Manufacturing method of electrolytic iron foil

By controlling electrolytic iron foil manufacturing conditions, high-purity and flexible electrolytic iron foil is produced, addressing the limitations of existing methods and ensuring smoothness and flexibility for applications like battery current collectors.

JP7590616B1Active Publication Date: 2024-11-26TOHO ZINC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024119421
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-26
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Existing methods for manufacturing electrolytic iron foil using an insoluble anode fail to produce high-purity, smooth, and flexible foil with no pinholes or distortions, especially when considering the use of a cathode drum for peeling.

Method used

A method involving precise control of manufacturing conditions such as electrolyte temperature (50-90°C), Fe content (40-200 g/L), pH (2.0-4.0), current density (50-500 A/m²), and impurity levels (≤38 ppm) is employed, using a cathode drum and a soluble anode with a mesh-like insoluble anode case.

Benefits of technology

This method enables the production of high-purity electrolytic iron foil with excellent smoothness and flexibility, suitable for applications like battery current collectors and laminated core materials, while avoiding impurity-related defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590616000001_ABST
    Figure 0007590616000001_ABST
Patent Text Reader

Abstract

An object of the present invention is to provide a method for producing electrolytic iron foil that is high in purity and has excellent smoothness and flexibility. [Solution] The method for producing electrolytic iron foil according to the present invention includes a step of forming electrolytic iron foil F on the surface of the cathode drum 1 by passing a current through the cathode drum 1 and the anode 2, using a cathode drum 1 that rotates while at least a part of it is immersed in an electrolytic solution 3, and an anode 2 that is disposed in the electrolytic solution 3 so as to face the cathode drum 1. The anode 2 includes an insoluble anode case 21 and a soluble raw iron 22 that is placed inside the anode case 21, the temperature of the electrolytic solution 3 is 50 to 90°C, and the Fe in the electrolytic solution 3 is 100% or more. 2+ The content of is 40 to 200 g / L, the pH of the electrolyte 3 is 2.0 to 4.0, and the current density of the current is 50 to 500 A / m 2 It is.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing electrolytic iron foil, and more particularly to a method for producing electrolytic iron foil using a cathode drum as a cathode. [Background technology]

[0002] Electrolytic iron foil not only has excellent mechanical properties such as strength and elongation, but also has the advantage of being cost-effective because it is made from abundant iron. Therefore, electrolytic iron foil has a wide range of applications, such as battery current collectors, battery exterior materials, and laminate core materials, and various research and development efforts have been conducted to date.

[0003] For example, Patent Document 1 proposes a method for producing electrolytic iron foil by using an insoluble anode to perform iron electrodeposition on an electroforming substrate and peeling off the iron electrodeposition layer, in which the ferrous ions, free iron acid, and temperature in the electrolyte are adjusted. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 58-73786 Summary of the Invention [Problem to be solved by the invention]

[0005] Although Patent Document 1 discloses a method using an insoluble anode, the present inventors attempted to produce an electrolytic iron foil with extremely high purity by a method using a soluble anode. The electrolytic iron foil is required to have not only high iron purity but also smoothness such as free from pinholes, distortion, and unevenness. In addition, since the present inventors are considering a manufacturing method using a cathode drum, the electrolytic iron foil is also required to have flexibility so that it can be appropriately peeled off from the cathode drum.

[0006] From this viewpoint, an object of the present invention is to provide a method for producing an electrolytic iron foil having high purity and excellent smoothness and flexibility. [Means for solving the problem]

[0007] As a result of carrying out numerous experiments and studies on electrolytic iron foil, the inventors discovered that in order to achieve high levels of purity, smoothness, and flexibility, it is necessary to specify the manufacturing conditions very precisely, and thus created the present invention.

