Rubber composition for tires and tires

The rubber composition for tires, combining silica and binder-coated carbon nanotube particles, addresses the challenge of achieving low heat generation and conductivity by improving dispersibility and processability.

JP7590175B2Active Publication Date: 2024-11-26TOYO TIRE CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020210755
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-26
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing rubber compositions for tires face challenges in achieving both low heat generation performance and electrical conductivity due to the aggregation of carbon nanotubes, which increases viscosity and complicates the kneading process.

Method used

A rubber composition is formulated by kneading diene rubber with silica and carbon nanotube particles coated with a binder and granulated to improve dispersibility, reducing aggregation and enhancing processability.

Benefits of technology

The composition achieves both low heat generation performance and electrical conductivity while improving processability, with carbon nanotube granulation reducing viscosity and enhancing dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590175000001
    Figure 0007590175000001
  • Figure 0007590175000002
    Figure 0007590175000002
  • Figure 0007590175000003
    Figure 0007590175000003
Patent Text Reader

Abstract

To provide a rubber composition for tires that strikes a balance between low heat generation and electric conductivity.SOLUTION: A rubber composition for tires according to an embodiment is produced by kneading a diene rubber, silica, and granular carbon nanotubes consisting of binder-coated, granulated carbon nanotubes. A tire according to an embodiment comprises the rubber composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tires and a tire using the same. [Background technology]

[0002] It is known that the use of silica as a filler in a rubber composition for tires improves wet performance, which is the running performance on wet roads, and low heat generation performance, which contributes to low fuel consumption. On the other hand, when carbon black as a reinforcing filler is replaced with silica, the conductivity of the rubber composition decreases, making the tire more likely to be charged, which may cause static electricity sparks or malfunction of electronic components.

[0003] Patent Document 1 discloses a conductive rubber composition in which a master batch in which carbon nanotubes are added to rubber having a Mooney viscosity of 30 or less is blended with rubber having a Mooney viscosity of 30 or less to improve electrical conductivity. Patent Document 2 discloses blending vapor-grown carbon fibers that have been subjected to a crushing treatment with a rubber composition in which a rubber reinforcing material is blended with a rubber component. Patent Document 3 discloses a rubber composition in which vapor-grown carbon fibers having a fiber diameter of 20 to 120 nm, a fiber length of 2 to 20 μm, and an aspect ratio of 20 to 1000 are blended with a rubber component.

[0004] On the other hand, Patent Document 4 discloses that in order to improve the handling properties of carbon nanotubes, carbon nanotubes are coated with rubber latex as a binder and granulated to obtain carbon nanotube granules. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-167216 A [Patent Document 2] JP 2010-275376 A [Patent Document 3] JP 2009-102630 A [Patent Document 4] Patent No. 6499781 Summary of the Invention [Problem to be solved by the invention]

[0006] Although carbon nanotubes have an excellent effect of improving electrical conductivity, when they are added to diene rubber and kneaded, the viscosity increases significantly due to the aggregation of carbon nanotubes, making the kneading process difficult. Therefore, even if carbon nanotubes are added to a rubber composition containing silica, it is difficult to achieve both the low heat generation performance of silica and the improved electrical conductivity of carbon nanotubes.

[0007] In view of the above, an object of an embodiment of the present invention is to provide a rubber composition for tires that can achieve both low heat generation performance and electrical conductivity. [Means for solving the problem]

[0008] A first embodiment of the present invention is a rubber composition for tires, which is obtained by kneading a diene rubber, silica, and carbon nanotube granules obtained by coating carbon nanotubes with a binder and granulating the carbon nanotubes.

[0009] A second embodiment of the present invention is a rubber composition for tires, comprising a diene rubber as a matrix rubber component, silica, and carbon nanotubes coated with at least one selected from the group consisting of rubber of rubber latex, a liquid polymer, and a mineral oil.

