described in WO 2017 / 126599.

[0027] In addition, commercially available products can also be used as the thermoplastic resin such as the alicyclic structure-containing polymer.Specifically, for example, commercially available products of the alicyclic structure-containing polymer include ZEONEX (registered trademark) manufactured by Zeon Corporation, APEL (registered trademark) manufactured by Mitsui Chemicals, Inc., ARTON (registered trademark) manufactured by JSR Corporation, and TOPAS (registered trademark) manufactured by Polyplastics Co., Ltd.In addition, for example, commercially available products of olefin resin include TPX (registered trademark) manufactured by Mitsui Chemicals, Inc.

[0028] The glass transition temperature (Tg) of the thermoplastic resin is not particularly limited, but is preferably 100° C. or higher, more preferably 120° C. or higher, and preferably 200° C. or lower, more preferably 160° C. or lower. If the glass transition temperature (Tg) of the thermoplastic resin is equal to or higher than the lower limit, the shape precision of the aspherical portion of the resin sheet can be further improved. If the glass transition temperature (Tg) of the thermoplastic resin film is equal to or lower than the upper limit, the production efficiency of the resin sheet can be improved and the shape precision of the aspherical portion can be further improved.

[0029] The resin sheet may contain components other than the resin components described above. Examples of components other than the resin components include additives such as light stabilizers, ultraviolet absorbers, infrared absorbers, antioxidants, release agents, antistatic agents, carbon materials (carbon, etc.), pigments, and dyes. The blending amounts of these components are not particularly limited and can be appropriately determined. For example, the total amount of these additives can be, for example, 20% by mass or less, preferably 10% by mass or less, based on 100% by mass of the resin components.

[0030] <Aspherical part> The aspheric portions are arranged at a density of 0.16 pieces / cm 2 The density of the aspheric portions must be 0.30 pieces / cm or more. 2It is preferable that the number of particles is 0.40 / cm or more. 2 More preferably, it is 3.0 particles / cm or more. 2 It is preferable that the number of particles is 2.0 or less per cm. 2 More preferably, it is 1.0 particles / cm or less. 2 More preferably, the number is 0.60 / cm or less. 2 It is particularly preferable that the arrangement density of the aspherical portions is 0.16 pieces / cm or less. 2 If the density of the aspherical portions is equal to or less than the upper limit, the birefringence can be reduced and the variation in thickness accuracy can be further reduced.

[0031] In addition, the minimum distance between adjacent aspherical portions must be 1.0 mm or more, preferably 3.0 mm or more, more preferably 5.0 mm or more, and even more preferably 7.0 mm or more. If the minimum distance between the aspherical portions is 1.0 mm or more, the variation in thickness accuracy of the aspherical portions can be reduced and the shape accuracy can be improved. In addition, if the minimum distance between the aspherical portions is 1.0 mm or more, the occurrence of air bubbles and air pockets in the resin sheet can be suppressed even when the resin sheet is manufactured using a molding method such as press molding. The minimum distance between the aspherical portions is usually 20 mm or less.

[0032] Furthermore, the diameter of the aspherical portion in plan view must be 1 mm or more and 15 mm or less, and is preferably 3 mm or more and 9 mm or less. If the diameter of the aspherical portion is within the above range, the variation in thickness accuracy of the aspherical portion can be reduced, and the shape accuracy can be improved.

[0033] The thickness of the center of the aspherical portion is preferably 50 μm or more, more preferably 100 μm or more, and is preferably 1500 μm or less, more preferably 1000 μm or less. If the thickness of the center of the aspherical portion is within the above range, it can be advantageously used as a transmission optical element such as a lens.

[0034] Furthermore, the variation in thickness accuracy of the aspherical portion is preferably 0.2 μm or less, and more preferably 0.1 μm or less. If the variation in thickness accuracy is equal to or less than the above upper limit, the birefringence of the aspherical portion can be reduced.

[0035] The phase difference of the aspherical portion must be 50 nm or less, and is preferably 20 nm or less. If the phase difference is equal to or less than the upper limit, the variation in thickness accuracy of the aspherical portion can be reduced, and the shape accuracy can be improved.

