Composition for indicator that changes color over time and indicator that changes color over time using the same

The composition for a color-changing indicator, featuring a polyamide resin binder, addresses the challenge of achieving both deep color density and water resistance by utilizing carbonic acid from air, ensuring the indicator maintains color intensity and integrity.

JP7589965B2Active Publication Date: 2024-11-26SAKURA COLOR PRODUCTS CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020121594
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-15
Publication Date
2024-11-26
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Existing color-changing indicators struggle to achieve both deep color density and good water resistance, as improving water resistance often compromises color density, and vice versa.

Method used

A composition for a color-changing indicator that includes a color-changing dye, a base, a basic inorganic compound, and a binder resin, with the binder resin comprising a polyamide resin, which enhances both color density and water resistance by using carbonic acid generated from carbon dioxide and water in the air.

Benefits of technology

The composition achieves deep color density while maintaining good water resistance, ensuring the indicator's quality does not deteriorate due to moisture and the discoloration layer does not peel off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589965000001
    Figure 0007589965000001
  • Figure 0007589965000002
    Figure 0007589965000002
Patent Text Reader

Abstract

To provide a temporally color-changing indicator that can achieve both of high coloring density and excellent water resistance, and a composition for the temporally color-changing indicator using the same.SOLUTION: A composition for a temporally color-changing indicator includes a color-changing dye, a base, a basic inorganic compound and a binder resin, the binder resin including a polyamide resin. A temporally color-changing indicator has, on a base material, a color-changing layer formed from the composition for the temporally color-changing indicator.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for a time-changing indicator and a time-changing indicator using the same. [Background technology]

[0002] Various indicators that change color over time using color changes have been proposed. For example, the quality and function of products such as insect repellents, air fresheners, deodorants, and dehumidifiers change depending on the storage location and environmental conditions during use and the time (elapsed time) that the product is left in those environments. Therefore, in order to manage the quality of these products, indicators are needed to grasp the environmental conditions in which the product is placed and the elapsed time.

[0003] Conventionally, such indicators that change color over time include indicators that utilize the change in pH of a coating film caused by carbon dioxide generated by carbon dioxide and water in the air, causing a dye that changes color over time depending on the pH (acidic / basic), and the onset of color change can be manipulated as desired (see Patent Document 1). However, generally, when the water resistance of a coating film is improved, it becomes difficult for moisture to penetrate into the coating film, so the amount of carbonic acid produced by carbon dioxide and water in the air decreases, and the color density may not be sufficiently dark, resulting in insufficient visibility. Thus, there is room for further improvement in order to achieve both a deep color density and good water resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-76050 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above, and aims to provide a time-discoloring indicator that can achieve both deep color density and good water resistance, and a composition for a time-discoloring indicator used therein. [Means for solving the problem]

[0006] As a result of intensive research into achieving the above-mentioned object, the present inventors have discovered that the above-mentioned object can be achieved by providing a composition for a time-discoloring indicator, the composition comprising a color-changing dye, a base, a basic inorganic compound, and a binder resin, wherein the binder resin comprises a polyamide resin, and a time-discoloring indicator using the same, and have thus completed the present invention. That is, the present invention relates to the following composition for a time-changing indicator and a time-changing indicator using the same.

[0007] 1. A composition for a time-changing indicator, comprising a color-changing dye, a base, a basic inorganic compound and a binder resin, the binder resin comprising a polyamide resin. 2. The composition for a time-changing indicator according to item 1, wherein the base comprises at least one selected from an alkali metal hydroxide and ammonia. 3. A composition for a time-changing indicator, comprising a color-changing dye, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, wherein the binder resin comprises a polyamide resin. 4. The composition for a time-discoloring indicator according to any one of items 1 to 3, wherein the content of the polyamide resin is 1 to 90% by weight based on 100% by weight of the total solid content of the composition for a time-discoloring indicator. 5. The composition for a time-changing indicator according to any one of items 1 to 4, wherein the basic inorganic compound contains a hydroxide of an element of Group 2 of the periodic table. 6. The composition for a time-changing indicator according to any one of items 1 to 5, wherein the content of the basic inorganic compound is 1 to 50% by weight, based on 100% by weight of the total solid content of the composition for a time-changing indicator. 7. The composition for a time-discoloring indicator according to any one of items 1 to 6, wherein the binder resin further comprises, in addition to the polyamide resin, at least one selected from a petroleum-based hydrocarbon resin, a vinyl resin, a butyral resin, an alkyd resin, an epoxy resin, a fluororesin, a silicone resin, a polyester resin, a coumarone resin, a polyimide resin, an alicyclic resin, an acrylic resin, a rosin resin, a rosin ester resin, a ketone resin, a hydrogenated ketone resin, and a cellulose resin. 8. The composition for a time-changing indicator according to any one of items 1 to 7, further comprising a non-color-changing pigment. 9. A time-changing indicator having a color-changing layer formed from the composition for a time-changing indicator according to any one of items 1 to 8 on a substrate. 10. A substrate and a color-changing layer, A time-changing indicator, wherein the color-changing layer comprises a color-changing dye, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, and the binder resin comprises a polyamide resin. 11. The indicator that changes color over time according to item 9 or 10, further comprising a non-color-changing layer. 12. The indicator according to any one of items 9 to 11, further comprising an overcoat layer. 13. A printed matter having a printed layer formed from the composition for a time-discoloring indicator according to any one of items 1 to 8. Effect of the Invention

