Electret material and method for producing the same
The electret material with a metastable zirconia phase dispersed in an oxide ceramic maintains strong polarization and heat resistance, addressing the limitations of existing piezoelectric materials for high-temperature applications.
Patent Information
- Application Number
- JP2020211648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing piezoelectric materials lack sufficient heat resistance and suffer from polarization relaxation due to viscoelasticity, making them unsuitable for long-term use at high temperatures.
An electret material composed of a first phase of zirconia with a metastable phase dispersed in a second phase of oxide ceramic, where the metastable phase undergoes a phase change during cooling, maintaining strong polarization and high heat resistance.
The material maintains strong polarization and exhibits excellent heat resistance, allowing it to be used at high temperatures effectively.
Smart Images

Figure 0007590862000002 
Figure 0007590862000003 
Figure 0007590862000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an electret material and a method for producing an electret material. [Background technology]
[0002] In some dielectric materials, such as permanent magnets, the dielectric polarization may remain after the electric field disappears. Such materials are called electrets in contrast to magnets, and are used in filters for dust collectors, microphones, etc.
[0003] For example, Patent Document 1 discloses a polymer composite piezoelectric material obtained by converting a compound having a polyimide resin and ferroelectric ceramic particles into an electret. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-287448 Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 discloses that the piezoelectric material can be used for a long period of time even at high temperatures of about 150° C. However, the heat resistance of the piezoelectric material described in Patent Document 1 is still insufficient, and furthermore, the viscoelasticity of the polymer causes relaxation of polarization, making it difficult to maintain polarization for a long period of time.
[0006] The present invention has been made to solve the above problems, and has an object to provide an electret material which has high heat resistance and is less susceptible to relaxation of polarization. [Means for solving the problem]
[0007] The electret material of the present invention is an electret material containing a first phase made of zirconia and a second phase made of an oxide-based ceramic different from the first phase, wherein the first phase is dispersed and scattered in the second phase, and the first phase is characterized in that the crystal system includes a metastable phase that is metastable at room temperature.
[0008] In the electret material of the present invention, the first phase made of zirconia contains a metastable phase whose crystal system is metastable at room temperature. Since the first phase containing the metastable phase is dispersed and scattered in the second phase, the phase change from the metastable phase to the stable phase, which is accompanied by a large volume expansion during the cooling process after sintering, is inhibited, and even when cooled to room temperature, some of the metastable phase remains. As a result, a strong compressive stress is applied and the restoring force of the dipoles is restricted, so that strong polarization tends to remain, making it suitable for use as an electret material. In addition, since it is formed only from ceramic materials that are stable up to high temperatures, it has excellent heat resistance that allows it to be used at high temperatures.
[0009] In the electret material of the present invention, the metastable phase is preferably tetragonal zirconia. When the metastable phase is tetragonal zirconia, the polarization tends to remain strong and it can be suitably used as a material for an electret.
[0010] In the electret material of the present invention, the first phase preferably does not contain a stabilizer. If the first phase does not contain a stabilizer, the volume change from the metastable phase to the stable phase upon cooling after sintering is maximized, maximizing the interaction with the second phase and making it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0011] In the electret material of the present invention, the first phase further contains a stabilizer, and the content of the stabilizer in the first phase is preferably 5 mol % or less. If the content of the stabilizer in the first phase is 5 mol % or less, the volume change from the metastable phase to the stable phase upon cooling after sintering becomes larger, which increases the interaction with the second phase and makes it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0012] In the electret material of the present invention, the content of the zirconia is preferably 5 wt % to 15 wt %. When the zirconia content is 5 wt% or more, it can exert a sufficient polarization effect and act as an electret, and when the zirconia content is 15 wt% or less, it can receive a strong compressive stress from the oxide ceramic and maintain the polarization. The content of zirconia does not take into consideration the weight of the stabilizer.
[0013] In the electret material of the present invention, at least a part of the first phase is present in a flat shape, and it is preferable that the orientation direction of the flat shapes is uniform. By making the first phase flat, it is thought that it becomes easier for the second phase to equally receive stress, making it easier to maintain the metastable phase. In addition, since the orientation direction of the flat shapes is uniform, it can be strongly polarized.
[0014] In the electret material of the present invention, the maximum length of the flat shape is preferably 0.2 μm to 10 μm. When the maximum length of the flat shape is 0.2 μm or more, the direction of the compressive stress from the first phase is aligned, and the restoring force of the dipoles can be more strongly restricted. When the maximum length of the flat shape is 10 μm or less, the internal stress is less likely to concentrate, and destruction due to the interaction between the first phase and the second phase is less likely to occur.
[0015] In the electret material of the present invention, the porosity is preferably 0.01% to 0.5%. When the porosity is 0.5% or less, the compressive stress received from the second phase can be efficiently transmitted to the first phase, and the function as an electret can be further enhanced.
[0016] In the electret material of the present invention, the oxide ceramic preferably contains at least one oxide selected from the group consisting of alumina, mullite, and magnesia. The above ceramic materials are stable up to the temperature range where zirconia becomes an electret, and can continue to bind the dipoles of zirconia during the cooling process after sintering. In addition, since they are unlikely to form a mixture with zirconia, the interface between the first and second phases is clearly formed, making the interaction stronger.
