Stretch sheet for absorbent articles and manufacturing method thereof
The elastic sheet for absorbent articles addresses breathability and stability issues by bonding non-stretched filaments to a nonwoven fabric with a roughened surface, improving air permeability and storage stability through a manufacturing method that prevents filament entanglement.
Patent Information
- Application Number
- JP2021019323
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-09
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-02-09
AI Technical Summary
Existing elastic sheets for absorbent articles face issues with breathability, blocking resistance, and storage stability due to the entanglement and adhesion of exposed elastic filaments during manufacturing and use.
A stretchable absorbent article is designed with non-stretched elastic filaments bonded to a nonwoven fabric without intersecting, where the exposed portion of the elastic filaments is coated with a roughened surface to reduce stickiness and improve handling, and a manufacturing method involves spinning elastic filaments onto a nonwoven fabric before solidification to prevent entanglement.
The solution enhances air permeability, blocking resistance, and storage stability by minimizing filament entanglement and adhesion, resulting in a more efficient and stable manufacturing process.
Smart Images

Figure 0007590883000002 
Figure 0007590883000003 
Figure 0007590883000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretch sheet for absorbent articles and a method for producing the same. [Background technology]
[0002] From the viewpoint of fitting absorbent articles such as diapers to the body, a stretchable sheet member formed by joining an elastic member such as rubber thread between two sheets is used as a constituent member of the absorbent article. For example, Patent Document 1 describes an example of such a sheet member, which is a stretch sheet having a structure in which a plurality of elastic filaments in a non-stretched state, which are arranged so as to extend in one direction without intersecting with each other, are sandwiched between two stretchable nonwoven fabrics.
[0003] Also, a technique is known in which particles are attached to the surface of a fiber to impart various properties to the fiber. For example, Patent Document 2 describes a nonwoven fabric containing constituent fibers in which a plurality of hydrophobic particles are fixed to the surface of the fiber, and a plurality of protrusions caused by the particles protrude from the surface of the fiber. The nonwoven fabric described in Patent Document 2 is difficult to sense wetness even when wet, and is said to be useful as a member located farthest from the wearer's skin in an absorbent article.
[0004] Patent Document 3 describes a core-sheath composite elastic filament having elasticity, in which a large number of circumferentially raised ridges are arranged in the fiber axis direction and the filament has a rough surface. The composite elastic filament described in Patent Document 3 has a small coefficient of friction on the surface, and it is said that clothing that comes into direct contact with the skin, such as stockings, made using the filament adheres closely to the skin due to its elasticity, but does not feel slimy like polyurethane elastic threads and provides a comfortable fit. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-30182 A [Patent Document 2] JP 2016-108714 A [Patent Document 3] International Publication No. 1992 / 000408 Summary of the Invention [Problem to be solved by the invention]
[0006] The stretch sheet described in Patent Document 1, when used as a material for forming various worn articles including absorbent articles, exhibits excellent fitting due to the action of the elastic filaments and can effectively prevent the worn article from slipping down, but in particular, a stretch sheet configured with elastic filaments interposed between two nonwoven fabrics has room for improvement in terms of breathability, since it is configured with multiple nonwoven fabrics laminated together, even though the nonwoven fabric alone has a relatively small airflow resistance. Therefore, as an improvement technique for a stretch sheet with such a configuration, a configuration in which multiple elastic filaments are bonded to one side of a single nonwoven fabric in a state where they are exposed, is considered. However, when a stretch sheet having such exposed elastic filaments is produced, the molten or softened elastic filaments spun from the spinning nozzle come into contact with one of a pair of rolls that take up the elastic filaments together with the nonwoven fabric and clamp them together, and this can cause the elastic filaments to become entangled by the one roll, resulting in problems such as not being able to achieve the designed quality or contaminating the production equipment.In addition, after production, the exposed elastic filaments become sticky, which can easily cause so-called blocking, leaving room for improvement in terms of handling and storage stability.
[0007] An object of the present invention is to provide a stretch sheet for absorbent articles which has excellent breathability, blocking resistance and storage stability, and a method for producing the same. [Means for solving the problem]
[0008] The present invention is a stretch sheet for absorbent articles, comprising a plurality of unstretched elastic filaments arranged so as to extend in one direction without crossing each other and bonded by fusion to one side of an extensible nonwoven fabric. In one embodiment of the stretch sheet for absorbent articles of the present invention, the portions of the elastic filaments other than the fused portions with the nonwoven fabric are exposed, and the surfaces of the exposed portions of the elastic filaments are provided with roughness due to the unevenness of the elastic filaments themselves.