[0008] The composition for a time-changing indicator of the present invention and a time-changing indicator using the same can achieve both deep color density and good water resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The composition for a time-changing indicator of the present invention (hereinafter, also simply referred to as the "composition") and the time-changing indicator using the same (hereinafter, also simply referred to as the "indicator") will be described in detail below.

[0010] (1) Composition for indicator that changes color over time The composition for a time-changing indicator of the present invention comprises a color-changing dye, a base, a basic inorganic compound, and a binder resin, and the binder resin comprises a polyamide resin. By using this composition, and in particular by using a polyamide resin as the binder resin, it is possible to achieve both a high color density and good water resistance of the composition and the indicator. In this specification, water resistance mainly means that the composition is not deteriorated by moisture and that the base material and the color-changing layer of the indicator do not peel off in the presence of moisture.

[0011] (Discoloration pigment) The color-changing dye is not particularly limited as long as it changes color with a base and recolors with carbon dioxide generated from carbon dioxide and water in the air, and examples of the color-changing dye include basic dyes, etc. Examples of the basic dye include, but are not particularly limited to, diarylmethane-based basic dyes, triarylmethane-based basic dyes, azo-based basic dyes, nitrogen-containing heterocyclic compound-based basic dyes, polymethine-based basic dyes, etc. The above-mentioned color-changing dyes can be used alone or in combination of two or more.

[0012] Among the above-mentioned color-changing dyes, from the viewpoint of color-changing properties in an acid-base reaction, triarylmethane-based basic dyes are preferred, triphenylmethane-based basic dyes are more preferred, and CI Basic Violet 3, CI Basic Violet 4, and the like are even more preferred.

[0013] The content (solid content) of the color-changing pigment can be appropriately determined depending on the type of color-changing pigment, the desired hue, etc., but is preferably 0.5 to 30% by weight, more preferably 1 to 15% by weight, based on 100% by weight of the total solid content of the composition for a time-changing indicator. If the content of the color-changing pigment is less than 0.5% by weight, the color of the indicator after color change may be lighter, and if it exceeds 30% by weight, the color of the composition and the initial color of the indicator (the color of the color-changing layer immediately after the preparation of the indicator) may be colored rather than colorless.

[0014] In this specification, the phrase "100% by weight of the total solid content of the composition for a time-discoloring indicator" means 100% by weight of the total solid content of each component contained in the composition.

[0015] Here, the color change of the color-changing dye will be described by taking a triphenylmethane-based basic dye as an example of the color-changing dye. The triphenylmethane basic dye itself is colored. When a base is added to it, the colored dye structure of the triphenylmethane basic dye changes to a colorless dye structure, and the mixture becomes colorless. However, when the colorless mixture is treated with an acid, the colorless dye structure of the triphenylmethane basic dye returns to a colored dye structure, and the mixture becomes colored. An example of the change in the dye structure (for example, in the case of CI Basic Red 9) is shown in the following formula. [ka]

[0016] In the present invention, the above reaction is utilized, and carbonic acid formed from carbon dioxide and water in the atmosphere acts as an acid, thereby returning the above color-changing pigment to its original colored dye structure in the indicator composition that changes color over time, thereby restoring the color. In this specification, the color-changing dye may have either a colored dye structure or a colorless dye structure.

[0017] The composition for a time-discoloring indicator of the present invention contains a color-changing dye, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, and the binder resin contains a polyamide resin. The alkali metal salt and / or ammonium salt in the composition is a product derived from the base when the color-changing dye reacts with the base to change the color-changing dye into a colorless dye structure.

[0018] (base) The composition for a time-changing indicator of the present invention contains a base, which causes a chemical change in the color-changing pigment, changing the colored dye structure to a colorless dye structure, thereby making the composition colorless. The base is not particularly limited as long as it can change the color of the color-changing pigment, but examples of the base include alkali metal hydroxides, ammonia, etc., from the viewpoint of solubility, etc. The base can be used alone or in combination of two or more kinds. The alkali metal hydroxide is not particularly limited, but examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, etc. From the viewpoint of ionization tendency, sodium hydroxide and potassium hydroxide are preferred.