[0036] <Properties of resin sheet> The resin sheet must have a thickness of 500 μm or less at its thinnest part, and the thickness of the thinnest part of the resin sheet is preferably 50 μm or more, more preferably 100 μm or more, and preferably 300 μm or less, and more preferably 200 μm or less. If the thickness of the thinnest part is equal to or less than the upper limit, the variation in thickness accuracy of the aspheric part can be reduced and the shape accuracy can be improved. If the thickness of the thinnest part is equal to or more than the lower limit, the strength of the resin sheet can be sufficiently ensured.

[0037] (Method of manufacturing resin sheet) The method for producing a resin sheet of the present invention is a method for producing a resin sheet having a plurality of aspherical portions separated from each other by hot press molding a thermoplastic resin film formed using a thermoplastic resin, and is not particularly limited, and can be used, for example, when producing the resin sheet of the present invention described above. The method for producing a resin sheet of the present invention includes, for example, a "heat press step" in which a thermoplastic resin film is heated and pressed by at least a pair of dies and held for a certain period of time to obtain a heat press film, a "die cooling step" in which the pair of dies are cooled to a temperature below the glass transition temperature of the thermoplastic resin after the heat press step to cool the heat press film, and a "release step" in which the heat press film is released from the pair of dies after the die cooling step to obtain a resin sheet, and is characterized in that the heat press in the heat press step is performed at a press temperature 40° C. or higher than the glass transition temperature of the thermoplastic resin, and the press pressure is increased to the final press pressure at an average increase rate of 0.1 MPa / sec or less.

[0038] In the resin sheet manufacturing method of the present invention, the average increase rate of the press pressure and the press temperature during hot press molding are within a predetermined range, so that a resin sheet having a small variation in thickness accuracy and a plurality of aspherical portions with high shape accuracy can be easily manufactured.

[0039] The method for producing a resin sheet of the present invention may include a conveying step of conveying the thermoplastic resin film along a predetermined conveying direction prior to the heat pressing step. The atmospheric pressure of the environment in which each step of the method for producing a resin sheet of the present invention is carried out is not particularly limited and may be within the range of standard conditions specified in JIS Z8703. Each step of the method for producing a resin sheet of the present invention may be carried out by any means without being particularly limited, but is preferably carried out using a so-called roll-to-roll type manufacturing means. This is because the manufacturing efficiency of the resin sheet can be improved by carrying out each step using a roll-to-roll type manufacturing means.

[0040] <Resin sheet> The resin sheet produced by the method for producing a resin sheet of the present invention is not particularly limited as long as it has a plurality of aspherical portions spaced apart from each other. In particular, it is preferable that the resin sheet has the same properties as the resin sheet of the present invention described above.

[0041] <Thermoplastic resin film> The thermoplastic resin used for the thermoplastic resin film is not particularly limited, and may be, for example, the same as the thermoplastic resin for the resin sheet of the present invention described above. Note that the term "film" refers to an object having a shape in which the front and back surfaces (i.e., main surfaces) face each other at a distance equal to the thickness of the object.

[0042] The method for producing the thermoplastic resin film is not particularly limited, and any suitable method known in the art can be used. For example, a molding material for producing a thermoplastic resin film can be obtained by mixing predetermined components, and then the thermoplastic resin film can be obtained by melt extrusion molding, melt casting molding, injection molding, or the like.

[0043] The thickness of the thermoplastic resin film can be appropriately selected according to the diameter of the aspherical part of the resin sheet to be produced. For example, the thickness of the thermoplastic resin film is usually 50 μm or more, preferably 70 μm or more, and usually 500 μm or less, preferably 400 μm or less. In addition, when the thickness of the thermoplastic resin film varies, the thickness of the thermoplastic resin film corresponds to the simple arithmetic average value of the thickness at multiple randomly selected measurement points.

[0044] <Transportation process> In the conveying step, prior to the heat pressing step, the thermoplastic resin film is conveyed along a predetermined conveying direction to a position where the heat pressing is performed. The conveying direction is preferably a direction along the longitudinal direction perpendicular to the width direction of the thermoplastic film.