[0009] The present invention also relates to a method for producing a stretch sheet for absorbent articles, in which a plurality of unstretched elastic filaments are bonded in an exposed state to one side of an extensible nonwoven fabric, the filaments being arranged so as to extend in one direction without crossing each other. One embodiment of the manufacturing method of a stretch sheet for absorbent articles of the present invention includes a composite nonwoven fabric manufacturing step in which a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are brought into contact with one side of an original nonwoven fabric before the elastic filaments solidify, to obtain a composite nonwoven fabric in which the elastic filaments are fused and exposed on one side of the original nonwoven fabric. One embodiment of the method for producing a stretch sheet for absorbent articles of the present invention includes a surface roughening step of forming irregularities on the surfaces of the elastic filaments in the areas that are not in contact with the original nonwoven fabric. One embodiment of the method for producing a stretch sheet for absorbent articles of the present invention includes a step of stretching the composite nonwoven fabric.
[0010] Another embodiment of the method for producing a stretch sheet for absorbent articles of the present invention includes the steps of: contacting a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles with one side of an original nonwoven fabric before the elastic filaments are solidified to obtain a composite nonwoven fabric in which the elastic filaments are fused to one side of the original nonwoven fabric; and contacting a release sheet with the portions of the surfaces of the elastic filaments that are not in contact with the original nonwoven fabric to obtain a laminated sheet in which the elastic filaments are interposed between the original nonwoven fabric and the release sheet. removing the release sheet from the laminate sheet; and stretching the composite nonwoven fabric. In another embodiment of the method for producing a stretch sheet for absorbent articles of the present invention, the release sheet is mainly made of a material that does not melt or thermally decompose at 200°C. Other features, advantages and embodiments of the present invention are described below. Effect of the Invention
[0011] According to the present invention, there is provided a stretch sheet for absorbent articles that has excellent breathability, blocking resistance, and excellent storage stability. Furthermore, according to the manufacturing method of the stretch sheet for absorbent articles of the present invention, the stretch sheet for absorbent articles can be efficiently manufactured. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view showing one embodiment of a stretch sheet for absorbent articles according to the present invention. [Diagram 2] FIG. 2 is an electron microscope photograph (observation magnification: 150 times) of an elastic filament and its vicinity in one embodiment of the stretch sheet for absorbent articles of the present invention. [Diagram 3] FIG. 3 is a perspective view that illustrates an example of a composite nonwoven fabric manufacturing process in the method of manufacturing a stretch sheet for absorbent articles of the present invention. [Figure 4] FIG. 4 is a perspective view that illustrates an example of a stretching step in the method of producing a stretch sheet for absorbent articles of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing an example of a surface roughening step in the manufacturing method of a stretch sheet for absorbent articles of the present invention, and is a schematic cross-sectional view along the radial direction of a pair of rolls to which elastic filaments in a molten or softened state are supplied. [Figure 6] FIG. 6 is a view corresponding to FIG. 5, showing another example of the surface roughening step in the manufacturing method of the stretch sheet for absorbent articles of the present invention. [Figure 7] FIG. 7 is a diagram corresponding to FIG. 5 showing an example of a step for obtaining a laminated sheet in one embodiment of the method for producing a stretch sheet for absorbent articles of the present invention. [Figure 8]FIG. 8 is a view corresponding to FIG. 5 showing another example of the step of obtaining a laminated sheet in one embodiment of the method for producing a stretch sheet for absorbent articles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described below based on preferred embodiments with reference to the drawings. In the following description of the drawings, the same or similar parts are denoted by the same or similar reference numerals. The drawings are basically schematic, and the ratio of each dimension may differ from the actual one.
[0014] Figure 1 shows a stretch sheet 1, which is one embodiment of the stretch sheet for absorbent articles of the present invention. The stretch sheet 1 is composed of a plurality of elastic filaments 3 in an unstretched state, arranged so as to extend in one direction without intersecting each other, and bonded by fusion to one side of an extensible nonwoven fabric 2.
[0015] The stretch sheet 1 of this embodiment has a longitudinal direction X and a width direction Y perpendicular to the longitudinal direction X. The longitudinal direction X coincides with the flow direction during production of the stretch sheet 1, that is, the so-called machine direction (hereinafter also referred to as "MD"), and the width direction Y coincides with a cross direction (CD) perpendicular to the MD.