[0017] The method for producing an electret material of the present invention contains a first phase made of zirconia and a second phase made of an oxide-based ceramic different from the first phase, the first phase being dispersed and scattered in the second phase, and the first phase having a metastable phase whose crystal system is metastable at room temperature. The method for producing an electret material includes a mixture preparation step of preparing a mixture of the zirconia, the oxide-based ceramic, and an organic binder, a molding step of molding the mixture into a predetermined shape to produce a molded body, a degreasing step of removing the organic binder from the molded body, and a sintering step of sintering the molded body from which the organic binder has been removed.
[0018] In the method for producing an electret material of the present invention, the electret material is produced so that the first phase contains a metastable phase whose crystal system is metastable at room temperature. In the case of a first phase made of zirconia, the stable phase usually occupies the majority at room temperature, but by dispersing the first phase in the second phase, the phase change from the metastable phase to the stable phase, which is accompanied by a large volume expansion during the cooling process after sintering, is inhibited, and even when cooled to room temperature, some of the metastable phase remains. As a result, a strong compressive stress is applied to the first phase, and the restoring force of the dipoles is restricted, so that the polarization tends to remain strong, and an electret material that can be suitably used as a material for electrets is obtained.
[0019] In the method for producing an electret material of the present invention, the metastable phase is preferably tetragonal zirconia. When the metastable phase is tetragonal zirconia, the polarization tends to remain strong and it can be suitably used as a material for an electret.
[0020] In the method for producing an electret material of the present invention, it is preferable that the zirconia used in the mixture preparation step does not contain a stabilizer. Since zirconia does not contain a stabilizer, the volume change from the metastable phase to the stable phase upon cooling after sintering is maximized, maximizing the interaction with the second phase and making it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0021] In the method for producing an electret material of the present invention, the zirconia used in the mixture preparation step preferably contains a stabilizer, and the content of the stabilizer in the zirconia is preferably 5 mol % or less. By adding a stabilizer to zirconia, the proportion of the metastable phase in the first phase can be increased. On the other hand, if the content of the stabilizer in the first phase exceeds 5 mol%, the ion conduction effect of the stabilizer may reduce polarization.
[0022] In the method for producing an electret material of the present invention, the sintering temperature in the sintering step is preferably 1300°C to 1500°C. If the sintering temperature is 1300℃ or higher, the first phase zirconia, which was monoclinic zirconia in the raw material stage, can be transformed into tetragonal zirconia, which is a metastable phase. Also, since the sintering temperature is 1500℃ or lower, the particles are less likely to become coarse, resulting in a fine structure that is easier to polarize.
[0023] In the method for producing an electret material of the present invention, it is preferable to apply uniaxial pressure to the green body in the molding step or the sintering step. By applying uniaxial pressure to the compact, the orientation direction of the first phase in the compact can be aligned and it can be flattened. This operation allows the production of an electret material in which the first phase can be strongly polarized.
[0024] In the method for producing an electret material of the present invention, the uniaxial pressing is performed in the sintering step, and the surface pressure of the uniaxial pressing is preferably 15 MPa to 150 MPa. By applying uniaxial pressure in the sintering process, the orientation state of the first phase in the compact can be fixed while sintering proceeds, making it possible to obtain an electret material in which the first phase can be strongly polarized. In addition, by sintering under a surface pressure of 15 MPa or more, a strong second phase can be formed that can suppress expansion when the first phase transitions from a metastable phase to a stable phase during cooling after sintering. Furthermore, even if the sintering temperatures of the first and second phases are different, they can be sintered simultaneously at the lower sintering temperature due to the action of pressure.
[0025] In the method for producing an electret material of the present invention, the weight ratio of the zirconia to the total weight of the zirconia and the oxide ceramic in the mixture is preferably 5 wt % to 15 wt %. When the weight percentage of zirconia is 5 wt% or more, it can exert a sufficient polarization effect and act as an electret, and when the weight percentage of zirconia is 15 wt% or less, it can maintain polarization even when subjected to a strong compressive stress from the oxide ceramics. The content of zirconia does not take into consideration the weight of the stabilizer.