[0010] A third embodiment of the present invention is a tire comprising these rubber compositions for tires. Effect of the Invention

[0011] According to the embodiment of the present invention, it is possible to achieve both low heat generation performance and electrical conductivity, and also to improve processability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The rubber composition for tires according to the embodiment is produced by kneading a diene rubber, silica, and carbon nanotube granules obtained by coating carbon nanotubes with a binder and granulating the carbon nanotubes.

[0013] The diene rubber as the matrix rubber component is not particularly limited, and various diene rubbers that are usually used in rubber compositions for tires can be used. For example, natural rubber (NR), synthetic isoprene rubber (IR), polybutadiene rubber (BR), styrene butadiene rubber (SBR), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, etc. can be mentioned, and any one of them can be used alone or in combination of two or more. Specific examples of each of these diene rubbers include modified diene rubbers that are modified by introducing functional groups such as amino groups and hydroxy groups into the molecular terminals or molecular chains. Here, the matrix rubber component is a rubber component that constitutes a continuous phase in a rubber composition, and fillers such as silica and carbon nanotube particles are dispersed as dispersoids in the matrix rubber component. Note that even when a diene rubber latex is used as a binder for the carbon nanotube particles, the rubber of the diene rubber latex is not included in the matrix rubber component referred to here.

[0014] The diene rubber as the matrix rubber component preferably contains at least one selected from the group consisting of natural rubber, polybutadiene rubber, and styrene-butadiene rubber. More preferably, the diene rubber contains 50 to 100 parts by mass of styrene-butadiene rubber and 0 to 50 parts by mass of natural rubber and / or polybutadiene rubber, and in this case, the styrene-butadiene rubber may be used alone.

[0015] The silica is blended as a filler, and blending silica can improve the balance between low heat generation performance and wet performance. The silica is not particularly limited, and for example, wet silica such as wet precipitation silica or wet gel silica may be used.

[0016] The BET specific surface area of ​​the silica (measured according to the BET method described in JIS K6430) is not particularly limited, and is, for example, 100 to 300 m 2 / g is also acceptable, 150 to 250m 2 / g is also acceptable.

[0017] The compounding amount of silica is preferably 50 to 150 parts by mass relative to 100 parts by mass of the diene rubber as the matrix rubber component. By compounding the silica in an amount of 50 parts by mass or more, the effect of improving the low heat generation performance inherent to silica compounding can be enhanced, and by compounding the silica in an amount of 150 parts by mass or less, deterioration of processability can be suppressed. The compounding amount of silica is more preferably 60 to 120 parts by mass, and further preferably 60 to 100 parts by mass relative to 100 parts by mass of the diene rubber.

[0018] In the rubber composition for tires according to the present embodiment, the filler preferably contains silica as a main component. The filler may be silica alone or may be used in combination with silica and carbon black, but it is preferable that the filler contains more than 70 mass% silica, and more preferably does not substantially contain carbon black. Note that carbon nanotubes are not included in the carbon black referred to here.

[0019] The rubber composition for tires according to the present embodiment may contain a silane coupling agent together with silica. Examples of the silane coupling agent include sulfide silane and mercapto silane. The amount of the silane coupling agent is not particularly limited, and may be, for example, 2 to 20 mass% based on the amount of silica.

[0020] The rubber composition for tires according to the present embodiment contains carbon nanotube granules. The carbon nanotube granules are formed by coating carbon nanotubes with a binder and granulating them. This prevents carbon nanotubes from scattering, improves handling, and reduces environmental and safety risks. In addition, by coating the carbon nanotubes, the aggregation of the carbon nanotubes is suppressed, and they are easily mixed into the diene rubber as a matrix rubber component, resulting in good dispersibility. As a result, in a rubber composition containing silica, it is possible to achieve both low heat generation performance and electrical conductivity, and to improve processability.

[0021] Carbon nanotubes have a cylindrical structure of graphite sheets whose main structure is a six-membered carbon ring structure. Examples of carbon nanotubes include single-wall nanotubes, multi-wall nanotubes, double-wall nanotubes, and cup-stack nanotubes, and any known carbon nanotube can be used.