[0019] The content (solid content) of the base is preferably 0.05 to 15 wt %, more preferably 0.1 to 5 wt %, based on 100 wt % of the total solid content of the composition for a time-discoloring indicator. If the content of the base is less than 0.05 wt %, the color-discoloring pigment may not change color easily, and the color of the composition and the initial color of the indicator may not become colorless easily. If the content of the base is more than 15 wt %, the base may not dissolve easily in the solvent.

[0020] In addition, as described above, when the composition of the present invention contains an alkali metal salt and / or an ammonium salt, which is a derivative of the base when the color-changing pigment reacts with the base and the color-changing pigment changes to a colorless dye structure, the content of the alkali metal salt and / or the ammonium salt is the same as the content of the base described above. The alkali metal salts and ammonium salts are salts appropriate for the color-changing dye used, and examples thereof include chloride salts and sulfonate salts. When an excess amount of base is used relative to the color-changing dye, the composition may contain a base (at least one selected from alkali metal hydroxides and ammonia) in addition to the above-mentioned alkali metal salts and ammonium salts.

[0021] (Basic inorganic compounds) The composition for a time-changing indicator of the present invention contains a basic inorganic compound, and thus the color density of the composition can be increased when the composition changes color. In other words, it is considered that the basic inorganic compound acts as a color-changing assistant for the composition, thereby increasing the color density.

[0022] The basic inorganic compound is not particularly limited as long as it has the ability to adsorb carbon dioxide and has low solubility in water and alcohol, and examples thereof include hydroxides of Group 2 elements of the periodic table. Preferred examples of the hydroxide of Group 2 elements of the periodic table include calcium hydroxide, magnesium hydroxide, barium hydroxide, strontium hydroxide, etc. The basic inorganic compounds can be used alone or in combination of two or more. In addition, since the basic inorganic compound has low solubility in water and alcohol, it is considered that it has almost no effect on decolorizing the color-changing pigment. In addition, the basic inorganic compound adsorbs carbon dioxide in the air, which reacts with water in the air to form carbonic acid, which is considered to be able to cause the color-changing pigment to recolor. In addition, since the basic inorganic compound is white, it is considered that it also acts as an extender pigment, and has the effect of making the color appear darker when made into a paint film.

[0023] The content (solid content) of the basic inorganic compound is preferably 1 to 50 wt %, more preferably 3 to 15 wt %, based on the total solid content of the composition for a time-discoloring indicator (100 wt %). If the content of the basic inorganic compound is less than 1 wt %, the coloring concentration may be low, and if it exceeds 50 wt %, the adhesiveness of the indicator to the substrate may be easily reduced when the composition is used in the color-discoloring layer of the indicator. The content of the basic inorganic compound can be appropriately adjusted in consideration of other components.

[0024] (binder resin) In the composition for a time-discoloring indicator of the present invention, it is necessary to contain a polyamide resin as a binder resin. The polyamide resin acts not only as a binder resin but also as a color-discoloring assistant, and can deepen the color density of the composition and the indicator. In addition, since polyamide resin has amide groups in its molecule, it is highly water absorbent despite being a hydrophobic resin. Therefore, it absorbs moisture in the air, which easily reacts with carbon dioxide in the air to form carbon dioxide, which is thought to easily cause a color-changing reaction of the color-changing pigment. Furthermore, polyamide resin as a whole is hydrophobic and does not deteriorate due to moisture. Furthermore, even if a composition containing polyamide resin is used in an indicator, the indicator substrate and color-changing layer will not peel off in the presence of moisture, and the indicator is also water-resistant. The polyamide resin is not particularly limited as long as it does not inhibit the acid-base reaction of the color-changing pigment and has water absorbency, but examples thereof include Vegichem Green V756, Vegichem Green V744, Vegichem Green V725 (all manufactured by Tsuno Food Industries), Polymide S-40E (manufactured by Sanyo Chemical Industries), and the like.

[0025] The content (solid content) of the polyamide resin is preferably 1 to 90% by weight, more preferably 15 to 85% by weight, based on 100% by weight of the total solid content of the composition for a time-discoloring indicator. If the content of the binder resin is less than 1% by weight, the color density may be low, and if it exceeds 90% by weight, the viscosity of the composition may be high, which may affect the printability.

[0026] The composition for a time-discoloring indicator of the present invention may contain a binder resin other than the polyamide resin. The binder resin other than the polyamide resin is not particularly limited as long as it does not inhibit the acid-base reaction of the color-changing dye, and examples thereof include petroleum-based hydrocarbon resins, vinyl resins, butyral resins, alkyd resins, epoxy resins, fluororesins, silicone resins, polyester resins, coumarone resins, polyimide resins, alicyclic resins, acrylic resins, rosin resins, rosin ester resins, ketone resins, hydrogenated ketone resins, cellulose resins, etc. The binder resins may be used alone or in combination of two or more.