[0026] In the method for producing an electret material of the present invention, the oxide ceramic preferably contains at least one oxide selected from the group consisting of alumina, mullite, and magnesia. The above oxide ceramic materials are stable up to the temperature range where zirconia becomes an electret, and can continue to bind the dipoles of zirconia during the cooling process after sintering. In addition, since they are unlikely to form a mixture with zirconia, the interface between the first and second phases is clearly formed, making the interaction stronger. Effect of the Invention
[0027] According to the electret material of the present invention, the first phase made of zirconia contains a metastable phase whose crystal system is metastable at room temperature, so that the polarization is strong and likely to remain, and it can be suitably used as a material for electrets. In addition, since it is formed only of ceramic materials that are stable up to high temperatures, it has excellent heat resistance that allows it to be used at high temperatures. According to the method for producing an electret material of the present invention, the electret material is produced so that the first phase made of zirconia contains a metastable phase whose crystal system is metastable at room temperature, so that the obtained electret material has a strong polarization and is likely to remain, and can be suitably used as a material for electrets. In addition, since it can be formed only from ceramic materials that are stable up to high temperatures, it is possible to obtain an electret material with high heat resistance that can be used at high temperatures. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of the distribution state of the first phase and the second phase in the electret material of the present invention. [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of an example of the electret treatment. [Diagram 3] FIG. 3 is a diagram showing XRD patterns of the electret materials according to Examples 1 and 3 and Comparative Example 1. [Figure 4] FIG. 4 is an SEM photograph of a cross section of the electret material according to Example 1. [Diagram 5] FIG. 5 is an SEM photograph of a cross section of the electret material according to Example 2. [Figure 6] FIG. 6 is an SEM photograph of a cross section of the electret material according to Example 3. [Figure 7] FIG. 7 is a schematic diagram showing an example of a measuring device for measuring the polarization characteristics of an electret material. [Figure 8] FIG. 8 is a chart of the leakage current of the electret material according to Example 1. [Figure 9] FIG. 9 is a chart of the leakage current of the electret material according to Example 2. [Figure 10] FIG. 10 is a chart of the leakage current of the electret material according to Example 3. [Figure 11A] FIG. 11A is a diagram showing the distribution of the surface potential on the surface (+ side) of the electret material according to Example 1. [Figure 11B] FIG. 11B is a diagram showing the distribution of the surface potential on the surface (-side) of the electret material according to Example 1. [Figure 12A] FIG. 12A is a diagram showing the distribution of surface potential on the surface (+ side) of the electret material according to Example 2. [Figure 12B] FIG. 12B is a diagram showing the distribution of the surface potential on the surface (-side) of the electret material according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The electret material and the method for producing the electret material of the present invention will be described in detail below, but the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention. The present invention also includes an appropriate combination of the preferred embodiments of the present invention.
[0030] [Electret materials] The electret material of the present invention is an electret material containing a first phase made of zirconia and a second phase made of an oxide-based ceramic different from the first phase, wherein the first phase is dispersed and scattered in the second phase, and the first phase is characterized in that the crystal system includes a metastable phase that is metastable at room temperature.
[0031] FIG. 1 is a diagram showing a schematic diagram of the distribution state of the first phase and the second phase in the electret material of the present invention. As shown in FIG. 1, the electret material 1 contains a first phase 10 and a second phase 20 . The first phase 10 is dispersed and interspersed within the second phase 20 . Moreover, the first phase 10 contains a metastable phase whose crystal system is metastable at room temperature.
[0032] In a state where the first phase 10 is dispersed and scattered in the second phase 20, the periphery of the first phase 10 is covered with the second phase 20. Therefore, when the electret material is cooled after being heated, the first phase 10 receives a compressive stress from the second phase 20. Since the volume expansion of the first phase 10 is restricted by this compressive stress, the phase transition from the metastable phase to the stable phase, which would result in a volume expansion of about 4%, is prevented, and the metastable phase remains even at room temperature.
[0033] In addition, when specifying the shape of the first phase, the shape is specified by regarding the first phase surrounded by the second phase as one unit, rather than the shape of the zirconia particles or the shape of the crystallites that constitute the first phase.
[0034] The first phase consists of zirconia. Crystal systems of zirconia include monoclinic zirconia, which is a stable phase at room temperature, and tetragonal zirconia and cubic zirconia, which are metastable phases at room temperature.
[0035] The stable phase is monoclinic zirconia. The metastable phase is preferably tetragonal zirconia. Tetragonal zirconia has strong polarization and tends to remain, so if the metastable phase is tetragonal zirconia, it becomes an electret material with excellent polarization characteristics.
[0036] The type of zirconia crystal system can be confirmed by comparing the peak positions in a diffraction pattern obtained by X-ray diffraction (XRD) with those of a known measurement sample.
[0037] When zirconia is heated, the stable phase changes from monoclinic to tetragonal at 1170°C. When the phase changes from monoclinic to tetragonal, a volumetric shrinkage of about 4% occurs, so the first phase that is heated to a temperature of 1170°C or higher rapidly becomes smaller in volume. On the other hand, when cooled, the phase changes from tetragonal to monoclinic, but this is accompanied by a volume expansion of about 4%. In the electret material of the present invention, the first phase made of zirconia is dispersed and scattered in the second phase made of oxide-based ceramics, so that the first and second phases form a composite material. As a result, they exert a mechanical interaction with each other, and the second phase, which is the oxide-based ceramics, exerts a strong restraining force on the first phase, which is the zirconia, restraining the volume expansion and allowing the tetragonal crystals, which are metastable phases, to remain. Furthermore, it is believed that the strong restraining force of the second phase makes it difficult for the dipoles inside the metastable phase to rotate, and therefore strong polarization can be maintained.
[0038] The content of zirconia in the electret material of the present invention is preferably 5 wt % to 15 wt %. When the zirconia content is 5 wt% or more, it can exert a sufficient polarization effect and act as an electret, and when the zirconia content is 15 wt% or less, it can receive a strong compressive stress from the oxide ceramic and maintain the polarization. The content of zirconia does not take into consideration the weight of a stabilizer, which will be described later.
