container

The container design with a hard resin outer and elastomer-covered openings enhances air barrier properties, preventing deterioration and leakage, and facilitates easy dispensing of contents.

JP7589749B2Active Publication Date: 2024-11-26TOAGOSEI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022563809
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2021-11-17
Publication Date
2024-11-26
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

Existing adhesive and sealant containers lack adequate air barrier properties, leading to deterioration and leakage due to air ingress, and the applicator tip is not adequately protected, resulting in poor sealing and potential contamination.

Method used

A container design featuring a hard resin outer container enclosing a flexible inner container, with elastomer-covered openings and a cap that covers the nozzle, providing improved air barrier properties and easy content discharge.

Benefits of technology

The design prevents air ingress, maintains content integrity, and ensures easy dispensing, reducing deterioration and leakage, while allowing for secure handling and storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589749000006
    Figure 0007589749000006
  • Figure 0007589749000007
    Figure 0007589749000007
  • Figure 0007589749000008
    Figure 0007589749000008
Patent Text Reader

Abstract

A container according to the present invention comprises: an inner container provided with a nozzle part that discharges an adhesive filled therein; a cylindrical outer container made of a hard resin, the outer container enclosing the inner container and having an opening formed in an outer circumferential wall; a pressing part made of an elastomer, the pressing part being provided on the outer circumferential wall of the outer container and covering the opening; and a cap covering the nozzle part projected from the outer container and being attachable to and removable from the outer container.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a container. [Background technology]

[0002] JP 2019-508236 A describes an apparatus for applying an adhesive and / or sealant, the apparatus comprising a housing for accommodating a container, the housing including an accommodation space for accommodating the container, a closable application tip connected to the accommodation space and capable of discharging the adhesive and / or sealant, a stable casing for the accommodation space, and at least one area of ​​the housing designed as a deformable pressure area and capable of applying pressure from the outside onto the container that can be placed in the accommodation space. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2019-508236 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the device described in JP-A-2019-508236, the deformable pressure area that applies pressure to the container is a leaf spring formed by forming a slit in the housing. As is clear from this, in this device, the sealing property of the housing itself is not taken into consideration. In addition, in the device described in Patent Document 1, the application tip is not housed in the housing, and the closing cap covers only a part of the application tip. In other words, in the device described in Patent Document 1, the sealing property of the container is not ensured by the housing, and the entire application tip is not protected. For this reason, air is likely to enter the container and the application tip is likely to deteriorate, which may cause the adhesive and / or sealant in the container to deteriorate. In addition, in the device described in JP 2019-508236 A, the leaf spring does not bend unless the free end of the leaf spring is pressed, and pressure cannot be applied to the container. The present disclosure has been made in consideration of the above-mentioned current situation, and provides a container that has improved air barrier properties and allows the contents of an inner container enclosed in an outer container to be easily discharged. [Means for solving the problem]

[0005] The container of the first embodiment comprises an inner container having a nozzle portion for dispensing the filled contents, a cylindrical outer container made of hard resin that contains the inner container and has an opening formed in its outer wall, an elastomer pressing portion provided on the outer wall and covering the opening, and a cap that covers the nozzle portion protruding from the outer container and is detachable from the outer container.

[0006] A container according to a second aspect is the container according to the first aspect, further comprising a seat at an end of the outer container opposite the cap.

[0007] A container according to a third aspect is the container according to the first or second aspect, wherein a pair of the openings covered by the pressing portion are provided symmetrically with respect to a central axis of the outer container.

[0008] The container according to a fourth aspect is the container according to the third aspect, further comprising the elastomer connecting portion that connects the pair of pressing portions together so that they are wrapped around the outer peripheral wall of the outer container.

[0009] A container according to a fifth aspect is the container according to the fourth aspect, further comprising an elastomer extension portion extending from the connecting portion toward the base of the outer container.

[0010] A container according to a sixth aspect is the container according to any one of the first to fifth aspects, wherein a plurality of ribs are formed on the outer periphery of the cap.

[0011] A container according to a seventh aspect is the container according to any one of the first to sixth aspects, wherein the outer peripheral wall of the outer container increases in diameter from the end on the cap side toward the seat.

[0012] A container according to an eighth embodiment is the container according to any one of the first to seventh embodiments, wherein the content is an adhesive.

[0013] A container according to a ninth aspect is the container according to the eighth aspect, wherein the inner container is made of polyolefin.

[0014] A container according to a tenth aspect is the container according to the ninth aspect, wherein the cap is made of polyolefin.

[0015] The container according to an eleventh aspect is the container according to any one of the second to tenth aspects, further comprising a desiccant on the inside of the base.

[0016] A container according to a twelfth aspect is the container according to any one of the first to eleventh aspects, wherein a recess is formed on the surface of the pressing portion.

[0017] A container according to a thirteenth aspect is the container according to any one of the first to twelfth aspects, wherein the pressing portion has a protruding portion protruding from an outer peripheral wall of the outer container.

[0018] A container according to a fourteenth aspect is the container according to the thirteenth aspect, wherein the maximum thickness of the raised portion is within the range of 0.2 mm or more and 1.0 mm or less.

[0019] A container according to a fifteenth aspect is the container according to any one of the first to fourteenth aspects, wherein the elastomer has an A hardness in the range of 40 or more and less than 80.

[0020] A container according to a sixteenth aspect is the container according to any one of the first to fifteenth aspects, wherein the elastomer has a moisture permeability of 2.0 g / m2 for a sample having a thickness of 0.5 mm as measured in accordance with JIS Z 0208. 2 Less than 24 hours.

[0021] A container according to a seventeenth aspect is the container according to any one of the first to sixteenth aspects, wherein the elastomer has an oxygen permeability coefficient of 1.0×10 measured in accordance with JIS K 7126. -15 mol m / Pa s m 2 is less than. Effect of the Invention

[0022] In the container according to the first aspect, the opening formed in the outer peripheral wall of the outer container is covered with a pressing part made of an elastomer, so that the content filled in the inner container can be easily discharged from the nozzle by pressing the pressing part with a finger to press the inner container.

[0023] Furthermore, in the container according to the first aspect, the cap is attached to the outer container and covers the nozzle portion protruding from the outer container, which improves the air barrier properties of the container compared to a configuration in which the cap is detachably provided on the inner container.

[0024] Furthermore, according to the container of the first aspect, the inner container is enclosed in a cylindrical outer container made of hard resin, which prevents the contents from being discharged from the nozzle of the inner container even if the container is pressed carelessly.

[0025] According to the container of the second aspect, the container can be stood on a workbench or the like with the base facing down and the nozzle portion facing up.

[0026] According to the container of the third aspect, when the pair of pressing portions is pressed to eject the contents from the nozzle portion, the pair of pressing portions can be easily pinched and pressed with the thumb and index finger.

[0027] According to the container of the fourth aspect, the pressing parts are prevented from peeling off from the outer container, compared to a configuration in which the pair of pressing parts are not integrally connected.

[0028] According to the container of the fifth aspect, the peeling of the pressing portion from the outer container is suppressed, compared to a configuration without an extension portion.

[0029] According to the container of the sixth aspect, the cap can be easily gripped when attaching or detaching the cap.

[0030] According to the container of the seventh aspect, the outer container has a larger diameter from the end on the cap side toward the base, which makes it less likely to tip over when placed on a workbench or the like with the nozzle facing up.

[0031] According to the container of the eighth aspect, the adhesive filled in the inner container is less likely to deteriorate when not in use.

[0032] According to the container of the ninth aspect, the adhesive remaining inside the inner container is less likely to harden.

[0033] According to the container of the tenth aspect, the adhesive remaining on the tip of the nozzle portion covered with the cap is less likely to harden.

[0034] According to the container of the eleventh aspect, the internal space of the container can be dried.

[0035] According to the container of the twelfth aspect, when pressing the pressing portion, the thumb and index finger can fit into the recess.

[0036] According to the container of the thirteenth aspect, the position of the pressing part can be determined by feel.

[0037] According to the container of the fourteenth aspect, the position of the pressing part can be easily determined by touch, compared to a configuration in which the maximum thickness of the raised part is less than 0.2 mm, and the inner container can be easily pressed by pressing the pressing part with the thumb and index finger, compared to a configuration in which the maximum thickness of the raised part is more than 1.0 mm.

[0038] According to the container of the fifteenth aspect, it is easier to adjust the amount of the content discharged by pressing the pressing part, compared to a configuration in which the elastomer has an A-hardness of less than 40. Also, it is easier to adjust the amount of the content discharged by pressing the pressing part, compared to a configuration in which the elastomer has an A-hardness of 80 or more.

