Method for manufacturing a nonlinear optical device

By using a low concentration solvent to fill recesses and then adding a high concentration nonlinear optical polymer solution under reduced pressure, the method addresses void formation issues in nonlinear optical devices, enhancing optical performance and miniaturization.

JP7590438B2Active Publication Date: 2024-11-26NAT INST OF INFORMATION & COMM TECH +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022540154
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-31
Filing Date
2021-07-14
Publication Date
2024-11-26
Estimated Expiration
2041-07-14

Smart Images

  • Figure 0007590438000006
    Figure 0007590438000006
  • Figure 0007590438000007
    Figure 0007590438000007
  • Figure 0007590438000008
    Figure 0007590438000008
Patent Text Reader

Abstract

The present invention provides a method for producing a nonlinear optical device. A recessed part (10) is formed in the surface of a semiconductor substrate (100). The recessed part (10) is filled with a first liquid material (31) in a reduced pressure environment. A third liquid material (33) is prepared by bringing a second liquid material (32) into contact with the first liquid material (31) that fills the recessed part (10). A buried part (310) is formed by solidifying the third liquid material (33). The first liquid material (31) contains a first solute and a first solvent, or alternatively, is composed only of the first solvent. The second liquid material (32) contains a second solute and a second solvent. The second solute contains a nonlinear optical polymer. The concentration of the second solute in the second liquid material (32) is higher than the concentration of the first solute in the first liquid material (31).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a nonlinear optical device. This application claims priority to Japanese Patent Application No. 2020-130371, filed on July 31, 2020. The entire contents of the Japanese Patent Application are incorporated herein by reference. [Background technology]

[0002] Methods of filling minute recesses formed on the surface of a substrate with a liquid material have been investigated (see, for example, Patent Documents 1 to 5 and Non-Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-071934 A [Patent Document 2] JP 2004-103817 A [Patent Document 3] Special Publication No. 2007-509769 [Patent Document 4] JP 2011-210942 A [Patent Document 5] JP 2014-099525 A

[0004] [Non-Patent Document 1] H. Hiroshima, M. Komuro, “Control of Bubble Defects in UV Nanoimprint” Japanese Journal Applied Physics, Vol. 46, pp. 6391-6394 (Sep. 2007) Summary of the Invention

[0005] A method for manufacturing a nonlinear optical device according to one aspect of the present disclosure includes the steps of: forming a recess in a surface of a semiconductor substrate; filling the recess with a first liquid material under a reduced pressure environment; preparing a third liquid material by contacting the first liquid material filled in the recess with a second liquid material; and, solidifying the third liquid material to form a filling portion; Including, the first liquid material contains a first solute and a first solvent, or consists of the first solvent alone; the second liquid material includes a second solute and a second solvent; the second solute comprises a nonlinear optical polymer; A concentration of the second solute in the second liquid material is higher than a concentration of the first solute in the first liquid material. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic flow chart of the method for manufacturing a nonlinear optical device according to the present embodiment. [Diagram 2] FIG. 2 is a first schematic cross-sectional view showing a manufacturing process of the nonlinear optical device of this embodiment. [Diagram 3] FIG. 3 is a schematic top view showing a first example of the recess. [Figure 4] FIG. 4 is a schematic top view showing a second example of the recess. [Diagram 5] 5A to 5C are second schematic cross-sectional views illustrating the manufacturing process of the nonlinear optical device of this embodiment. [Figure 6] FIG. 6 is a third schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. [Figure 7] FIG. 7 is a fourth schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. [Figure 8] FIG. 8 is a fifth schematic cross-sectional view showing a manufacturing process of the nonlinear optical device of this embodiment. [Figure 9] FIG. 9 is a sixth schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. [Figure 10] FIG. 10 is a first schematic cross-sectional view showing the manufacturing process of No. 2. [Figure 11] FIG. 11 is a second schematic cross-sectional view showing the manufacturing process of No. 2. [Figure 12] FIG. 12 is a schematic cross-sectional view showing the manufacturing process of No. 3. [Figure 13] FIG. 13 is a schematic top view of the evaluation device. [Figure 14] Figure 14 shows an example of the measurement of the light propagation streak image of No. 2. [Figure 15] Figure 15 shows an example of the propagation loss calculation for No. 2. [Figure 16] FIG. 16 shows the evaluation results for No. 1 to No. 3. [Figure 17] FIG. 17 is a schematic cross-sectional view showing an example of the bottom portion. [Figure 18] FIG. 18 is an example of a synthetic scheme for a side chain copolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] <Problems to be Solved by This Disclosure> In nonlinear optical (NLO) devices, embedded A buried structure is being considered. The buried structure is formed by filling a recess formed on the surface of a semiconductor substrate with an NLO polymer. For example, a polymer solution in which an NLO polymer is dissolved is used. That is, the polymer solution is applied to the surface of a semiconductor substrate having a recess, and the buried structure can be formed by solidifying the polymer solution.

[0008] As NLO devices become smaller and more highly integrated, it becomes necessary to fill narrower and deeper recesses with the polymer solution. The narrower and deeper the recess, the more likely it is that voids will remain in the recess after filling. For example, if the buried portion contains an optical waveguide, the voids in the buried portion can scatter light, which can result in propagation losses.

[0009] In order to reduce the voids, for example, it is conceivable to heat the polymer solution filled in the recesses. By increasing the temperature of the polymer solution, the air bubbles become more mobile, which is expected to reduce the voids.

[0010] Here, the NLO polymer includes, for example, a host polymer and guest molecules. The guest molecules are dispersed in the host polymer. The guest molecules are polar molecules and have NLO activity. When the polymer solution is heated, the temperature of the polymer solution increases to a level that causes the NLO polymer to flow, and the guest molecules may aggregate due to dipole-dipole interactions. The aggregation of the guest molecules may result in the loss of NLO activity.

[0011] In order to reduce the voids, for example, it is conceivable to fill the recesses with a polymer solution under a pressurized atmosphere. It is believed that the pressurization causes the bubbles to shrink. The shrinkage of the bubbles is expected to reduce the voids. However, the bubbles only become smaller in inverse proportion to the pressure. Therefore, it is believed that the voids cannot be completely removed.

[0012] In order to reduce the voids, it is possible to degas the polymer solution filled in the recesses, for example, under a reduced pressure atmosphere. It is thought that degassing under reduced pressure is accompanied by the evaporation of the solvent. The evaporation of the solvent occurs at the surface of the polymer solution. Therefore, solidification starts from the surface of the polymer solution. During degassing under reduced pressure, the polymer solution may solidify from the surface, which may hinder degassing or cause unevenness to form on the surface of the embedded part. For example, if the embedded part includes an optical waveguide, the unevenness of the surface may deteriorate the optical properties. Therefore, it is required to keep the optical waveguide away from the surface so that the effect on the optical properties is sufficiently small. As a result, the miniaturization of NLO devices may be hindered.