[0008] The above problems can be solved by the following measures. The method for producing electrolytic iron foil according to the present invention includes a step of forming electrolytic iron foil on a surface of a cathode drum by passing a current through the cathode drum and the anode, the anode comprising an insoluble anode case and a soluble raw iron placed inside the anode case, the temperature of the electrolyte being 50 to 90°C, and the Fe content of the electrolyte being 100% or less. 2+ The content of the electrolyte is 40 to 200 g / L, the pH of the electrolyte is 2.0 to 4.0, and the current density of the current is 50 to 500 A / m 2 It is. The method for producing electrolytic iron foil according to the present invention is characterized by the temperature of the electrolyte, the Fe content of the electrolyte, 2+ By precisely specifying the content of, the pH of the electrolyte, and the current density, it is possible to continuously produce an electrolytic iron foil that is high in purity and has excellent smoothness and flexibility. In the method for producing electrolytic iron foil according to the present invention, the total content of C, P, S, Si, Co, Cu, Mn, and Ni in the electrolytic iron foil is preferably 38 ppm or less. The method for producing electrolytic iron foil according to the present invention specifies the total content of impurities to be equal to or less than a predetermined value, thereby making it possible to more reliably achieve high purity in the produced electrolytic iron foil. In the method for producing an electrolytic iron foil according to the present invention, the temperature of the electrolytic solution is [A]° C., the pH of the electrolytic solution is [B], and the current density of the current is [C] A / m 2The electrolyte solution is then charged to Fe. 2+ When the content is [D] g / L, it is preferable that the value calculated by 2.5A+30B-0.1C+0.05D-190 is 0 or more. The method for producing electrolytic iron foil according to the present invention, in which the value calculated by a predetermined formula is 0 or more, can more reliably produce electrolytic iron foil with high purity and excellent smoothness and flexibility. Effect of the Invention

[0009] According to the method for producing electrolytic iron foil of the present invention, it is possible to produce electrolytic iron foil that is high in purity and has excellent smoothness and flexibility. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram for explaining a method for producing an electrolytic iron foil according to the present embodiment. [Diagram 2] FIG. 1 is a schematic diagram of an anode used when producing an electrolytic iron foil according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] First, the "electrolytic iron foil" manufactured by the manufacturing method of the electrolytic iron foil according to the present embodiment will be described.

[0012] [Electrolytic iron foil] The electrolytic iron foil is an iron foil obtained through an electrolytic iron foil forming process described below, and the iron foil contains impurities other than iron. The electrolytic iron foil can be used for, but is not limited to, battery current collectors, battery exterior materials, and laminated core materials (for power electronics).

[0013] (impurities) The impurities contained in the electrolytic iron foil are impurities that are inevitably mixed in during production, and specific examples thereof include C, P, S, Si, Co, Cu, Mn, and Ni. The total content of these impurities is preferably 38 ppm or less, and more preferably 35 ppm or less. By having the total impurity content of the electrolytic iron foil be equal to or less than a predetermined value, in other words, by having the iron purity of the electrolytic iron foil be high, not only do various properties (mechanical properties and magnetic properties) become excellent, but the movement of dislocations is less likely to be hindered by impurities, so that processability is excellent, and furthermore, rust generation is suppressed. Furthermore, the content of each of the components listed as the above impurities is not particularly limited, but it is preferable that C is 20 ppm or less, and each of the other components is 5 ppm or less. In this specification, 1 ppm is synonymous with 0.0001 wt% (mass%).

[0014] (Thickness) The thickness of the electrolytic iron foil can be, for example, 20 to 200 μm. From the viewpoints of strength and ease of handling during processing, the thickness of the electrolytic iron foil is preferably 50 μm or more. However, it is possible to reduce the thickness of the electrolytic iron foil to 10 μm or less by processing such as rolling.

[0015] [Method of manufacturing electrolytic iron foil according to the present embodiment] Next, a method for producing an electrolytic iron foil according to this embodiment will be described with reference to Figs. The method for producing an electrolytic iron foil according to this embodiment includes an electrolytic iron foil forming step, and may include other steps as appropriate. Each step will now be described in detail.

[0016] (Electrolytic iron foil forming process) As shown in FIG. 1, in the electrolytic iron foil forming process, a current is passed through a cathode drum 1 and an anode 2 to form an electrolytic iron foil F on the surface of the cathode drum 1. In detail, in the electrolytic iron foil forming process, a constant current is applied to the cathode drum 1 and the anode 2, and Fe is discharged from the anode 2. 2+ The ions are dissolved in electrolyte 3, and the Fe 2+ The ions are deposited (electrolytically deposited) on the surface of the cathode drum 1 as electrolytic iron foil F. In addition, from anode 2, Fe 2+ When ions are dissolved, elements with a lower ionization tendency (higher equilibrium potential) than Fe are less likely to dissolve, and when electrolytic iron foil F is deposited on the cathode drum 1, elements with a higher ionization tendency (lower equilibrium potential) than Fe are less likely to precipitate, thereby achieving high purity of the electrolytic iron foil F that is formed.

