Phosphor powder, light-emitting device, image display device and lighting device
A phosphor powder with a tailored composition and optimized parameters enhances blue light conversion efficiency and internal quantum efficiency, addressing the limitations of existing phosphors in light emitting devices.
Patent Information
- Application Number
- JP2022561861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-13
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-04
AI Technical Summary
The phosphors described in existing technologies have room for improvement in terms of blue light conversion efficiency, specifically in increasing internal quantum efficiency.
A phosphor powder with a specific chemical composition represented by the general formula M x (Si,Al) 2 (N,O) 3±y, where M is Li and one or more alkaline earth metal elements, with a part of M replaced by Ce, and optimized parameters such as Si/Al ratio, O/N ratio, and Li and Ce content, resulting in a light absorption rate of less than 10% at 700 nm, is developed.
The phosphor powder exhibits high internal quantum efficiency and improved blue light conversion efficiency, maintaining excellent heat resistance and chemical stability, suitable for various light emitting devices.
Smart Images

Figure 0007590450000002 
Figure 0007590450000003 
Figure 0007590450000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphor powder, a light emitting device, an image display device, and an illumination device. [Background technology]
[0002] In order to manufacture white LEDs (Light Emitting Diodes), phosphors are usually used as wavelength conversion materials to obtain white light from blue light emitted from blue LEDs. With the widespread use of white LEDs for lighting applications and the consideration of applying white LEDs to image display devices, development of phosphors capable of converting blue light into light with longer wavelengths is ongoing.
[0003] One aspect of improving phosphors is to modify the chemical composition of the phosphor. For example, Patent Document 1 discloses a compound of the general formula M x (Si,Al)2(N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.23), in which part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, and 5 to 50 mol % of M is Li and 0.5 to 10 mol % of M is Ce. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5969391 Summary of the Invention [Problem to be solved by the invention]
[0005] As found by the present inventors, the phosphor described in Patent Document 1 has room for improvement in terms of blue light conversion efficiency, specifically, in terms of increasing the internal quantum efficiency.
[0006] The present inventors have carried out investigations with the aim of providing a phosphor powder having high internal quantum efficiency and improved blue light conversion efficiency. [Means for solving the problem]
[0007] As a result of their investigations, the inventors have completed the invention provided below.
[0008] According to the present invention, General formula M x (Si,Al)2(N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, Light absorptance A at a wavelength of 700 nm 700 Phosphor powder with a content of 10% or less is provided.
[0009] Further, according to the present invention, A light emitting device comprising the above phosphor powder and a light source. is provided.
[0010] Further, according to the present invention, An image display device including the light emitting device is provided.
[0011] Further, according to the present invention, A lighting device including the light-emitting device described above is provided. Effect of the Invention
[0012] The phosphor powder of the present invention has high internal quantum efficiency and good blue light conversion efficiency. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view showing an example of the structure of a light-emitting device. [Diagram 2] 1 shows an XRD pattern obtained by measuring the phosphor of Example 1 by powder X-ray diffraction (XRD). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar symbols and descriptions thereof will be omitted as appropriate. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.
[0015] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass".
[0016] <Phosphor powder> The phosphor powder of this embodiment is represented by the general formula M x (Si,Al)2(N,O) 3±y In this general formula, M is Li and one or more alkaline earth metal elements, and 0.52≦x≦0.9 and 0.06≦y≦0.36. Also, a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce. In addition, the light absorptance A of the phosphor powder of this embodiment at a wavelength of 700 nm 700 is less than 10%.
[0017] The phosphor powder of this embodiment comprises at least A 700is 10% or less, and thus differs from the phosphor described in Patent Document 1. The phosphor powder of the present embodiment converts blue light into light with a longer wavelength more efficiently, for example, in terms of internal quantum efficiency, compared to the phosphor described in Patent Document 1.
[0018] The absorption of phosphors can be classified into two types: light absorption accompanying electronic transition of the luminescent center ion, and light absorption unrelated to fluorescent emission caused by impurities or crystal defects in the host material. When a phosphor that emits visible light is irradiated with light in the near infrared range, for example, light with a wavelength of 700 nm, the light absorption is unrelated to fluorescent emission. Therefore, the absorptivity of light with a wavelength of 700 nm is considered to be related to the fluorescent properties. In order to quantitatively evaluate the relationship between the optical absorptance and the fluorescent properties, the present inventors have used a compound represented by the general formula M x (Si,Al)2(N,O) 3±y We created various phosphors with the above formula and measured the absorption rate of light with a wavelength of 700 nm. 700 It has been found that when is small, the internal quantum efficiency tends to be high. Based on this finding, the present inventors have proposed a method for producing a compound represented by the general formula M x (Si,Al)2(N,O) 3±y The phosphor is represented by the formula: 700 The researchers have now succeeded in creating a new phosphor powder with an internal quantum efficiency of less than 10%.
[0019] The phosphor powder of this embodiment can be manufactured by using appropriate materials and by selecting appropriate manufacturing methods and conditions. Examples of "appropriate manufacturing methods and conditions" include one or more of the following: (i) acid-treating the phosphor powder under specific conditions, (ii) subjecting the phosphor powder to an appropriate classification process (preferably sedimentation classification), and (iii) devising a method for pulverizing the phosphor powder. Details of the manufacturing methods and conditions will be described later.