[0013] It is an objective of the present disclosure to form implants in NLO devices that have smooth surfaces and few voids.

[0014] <Advantages of this disclosure> According to the present disclosure, it is expected that a filling portion having a smooth surface and few voids will be formed.

[0015] <Description of the embodiments of the present disclosure> First, the embodiments of the present disclosure and their explanations are listed. However, the mechanism of action of the present disclosure includes assumptions. The correctness or incorrectness of the mechanism of action does not limit the scope of the claims.

[0016] [1] A method for manufacturing a nonlinear optical device according to one embodiment of the present disclosure includes the following steps (a) to (d): (a) A recess is formed in the surface of a semiconductor substrate. (b) In a reduced pressure environment, the recess is filled with a first liquid material. (c) A third liquid material is prepared by bringing a second liquid material into contact with the first liquid material filled in the recess. (d) The third liquid material is solidified to form the embedded portion. The first liquid material includes a first solute and a first solvent, or consists of only the first solvent. The second liquid material includes a second solute and a second solvent. The second solute includes a nonlinear optical polymer. The concentration of the second solute in the second liquid material is higher than the concentration of the first solute in the first liquid material.

[0017] The second liquid material of the present disclosure has a higher concentration than the first liquid material. Herein, the second liquid material is also referred to as a "high concentration solution." The first liquid material is also referred to as a "low concentration solution." However, "high concentration" and "low concentration" refer to the relative concentrations between the second liquid material and the first liquid material, and do not refer to the absolute concentrations.

[0018] In the method of manufacturing an NLO device of the present disclosure, a low concentration solution (first liquid material) is first filled into the recesses. The first liquid material may consist of a solvent only. The low concentration solution may have a low viscosity. It is believed that the low concentration solution easily enters the recesses. It is believed that air bubbles easily move in the low concentration solution. In other words, it is believed that air bubbles easily escape.

[0019] Furthermore, it is believed that solidification of a low-concentration solution does not progress easily from the surface even when exposed to a reduced pressure environment.

[0020] After the recess is filled with the low concentration solution, the high concentration solution (second liquid material) is added to the low concentration solution. A mixed solution (third liquid material) is formed by diffusion of the solute (NLO polymer) from the high concentration solution to the low concentration solution. The mixed solution in the recess is solidified to form the embedded portion. In this disclosure, "solidification" refers to the precipitation of the solute by substantially removing the solvent from the solution.

[0021] As described above, in the method of manufacturing an NLO device of the present disclosure, the low concentration solution (first liquid material) can penetrate into every corner of the recess, which is expected to reduce air bubbles. Therefore, it is expected that the number of voids will be reduced even in the filled part after solidification.

[0022] Furthermore, it is believed that in the low concentration solution (first liquid material), solidification does not proceed easily from the surface, and therefore it is expected that the surface of the embedded portion will be smooth.

[0023] [2] In the method for producing a nonlinear optical device according to the above [1], The first solute may include, for example, a nonlinear optical polymer.

[0024] [3] In the method for producing a nonlinear optical device according to the above [1] or [2], At least a portion of the recess may be formed, for example, to extend linearly along the surface of the semiconductor substrate.

[0025] The linearly extending recess may also be referred to as a "slot," etc. By forming the recess in a linear manner, for example, a slot waveguide type NLO device may be manufactured.

[0026] [4] The method for producing a nonlinear optical device according to any one of [1] to [3] above, The ratio of the depth of the recess to the width of the recess may be, for example, from 0.5 to 12.

[0027] Hereinafter, the ratio of the depth (d) of the recess to the width (w) of the recess will be referred to as the aspect ratio (d / w). With an aspect ratio of 0.5 or more, for example, high integration is expected. With an aspect ratio of 12 or less, for example, reduction of voids is expected.

[0028] [5] The method for producing a nonlinear optical device according to any one of [1] to [4] above, The recess may, for example, have a width of 170 nm or less.

[0029] The disclosed method for fabricating NLO devices is expected to reduce voids, even in narrow recesses having widths of, for example, 170 nm or less.

[0030] [6] The method for producing a nonlinear optical device according to any one of [1] to [5] above, The concentration of the first solute in the first liquid material may be, for example, 0% to 35% by mass, and the concentration of the second solute in the second liquid material may be, for example, 5% to 40% by mass.

[0031] For example, by setting the concentration of the first liquid material to 35% by mass or less, it is expected that the number of voids will be reduced. For example, by setting the concentration of the second liquid material to 40% by mass or less, the time required for diffusion of the solute may be shortened.

[0032] [7] The method for producing a nonlinear optical device according to any one of [1] to [6] above, The nonlinear optical polymer may be, for example, a polymer represented by the following formula (I): [ka] The present invention may include a structure represented by: In the above formula (I), R 1 and R 2each independently represents a hydrogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, an alkoxy group, a haloalkyl group, an aryl group, a hydroxy group, a thiol group, or an amino group.

[0033] The structure of the above formula (I) can be an electron-withdrawing group (acceptor). In the NLO polymer containing the structure of the above formula (I), a large NLO effect is expected.

[0034] [8] The method for producing a nonlinear optical device according to any one of [1] to [7] above, Each of the first solvent and the second solvent may contain at least one selected from the group consisting of, for example, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, acetylacetone, methyl amyl ketone, n-methyl ketone, γ-butyrolactone, tetrahydrofuran, chloroform, dibromomethane, 1,2-dichloroethane, 1,2-dibromoethane, 1,1,2-trichloroethane, 1,1,2,2-tetrachloroethane, 1,1,2-tribromoethane, 1,1,2,2-tetrabromoethane, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, butyl lactate, propylene glycol methyl ether, propylene glycol monomethyl ether acetate, and ethyl cellosolve acetate.

[0035] [9] The method for producing a nonlinear optical device according to any one of [1] to [8] above, The second solvent may be, for example, the same material as the first solvent. The second solute may be, for example, the same material as the first solute.

[0036] When the second solvent is the same material as the first solvent and the second solute is the same material as the first solute, for example, it is expected that the second liquid material and the first liquid material will be mixed uniformly.

[0037]

[10] The method for producing a nonlinear optical device according to the above [1], The first solute may include, for example, a nonlinear optical polymer. For example, at least a portion of the recess may be formed to extend linearly along a surface of the semiconductor substrate. A ratio of the depth of the recess to the width of the recess may be between 0.5 and 12. The recess may have a width of 170 nm or less. A concentration of the first solute in the first liquid material may be between 0% and 35% by weight. A concentration of the second solute in the second liquid material may be between 5% and 40% by weight.

[0038] <Details of the embodiment of the present disclosure> Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described in detail. However, the following description does not limit the scope of the claims.