[0039] The first phase may or may not contain a stabilizing agent. The stabilizer contained in zirconia is not particularly limited, but metal oxides can be used. For example, CaO, Y2O3, CeO2, etc. can be used, and zirconia with the addition of CaO is called CaO stabilized zirconia (CSZ), and zirconia with the addition of Y2O3 is called Y2O3 stabilized zirconia (YSZ). Among them, zirconia with the addition of Y2O3 can be used stably even at high temperatures. The above-mentioned polarization effect is not observed in stabilized zirconia that becomes a tetragonal crystal at room temperature due to the addition of the above-mentioned stabilizer, but the above-mentioned polarization effect is observed in partially stabilized zirconia in which a stable phase and a metastable phase are mixed at room temperature due to the addition of the above-mentioned stabilizer, and in zirconia that does not substantially contain a stabilizer. Therefore, the first phase containing partially stabilized zirconia or zirconia that does not substantially contain a stabilizer is subjected to a strong compressive stress from the second phase at or below the phase transition temperature, so that the dipole of the zirconia that constitutes the first phase can be maintained in a fixed state, and an electret with strong residual polarization can be obtained. On the other hand, if the first phase does not contain a stabilizer, the volume change from the metastable phase to the stable phase upon cooling after sintering is maximized, maximizing the interaction with the second phase and making it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0040] When the first phase contains a stabilizer, the content of the stabilizer in the first phase is preferably 5 mol % or less, more preferably 0.5 mol % or less, and even more preferably the first phase is substantially free of stabilizer. If the content of the stabilizer in the first phase is 5 mol% or less, the volume change from the metastable phase to the stable phase during cooling after sintering becomes larger, so that the interaction with the second phase becomes larger and the metastable phase is more likely to remain, so that the electret effect can be strengthened. This effect can be more effectively expressed when Y2O3 is added. Therefore, Y2O3 is particularly preferable as an additive.
[0041] In the electret material of the present invention, at least a part of the first phase preferably exists in a flat shape. Furthermore, it is preferable that the flat shapes are aligned in the same direction. By making the first phase flat, it is thought that it becomes easier for the second phase to equally receive stress, making it easier to maintain the metastable phase. In addition, since the orientation direction of the flat shapes is uniform, it can be strongly polarized. The shape of the first phase 10 shown in Fig. 1 is a flat shape in which the length in the x direction is longer than the length in the y direction. In Fig. 1, the first phase 10 can be said to be oriented along the x direction.
[0042] The maximum length of the flat shape is preferably 0.2 μm to 10 μm. When the maximum length of the flattened region is 0.2 μm or more, the direction of the compressive stress from the first phase is aligned, and the restoring force of the dipoles can be more strongly restrained. When the maximum length of the flattened region is 10 μm or less, the internal stress is less likely to concentrate, and destruction due to the interaction between the first phase and the second phase is less likely to occur. In the electret material 1 shown in FIG. 1, the maximum length of the first phase 10 is the length in the x direction. The maximum length of the flat shape is the maximum value of the major axis of the first phase that can be confirmed within the field of view in an image of a cross section of the electret material observed with an SEM (magnification: 1000 times to 10000 times).
[0043] The second phase is made of an oxide-based ceramic different from that of the first phase. The oxide ceramic preferably contains at least one oxide selected from the group consisting of alumina, mullite and magnesia, and more preferably contains alumina. The oxide ceramic materials mentioned above are stable up to the temperature range where zirconia becomes electret, and can continue to bind the dipoles of zirconia during the cooling process. In addition, since they are unlikely to form a mixture with zirconia, the interface between the first and second phases is clearly formed, making the interaction stronger.
[0044] In the cross section of the electret material of the present invention, the area ratio of the first phase is preferably 3.5% to 10%. When the area ratio of the first phase is 3.5% or more, sufficient polarization is obtained and the material can be suitably used as an electret. When the area ratio of the first phase is 10% or less, the first phase can be maintained in a dispersed and scattered state in the second phase, and the material can be easily subjected to compressive stress by the second phase. The area ratio of the first phase in the cross section of the electret material is determined by the ratio of the total area of the first phase to the total area in the field of view of the cross section of the electret material observed with an SEM (magnification 1000 times to 10000 times).
[0045] In the electret material of the present invention, the porosity is preferably 0.01% to 0.5%. When the porosity is 0.5% or less, the compressive stress received from the second phase can be efficiently transmitted to the first phase, and the function as an electret can be further enhanced. The porosity of the electret material can be adjusted by adjusting the molding pressure when molding the electret material. The higher the molding pressure, the smaller the porosity. The porosity of the ceramic material can be determined from the pore volume and pore size distribution of the ceramic material measured using mercury intrusion porosimetry. The pore volume and pore size distribution of the ceramic material are measured by setting the surface tension and contact angle of mercury to 485 mN / m and 130°, respectively, and injecting mercury at a pressure ranging from atmospheric pressure to 200 MPa.