[0022] The fiber diameter of the carbon nanotube is not particularly limited and may be, for example, 0.1 to 300 nm, 1 to 200 nm, or 5 to 50 nm. The fiber length of the carbon nanotube is also not particularly limited and may be, for example, 1 to 500 μm, 3 to 100 μm, or 5 to 50 μm.

[0023] The binder is a coating material that coats the carbon nanotubes, and it is sufficient that at least a portion of the surface of the carbon nanotubes is coated with the binder, and it is not necessary that the entire surface of the carbon nanotubes is coated with the binder. By coating the carbon nanotubes with the binder, the carbon nanotubes can be bonded together and granulated, and the handling properties can be improved.

[0024] The carbon nanotube granules may be partially or completely crushed during kneading with the diene rubber, or may remain as granules before kneading without being crushed. In one embodiment, the rubber composition after kneading may contain partially crushed granules. In this way, the binder may have an adhesive strength that is such that it is partially or completely crushed during kneading, and by being crushed during kneading, the dispersibility of the carbon nanotubes in the diene rubber as the matrix rubber component can be further improved.

[0025] As the binder, for example, rubber latex, liquid polymer, mineral oil, etc. are preferably used. That is, the carbon nanotube granules are preferably obtained by coating and granulating carbon nanotubes using at least one binder selected from the group consisting of rubber latex, liquid polymer, and mineral oil. In the carbon nanotube granules, the carbon nanotubes are coated with at least one coating material selected from the group consisting of rubber of rubber latex, liquid polymer, and mineral oil, and the carbon nanotube granules are formed by granulating the carbon nanotubes using these coating materials as binders.

[0026] Examples of the rubber latex include diene-based rubber latexes such as natural rubber latex, polybutadiene latex, styrene-butadiene copolymer latex, acrylonitrile-butadiene copolymer latex, chloroprene rubber latex, etc. The rubber of the diene-based rubber latex may be the same or different from the diene-based rubber as the matrix rubber component.

[0027] The liquid polymer is a polymer that is liquid at room temperature (23° C.), and examples of the liquid polymer include polymers (including oligomers) having a weight average molecular weight Mw of 10,000 or less. Specific examples of the liquid polymer include polyethylene, silicone, and poly-α-olefin.

[0028] Examples of mineral oils include liquid paraffin, paraffin-based mineral oil, naphthenic mineral oil, and aromatic mineral oil.

[0029] The amount of binder relative to the carbon nanotubes is not particularly limited. For example, the amount of carbon nanotubes relative to 100 parts by mass of binder is preferably 100 to 5000 parts by mass, more preferably 200 to 4000 parts by mass, and even more preferably 300 to 3000 parts by mass, and may be 500 to 2000 parts by mass.

[0030] The size of the carbon nanotube granules is not particularly limited, and may be, for example, an average particle size of 0.1 to 3.0 mm, 0.3 to 2.5 mm, or 0.5 to 2.0 mm. Here, the average particle size is the arithmetic mean value of particle sizes measured for 50 granules randomly selected by microscopic observation.

[0031] The method for producing the carbon nanotube granules is not particularly limited, but when rubber latex is used as a binder, the following methods (A) to (C) described in the above Patent Document 4 (Japanese Patent No. 6499781) are included. The production method described in Japanese Patent No. 6499781 is incorporated herein by reference.

[0032] Manufacturing method (A): Carbon nanotubes and water are mixed and stirred to prepare a dispersion, rubber latex is added to the dispersion and mixed, and while stirring the resulting mixture, a non-water-soluble solvent is added dropwise to transfer the carbon nanotubes from the aqueous phase to the rubber phase to form granules, the aqueous phase and the granules are separated, and the separated granules are dried.

[0033] Manufacturing method (B): Water and rubber latex are mixed and stirred to prepare a dispersion, carbon nanotubes are added to the dispersion and mixed, and while stirring the resulting mixture, a non-water-soluble solvent is added dropwise to transfer the carbon nanotubes from the aqueous phase to the rubber phase to form granules, the aqueous phase and the granules are separated, and the separated granules are dried.