[0039] According to the container of the sixteenth embodiment, the moisture permeability of the elastomer in a sample having a thickness of 0.5 mm is 2.0 g / m 2 The water vapor barrier properties of the container are improved compared to configurations with a shelf life of 24 hours or more.

[0040] According to the container of the seventeenth aspect, the oxygen permeability coefficient of the elastomer is 1.0×10 -15 mol m / Pa s m 2 Compared with the above configuration, the air barrier properties of the container are improved. [Brief description of the drawings]

[0041] [Figure 1] FIG. 2 is a front view of a container according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a side view of a container according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a front cross-sectional view of a container according to an embodiment of the present disclosure. [Figure 4] FIG. 2 is a cross-sectional front view of a container according to an embodiment of the present disclosure with the cap removed. [Diagram 5] 1 is an enlarged front cross-sectional view of a container according to an embodiment of the present disclosure, showing the area around a pressing portion. [Figure 6] FIG. 1 is a perspective view of a container according to an embodiment of the present disclosure. [Figure 7] FIG. 1 is a perspective view of a container according to an embodiment of the present disclosure with the cap removed. [Figure 8] FIG. 2 is an exploded perspective view of a container according to an embodiment of the present disclosure. [Figure 9] FIG. 2 is a perspective view of an outer container according to an embodiment of the present disclosure. [Figure 10]FIG. 1 is a schematic diagram of an outer container being held between thumb and index finger according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] An example of a container according to an embodiment of the present disclosure will be described with reference to FIGS.

[0043] The matters shown herein are illustrative and are for illustrative purposes of the embodiments of the present disclosure, and are described for the purpose of providing what is believed to be the most effective and easily understandable explanation of the principles and conceptual features of the present disclosure. In this respect, it is not intended to show structural details of the present disclosure beyond the extent necessary for a fundamental understanding of the present disclosure, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present disclosure can be actually embodied.

[0044] (container 10) 8, the container 10 according to this embodiment includes an inner container 20 filled with a content, and an outer container 70 that encloses and protects the inner container 20. A cap 40 and a base 50 are attached to the outer container 70. A desiccant 60 is accommodated in the base 50.

[0045] (Inner container 20) The inner container 20 includes a main body 22 and a nozzle 24. As shown in Figs. 3, 4 and 8, the main body 22 is a cylindrical member with a bottom that extends in one direction. The main body 22 is flexible. The main body 22 has a bottom 22a and an opening 22b formed at the end opposite the bottom 22a. A male screw portion 22c is formed on the outer circumferential wall of the end of the main body 22 on the opening 22b side.

[0046] An example of the contents is a liquid, paste, or jelly adhesive, which is filled inside the main body 22. Specific examples of the adhesive include a 2-cyanoacrylate adhesive, an epoxy resin adhesive, a rubber adhesive, a urethane resin adhesive, and a silicone resin adhesive.

[0047] In the present disclosure, the contents filled in the main body 22 of the inner container 20 are not limited to adhesives, and their properties are not limited to liquid, paste, or jelly. The contents in the present disclosure may be, for example, chemical products such as hardeners, coating agents, shoe polish, and wax, food products such as wasabi, ginger, mustard, garlic, and chocolate, daily necessities such as toothpaste, cosmetics, and hair dye, medicines such as ointments, and stationery such as paints.

[0048] (Nozzle part 24) The nozzle portion 24 is provided at the end of the opening 22b side of the main body portion 22, and is a substantially cylindrical member that extends in one direction and has both ends open in the longitudinal direction. The nozzle portion 24 has a tapered tip portion 24a on the opposite side of the opening 22b of the main body portion 22. The nozzle portion 24 has an expanded diameter portion 24b, which is a peripheral wall having a larger diameter than the peripheral walls of the other nozzle portions 24, at the end of the opening 22b side of the main body portion 22. In addition, a female thread portion 24c corresponding to the male thread portion 22c of the main body portion 22 is formed on the inner peripheral wall of the expanded diameter portion 24b of the nozzle portion 24. The nozzle portion 24 is connected to the main body portion 22 by screwing the female thread portion 24c into the male thread portion 22c.

[0049] The main body 22 of the inner container 20 is flexible. As a result, when the peripheral wall of the main body 22 is pressed, the contents such as adhesive filled in the main body 22 are discharged from the opening on the tip 24a side of the nozzle 24.

[0050] The inner container 20 is preferably formed of a material that is inactive to the adhesive and does not have permeability or transparency to the adhesive. Specifically, the inner container 20 is preferably formed of a polyolefin resin such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate, and more preferably formed of a polyolefin resin. That is, the inner container 20 is more preferably made of polyolefin. The material forming the inner container 20 according to the present disclosure is not particularly limited, and may be a material such as a metal such as aluminum, tin, or lead.

[0051] (outer container 70) 9, the outer container 70 is a member that encloses the inner container 20 with the tip of the nozzle portion 24 protruding. The outer container 70 includes a main body portion 72 and an elastomer portion 80.

[0052] (Main body portion 72) The main body 72 is a generally cylindrical member extending in one direction and opening at both ends in the longitudinal direction. The outer peripheral wall of the main body 72 expands in diameter in a generally tapered manner from the end on the nozzle portion 24 side of the inner container 20 to the end opposite the nozzle portion 24. As shown in Fig. 8, the inner container 20 is inserted into the inside of the main body 72 from the opening opposite the side from which the tip of the nozzle portion 24 of the inner container 20 protrudes. Also, as shown in Figs. 3 and 4, the main body 72 has a structure that can be fitted with the outer diameter portion of the expanded diameter portion 24b of the inner container 20 so that the tip of the nozzle portion 24 of the inner container 20 inserted into the main body 72 protrudes.

[0053] The main body 72 has a male thread portion 72a formed on the outer peripheral wall at the end on the nozzle portion 24 side of the inner container 20. In addition, the main body 72 has a fitting portion 72b formed on the end opposite to the side where the tip of the nozzle portion 24 of the inner container 20 protrudes, the fitting portion 72b having a structure capable of fitting with the inner wall of the outer peripheral wall of the base 50, which will be described later.

[0054] 3, 4, and 9, an opening 74 is formed in a substantially rectangular shape penetrating the outer peripheral wall of the main body 72 at a portion overlapping a portion of the outer peripheral wall that is closer to the bottom than the male thread portion 22c of the main body 22 of the inner container 20 when viewed in the radial direction of the main body 72. The opening 74 is rectangular when viewed in the radial direction of the main body 72, and a pair of openings 74 are formed in the outer peripheral wall of the main body 72 at positions that are symmetrical with respect to the central axis of the main body 72. That is, a pair of openings 74 is provided in the outer peripheral wall of the outer container 70, symmetrical with respect to the central axis of the outer container 70.

[0055] 9, a covering portion 76 is formed on the outer peripheral wall of the main body portion 72 at least around the opening 74, which is recessed with respect to the outer peripheral wall and is a portion that covers an elastomer portion 80 described below. The covering portion 76 has a first covering portion 77 formed between the male thread portion 72a and the fitting portion 72b, and a second covering portion 78 formed on the fitting portion 72b.

[0056] The first covering portion 77 is formed so as to be wound around the pair of openings 74 in the circumferential direction on the outer peripheral wall of the main body portion 72. In other words, the openings 74 are located between the edges on both sides of the first covering portion 77 in the axial direction of the main body portion 72. A pair of rib portions 77a extending along the axial direction and standing in the radial direction so as to be flush with the outer peripheral wall of the main body portion 72 is formed in a part of the portion of the first covering portion 77 sandwiched between the pair of openings 74 in the circumferential direction. The first covering portion 77 also has a groove-shaped first extension groove 77b extending along the axial direction of the outer container toward the fitting portion 72b and connected to the second covering portion 78.

[0057] The second covering portion 78 is formed such that a part of the peripheral wall of the fitting portion 72b is wrapped around the outer peripheral wall of the other fitting portion 72b in a ring shape in the circumferential direction. The second covering portion 78 also extends along the axial direction of the outer container 70 toward the first extension groove 77b of the first covering portion 77, and has a groove-shaped second extension groove 78b that bites into the first extension groove 77b.

[0058] The main body 72 is made of a hard resin. The hard resin forming the main body 72 is preferably a synthetic resin that is inactive to the adhesive and does not have permeability or transparency to the adhesive. Specifically, the hard resin forming the main body 72 is preferably a polyolefin resin such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, or ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate, and more preferably a polyolefin resin.