[0046] The electret material of the present invention can be polarized by subjecting it to an electret treatment. An example of the electret treatment will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the electret treatment. 2, in the electret treatment, a pair of electrodes 30 is formed on the surfaces of the electret material 1 facing each other in the y direction, a voltage is applied under heating, and the material is cooled in this state, thereby polarizing the metastable phase contained in the first phase 10. The direction in which the first phase 10 is polarized is the opposite direction to the direction of the voltage applied to the electret material 1 via the pair of electrodes 30. Polarization occurs at the surfaces of the crystallites of the metastable phase, so that if the first phase 10 has a flat shape and is oriented along the x direction, it can be strongly polarized in the y direction.
[0047] [Method of manufacturing electret material] The method for producing an electret material of the present invention contains a first phase made of zirconia and a second phase made of an oxide-based ceramic different from the first phase, the first phase being dispersed and scattered in the second phase, and the first phase having a metastable phase whose crystal system is metastable at room temperature. The method for producing an electret material includes a mixture preparation step of preparing a mixture of the zirconia, the oxide-based ceramic, and an organic binder, a molding step of molding the mixture into a predetermined shape to produce a molded body, a degreasing step of removing the organic binder from the molded body, and a sintering step of sintering the molded body from which the organic binder has been removed.
[0048] [Mixture preparation process] In the mixture preparation step, a mixture is prepared by mixing zirconia, an oxide-based ceramic different from the zirconia, and an organic binder.
[0049] Zirconia contains a metastable phase whose crystal system is metastable at room temperature. The metastable phase is preferably tetragonal zirconia.
[0050] The zirconia may be free or free of a stabilizer. The stabilizer contained in zirconia is not particularly limited, but metal oxides can be used. For example, CaO, Y2O3, CeO2, etc. can be used. Zirconia with added CaO is called CaO stabilized zirconia (CSZ), and zirconia with added Y2O3 is called Y2O3 stabilized zirconia (YSZ). The above-mentioned polarization effect is not observed in stabilized zirconia that becomes a tetragonal crystal even at room temperature due to the addition of the above-mentioned stabilizer, but the above-mentioned polarization effect is observed in partially stabilized zirconia in which a stable phase and a metastable phase are mixed at room temperature due to the addition of the above-mentioned stabilizer, and in zirconia that does not substantially contain a stabilizer. Therefore, the first phase containing partially stabilized zirconia or zirconia that does not substantially contain a stabilizer is subjected to a strong compressive stress from the second phase at or below the phase transition temperature, so that the dipole of the zirconia that constitutes the first phase can be maintained in a fixed state, and an electret with strong residual polarization can be obtained. On the other hand, if the zirconia does not contain a stabilizer, the volume change from the metastable phase to the stable phase upon cooling after sintering is maximized, maximizing the interaction with the second phase and making it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0051] When the zirconia contains a stabilizer, the content of the stabilizer in the zirconia is preferably 5 mol % or less, more preferably 0.5 mol % or less, and even more preferably contains substantially no stabilizer. If the content of the stabilizer in the zirconia is 5 mol% or less, the volume change from the metastable phase to the stable phase during cooling after sintering becomes larger, which increases the interaction with the second phase and makes it easier to retain the metastable phase, thereby strengthening the electret effect. This effect is more effectively manifested when Y2O3 is added.
[0052] When the first phase containing a stabilizer is formed in the mixture preparation step, it is preferable to use zirconia containing a stabilizer.
[0053] The oxide ceramic preferably contains at least one oxide selected from the group consisting of alumina, mullite and magnesia, and more preferably contains alumina. The above oxide ceramic materials are stable up to the temperature range where zirconia becomes an electret, and can continue to bind the dipoles of zirconia during the cooling process after sintering. In addition, since they are unlikely to form a mixture with zirconia, the interface between the first and second phases is clearly formed, making the interaction stronger.
[0054] In the method for producing an electret material of the present invention, the weight ratio of the zirconia to the total weight of the zirconia and the oxide ceramic in the mixture is preferably 5 wt % to 15 wt %. When the weight percentage of zirconia is 5 wt% or more, it can exert a sufficient polarization effect and act as an electret, and when the weight percentage of zirconia is 15 wt% or less, it can maintain polarization even when subjected to a strong compressive stress from the oxide ceramics.
[0055] Examples of the organic binder include acrylic organic binders such as polymethyl methacrylate, polyvinyl alcohol, and paraffin.
[0056] In addition to the zirconia, oxide ceramics, and organic binder, additives can be added to the mixture as appropriate. Examples of additives include plasticizers, solvents, and dispersants, and can be used as appropriate depending on the properties of the mixture. Examples of the solvent include 1-butanol, toluene, and isopropyl alcohol. Among the above solvents, those that have low solubility in the organic binder (poor solvents) are preferred. In the case of an acrylic organic binder, 1-butanol and the like can be mentioned.
[0057] In the mixture preparation step, partially stabilized zirconia containing a stabilizer may be used, but a two-stage method may be used in which zirconia and a stabilizer are separately prepared and mixed in advance, and then mixed with the raw material of the oxide-based ceramics. In this case, in the first stage of mixing the zirconia and the stabilizer, it is preferable to perform dry mixing that is less likely to cause aggregation so that they are mixed uniformly. On the other hand, it is preferable to mix with the oxide-based ceramics by making them into a paste and then performing wet mixing. By performing the method in this way, it is possible to obtain a structure in which the zirconia and the stabilizer are mixed uniformly and the first phase is dispersed and scattered throughout the second phase.