[0034] Manufacturing method (C): Rubber latex, carbon nanotubes, and water are mixed and stirred, and a non-water-soluble solvent is added dropwise to the resulting mixture to transfer the carbon nanotubes from the aqueous phase to the rubber phase, forming granules. The aqueous phase and the granules are then separated, and the separated granules are dried.

[0035] In the above-mentioned production method, examples of the non-water-soluble solvent include toluene, xylene, hexane, tetrahydrofuran, benzene, cyclohexane, and carbon tetrachloride.

[0036] The amount of carbon nanotube particles added is not particularly limited, and may be, for example, 0.5 to 30 parts by mass, 1 to 25 parts by mass, or 2 to 20 parts by mass per 100 parts by mass of the diene rubber as the matrix rubber component.

[0037] Preferably, the carbon nanotube granules are blended so that the volume fraction of the carbon nanotubes in the rubber composition for tires is 0.5 to 5.0%. The volume fraction is the volume fraction of the carbon nanotubes contained in the rubber composition when the entire rubber composition for tires is taken as 100%. When the volume fraction of the carbon nanotubes is 0.5% or more, the effect of improving the electrical conductivity can be enhanced, and when the volume fraction of the carbon nanotubes is 5.0% or less, the effect of improving the low heat generation performance and the processability can be enhanced. The volume fraction of the carbon nanotubes is preferably 0.7 to 4.0%, more preferably 1.0 to 3.0%.

[0038] In addition to the above-mentioned components, the rubber composition for tires according to the present embodiment may contain various additives that are generally used in rubber compositions, such as zinc oxide, stearic acid, oil, wax, an antioxidant, a vulcanizing agent, and a vulcanization accelerator.

[0039] As the vulcanizing agent, sulfur is preferably used. The amount of the vulcanizing agent is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the diene rubber as the matrix rubber component.

[0040] Examples of the vulcanization accelerator include various vulcanization accelerators such as sulfenamide-based, thiuram-based, thiazole-based, guanidine-based, and dithiocarbamate-based, and any one of them can be used alone or in combination of two or more. The amount of the vulcanization accelerator is not particularly limited, but is preferably 0.1 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the diene rubber as the matrix rubber component.

[0041] The rubber composition for tires according to the present embodiment is obtained by kneading diene rubber, silica, and carbon nanotube granules as matrix rubber components, and may be kneaded with the above-mentioned additives as optional components. For kneading, a mixer such as a Banbury mixer, kneader, or roll that is usually used for preparing rubber compositions may be used, and kneading may be performed according to a conventional method. For example, in the first mixing stage (non-pro kneading step), additives other than vulcanizing agent and vulcanization accelerator are added and mixed with silica and carbon nanotube granules to diene rubber. Next, in the final mixing stage (pro kneading step), vulcanizing agent and vulcanization accelerator are added and mixed to the obtained mixture to prepare an unvulcanized rubber composition.

[0042] In the obtained rubber composition for tires, the carbon nanotube granules may be present as granules before kneading as described above, may be partially crushed, may be completely crushed and no longer have a granular form, or may be a mixture of one or more of these forms. Therefore, the rubber composition for tires according to one embodiment contains a diene rubber as a matrix rubber component, silica, and carbon nanotubes coated with at least one selected from the group consisting of rubber derived from rubber latex, a liquid polymer, and a mineral oil, and the carbon nanotubes may be contained in the form of granules, or may be contained in the form of partially or completely crushed.

[0043] The rubber composition for tires according to the present embodiment can be used for various applications and for tires of various sizes, such as tires for passenger cars and heavy-duty tires for trucks and buses, and can be applied to various parts of tires, such as the tread portion, sidewall portion, etc. It is preferably used as tire tread rubber, i.e., it is a rubber composition for tire treads.

[0044] The tire according to the present embodiment is produced using the rubber composition for tires. The tire is preferably a pneumatic tire. As an embodiment, the tire may be provided with a tread rubber made of the rubber composition. The tire can be manufactured by producing tire components such as tread rubber using the rubber composition with a rubber extruder or the like, combining the tire components with other tire components to produce an unvulcanized tire (green tire), and then vulcanizing and molding the tire at, for example, 140 to 180°C.