[0059] In the outer peripheral wall of the main body 72, the portion overlapping with the main body 22 of the inner container 20 when viewed from the radial direction preferably has a maximum thickness in the range of 1.0 mm to 2.0 mm. More preferably, the maximum thickness of this portion is in the range of 1.2 mm to 1.8 mm. In this embodiment, the maximum thickness of this portion is 1.5 mm.

[0060] The elastomer portion 80 will be described in detail later.

[0061] (Cap 40) 1 to 3, 6 and 8, the cap 40 is detachably provided on the end of the outer container 70, which is the side from which the nozzle portion 24 of the inner container 20 protrudes. The cap 40 is a cylindrical member that covers the nozzle portion 24 of the inner container 20 protruding from the outer container 70. The cap 40 has an outer cylindrical portion 42 and an inner cylindrical portion 44.

[0062] The outer cylinder 42 is a cylindrical part with one end closed and the other end open. The closed part of the outer cylinder 42 is the top 42a. A female thread 42b corresponding to the male thread 72a of the outer container 70 is formed on the inner periphery of the opening side of the outer cylinder 42. The cap 40 is attached to the outer container 70 by screwing the female thread 42b of the outer cylinder 42 into the male thread 72a of the outer container 70. The outer cylinder 42 is tapered from the top 42a to the opening. When the cap 40 is attached to the outer container 70, the wall surface of the outer periphery of the outer cylinder 42 is along the wall surface of the outer peripheral wall of the outer container 70 and is approximately flush with the wall surface.

[0063] The outer tubular portion 42 is formed with a plurality of ribs 42c which stand radially from the outer periphery of the outer tubular portion 42 and extend along the axial direction of the outer tubular portion 42. Specifically, the outer tubular portion 42 is formed with four ribs 42c symmetrically with respect to the central axis of the outer tubular portion 42.

[0064] The inner cylinder portion 44 is a cylindrical portion that stands from the inner wall of the top portion 42a of the outer cylinder portion 42 toward the opening of the outer cylinder portion 42. The end of the inner cylinder portion 44 on the opening side of the outer cylinder portion 42 is open. When the cap 40 is attached to the outer container 70, the inner cylinder portion 44 fits into the outer peripheral wall of the tip portion 24a of the nozzle portion 24 of the inner container 20 to accommodate the tip portion 24a inside.

[0065] The cap 40 is made of a hard resin. The hard resin forming the cap 40 is preferably a synthetic resin that is inactive to the adhesive and does not have permeability or transparency to the adhesive. Specifically, the hard resin forming the cap 40 is preferably a polyolefin resin such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, or ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate, and more preferably a polyolefin resin.

[0066] (Pedestal 50) 1 to 3, 6 and 8, the base 50 is a cylindrical member detachably provided on the fitting portion 72b of the outer container 70. The base 50 has an outer cylindrical portion 52, an inner cylindrical portion 54, and a connecting portion 56.

[0067] The outer cylinder portion 52 is a cylindrical portion with both ends open. One end of the outer cylinder portion 52 is a fitting portion 52a that is attached to the outer container 70 by fitting the inner peripheral wall of the end to the outer peripheral wall of the fitting portion 72b of the outer container 70. The end of the outer cylinder portion 52 opposite to the fitting portion 52a is a leg portion 52b. The end face of the leg portion 52b of the outer cylinder portion 52 attached to the outer container 70 is perpendicular to the central axis of the outer container 70. The outer peripheral portion of the outer cylinder portion 52 expands in diameter from the fitting portion 52a side to the leg portion 52b side. When the base 50 is attached to the outer container 70, the wall surface of the outer peripheral portion of the outer cylinder portion 52 is along the wall surface of the outer peripheral wall of the outer container 70 and is approximately flush.

[0068] The inner cylinder portion 54 is disposed inside the outer cylinder portion 52, and is a cylindrical portion with a bottom that is open at the end on the fitting portion 52a side. The connecting portion 56 connects the outer cylinder portion 52 and the inner cylinder portion 54, and is a portion that separates the space between the outer cylinder portion 52 and the inner cylinder portion 54 so that the fitting portion 52a side and the leg portion 52b side do not communicate with each other.

[0069] The base 50 is made of a hard resin. The hard resin forming the base 50 is preferably a synthetic resin that is inactive to the adhesive and does not have permeability or transparency to the adhesive. Specifically, the hard resin forming the base 50 is preferably a polyolefin resin such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, or ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate, and more preferably a polyolefin resin.

[0070] When the base 50 and the cap 40 are attached to the outer container 70, the internal space of the container 10 is sealed. That is, when the base 50 and the cap 40 are attached to the outer container 70, the container 10 has air barrier properties.

[0071] (Desiccant 60) The desiccant 60 is a cylindrical member housed inside the inner cylinder portion 54 of the base 50. The desiccant 60 absorbs moisture contained in the air in the space surrounded by the outer container 70, the cap 40, and the base 50. In other words, the desiccant 60 absorbs moisture contained in the air in the internal space of the container 10.

[0072] (Elastomer part 80) 1 to 4, 8 and 9, the elastomer portion 80 is an elastomer member provided on the outer peripheral wall of the main body portion 72 and covering the covering portion 76. The elastomer portion 80 has a first elastomer portion 82 covering the first covering portion 77 and a second elastomer portion 90 covering the second covering portion 78.

[0073] (First elastomer portion 82) The first elastomer portion 82 is provided so as to cover the first covering portion 77 of the main body portion 72, and is formed so as to be wound circumferentially around the outer circumferential wall of the main body portion 72. The first elastomer portion 82 has a pressing portion 84 and a connecting portion 86. The first elastomer portion 82 is formed so that a portion other than the pressing portion 84 is substantially flush with the outer circumferential wall of the main body portion 72.

[0074] (Pressing portion 84) The pressing portion 84 is a portion of the first elastomer portion 82 that covers the openings 74 of the main body portion 72. A pair of pressing portions 84 are formed corresponding to the pair of openings 74. The pressing portion 84 has a raised portion 84a and a recessed portion 84b.

[0075] 1, 2, and 5 to 9, the raised portion 84a is a portion of the pressing portion 84 that is raised from the outer peripheral wall of the main body portion 72 and has a substantially rectangular shape when viewed in the radial direction of the main body portion 72. The maximum thickness T max The maximum thickness T of the raised portion 84a is preferably within a range of 0.2 mm or more and 1.0 mm or less. maxMore preferably, the maximum radial thickness T of the raised portion 84a in the embodiment is in the range of 0.3 mm or more and 0.5 mm or less. max is 0.35 mm.

[0076] The recess 84b is formed in the center of the surface of the raised portion 84a, and is an elliptical depression concave with respect to the raised portion 84a when viewed from the radial direction. The maximum depth of the recess 84b is preferably in the range of 0.2 mm or more and 0.8 mm or less. Furthermore, the maximum depth of the recess 84b is more preferably in the range of 0.4 mm or more and 0.6 mm or less. In the embodiment, the maximum depth of the recess 84b is 0.5 mm.

[0077] The pressing portion 84 is formed such that a portion on the inner peripheral wall side of the main body portion 72 is substantially flush with the inner peripheral wall of the main body portion 72. In addition, the pressing portion 84 is elastically deformed when pressed radially from the outer peripheral side, and can press the outer peripheral wall of the main body portion 22 by reaching the main body portion 22 of the inner container 20.

[0078] (Connection part 86) The connecting portion 86 is a portion of the first elastomer portion 82 that integrally connects the pair of pressing portions 84 to the first covering portion 77 of the outer peripheral wall of the main body portion 72 so as to be wound in the circumferential direction. The connecting portion 86 is formed along the first covering portion 77. The connecting portion 86 has a first extension portion 86a formed in the first extension groove 77b of the first covering portion 77. The first extension portion 86a extends along the first extension groove 77b toward the fitting portion 72b, and is connected to the second elastomer portion 90. That is, the first extension portion 86a of the connecting portion 86 extends toward the seat 50 that fits with the fitting portion 72b. The first extension portion 86a is an example of an extension portion.

[0079] (Second elastomer portion 90) The second elastomer portion 90 is provided so as to cover the second covering portion 78 of the fitting portion 72b, and is formed so as to be wound around the second covering portion 78 on the outer peripheral wall of the fitting portion 72b in the circumferential direction. The second elastomer portion 90 is formed in the second extension groove 78b of the fitting portion 72b, and has a second extension portion 92 that integrally connects the second elastomer portion 90 to the first extension portion 86a of the first elastomer portion 82. The second elastomer portion 90 is formed so as to be approximately flush with the outer peripheral wall of the fitting portion 72b.