[0058] Alternatively, the first phase may be precipitated from a mixture in which the first phase and the second phase are uniformly mixed. Specifically, for example, a method can be exemplified in which alumina, which is an oxide ceramic, and zirconia are dispersed in a solution in which an organic binder and a poor solvent are mixed, and as the poor solvent evaporates, the organic binder is precipitated by spinodal decomposition, while promoting the aggregation of zirconia, which has a high affinity with the organic binder. Because the zirconia is aggregated at the raw material stage, a flat first phase is obtained by subsequent molding, which can improve the polarization characteristics.
[0059] [Molding process] In the molding step, the mixture is molded into a predetermined shape to produce a molded body. The shape of the molded product is not particularly limited, and examples thereof include a plate shape, a ring shape, and the like. The plate-shaped molded product may be produced, for example, by laminating sheets obtained by molding the mixture into a sheet shape, or by directly pressing or extruding the mixture into a plate shape. In pressure molding, the zirconia, which corresponds to the first phase, is crushed in the direction of pressure, resulting in a flat shape. In uniaxial pressing, which can be molded into a plate, the material is crushed so that the first phase is oriented along a plane perpendicular to the pressing direction, while in extrusion molding, the first phase is oriented along the extrusion direction.
[0060] In the molding step, it is preferable to apply uniaxial pressure to the molded body. By applying uniaxial pressure to the compact, the orientation direction of the first phase in the compact can be aligned and it can be flattened. This operation allows the production of an electret material in which the first phase can be strongly polarized.
[0061] [Degreasing process] In the degreasing step, the organic binder is removed from the compact. Prior to the degreasing step, the solvent may be dried from the molded body. The debinding step can be carried out, for example, by heating the compact at a temperature of about 1000°C.
[0062] [Sintering process] In the sintering step, the green body from which the organic binder has been removed (also called a degreased body) is sintered. Because the solid-state reaction rate between zirconia and oxide ceramics is extremely slow, the first and second phases are hardly mixed during the sintering process, and a dispersed state of the first phase is formed that corresponds to the agglomerated state of the mixture. Therefore, the sintering process fixes the first phase, zirconia, in a dispersed and scattered state in the second phase, oxide ceramics.
[0063] The sintering temperature in the sintering step is preferably 1300°C to 1500°C. If the sintering temperature is 1300°C or higher, the first phase zirconia, which was monoclinic zirconia in the raw material stage, can be transformed into tetragonal zirconia, which is a metastable phase. Also, if the sintering temperature is 1500°C or lower, the particles are less likely to coarsen, resulting in a fine structure that is more likely to be polarized.
[0064] In the sintering step, it is preferable to apply uniaxial pressure to the compact. In particular, when uniaxial pressure is not applied to the green body in the compacting step, it is preferable to apply uniaxial pressure to the green body in the sintering step. The surface pressure of the uniaxial pressing carried out in the sintering step is preferably 15 MPa to 150 MPa. By applying uniaxial pressure in the sintering process, the orientation state of the first phase in the compact can be fixed while sintering proceeds, making it possible to obtain an electret material in which the first phase can be strongly polarized. In addition, by sintering under a surface pressure of 15 MPa or more, a strong second phase can be formed that can suppress expansion when the first phase transitions from a metastable phase to a stable phase during cooling after sintering. Furthermore, even if the sintering temperatures of the first and second phases are different, they can be sintered simultaneously at the lower sintering temperature due to the action of pressure without excessive particle coarsening.
[0065] The flat first phase can be formed not only during the molding stage but also during the sintering stage. In order to form a flat shape during the sintering stage, hot pressing using a uniaxial mold, SPS, etc. can be used. In addition, by applying pressure at the same time as sintering, the phase transition to the stable phase of zirconia at the phase transition temperature can be suppressed.
[0066] In the method for producing an electret material of the present invention, in the mixture preparation step, the volume ratio of the zirconia to the total volume of the zirconia and the oxide ceramic is preferably 3.5% to 10%. The volume ratio of zirconia is calculated from the mass and true density of each raw material (zirconia and oxide ceramics before mixing) used in the mixture preparation process, and the volume ratio is compared. By setting the volume ratio at the raw material stage, it is possible to obtain a sintered body with the desired volume ratio of the first and second phases, even if raw materials with different true densities are used. EXAMPLES
[0067] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to only the following examples.
[0068] Example 1 (Mixture preparation process) A mixture was obtained by mixing 0.480 parts by weight of alumina, 0.053 parts by weight of zirconia, 0.182 parts by weight of an acrylic organic binder, 0.027 parts by weight of an adipate ester plasticizer (bis(2-ethylhexyl) adipate), 0.008 parts by weight of a plasticizer, FLOWLEN G-700 (a carboxyl group-containing polymer composition), and 0.246 parts by weight of a solvent, 1-butanol, in a ball mill.
[0069] (molding process) The resulting mixture was formed into a sheet by a doctor blade method and dried at 100° C. for 2 hours.