[0045] <Heat pressing process> In the heat pressing step, the thermoplastic resin film is heat pressed by at least a pair of dies at a predetermined average pressure increase rate and press temperature to obtain a heat pressed film. In the heat pressing step, there is no particular limitation as long as at least a pair of dies is used, and the thermoplastic resin film may be heat pressed by a pair of dies, or different parts of one thermoplastic resin film may be heat pressed simultaneously or at different times by multiple pairs of dies. In the manufacturing method of the resin sheet of the present invention, the occurrence of birefringence in the aspherical part of the obtained resin sheet can be suppressed by subjecting the thermoplastic resin film to heat pressing using a die, regardless of the injection molding method.

[0046] [Mold] The mold is not particularly limited as long as at least one of the molds has a plurality of cavities which are regions for forming aspheric portions, and a mold of any shape, such as a flat mold, can be used. The material used for the mold can be any known material. For example, carbon steel, stainless steel, and alloys based on these can be mentioned. Among them, from the viewpoint of workability and hardness, stainless steel such as STAVAX (registered trademark) material (manufactured by Woodholm) is preferable. From the viewpoint of mold releasability, it is preferable to use a mold whose surface is plated with metals such as chromium, titanium, and nickel, and it is more preferable to use a mold whose surface is plated with electroless nickel-phosphorus plating.

[0047] At least one of the molds used in the manufacturing method of the present invention has a plurality of cavities arranged discretely in a planar direction of the mold. The plurality of cavities are preferably arranged at equal intervals in the planar direction of the mold. Here, both of the pair of dies may have a plurality of cavities. This is because molding using a pair of dies each having a cavity portion allows efficient production of a resin sheet with both sides shaped. Note that the shapes of the pair of dies may be the same or different depending on the shape of the resin sheet to be produced.

[0048] The cavity has a density of 0.16 pieces / cm 2 It is preferable that the number of particles is 0.30 / cm or more. 2 More preferably, it is 0.40 particles / cm or more. 2 More preferably, it is 3.0 particles / cm or more. 2 It is preferable that the number of particles is 2.0 or less per cm. 2 More preferably, it is 1.0 particles / cm or less. 2 More preferably, the number is 0.60 / cm or less. 2 It is particularly preferable that the cavity density is 0.16 / cm or less. 2 If the density of the cavities is equal to or less than the upper limit, the birefringence can be reduced and the variation in thickness precision can be further reduced.

[0049] In addition, the minimum distance between adjacent cavity portions is preferably 1.0 mm or more, more preferably 3.0 mm or more, even more preferably 5.0 mm or more, and particularly preferably 7.0 mm or more. If the minimum distance between cavity portions is 1.0 mm or more, the variation in thickness accuracy of the aspheric portion of the obtained resin sheet can be reduced and the shape accuracy can be improved. In addition, if the minimum distance between cavity portions is 1.0 mm or more, the occurrence of air bubbles and air pockets in the resin sheet can be suppressed. The minimum distance between cavity portions is usually 20 mm or less.

[0050] Furthermore, the diameter of the cavity in plan view is preferably 1 mm or more and 15 mm or less, more preferably 3 mm or more, and more preferably 9 mm or less. If the diameter of the cavity is within the above range, the variation in thickness accuracy of the aspheric portion of the obtained resin sheet can be reduced, and the shape accuracy can be improved.

[0051] Furthermore, the depth of the center of the cavity when the mold is closed (the distance in the direction corresponding to the thickness direction of the aspherical portion to be formed) is preferably 50 μm or more, more preferably 100 μm or more, and preferably 1500 μm or less, more preferably 1000 μm or less. If the distance between the centers of the cavity is within the above range, the aspherical portion of the obtained resin sheet can be advantageously used as a transmission type optical element such as a lens.

[0052] Furthermore, the minimum distance between the resin sheet forming surfaces of the mold in a closed state (closed mold state) is preferably 50 μm or more, more preferably 100 μm or more, and preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less. If the minimum distance is equal to or less than the upper limit, the variation in thickness accuracy of the aspherical portion of the obtained resin sheet can be reduced and the shape accuracy can be improved. Furthermore, if the minimum distance is equal to or more than the lower limit, the strength of the obtained resin sheet can be sufficiently ensured.