[0020] The phosphor powder of this embodiment will be described further.
[0021] (Crystal structure, chemical composition, etc.) The skeletal structure of the phosphor crystal is composed of (Si,Al)-(N,O)4 regular tetrahedrons bonded together, with the M element located in the gap between them. The composition of the above general formula is valid in a wide range where electrical neutrality is maintained by the overall parameters of the valence and amount of the M element, the Si / Al ratio, and the N / O ratio. A representative phosphor represented by the above general formula is CaAlSiN3, where the M element is Ca and x=1, Si / Al=1, and O / N=0. When part of the Ca in CaAlSiN3 is replaced with Eu, it becomes a red phosphor, and when it is replaced with Ce, it becomes a yellow to orange phosphor.
[0022] The crystal structure of the phosphor particles contained in the phosphor powder of this embodiment is usually based on CaAlSiN3 crystals. One of the features of this phosphor particle is that the constituent elements and composition have been significantly changed so that very high luminous efficiency can be obtained even with Ce activation. In the above general formula, the M element is a combination of Li and an alkaline earth metal element, and a part of it is replaced with Ce, which serves as the luminescence center. By using Li, the average valence of the M element can be widely controlled by combining it with a divalent alkaline earth element and a trivalent Ce element. + The ionic radius of is very small, and the crystal size can be changed significantly depending on the amount of isotopic fraction, resulting in a wide variety of fluorescent emissions. The coefficient x of the M element in the above general formula is 0.52 to 0.9, preferably 0.6 to 0.9, more preferably 0.7 to 0.9. When the coefficient x exceeds 0.9, that is, when it approaches CaAlSiN3 crystal, the fluorescence intensity tends to decrease, and when the coefficient x is smaller than 0.52, a large amount of a different phase other than the target crystal phase is generated, so that the fluorescence intensity tends to decrease significantly.
[0023] In this embodiment, electrical neutrality is maintained by the average valence and amount of M element, the Si / Al ratio, and the O / N ratio, and in the case of a single crystal without defects, y=0. However, when considering the composition of the phosphor as a whole, a second crystal phase or an amorphous phase may exist, and when considering the crystal itself, the charge balance may be lost due to crystal defects. In this embodiment, from the viewpoint of increasing the fluorescence intensity, y is preferably 0.06 to 0.36, more preferably 0.1 to 0.35, and even more preferably 0.06 to 0.23.
[0024] In this embodiment, the O / N atomic ratio (molar ratio) is 0 to 0.1, preferably 0.01 to 0.08, and more preferably 0.02 to 0.07. If the O / N atomic ratio is too large, the amount of heterophase generated increases, the luminous efficiency decreases, and the covalent bond of the crystal decreases, which tends to cause deterioration of temperature characteristics (reduction in luminance at high temperatures).
[0025] The Si / Al atomic ratio (molar ratio) is usually determined by the average valence or amount of the M element and the O / N atomic ratio being within a predetermined range. The Si / Al atomic ratio is 1.5 or more and 6 or less, preferably 2 or more and 4 or less, and more preferably 2.5 or more and 4 or less.
[0026] The Li content in the phosphor particles is 5 to 50 mol %, preferably 15 to 45 mol %, and more preferably 25 to 45 mol % of the element M. The effect of Li is easily exhibited at 5 mol % or more, but if it exceeds 50 mol %, the intended crystal structure of the phosphor cannot be maintained and a different phase is generated, which tends to reduce the luminous efficiency. Just to be clear, the "Li content" refers to the Li content in the final phosphor powder, not the amount based on the raw material mixture. The Li compounds used as raw materials have a high vapor pressure and are easily volatilized, and when attempting to synthesize nitrides and oxynitrides at high temperatures, a considerable amount of them volatilize. In other words, the Li content based on the raw material mixture is significantly different from the content in the final product, so it does not mean the Li content in the phosphor.
[0027] If the content of Ce, which is the luminescent center of the phosphor particles, is too low, its contribution to luminescence tends to be small, and if it is too high, Ce 3+ Concentration quenching of the phosphor tends to occur due to energy transfer between the elements. Therefore, the Ce content is 0.5 to 10 mol %, and preferably 0.5 to 5 mol %, of the M element.
[0028] The alkaline earth metal element used as the M element in the above general formula may be any element, but when Ca is used, high fluorescence intensity is obtained and the crystal structure is stabilized in a wide composition range. Therefore, it is preferable that the M element contains Ca. The M element may be a combination of multiple alkaline earth metal elements, for example, a part of the Ca element may be replaced with the Sr element.
[0029] The crystal structure of the phosphor particles is an orthorhombic system, and may be the same structure as the CaAlSiN3 crystal described above. The lattice constants of the CaAlSiN3 crystal are, for example, a=0.98007 nm, b=0.56497 nm, and c=0.50627 nm. In this embodiment, the lattice constants are usually a=0.935-0.965 nm, b=0.550-0.570 nm, and c=0.480-0.500 nm, all of which are smaller than those of the CaAlSiN3 crystal. This range of lattice constants reflects the above-mentioned constituent elements and composition.