[0017] (cathode) As shown in FIG. 1, a cathode 1 used in the electrolytic iron foil forming process is a cathode drum 1 having a drum shape (cylindrical shape). If the material of the cathode drum 1 is stainless steel, corrosion may progress due to the components of the electrolyte 3 during long-term use, which may make it difficult to peel the electrolytic iron foil F from the cathode drum 1. In addition, if the material of the cathode drum 1 is stainless steel, the components of the stainless steel may dissolve into the electrolyte 3 and increase the impurities in the electrolytic iron foil F. Therefore, the material of the cathode drum 1 is preferably pure titanium or a titanium alloy, which does not involve such concerns. The width and outer diameter of the cathode drum 1 are not particularly limited, and may be appropriately set according to the required size of the electrolytic iron foil F. In Fig. 1, the cathode drum 1 is partially immersed in the electrolytic solution, but the entire drum may be immersed since it is sufficient that at least the surface on which the electrolytic iron foil F is to be formed is immersed. In Fig. 1, the cathode drum 1 is shown rotating clockwise, but it may also be rotated counterclockwise to pull out the electrolytic iron foil F from the right side of the drum.

[0018] (anode) As shown in FIG. 1, an anode 2 used in the electrolytic iron foil forming process is disposed in an electrolytic solution 3 so as to face a cathode drum 1 . 2, the anode 2 is configured to include an insoluble anode case 21 and a soluble raw iron 22 that is put inside the case 21. The anode case 21 also has a surface facing the cathode drum 1, which allows the raw iron 22 inside the case 21 to be appropriately soluble in the electrolyte 3. 2+The anode 2 (anode case 21) has a mesh-like surface 21a through which ions can be eluted. The anode 2 (anode case 21) is disposed such that the mesh-like surface 21a facing the cathode drum 1 is curved to fit along the lower surface of the cathode drum 1, and the surface 21a is spaced a predetermined distance (for example, 10 to 100 mm) from the lower surface of the cathode drum 1. The raw material iron 22 acts as a soluble anode, and Fe 2+ The raw material of iron from which ions are eluted can be pure iron, iron scrap, etc. On the other hand, the material of the anode case 21 need only be insoluble, but for the same reasons as those for the cathode drum 1, pure titanium or a titanium alloy is preferable. 1 and 2, the anode case 21 is composed of two members, but it may be composed of one member or three or more members. However, the anode case 21 is preferably configured to have an input port 21b that is open at the top so that raw iron 22 consumed during the electrolytic iron foil formation process can be easily input.

[0019] (electrolyte) The electrolyte 3 used in the electrolytic iron foil formation step is a liquid for electrolytic deposition stored in an electrolytic cell 4 . The electrolyte 3 is Fe 2+ Although the liquid composition is not particularly limited as long as it satisfies the above content, it contains an anionic surfactant, for example, sodium dodecyl sulfate, linear alkylbenzene sulfonate, linear alkylnaphthalene sulfonate, etc. The content of the anionic surfactant in the electrolytic solution 3 is preferably 0.1 to 10 g / L, and more preferably 0.5 to 5 g / L. In the electrolytic iron foil forming process, hydrogen generation is a reaction that occurs competitively with the electrodeposition of iron on the cathode. If hydrogen remains on the electrodeposited iron and is insulated by hydrogen bubbles, iron cannot be electrodeposited at that location, and traces of the bubbles remain. To avoid such a situation, the content of the anionic surfactant is preferably equal to or greater than the above-mentioned predetermined value.

[0020] (Electrolyte: Temperature) The temperature of the electrolytic solution 3 is preferably from 50 to 90°C, and more preferably from 50 to 70°C. If the temperature of the electrolyte 3 is less than 50°C, the electrolytic iron foil F formed may become brittle and lose its flexibility. On the other hand, if the temperature of the electrolyte 3 exceeds 90°C, water will evaporate rapidly, which may cause the balance of the iron concentration and pH to be easily lost. In addition, the high temperature of the electrolyte 3 may cause it to be easily oxidized, and the ions Fe in the electrolyte may be easily dissolved. 2+ Fe 3+ This causes iron(III) hydroxide particles to become physically mixed into the electrolytic iron foil, making it prone to causing poor electrodeposition.

[0021] (Electrolyte:Fe 2+ Content of Electrolyte 3 Fe 2+ The content is preferably 40 to 200 g / L. Electrolyte 3 Fe 2+ If the content of Fe in the electrolyte 3 is less than 40 g / L, the amount of impurities in the electrolytic iron foil F may increase, and pinholes may occur. 2+ If the content exceeds 200 g / L, the amount of impurities in the electrolytic iron foil F formed may increase, and distortion may occur.