[0045] In addition, the various numerical ranges, including the above-mentioned blending amounts and fiber diameters, can be arbitrarily combined with their upper and lower limits, and all of these combinations are considered to be preferred numerical ranges and are described in this specification. EXAMPLES

[0046] Examples will be shown below, but the present invention is not limited to these examples.

[0047] The components used in the examples and comparative examples are as follows. SBR: Styrene butadiene rubber, JSR Corporation "JSR1502" BR: Polybutadiene rubber, Ube Industries, Ltd. "UBEPOL BR150B" NR: Natural rubber, RSS#3 Silica 1: Tosoh Silica Corporation's "Nipsil AQ" BET specific surface area: 205 m 2 / g Silica 2: Evonik Industries "ULTRASIL 9100GR" BET specific surface area: 235 m 2 / g Silane coupling agent: Evonik Industries "Si69" Oil: ENEOS Corporation "Process NC140" CNT: Carbon nanotube, Kumho's "K-Nanos-100P" (fiber diameter: 8-15 nm, fiber length: 26 μm) Carbon black: N339 Zinc oxide: "No. 1 zinc oxide" manufactured by Mitsui Mining & Smelting Co., Ltd. Stearic acid: Kao Corporation's "Lunac S-20" Wax: "OZOACE0355" manufactured by Nippon Seiro Co., Ltd. Anti-aging agent: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, "Nocrac 6C" manufactured by Ouchi Shinko Chemical Co., Ltd. Sulfur: Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: "Soxinol CZ" manufactured by Sumitomo Chemical Co., Ltd.

[0048] CNT granules 1: Carbon nanotube granules prepared by the following method in accordance with the method described in Japanese Patent No. 6499781. A 10L stainless steel round container was equipped with a homogenizer with a maximum speed of 10,000 rpm and a portable mixer with paddle blades. 7.4g of concentrated natural rubber latex (manufactured by Resitex, rubber concentration: 60% by mass) was added to 4455g of water. 45g of CNT (Kumho's "K-Nanos-100P") was added little by little while stirring at about 600 rpm until the entire amount was added. The mixer was switched to a homogenizer and dispersed at about 6000 rpm for 30 minutes. A few drops of the obtained dispersion were taken on a glass plate with a dropper and spread with a spatula. Undispersed lumps were visually and finger-examined, and no rough undispersed lumps were found. Here, the CNT concentration in water was about 1% by mass, and the ratio of rubber (solid rubber content of rubber latex) to CNT was about 10% by mass. Next, the homogenizer was switched to a portable mixer, and while stirring at 700 rpm, 400 g of toluene was dropped as a non-water-soluble solvent using an automatic dropping device over 20 minutes to obtain granules with a diameter of about 1 mm. The obtained granules were separated from the water using a 60 mesh sieve, and then naturally dried at room temperature in a draft for about 20 hours. Next, the granules were heated at 70 to 80°C using a vacuum dryer, and dried until the heat loss of the solvent and remaining water in the granules at 150°C for 1 hour was 0.5 mass% or less, obtaining CNT granules 1.

[0049] CNT granules 2: CNT granules 2 were obtained in the same manner as CNT granules 1, except that 5.0 g of liquid paraffin (manufactured by Nacalai Tesque, Inc.) was used instead of 7.4 g of concentrated natural rubber latex.

[0050] CNT granule 3: CNT granule 3 was obtained in the same manner as CNT granule 1, except that 9.0 g of styrene-butadiene copolymer latex ("Rodex" manufactured by JSR Corporation, rubber concentration: 50 mass%) was used instead of 7.4 g of concentrated natural rubber latex.

[0051] CNT granules 4: CNT granules 4 was obtained in the same manner as CNT granules 1, except that Kumho's "K-Nanos-300P" (fiber diameter: 8-28 nm, fiber length: 50 μm) was used instead of Kumho's "K-Nanos-100P" as the CNTs.