[0080] (Regarding the material of the elastomer portion 80) The elastomer forming the elastomer portion 80 preferably has flexibility (A hardness), air barrier properties (moisture permeability, oxygen permeability coefficient), moldability, and fusion properties. Specifically, the elastomer is preferably an elastomer composition X containing an isobutylene block copolymer A composed of an isobutylene polymer block and an aromatic vinyl polymer block, and a medium-low pressure polyethylene resin B. The elastomer portion 80 in this embodiment is formed from the elastomer composition X.

[0081] The isobutylene polymer block is a block containing a structural unit derived from an isobutylene compound (hereinafter also referred to as an isobutylene compound unit).

[0082] Of all the structural units constituting the isobutylene polymer block, the content of the isobutylene compound units is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, from the viewpoint of water vapor barrier properties at high temperatures.

[0083] The isobutylene polymer block may contain structural units derived from monomers other than isobutylene, as long as the effects of the present disclosure are not impaired. Examples of other monomers include aliphatic olefins, alicyclic olefins, aromatic vinyls, dienes, vinyl ethers, vinyl silanes, vinyl carbazole, β-pinene, and acenaphthylene.

[0084] The content of the isobutylene polymer block in the isobutylene block copolymer A is preferably from 50 to 90% by mass, more preferably from 55 to 85% by mass, and further preferably from 60 to 80% by mass.

[0085] The aromatic vinyl polymer block contains a structural unit derived from an aromatic vinyl compound (hereinafter also referred to as an aromatic vinyl compound unit). Examples of the aromatic vinyl compound include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,3-dimethylstyrene, vinylnaphthalene, etc., and two or more of these may be used in combination. Among these, styrene, which is easily available, is preferred.

[0086] The content of aromatic vinyl compound units in all structural units constituting the aromatic vinyl polymer block is preferably 80 mass % or more, more preferably 90 mass % or more, and even more preferably 95 mass % or more.

[0087] The aromatic vinyl polymer block may contain structural units derived from monomers other than aromatic vinyl compounds, as long as the effects of the present disclosure are not impaired. Examples of such other monomers include copolymerizable monomers capable of ion polymerization, such as butene, pentene, hexene, butadiene, isoprene, and methyl vinyl ether.

[0088] From the viewpoint of moldability, the content of the aromatic vinyl polymer block in the isobutylene block copolymer A is preferably 10 to 60 mass %, more preferably 15 to 50 mass %, and further preferably 20 to 40 mass %.

[0089] The weight average molecular weight of the isobutylene block copolymer A is preferably 10,000 or more from the viewpoint of air barrier property, and is preferably 300,000 or less from the viewpoints of flexibility and moldability. From these viewpoints, the weight average molecular weight of the isobutylene block copolymer A is preferably 10,000 to 300,000, more preferably 20,000 to 200,000, and even more preferably 30,000 to 100,000.

[0090] The isobutylene block copolymer A has an A hardness of preferably 10-50, more preferably 15-45, and further preferably 20-40.

[0091] The density of the isobutylene block copolymer A is preferably 0.920 to 0.970 g / cm 3 , more preferably 0.930 to 0.960 g / cm 3 , and more preferably 0.940 to 0.950 g / cm 3 It is.

[0092] The content of the isobutylene block copolymer A in the elastomer composition X is preferably from 25 to 99 mass %, more preferably from 25 to 98 mass %, and further preferably from 50 to 95 mass %.

[0093] From the viewpoint of fusion adhesion, the elastomer composition used in the container of the present disclosure preferably contains a polyethylene resin. Polyethylene resins can be roughly divided into medium- and low-pressure polyethylene resins and high-pressure polyethylene resins according to the difference in the production method, and linear high-density polyethylene resins (HDPE) are obtained by the medium- and low-pressure method, while low-density polyethylene resins (LDPE) with long chain branches are obtained by the high-pressure method. High-density polyethylene resins have high air barrier properties, while low-density polyethylene resins have low air barrier properties. Furthermore, in recent years, linear low-density polyethylene resins (L-LDPE) have also been known as a third polyethylene resin produced by the medium-pressure method, and their air barrier properties are higher than those of high-pressure polyethylene resins. Therefore, as the medium- and low-pressure polyethylene resins in the present disclosure, at least one of high-density polyethylene resins and linear low-density polyethylene resins is preferable, and high-density polyethylene resins are more preferable.

[0094] High-density polyethylene resin is produced by polymerizing ethylene at temperatures of 50 to 250°C and pressures of 50 to 200 atmospheres using a Ziegler catalyst (titanium-based) in the low-pressure method or a Phillips catalyst (chromium-based) in the medium-pressure method.

[0095] The density of the high density polyethylene resin is preferably 0.942 g / cm from the viewpoint of air barrier property. 3 More preferably, it is 0.945 to 0.970 g / cm 3 It is.

[0096] The density of the linear low-density polyethylene resin is preferably 0.915 to 0.935 g / cm from the viewpoint of air barrier property. 3 , more preferably 0.918 to 0.930 g / cm 3 It is.

[0097] While high density polyethylene resin (HDPE) and low density polyethylene resin (LDPE) are homopolyethylene polymers, linear low density polyethylene resin (L-LDPE) is a copolymer of ethylene and α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 3-methylpentene-1, 1-octene, 1-decene, and 4-methylpentene-1.

[0098] Of all the structural units constituting the linear low-density polyethylene resin, the content of structural units derived from α-olefin is preferably 4 to 17% by mass, more preferably 5 to 15% by mass.

[0099] Linear low-density polyethylene resin is produced by copolymerizing ethylene and α-olefin using a Phillips catalyst used in the medium pressure process. The copolymerization components give the conventional high-density polyethylene resin a short-branched structure, and the density is appropriately reduced by utilizing these short-chain branches. Therefore, linear low-density polyethylene resin is a polyethylene resin having a structure that is more linear than low-density polyethylene resin (LDPE) produced by a conventional high-pressure method and has more branches than high-density polyethylene resin. Linear low-density polyethylene resin can be produced by applying a production process of gas phase polymerization using a fluidized bed reactor, a stirred bed reactor, a tubular reactor, etc., for example, based on the method (gas phase polymerization method using a fluidized bed reactor) described in JP-A-54-148093 and JP-A-54-154488, etc.

[0100] From the viewpoint of moldability, the medium / low pressure polyethylene resin B has a melt mass flow rate (MFR) of preferably 0.5 to 50 g / 10 min, more preferably 1 to 30 g / 10 min, and further preferably 1.5 to 25 g / 10 min at 190° C. and a load of 21.2 N.

[0101] The moisture permeability of medium and low pressure polyethylene resin B is 2.0 g / m 2 Less than 24 hours is preferable, and 1.8 g / m is more preferable. 2 Less than 24h, preferably 1.6g / m 2 Less than 24h, preferably 1.0g / m 2 The moisture permeability here is the moisture permeability of a sheet sample having a thickness of 0.5 mm measured according to JIZ 0208 (cup method) at 40°C.

[0102] The oxygen permeability coefficient of medium and low pressure polyethylene resin B is 1.0×10 -15 mol m / Pa s m 2 Preferably, less than 0.8×10 -15 mol m / Pa s m 2 less than 0.6×10 -15 mol m / Pa s m 2 The oxygen permeability coefficient herein is a value measured by a method in accordance with JIS K 7126.

[0103] The content of medium- and low-pressure polyethylene resin B is 5 parts by mass or more from the viewpoints of moldability and fusion property, and 300 parts by mass or less from the viewpoint of flexibility, relative to 100 parts by mass of isobutylene block copolymer A. From these viewpoints, the content of medium- and low-pressure polyethylene resin B is 1 to 100 parts by mass, preferably 2 to 70 parts by mass, more preferably 3 to 60 parts by mass, and even more preferably 5 to 30 parts by mass, relative to 100 parts by mass of isobutylene block copolymer A.

[0104] From the viewpoint of flexibility, the content of the medium / low pressure polyethylene resin B in the elastomer composition X is preferably 0.5 to 50 mass %, more preferably 1 to 30 mass %, and further preferably 4 to 25 mass %.

[0105] From the viewpoints of flexibility and moldability, the elastomer composition X may further contain a rubber softener C. Examples of the rubber softener C include mineral oils such as paraffin oil, naphthene oil, and aromatic oil, and synthetic softeners such as polyolefin-based oils such as poly-α-olefin and polybutene, and among these, from the viewpoint of water vapor barrier properties, polyolefin-based oils are preferred, and polybutene oil is more preferred.