[0022] (Electrolyte: pH) The pH of the electrolytic solution 3 is preferably 2.0 to 4.0. If the pH of the electrolytic solution 3 is less than 2.0, the electrolytic iron foil F formed may contain a large amount of impurities and may have pinholes or distortion. On the other hand, if the pH of the electrolytic solution 3 is more than 4.0, the electrolytic iron foil F formed may be brittle and easily cracked. The pH can be adjusted by adding hydrochloric acid, sulfuric acid, or the like.

[0023] (current density) The current density of the current passed through the cathode drum 1 and the anode 2 in the electrolytic iron foil forming process is 50 to 500 A / m 2 is preferred. Current density is 50A / m 2If the current density is less than 500 A / m, the productivity is deteriorated. 2 If the temperature exceeds this range, the electrolytic iron foil F formed may contain a large amount of impurities, distortion may occur, and the electrolytic iron foil F formed may become brittle and lose its flexibility.

[0024] (Regarding the prescribed formula for manufacturing conditions) As described above, the method for producing the electrolytic iron foil according to the present embodiment is carried out by adjusting the temperature of the electrolytic solution, the pH of the electrolytic solution, the current density of the electric current, and the Fe content of the electrolytic solution. 2+ The four manufacturing conditions, "content of" and "content of" are very important and need to be precisely controlled. The inventors have found the following by examining the results of numerous experiments. In detail, the temperature of the electrolyte is [A] °C, the pH of the electrolyte is [B], and the current density is [C] A / m 2 The electrolyte Fe 2+ When the content of is [D] g / L, it has been confirmed that when the value calculated by "150{(A-60) / 60}+90{(B-3) / 3}-30{(C-300) / 300}+5{(D-100) / 100}+25", i.e., "2.5A+30B-0.1C+0.05D-190", is 0 or greater, electrolytic iron foil with high purity and excellent smoothness and flexibility can be produced more reliably. The value calculated by the above-mentioned formula is more preferably 0 or more and 100 or less, and further preferably 0 or more and 80 or less. The constants in the above formula are determined based on the results of numerous experiments.

[0025] (Other processes) The method for producing the electrolytic iron foil according to this embodiment may include, after the electrolytic iron foil formation step, a cleaning step for removing surface dirt, a drying step for drying moisture after cleaning, a heat treatment step for removing residual stress and adjusting the crystal structure, a slitting step for cutting to a desired width, and a winding step for recovering the electrolytic iron foil in a roll form as a product.

[0026] As described above, according to the method for producing an electrolytic iron foil according to the present embodiment, the temperature of the electrolyte, the Fe content of the electrolyte, 2+ By precisely specifying the content of, the pH of the electrolyte, and the current density, it is possible to produce an electrolytic iron foil that is high in purity and has excellent smoothness and flexibility. Since the electrolytic iron foil produced is high in purity, it not only has excellent properties (mechanical properties and magnetic properties), but also excellent processability and rust prevention properties. In addition, according to the manufacturing method of the electrolytic iron foil according to the present embodiment, since it is manufactured by an electrolytic method using a cathode drum and soluble raw iron charged into an anode case, it is possible to realize continuous manufacturing of high-purity electrolytic iron foil, and also to avoid the increase in cost due to rolling, compared to rolled iron foil manufactured by rolling. EXAMPLES

[0027] Next, the present invention will be described by way of examples which satisfy the requirements of the present invention and comparative examples which do not.

[0028] [Sample Production] A sample (electrolytic iron foil F) having a thickness of about 100 μm was manufactured using a cathode drum 1, an anode 2, and an electrolyte 3 having the configurations shown in FIGS. The temperature, pH, and iron concentration (Fe 2+ The content of the cathode drum 1 and the current density of the current applied to the anode drum 2 were as shown in Table 1. During the production, the conditions shown in Table 1 were kept approximately constant. The temperature and pH of the electrolyte 3 were measured using a commercially available thermometer and pH meter, and the iron concentration was measured by oxidation-reduction titration using potassium permanganate. The pH of the electrolyte 3 was adjusted by adding hydrochloric acid. The "value calculated by the specified formula" in Table 1 refers to "150{(A-60) / 60}+90{(B-3) / 3}-30{(C-300) / 300}+5{(D-100) / 100}+25, i.e., 2.5A+30B-0.1C+0.05D-190" (A: temperature of the electrolyte (℃), B: pH of the electrolyte, C: current density (A / m 2), D: Fe in the electrolyte 2+ The content of 1,2-dichlorophenyl phosphate (PPP) was 1,2-dichlorophenyl phosphate (PPP

