Phosphor powder, light-emitting device, image display device and lighting device
A phosphor powder with a specific composition and manufacturing process enhances blue light conversion efficiency and internal quantum efficiency, addressing the limitations of existing phosphors in light emitting devices.
Patent Information
- Application Number
- JP2022561858
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-13
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-04
AI Technical Summary
The phosphors described in existing technologies have room for improvement in terms of blue light conversion efficiency, specifically in increasing internal quantum efficiency.
A phosphor powder with a specific general formula M x (Si,Al) 2 (N,O) 3±y, where M is Li and one or more alkaline earth metal elements, and a part of M is replaced with Ce, with a Si/Al ratio of 1.5 to 6, an O/N atomic ratio of 0 to 0.1, and Li and Ce content of 5 to 50 mol% and 0.5 to 10 mol%, respectively, achieving a diffuse reflectance of 88% to 99.9% for light at 700 nm.
The phosphor powder exhibits high internal quantum efficiency and improved blue light conversion efficiency, maintaining excellent heat resistance and chemical stability, suitable for various light emitting devices.
Smart Images

Figure 0007590449000002 
Figure 0007590449000003 
Figure 0007590449000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphor powder, a light emitting device, an image display device, and an illumination device. [Background technology]
[0002] In order to manufacture a white LED (Light Emitting Diode), a phosphor is usually used as a wavelength conversion material to obtain white light from the blue light emitted from a blue LED. With the widespread use of white LEDs for lighting applications and the consideration of applying white LEDs to image display devices, development of phosphors capable of converting blue light into light with longer wavelengths is ongoing.
[0003] One aspect of improving phosphors is to modify the chemical composition of the phosphor. For example, Patent Document 1 discloses a compound of the general formula M x (Si,Al) 2 (N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.23), in which part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, and 5 to 50 mol % of M is Li and 0.5 to 10 mol % of M is Ce. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5969391 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have found that the phosphor described in Patent Document 1 has room for improvement in terms of blue light conversion efficiency, specifically, in terms of increasing the internal quantum efficiency.
[0006] The present inventors have carried out investigations with the aim of providing a phosphor powder having high internal quantum efficiency and improved blue light conversion efficiency. [Means for solving the problem]
[0007] As a result of their investigations, the inventors have completed the invention provided below.
[0008] According to the present invention, General formula M x (Si,Al) 2 (N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, Phosphor powder with a diffuse reflectance X1 of 88% or more and 99.9% or less for light with a wavelength of 700 nm is provided.
[0009] Further, according to the present invention, A light emitting device comprising the above phosphor powder and a light source. is provided.
[0010] Further, according to the present invention, An image display device including the light emitting device is provided.
[0011] Further, according to the present invention, A lighting device including the light-emitting device described above is provided. Effect of the Invention
[0012] The phosphor powder of the present invention has high internal quantum efficiency and good blue light conversion efficiency. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view showing an example of the structure of a light-emitting device. [Diagram 2] 1 shows an XRD pattern obtained by measuring the phosphor of Example 1 by powder X-ray diffraction (XRD). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar symbols and descriptions thereof will be omitted as appropriate. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.
[0015] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass."
[0016] <Phosphor powder> The phosphor powder of this embodiment is represented by the general formula M x (Si,Al) 2 (N,O) 3±y In this general formula, M is Li and one or more alkaline earth metal elements, and 0.52≦x≦0.9 and 0.06≦y≦0.36. Also, a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce. Moreover, the diffuse reflectance X1 of the phosphor powder of this embodiment for light with a wavelength of 700 nm is not less than 88% and not more than 99.9%.
[0017] The phosphor powder of this embodiment differs from the phosphor described in Patent Document 1 at least in that X1 is 88% or more and 99.9% or less. Compared to the phosphor described in Patent Document 1, the phosphor powder of this embodiment efficiently converts blue light into light with a long wavelength in terms of, for example, internal quantum efficiency.
[0018] The absorption of phosphors can be classified into two types: light absorption accompanying electronic transition of the luminescent center ion, and light absorption unrelated to the fluorescent emission caused by impurities, crystal defects of the host material, etc. When a phosphor that emits visible light is irradiated with light in the near infrared range, for example, light with a wavelength of 700 nm, the light absorption is unrelated to the fluorescent emission and is an indicator of a decrease in the fluorescent properties. In order to quantitatively evaluate the above-mentioned effect of light absorption, the present inventors have x (Si,Al) 2 (N,O) 3±y The inventors newly produced various phosphors represented by the general formula M x (Si,Al) 2 (N,O) 3±y and X1 is 88% or more and 99.9% or less. The inventors have succeeded in increasing the internal quantum efficiency of the phosphor powder.
[0019] The phosphor powder of this embodiment can be manufactured by using appropriate materials and by selecting appropriate manufacturing methods and conditions. Examples of "appropriate manufacturing methods and conditions" include one or more of the following: (i) acid-treating the phosphor powder under specific conditions, (ii) subjecting the phosphor powder to an appropriate classification process (e.g., sedimentation classification), and (iii) devising a method for pulverizing the phosphor powder. Details of the manufacturing methods and conditions will be described later.