[0027] Among binder resins other than polyamide resins, preferred examples include rosin resins, rosin ester resins, ketone resins, hydrogenated ketone resins, and cellulose-based resins, from the viewpoints of high adhesion to the substrate of the indicator and small effect on acid-base reactions. The rosin resin is not particularly limited, but preferred examples include Pine Crystal KE-100, Pine Crystal KE-311, Pine Crystal PE-590, and Pine Crystal KR-140 (all manufactured by Arakawa Chemical Industries, Ltd.). The rosin ester resin is not particularly limited, but preferred examples thereof include Super Ester A-75, Super Ester A-100, Super Ester A-115, Ester Gum H, Ester Gum HP, Pencel A, Pencel D-125, Pencel D-135, and Pencel D-160 (all manufactured by Arakawa Chemical Industries, Ltd.). The ketone resin is not particularly limited, but preferred examples thereof include Ketone Resin K-90 (manufactured by Arakawa Chemical Industries), TEGO VARIPLUS AP (manufactured by Evonik), Hilac 111 (manufactured by Hitachi Chemical), and POLYTONE K-90 (manufactured by Wally). The hydrogenated ketone resin is not particularly limited, but preferable examples thereof include TEGO VARIPLUS SK (manufactured by Evonik Corporation) and Hilac 110H (manufactured by Hitachi Chemical Co., Ltd.). The cellulose-based resin is not particularly limited as long as it is water-soluble, and preferred examples thereof include methyl cellulose, ethyl cellulose, and ethyl methyl cellulose.

[0028] When a binder resin other than a polyamide resin is contained, the content (solid content) of the binder resin other than a polyamide resin is preferably 1 to 89 wt %, and more preferably 10 to 70 wt %, based on 100 wt % of the total solid content of the composition for a time-discoloring indicator, from the viewpoints of adhesion to the substrate of the indicator and viscosity of the composition, etc.

[0029] (Non-discoloring pigment) The compositions of the present invention may further comprise a non-color changing pigment. In this specification, the non-color-changing dye means a dye that is not decolorized by the above-mentioned base. The non-color-changing dye is not particularly limited, but may be, for example, a pigment, a dye, or the like. The pigment may be, for example, an azo-based, phthalocyanine-based, perylene-based, or quinacridone-based pigment. The dye may be, for example, an azo-based, quinone-based, cyanine-based, phthalocyanine-based, or indigo-based dye. From the viewpoint of visibility after discoloration, it is preferable to select a complementary color of the color-changing dye. The non-color-changing dye may be used in one or more kinds. When a non-color-changing pigment is included, the color-changing pigment and the non-color-changing pigment are mixed uniformly in the composition, so the composition is no longer colorless. For example, when the color-changing pigment in the composition is blue and the non-color-changing pigment is yellow, the indicator using this composition has an initial color of yellow (because the color-changing pigment becomes colorless due to the base) and changes to green over time (because the color-changing pigment changes to blue over time). In addition, when a non-color-changing pigment is included, it is preferable that the initial color of the indicator is the color of the non-color-changing pigment. When a non-color-changing pigment is contained, its content (solid content) is preferably 0.5 to 30 wt %, more preferably 1 to 15 wt %, based on 100 wt % of the total solid content of the composition for a time-changing indicator, from the viewpoint of visibility.

[0030] (solvent) The composition of the present invention may further comprise a solvent. The solvent is not particularly limited as long as it can dissolve the color-changing dye, the base, and the binder resin including the polyamide resin, and examples thereof include various solvents such as water, alcohol (alcohol or polyhydric alcohol), ester, ether, ketone, hydrocarbon, glycol ether, etc. The solvent may be used alone or in combination of two or more.

[0031] The solvent may be appropriately selected depending on the solubility of the color-changing dye, base, and binder resin containing polyamide resin to be used, and is preferably one having an appropriate drying speed. As the solvent used for dissolving the color-changing dye and the binder resin containing the polyamide resin, for example, a ketone-based solvent, an alcohol-based solvent, a glycol ether-based solvent, or the like is preferable. Moreover, examples of the solvent used when dissolving the base include water and alcohols (eg, ethanol, isopropanol, methanol, etc.), and water is more preferred from the viewpoint of the solubility of the base.

[0032] When a solvent is contained, the content thereof can be appropriately determined depending on the types of the color-changing pigment, base, and binder resin including polyamide resin used, and is not particularly limited. From the viewpoint of improving the coatability of the composition and adjusting the drying time of the composition, the content thereof is preferably 40 to 900% by weight, and more preferably 60 to 600% by weight, relative to 100% by weight of the total solid content of the composition for a time-discoloring indicator.