[0039] Geometric terms in this embodiment (e.g., "parallel," "perpendicular," "straight line," etc.) indicate that the state may be substantially the same. The geometric terms in this embodiment should not be interpreted in a strict sense. For example, "parallel" indicates a state of being substantially parallel. In other words, "parallel" may deviate somewhat from the "parallel" state in the strict sense. "A state of being substantially parallel" may naturally include, for example, tolerances, errors, etc. in design, manufacturing, etc.

[0040] In this embodiment, unless otherwise specified, a description such as "0.5 to 12" indicates a range including a boundary value. For example, "0.5 to 12" indicates a range of "0.5 or more and 12 or less."

[0041] In the present embodiment, the "nonlinear optical device" refers to a product that includes at least a semiconductor substrate and a nonlinear optical polymer. For example, the nonlinear optical device may be composed of a semiconductor substrate and a nonlinear optical polymer. As long as it includes at least a semiconductor substrate and a nonlinear optical polymer, the nonlinear optical device may be any device. Examples of the nonlinear optical device include an optical modulator, an optical switch, an optical transceiver, an optical phased array, a LiDAR (Light Detection and Ranging), a terahertz wave generator, a terahertz wave detector ... It may be a T-wave detection device, a semiconductor substrate with a polymer film, or the like.

[0042] In this embodiment, a nonlinear optical device having an embedded portion is provided. The nonlinear optical device may have any structure as long as it has an embedded portion. The nonlinear optical device may have, for example, a slot waveguide structure, a photonic crystal structure, a metamaterial structure, a plasmon waveguide structure, or the like. Note that, as merely examples, a slot waveguide structure and a photonic crystal structure will be described later.

[0043] The "nonlinear optical polymer" in this embodiment is a polymer material that exhibits a nonlinear optical effect. The nonlinear optical effect may be, for example, an electro-optic effect, optical harmonic generation, optical Kerr effect, etc. That is, the "nonlinear optical polymer" in this embodiment includes an "electro-optic polymer." The "nonlinear optical device" in this embodiment includes an "electro-optic device."

[0044] In this embodiment, dimensions of 1 μm or less (e.g., the width of a recess) are measured in an electron microscope image. For one measurement object, electron microscope images are taken at three or more separate locations. In each electron microscope image, dimensions are measured at three or more locations. That is, dimensions are measured at nine or more locations. The arithmetic average value of the nine or more locations is regarded as the dimension of the measurement object. The electron microscope is arbitrarily selected depending on the measurement object. The electron microscope may be, for example, a transmission electron microscope (TEM) or the like, or a scanning electron microscope (SEM) or the like.

[0045] <Manufacturing method for nonlinear optical devices> 1 is a schematic flow chart of a method for manufacturing a nonlinear optical device according to the present embodiment. The method for manufacturing an NLO device according to the present embodiment includes "(a) forming a recess", "(b) filling a first liquid material", "(c) adding a second liquid material", and "(d) solidifying". The method for manufacturing an NLO device according to the present embodiment may further include "(e) poling" and the like.

[0046] (a) Formation of a recess 2 is a first schematic cross-sectional view showing a manufacturing process of the nonlinear optical device of this embodiment. The manufacturing method of the NLO device of this embodiment includes forming a recess 10 in a surface 101 of a semiconductor substrate 100.

[0047] (Semiconductor Substrate) The semiconductor substrate 100 may have any shape. The planar shape of the semiconductor substrate 100 may be, for example, circular or rectangular. The semiconductor substrate 100 may have a diameter of, for example, 25 mm to 300 mm. When the planar shape of the semiconductor substrate 100 is circular, the diameter of the semiconductor substrate 100 indicates the diameter of the circle. When the planar shape of the semiconductor substrate 100 is not circular, the diameter of the semiconductor substrate 100 indicates the distance between the two most distant points on the contour line of the semiconductor substrate 100.

[0048] The semiconductor substrate 100 may include any semiconductor material, such as silicon (Si), silicon carbide (SiC), indium phosphide (InP), gallium arsenide (GaAs), gallium nitride (GaN), diamond, silicon nitride (Si3N4), titanium oxide (TiO2), tantalum oxynitride (TaON), tantalum pentoxide (Ta2O5), and nitride oxynitride (VN). Niobium oxide (NbON), niobium pentoxide (Nb2O5), IZO (In2O3) x (ZnO) 1-x 〕, IGZO〔(In2O3) x (ZnO) y (Ga2O3) z , x+y+z=1], AZO〔( Al2O3) x (ZnO) 1-x 〕, and TTON〔(TiO2) x (TaON) 1-x 〕etc. In the above example, the stoichiometric composition formula is used as a representative example, but the material is not limited to a material strictly represented by a stoichiometric composition formula, and the semiconductor material represented by the stoichiometric composition formula is shown.

[0049] The semiconductor substrate 100 may have, for example, a single-layer structure. For example, the semiconductor substrate 100 may be composed of only a Si substrate 110. The semiconductor substrate 100 may have, for example, a multi-layer structure. The semiconductor substrate 100 may be, for example, a SOI (Silicon On Insulator) substrate. That is, the semiconductor substrate 100 may have, for example, a Si substrate 110, a BOX (Buried Oxide) layer 120, and a Si active layer 130. The Si active layer 130 may include a Si single crystal layer. The Si active layer may be doped with, for example, an impurity. The BOX layer 120 is interposed between the Si substrate 110 and the Si active layer 130. The BOX layer 120 includes silicon dioxide (SiO2). BO By forming an optical waveguide on the X layer 120, for example, a strong optical confinement effect is expected.

[0050] Each layer of the SOI substrate may have any thickness. The BOX layer 120 may have a thickness of, for example, 0.1 μm to 50 μm. The BOX layer 120 may have a thickness of, for example, 1 μm to 10 μm. The Si active layer 130 may have a thickness of, for example, 0.1 μm to 500 μm. The Si active layer 130 may have a thickness of, for example, 0.1 μm to 1 μm. The Si active layer 130 may have a thickness of, for example, 0.1 μm to 0.5 μm (100 nm to 500 nm). The Si substrate 110 may have a thickness of, for example, 100 μm to 1 mm.

[0051] (recess) The recess 10 may be formed by any method. For example, the recess 10 may be formed by patterning using lithography and reactive ion etching (RIE). For example, the periphery of the recess 10 may be scraped off so that the opening of the recess 10 is higher than the surrounding area.

[0052] The "recess 10" in this embodiment includes a sidewall 11 and a bottom 12. The sidewall 11 intersects with the surface 101 of the semiconductor substrate 100. The sidewall 11 may have a flat surface or a curved surface. For example, the sidewall 11 may be substantially perpendicular to the surface 101 of the semiconductor substrate 100. For example, the sidewall 11 may be inclined from the surface 101 of the semiconductor substrate 100.