[0020] The phosphor powder of this embodiment will be described further.
[0021] (Crystal structure, chemical composition, etc.) The phosphor crystal has a skeletal structure of (Si,Al)-(N,O) 4 It is composed of regular tetrahedrons bonded together, with the M element located in the gap between them. The composition of the above general formula can be established in a wide range in which electrical neutrality is maintained depending on the overall parameters of the valence and amount of the M element, the Si / Al ratio, and the N / O ratio. A representative phosphor represented by the above general formula is CaAlSiN, where the M element is Ca and x=1, Si / Al=1, and O / N=0. 3 There is CaAlSiN 3 When part of the Ca is replaced by Eu, a red phosphor is obtained, and when part of the Ca is replaced by Ce, a yellow to orange phosphor is obtained.
[0022] The crystal structure of the phosphor particles contained in the phosphor powder of this embodiment is usually CaAlSiN 3 One of the features of these phosphor particles is that the constituent elements and composition have been significantly changed to obtain extremely high luminous efficiency even when activated with Ce. In the above general formula, the M element is a combination of Li and an alkaline earth metal element, and a part of it is replaced with Ce, which serves as the luminescence center. By using Li, the average valence of the M element can be widely controlled by combining it with a divalent alkaline earth element and a trivalent Ce element. + The ionic radius of is very small, and the crystal size can be changed significantly depending on the amount of isotopic fraction, resulting in a wide variety of fluorescent emissions. The coefficient x of the M element in the above general formula is 0.52 or more and 0.9 or less, preferably 0.6 or more and 0.9 or less, and more preferably 0.7 or more and 0.9 or less. 3 The fluorescence intensity tends to decrease as one approaches the crystal, and when the coefficient x is smaller than 0.52, a large amount of a different phase other than the target crystal phase is generated, so that the fluorescence intensity tends to decrease significantly.
[0023] In this embodiment, electrical neutrality is maintained by the average valence and amount of M element, the Si / Al ratio, and the O / N ratio, and in the case of a single crystal without defects, y=0. However, when considering the composition of the phosphor as a whole, a second crystal phase or an amorphous phase may exist, and when considering the crystal itself, the charge balance may be lost due to crystal defects. In this embodiment, from the viewpoint of increasing the fluorescence intensity, y is preferably 0.06 to 0.36, more preferably 0.1 to 0.35, and even more preferably 0.06 to 0.23.
[0024] In this embodiment, the O / N atomic ratio (molar ratio) is 0 to 0.1, preferably 0.01 to 0.08, and more preferably 0.02 to 0.07. If the O / N atomic ratio is too large, the amount of heterophase generated increases, the luminous efficiency decreases, and the covalent bond of the crystal decreases, which tends to cause deterioration of temperature characteristics (reduction in luminance at high temperatures).
[0025] The Si / Al atomic ratio (molar ratio) is usually determined by the average valence or amount of the M element and the O / N atomic ratio being within a predetermined range. The Si / Al atomic ratio is 1.5 or more and 6 or less, preferably 2 or more and 4 or less, and more preferably 2.5 or more and 4 or less.
[0026] The Li content in the phosphor particles is 5 to 50 mol %, preferably 15 to 45 mol %, and more preferably 25 to 45 mol % of the element M. The effect of Li is easily exhibited at 5 mol % or more, but if it exceeds 50 mol %, the intended crystal structure of the phosphor cannot be maintained and a different phase is generated, which tends to reduce the luminous efficiency. Just to be clear, the "Li content" refers to the Li content in the final phosphor powder, not the amount based on the raw material mixture. The Li compounds used as raw materials have a high vapor pressure and are easily volatilized, and when attempting to synthesize nitrides and oxynitrides at high temperatures, a considerable amount of them volatilize. In other words, the Li content based on the raw material mixture is significantly different from the content in the final product, so it does not mean the Li content in the phosphor.
[0027] If the content of Ce, which is the luminescent center of phosphor particles, is too low, its contribution to luminescence tends to be small, and if it is too high, Ce 3+ Concentration quenching of the phosphor tends to occur due to energy transfer between the elements. Therefore, the Ce content is 0.5 to 10 mol %, and preferably 0.5 to 5 mol %, of the M element.
[0028] The alkaline earth metal element used as the M element in the above general formula may be any element, but when Ca is used, high fluorescence intensity is obtained and the crystal structure is stabilized in a wide composition range. Therefore, it is preferable that the M element contains Ca. The M element may be a combination of multiple alkaline earth metal elements, for example, a part of the Ca element may be replaced with the Sr element.