[0053] [Press temperature] In the heat press process, the press temperature (mold temperature) when the thermoplastic resin film is heat pressed with a pair of molds must be 40° C. higher than the glass transition temperature (Tg) of the thermoplastic resin (Tg+40° C.) or higher, and the press temperature is preferably 50° C. higher than the glass transition temperature (Tg+50° C.) or higher, and more preferably 55° C. higher than the glass transition temperature (Tg+55° C.). If the press temperature is equal to or higher than the lower limit, the variation in thickness accuracy of the aspherical portion of the obtained resin sheet can be reduced and the shape accuracy can be increased. From the viewpoint of efficiently producing the resin sheet, the press temperature is preferably equal to or lower than 80° C. higher than the glass transition temperature (Tg+80° C.). The pressing temperature is not particularly limited, and can be appropriately adjusted by controlling the temperature of the mold according to a known general method (for example, a temperature control method using a known heater, cooler, etc.).

[0054] [Press pressure] In the heat pressing step, the pressing pressure when the thermoplastic resin film is heat pressed with a mold is increased to a final pressing pressure at a predetermined pressure increase rate, and then optionally maintained at the final pressing pressure for a predetermined time.

[0055] -Boost speed- Here, the average pressure increase rate of the press pressure must be 0.1 MPa / sec or less, preferably 0.07 MPa / sec or less, and more preferably 0.05 MPa / sec or less. If the average pressure increase rate is equal to or less than the upper limit, the birefringence of the aspheric portion of the resulting resin sheet can be reduced and the shape precision can be improved. From the viewpoint of efficiently manufacturing the resin sheet, the average pressure increase rate is preferably 0.04 MPa / sec or more.

[0056] The rate at which the press pressure is increased does not have to be constant as long as the average rate is 0.1 MPa / sec or less. However, from the viewpoint of further reducing the birefringence of the aspheric portions of the resulting resin sheet and further improving the shape precision, the rate is preferably 0.1 MPa / sec or less throughout the entire heat pressing process, more preferably 0.07 MPa / sec or less, and even more preferably 0.05 MPa / sec or less. Furthermore, from the viewpoint of further improving the shape accuracy of the aspheric portion and further reducing the variation in birefringence and thickness accuracy, in the heat pressing process, it is preferable to increase the press pressure to the final press pressure at a constant increase rate, more preferably at a constant increase rate of 0.1 MPa / sec or less, even more preferably at a constant increase rate of 0.07 MPa / sec or less, and particularly preferably at a constant increase rate of 0.05 MPa / sec or less.

[0057] -Final press pressure- The final pressing pressure is not particularly limited and can be, for example, 1 MPa to 10 MPa. If the final pressing pressure is within the above range, the shape precision of the aspheric portion of the obtained resin sheet can be further improved, and the variation in birefringence and thickness precision can be further reduced.

[0058] [Other press conditions] The pressing time in the heat pressing step is not particularly limited and can be appropriately determined depending on the type and size of the thermoplastic resin film used, the shape and size of the target resin sheet, etc. For example, the time for increasing the pressing pressure to the final pressing pressure can be 20 seconds or more and 300 seconds or less, and the time for holding the pressing pressure at the final pressing pressure can be 0 seconds or more and 180 seconds or less.

[0059] <Mold cooling process> In the mold cooling step, the pair of molds are cooled to a temperature equal to or lower than the glass transition temperature of the thermoplastic resin film to cool the heat-pressed film. By carrying out this step, the shape precision of the aspherical portion of the resulting resin sheet can be improved. The start point of the mold cooling step can be, for example, the time when temperature control for cooling the mold is started after a predetermined time has elapsed from the start of the heat pressing step, or the time when heat input to the mold is stopped after a predetermined time has elapsed from the start of the heat pressing step. The end point of the mold cooling step can be the time when the mold temperature has dropped to the mold cooling temperature described below, or the time when a predetermined time (for example, 50 seconds) has elapsed from such a time.