[0053] In the cross section of FIG. 2, the bottom 12 connects a pair of opposing side walls 11. The bottom 12 may have, for example, a flat surface or a curved surface. In the cross section of FIG. 2, the bottom 12 may be, for example, a point. The bottom 12 may be, for example, parallel to the surface 101 of the semiconductor substrate 100. The bottom 12 may not be, for example, parallel to the surface 101 of the semiconductor substrate 100. The cross-sectional shape of the recess 10 may be, for example, rectangular, U-shaped, V-shaped, or the like. For example, as shown in FIG. 17, the width of the bottom 12 may be larger than the width of the opening.

[0054] When the semiconductor substrate 100 is an SOI substrate, the bottom portion 12 may be located, for example, in the Si active layer 130. The bottom portion 12 may be located, for example, in the BOX layer 120. The bottom portion 12 may be located, for example, in the Si substrate 110.

[0055] When the planar shape of the recess 10 is circular, the "width (w)" of the recess 10 indicates the diameter of the circle. When the planar shape of the recess 10 is not circular, the "width (w)" of the recess 10 indicates the minor axis of the planar shape of the recess 10. The "minor axis" in this embodiment is defined as follows. The straight line connecting the two most distant points on the contour line of the planar shape of the recess 10 is the major axis. The minor axis is the largest diameter among the diameters perpendicular to the major axis. Note that when the planar shape of the recess 10 extends linearly, the major axis may not be specified. In this case, in the top view of the recess (FIG. 3), the width in the direction perpendicular to the extension direction of the recess 10 is regarded as the width (w) of the recess 10.

[0056] The recess 10 may have any width (w). The recess 10 may have a width (w) of, for example, 170 nm or less. In the manufacturing method of the NLO device of this embodiment, even if the recess 10 is narrow, for example, having a width (w) of 170 nm or less, a reduction in voids is expected. The recess 10 may have a width (w) of, for example, 150 nm or less. The recess 10 may have a width (w) of, for example, 100 nm or less. The lower limit of the width (w) is arbitrary. The recess 10 may have a width (w) of, for example, 10 nm or more. The recess 10 may have a width (w) of, for example, 50 nm or more. The recess 10 may have a width (w) of, for example, 80 nm or more.

[0057] The "depth (d)" of the recess 10 indicates the shortest distance between the deepest point of the recess 10 and the opening of the recess 10 in a cross section (e.g., FIG. 2) perpendicular to the surface 101 of the semiconductor substrate 100. The recess 10 may have any depth (d). The recess 10 may have a depth (d) of, for example, 50 nm or more. The recess 10 may have a depth (d) of, for example, 100 nm or more. The recess 10 may have a depth (d) of, for example, 200 nm or more. The upper limit of the depth (d) is arbitrary. The recess 10 may have a depth (d) of, for example, 3 μm or less. The recess 10 may have a depth (d) of, for example, 2 μm or less. The recess 10 may have a depth (d) of, for example, 1 μm or less. The recess 10 may have a depth (d) of, for example, 300 nm or less.

[0058] The recess 10 may have any aspect ratio (d / w). The recess 10 may have an aspect ratio (d / w) of, for example, 0.5 to 12. With an aspect ratio (d / w) of 0.5 or more, for example, high integration is expected. The recess 10 may have an aspect ratio (d / w) of, for example, 1 or more. The recess 10 may have an aspect ratio (d / w) of, for example, 1.5 or more. With an aspect ratio (d / w) of 12 or less, for example, reduction of voids is expected. The recess 10 may have an aspect ratio (d / w) of, for example, 8 or less. The recess 10 may have an aspect ratio (d / w) of, for example, 4 or less. The recess 10 may have an aspect ratio (d / w) of, for example, 0.5 to 4.

[0059] The recess 10 may have any planar shape. The planar shape of the recess 10 may be, for example, a circle, a polygon, etc. The polygon may be, for example, a triangle, a rectangle, a pentagon, a hexagon, etc.

[0060] FIG. 3 is a schematic top view showing a first example of a recess. The recess 10 may be formed to extend linearly, for example. By filling the linearly extending recess with an NLO polymer, for example, a slot waveguide structure may be formed. The arrows in FIG. 3 indicate the direction of light propagation. The recess 10 may extend linearly, for example. The recess 10 may extend curvedly, for example. The recess 10 may extend in a broken line, for example. The recess 10 may branch into multiple parts, for example. For example, multiple recesses 10 may merge into one.

[0061] FIG. 4 is a schematic top view showing a second example of the recess. The recess 10 may form, for example, a photonic crystal structure. In the photonic crystal structure, the planar shape of the recess 10 may be, for example, a circle. For example, a plurality of recesses 10 are arranged in a triangular lattice on the surface 101 of the semiconductor substrate 100. For example, one row of the recesses 10 may be filled with an NLO polymer. The row filled with the NLO polymer may form a photonic crystal waveguide. The arrows in FIG. 4 indicate the propagation direction of light. Furthermore, a photonic crystal structure may be combined around a linearly extending slot structure. In this case, some of the recesses 10 out of the plurality of recesses 10 extend linearly along the surface of the semiconductor substrate 100. That is, at least a portion of the recess 10 may extend linearly along the surface of the semiconductor substrate 100.

[0062] 5 is a second schematic cross-sectional view showing a manufacturing process of the nonlinear optical device of this embodiment. In this embodiment, in addition to forming the recess 10, doping of impurities, formation of electrodes, etc. may be performed.

[0063] For example, a first doped region 131 and a second doped region 132 may be formed in a Si active layer 130. Each doped region may be formed by any method. For example, ion implantation or the like may be performed. Each of the first doped region 131 and the second doped region 132 may have, for example, an n-type conductivity. Each of the first doped region 131 and the second doped region 132 may be doped with an impurity such as phosphorus (P).

[0064] The first doped region 131 includes the sidewall 11 of the recess 10. The first doped region 131 may have a relatively low doping concentration. For example, it is expected that the first doped region 131 has a low doping concentration to reduce propagation loss.

[0065] The second doped region 132 is in contact with the electrode 200. The second doped region 132 may have a relatively high doping concentration. For example, it is expected that the contact resistance with the electrode 200 is reduced by the second doped region 132 having a high doping concentration.

[0066] The doping concentration in the first doping region 131 may be lower than the doping concentration in the second doping region 132. The doping concentration in the first doping region 131 may be lower than the doping concentration in the second doping region 132. 16 cm -3 From 1×10 17 cm -3 The doping concentration in the second doped region 132 may be, for example, 1×10 17 cm -3 From 1×10 18 cm -3 may be also possible.

[0067] In the present embodiment, the doping of the impurity may be performed at any timing. For example, the doping of the impurity may be performed before the formation of the recess 10. For example, the doping of the impurity may be performed after the formation of the recess 10.