[0029] The crystal structure of the phosphor particles is orthorhombic, and the aforementioned CaAlSiN 3 It may have the same structure as the crystal. CaAlSiN 3 The lattice constants of the crystal are, for example, a = 0.98007 nm, b = 0.56497 nm, and c = 0.50627 nm. In this embodiment, the lattice constants are usually a = 0.935 to 0.965 nm, b = 0.550 to 0.570 nm, and c = 0.480 to 0.500 nm, and CaAlSiN 3 The lattice constants of the crystalline phase are smaller than those of the crystalline phase. The range of lattice constants reflects the above-mentioned constituent elements and composition.
[0030] The crystal phase present in the phosphor particles is preferably the above-mentioned single crystal phase. However, the phosphor particles may contain other phases as long as they do not significantly affect the fluorescent properties. Examples of the other phases that have a small effect on the fluorescent properties when excited by blue light include α-sialon, AlN, and LiSi 2 N 3 , LiAlSi 2 N 4 The amount of the different phase is preferably such that the diffraction intensity of the other crystal phase is 40% or less of the strongest diffraction intensity of the above crystal phase when evaluated by powder X-ray diffraction method.
[0031] The phosphor powder of this embodiment is excited by light in a wide wavelength range from ultraviolet to visible light. For example, when irradiated with blue light of 455 nm in wavelength, it may emit broad fluorescent light with an orange peak wavelength of 570 to 610 nm and a half-width of the fluorescence spectrum of 125 nm or more. Such phosphor powder is suitable as a phosphor for a wide range of light emitting devices. The phosphor powder of this embodiment is also made of CaAlSiN 3 Like conventional nitride and oxynitride phosphors, such as those listed above, it has excellent heat resistance and chemical stability, and its brightness does not decrease much with increasing temperature. These characteristics make it particularly suitable for applications where durability is required.
[0032] (Diffuse reflectance) As already described, the diffuse reflectance X1 of the phosphor powder of this embodiment for light with a wavelength of 700 nm is 88% or more and 99.9% or less. X1 is preferably 90% or more and 99.9% or less, more preferably 92% or more and 99.9% or less, and particularly preferably 95% or more and 99.9% or less.
[0033] From another perspective, the diffuse reflectance X2 of the phosphor powder of this embodiment for light of the fluorescence peak wavelength is preferably 85% or more and 95% or less, more preferably 85.5% or more and 92% or less. When X2 is within such a numerical range, the emission intensity tends to be higher. When light of the fluorescence peak wavelength is irradiated to the phosphor, not only non-luminescent absorption due to impurities and crystal defects occurs, but also absorption due to electronic transition of the luminescence center ion occurs. For this reason, X2 is smaller than X1. However, light absorption near the peak wavelength can be an index of re-excitation emission, which is a factor in efficiency reduction. In other words, a moderately large X2 means that the contribution of excitation emission is small, and it is considered that a moderately large X2 further improves the fluorescence characteristics.
[0034] From another viewpoint, the difference between X2 and X1 (X2-X1) is preferably 4% to 8%, more preferably 4% to 7%, and particularly preferably 4% to 6%. Although the details are unclear, X2-X1 being 4% to 8% means that there is a good balance between the improvement of the fluorescent properties due to the increased absorptance when excited with blue light and the decrease in the fluorescent properties due to re-excitation emission, and therefore it is believed that this means that the properties of the phosphor are further improved.
[0035] (particle size distribution) By appropriately designing the particle size distribution of the phosphor powder of this embodiment, it may be possible to further increase the quantum efficiency and improve the balance of various performances. Specifically, the volume-based cumulative 50% diameter D50 (so-called median diameter) of the phosphor powder of this embodiment measured by a laser diffraction scattering method is preferably 8 μm or more and 25 μm or less, more preferably 10 μm or more and 20 μm or less, and even more preferably 12 μm or more and 20 μm or less.
[0036] From another perspective, the volume-based cumulative 10% diameter D of the phosphor powder of this embodiment measured by a laser diffraction scattering method 10 is preferably 2 μm or more and 15 μm or less, more preferably 5 μm or more and 12 μm or less. 10 The relatively large value of D corresponds to a relatively small amount of fines (too fine phosphor particles that tend to reduce the blue light conversion efficiency) in the phosphor powder. 10 When the value of is relatively large, the conversion efficiency of blue light tends to be higher.
[0037] From another perspective, the volume-based cumulative 90% diameter D of the phosphor powder of this embodiment measured by a laser diffraction scattering method 90 is preferably 15 μm or more and 50 μm or less, more preferably 18 μm or more and 40 μm or less. 90 That is, the amount of coarse particles in the phosphor powder is small. 90 A phosphor powder whose luminance is not too large is effective in reducing chromaticity variations in a light emitting device.
[0038] Generally, the larger the particle size of the powder, the smaller the effect of light scattering and the smaller the diffuse reflectance. In other words, there is a trade-off between particle size and the value of diffuse reflectance. However, the preferred particle size (D 50 Although the reflectance (e.g., 100 nm) is relatively large, the diffuse reflectance of the phosphor powder of this embodiment tends to be relatively large.