[0033] (Additives) In addition to the above-mentioned components, the composition of the present invention may contain known additives as optional components. The additives are not particularly limited, but examples thereof include leveling agents, thickeners, dispersants, etc. The leveling agent is not particularly limited, but examples thereof include silicone oil. The thickener is preferably one that can impart a thickening effect to the composition of the present invention and improve the coatability thereof, and examples of the thickener include silicate minerals and silicate synthetic products. The dispersant is preferably one that can better disperse the components in the composition of the present invention, particularly the basic inorganic compound, etc. Examples of the dispersant include polymer dispersants (e.g., Solsperse 41000, Solsperse 45000, Solsperse 54000, Solsperse 66000 (all manufactured by Lubrizol Corporation)), surfactants, etc. When the above-mentioned various additives are contained, their total content (solid content) is not particularly limited, but is preferably 0.01 to 30% by weight, and more preferably 0.1 to 15% by weight, based on 100% by weight of the total solid content of the composition for a time-discoloring indicator.

[0034] The method for preparing the composition for indicators that change color over time of the present invention is not particularly limited, but for example, the composition can be prepared by mixing and stirring the above-mentioned components by a known method. In addition, it is preferable that the composition is stored in a sealed container immediately after preparation, or used to form a color-changing layer of an indicator.

[0035] (2) Indicator that changes color over time The time-changing indicator of the present invention is characterized by having a color-changing layer formed from the composition of the present invention on a substrate. Furthermore, the time-discoloring indicator of the present invention comprises a substrate and a color-changing layer, the color-changing layer comprising a color-changing pigment, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, and the binder resin comprises a polyamide resin.

[0036] (base material) The substrate is not particularly limited as long as it can form and support a discoloration layer. For example, metal or alloy materials (aluminum foil, stainless steel foil, tin foil, tin foil, etc.), plastics (films or molded bodies of polyester (various polyesters such as polyethylene terephthalate), cellophane, acetyl cellulose, ethyl cellulose, polyethylene, polypropylene, polyvinyl chloride, rubber hydrochloride, polystyrene, polycarbonate, polyvinyl alcohol, polyvinyl fluoride, polyamide, polyethylene fluoride, etc.), fibers (paper, wood materials, nonwoven fabric, woven fabric, other fiber sheets), inorganic materials (ceramics, glass, concrete, gypsum), composite materials thereof, etc. can be used. The thickness of the substrate can be appropriately set according to the type of indicator.

[0037] (Discoloration layer) The color-changing layer is formed from the composition of the present invention. For example, a method of forming the color-changing layer includes a method of forming a coating film of the composition of the present invention on a substrate. Specifically, the color-changing layer can be formed by applying the composition of the present invention on a substrate and then drying the composition. The method for applying the composition of the present invention to a substrate is not particularly limited, and examples of the method include known application methods such as spin coating, slit coating, spray coating, and dip coating; known printing methods such as silk screen printing, gravure printing, offset printing, letterpress printing, and flexographic printing. In the present invention, application also includes concepts such as printing and immersion other than application. After the composition of the present invention is applied, the coating is dried. The drying temperature is not particularly limited, but is usually preferably about 80 to 200°C, and more preferably about 100 to 150°C. The thickness of the color-changing layer in the indicator of the present invention is not particularly limited, but from the viewpoints of visibility and handling of the printed matter, it is preferably about 500 nm to 2 mm, more preferably about 1 to 100 μm.

[0038] In addition, since the color-changing layer is formed by applying the composition of the present invention to a substrate and then drying it, the color-changing layer contains no or almost no solvent derived from the composition. As described above, in the composition, the color-changing dye reacts with the base to make the color-changing dye colorless. The alkali metal salt and / or ammonium salt (salt corresponding to the dye used) generated at that time is considered to be present in the color-changing layer of the indicator before the color change starts as a product derived from the base (at least one selected from alkali metal hydroxides and ammonia). Furthermore, when an excess of base is used relative to the color-changing dye in the composition used, a base (at least one selected from alkali metal hydroxides and ammonia) may be contained in the color-changing layer of the indicator before the initiation of color change, in addition to the above-mentioned alkali metal salts and ammonium salts. The content (solid content) of each component in the color-changing layer is preferably the same as the content (solid content) of each component in the above-mentioned composition.

[0039] (Non-discoloring layer) The indicator of the present invention may have a non-color-changing layer as a base layer in order to enhance the visibility of the color-changing layer. The non-color-changing layer is not particularly limited as long as it does not affect the acid-base reaction in the color-changing layer, and may be formed from a composition containing a pigment and / or a dye. Examples of the pigment include azo-based, phthalocyanine-based, perylene-based, quinacridone-based pigments, etc. Examples of the dye include azo-based, quinone-based, cyanine-based, phthalocyanine-based, indigo-based dyes, etc. The composition for the non-color-changing layer may contain a binder resin, an extender, a solvent, etc., as necessary. Examples of the binder resin, extender, and solvent include those similar to those described above, and each of them may be used alone or in combination of two or more. The method for forming the non-color-changing layer is not particularly limited, and the same known coating method, printing method, etc. as the above-mentioned color-changing layer can be used. The thickness of the non-color-changing layer can be appropriately set depending on the type of indicator.