[0068] The electrode 200 may include at least one selected from the group consisting of, for example, aluminum (Al), tungsten (W), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), chromium (Cr), molybdenum (Mo), tantalum (Ta), niobium (Nb), nickel (Ni), cobalt (Co), gold (Au), silver (Ag), copper (Cu), and platinum (Pt). The electrode 200 may be formed by any method. For example, the electrode 200 may be formed by a deposition method or the like. The electrode 200 may be, for example, a signal electrode or the like. The electrode 200 may be, for example, a ground electrode or the like.

[0069] In this embodiment, the electrode 200 may be formed at any timing. For example, the electrode 200 may be formed before the application of the polymer solution. For example, the electrode 200 may be formed after the polymer film 300 is formed.

[0070] (b) Filling with first liquid material 6 is a third schematic cross-sectional view showing a manufacturing process of the nonlinear optical device of this embodiment. The manufacturing method of the NLO device of this embodiment includes filling the recess 10 with a first liquid material 31 in a reduced pressure environment.

[0071] The first liquid material 31 is filled into the recess 10 by any method. For example, the first liquid material 31 may be applied to the surface 101 of the semiconductor substrate 100 by a spin coating method or the like. For example, a spin coater or the like capable of controlling the atmospheric pressure may be used.

[0072] In this embodiment, the "reduced pressure atmosphere" refers to an atmosphere having a pressure less than atmospheric pressure. It is believed that degassing is promoted under a reduced pressure atmosphere. The first liquid material 31 is a low concentration solution or a solvent itself. It is believed that solidification of the material is unlikely to occur on the surface of the first liquid material 31. The reduced pressure atmosphere may have a pressure of, for example, 0.1 Pa to 90 kPa. The reduced pressure atmosphere may have a pressure of, for example, 100 Pa to 80 kPa. The reduced pressure atmosphere may have a pressure of, for example, 3 kPa to 70 kPa.

[0073] The first liquid material 31 includes a first solute and a first solvent, or the first liquid material 31 consists only of the first solvent. The first solute is dissolved in the first solvent. The concentration of the first solute in the first liquid material 31 may be, for example, 0% to 35% by mass. The concentration of the first solute in the first liquid material 31 may be, for example, 0% to 20% by mass. The concentration of the first solute in the first liquid material 31 may be, for example, 0% to 10% by mass.

[0074] The first liquid material 31 may have a low viscosity. The first liquid material may have a viscosity of, for example, 1 mPa·s to 2000 mPa·s. The first liquid material may have a viscosity of, for example, 1 mPa·s to 1000 mPa·s. The first liquid material may have a viscosity of, for example, 1 mPa·s to 10 mPa·s. The "viscosity" of the liquid in this embodiment is measured using a micro-sample viscometer (product name "micro V") manufactured by RheoSense. The viscosity can be measured by a viscometer equivalent to the above viscometer. The measurement temperature is 25°C ± 1°C. For one object to be measured, the viscosity is measured three or more times. The arithmetic mean value of the three or more results is regarded as the viscosity of the object to be measured.

[0075] (solvent) The first solvent may contain any component. The first solvent may contain at least one selected from the group consisting of, for example, acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, acetylacetone, methyl amyl ketone, n-methyl ketone, γ-butyrolactone, tetrahydrofuran, chloroform, dibromomethane, 1,2-dichloroethane, 1,2-dibromoethane, 1,1,2-trichloroethane, 1,1,2,2-tetrachloroethane, 1,1,2-tribromoethane, 1,1,2,2-tetrabromoethane, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, butyl lactate, propylene glycol methyl ether, propylene glycol monomethyl ether acetate, and ethyl cellosolve acetate.

[0076] (solute) The first solute may include any component. The first solute may be substantially composed of only one component, or may be composed of multiple components. The first solute may include, for example, a low molecular weight compound, an oligomer, a polymer, etc.

[0077] The first solute may include, for example, a surfactant. The surfactant may function, for example, as an evaporation inhibitor of the solvent. When the surfactant functions as an evaporation inhibitor, evaporation of the solvent may be reduced, for example, on the surfaces of the first liquid material 31 and the third liquid material 33 (described later). As a result, for example, the surface roughness of the polymer film 300 (described later) is expected to be reduced. The surfactant may include, for example, a fluorine-based surfactant (for example, a product name "Megafac" manufactured by DIC Corporation, etc.).

[0078] The first solute may include, for example, NLO dye molecules. NLO dye molecules refer to molecules having NLO activity. The NLO dye molecules may include, for example, electro-optic (EO) dye molecules, which will be described later. By including NLO dye molecules in the first solute, it is expected that the orientation of the NLO dye molecules will be improved, for example, during a poling process.

[0079] The first solute may include, for example, an NLO polymer. The first solute may consist essentially of an NLO polymer. An NLO polymer is a polymer material that exhibits a nonlinear optical effect. The NLO polymer may include, for example, an EO polymer, etc. The NLO polymer may consist essentially of an EO polymer, for example.

[0080] (EO polymer) The EO polymer exhibits an electro-optic effect. The EO polymer may include any component as long as it exhibits the electro-optic effect. The EO polymer may include, for example, a guest / host polymer. The guest / host polymer includes a guest molecule and a host polymer. The guest molecule is dispersed in the host polymer. The concentration of the guest molecule in the guest / host polymer may be, for example, 10% to 50% by weight. The host polymer may include, for example, polymethyl methacrylate (PMMA), polycarbonate (PC), etc.

[0081] The guest molecule exhibits an electro-optic effect. The guest molecule is also referred to as an "EO dye molecule." The guest molecule may include, for example, an electron-donating group (donor), a linking group, and an electron-withdrawing group (acceptor). The linking group links the donor and the acceptor. The linking group may include, for example, a π-conjugated structure. The linking group may be, for example, any of the following formulae (II) to (IV): [ka] The present invention may include a structure represented by:

[0082] The donor may be, for example, a compound represented by the following formula (V): [ka] The present invention may include a structure represented by: In the above formula (V), R 3 and R 4 each independently represents a hydrogen atom, an alkyl group, a hydroxyalkyl group, a haloalkyl group, an aryl group, or the like.

[0083] The acceptor may be, for example, a compound represented by the following formula (I): [ka] That is, the NLO polymer may include a structure represented by formula (I) above.

[0084] In the above formula (I), R 1 and R 2 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, an alkoxy group, a haloalkyl group, an aryl group, a hydroxy group, a thiol group, or an amino group.

[0085] EO polymers containing the acceptor of formula (I) above can exhibit a large electro-optic effect. The alkyl group may be, for example, a methyl group. The haloalkyl group may be, for example, a trifluoromethyl group. R 1 , R 2 When is an aryl group, the aryl group may be substituted. The aryl group may be, for example, a phenyl group, a naphthyl group, etc. The hydrogen atom of the aryl group may be substituted, for example, by a halogen atom, an alkyl group, a haloalkyl group, etc.