[0106] The kinetic viscosity of the rubber softener C at 40°C is preferably 3,000 to 20,000 mm from the viewpoint of long-term heat resistance and air barrier property. 2 / s, more preferably 4,000 to 17,500 mm 2 / s, and more preferably 5,000 to 15,000 mm 2 / s.

[0107] The number average molecular weight of the rubber softener C is preferably 600 to 2000, more preferably 800 to 1500, and further preferably 900 to 1200, from the viewpoints of long-term heat resistance and air barrier property.

[0108] Moreover, the content of the rubber softener C in the elastomer composition X is preferably 50% by mass or less, and more preferably 30% by mass or less, from the viewpoint of moldability.

[0109] From the viewpoint of fusion adhesion to L-LDPE, the elastomer composition X may further contain a block copolymer D having a crystalline ethylene block and an amorphous ethylene-α-olefin block.

[0110] Examples of the α-olefin include 1-butene, 1-octene, 1-hexene, and 4-methylpentene-1. Among them, 1-butene is preferable, and the block copolymer D is preferably a block copolymer (CEBC) having a crystalline ethylene block and an amorphous ethylene-butene block. In the present disclosure, the block copolymer D may be used alone or in combination of two or more kinds.

[0111] In addition, the block copolymer D may have a linear structure or a radial structure as a block bonding state. Examples of commercially available products having a linear structure include Dynaron 6101 and Dynaron 6200P (manufactured by JSR Corporation), and examples of commercially available products having a radial structure include Dynaron 6201B (manufactured by JSR Corporation). In the present disclosure, either structure can be preferably used, but in the case of the same weight average molecular weight, a radial structure with high melt fluidity is more preferable.

[0112] The A hardness of the block copolymer D is preferably 40 or more from the viewpoint of compatibility between the isobutylene-based block copolymer A and the medium-low density polyethylene resin B, and is preferably 95 or less from the viewpoint of flexibility of the composition. From these viewpoints, the A hardness of the block copolymer D is preferably 40 to 95, more preferably 50 to 90, and further preferably 60 to 80.

[0113] The content of block copolymer D is preferably 1 part by mass or more per 100 parts by mass of isobutylene-based block copolymer A from the viewpoint of compatibility between the isobutylene-based block copolymer A and the medium-low density polyethylene resin B, and is preferably 50 parts by mass or less from the viewpoint of flexibility. From these viewpoints, the content of block copolymer D is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of isobutylene-based block copolymer A.

[0114] The elastomer composition X may contain an inorganic filler E from the viewpoint of water vapor barrier properties.

[0115] Examples of the inorganic filler E include talc, mica, calcium carbonate, clay, titanium oxide, magnesium carbonate, barium sulfate, calcium sulfate, calcium sulfite, calcium phosphate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, magnesium oxide, iron oxide, zinc oxide, alumina, silica, diatomaceous earth, dolomite, gypsum, calcined clay, asbestos, calcium silicate, bentonite, white carbon, carbon black, iron powder, aluminum powder, stone powder, blast furnace slag, fly ash, cement, and zirconia powder. Of these, talc is preferred from the viewpoints of water vapor barrier properties and dispersibility.

[0116] Inorganic fillers are known in various shapes such as granular, plate-like, rod-like, fibrous, whisker-like, etc., but in the present disclosure, plate-like fillers are preferred from the viewpoint of water vapor barrier property and air barrier property. The plate-like shape refers to a shape in which the ratio of the major axis to the thickness (major axis / thickness) is 5 or more, preferably 10 to 500.

[0117] From the viewpoint of dispersibility, the volume-based median diameter of the inorganic filler E is preferably 1.5 μm or more, and from the viewpoint of water vapor barrier property, it is preferably 50 μm or less. From these viewpoints, the volume-based median diameter of the plate-like inorganic filler is preferably 1.5 to 50 μm, more preferably 1.75 to 30 μm, and even more preferably 2.0 to 15 μm.

[0118] From the viewpoint of flexibility, the content of inorganic filler E is preferably 500 parts by mass or less per 100 parts by mass of isobutylene-based block copolymer A. From these viewpoints, the content of inorganic filler E is preferably 500 parts by mass or less, more preferably 400 parts by mass or less, and even more preferably 300 parts by mass or less per 100 parts by mass of isobutylene-based block copolymer A.

[0119] Furthermore, the elastomer composition X may contain, as necessary, various additives such as a reinforcing agent such as carbon black, silica, carbon fiber, or glass fiber; an insulating thermally conductive filler, a pigment, a flame retardant, an antistatic agent, a release agent, a tackifier, a crosslinking agent, a crosslinking assistant, a foaming agent, or a fragrance, within a range that does not impair the effects of the present disclosure.

[0120] Furthermore, the elastomer composition X may contain other thermoplastic resins or thermoplastic elastomers as long as the effects of the present disclosure are not impaired.

[0121] The elastomer composition X in the present disclosure is obtained by appropriately mixing an isobutylene-based block copolymer A, a medium- to low-pressure polyethylene resin B, and, if necessary, additives such as a rubber softener C, a block copolymer D, and an inorganic filler E, followed by solidification.

[0122] The term "mixing" in the present disclosure is not particularly limited as long as it is a method that allows various raw materials to be mixed well, and various raw materials may be mixed by dissolving them in an organic solvent in which they can be dissolved, or by heating and melting and kneading. However, it is preferable that the raw materials are mixed under temperature conditions where the isobutylene block copolymer A and the medium-low pressure polyethylene resin B are melted.

[0123] When various raw materials are heated, melted, and kneaded, any heating and melting kneading machine can be used, for example, a Banbury mixer, a roll mixer, an extruder, etc., and from the viewpoint of uniform mixing and productivity, it is preferable to use a twin-screw extruder. The components may be mixed in advance using a mixing device such as a Henschel mixer and fed from one hopper to the extruder, or each component may be charged into two hoppers and fed while being measured using a screw or the like below the hoppers.

[0124] The product obtained by mixing the raw materials constituting the elastomer composition X can be in the form of pellets, powder, sheet, etc., depending on the application. For example, the mixture is melt-kneaded and extruded into strands using an extruder, and then cut into cylindrical or rice-grain-shaped pellets using a cutter while being cooled in cold water. The pellets obtained are usually made into a predetermined sheet-shaped molded product or molded product by injection molding or extrusion molding. The melt-kneaded product can also be made into pellets using a rudder or the like and used as a raw material for molding.

[0125] From the viewpoint of ease of adjusting the discharge amount of the contents, the A hardness of the elastomer composition X according to the present disclosure is preferably in the range of 40 or more and less than 80, more preferably in the range of 50 or more and less than 75, and further preferably in the range of 60 or more and less than 70.

[0126] The melt mass-flow rate (MFR) of the elastomer composition X according to the present disclosure is, from the viewpoints of moldability and fusion property, preferably 0.1 g / 10 min or more, more preferably 1.0 to 15.0 g / 10 min, even more preferably 1.0 to 10.0 g / 10 min, and still more preferably 2.0 to 4.0 g / 10 min or more at 190° C. and a load of 21.2 N.

[0127] The moisture permeability of the elastomer composition X according to the present disclosure is preferably 2.0 g / m from the viewpoint of protecting the contents (long-term storage). 2 Less than 24h, preferably 1.8g / m 2 Less than 24h, preferably 1.6g / m 2The moisture permeability herein is the moisture permeability at 40°C in a sample having a thickness of 0.5 mm measured according to JIS Z 0208 (cup method).

[0128] The oxygen permeability coefficient of the elastomer composition X according to the present disclosure is 1.0×10 -15 mol m / Pa s m 2 Preferably, less than 0.8×10 -15 mol m / Pa s m 2 less than 0.6×10 -15 mol m / Pa s m 2 The oxygen permeability coefficient herein is a value measured by a method in accordance with JIS K 7126.

[0129] The outer container 70 according to the present disclosure is obtained in a state where the elastomer portion 80 is fused to the main body portion 72 by two-color molding of the elastomer composition X and a polyolefin resin.

[0130] In the present disclosure, fusion refers to a phenomenon in which heat equal to or higher than the melting point of elastomer composition X is applied to melt the elastomer composition, and then the temperature is lowered to the melting point or lower to solidify the elastomer composition, thereby adhering to the interface of the fusion target. Heat can be applied using a heat press, a heated roll machine, a hot air generator, heated steam, an ultrasonic welder, a high-frequency welder, a laser, or the like. Therefore, even if the interface of the fusion portion has a complex three-dimensional shape, the elastomer composition can be molded and integrated by fitting well to the complex three-dimensional shape.