[0029] The conditions other than those shown in Table 1 were as follows, and were the same for each sample. (Cathode drum 1) Material: Pure titanium Outer diameter: 300cm Width: 200cm Rotation speed: Controlled so that the sample thickness is approximately 100 μm (Anode 2) Anode case 21 material: Pure titanium Distance between anode case 21 and cathode drum 1: 5 cm Total circumferential length of anode case 21 (mesh surface 21a): 60 cm (= 30 cm × 2) Width of anode case 21 (mesh surface 21a): 180 cm Raw iron 22: Pure iron Amount of raw iron 22 added: 10kg (Electrolyte 3) Liquid composition: 40-200 g / L of ferrous chloride, 1 g / L of anionic surfactant, and the remainder of the solution is water to obtain the iron concentration shown in Table 1. Agitation: Pump agitation (Electrolytic cell 4) Material: Fiber Reinforced Plastic (FRP)

[0030] (Measurement method) For each sample produced by the above method, the content of each element as an impurity was measured using an EMIA-920V manufactured by Horiba, Ltd., a UV-1900i manufactured by Shimadzu Corporation, and an ICPE-9820 manufactured by Shimadzu Corporation. The measurement results are shown in Table 2.

[0031] (For each evaluation) Regarding "high purity," a sample was rated as "Good (high purity)" when the total content of each element in the above-mentioned measurement results was 38 ppm or less, and a sample was rated as "Poor (not high purity)" when the total content exceeded 38 ppm. Regarding "smoothness," the surface of a sample (5 cm x 5 cm) was visually inspected; if no pinholes, distortions, or unevenness were found, it was rated as "Good (excellent smoothness)," and if pinholes or distortions were found, it was rated as "Pinhole (not excellent smoothness)" or "Distortion (not excellent smoothness)," respectively. Regarding "flexibility," when a sample (length 10 cm, width 19 cm) was peeled off from cathode drum 1, if it was able to be peeled off properly, it was rated as "Good (excellent flexibility)," and if cracks or other problems occurred and it was not possible to recover it as foil, it was rated as "Poor flexibility (poor flexibility)." Table 3 shows the evaluation results.

[0032] [Table 1]

[0033] [Table 2]

[0034] [Table 3]

[0035] (Review of results) Samples 1 to 7 satisfied all of the manufacturing conditions stipulated in the present invention, and therefore were found to be "high purity" and to be excellent in "smoothness" and "flexibility." The details are as follows. Since Sample 1 was produced under the conditions shown in Table 1, there were no nodular electrodeposits caused by impurities, and a smooth electrolytic iron foil was obtained. In sample 2, the temperature of the electrolyte was set lower than in sample 1, resulting in an electrolytic iron foil that was slightly harder, but it was smooth and had no significant difference in the amount of impurities. For sample 3, the current density was set higher and the iron concentration in the electrolyte lower than in sample 1, creating conditions that would cause hydrogen generation to occur in competition with iron electrodeposition. This resulted in a smooth, pinhole-free electrolytic iron foil, and the amount of impurities was also kept low. For sample 4, the pH of the electrolyte was higher and the current density was set significantly lower than for sample 3 to slowly deposit iron, resulting in an electrolytic iron foil with excellent flexibility and relatively few impurities. However, since sample 4 has a slow production speed due to its low current density, it is not suitable for mass production, but it was confirmed that it is effective for small-scale production. For sample 5, the electrolyte temperature was set high, the pH of the electrolyte was set low, and the current density was set high, creating conditions that favored hydrogen generation, which occurs in competition with iron electrodeposition. However, because the electrolyte temperature was maintained at 70°C or higher (and did not fall below 70°C), a smooth electrolytic iron foil with few impurities was obtained. For sample 6, the pH of the electrolyte was set higher than for sample 5, the current density was significantly lower, and the iron concentration in the electrolyte was set higher to slowly deposit iron, but the resulting electrolytic iron foil had fewer impurities (particularly an electrolytic iron foil with a lower amount of C) than sample 4. Like sample 4, sample 6 was confirmed to be effective for small-scale production. For sample 7, the pH of the electrolyte was higher than for samples 5 and 6, the current density was intermediate between the two, and the iron concentration in the electrolyte was set lower, but the resulting electrolytic iron foil was smooth and had fewer impurities. In addition, because the temperature and pH of the electrolyte were higher, the divalent iron ions (Fe 2+ ) is a trivalent iron ion (Fe 3+ ) and is easily generated in the electrolyte as iron hydroxide. Therefore, care must be taken to manage the flow rate (stirring speed) of the electrolyte, as there is a risk of iron hydroxide being physically mixed into the electrolytic iron foil.