[0086] In the above formula (I), for example, R 1 and R 2 may each independently represent a hydrogen atom, a methyl group, a trifluoromethyl group, or a phenyl group.

[0087] For example, an EO polymer may be formed by binding an EO dye molecule as a side chain to a linear polymer. The EO dye molecule may be bound to the linear polymer (main chain) by, for example, a reaction of a reactive group (e.g., a hydroxyl group, etc.) contained in a donor. The linear polymer may be a homopolymer or a copolymer. The copolymer may be, for example, any of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer. In this embodiment, an EO polymer in which an EO dye molecule is bound to a linear copolymer as a side chain is also referred to as a "side chain copolymer."

[0088] Figure 18 shows an example of a synthesis scheme for a side chain copolymer. First, a linear copolymer is synthesized by copolymerization of dicyclopentanyl methacrylate (DCPMA) and 2-methacryloyloxyethyl isocyanate (MOI). The EO dye molecule has one hydroxyl group. The EO dye molecule is introduced as a side chain of the linear copolymer.

[0089] For example, multiple polymer chains may be cross-linked by an EO dye molecule. For example, if an EO dye molecule has two reactive groups, the EO dye molecule may cross-link two polymer chains. In this embodiment, an EO polymer cross-linked by an EO dye molecule is also referred to as a "cross-linked copolymer."

[0090] In guest / host polymers, it is believed that the guest molecules (EO dye molecules) tend to aggregate when the concentration of guest molecules is high. In side chain copolymers and cross-linked copolymers, it is believed that it is easier to increase the concentration of EO dye molecules because EO dye molecules are less likely to aggregate.

[0091] (c) Addition of a second liquid material Fig. 7 is a fourth schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. Fig. 8 is a fifth schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. The manufacturing method of the NLO device of this embodiment includes preparing a third liquid material 33 by contacting a second liquid material 32 with a first liquid material 31 filled in the recess 10.

[0092] The second liquid material 32 comes into contact with the first liquid material 31 by any method. For example, the second liquid material 32 may be dropped onto the liquid surface of the first liquid material 31. For example, the second liquid material 32 may be applied onto the liquid surface of the first liquid material 31. For example, the second liquid material 32 may be sprayed onto the liquid surface of the first liquid material 31.

[0093] The second liquid material 32 includes a second solute and a second solvent. The second solute is dissolved in the second solvent. The second solute includes an NLO polymer. The second solute may, for example, consist essentially of an NLO polymer. The second solute may further include other components as long as it includes an NLO polymer. The second solute may further include, for example, the above-mentioned surfactant, etc.

[0094] For example, when the first solute does not include an NLO polymer, the second solute and the first solute are different materials, and when the first solute includes an NLO polymer, the second solute and the first solute may be different materials or may be the same material.

[0095] The second solvent may, for example, include the material described as the first solvent. The second solvent may, for example, be a different material from the first solvent. The second solvent may, for example, be the same material as the first solvent. By the second solute being the same material as the first solute and the second solvent being the same material as the first solvent, for example, it is expected that the second liquid material 32 and the first liquid material 31 will be mixed uniformly.

[0096] The second liquid material 32 is a high-concentration solution. The concentration of the second solute in the second liquid material 32 is higher than the concentration of the first solute in the first liquid material 31. The concentration of the second liquid material 32 may be, for example, 5% to 40% by mass. The concentration of the second liquid material 32 may be, for example, 10% to 30% by mass. The concentration of the second liquid material 32 may be, for example, 10% to 20% by mass.

[0097] The difference between the concentration of the second liquid material 32 and the concentration of the first liquid material 31 may be, for example, more than 0 mass % and not more than 40 mass %. The difference between the concentration of the second liquid material 32 and the concentration of the first liquid material 31 may be, for example, 5 mass % to 40 mass %. The difference between the concentration of the second liquid material 32 and the concentration of the first liquid material 31 may be, for example, 10 mass % to 20 mass %.

[0098] The second liquid material 32 may have a higher viscosity than the first liquid material 31. The second liquid material 32 may have a viscosity of, for example, 2 mPa·s to 2500 mPa·s. The second liquid material 32 may have a viscosity of, for example, 5 mPa·s to 2500 mPa·s. The second liquid material 32 may have a viscosity of, for example, 10 mPa·s to 2500 mPa·s. The second liquid material 32 may have a viscosity of, for example, 100 mPa·s to 2500 mPa·s. The second liquid material 32 may have a viscosity of, for example, 1000 mPa·s to 2500 mPa·s.

[0099] The third liquid material 33 is prepared by diffusing the solute from the second liquid material 32 into the first liquid material 31. To promote the diffusion of the solute, the liquid material may be heated. However, the heating temperature is adjusted so that the solute does not aggregate. For example, the solute may be diffused in a temperature environment of 20°C to 80°C. For example, the solute may be diffused in a temperature environment of 30°C to 60°C.

[0100] The diffusion of the solute may be carried out, for example, under normal pressure or under pressurized pressure.

[0101] The third liquid material may be prepared to have a substantially uniform concentration. The concentration of the solute in the third liquid material 33 may be, for example, 5% to 40% by mass. The concentration of the solute in the third liquid material 33 may be, for example, 5% to 20% by mass. The concentration of the solute in the third liquid material 33 may be, for example, 5% to 10% by mass.

[0102] (d) Solidification 9 is a sixth schematic cross-sectional view showing the manufacturing process of the nonlinear optical device of this embodiment. The manufacturing method of the NLO device of this embodiment includes forming the embedded portion 310 by solidifying the third liquid material 33. The formation of the embedded portion 310 completes the NLO device 1000.

[0103] The third liquid material 33 solidifies to form a polymer film 300. The first solvent and the second solvent can be removed from the third liquid material 33 by any method. For example, at least one method selected from the group consisting of natural drying, reduced pressure drying, spin drying, hot air drying, and infrared drying may be performed.

[0104] The polymer film 300 includes a buried portion 310. The buried portion 310 is buried in the recess 10. A part or the whole of the buried portion 310 may form, for example, an optical waveguide. The buried portion 310 of this embodiment may have a low porosity. Therefore, it is expected that the propagation loss in the optical waveguide is small.

[0105] The polymer film 300 (embedded portion 310) of this embodiment may have a smooth surface. The polymer film 300 may have, for example, a small surface roughness. The polymer film 300 may have, for example, a predetermined surface smoothness. The polymer film 300 having a smooth surface may provide a miniaturizable NLO device.

[0106] (e) Polling The method for manufacturing the NLO device of this embodiment may further include, for example, subjecting the embedded portion 310 to a poling process.