[0131] Therefore, the elastomer composition X can be integrated with a polyolefin resin to form a composite molded product. This allows the composite of components having complex joint surfaces or joint surfaces with different shapes. This composite molded product can be obtained by molding using a method such as injection molding, injection compression molding, insert molding, multi-color molding, vacuum molding, compressed air molding, blow molding, heat press molding, foam molding, laser fusion molding, and extrusion molding.

[0132] (Example) Examples of composite molded articles made of the elastomer composition X according to the present disclosure and polyolefin resin will be specifically described below. Various physical properties of the raw materials used in the examples and comparative examples were measured by the following methods.

[0133] <Component A: Isobutylene block copolymer, etc.> [Block Copolymer Composition] Proton NMR measurement is performed using a nuclear magnetic resonance apparatus (DPX-400, manufactured by BRUKER, Germany) to determine the content of styrene and / or styrene derivatives, i.e., the content of aromatic vinyl polymer blocks, by quantifying the characteristic groups of styrene. The contents of other monomer units can also be determined by proton NMR measurement.

[0134] [Weight average molecular weight (Mw)] The molecular weight is measured in terms of polystyrene by gel permeation chromatography under the following measurement conditions to determine the weight average molecular weight.

[0135] Measuring Equipment Pump: JASCO (Japan Spectroscopic Corporation), PU-980 Column oven: Showa Denko AO-50 Detector: Hitachi, RI (differential refractometer) detector L-3300 Column type: Showa Denko K-805L (8.0 x 300 mm) and K-804L (8.0 x 300 mm) in series Column temperature: 40℃ Guard column: KG (4.6 x 10 mm) Eluent: Chloroform ·Eluent flow rate: 1.0ml / min Sample concentration: Approximately 1mg / ml Sample solution filtration: Polytetrafluoroethylene 0.45μm pore size disposable filter Standard sample for calibration curve: Polystyrene manufactured by Showa Denko K.K.

[0136] [A hardness] Three 2 mm thick plate-shaped injection molded samples are stacked (total thickness 6 mm) and the A hardness (value 15 seconds after the start of the test) is measured according to JIS K6253. The measurement is performed after conditioning the injection molded samples for one day in a room at a temperature of 23°C and a humidity of 50%.

[0137] 〔density〕 Using an Alpha Mirage precision electronic specific gravity meter, SD-200L, mass is measured in air and water at 23°C and density is calculated.

[0138] <Component B: Polyethylene resin, etc.> 〔density〕 Using an Alpha Mirage precision electronic specific gravity meter "SD-200L," mass is measured in air and in ethanol at 23°C, and density is calculated.

[0139] [Melt Mass Flow Rate (MFR)] Measured in accordance with ASTM D1238 at 190°C and a load of 21.2N.

[0140] [Moisture permeability] The measurement is performed in accordance with JIS Z 0208 (cup method) using a moisture permeability cup (diameter 70 mm) manufactured by Yasuda Seiki Seisakusho under conditions of 40°C x 90% RH and sheet thickness of 0.5 mm.

[0141] [Oxygen permeability coefficient] The gas permeability is measured at 23°C using a gas permeability measuring device "BR-3" manufactured by Toyo Seiki Seisakusho Co., Ltd., in accordance with the method of JIS K 7126. The test specimen is 90 mm x 90 mm x 0.5 mmt, with a permeability area of ​​38.5 cm. 2 Use the following.

[0142] <Component C: Rubber softener> [Kinematic viscosity] Measured at a temperature of 40°C in accordance with JIS Z 8803.

[0143] [Number average molecular weight] Using the same method as for Component A, calculate the number average molecular weight in terms of polystyrene.

[0144] <Component D: Block copolymer having a crystalline ethylene block and an amorphous ethylene-α-olefin block> [A hardness] Three 2 mm thick plate-shaped injection molded samples are stacked (total thickness 6 mm) and the A hardness (value 15 seconds after the start of the test) is measured according to JIS K6253. The measurement is performed after conditioning the injection molded samples for one day in a room at a temperature of 23°C and a humidity of 50%.

[0145] 〔density〕 Using an Alpha Mirage precision electronic specific gravity meter, SD-200L, the mass is measured in air and in ethanol at a temperature of 23°C, and the density is calculated.

[0146] <Component E: Inorganic filler> [Volume-based median diameter] In accordance with the laser diffraction / scattering method defined in JIS M8511, 0.1 g of sample was dispersed in 10 mL of deionized water and dispersed with 70 W ultrasonic waves for 30 seconds. The particle size distribution of the slurry was measured using a Malvern Instruments Mastersizer 2000, and the 50% value of the volume-based cumulative fraction was taken as the volume-based median diameter.

[0147] (1) Preparation of elastomer composition (pellets) The raw materials other than the softener (component C) were dry blended, and then the softener was impregnated into the mixture to produce a mixture. The mixture was then melt-kneaded in an extruder under the following conditions, extruded into strands, and cut into pellets of about 3 mm in diameter and about 3 mm in thickness with a cutter while being cooled in cold water.

[0148] [Melt-kneading conditions] Extruder: KZW32TW-60MG-NH (product name, manufactured by Technovel Co., Ltd.) Cylinder temperature: 180~220℃ Screw rotation speed: 300 r / min

[0149] Details of the raw materials used in producing the pellets of the elastomer composition are shown in the following Tables 1 to 3. In producing the pellets of the elastomer composition, pellets of the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5, which have different ratios of the raw materials, were produced. Details of the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5 will be described later.

[0150] (Table 1) JPEG0007589749000001.jpg46163

[0151] (Table 2) JPEG0007589749000002.jpg52163

[0152] (Table 3) JPEG0007589749000003.jpg52164

[0153] (2) Preparation of a molded product of a thermoplastic elastomer composition Pellets of the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5 were injection molded under the conditions below to prepare plates having a thickness of 2 mm, a width of 125 mm, and a length of 125 mm.

[0154] [Injection molding conditions] Injection molding machine: 100MSIII-10E (product name, manufactured by Mitsubishi Heavy Industries, Ltd.) Injection molding temperature: 200℃ Injection pressure: 30% Injection time: 3sec Mold temperature: 40℃

[0155] (3) Preparation of composite compact Pellets of polyolefin resins, HDPE (Nipolon Hard 4020 manufactured by Tosoh Corporation) and L-LDPE (Evolue SP2520 manufactured by Prime Polymer Co., Ltd.), were injection molded under the conditions below to produce resin plates of 2 mm thickness x 125 mm width x 125 mm length. These were then cut with a cutter to obtain fusion test substrates of 2 mm thickness x 25 mm width x 125 mm length.

[0156] [Resin plate molding conditions] Gate: Film Gate Cylinder temperature: 200℃ Measurement value: 55mm Pressure holding switch position: 3.8mm

[0157] The prepared resin plate was inserted into a mold having a thickness of 4 mm, a width of 25 mm, and a length of 125 mm, and the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5 were injection molded to prepare rectangular composite molded bodies.

[0158] <Injection molding conditions> Injection molding machine: Mitsubishi Heavy Industries, Ltd., 100MSIII-10E Injection molding temperature: 240℃ Injection pressure: 98MPa, injection speed: 50%, holding pressure: 20%, holding time: 10sec Injection time: 2sec Mold temperature: 40℃

[0159] The following evaluations were carried out on the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5 and the composite molded articles using the elastomer compositions. The compositions and evaluation results of the elastomer compositions of Examples 1 to 7 and Comparative Examples 1 to 5 are shown in Tables 4 and 5.

[0160] [A hardness of elastomer composition] Three 2 mm thick plate-shaped injection molded samples are stacked (total thickness 6 mm) and the A hardness (value 15 seconds after the start of the test) is measured according to JIS K6253. The measurement is performed after conditioning the injection molded samples for one day in a room at a temperature of 23°C and a humidity of 50%.

[0161] [MFR of elastomer composition] Measured in accordance with ASTM D1238 at 190°C and a load of 21.2N.

[0162] [Moisture permeability of elastomer composition] The elastomer composition was placed in a press mold measuring 0.5 mm in thickness × 100 mm in width × 120 mm in length, and hot-pressed for 2 minutes using a hot press machine (Toho Machinery Co., Ltd., hydraulic molding machine TB-50-2 type) heated to 200°C, followed by cooling and pressing for 3 minutes to produce a sheet-like press molded body with a thickness of 0.5 mm as a test specimen. The measurement was performed in accordance with JIS Z 0208 (cup method) using a moisture permeability cup (diameter 70 mm) manufactured by Yasuda Seiki Seisakusho under conditions of 40°C x 90% RH and sheet thickness of 0.5 mm.