[0040] In the present invention, the color-changing layer and the non-color-changing layer may be combined in any way. For example, the color-changing layer and the non-color-changing layer may be formed so that the color difference between the color-changing layer and the non-color-changing layer can be distinguished only by the color change of the color-changing layer, or the color difference between the color-changing layer and the non-color-changing layer can be eliminated only by the color change. In the present invention, it is particularly preferable to form the color-changing layer and the non-color-changing layer so that the color difference between the color-changing layer and the non-color-changing layer can be distinguished only by the color change. In order to make the color difference discernible, the color-changing layer and the non-color-changing layer may be formed so that at least one of characters, designs, and symbols appears only when the color-changing layer changes color. In the present invention, the characters, designs, and symbols include all information that notifies the user of a color change. These characters, etc. may be designed appropriately depending on the purpose of use, etc. Furthermore, the color-changing layer and the non-color-changing layer may be different colors from each other before the color change. For example, the two layers may be substantially the same color, and the color difference (contrast) between the color-changing layer and the non-color-changing layer may be distinguished only after the color change. In the present invention, preferred embodiments of the layer structure include, for example, (i) an indicator in which a color-changing layer is formed adjacent to at least one of the main surfaces of a substrate, and (ii) an indicator in which the non-color-changing layer and the color-changing layer are formed in that order on a substrate, the non-color-changing layer is formed adjacent to the main surface of the substrate, and the color-changing layer is formed adjacent to the main surface of the non-color-changing layer.

[0041] (Overcoat layer) The indicator of the present invention may optionally have an overcoat layer. The overcoat layer is disposed on the outermost layer of the indicator. Therefore, in either case where only a color-changing layer is provided on the substrate, or where a color-changing layer and a non-color-changing layer are provided on the substrate (for example, the layer configurations (i) and (ii) above), an overcoat layer is formed adjacent to the color-changing layer and disposed on the outermost layer of the indicator. The overcoat layer can be used mainly for the following purposes: (a) to prevent the color-changing layer of the indicator from coming into direct contact with the outside air, thereby controlling the color-changing sensitivity of the indicator (suppressing color change), and (b) to promote the color change of the indicator (particularly color change in a low-humidity environment), thereby improving the visibility of the color change of the indicator. In both of the above cases (a) and (b), the formation of the overcoat layer can also increase the coating strength of the color-changing layer.

[0042] The above case (a) will be explained below. The overcoat layer is not particularly limited as long as it does not inhibit the acid-base reaction of the color-changing dye, and can be formed from a composition containing a resin. The resin may be the same as the binder resin other than polyamide resin, and one or more of them may be used.

[0043] The composition for the overcoat layer may contain a solvent, etc., as necessary. For example, the above-mentioned resin may be dissolved in a solvent before use. The solvent may be the same as those described above, and may be used alone or in combination of two or more. The method for forming the overcoat layer is not particularly limited, and the same known coating method, printing method, etc. as for the color-changing layer can be used. The thickness of the overcoat layer is not particularly limited, but from the viewpoint of handling of the printed matter, it is preferably about 500 nm to 2 mm, and more preferably about 1 to 100 μm.

[0044] Next, the above case (b) will be explained below. The overcoat layer is not particularly limited as long as it does not inhibit the acid-base reaction of the color-changing dye, and can be formed from a composition containing a resin. The resin is different from the above-mentioned (a) and may be, for example, a resin or resin composition having an acid group, such as a vinylidene chloride-vinyl chloride-based special copolymer resin (e.g., Ixan SGA-1 (manufactured by Solvay Specialty Polymers)). The resin or resin composition having an acid group may have an acid group (a group that can act as an acid) in the resin, or may have an acidic substance having an acid group in the resin composition. One or more types of the resin may be used. The resin used in case (b) has the function of preventing the discoloration layer from coming into direct contact with the outside air and the function of promoting discoloration of the discoloration layer. It is considered that in a low humidity environment where carbon dioxide is not easily generated due to moisture in the air or carbon dioxide, the discoloration promoting function of the resin becomes apparent, while in a high humidity environment where carbon dioxide is easily generated, the function of the resin in suppressing the generation of carbon dioxide becomes apparent.

[0045] In the case of (b), since the overcoat layer accelerates the discoloration of the indicator (particularly discoloration in a low humidity environment), an overcoat layer is formed on the outermost layer of the indicator when the indicator starts to be used. This makes it possible to make the time when the indicator starts to be used the same as the time when the indicator starts to discolor, so that a resin or resin composition having an acid group can be used as the resin for the overcoat layer.