[0030] The crystal phase present in the phosphor particles is preferably the above-mentioned single crystal phase. However, the phosphor particles may contain other phases as long as they do not significantly affect the fluorescent properties. Examples of the other phases that have a small effect on the fluorescent properties when excited by blue light include α-sialon, AlN, LiSi2N3, and LiAlSi2N4. The amount of the other phase is preferably such that the diffraction intensity of the other crystal phase is 40% or less of the strongest diffraction intensity of the above-mentioned crystal phase when evaluated by powder X-ray diffraction method.
[0031] The phosphor powder of this embodiment is excited by light in a wide wavelength range from ultraviolet to visible light. For example, when blue light with a wavelength of 455 nm is irradiated, it may emit broad fluorescent light with an orange peak wavelength of 570 to 610 nm and a half-width of the fluorescence spectrum of 125 nm or more. Such phosphor powder is suitable as a phosphor for a wide range of light-emitting devices. In addition, the phosphor powder of this embodiment has excellent heat resistance and chemical stability, similar to conventional nitride / oxynitride phosphors represented by CaAlSiN3, and has the property of small decrease in luminance due to temperature rise. Such a property is particularly suitable for applications requiring durability.
[0032] (Light Absorption Rate) As already mentioned, the light absorptance A of the phosphor powder of this embodiment at a wavelength of 700 nm 700 is less than 10%. 700 is preferably 1% or more and 10% or less, more preferably 2% or more and 10% or less, and particularly preferably 3% or more and 10% or less.
[0033] From another perspective, the light absorptance of the phosphor powder of this embodiment at a wavelength of 600 nm is A 600 (%), A 600 -A 700 is preferably 6% or more and 10% or less, more preferably 7% or more and 10% or less, and even more preferably 7% or more and 9% or less. 600 -A 700 Phosphor powders with an appropriate value for λ tend to have better blue light conversion efficiency. Although the details are unknown, the general formula M x (Si,Al)2(N,O) 3±y When blue light is irradiated onto a phosphor represented by the formula, the peak wavelength of the emission (fluorescence) is approximately 600 nm, so the light absorptance A at a wavelength of 600 nm is 600 The above indicators (A 600 -A 700 ) may be correlated with the blue light conversion efficiency. For example, A 600 -A 700A value of 6% or more and 10% or less may indicate a good balance between the improvement of the fluorescence properties due to the increased absorptance when excited with blue light and the decrease in the fluorescence properties due to re-excitation emission.
[0034] From another perspective, the light absorptance A of the phosphor powder of this embodiment at a wavelength of 600 nm 600 The value itself is preferably 8% or more and 20% or less, more preferably 10% or more and 20% or less, and further preferably 11% or more and 17% or less. When a phosphor is irradiated with light having a wavelength of 600 nm, which is approximately the peak wavelength of fluorescence, it is thought that not only non-luminescent absorption due to impurities and crystal defects occurs, but also absorption due to electronic transitions of the luminescent center ions. 600 A 700 However, the optical absorption near the peak wavelength can be an indicator of re-excited emission, which is a factor in reducing efficiency. 600 is not too large, it means that the contribution of excitation emission is small, and A 600 It is believed that the fluorescent properties are further improved by not having too large.
[0035] (particle size distribution) By appropriately designing the particle size distribution of the phosphor powder of this embodiment, it may be possible to further increase the quantum efficiency and improve the balance of various performances. Specifically, the volume-based cumulative 50% diameter D of the phosphor powder of this embodiment measured by a laser diffraction scattering method 50 (so-called median diameter) is preferably 8 μm or more and 25 μm or less, more preferably 10 μm or more and 20 μm or less, and further preferably 12 μm or more and 20 μm or less.
[0036] From another perspective, the volume-based cumulative 10% diameter D of the phosphor powder of this embodiment measured by a laser diffraction scattering method 10 is preferably 2 μm or more and 15 μm or less, more preferably 5 μm or more and 12 μm or less. 10The relatively large value of D corresponds to a relatively small amount of fines (too fine phosphor particles that tend to reduce the blue light conversion efficiency) in the phosphor powder. 10 When the value of is relatively large, the conversion efficiency of blue light tends to be higher.
[0037] From another perspective, the volume-based cumulative 90% diameter D of the phosphor powder of this embodiment measured by a laser diffraction scattering method 90 is preferably 15 μm or more and 50 μm or less, more preferably 18 μm or more and 40 μm or less. 90 That is, the amount of coarse particles in the phosphor powder is small. 90 A phosphor powder whose luminance is not too large is effective in reducing chromaticity variations in a light emitting device.
[0038] Generally, the larger the particle size of the powder, the smaller the effect of light scattering and the higher the light absorptance. In other words, there is a trade-off between particle size and the light absorptance. However, the preferred particle size (D 50 Although the optical absorptance of the phosphor powder of this embodiment is relatively large, the optical absorptance of the phosphor powder of this embodiment tends to be relatively small.