[0163] [Oxygen Permeability of Elastomer Composition] The elastomer composition was placed in a press mold measuring 0.5 mm thick x 100 mm wide x 120 mm long, and then hot pressed for 2 minutes using a hot press machine (Toho Machinery Co., Ltd., hydraulic molding machine TB-50-2 type) heated to 200°C, followed by cooling and pressing for 3 minutes to produce a sheet-like press molded body having a thickness of 0.5 mm as a test specimen. The test specimen dimensions were 90 mm x 90 mm x 0.5 mmt, with a permeation area of ​​38.5 cm. 2 The following items were used. The measurement was performed at 23°C using a gas permeability measuring device "BR-3" manufactured by Toyo Seiki Seisakusho Co., Ltd. according to a method conforming to JIS K 7126.

[0164] [Fusion properties of composite molded body] Using the composite molded body, a tensile test was performed at 50 mm / min in a 180° direction between the elastomer composition layer (skin layer) and the polyolefin resin layer (base layer) at an ambient temperature of 23° C. to measure the peel strength (unit: N / 25 mm) between the skin layer and the base layer. The peel strength is preferably 120 N / 25 mm or more.

[0165] (Table 4) JPEG0007589749000004.jpg22977

[0166] (Table 5) JPEG0007589749000005.jpg23490

[0167] From the results shown in Tables 4 and 5 above, it is apparent that the composite molded articles of Examples 1 to 7 have excellent air barrier properties for the elastomer composition, and the fusion between the elastomer composition and the polyethylene resin is also strong. In contrast, in Comparative Example 1 and Comparative Example 2, in which the elastomer composition does not contain polyethylene resin, the moisture permeability is 2.0 g / m 2 The water vapor barrier properties are inferior to those of Examples 1 to 7, being longer than 24 hr. Comparative Example 3, in which the elastomer composition contains a low-density polyethylene resin, which is a high-pressure polyethylene resin, as the polyethylene resin, and Comparative Example 4, in which the elastomer composition contains a polypropylene resin instead of the polyethylene resin, show insufficient fusion properties with respect to HDPE. Comparative Example 5, in which SEBS is contained instead of the isobutylene block copolymer, has a moisture permeability of 2.0 g / m 2 The water vapor barrier properties are inferior to those of Examples 1 to 7. Reference Example 1 shows the results of measuring the physical properties of component A, "SIBSTAR 062T," in the same manner as the elastomer compositions of the Examples and Comparative Examples. It shows that the isobutylene block copolymer itself hardly melts to HDPE, but when mixed with a specified amount of medium / low pressure polyethylene resin, it becomes melt-adhesive to HDPE.

[0168] (Action and Effects) Next, the operation and effects of the embodiment will be described. In this description, when describing a comparative embodiment to the embodiment, if the same parts as those in the container 10 of the embodiment are used, the reference numerals and names of the parts will be used as they are.

[0169] The container 10 of the embodiment has an opening 74 formed in the outer peripheral wall of the outer container 70 covered with an elastomer pressing part 84. Therefore, as shown in Figures 4 and 7, when the cap 40 is removed from the outer container 70, the container 10 can easily discharge the contents of the inner container 20 from the nozzle part 24 by pressing the pressing part 84 with a finger or the like to press the main body part 22 of the inner container 20.

[0170] Moreover, the container 10 of the embodiment has a configuration in which the cap 40 is detachably provided on the outer container 70. In the container 10 of the embodiment, the cap 40 is attached to the outer container 70 and covers the nozzle portion 24 of the inner container 20 protruding from the outer container 70. This improves the air barrier properties of the container 10 compared to a configuration in which the cap 40 is detachably provided on the inner container 20.

[0171] Moreover, the container 10 of the embodiment has a configuration in which the outer container 70 made of hard resin encloses the inner container 20. Therefore, the container 10 of the embodiment prevents the contents from being discharged from the nozzle portion 24 of the inner container 20 even if the container 10 is pressed inadvertently.

[0172] Furthermore, the container 10 of the embodiment has a configuration in which a base 50 is provided at the end of the outer container 70 opposite to the cap 40. Therefore, the container 10 of the embodiment can be stood on a workbench or the like with the base 50 facing down and the tip portion 24a of the nozzle portion 24 facing up. This allows the user of the container 10 to stand the container 10 on a workbench or the like when interrupting the operation of discharging the contents filled in the inner container 20, so that the contents do not leak from the nozzle portion 24.

[0173] Moreover, the container 10 of the embodiment has a configuration in which a pair of openings 74 are provided symmetrically with respect to the central axis of the outer container 70. Therefore, in the container 10 of the embodiment, when the pair of pressing portions 84 is pressed to eject the contents from the nozzle portion 24, the pair of pressing portions 84 can be easily pinched and pressed with the thumb and index finger (see FIG. 10).

[0174] Moreover, the container 10 of the embodiment has a connecting portion 86 that integrally connects the pair of pressing portions 84 so as to be wrapped around the outer peripheral wall of the outer container 70. Therefore, in the container 10 of the embodiment, peeling of the pressing portions 84 from the outer container 70 is suppressed compared to a configuration in which the pair of pressing portions 84 are not integrally connected.

[0175] Moreover, the container 10 of the embodiment has a first extension portion 86a extending from the connecting portion 86 toward the base 50. Therefore, the container 10 of the embodiment has a larger fusion area of ​​the elastomer portion 80 to the outer container 70 compared to a configuration not having the first extension portion 86a, and thus peeling of the pressing portion 84 from the outer container 70 is suppressed.

[0176] Moreover, the container 10 of the embodiment has a configuration in which a plurality of ribs 42c are formed on the outer peripheral wall of the outer tube portion 42 of the cap 40. Therefore, in the container 10 of the embodiment, when a user manually attaches or detaches the cap 40, the user's fingers can be caught on the ribs, making it easier to grip the cap.

[0177] Moreover, the container 10 of the embodiment has a configuration in which the outer peripheral wall of the outer container 70 increases in diameter from the end on the cap 40 side toward the base 50. Therefore, the container 10 of the embodiment is unlikely to tip over when placed on a workbench or the like with the tip 24a of the nozzle portion 24 facing upward.

[0178] Moreover, the container 10 of the embodiment has a configuration in which the content of the inner container 20 is an adhesive. Therefore, the container 10 of the embodiment has air barrier properties, and the adhesive filled in the inner container 20 is unlikely to deteriorate when not in use.

[0179] Moreover, the container 10 of the embodiment has a configuration in which the inner container 20 is made of polyolefin. Therefore, in the container 10 of the embodiment, the adhesive remaining inside the nozzle portion 24 is difficult to harden.

[0180] In addition, the container 10 of the embodiment has a configuration in which the cap 40 is made of polyolefin. Therefore, in the container 10 of the embodiment, the adhesive remaining on the tip 24a of the nozzle portion 24 covered by the cap 40 is difficult to harden.

[0181] Moreover, the container 10 of the embodiment has a configuration in which a desiccant 60 is provided inside the base 50. Therefore, the container 10 of the embodiment can absorb moisture contained in the air in the internal space of the container 10, thereby drying the space.

[0182] Moreover, the container 10 of the embodiment has a configuration in which a recess 84b is formed on the surface of the pressing portion 84. Therefore, the container 10 of the embodiment allows the thumb and index finger to fit into the recess 84b when pressing the pressing portion 84 (see FIG. 10).

[0183] Furthermore, in the container 10 of the embodiment, the pressing portion 84 has a raised portion 84a. Therefore, in the container 10 of the embodiment, the user can sense the position of the pressing portion 84 by touch.

[0184] In addition, the container 10 of the embodiment has a maximum thickness T max The maximum thickness T max In comparison with a configuration in which the maximum thickness T of the raised portion 84a is less than 0.2 mm, the user can easily determine the position of the pressing portion 84 by touch. max In comparison with a configuration in which the thickness exceeds 1.0 mm, the inner container 20 can be easily pressed by pressing the pressing portion 84 with the thumb and index finger.

[0185] Moreover, the container 10 of the embodiment has a configuration in which the A-hardness of the elastomer composition X is in the range of 40 or more and less than 80. Therefore, the container 10 of the embodiment has an easier adjustment of the amount of the content discharged by pressing the pressing portion 84 than a configuration in which the A-hardness of the elastomer forming the pressing portion 84 is less than 40. Moreover, the container 10 of the embodiment has an easier adjustment of the amount of the content discharged by pressing the pressing portion 84 than a configuration in which the A-hardness of the elastomer forming the pressing portion 84 is 80 or more.