[0060] [Mold cooling temperature] The mold cooling temperature must be equal to or lower than the glass transition temperature (Tg) of the thermoplastic resin, and is preferably equal to or lower than a temperature 15°C lower than the glass transition temperature (Tg-15°C), and more preferably equal to or lower than a temperature 30°C lower than the glass transition temperature (Tg-30°C). The mold cooling temperature is preferably equal to or higher than a temperature 80°C lower than the glass transition temperature (Tg-80°C), and more preferably equal to or higher than a temperature 75°C lower than the glass transition temperature (Tg-75°C). If the mold cooling temperature is equal to or lower than the upper limit, the resin sheet is easily released in the release step described below, and the shape precision of the aspherical portion of the resin sheet obtained can be effectively improved. If the mold cooling temperature is equal to or higher than the lower limit, the production efficiency of the resin sheet can be further improved.

[0061] [Other mold cooling conditions] The mold cooling time and mold cooling rate are not particularly limited and can be appropriately determined depending on the type and size of the thermoplastic resin film, the shape and size of the aspherical portion of the intended resin sheet, etc. For example, the mold cooling time can be 10 seconds or more and 100 seconds or less, and the mold cooling rate can be 50° C. / min or more and 300° C. / min or less.

[0062] <Mold release process> In the demolding step, after the die cooling step, the heat-pressed film is demolded from the die to obtain a resin sheet. At this time, from the viewpoint of increasing the shape accuracy of the aspheric portion of the resin sheet, it is preferable to demold the heat-pressed film while applying tension. Here, it is preferable that the tension acts as a force along the conveying direction. In addition, the method of controlling the tension in the demolding step is not particularly limited, and can be controlled by a known method. For example, it can be controlled by a roll for unwinding the heat-pressed film, a roll for winding the heat-pressed film, or a nip roll separately provided for tension control. Furthermore, it is preferable that tension is applied continuously or intermittently to the thermoplastic resin film not only in the mold release step but also in each step from the mold heating step in which the thermoplastic resin film contacts one of the pair of molds in the above-mentioned heat pressing step until the start of the mold release step. This is because the shape precision of the aspherical part of the obtained resin sheet can be further improved. Of course, tension may also be applied to the thermoplastic resin film in other steps performed outside the above period. That is, tension may be applied to the thermoplastic resin film through all steps from the conveying step to the steps that can be performed after the mold release step.

[0063] [tension] The magnitude of tension applied to the heat press film in the transport direction is preferably 1N or more, more preferably 10N or more, and preferably 2000N or less, more preferably 1000N or less per 1m of width of the thermoplastic resin film. The "width of the thermoplastic resin film" refers to the direction perpendicular to the transport direction. If the magnitude of the tension is equal to or greater than the lower limit, the shape precision of the aspherical portion of the resulting resin sheet can be further improved. If the magnitude of the tension is equal to or less than the upper limit, the heat press film is prevented from breaking, and the manufacturing efficiency of the resin sheet can be further improved. EXAMPLES

[0064] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples. In the examples and comparative examples, the glass transition temperature of the thermoplastic resin was measured as follows. In the examples and comparative examples, the shape accuracy, thickness accuracy variations, and phase difference of the aspheric portion of the resin sheet were evaluated as follows.

[0065] <Glass transition temperature of thermoplastic resin film> The glass transition temperature (Tg) of the thermoplastic resin was measured using a differential scanning calorimeter (manufactured by SII Nano Technology, "DSC6220") at a temperature rise rate of 10°C / min in accordance with JIS K7121.