[0070] (Degreasing process) The obtained green body was heated at a temperature of 1000° C. for 1 hour to degrease the green body.
[0071] (Sintering process) The degreased molded body was heated at 1450°C for 3 hours while applying uniaxial pressure at a surface pressure of 40 MPa using a hot press, thereby obtaining the electret material according to Example 1. The shape of the electret material according to Example 1 was a plate shape with a thickness of 1 mm.
[0072] Example 2 An electret material according to Example 2 was obtained in the same manner as in Example 1, except that 0.246 parts by weight of 1-butanol was changed to 0.246 parts by weight of toluene.
[0073] Example 3 An electret material according to Example 3 was obtained in the same manner as in Example 2, except that 0.053 parts by weight of zirconia was changed to 0.053 parts by weight of partially stabilized zirconia (p-YSZ) containing 6 mol % of Y2O3.
[0074] Comparative Example 1 An electret material according to Comparative Example 1 was obtained in the same manner as in Example 1, except that zirconia was not added and the amount of alumina added was changed to 0.533 parts by weight.
[0075] Comparative Example 2 An electret material according to Comparative Example 2 was obtained in the same manner as in Example 1, except that no alumina was added and the amount of zirconia added was changed to 0.533 parts by weight.
[0076] Comparative Example 3 An electret material according to Comparative Example 3 was obtained in the same manner as in Comparative Example 2, except that zirconia was changed to stabilized zirconia (YSZ) containing 10 mol % of Y2O3.
[0077] (Crystalline Measurement) The electret materials according to each of the examples and comparative examples were subjected to X-ray diffraction (XRD) measurement, and the obtained diffraction patterns were compared with those of known compounds to identify the crystal system of the zirconia contained in the electret materials. The results are shown in Table 1. FIG. 3 is a diagram showing XRD patterns of the electret materials according to Examples 1 and 3 and Comparative Example 1.
[0078] (Observation of the dispersion state and shape of the first phase) The cross section of the electret material was observed by SEM to observe the dispersion state of the first phase relative to the second phase and the shape of the first phase. At this time, the orientation direction of the first phase and the maximum length of the first phase were also obtained. The results are shown in Table 1. In addition, SEM photographs of Examples 1 to 3 are shown in Figures 4 to 6. Figure 4 is an SEM photograph of the cross section of the electret material according to Example 1, Figure 5 is an SEM photograph of the cross section of the electret material according to Example 2, and Figure 6 is an SEM photograph of the cross section of the electret material according to Example 3.
[0079] (Leakage current measurement) The electret properties of the electret materials according to each of the examples and comparative examples were measured using a measuring device shown in FIG. FIG. 7 is a schematic diagram showing an example of a measuring device for measuring the polarization characteristics of an electret material. In the measuring device shown in FIG. 7, a pair of Pt electrodes 30a, 30b were provided on the opposing surfaces 1a and 1b of the electret material 1, and while a predetermined voltage (4 kV) was applied to the electret material 1 via the Pt electrodes 30a, 30b, the entire electret material was heated to 900° C. in the muffle furnace 100, and the voltage and the leakage current flowing between the Pt electrodes were monitored. After the temperature reached 900°C, the device was cooled to room temperature while maintaining the voltage application. The occurrence of leakage current was evaluated according to the following criteria. The results are shown in Table 1. In addition, for Examples 1 to 3, leakage current charts are shown in Figures 8 to 10. Figure 8 is a leakage current chart of the electret material according to Example 1, Figure 9 is a leakage current chart of the electret material according to Example 2, and Figure 10 is a leakage current chart of the electret material according to Example 3. From the results of each chart, the peak current characteristics were evaluated according to the following criteria. The results are shown in Table 1. ○: A peak is observed in the leakage current. △: Leakage current occurs, but is not at a peak. ×: No leakage current occurs.
[0080] (Checking the polarization state) The polarization state of the electret according to each example and comparative example was confirmed at different locations using a surface potential meter Model 1344 manufactured by Trek Japan, and the overall polarization state was confirmed. The difference between the maximum value of the surface potential (voltage) of the surface on the positive potential side and the minimum value of the surface potential (voltage) of the surface on the negative potential side was taken as the polarization voltage. The polarization states of the electrets according to Examples 1 and 2 are shown in Figs. 11A, 11B, 12A, and 12B. Fig. 11A is a diagram showing the distribution of the surface potential on the surface (+ side) of the electret material according to Example 1, Fig. 11B is a diagram showing the distribution of the surface potential on the surface (- side) of the electret material according to Example 1, Fig. 12A is a diagram showing the distribution of the surface potential on the surface (+ side) of the electret material according to Example 2, and Fig. 12B is a diagram showing the distribution of the surface potential on the surface (- side) of the electret material according to Example 2. 11A, 11B, 12A, and 12B, the vertical axis indicates the surface potential, and two axes perpendicular to this indicate the position (coordinates) on the electret surface. 11A, 11B, 12A, and 12B, the polarization voltages on the surfaces of the electrets according to Examples 1 and 2 were nonuniform. Although not shown, the polarization voltages on the surfaces of the electrets according to Example 3 were also nonuniform.