[0039] (Manufacturing method) The phosphor powder of this embodiment can be produced, for example, by a series of steps including the following (1) to (4), a series of steps including (1) to (3) and (5), or a series of steps including (1) to (5). From the viewpoint of appropriately adjusting the non-luminescent absorption of the phosphor powder, the phosphor powder production process preferably includes (4) an acid treatment step and / or (5) a classification step (preferably sedimentation classification). (1) Preparation process of raw material mixture powder (2) Firing process (3) Crushing process of the fired material (4) Acid treatment process (5) Classification step (preferably sedimentation classification)
[0040] Below, (1) to (5) will be explained in detail.
[0041] (1) Preparation process of raw material mixture powder In the step of preparing the raw material mixed powder, suitable raw material powders are usually mixed to obtain the raw material mixed powder. As the raw material powder, nitrides of the constituent elements, i.e., silicon nitride, aluminum nitride, lithium nitride, cerium nitride, and nitrides of alkaline earth elements (e.g., calcium nitride), are preferably used. Generally, nitride powders are unstable in air, and the particle surfaces are covered with an oxide layer, so that even when a nitride raw material is used, a certain amount of oxide is ultimately contained in the raw material. When controlling the O / N ratio of the phosphor, these factors must be taken into consideration, and if there is a shortage of oxygen, a portion of the nitride may be made into an oxide (including compounds that become oxides by heat treatment). An example of an oxide is cerium oxide.
[0042] Among the raw material powders, the lithium compound is highly volatile due to heating, and depending on the sintering conditions, most of the lithium compound may volatilize. Therefore, it is preferable to determine the blending amount of the lithium compound according to the sintering conditions, taking into consideration the amount of volatilization during the sintering process.
[0043] Among the nitride raw material powders, lithium nitride, cerium nitride, and nitrides of alkaline earth elements react violently with moisture in the air, so it is preferable to handle these in a glove box substituted with an inert atmosphere. From the viewpoint of operational efficiency, it is preferable to (i) first weigh out predetermined amounts of silicon nitride, aluminum nitride and various oxide raw material powders that can be handled in air, and thoroughly mix them in advance in air to prepare a premixed powder, and (ii) then mix the premixed powder with a substance that easily reacts with moisture, such as lithium nitride, in a glove box to prepare the raw material mixed powder.
[0044] (2) Firing process In the firing step, the raw material mixture powder prepared in the (1) raw material mixture powder preparation step is filled into an appropriate container and heated using a firing furnace or the like.
[0045] The firing temperature is preferably from 1600 to 2000° C., and more preferably from 1700 to 1900° C., from the viewpoints of sufficiently promoting the reaction and suppressing the volatilization of lithium. The baking time is preferably from 2 to 24 hours, more preferably from 4 to 16 hours, from the viewpoint of sufficiently promoting the reaction and suppressing the volatilization of lithium.
[0046] The firing step is preferably carried out in a nitrogen atmosphere. It is also preferable to appropriately adjust the pressure of the firing atmosphere. Specifically, the pressure of the firing atmosphere is preferably 0.5 MPa·G or higher. When the firing temperature is 1800°C or higher, in particular, the phosphor tends to decompose easily, but by keeping the pressure of the firing atmosphere high, the decomposition of the phosphor can be suppressed. Incidentally, when industrial productivity is taken into consideration, the pressure of the firing atmosphere is preferably less than 1 MPa·G.
[0047] The container for filling the raw material mixture powder is preferably made of a material that is stable in a high-temperature nitrogen atmosphere and does not react with the raw material mixture powder or its reaction products. The material of the container is preferably boron nitride.
[0048] (3) Crushing process of the fired material The fired product obtained in (2) is usually in the form of lumps, and is therefore preferably pulverized to a relatively small size by applying mechanical force. For the pulverization, various devices such as a crusher, a mortar, a ball mill, a vibration mill, a jet mill, a stamp mill, etc. may be used. Two or more of these devices may be combined to perform pulverization. In the examples shown below, a coarsely pulverized product of the fired material is first obtained using a stamp mill, and then the coarsely pulverized product is further pulverized using a jet mill. Although the details are unclear, it is believed that by performing such pulverization, A 700 It is easy to obtain phosphor powder with a content of 10% or less.
[0049] (4) Acid treatment process In the acid treatment step, for example, the crushed material obtained in (3) above is immersed in an acidic aqueous solution. Although the details are unclear, it is believed that the acid treatment removes or reduces "heterogeneous phases" in the phosphor that do not contribute to light emission or that reduce the light emission efficiency. 700 A value of 10% or less may correspond to the elimination or reduction of foreign phases.