[0186] In addition, the container 10 of the embodiment has a moisture permeability of 2.0 g / m2 for a sample having a thickness of 0.5 mm, as measured in accordance with JIS Z 0208. 2 Therefore, in the container 10 of the embodiment, the moisture permeability of the elastomer forming the pressing portion 84 is 2.0 g / m2 or less in a sample having a thickness of 0.5 mm. 2 The water vapor barrier properties of the container 10 are improved compared to a configuration in which the resistance is 24 hours or more.

[0187] In addition, the container 10 of the embodiment has an oxygen permeability coefficient of 1.0×10 -15 mol m / Pa s m 2 Therefore, in the container 10 of the embodiment, the oxygen permeability coefficient of the elastomer forming the pressing portion 84 is less than 1.0×10 -15 mol m / Pa s m 2 Compared to the above configuration, the air barrier properties of the container 10 are improved.

[0188] As described above, the embodiments of the present disclosure have been described in detail, but the present disclosure is not limited to the above embodiments, and various modifications, changes, and improvements are possible within the scope of the technical idea of ​​the present disclosure.

[0189] For example, the container 10 in the embodiment includes a base 50. However, the container 10 according to the present disclosure may not include the base 50 as long as the outer container 70 and the cap 40 alone provide an air barrier to the inner container 20.

[0190] In the embodiment, the openings 74 are provided in a pair symmetrically with respect to the central axis of the outer container 70. However, the openings 74 according to the present disclosure are not limited to being provided in a pair symmetrically with respect to the central axis of the outer container 70. The openings 74 according to the present disclosure may be configured such that only one opening is provided on the outer peripheral wall of the outer container 70, or may be configured such that three or more openings are provided. Furthermore, the multiple openings 74 provided on the outer container 70 according to the present disclosure may not be symmetrically with respect to the central axis of the outer container 70.

[0191] Moreover, the container 10 of the embodiment has a configuration in which the pair of pressing portions 84 are integrally connected by the connecting portion 86. However, the pair of pressing portions 84 according to the present disclosure may have a configuration in which they are not integrally connected.

[0192] Moreover, the container 10 of the embodiment has the first extension portion 86a. However, the container 10 according to the present disclosure may have a configuration that does not have the first extension portion 86a. Moreover, the container 10 according to the present disclosure may have a configuration in which the first elastomer portion 82 and the second elastomer portion 90 are not connected. Moreover, the container 10 according to the present disclosure may have a configuration in which the second elastomer portion 90 is not included.

[0193] Furthermore, the cap 40 in the embodiment is formed with the rib 42c. However, the cap 40 according to the present disclosure may not be formed with the rib 42c.

[0194] In addition, the outer container 70, the cap 40, and the base 50 according to the embodiment have a configuration in which the diameter increases from the end on the cap 40 side toward the base 50. However, the outer container 70, the cap 40, and the base 50 according to the present disclosure may not have a configuration in which the diameter increases or decreases, and may have a configuration in which the outer diameter of each outer peripheral wall is uniform. In addition, the outer container 70, the cap 40, and the base 50 according to the present disclosure may have a configuration in which the outer peripheral walls are different and are not flush with each other.

[0195] In the embodiment, the recess 84b of the pressing portion 84 is elliptical when viewed from the radial direction. However, the recess 84b in the present disclosure is not limited to an elliptical shape. The recess 84b in the present disclosure may be circular or teardrop-shaped when viewed from the radial direction. The recess 84b in the present disclosure may be polygonal, such as triangular or rectangular, when viewed from the radial direction.

[0196] In the embodiment, the raised portion 84a of the pressing portion 84 is formed with a recess 84b that is recessed relative to the raised portion 84a. However, the raised portion 84a according to the present disclosure may be formed with a protrusion that is protruding relative to the raised portion 84a. The pressing portion 84 according to the present disclosure may not be formed with the recess 84b or the protrusion.

[0197] In addition, in the container 10 of the embodiment, the pressing portion 84 has the raised portion 84a. However, in the container 10 according to the present disclosure, the pressing portion 84 does not necessarily have to have the raised portion 84a.

[0198] In the container 10 of the embodiment, the elastomer portion 80 is approximately flush with the outer peripheral wall of the main body portion 72 of the outer container 70. However, the elastomer portion 80 according to the present disclosure may have a step with respect to the outer peripheral wall of the main body portion 72 of the outer container 70.

[0199] In addition, in the container 10 of the embodiment, the main body 72 of the outer container 70 is substantially cylindrical. However, the outer container 70 according to the present disclosure is not limited to being substantially cylindrical as long as it is cylindrical, and may be substantially rectangular when viewed from the radial direction.

[0200] Moreover, the container 10 of the embodiment includes the desiccant 60. However, the container 10 according to the present disclosure does not necessarily need to include the desiccant 60.

[0201] The disclosure of Japanese Patent Application No. 2020-193893, filed on November 20, 2020, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. An inner container having a nozzle portion for discharging the filled contents; a cylindrical outer container made of hard resin that contains the inner container and has an opening on its outer circumferential wall; A pressing portion made of an elastomer provided on the outer peripheral wall and covering the opening; a cap that covers the nozzle portion protruding from the outer container and is detachable from the outer container; Equipped with the pressing portion is a part of an elastomer member that is wound around the outer container in a circumferential direction and covers a part of the outer peripheral wall, the part covering the opening, The inner container is a flexible material formed of any one of polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, nylon, polyethylene terephthalate, aluminum, tin, and lead; The outer container is a hard resin formed of polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate. container.

2. The container of claim 1 , further comprising a seat at an end of the outer container opposite the cap.

3. 3. The container according to claim 1, wherein a pair of the openings covered by the pressing portion are provided symmetrically with respect to a central axis of the outer container.

4. An inner container having a nozzle portion for discharging the filled contents; a cylindrical outer container made of hard resin that contains the inner container and has an opening on its outer circumferential wall; A pressing portion made of an elastomer provided on the outer peripheral wall and covering the opening; a cap that covers the nozzle portion protruding from the outer container and is detachable from the outer container; Equipped with a pair of the openings covered by the pressing portion are provided symmetrically with respect to a central axis of the outer container, The pair of pressing parts further includes the elastomer connecting part that is integrally connected to the outer circumferential wall of the outer container so as to be wrapped around the outer circumferential wall of the outer container, The inner container is a flexible material formed of any one of polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, nylon, polyethylene terephthalate, aluminum, tin, and lead; The outer container is a hard resin formed of polyethylene, polypropylene, ethylene-vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, nylon, or polyethylene terephthalate. container.

5. Further comprising a base at an end of the outer container opposite the cap, 5. The container of claim 4, further comprising an elastomeric extension extending from said connector toward said seat of said outer container.

6. 6. The container according to claim 1, wherein a plurality of ribs are formed on the outer periphery of the cap.

7. The container according to claim 2 , wherein the outer peripheral wall of the outer container increases in diameter from the end on the cap side toward the base.

8. The container according to any one of claims 1 to 7, wherein the content is an adhesive.

9. 9. The container of claim 8, wherein the inner container is made of polyolefin.

10. 10. The container of claim 9, wherein the cap is made of a polyolefin.

11. The container of claim 2 further comprising a desiccant on the inside of the base.

12. The container according to any one of claims 1 to 11, wherein a recess is formed on the surface of the pressing portion.

13. The container according to any one of claims 1 to 12, wherein the pressing portion has a raised portion that is raised higher than an outer peripheral wall of the outer container.

14. The container according to claim 13, wherein the maximum thickness of the raised portion is within a range of 0.2 mm or more and 1.0 mm or less.

15. The container according to any one of claims 1 to 14, wherein the elastomer has an A hardness in the range of 40 or more and less than 80.

16. The elastomer has a moisture permeability of 2.0 g / m2 for a sample having a thickness of 0.5 mm, as measured in accordance with JIS Z 0208. 2 A container according to any one of claims 1 to 15, which has a shelf life of less than 24 hours.

17. The elastomer has an oxygen permeability coefficient of 1.0×10 measured in accordance with JIS K 7126. -15 mol・m / Pa・s・m 2 The container according to any one of claims 1 to 16, wherein the container has a mass of less than 1000 sq.

18. The elastomeric member comprises: The pressing portion covers the recess on the outer peripheral wall, and a portion other than the pressing portion is formed flush with the outer peripheral wall around the recess.

2. The container of claim 1.

Citation Information

Patent Citations

  • spanner

    JP1994046863U

  • Water-repellent liquid container

    JP1996048358A

  • Pen type instantaneous adhesive container

    JP1998337523A

  • Refill type double vessel

    JP2002308331A

  • Composite container for adhesive

    JP2004182249A