[0081] [Table 1]
[0082] In the electret materials according to Examples 1 and 2, the leakage current increased at about 700° C., but as the temperature increased, the leakage current stopped flowing. From the above, it is considered that the electret materials according to Examples 1 and 2 did not function as dielectrics at low temperatures because the dipoles of the electret materials could not rotate, but at around 700°C, the dipoles rotate, allowing current to flow and causing the materials to function as dielectrics. Moreover, the surfaces of the electret materials according to Examples 1 and 2 exhibited polarization voltages of 1061.9 V (maximum value: +959.9 V, minimum value: -102.0 V) and 175.9 V (maximum value: +103.8 V, minimum value: -72.1 V), respectively.
[0083] When comparing Example 1 and Example 2, the polarization in Example 1 was larger, which is believed to be due to the particle shape of the zirconia before the sintering process. 1-butanol was used as the solvent in Example 1. It is believed that because 1-butanol is a poor solvent with low solubility for the organic binder, aggregation of zirconia and the organic binder occurred during the drying process, resulting in flat-shaped zirconia particles. On the other hand, toluene was used as the solvent in Example 2. Because toluene is a good solvent with high solubility for the organic binder, it is believed that the zirconia and the organic binder did not aggregate during the drying process, and flat zirconia particles were not obtained.
[0084] In Example 3, leakage current occurred from about 700° C., and the occurrence of leakage current continued until 900° C. when heating was terminated. On the other hand, slight polarization was observed on the surface of the electret material according to Example 3. From the above, it is considered that in the electret material according to Example 3, the polarization of the first phase was alleviated by the addition of the stabilizer.
[0085] In Comparative Examples 1 and 2, no leakage current occurred. The reason why Comparative Example 1 did not show any leakage current is believed to be because it did not contain zirconia, which acts as a dielectric. The reason why Comparative Example 2 did not show any leakage current is believed to be that the zirconia that serves as the dielectric was not dispersed and scattered throughout the oxide-based ceramics, and therefore there was no means of restraining the volume expansion that occurred when the tetragonal zirconia changed phase to monoclinic zirconia upon cooling. In addition, in Comparative Examples 1 and 2, no polarization was observed on the surface of the electret material.
[0086] Comparative Example 3 was a simple conductor of oxygen ions, and therefore showed leakage current in a certain temperature range but did not show electret properties. [Industrial Applicability]
[0087] Since the electret material of the present invention can maintain polarization even at high temperatures, it can control plasma at high temperatures and collect particles, and can be suitably used as parts for semiconductor manufacturing equipment such as susceptors, plasma etching parts, and dummy wafers. [Explanation of symbols]
[0088] 1 Electret materials 1a, 1b Electret material surface 10 Phase 1 20 Phase 2 30 electrodes 30a, 30b Pt electrode 100 Muffle furnace
Claims
1. An electret material containing a first phase made of zirconia and a second phase made of alumina, The first phase is dispersed and interspersed within the second phase, The first phase includes a metastable phase having a crystal system that is metastable at room temperature, The first phase does not contain a stabilizer or the content of the stabilizer is 5 mol % or less, The electret material has a zirconia content of 5 wt % to 15 wt %.
2. 2. The electret material of claim 1, wherein the metastable phase is tetragonal zirconia.
3. The electret material according to claim 1 or 2, wherein at least a portion of the first phase is present in a flat shape, and the alignment direction of the flat shapes is uniform.
4. The electret material according to claim 3, wherein the maximum length of the flat shape is 0.2 μm to 10 μm.
5. The electret material according to any one of claims 1 to 4, wherein the porosity is 0.01% to 0.5%.
6. A method for producing an electret material comprising: a first phase made of zirconia; and a second phase made of alumina, the first phase being dispersed and scattered in the second phase; and the first phase including a metastable phase having a crystal system that is metastable at room temperature, a mixture preparation step of preparing a mixture by mixing the zirconia, the alumina, and an organic binder; A molding step of forming a molded body by molding the mixture into a predetermined shape; a degreasing step of removing the organic binder from the compact; a sintering step of sintering the molded body from which the organic binder has been removed; It consists of: The zirconia used in the mixture preparation step does not contain a stabilizer or has a stabilizer content of 5 mol% or less; A method for producing an electret material, characterized in that a weight ratio of the zirconia to a total weight of the zirconia and the alumina in the mixture is 5 wt % to 15 wt %.
7. The method for producing an electret material according to claim 6, wherein the metastable phase is tetragonal zirconia.
8. The method for producing an electret material according to claim 6 or 7, wherein the sintering temperature in the sintering step is 1300°C to 1500°C.
9. The method for producing an electret material according to any one of claims 6 to 8, wherein uniaxial pressure is applied to the green body in the molding step or the sintering step.
10. The uniaxial pressing is performed in the sintering step, The method for producing an electret material according to claim 9, wherein the surface pressure of the uniaxial press is 15 MPa to 150 MPa.
Citation Information
Patent Citations
massager
JP1984025748A
Alumina-zirconia compounded sintered material
JP1991223159A
High molecular composite piezoelectric material and its production
JP1994287448A
Production of ceramics sintered compact
JP1995291722A
Electret and electrostatic induction type conversion device
JP2009253050A