[0039] (Manufacturing method) The phosphor powder of this embodiment can be produced, for example, by a series of steps including the following (1) to (4), a series of steps including (1) to (3) and (5), or a series of steps including (1) to (5). From the viewpoint of appropriately adjusting the diffuse reflectance of the phosphor powder, the phosphor powder production process preferably includes (4) an acid treatment step and / or (5) a classification step (preferably sedimentation classification). (1) Preparation process of raw material mixture powder (2) Firing process (3) Crushing process of the fired material (4) Acid treatment process (5) Classification step (preferably sedimentation classification)
[0040] Below, (1) to (5) will be explained in detail.
[0041] (1) Preparation process of raw material mixture powder In the step of preparing the raw material mixed powder, suitable raw material powders are usually mixed to obtain the raw material mixed powder. As the raw material powder, nitrides of the constituent elements, i.e., silicon nitride, aluminum nitride, lithium nitride, cerium nitride, and nitrides of alkaline earth elements (e.g., calcium nitride), are preferably used. Generally, nitride powders are unstable in air, and the particle surfaces are covered with an oxide layer, so that even when a nitride raw material is used, a certain amount of oxide is ultimately contained in the raw material. When controlling the O / N ratio of the phosphor, these factors must be taken into consideration, and if there is a shortage of oxygen, a portion of the nitride may be made into an oxide (including compounds that become oxides by heat treatment). An example of an oxide is cerium oxide.
[0042] Among the raw material powders, the lithium compound is highly volatile due to heating, and depending on the sintering conditions, most of the lithium compound may volatilize. Therefore, it is preferable to determine the blending amount of the lithium compound according to the sintering conditions, taking into consideration the amount of volatilization during the sintering process.
[0043] Among the nitride raw material powders, lithium nitride, cerium nitride, and nitrides of alkaline earth elements react violently with moisture in the air, so it is preferable to handle these in a glove box substituted with an inert atmosphere. From the viewpoint of operational efficiency, it is preferable to (i) first weigh out predetermined amounts of silicon nitride, aluminum nitride and various oxide raw material powders that can be handled in air, and thoroughly mix them in advance in air to prepare a premixed powder, and (ii) then mix the premixed powder with a substance that easily reacts with moisture, such as lithium nitride, in a glove box to prepare the raw material mixed powder.
[0044] (2) Firing process In the firing step, the raw material mixture powder prepared in the (1) raw material mixture powder preparation step is filled into an appropriate container and heated using a firing furnace or the like.
[0045] The firing temperature is preferably from 1600 to 2000° C., and more preferably from 1700 to 1900° C., from the viewpoints of sufficiently promoting the reaction and suppressing the volatilization of lithium. The baking time is preferably from 2 to 24 hours, more preferably from 4 to 16 hours, from the viewpoint of sufficiently promoting the reaction and suppressing the volatilization of lithium.
[0046] The firing step is preferably carried out in a nitrogen atmosphere. It is also preferable to appropriately adjust the pressure of the firing atmosphere. Specifically, the pressure of the firing atmosphere is preferably 0.5 MPa·G or higher. When the firing temperature is 1800°C or higher, in particular, the phosphor tends to decompose easily, but by keeping the pressure of the firing atmosphere high, the decomposition of the phosphor can be suppressed. Incidentally, when industrial productivity is taken into consideration, the pressure of the firing atmosphere is preferably less than 1 MPa·G.
[0047] The container for filling the raw material mixture powder is preferably made of a material that is stable in a high-temperature nitrogen atmosphere and does not react with the raw material mixture powder or its reaction products. The material of the container is preferably boron nitride.
[0048] (3) Crushing process of the fired material The fired product obtained in (2) is usually in the form of lumps, and is therefore preferably pulverized to a relatively small size by applying mechanical force. For the pulverization, various devices such as a crusher, a mortar, a ball mill, a vibration mill, a jet mill, a stamp mill, etc. may be used. Two or more of these devices may be combined for pulverization. In the examples shown below, a stamp mill is used to obtain a coarsely pulverized product of the fired material, and then the coarsely pulverized product is further pulverized using a jet mill. Although the details are unclear, such pulverization makes it easy to obtain a phosphor powder having a diffuse reflectance X1 of 88% or more and 99.9% or less.
[0049] (4) Acid treatment process In the acid treatment step, for example, the pulverized material obtained in (3) above is immersed in an acidic aqueous solution. Although the details are unclear, it is believed that the acid treatment removes or reduces "heterogeneous phases" in the phosphor that do not contribute to light emission or that reduce the light emission efficiency. Incidentally, as mentioned above, the fact that the diffuse reflectance X1 of the phosphor powder is 88% or more and 99.9% or less may correspond to the removal or reduction of heterogeneous phases.