[0066] <Shape accuracy> An aspheric portion was punched out of the resin sheet to prepare a measurement sample. Next, for 300 measurement samples of the punched aspheric portions, a shape measuring instrument (Panasonic, "UA-3P") was used to measure the PV value (the maximum error in the shape of the surface of the measurement sample relative to the reference surface, i.e., the difference between the highest point (Peak) and the lowest point (Valley) within the measurement range) based on the design value of the aspheric surface. The simple average of the measured PV values ​​was then evaluated as shape accuracy according to the following criteria. A: Simple average value of PV value is 0.5μm or less B: Simple average value of PV value is more than 0.5 μm and less than 1.0 μm C: Simple average value of PV value is more than 1.0μm <Variation in thickness accuracy> An aspheric portion was punched out of the resin sheet to prepare a measurement sample. Next, the thickness of the center of 300 measurement samples of the punched aspheric portions was measured using a shape measuring instrument (manufactured by Panasonic, "UA-3P"), and the standard deviation of the measured thickness was evaluated as the variation in thickness precision according to the following criteria. A: Standard deviation is 0.1 μm or less B: Standard deviation is more than 0.1μm and less than 0.2μm C: Standard deviation is over 0.2μm <Phase difference> An aspheric portion was punched out of the resin sheet to prepare a measurement sample. Next, the phase difference was measured for 300 measurement samples from the punched aspheric portions using a resin molded lens inspection system ("WPA-100" manufactured by Photonics Lattice, Inc.). The retardation values ​​were normalized to the measurement wavelength (543 nm) and the simple average value was used to evaluate the film according to the following criteria: A smaller retardation value means a smaller birefringence. A: Simple average phase difference is 20 nm or less B: Simple average phase difference is more than 20 nm and less than 50 nm C: Simple average phase difference is more than 50 nm

[0067] Example 1 Thermoplastic resin containing a norbornene-based ring-opening polymer hydride (ZEONEX E48R (Zeon Corporation), glass transition temperature: 139°C) was placed in a film extrusion molding machine (single-screw extruder, φ=20mm, GSI Creos Corporation), melted at 260°C, extruded from a T-die, and cooled to obtain a thermoplastic resin film with a thickness of 500μm and a width of 295mm. The direction perpendicular to the width direction of the thermoplastic film was the longitudinal direction, and the film had a sufficient length for molding by roll-to-roll molding. The thermoplastic resin film obtained as described above was set in a heat press molding machine equipped with a pair of dies having a temperature control device (transportation step). The pair of dies used had the properties shown in Table 1. Then, the temperature of the mold was raised to the pressing temperature shown in Table 1, and then the thermoplastic resin film was hot-pressed under the conditions shown in Table 1 (hot-pressing step). Furthermore, while the heat-pressed film was still pressed, the pair of dies were cooled to 100° C. to cool the heat-pressed film sandwiched between the dies (die cooling step). Thereafter, the mold was opened to complete the mold cooling step, and the resin sheet having the properties shown in Table 1 was peeled off from the mold (mold releasing step). The obtained resin sheet was subjected to various evaluations as described above, and the results are shown in Table 1 together with the time required from the start of the conveying step to the completion of the demolding step (cycle time).

[0068] Example 2 Resin sheets were produced and various evaluations were carried out in the same manner as in Example 1, except that the pressure increase rate during the heat press was changed to the rate shown in Table 1. The results are shown in Table 1.

[0069] (Examples 3 to 4) Resin sheets were produced and various evaluations were carried out in the same manner as in Example 1, except that the pressing temperature was changed to the temperature shown in Table 1. The results are shown in Table 1.

[0070] (Examples 5 to 7) A resin sheet was produced and various evaluations were carried out in the same manner as in Example 1, except that the mold was changed to one shown in Table 1. The results are shown in Table 1.

[0071] Example 8 A thermoplastic resin film containing a norbornene-ethylene random copolymer obtained by random addition polymerization using norbornene and ethylene as monomers (TOPAS6013 (manufactured by Polyplastics), glass transition temperature: 138°C) was used, and a resin sheet was produced in the same manner as in Example 1, except that the pressing temperature was changed to the temperature shown in Table 1, and various evaluations were performed. The results are shown in Table 1.

[0072] Example 9 A resin sheet was produced in the same manner as in Example 1, except that a polycarbonate resin (Wonderlite PC-115 (manufactured by Asahi Kasei Corporation), glass transition temperature: 145° C.) was used as the thermoplastic resin film and the pressing temperature was changed to the temperature shown in Table 1, and various evaluations were performed. The results are shown in Table 1.