[0050] The acidic aqueous solution may be an acidic aqueous solution containing one acid selected from the group consisting of hydrofluoric acid, nitric acid, hydrochloric acid, etc., or a mixed acid aqueous solution obtained by mixing two or more of the above acids. As the acid, nitric acid or hydrochloric acid is preferred, and hydrochloric acid is more preferred. The concentration of the acidic aqueous solution is appropriately set depending on the strength of the acid used, and is, for example, 0.5 to 50% by mass, preferably 1 to 30% by mass, and more preferably 1 to 10% by mass. The temperature at which the acid treatment is carried out is preferably 25° C. or higher and 90° C. or lower, and more preferably 60° C. or higher and 90° C. or lower. 700 It is easy to obtain phosphor powder with a content of 10% or less. The time for the acid treatment (immersion time) is preferably from 15 minutes to 80 minutes, and more preferably from 15 minutes to 60 minutes. After the acid treatment, the phosphor powder is preferably thoroughly washed with water and dried.
[0051] (5) Classification process In order to reduce the amount of fine powder (too fine phosphor particles that tend to reduce the blue light conversion efficiency) in the powder, it is preferable to carry out an appropriate classification process. In order to effectively remove the fine powder, the classification method is preferably sedimentation classification as described below.
[0052] First, the powder obtained in the (3) pulverization step of the fired product, or the powder that has been subjected to the (4) acid treatment step, is dispersed in an appropriate liquid, such as an aqueous solution of sodium hexametaphosphate, to prepare a dispersion. Next, the dispersion is left to stand for a certain period of time to allow the powders in the dispersion that have relatively large particle sizes to settle. The supernatant is then drained. Thereafter, a new aqueous solution of sodium hexametaphosphate is added to the container in which the precipitate remains, the powder is dispersed, the container is left to stand, and the supernatant liquid is discharged. This operation is repeated several times. The term "several times" refers to preferably 5 times or more. There is no particular upper limit to the number of times, but from the viewpoint of cost, etc., it is, for example, 15 times or less, specifically 10 times or less.
[0053] Classification can reduce the amount of fines in the powder (phosphor particles that are too fine, which tend to reduce the blue light conversion efficiency). 700 The fact that the content of the fine powder in the phosphor powder is less than 10% may be related to the small amount of fine powder in the phosphor powder.
[0054] The specific conditions for classification are finally A 700 There are no particular limitations as long as a phosphor powder having a particle size of 10% or less can be obtained. As a guideline, it is preferable to set the classification conditions so that fine powder having a particle size of 10 μm or less is removed, and it is more preferable to set the classification conditions so that fine powder having a particle size of 7.5 μm or less is removed. In the case of sedimentation classification, the conditions can be set with reference to Stokes' equation, which relates to the sedimentation velocity of particles.
[0055] <Light-emitting device, image display device, and lighting device> A light emitting device can be obtained by combining the phosphor powder of this embodiment with a light source. The luminescent light source typically emits ultraviolet or visible light. For example, when the luminescent light source is a blue LED, the blue light emitted from the luminescent light source hits the phosphor powder, and the blue light is converted into light with a longer wavelength. That is, the phosphor powder of the present embodiment can be used as a wavelength conversion material that converts blue light into light with a longer wavelength.
[0056] An example of a specific configuration of the light emitting device will be described with reference to FIG. 1 is a schematic cross-sectional view showing an example of the structure of a light emitting device. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, a bonding wire 170, a bonding wire 172, and a composite 40.
[0057] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. By mounting the light emitting element 120 on the heat sink 130, it is possible to improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.
[0058] The light emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm to 500 nm, which corresponds to near ultraviolet to blue light, can be used as the light emitting element 120. One electrode (not shown) disposed on the upper surface side of the light emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.
[0059] A generally funnel-shaped recess whose hole diameter gradually increases from the bottom surface toward the top is formed in the case 140. The light emitting element 120 is provided on the bottom surface of the recess. The wall surface of the recess surrounding the light emitting element 120 serves as a reflector.
[0060] The composite 40 is filled in the recess whose wall is formed by the case 140. The composite 40 is a wavelength conversion member that converts the excitation light emitted from the light emitting element 120 into light with a longer wavelength. The composite 40 is obtained by dispersing at least the phosphor powder of this embodiment in an encapsulant 30 such as a resin. In order to obtain white light of higher quality, the encapsulant 30 may contain not only the phosphor powder of this embodiment but also other phosphor powders. The light emitting device 100 emits a mixed color of light from the light emitting element 120 and light emitted from the phosphor particles 1 which are excited by absorbing the light emitted from the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light from the light emitting element 120 and the light generated from the phosphor particles 1.
[0061] Incidentally, although a surface mount type light emitting device is illustrated in FIG. 1, the light emitting device is not limited to the surface mount type, and may be a bullet type, a COB (chip on board) type, or a CSP (chip scale package) type.
[0062] The light emitting device can be used in image display devices such as displays, and lighting devices. For example, a liquid crystal display can be manufactured using the light emitting device 100 as a backlight. Also, a lighting device can be manufactured using one or more light emitting devices 100 and providing appropriate wiring.