[0050] The acidic aqueous solution may be an acidic aqueous solution containing one acid selected from the group consisting of hydrofluoric acid, nitric acid, hydrochloric acid, etc., or a mixed acid aqueous solution obtained by mixing two or more of the above acids. As the acid, nitric acid or hydrochloric acid is preferred, and hydrochloric acid is more preferred. The concentration of the acidic aqueous solution is appropriately set depending on the strength of the acid used, and is, for example, 0.5 to 50% by mass, preferably 1 to 30% by mass, and more preferably 1 to 10% by mass. The temperature when carrying out the acid treatment is preferably from 25 to 90° C., more preferably from 60 to 90° C. By carrying out the treatment at a relatively high temperature, it is easy to obtain a phosphor powder having a diffuse reflectance X1 of from 88 to 99.9%. The time for the acid treatment (immersion time) is preferably from 15 minutes to 80 minutes, and more preferably from 15 minutes to 60 minutes. After the acid treatment, the phosphor powder is preferably thoroughly washed with water and dried.
[0051] (5) Classification (sedimentation classification) process In order to reduce the amount of fine powder (too fine phosphor particles that tend to reduce the blue light conversion efficiency) in the powder, it is preferable to carry out an appropriate classification process. In order to effectively remove the fine powder, the classification method is preferably sedimentation classification as described below.
[0052] First, typically, the powder obtained in the (3) pulverization step of the fired product, or the powder that has been subjected to the (4) acid treatment step is dispersed in a suitable liquid, such as an aqueous solution of sodium hexametaphosphate, in a container to prepare a dispersion. Next, the dispersion is left to stand for a certain period of time to allow the powders in the dispersion that have relatively large particle sizes to settle. The supernatant is then drained. Further, after that, a new aqueous solution of sodium hexametaphosphate is added to the container in which the precipitate remains, the phosphor is dispersed, the container is left to stand, and the supernatant liquid is discharged. This operation is repeated several times. By "several times," it is preferably five times or more. There is no particular upper limit to the number of times, but from the viewpoint of cost, etc., it is, for example, 15 times or less, specifically 10 times or less.
[0053] By classifying, it is possible to reduce the amount of fine powder (too fine phosphor particles that tend to reduce the conversion efficiency of blue light) in the powder. Incidentally, the diffuse reflectance X1 of the phosphor powder being 88% or more and 99.9% or less may correspond to a small amount of fine powder in the phosphor powder.
[0054] The specific classification conditions are not particularly limited as long as a phosphor powder having a diffuse reflectance X1 of 88% or more and 99.9% or less can be obtained. As a guideline, it is preferable to set the classification conditions so that fine powder having a particle size of 10 μm or less is removed, and it is more preferable to set the classification conditions so that fine powder having a particle size of 7.5 μm or less is removed. When setting the conditions, in the case of sedimentation classification, Stokes' equation regarding the sedimentation velocity of particles can be referred to.
[0055] <Light-emitting device, image display device, and lighting device> A light emitting device can be obtained by combining the phosphor powder of this embodiment with a light source. The luminescent light source typically emits ultraviolet or visible light. For example, when the luminescent light source is a blue LED, the blue light emitted from the luminescent light source hits the phosphor powder, and the blue light is converted into light with a longer wavelength. That is, the phosphor powder of the present embodiment can be used as a wavelength conversion material that converts blue light into light with a longer wavelength.
[0056] An example of a specific configuration of the light emitting device will be described with reference to FIG. 1 is a schematic cross-sectional view showing an example of the structure of a light emitting device. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, a bonding wire 170, a bonding wire 172, and a composite 40.
[0057] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. By mounting the light emitting element 120 on the heat sink 130, it is possible to improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.
[0058] The light emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm to 500 nm, which corresponds to near ultraviolet to blue light, can be used as the light emitting element 120. One electrode (not shown) disposed on the upper surface side of the light emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.
[0059] A generally funnel-shaped recess whose hole diameter gradually increases from the bottom surface toward the top is formed in the case 140. The light emitting element 120 is provided on the bottom surface of the recess. The wall surface of the recess surrounding the light emitting element 120 serves as a reflector.
[0060] The composite 40 is filled in the recess whose wall is formed by the case 140. The composite 40 is a wavelength conversion member that converts the excitation light emitted from the light emitting element 120 into light with a longer wavelength. The composite 40 is obtained by dispersing at least the phosphor powder of this embodiment in an encapsulant 30 such as a resin. In order to obtain white light of higher quality, the encapsulant 30 may contain not only the phosphor powder of this embodiment but also other phosphor powders. The light emitting device 100 emits a mixed color of light from the light emitting element 120 and light emitted from the phosphor particles 1 which are excited by absorbing the light emitted from the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light from the light emitting element 120 and the light generated from the phosphor particles 1.
[0061] Incidentally, although a surface mount type light emitting device is illustrated in FIG. 1, the light emitting device is not limited to the surface mount type, and may be a bullet type, a COB (chip on board) type, or a CSP (chip scale package) type.
[0062] The light emitting device can be used in image display devices such as displays, and lighting devices. For example, a liquid crystal display can be manufactured using the light emitting device 100 as a backlight. Also, a lighting device can be manufactured using one or more light emitting devices 100 and providing appropriate wiring.