[0052] [Example 1: Rubber composition and evaluation] Using a Banbury mixer, in accordance with the formulation (parts by mass) shown in Table 1 below, first, in the first mixing stage, compounding ingredients other than sulfur and vulcanization accelerator were added to the rubber component and kneaded (discharge temperature = 160 ° C.). Next, in the final mixing stage, sulfur and vulcanization accelerator were added to the obtained kneaded product and kneaded (discharge temperature = 90 ° C.). In this way, a rubber composition was prepared.

[0053] The rubber compositions thus obtained were evaluated for processability, and also vulcanized at 160°C for 30 minutes to prepare test pieces of a prescribed shape, which were then used to evaluate low heat generation performance and electrical conductivity. The methods of measurement and evaluation are as follows. The results are shown in Table 1 below. In Table 1, "Silica (volume %)" and "CNT (volume %)" indicate the volume fractions of silica and carbon nanotubes in the rubber composition.

[0054] Processability: In accordance with JIS K6300, a rotorless Mooney tester manufactured by Toyo Seiki Co., Ltd. was used to preheat unvulcanized rubber at 100°C for 1 minute, and the torque value after 4 minutes was measured in Mooney units and expressed as an index with the value of Comparative Example 1 set at 100. The smaller the index, the lower the Mooney viscosity and the better the processability.

[0055] Low heat generation performance: In accordance with JIS K6394, the loss factor tan δ was measured under conditions of a frequency of 10 Hz, static strain of 10%, dynamic strain of 2%, and a temperature of 70°C, and expressed as an index with the value of Comparative Example 1 set at 100. The smaller the index, the smaller the tan δ and the less likely it is to generate heat, i.e., the more excellent the low heat generation performance (fuel economy).

[0056] Electrical conductivity: Electrical volume resistivity was measured using Mitsubishi Chemical Analytech's "Hirester UP," the measured value was taken in common logarithm, and expressed as an index with the value of Comparative Example 1 set at 100. The smaller the index, the smaller the electrical resistance and the better the electrical conductivity.

[0057] [Table 1]

[0058] As shown in Table 1, in comparison with Comparative Example 1 in which carbon nanotubes were blended as they were, Examples 1 to 7 in which carbon nanotube granules formed by coating and granulating carbon nanotubes with rubber latex as a binder were used showed a reduced viscosity of the unvulcanized rubber, excellent processability, and improved low heat generation performance and electrical conductivity. Comparative Example 2 in which carbon black was blended instead of carbon nanotubes showed improved processability and low heat generation performance compared to Comparative Example 1, but electrical conductivity was significantly worse.

[0059] When the cross-section of the vulcanized rubber composition of Example 1 was observed under a microscope at 30x magnification, it was confirmed that the carbon nanotube granules were present in a partially crushed form, that is, they did not remain in the same form as the granules before kneading, but were crushed to present as smaller particles.

[0060] [Example 2: Rubber composition and evaluation] The amount of silica and other components was increased according to the formulation (parts by mass) shown in Table 2 below, but otherwise the rubber composition was prepared in the same manner as in Example 1, test pieces were prepared, and then processability, low heat generation performance, and electrical conductivity were evaluated. Each measurement and evaluation method was as described above, and all were shown here as indexes with the value of Comparative Example 3 set at 100.

[0061] [Table 2]

[0062] As shown in Table 2, even when silica was highly loaded, in the cases of Examples 8 to 12, which used carbon nanotube granules, as in the first example, the viscosity of the unvulcanized rubber was reduced and processability was excellent, and both the low heat generation performance and electrical conductivity were improved compared to Comparative Example 3, in which carbon nanotubes were directly loaded.

[0063] [Third Example: Rubber Composition and Evaluation] The amount of silica and other components was increased according to the formulation (parts by mass) shown in Table 3 below, but otherwise the rubber composition was prepared in the same manner as in Example 1, test pieces were prepared, and then processability, low heat generation performance, and electrical conductivity were evaluated. Each measurement and evaluation method was as described above, and all were shown here as indexes with the value of Comparative Example 4 set at 100.