[0063] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. General formula M x (Si,Al) 2 (N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, Light absorptance A at a wavelength of 700 nm 700 The phosphor powder has a content of 10% or less. 2. 1. The phosphor powder according to claim 1, The light absorption rate at a wavelength of 600 nm is A 600 (%), A 600 -A 700 The phosphor powder has a content of 6% or more and 10% or less. 3. 1. or 2. The phosphor powder according to claim 1, Volume-based cumulative 50% diameter D measured by laser diffraction scattering method 50 The phosphor powder has a size of 8 μm or more and 25 μm or less. 4. The phosphor powder according to any one of 1. to 3., Volume-based cumulative 10% diameter D measured by laser diffraction scattering method 10 The phosphor powder has a particle size of 5 μm or more and 12 μm or less. 5. A light emitting device comprising the phosphor powder according to any one of 1. to 4. and a light source. 6. 5. The light-emitting device according to claim 5, A light-emitting device in which a light-emitting source emits ultraviolet or visible light. 7. An image display device comprising the light emitting device according to 5. or 6. 8. 5. An illumination device comprising the light-emitting device according to 5. or 6. EXAMPLES
[0064] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.
[0065] <Production of phosphor powder> Example 1 (1) Preparation of raw material mixture First, premixing was performed. Specifically, among the raw materials listed in Table 1, Si3N4, AlN, and CeO2 were mixed (dry blended) for 30 minutes using a small V-type mixer, and then sieved through a nylon sieve with 150 μm openings. This resulted in a premixed powder. Next, in a glove box with a nitrogen atmosphere, the remaining raw materials (Ca3N2 and Li3N) shown in Table 1 were added to the premixed powder, thoroughly dry-blended, and then sieved through a sieve with 500 μm openings to obtain a raw material mixed powder.
[0066] (2) Firing The raw material powder mixture was packed into a boron nitride container, which was then placed in a furnace and sintered at 1800°C for 8 hours in a N2 atmosphere of 0.72 MPa·G.
[0067] (3) Grinding of the fired product The fired product obtained in (2) was pulverized using a stamp mill. The pulverization using the stamp mill was repeated until the passing rate of the product through a vibrating sieve with an opening of 250 μm exceeded 90%. The fired product that had been pulverized by the stamp mill was further pulverized by a jet mill (PJM-80SP, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) under the following pulverization conditions: sample supply rate: 50 g / min, pulverization air pressure: 0.3 MPa.
[0068] (4) Acid treatment The pulverized fired product was put into hydrochloric acid for acid treatment. Specifically, first, 35-37% by mass hydrochloric acid and distilled water were mixed in a volume ratio of 50 mL:300 mL to prepare an aqueous hydrochloric acid solution heated to 80° C. The fired product pulverized in (3) was added to this aqueous hydrochloric acid solution and stirred for 0.5 hours for acid treatment. The acid-treated fired product was thoroughly washed with distilled water and then dried at 110° C. for 3 hours. Then, it was passed through a sieve with 45 μm openings to remove coarse / agglomerated particles.
[0069] (5) Removal of fine particles by sedimentation classification First, a 0.05% by mass aqueous solution of sodium hexametaphosphate was prepared, and this aqueous solution was poured into a container having an inner diameter of 70 mm and a height of 120 mm to a height of 110 mm. Next, the acid-treated fired material was placed in a container containing the above aqueous solution, thoroughly stirred to disperse it, and then left to stand for 22 minutes. After leaving it to stand, the supernatant liquid was removed from the top by 90 mm. Then, an aqueous solution of sodium hexametaphosphate was added to a height of 110 mm, and the powder was again dispersed by stirring, and the same process was carried out. This operation was repeated seven times to remove the fine powder contained in the acid-treated powder. (Incidentally, the classification point is 7.5 μm based on Stokes' law.) Thereafter, the slurry at the bottom of the container was filtered while being washed with water to recover the solid matter, which was then dried at 110° C. for 3 hours and passed through a sieve with 45 μm openings to break down the agglomerated particles. In this manner, a phosphor powder was obtained.
[0070] Example 2 A phosphor powder was obtained in the same manner as in Example 1, except that the sedimentation classification was not carried out.
[0071] Example 3 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials used were those listed in Table 1, (b) no acid treatment was performed (the fired material pulverized in a jet mill was subjected to sedimentation classification without acid treatment), and (c) the pulverization air pressure in the jet mill pulverization was set to 0.6 MPa.
[0072] Example 4 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials shown in Table 1 were used, and (b) the sedimentation classification was not carried out.
[0073] Example 5 A phosphor powder was obtained in the same manner as in Example 4, except that in the acid treatment, nitric acid with a concentration of 60 mass % was used instead of hydrochloric acid.
[0074] Example 6 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials listed in Table 1 were used, and (b) acid treatment was not performed (the fired material pulverized in a jet mill was subjected to sedimentation classification without acid treatment).
[0075] Comparative Example 1 A phosphor powder was obtained in the same manner as in Example 4, except that the acid treatment was not carried out.
[0076] Example 7 A phosphor powder was obtained in the same manner as in Example 1, except that (a) the raw materials listed in Table 1 were used, (b) acid treatment was not performed (the fired material pulverized by the jet mill was subjected to sedimentation classification without acid treatment), and (c) the fired material pulverized by the jet mill was passed through a sieve with a mesh size of 45 μm to remove coarse / agglomerated particles, and then subjected to sedimentation classification.