[0063] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. General formula M x (Si,Al) 2 (N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, A phosphor powder having a diffuse reflectance X1 for light with a wavelength of 700 nm of 88% or more and 99.9% or less. 2. 1. The phosphor powder according to claim 1, The phosphor powder has a diffuse reflectance X2 of 85% or more and 95% or less for light having a fluorescence peak wavelength. 3. 1. or 2. The phosphor powder according to claim 1, A phosphor powder in which the difference X1-X2 between the diffuse reflectance X1 for light with a wavelength of 700 nm and the diffuse reflectance X2 for light with a fluorescence peak wavelength is 4% or more and 8% or less. 4. The phosphor powder according to any one of 1. to 3., Volume-based cumulative 50% diameter D measured by laser diffraction scattering method 50 The phosphor powder has a size of 8 μm or more and 25 μm or less. 5. A light emitting device comprising the phosphor powder according to any one of 1. to 4. and a light source. 6. 5. The light-emitting device according to claim 5, A light-emitting device in which a light-emitting source emits ultraviolet or visible light. 7. An image display device comprising the light emitting device according to 5. or 6. 8. 5. An illumination device comprising the light-emitting device according to 5. or 6. EXAMPLES
[0064] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.
[0065] <Production of phosphor powder> Example 1 (1) Preparation of raw material mixture First, pre-mixing was performed. Specifically, of the raw materials listed in Table 1, Si 3 N 4 , AlN and CeO 2 The mixture was mixed (dry blended) for 30 minutes using a small V-type mixer, and then sieved through a nylon sieve with 150 μm openings to obtain a premixed powder. Next, in a nitrogen atmosphere glove box, the remaining raw materials listed in Table 1 (Ca 3 N 2 and Li 3 N) was added, thoroughly dry-blended, and then sieved through a sieve with 500 μm openings to obtain a raw material mixed powder.
[0066] (2) Firing The raw material powder mixture was packed into a boron nitride container. This container was placed in a furnace, and the raw material powder mixture was heated under N of 0.72 MPa G. 2 The mixture was sintered in an atmosphere at 1800°C for 8 hours.
[0067] (3) Grinding of the fired product The fired product obtained in (2) was pulverized using a stamp mill. The pulverization using the stamp mill was repeated until the passing rate of the product through a vibrating sieve with an opening of 250 μm exceeded 90%. The fired product that had been pulverized by the stamp mill was further pulverized by a jet mill (PJM-80SP, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) under the following pulverization conditions: sample supply rate: 50 g / min, pulverization air pressure: 0.3 MPa.
[0068] (4) Acid treatment The pulverized fired product was put into hydrochloric acid for acid treatment. Specifically, first, 35-37% by mass hydrochloric acid and distilled water were mixed in a volume ratio of 50 mL:300 mL to prepare an aqueous hydrochloric acid solution heated to 80° C. The fired product pulverized in (3) was added to this aqueous hydrochloric acid solution and stirred for 0.5 hours for acid treatment. The acid-treated fired product was thoroughly washed with distilled water and then dried at 110° C. for 3 hours. Then, it was passed through a sieve with 45 μm openings to remove coarse / agglomerated particles.
[0069] (5) Removal of fine particles by sedimentation classification First, a 0.05% by mass aqueous solution of sodium hexametaphosphate was prepared, and this aqueous solution was poured into a container having an inner diameter of 70 mm and a height of 120 mm to a height of 110 mm. Next, the acid-treated baked product was placed in a container containing the above aqueous solution, thoroughly stirred to disperse, and then left to stand for 22 minutes. After standing, the supernatant liquid was removed from the top by 90 mm. Then, an aqueous solution of sodium hexametaphosphate was added to a height of 110 mm, and the powder was again dispersed by stirring, and the same treatment was carried out. This operation was repeated seven times to remove the fine powder contained in the acid-treated powder (incidentally, the classification point is 7.5 μm according to Stokes' law). Thereafter, the slurry at the bottom of the container was filtered while being washed with water to recover the solid matter, which was then dried at 110° C. for 3 hours and passed through a sieve with 45 μm openings to break down the agglomerated particles. In this manner, a phosphor powder was obtained.
[0070] Example 2 A phosphor powder was obtained in the same manner as in Example 1, except that the sedimentation classification was not carried out.
[0071] Example 3 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials used were those listed in Table 1, (b) no acid treatment was performed (the fired material pulverized in a jet mill was subjected to sedimentation classification without acid treatment), and (c) the pulverization air pressure in the jet mill pulverization was set to 0.6 MPa.
[0072] Example 4 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials shown in Table 1 were used, and (b) sedimentation classification was not carried out.
[0073] Example 5 A phosphor powder was obtained in the same manner as in Example 4, except that in the acid treatment, nitric acid with a concentration of 60 mass % was used instead of hydrochloric acid.
[0074] Example 6 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials listed in Table 1 were used, and (b) acid treatment was not performed (the fired material pulverized in a jet mill was subjected to sedimentation classification without acid treatment).