[0073] Example 10 A resin sheet was produced in the same manner as in Example 1, except that a polymethyl methacrylate resin (Delpet 80NH (manufactured by Asahi Kasei Chemicals Corporation), glass transition temperature: 100° C.) was used as the thermoplastic resin film and the pressing temperature was changed to the temperature shown in Table 1, and various evaluations were performed. The results are shown in Table 1.

[0074] Example 11 A resin sheet was produced in the same manner as in Example 1, except that a polyester resin (OKP-1 (manufactured by Osaka Gas Chemicals Co., Ltd.), glass transition temperature: 132°C) was used as the thermoplastic resin film and the pressing temperature was changed to the temperature shown in Table 1, and various evaluations were performed. The results are shown in Table 1.

[0075] Comparative Example 1 Resin sheets were produced and various evaluations were carried out in the same manner as in Example 1, except that the pressure increase rate during the heat press was changed to the rate shown in Table 1. The results are shown in Table 1.

[0076] Comparative Example 2 Resin sheets were produced and various evaluations were carried out in the same manner as in Example 1, except that the pressing temperature was changed to the temperature shown in Table 1. The results are shown in Table 1.

[0077] Comparative Example 3 A resin sheet was produced and various evaluations were carried out in the same manner as in Example 1, except that the mold was changed to one shown in Table 1. The results are shown in Table 1.

[0078] [Table 1]

[0079] From Table 1, it can be seen that the resin sheets of Examples 1 to 11 have a small variation in thickness accuracy and have multiple aspherical portions with high shape accuracy. It can also be seen that the resin sheet of Comparative Example 1 has low shape accuracy of the aspherical portions, and furthermore, the resin sheets of Comparative Examples 2 and 3 have large variation in thickness accuracy of the aspherical portions and low shape accuracy. [Industrial Applicability]

[0080] According to the present invention, it is possible to provide a resin sheet having a plurality of aspheric portions with small variation in thickness accuracy and high shape accuracy. [Explanation of symbols]

[0081] 10 Resin sheet 11 Aspherical part

Claims

1. A method for producing a resin sheet having a plurality of aspherical portions spaced apart from one another by hot press molding a thermoplastic resin film formed using a thermoplastic resin, comprising the steps of: The heat press molding is performed at a press temperature that is 40° C. or more higher than the glass transition temperature of the thermoplastic resin, and the press pressure is increased to a final press pressure at an average pressure increase rate of 0.1 MPa / sec or less.

2. The method for producing a resin sheet according to claim 1 , wherein the pressing pressure is increased to a final pressing pressure at a constant pressure increase rate of 0.1 MPa / sec or less.

3. The method for producing a resin sheet according to claim 1 , wherein at least one surface of the aspherical portion has a cross-sectional shape in a thickness direction having an inflection point.

4. A resin sheet having a plurality of aspherical portions formed by using a thermoplastic resin, The density of the aspherical portions is 0.16 pieces / cm 2 That's all. The minimum distance between adjacent aspheric portions is 1.0 mm or more; The diameter of the aspherical portion in a plan view is 1 mm or more and 15 mm or less, The phase difference of the aspherical portion is 50 nm or less, A resin sheet having a thickness of 500 μm or less at its thinnest portion.

5. The resin sheet according to claim 4 , wherein the variation in thickness precision of the aspheric portion is 0.2 μm or less.

6. The resin sheet according to claim 4 , wherein at least one surface of the aspheric portion has a cross-sectional shape in a thickness direction having an inflection point.

7. The heat press molding is performed by heat pressing the thermoplastic resin film using at least a pair of dies, The method for manufacturing a resin sheet according to any one of claims 1 to 3, wherein at least one of the pair of molds has a plurality of cavity portions which are aspheric portion forming regions, and the minimum distance between adjacent cavity portions is 1.0 mm or more.

Citation Information

Patent Citations

  • Lens array sheet and its forming method

    JP2004198536A

  • Manufacturing method of plastic thin film

    JP2009090616A

  • Method and apparatus for manufacturing shaped article

    JP2010264652A

  • Method and apparatus for manufacturing molding

    JP2011224990A

  • Microlens array, method for manufacturing microlens array, light-emitting device and illuminating device

    JP2012181515A