[0077] <Confirmation of chemical composition / crystal structure> The composition of some of the phosphor powders was analyzed as follows. Amounts of Ca, Li, Ce, Si and Al: The phosphor powder was dissolved by an alkali fusion method, and then the amounts were measured using an ICP emission spectrometer (CIROS-120, manufactured by Rigaku Corporation). Amounts of O and N: Measured using an oxygen / nitrogen analyzer (HORIBA, EMGA-920). Based on the measurement results, the general formula M x (Si,Al)2(N,O) 3±y The x, y, Si / Al atomic ratio, O / N atomic ratio, Li ratio of M, and Ce ratio of M were determined. The impurity elements Cr and Fe were measured by dissolving the phosphor powder in a mixed acid of hydrofluoric acid and nitric acid by pressure acid decomposition, and then measuring the impurity elements by an ICP emission spectrometer.
[0078] For the phosphor of Example 1, powder X-ray diffraction (XRD) measurement was also performed using Cu-Kα radiation using an X-ray diffractometer (Ultima IV-N manufactured by Rigaku Corporation). The obtained XRD pattern is shown in Figure 2. Analysis of the obtained XRD pattern confirmed that the main phase was an orthorhombic crystal with lattice constants a = 0.9486 nm, b = 0.5586 nm, and c = 0.4933 nm, and that a small amount of LiAlSi2N4 was present as a heterophase.
[0079] Incidentally, the mixing ratio of the raw materials was the same in all of the examples 3, 4, and 5, and the manufacturing process up to the pulverization of the fired material was the same in all of these examples. From these facts, it is considered that the chemical composition of the phosphor powder in Examples 4 and 5 is almost the same as that of the phosphor powder in Example 3, and therefore the chemical composition of the phosphor powder in Examples 4 and 5 was not measured.
[0080] <Measurement of light absorptance at a wavelength of 700 nm> The light absorptance of each phosphor powder at a wavelength of 700 nm was determined by the following procedure using a spectrophotometer equipped with an integrating sphere (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.). (1) A standard reflector (Spectralon, manufactured by Labsphere) with a reflectance of 99% was attached to a predetermined position (sample part) in the integrating sphere, and monochromatic light with a wavelength of 700 nm from a light emission source (Xe lamp) was irradiated onto the standard reflector. Then, the number of photons (Qex) of the excitation light was calculated in the wavelength range of 695 to 710 nm. (2) The number of excited reflected photons (Qref) of the sample was calculated in the same manner as in (1) except that the standard reflector was replaced with a measurement sample. The measurement sample was prepared by filling the hollow of a concave cell with phosphor powder so that the surface was smooth. (3) According to the formula (Qex-Qref) / Qex, the light absorption rate A at a wavelength of 700 nm is 700 was calculated.
[0081] <Measurement of light absorption at a wavelength of 600 nm> Using a spectrophotometer equipped with an integrating sphere (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.), the light absorptance of each phosphor powder at a wavelength of 600 nm was determined according to the following procedure. (1) A standard reflector (Spectralon, manufactured by Labsphere) with a reflectance of 99% was attached to a predetermined position (sample part) in the integrating sphere, and monochromatic light with a wavelength of 600 nm from a light emission source (Xe lamp) was irradiated onto the standard reflector. Then, the number of photons (Qex) of the excitation light was calculated in the wavelength range of 595 to 610 nm. (2) The number of excited reflected photons (Qref) of the sample was calculated in the same manner as in (1) except that the standard reflector was replaced with a measurement sample. The measurement sample was prepared by filling the hollow of a concave cell with phosphor powder so that the surface was smooth. (3) According to the formula (Qex-Qref) / Qex, the light absorption rate A at a wavelength of 600 nm is 600 was calculated.
[0082] <Measurement of particle size distribution> The particle size distribution was measured by a laser diffraction scattering method in accordance with JIS R 1629: 1997 using an LS13 320 (manufactured by Beckman Coulter, Inc.) Water was used as the measurement solvent. Specifically, a small amount of phosphor powder was first added to an aqueous solution containing 0.05% by mass of sodium hexametaphosphate as a dispersant. Next, a dispersion was prepared by dispersing the powder using a horn-type ultrasonic homogenizer (output: 300 W, horn diameter: 26 mm). The particle size distribution was measured using this dispersion. The 10% volume diameter (D 10 ), 50% volume diameter (D 50 ) and 90% volume diameter (D 90 ) was sought.
[0083] <Evaluation> (Fluorescence peak intensity) The fluorescence spectrum of the phosphor powder was measured using a spectrofluorophotometer (Hitachi High-Tech Science, F-7000) corrected with Rhodamine B and a secondary standard light source. Specifically, the fluorescence spectrum emitted by exciting the phosphor powder with monochromatic light of 455 nm was measured, and the fluorescence peak intensity and fluorescence peak wavelength were obtained. The fluorescence peak intensity varies depending on the measurement device and conditions. The fluorescence peak intensity shown in the table below is a value when the fluorescence peak intensity of a standard sample (YAG, more specifically, P46Y3 manufactured by Mitsubishi Chemical Corporation) is set to 100.