[0075] Comparative Example 1 Phosphor powders were obtained in the same manner as in Example 4, except that (a) the raw materials shown in Table 1 were used, and (b) the acid treatment was not carried out.
[0076] Example 7 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials listed in Table 1 were used, (b) acid treatment was not performed (the fired material pulverized by the jet mill was subjected to sedimentation classification without acid treatment), and (c) the fired material pulverized by the jet mill was passed through a sieve with a mesh size of 45 μm to remove coarse / agglomerated particles, and then subjected to sedimentation classification.
[0077] Example 8 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials listed in Table 1 were used, (b) acid treatment was not performed (the fired material ground in the jet mill was subjected to sedimentation classification without acid treatment), (c) the grinding air pressure in the jet mill grinding was set to 0.4 MPa, and (d) the fired material ground in the jet mill was passed through a sieve with 45 μm openings to remove coarse / agglomerated particles before being subjected to sedimentation classification.
[0078] <Confirmation of chemical composition / crystal structure> The composition of some of the phosphor powders was analyzed as follows. Amounts of Ca, Li, Ce, Si and Al: The phosphor powder was dissolved by an alkali fusion method, and then the amounts were measured using an ICP emission spectrometer (CIROS-120, manufactured by Rigaku Corporation). Amounts of O and N: Measured using an oxygen / nitrogen analyzer (HORIBA, EMGA-920). Based on the measurement results, the general formula M x (Si,Al) 2 (N,O) 3±y The x, y, Si / Al atomic ratio, O / N atomic ratio, Li ratio of M, and Ce ratio of M were determined. The impurity elements Cr and Fe were measured by dissolving the phosphor powder in a mixed acid of hydrofluoric acid and nitric acid by pressure acid decomposition, and then measuring the impurity elements by an ICP emission spectrometer.
[0079] For the phosphor of Example 1, powder X-ray diffraction (XRD) measurement was also performed using an X-ray diffractometer (Ultima IV-N manufactured by Rigaku Corporation) with Cu-Kα radiation. The obtained XRD pattern is shown in Figure 2. Analysis of the obtained XRD pattern revealed that the main phase was an orthorhombic crystal with lattice constants a = 0.9486 nm, b = 0.5586 nm, and c = 0.4933 nm, with a small amount of LiAlSi 2 N 4 The presence of was confirmed.
[0080] Incidentally, the chemical composition of the phosphor powders in Examples 4 and 5 was hardly measured. However, the manufacturing process up to the pulverization of the fired material was the same in Example 3, Examples 4, and 5, and the composition of the raw material mixed powder in Examples 4 and 5 was the same as in Example 3. Furthermore, although the manufacturing procedures differ between Example 3 and Examples 4 and 5, it is difficult to imagine that the difference has a significant effect on the chemical composition. Therefore, the measurement of the chemical composition of the phosphor powders in Examples 4 and 5 was omitted. Similarly, the chemical composition of the phosphor powder of Example 8 is similar to that of Example 7. Although the manufacturing procedures are different between Examples 7 and 8, it is difficult to imagine that the differences have a significant effect on the chemical composition. Therefore, the measurement of the chemical composition of the phosphor powder of Example 8 was omitted.
[0081] <Measurement of diffuse reflectance> The diffuse reflectance was measured using an ultraviolet-visible spectrophotometer (V-550) manufactured by JASCO Corporation equipped with an integrating sphere device (ISV-469). During the measurement, baseline correction was performed using a standard reflector (Spectralon). The solid sample holder filled with the phosphor powder was attached to a predetermined position in the apparatus, and the diffuse reflectance spectrum was measured in the wavelength range of 500 to 850 nm, and the diffuse reflectance for light with a wavelength of 700 nm and for light with the fluorescent peak wavelength of the phosphor powder (described later) was calculated.
[0082] <Measurement of particle size distribution> The particle size distribution was measured by a laser diffraction scattering method in accordance with JIS R 1629: 1997 using an LS13 320 (manufactured by Beckman Coulter, Inc.) Water was used as the measurement solvent. Specifically, a small amount of phosphor powder was first added to an aqueous solution containing 0.05% by mass of sodium hexametaphosphate as a dispersant. A dispersion was then prepared by dispersing the powder using a horn-type ultrasonic homogenizer (output: 300 W, horn diameter: 26 mm). An appropriate amount of this dispersion was added to the measurement solvent to measure the particle size distribution. From the obtained cumulative volume frequency distribution curve, the 10% volume diameter (D 10 ), 50% volume diameter (D 50 ) and 90% volume diameter (D 90 ) was sought.
[0083] <Evaluation> (Fluorescence peak intensity) The fluorescence spectrum of the phosphor powder was measured using a spectrofluorophotometer (Hitachi High-Tech Science, F-7000) corrected with Rhodamine B and a secondary standard light source. Specifically, the fluorescence spectrum emitted by exciting the phosphor powder with monochromatic light of 455 nm was measured, and the fluorescence peak intensity and fluorescence peak wavelength were obtained. The fluorescence peak intensity varies depending on the measurement device and conditions. The fluorescence peak intensity shown in the table below is a value when the fluorescence peak intensity of a standard sample (YAG, more specifically, P46Y3 manufactured by Mitsubishi Chemical Corporation) is set to 100.