[0064] [Table 3]

[0065] As shown in Table 3, even when silica was further loaded, in Example 13 using carbon nanotube granules, as in Example 1, the viscosity of the unvulcanized rubber was reduced and processability was excellent, and both the low heat generation performance and electrical conductivity were improved compared to Comparative Example 4 in which carbon nanotubes were directly loaded.

[0066] [Example 4: Rubber composition and evaluation] The type of silica was changed according to the compounding (parts by mass) shown in Table 4 below, but otherwise rubber compositions were prepared in the same manner as in Example 1, test pieces were prepared, and then processability, low heat generation performance, and electrical conductivity were evaluated. Each measurement and evaluation method was as described above, and all were shown here as indexes with the value of Comparative Example 5 set at 100.

[0067] [Table 4]

[0068] As shown in Table 4, even when silica 2 having a small particle size was blended, in Example 14 using carbon nanotube granules, as in the first example, the viscosity of the unvulcanized rubber was reduced and processability was excellent, and both the low heat generation performance and electrical conductivity were improved compared to Comparative Example 5 in which carbon nanotubes were blended as is.

[0069] [Fifth Example: Rubber Composition and Evaluation] The diene rubber component was changed according to the compounding (parts by mass) shown in Table 5 below, and otherwise rubber compositions were prepared in the same manner as in Example 1, test pieces were prepared, and then processability, low heat generation performance, and electrical conductivity were evaluated. Each measurement and evaluation method was as described above, and all were shown here as indexes with the value of Comparative Example 6 set to 100.

[0070] [Table 5]

[0071] As shown in Table 5, even when a blend of SBR and BR was used as the diene rubber for the matrix rubber component, in Example 15 using carbon nanotube granules, as in the first example, the viscosity of the unvulcanized rubber was reduced and processability was excellent, and both the low heat generation performance and electrical conductivity were improved compared to Comparative Example 6 in which carbon nanotubes were directly blended.

[0072] [Sixth Example: Rubber Composition and Evaluation] The diene rubber component was changed according to the compounding (parts by mass) shown in Table 6 below, and otherwise rubber compositions were prepared in the same manner as in Example 1, test pieces were prepared, and then processability, low heat generation performance, and electrical conductivity were evaluated. Each measurement and evaluation method was as described above, and all were shown here as indexes with the value of Comparative Example 7 set at 100.

[0073] [Table 6]

[0074] As shown in Table 6, even when a blend of SBR and NR was used as the diene rubber for the matrix rubber component, in Example 16 using carbon nanotube granules, as in Example 1, the viscosity of the unvulcanized rubber was reduced and processability was excellent, and both the low heat generation performance and electrical conductivity were improved compared to Comparative Example 7 in which carbon nanotubes were directly blended.

[0075] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. A rubber composition for tires is obtained by kneading a diene rubber, silica, and carbon nanotube granules obtained by coating carbon nanotubes with a binder and granulating the carbon nanotubes, and does not contain carbon black.

2. 2. The rubber composition for tires according to claim 1, wherein a volume fraction of said carbon nanotubes in said rubber composition for tires is 0.5 to 5.0%.

3. 3. The rubber composition for tires according to claim 1, comprising 50 to 150 parts by mass of said silica per 100 parts by mass of said diene rubber.

4. The rubber composition for tires according to any one of claims 1 to 3, wherein the carbon nanotube granules are formed by coating and granulating carbon nanotubes using at least one binder selected from the group consisting of rubber latex, liquid polymers, and mineral oils.

5. A tire comprising the rubber composition for tires according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Manufacture of pipe interior build-up clad pipe

    JP1989099781A

  • Rubber composition

    JP2009102630A

  • Rubber composition and tire using the same

    JP2010275376A

  • Conductive rubber composition and master batch as raw material of the same

    JP2012167216A

  • Rubber master batch and method for producing the same, and rubber composition obtained from the rubber master batch

    JP2018100334A