[0107] For example, if the implant portion 310 includes an EO polymer, the glass transition temperature (T g The buried portion 310 is heated until the buried portion 310 reaches the vicinity of the electrode 200. A constant voltage is applied. This places the embedded portion 310 in an electric field. The EO dye molecules are oriented along the direction of the electric field. With the voltage applied, the EO polymer is cooled to room temperature. This allows the EO dye molecules to be fixed in an oriented state. EXAMPLES

[0108] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described. However, the following description does not limit the scope of the claims.

[0109] <Manufacture of nonlinear optical devices> An evaluation device (NLO device) is manufactured by the following manufacturing methods No. 1 to No. 3. The evaluation device in this example is a slot waveguide type optical modulator.

[0110] <No.1> (a) Formation of a recess An SOI substrate is prepared as the semiconductor substrate 100. A recess 10 is formed by photolithographic patterning and RIE. The recess 10 in this embodiment is a linearly extending slot. The width (w) of the recess 10 is 134 nm. The depth (d) of the recess 10 is 302 nm. The bottom 12 of the recess 10 is located within the BOX layer 120.

[0111] (b) Filling with first liquid material In this embodiment, the first liquid material 31 is composed of only the first solvent. The first solvent is cyclohexanone. The concentration of the first solute in the first liquid material 31 is 0 mass %.

[0112] The first liquid material 31 is dropped onto the surface of the semiconductor substrate 100. After dropping, the first liquid material 31 is left to stand for 10 minutes in a reduced pressure atmosphere, thereby allowing the first liquid material 31 to be sufficiently degassed. This allows the first liquid material 31 to fill the recesses 10. After filling, the semiconductor substrate 100 is rotated at 500 rpm for 3 seconds by a spin coater. This allows excess first liquid material 31 to be removed.

[0113] (c) Addition of a second liquid material An EO polymer is prepared as a second solute. The EO polymer is a cross-linked copolymer. Cyclohexanone is prepared as a second solvent. The second solute is dissolved in the second solvent to prepare a second liquid material 32. The concentration of the second solvent in the second liquid material 32 is 16% by mass. The concentration of the second solute in the second liquid material 32 (16% by mass) is higher than the concentration of the first solute in the first liquid material 31 (0% by mass).

[0114] The second liquid material 32 is dropped onto the first liquid material 31. That is, the second liquid material 32 comes into contact with the first liquid material 31. In a room temperature environment, the second solute (EO polymer) diffuses to prepare a third liquid material 33. The third liquid material 33 is prepared to have a substantially uniform concentration.

[0115] (d) Solidification After the second liquid material 32 is dropped, the semiconductor substrate 100 is spun at 1500 rpm for 60 seconds by a spin coater. This causes the third liquid material 33 to spread almost uniformly over the surface of the semiconductor substrate 100, while the first and second solvents evaporate. As a result, the second solute precipitates in the recess 10. That is, the third liquid material 33 solidifies. This forms a polymer film 300. The portion of the polymer film 300 that has entered the recess 10 forms a buried portion 310. The polymer film 300 is then heated to a glass transition temperature (T g ) and heat-treated for 1 hour in a reduced pressure atmosphere to remove the remaining first The solvent and the second solvent are removed.

[0116] (e) Polling The embedded portion 310 is heated to a temperature above the glass transition temperature (T g ) Heating In this state, the buried portion 310 is placed in an electric field. Thereafter, while the electric field is maintained, the temperature of the buried portion 310 is lowered. In this manner, the evaluation device is manufactured.

[0117] <No.2> 10 is a first schematic cross-sectional view showing the manufacturing process of No. 2. As in No. 1, a semiconductor substrate 100 having a recess 10 is prepared. A polymer solution 35 is prepared. The solvent of the polymer solution 35 is cyclohexanone. The solute is the same EO polymer as in No. 1. The concentration of the polymer solution 35 is 16% by mass.

[0118] A spin coater is used to apply the polymer solution 35 to the surface of the semiconductor substrate 100 under normal pressure. This causes the polymer solution 35 to fill the recesses 10. It is believed that air bubbles 1 are difficult to escape from the recesses 10 due to the normal pressure atmosphere.

[0119] 11 is a second schematic cross-sectional view showing the manufacturing process of No. 2. The polymer solution 35 is solidified to form a polymer film 300. It is believed that voids 2 remain in the embedded portion 310. After the formation of the polymer film 300, a poling treatment is carried out in the same manner as in No. 1.

[0120] <No.3> 12 is a schematic cross-sectional view showing the manufacturing process of No.3. Polymer solution 35 is applied and filled in a reduced pressure environment. It is believed that the reduced pressure degassing reduces the number of bubbles 1 compared to No.2. However, it is believed that as the surface of polymer solution 35 solidifies, irregularities are formed on the surface of polymer film 300. After the polymer film 300 is formed, a poling treatment is performed in the same manner as No.1.

[0121] <Evaluation> A first near-infrared camera is disposed above the semiconductor substrate 100. An image of light propagating streaks caused by scattering of light propagating through the buried portion 310 is captured by the first near-infrared camera.

[0122] An example of measuring the propagation loss will be described with reference to Fig. 13 to Fig. 15. Fig. 13 is a schematic top view of an evaluation device. The evaluation device 2000 is symmetrical. The evaluation device 2000 is configured by connecting a first polymer waveguide 2001, a first spot size converter 2002, a first Si strip waveguide 2003, a second spot size converter 2004, a Si slot waveguide 2005, a third spot size converter 2006, a second Si strip waveguide 2007, a fourth spot size converter 2008, and a second polymer waveguide 2009 in this order. The length of the Si slot waveguide 2005 is 1736 µm.

[0123] The light propagation streak image No. 2 is shown in Fig. 14. The light propagation streak image in Fig. 14 is photographed in the Si slot waveguide 2005 in Fig. 13. As shown in Fig. 15, the scattered light intensity (relative value) of the light propagation streak image is plotted against the position (Z) in the Si slot waveguide 2005. The group of plots is approximated to an exponential function by the least squares method to obtain the propagation loss.

[0124] A second near-infrared camera is disposed in the direction of the end face of the semiconductor substrate 100. An optical output near-field image is captured by the second near-infrared camera. The optical output (relative value) is calculated from the optical attenuator value that results in an optical intensity equivalent to that of the optical output near-field image.

[0125] The evaluation device 2000 is broken so as to cross the Si slot waveguide 2005. The fracture surface is observed by SEM to confirm the presence or absence of voids in the embedded portion 310. The presence or absence of voids is confirmed in each of five or more fracture surfaces. The void ratio is calculated by the following formula.

[0126] Porosity (%) = {(number of fracture surfaces with voids) / (number of fracture surfaces observed)} × 100

[0127] <Result> FIG. 16 shows the evaluation results for No. 1 to No. 3. In the cross-sectional SEM image, voids are confirmed. The voids are areas where the bottom 12 of the recess 10 is not filled with the polymer.