[0084] (Internal and external quantum yields) The internal quantum efficiency and external quantum efficiency of each phosphor powder were determined using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.) according to the following procedure. (1) The phosphor powder was filled into the recess of the concave cell so that the surface was smooth. This concave cell was attached to a predetermined position (sample part) in the integrating sphere. Monochromatic light, which was split into a wavelength of 455 nm from a light source (Xe lamp), was introduced into the integrating sphere using an optical fiber. This monochromatic light (excitation light) was irradiated onto the phosphor powder filled into the recess of the concave cell, and the fluorescence spectrum was measured. From the obtained spectrum data, the peak wavelength was obtained, and the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) were calculated. The number of excitation reflected light photons was calculated in the wavelength range of 450 nm to 465 nm, and the number of fluorescence photons was calculated in the wavelength range of 465 nm to 800 nm. (2) In addition, instead of the concave cell, a standard reflector with a reflectance of 99% (Spectralon, manufactured by Labsphere) was attached to the sample section to measure the spectrum of the excitation light with a wavelength of 455 nm. The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 nm to 465 nm. (3) The internal quantum efficiency and external quantum efficiency were calculated from Qref, Qem, and Qex obtained in (1) and (2) above according to the following formula. Internal quantum efficiency = (Qem / (Qex-Qref)) x 100 External quantum efficiency = (Qem / Qex) x 100
[0085] Various information is summarized in Table 1. In Table 1, "ND" stands for Not Detected.
[0086] In addition, the raw materials listed in the "Raw materials used" column in Table 1 are as follows.
[0087] Ca3N2-1: Ca3N2 manufactured by Taiheiyo Cement Corporation Ca3N2-2: Ca3N2 manufactured by CERAC (now Materion)
[0088] Li3N-1: Li3N manufactured by Materion Li3N-2: Li3N manufactured by CERAC (now Materion) Li3N-3: Li3N manufactured by High Purity Chemical Laboratory
[0089] CeO2-1: CeO2, C grade, manufactured by Shin-Etsu Chemical Co., Ltd.
[0090] Si3N4-1: Si3N4 manufactured by Ube Industries, E10 grade
[0091] AlN-1: Tokuyama AlN, E grade
[0092] [Table 1]
[0093] As shown in Table 1, the general formula M x (Si,Al)2(N,O) 3±y The phosphor particles have a light absorption coefficient A at a wavelength of 700 nm. 700 The phosphor powders (Examples 1 to 7) having a value of 10% or less exhibited good fluorescence peak intensity, internal quantum efficiency and external quantum efficiency. On the other hand, A 700 The phosphor powder having a content of more than 10% (Comparative Example 1) was inferior to Examples 1 to 7 at least in internal quantum efficiency.
[0094] Looking more closely at Table 1, a comparison of Examples 1 to 6 with Example 7 reveals that A 600 -A 700 It can be seen that the relative fluorescence peak intensity, internal quantum efficiency, and external quantum efficiency are increased by keeping the ratio of the luminescence intensity to the fluorescence intensity within the range of 6% to 10%.
[0095] This application claims priority based on Japanese Patent Application No. 2020-189210, filed on November 13, 2020, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]
[0096] 1. Phosphor particles 30 Encapsulating material 40 Complex 100 Light emitting device 120 Light emitting element 130 Heat sink 140 cases 150 First lead frame 160 Second lead frame 170 Bonding Wire 172 Bonding Wire
Claims
1. General formula M x (Si, Al) 2 (N, O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≦x≦0.9, 0.06≦y≦0.36), a part of M is substituted with Ce element, the Si / Al atomic ratio is 1.5 or more and 6 or less, and the O / N atomic ratio is 0 or more and 0.1 or less, 5 to 50 mol % of M is Li, and 0.5 to 10 mol % of M is Ce, Light absorptance A at a wavelength of 700 nm 700 The phosphor powder has a content of 2% or more and 9.2% or less.
2. The phosphor powder according to claim 1 , The light absorption rate at a wavelength of 600 nm is A 600 (%), A 600 -A 700 The phosphor powder has a content of 6% or more and 10% or less.
3. The phosphor powder according to claim 1 or 2, Volume-based cumulative 50% diameter D measured by laser diffraction scattering method 50 The phosphor powder has a particle size of 8 μm or more and 25 μm or less.
4. The phosphor powder according to any one of claims 1 to 3, Volume-based cumulative 10% diameter D measured by laser diffraction scattering method 10 The phosphor powder has a particle size of 5 μm or more and 12 μm or less.
5. A light emitting device comprising the phosphor powder according to any one of claims 1 to 4 and a light source.
6. 6. The light emitting device according to claim 5, A light-emitting device in which a light-emitting source emits ultraviolet or visible light.
7. An image display device comprising the light emitting device according to claim 5 .
8. An illumination device comprising the light-emitting device according to claim 5 or 6.
Citation Information
Patent Citations
Rocking device for cable crane
JP1984069391A
Phosphor, method for producing same, light-emitting device, and image display apparatus
WO2010110457A1
Phosphor, and light-emitting device and use thereof
WO2012067130A1
Phosphor, light-emitting element and lighting device
WO2014077132A1