[0036] On the other hand, Samples 8 to 12 did not satisfy at least one of the production conditions defined in the present invention, and therefore did not provide favorable results. In sample 8, the temperature and pH of the electrolyte were set lower than in sample 1, and in particular, the pH was below the designated value, so that hydrogen generation, which occurs in competition with iron deposition, became dominant, and many pinholes due to hydrogen generation were observed on the surface of the electrolytic iron foil. In addition, sample 8 contained a large amount of impurities, and was evaluated as not being of high purity. In Sample 9, the current density was set higher than in Sample 1, and because the current density exceeded the specified value, the production speed was faster, but the electrolytic iron foil was warped toward the anode at the end of the cathode drum, resulting in a distorted electrolytic iron foil. In addition, Sample 9 contained a large amount of impurities, and was evaluated as not being of high purity. In Sample 10, the current density and the iron concentration of the electrolyte were set significantly lower than in Sample 8, and both were below the specified values, resulting in numerous pinholes. In addition, Sample 10 contained a large amount of impurities and was evaluated as not being of high purity. In Sample 11, the temperature of the electrolyte was set lower and the pH and iron concentration of the electrolyte were set higher than those of Sample 3. Since the temperature of the electrolyte was below the specified value, the electrolytic iron foil was quite brittle and immediately cracked when an attempt was made to peel it off from the cathode drum, making it impossible to recover the foil. In sample 12, the pH of the electrolyte was the same as in sample 8, but the iron concentration of the electrolyte was set high. However, as in sample 9, the electrolytic iron foil was warped toward the anode at the end of the cathode drum, resulting in a distorted electrolytic iron foil. In addition, sample 12 had a high amount of impurities and was evaluated as not being of high purity. Combining the results of sample 12 and sample 8, it was confirmed that the pH of the electrolyte has a significant impact on each effect.

[0037] Furthermore, as shown in Table 1, Samples 1 to 7, which were able to exhibit the respective effects of the present invention (high purity, smoothness, flexibility), had values ​​calculated by the predetermined formula of 0 or more. On the other hand, Samples 8 to 12, which were unable to exhibit one or more of the respective effects of the present invention, had values ​​calculated by the predetermined formula of less than 0. From the above, it has been found that the specified formula proposed by the inventors is a clear indicator of whether or not each effect of the present invention is achieved, and it has been confirmed that each effect of the present invention is more reliably achieved when the value calculated by the specified formula is 0 or greater. [Explanation of symbols]

[0038] 1 Cathode drum 2 Anode 21 Anode case 21a Mesh surface 21b Inlet 22 Raw Iron 3 Electrolyte 4 Electrolytic cell F Electrolytic iron foil

Claims

1. The method includes a step of forming an electrolytic iron foil on a surface of a cathode drum by passing a current through the cathode drum and the anode, the step including: using a cathode drum that rotates while at least a portion of the cathode drum is immersed in an electrolytic solution; and an anode that is disposed in the electrolytic solution so as to face the cathode drum. The anode comprises an insoluble anode case and a soluble raw iron introduced into the anode case; The temperature of the electrolyte is 50 to 90° C. The Fe in the electrolyte 2+ The content is 40 to 200 g / L, The pH of the electrolyte is 2.0 to 4.0; The current density of the current is 50 to 500 A / m 2 A method for producing electrolytic iron foil.

2. 2. The method for producing an electrolytic iron foil according to claim 1, wherein the total content of C, P, S, Si, Co, Cu, Mn, and Ni in the electrolytic iron foil is 38 ppm or less.

3. The temperature of the electrolytic solution is [A] °C, the pH of the electrolytic solution is [B], and the current density of the current is [C] A / m 2 The Fe of the electrolyte 2+ The method for producing an electrolytic iron foil according to claim 1 or 2, wherein the value calculated by 2.5A + 30B - 0.1C + 0.05D - 190 is 0 or more, when the content of [D] g / L is [D] g / L.

Citation Information

Patent Citations

  • Self-control electrolytic iron foil solution

    CN113481548A

  • Manufacture of electrolytic iron foil

    JP1983073786A

  • Method and device for electrodeposition of iron system

    JP1990236297A

  • Preparation of iron foil through electro- deposition

    JP1993078880A

  • Electrolytic iron foil

    WO2022014668A1