[0128] In the cross-sectional SEM image of No. 2, voids are confirmed in many cases. The porosity of No. 2 is 71%. It is considered that a large number of voids remain in the buried portion 310. The propagation loss is the largest and the optical output is the lowest.

[0129] In the cross-sectional SEM image of No.3, the number of voids has been reduced compared to No.2. The porosity of No.3 is 9%. It is believed that the voids have been reduced by decompression and degassing. However, since the voids can be confirmed, albeit few in number, it is believed that a small amount of voids remain. No.3 has a reduced propagation loss and an increased optical output compared to No.2. Furthermore, in No.3, as a result of the surface solidification of the polymer solution 35, irregularities are formed on the surface of the polymer film 300 (embedded portion 310).

[0130] No voids can be confirmed in the cross-sectional SEM image of No.1. The porosity of No.1 is 0%. The propagation loss of No.1 is smaller than that of No.2 and No.3. The optical output of No.1 is higher than that of No.2 and No.3. It is believed that the first liquid material 31 easily penetrates into the recesses 10, which significantly reduces the voids. It is also believed that the voids are substantially completely removed in No.1. The surface of the polymer film 300 in No.1 may be smooth. This is believed to be because surface solidification is unlikely to occur in the first liquid material 31.

[0131] <Additional Notes> In the present disclosure, NLO devices as set forth in the following appendix 1 to appendix 3 may also be provided.

[0132] Appendix 1 A semiconductor substrate; A polymer membrane; Including, A recess is formed on a surface of the semiconductor substrate, the recess extends along the surface of the semiconductor substrate; the polymer film covering at least a portion of the surface of the semiconductor substrate; the polymer film includes a recessed portion; The embedded portion is embedded in the recess, the embedding portion includes a nonlinear optical polymer; The propagation loss in the embedded portion is equal to or less than a predetermined value. Nonlinear optical devices.

[0133] Appendix 2 The porosity in the embedded portion is equal to or less than a predetermined value. A nonlinear optical device according to claim 1.

[0134] Appendix 3 The surface roughness of the polymer film is equal to or less than a predetermined value. A nonlinear optical device according to claim 1 or 2.

[0135] The present embodiment and the present example are illustrative in all respects. The present embodiment and the present example are not limiting. For example, it is originally intended that any configurations may be extracted from the present embodiment and the present example, and that they may be arbitrarily combined.

[0136] The technical scope defined based on the description of the claims encompasses all modifications within the meaning equivalent to the description of the claims. Furthermore, the technical scope defined based on the description of the claims encompasses all modifications within the scope equivalent to the description of the claims. [Explanation of symbols]

[0137] 1 bubble, 2 void, 10 recess, 11 side wall, 12 bottom, 31 first liquid material, 32 second liquid material, 33 third liquid material, 35 polymer solution, 100 semiconductor substrate, 101 surface, 110 Si substrate, 120 BOX layer, 130 Si active layer, 131 first doping region, 132 second doping region, 200 electrode, 300 polymer film, 310 buried portion, 1000 nonlinear optical device, 2000 evaluation device, 2001 first polymer waveguide, 2002 first spot size converter, 2003 first Si strip waveguide, 2004 second spot size converter, 2005 Si slot waveguide, 2006 third spot size converter, 2007 second Si strip waveguide, 2008 fourth spot size converter, 2009 second polymer waveguide.

Claims

1. forming a recess in a surface of a semiconductor substrate; filling the recess with a first liquid material under a reduced pressure environment; preparing a third liquid material by contacting a second liquid material with the first liquid material filled in the recess; and, forming a filling portion by solidifying the third liquid material; Including, the first liquid material contains a first solute and a first solvent, or consists of the first solvent alone; the second liquid material includes a second solute and a second solvent; the second solute comprises a nonlinear optical polymer; A concentration of the second solute in the second liquid material is higher than a concentration of the first solute in the first liquid material. A method for fabricating a nonlinear optical device.

2. the first solute comprises a nonlinear optical polymer; A method for manufacturing the nonlinear optical device according to claim 1 .

3. At least a portion of the recess is formed to extend linearly along the surface of the semiconductor substrate.

3. A method for producing the nonlinear optical device according to claim 1 or 2.

4. the ratio of the depth of the recess to the width of the recess is from 0.5 to 12; A method for manufacturing the nonlinear optical device according to any one of claims 1 to 3.

5. The recess has a width of 170 nm or less. A method for manufacturing the nonlinear optical device according to any one of claims 1 to 4.

6. a concentration of the first solute in the first liquid material is from 0% by mass to 35% by mass; The concentration of the second solute in the second liquid material is 5% by mass to 40% by mass. A method for manufacturing the nonlinear optical device according to any one of claims 1 to 5.

7. The nonlinear optical polymer has the following formula (I): 【Chemistry 1】 The structure includes: In the above formula (I), R 1 and R 2 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, an alkoxy group, a haloalkyl group, an aryl group, a hydroxyl group, a thiol group, or an amino group; A method for manufacturing the nonlinear optical device according to any one of claims 1 to 6.

8. Each of the first solvent and the second solvent includes at least one selected from the group consisting of acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, acetylacetone, methyl amyl ketone, n-methyl ketone, γ-butyrolactone, tetrahydrofuran, chloroform, dibromomethane, 1,2-dichloroethane, 1,2-dibromoethane, 1,1,2-trichloroethane, 1,1,2,2-tetrachloroethane, 1,1,2-tribromoethane, 1,1,2,2-tetrabromoethane, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, butyl lactate, propylene glycol methyl ether, propylene glycol monomethyl ether acetate, and ethyl cellosolve acetate; A method for manufacturing the nonlinear optical device according to any one of claims 1 to 7.

9. The second solvent is the same material as the first solvent, The second solute is the same material as the first solute. A method for manufacturing the nonlinear optical device according to any one of claims 1 to 8.

10. the first solute comprises a nonlinear optical polymer; At least a portion of the recess is formed to extend linearly along the surface of the semiconductor substrate, The first liquid material is filled into the recess under a reduced pressure atmosphere; a ratio of the depth of the recess to the width of the recess is between 0.5 and 12; The recess has a width of 170 nm or less, a concentration of the first solute in the first liquid material is from 0% by mass to 35% by mass; The concentration of the second solute in the second liquid material is 5% by mass to 40% by mass. A method for manufacturing the nonlinear optical device according to claim 1 .

Citation Information

Patent Citations

  • Optical function element and method of manufacturing the same

    JP2003295143A

  • Method for manufacturing fine pattern and transfer material

    JP2004071934A

  • Imprint method and device

    JP2004103817A

  • Optical element and method for manufacturing same

    JP2007108515A

  • Single phase fluid imprint lithography method

    JP2007509769A