[0046] The composition for the overcoat layer may contain a solvent, etc., as necessary. For example, the above-mentioned resin may be dissolved in a solvent before use. The solvent may be the same as those described above, and may be used alone or in combination of two or more. The method for forming the overcoat layer is not particularly limited, and the same known coating method, printing method, etc. as the above-mentioned color-changing layer can be used. From the viewpoint of forming the overcoat layer at the start of use of the indicator, it is preferable to use the coating method among the above-mentioned methods. Further, examples of the method for forming the overcoat layer when the indicator is first used include a method in which the composition for the overcoat layer is applied to the color-changing layer with a brush, marker, spray, etc., immediately before use; a method in which an overcoat layer printed on a separate film is attached to the color-changing layer immediately before use; a method in which a spacer is provided between the color-changing layer and the overcoat layer, and the spacer is pulled out immediately before use, etc. The spacer is not particularly limited, but examples thereof include a plastic film, etc. The thickness of the overcoat layer is not particularly limited, but from the viewpoint of handling of the printed matter, it is preferably about 500 nm to 2 mm, and more preferably about 1 to 100 μm.

[0047] (Adhesive layer) The indicator of the present invention may have an adhesive layer on the back surface of the substrate (the surface opposite to the surface on which the color-changing layer is formed) as necessary. By having an adhesive layer on the back surface of the substrate, the indicator of the present invention can be reliably fixed to an object. The component of the adhesive layer is not particularly limited, and examples thereof include acrylic, urethane, silicone, etc. The thickness of the adhesive layer can be appropriately set depending on the type of indicator.

[0048] (indicator) The shape of the indicator of the present invention is not particularly limited, and a wide variety of shapes adopted for known indicators can be used.

[0049] The method for producing the indicator of the present invention is not particularly limited. For example, as described above, the respective raw materials are mixed and stirred to prepare a composition for a time-changing indicator, and this composition is used to form a color-changing layer on a substrate, thereby producing the indicator.

[0050] The obtained indicator is preferably stored in an absolutely dry space or in an absolutely dry atmosphere until it is used, and then exposed to the air when it is first used. By storing the indicator in an absolutely dry atmosphere in this manner, the initial color of the indicator can be maintained and the start of color change can be prevented, and the color change can be started when the indicator is first used. The method of storing the indicator in an absolute dry space or atmosphere is not particularly limited, but examples thereof include a method of storing the indicator in a plastic (polyethylene terephthalate, polypropylene, polyester, etc.) bag onto which a metal (aluminum, etc.) is vapor-deposited. Another example includes a method of storing the indicator in a state close to an absolute dry atmosphere by providing a film (material: polyethylene terephthalate, polypropylene, polyester, etc.) onto which a metal (aluminum, etc.) is vapor-deposited on at least the side of the indicator having a color-changing layer, thereby sealing at least the side of the indicator on the color-changing layer side. In this case, it is preferable to provide a metal vapor-deposited film on both sides of the indicator. Another example includes a method of storing the indicator by combining the above methods. The method for providing a metal vapor deposition film on one or both sides of the indicator is not particularly limited, but can be, for example, by attaching it via an adhesive layer, etc. The adhesive layer is not particularly limited, and examples thereof include the same adhesive layer as the above-mentioned adhesive layer. The indicator of the present invention can be stored as described above before use, and when use is started, the indicator can be removed from the metal-coated plastic bag and / or the metal-coated film of the indicator can be peeled off, thereby placing the indicator in the same environment as the product to which it is applied.

[0051] The use of the indicator of the present invention is not particularly limited, but suitable examples include application to products with expiration dates, such as food, insect repellents, dehumidifiers, and deodorants.

[0052] (Printed material) The printed matter of the present invention has a printed layer formed from the above-mentioned composition for indicators that change color over time. The object on which the composition of the present invention is printed includes products that are subject to product management, etc. Examples of the products include, but are not limited to, foods, insect repellents, dehumidifiers, deodorants, and other products that have expiration dates. When the composition of the present invention can be directly printed on the product, it may be printed directly on the product, and when it cannot be directly printed on the product, it may be printed on the outer packaging bag or the like of the product. When the printed matter is to be stored in an absolute dry atmosphere, it can be stored in the same manner as the above-mentioned indicator. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0054] (Examples 1 to 6, Comparative Examples 1 to 3) A composition for indicators that changes color over time was prepared by mixing and stirring the raw materials shown in Table 1 below. This composition was applied to a polyethylene terephthalate (PET) film (Toyobo Espet, corona treated surface) to a thickness of about 40 μm using a coater and dried (70°C x 3 minutes) to prepare an indicator having a color-changing layer on a substrate.