[0084] (Internal and external quantum efficiency) The internal quantum efficiency and external quantum efficiency of each phosphor powder were determined using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.) according to the following procedure. (1) The phosphor powder was filled into the recess of the concave cell so that the surface was smooth. This concave cell was attached to a predetermined position (sample part) in the integrating sphere. Monochromatic light, which was split into a wavelength of 455 nm from a light source (Xe lamp), was introduced into the integrating sphere using an optical fiber. This monochromatic light (excitation light) was irradiated onto the phosphor powder filled into the recess of the concave cell, and the fluorescence spectrum was measured. From the obtained spectrum data, the peak wavelength was obtained, and the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) were calculated. The number of excitation reflected light photons was calculated in the wavelength range of 450 nm to 465 nm, and the number of fluorescence photons was calculated in the wavelength range of 465 nm to 800 nm. (2) In addition, instead of the concave cell, a standard reflector with a reflectance of 99% (Spectralon, manufactured by Labsphere) was attached to the sample section to measure the spectrum of the excitation light with a wavelength of 455 nm. The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 nm to 465 nm. (3) The internal quantum efficiency and external quantum efficiency were calculated from Qref, Qem, and Qex obtained in (1) and (2) above according to the following formula. Internal quantum efficiency = (Qem / (Qex-Qref)) x 100 External quantum efficiency = (Qem / Qex) x 100
[0085] Various information is summarized in Table 1. In Table 1, "ND" stands for Not Detected.
[0086] In addition, the raw materials listed in the "Raw materials used" column in Table 1 are as follows.
[0087] Ca 3 N 2 -1: Ca manufactured by Taiheiyo Cement Corporation 3 N 2 Ca 3 N 2 -2: Ca manufactured by CERAC (now Materion) 3 N 2
[0088] Li 3 N-1: Li manufactured by Materion 3 N Li 3 N-2: Li manufactured by CERAC (now Materion) 3 N Li 3 N-3: Li produced by High Purity Chemical Laboratory 3 N
[0089] CEO 2 -1: CeO manufactured by Shin-Etsu Chemical Co., Ltd. 2 , C grade
[0090] S 3 N 4 -1: Si manufactured by Ube Industries 3 N 4 , E10 grade
[0091] AlN-1: Tokuyama AlN, E grade
[0092] [Table 1]
[0093] As shown in Table 1, the general formula M x (Si,Al) 2 (N,O) 3±y The phosphor powders (Examples 1 to 8) containing phosphor particles represented by the formula (1) and having a diffuse reflectance X1 of 88% or more and 99.9% or less exhibited good fluorescence peak intensity, internal quantum efficiency and external quantum efficiency. On the other hand, the phosphor powder (Comparative Example 1) having a diffuse reflectance X1 of less than 88% was inferior to Examples 1 to 8 at least in internal quantum efficiency.
[0094] This application claims priority based on Japanese Patent Application No. 2020-189203, filed on November 13, 2020, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]
[0095] 1. Phosphor particles 30 Encapsulating material 40 Complex 100 Light emitting device 120 Light emitting element 130 Heat sink 140 cases 150 First lead frame 160 Second lead frame 170 Bonding Wire 172 Bonding Wire
Claims
1. General formula M x (Si, Al) 2 (N, O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, A phosphor powder having a diffuse reflectance X1 for light having a wavelength of 700 nm of 90.5% or more and 99.9% or less.
2. The phosphor powder according to claim 1 , The phosphor powder has a diffuse reflectance X2 of 85% or more and 95% or less for light having a fluorescence peak wavelength.
3. The phosphor powder according to claim 1 or 2, A phosphor powder in which the difference X1-X2 between the diffuse reflectance X1 for light with a wavelength of 700 nm and the diffuse reflectance X2 for light with a fluorescence peak wavelength is 4% or more and 8% or less.
4. The phosphor powder according to any one of claims 1 to 3, Volume-based cumulative 50% diameter D measured by laser diffraction scattering method 50 The phosphor powder has a particle size of 8 μm or more and 25 μm or less.
5. A light emitting device comprising the phosphor powder according to any one of claims 1 to 4 and a light source.
6. 6. The light emitting device according to claim 5, A light-emitting device in which a light-emitting source emits ultraviolet or visible light.
7. An image display device comprising the light emitting device according to claim 5 .
8. An illumination device comprising the light-emitting device according to claim 5 or 6.
Citation Information
Patent Citations
Rocking device for cable crane
JP1984069391A
Phosphor, method for producing same, light-emitting device, and image display apparatus
WO2010110457A1
Phosphor, and light-emitting device and use thereof
WO2012067130A1
Phosphor, light-emitting element and lighting device
WO2014077132A1