[0055] [Table 1]

[0056] In Table 1, each component other than the solvent indicates the solid content. The binder resin and other components in Table 1 are described as follows: Vegichem Green V756 (Tsukuno Foods Industry): Polyamide resin Vegichem Green V744 (Tsukuno Food Industry): Polyamide resin Ethocel 4 (Dow Chemical): Ethyl cellulose Ethocel 10 (Dow Chemical): Ethyl cellulose HPC-SSL (Nippon Soda): Hydroxypropyl cellulose Super Ester A-75 (Arakawa Chemical Industries): Special rosin ester resin Super Ester A-100 (Arakawa Chemical Industries): Special rosin ester resin Solsperse 41000 (Lubrizol): Dispersant for calcium hydroxide Dowanol PM (Dow Chemical): propylene glycol monomethyl ether

[0057] In addition, the following tests were carried out using the above indicator, and the results are shown in Table 1. Discoloration test: First, the chromaticity of the initial color was measured. Next, the indicator was left in an environment of 20℃ x 65%, and the chromaticity of the indicator's discolored layer was measured at regular intervals to determine the difference in chromaticity from the initial color. The chromaticity was also measured using a Konica Minolta FD-5 fluorescent spectrodensitometer. Water resistance test: After leaving the indicator in an environment of 20℃ x 65% humidity for 3 days, a drop of water was dropped onto the surface of the indicator with the discoloration layer and left for 1 minute. The dropped water was then wiped off with tissue paper and the state of the discoloration layer (coating film) was evaluated. ○: The discolored layer does not peel off from the substrate and remains as it is. ×: Discolored layer peels off from the substrate

[0058] The chromaticity difference (color difference) ΔE*ab was calculated according to the following formula. ΔE*ab=[(L*2-L*1) 2 +(a*2-a*1) 2 +(b*2-b*1) 2 ] 1 / 2 The color difference between the initial color and the chromaticity after a certain time had passed was calculated by taking the initial chromaticity of the indicator's color-changing layer as L*1, a*1, b*1, and the chromaticity after a certain time had passed as L*2, a*2, b*2.

[0059] From the results in Table 1, in Examples 1 to 6, the ΔE*ab difference between the initial color and the chromaticity after a certain time had elapsed increased over time, the coloring density was deep, the visibility was excellent, and further, the water resistance was good. On the other hand, in Comparative Example 1, the color density was good, but because it used hydroxypropyl cellulose, a water-soluble resin, it was altered by moisture, the color-changing layer peeled off from the indicator substrate, and water resistance was poor. In Comparative Examples 2 and 3, the water resistance was good, but the color difference (ΔE*ab) was small and the color density was low, so the visibility was poor.

Claims

1. The color-changing dye, the base, the basic inorganic compound, and the binder resin are included. the base is at least one selected from an alkali metal hydroxide and ammonia, the basic inorganic compound is a hydroxide of an element of Group 2 of the periodic table; The binder resin includes a polyamide resin, and The content of the basic inorganic compound is 1 to 15% by weight based on 100% by weight of the total solid content of the composition for a time-discoloring indicator. A composition for use as an indicator that changes color over time.

2. The composition comprises a color-changing dye, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, the basic inorganic compound is a hydroxide of an element of Group 2 of the periodic table; The binder resin includes a polyamide resin, and The content of the basic inorganic compound is 1 to 15% by weight based on 100% by weight of the total solid content of the composition for a time-discoloring indicator. A composition for use as an indicator that changes color over time.

3. 3. The composition for a time-discoloring indicator according to claim 1, wherein the content of the polyamide resin is 1 to 90% by weight based on 100% by weight of the total solid content of the composition for a time-discoloring indicator.

4. The composition for a time-discoloring indicator according to any one of claims 1 to 3, wherein the binder resin further comprises, in addition to the polyamide resin, at least one selected from a petroleum-based hydrocarbon resin, a vinyl resin, a butyral resin, an alkyd resin, an epoxy resin, a fluororesin, a silicone resin, a polyester resin, a coumarone resin, a polyimide resin, an alicyclic resin, an acrylic resin, a rosin resin, a rosin ester resin, a ketone resin, a hydrogenated ketone resin, and a cellulose resin.

5. The composition for a time-changing indicator according to any one of claims 1 to 4, further comprising a non-color-changing dye.

6. A color-changing indicator having a color-changing layer formed from the composition for a color-changing indicator according to any one of claims 1 to 5 on a substrate.

7. A substrate and a color-changing layer are included. the color-changing layer contains a color-changing dye, a basic inorganic compound, a binder resin, and an alkali metal salt and / or an ammonium salt, the basic inorganic compound is a hydroxide of an element of Group 2 of the periodic table; The binder resin includes a polyamide resin, and The content of the basic inorganic compound is 1 to 15% by weight based on 100% by weight of the color-changing layer. Aging indicator.

8. 8. The indicator according to claim 6 or 7, further comprising a non-color-changing layer, the non-color-changing layer including a pigment and / or a dye, and disposed between the substrate and the color-changing layer.

9. The indicator according to any one of claims 6 to 8, further comprising an overcoat layer.

10. A printed matter having a printed layer formed from the composition for a time-discoloring indicator according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Plastic intaglio table printing ink for printing quick-frozen food packaging material and preparation method thereof

    CN106433296A

  • Printing ink binder and printing ink containing same

    JP1984105066A

  • Polyamide resin improved in its water solubility

    JP1987243619A

  • Article sorting device

    JP1989002906A

  • Time indicator

    JP1999014616A