[0016] The nonwoven fabric 2 has extensibility. In this embodiment, the nonwoven fabric 2 is extensible in the direction in which the elastic filaments 3 extend (longitudinal direction X). Specifically, for example, a "nonwoven fabric having extensibility" means that the nonwoven fabric has an extensibility rate (change in length) of 30% or more as measured by the method described below. The extensibility rate of the nonwoven fabric 2 is not particularly limited, but from the viewpoint of improving the stretchability of the stretch sheet 1, it is preferably 100% or more and 300% or less.
[0017] <Method of measuring elongation rate> Two marks extending in the width direction are made on the stretch sheet 1 to be measured, spaced 1 cm apart in the longitudinal direction, and the elastic filaments 3 are removed from the stretch sheet 1. A rectangular shape in plan view, measuring 2 cm in the longitudinal direction and 1 cm in width, including the two marks, is cut out from the remaining nonwoven fabric 2 to prepare a test piece. In preparing such a test piece, the elastic filaments 3 are removed from the stretch sheet 1 by using an organic solvent in which the nonwoven fabric 2 is insoluble and only the elastic filaments 3 is soluble, and then the nonwoven fabric 2 is naturally dried after dissolving only the elastic filaments 3. For example, when the elastic filaments 3 are made of a styrene-based block copolymer of a thermoplastic elastomer and the nonwoven fabric 2 is made of polypropylene, toluene can be used as the organic solvent. The longitudinal direction of the test piece is aligned with the tensile direction, and the two marks on the test piece are attached to the chucks of a tensile tester (Tensilon tensile tester, RTM100, manufactured by Orientec Co., Ltd.). At this time, the distance between the chucks is 1 cm. Next, the test piece is pulled to a load of 50 g at a pulling speed of 100 mm / min, and the length of the test piece is measured. Then, the elongation rate is calculated by the following formula. Elongation rate (%) = [{length of test piece after pulling (mm) - length of test piece before pulling (mm)} / length of test piece before pulling (mm) ×] 100
[0018] In addition, when the stretch sheet to be measured is used as a component of another article such as an absorbent article, and the stretch sheet is removed for evaluation and measurement, if the stretch sheet is fixed to the other component by adhesive, fusion, etc., the fixed portion is released by applying an organic solvent to it, blowing cold air from a cold spray, etc., before the stretch sheet is removed. This procedure is common to all measurements in this specification.
[0019] Specific examples of "extensible nonwoven fabrics" include the following (1) and (2). (1) A form in which the constituent fibers of the nonwoven fabric themselves extend. (2) Although the constituent fibers themselves do not stretch, the fibers that were bonded at the intersections become separated, the three-dimensional structure formed by multiple fibers due to bonding between fibers, etc., changes structurally, the constituent fibers are torn, or slack fibers are stretched, causing the nonwoven fabric as a whole to stretch.
[0020] In this embodiment, the nonwoven fabric 2 has the above-mentioned form (2). Specifically, as shown in FIG. 1, the nonwoven fabric 2 has a low basis weight portion (low basis weight portion) 21 and a high basis weight portion (high basis weight portion) 22 in which the material (fiber) forming the nonwoven fabric 2 is more than that of the low basis weight portion 21. The low basis weight portion 21 and the high basis weight portion 22 are alternately arranged in the extension direction (longitudinal direction X) of the elastic filament 3. The low basis weight portion 21 and the high basis weight portion 22 each extend along the width direction Y perpendicular to the extension direction of the elastic filament 3. The low basis weight portion 21 and the high basis weight portion 22 are formed on the nonwoven fabric 2 by a stretchability imparting process described later. The stretchability imparting process provides the nonwoven fabric 2 with extensibility that allows it to be stretched along the extension direction (longitudinal direction X) of the elastic filament 3.
[0021] In this embodiment, the multiple elastic filaments 3 each extend continuously and linearly over the entire length of the stretch sheet 1 in the longitudinal direction X. In the present invention, the elastic filaments 3 need not cross each other, and may, for example, extend in one direction while meandering. The elastic filaments 3 are joined to the nonwoven fabric 2 in an unstretched state. The "unstretched state" here refers to the most contracted state when no external force is acting on the elastic filaments 3, and is basically the same as the "natural state."
[0022] The elastic filaments 3 are joined to the nonwoven fabric 2 by fusion. In other words, the elastic filaments 3 and the nonwoven fabric 2 are joined by melting at least one of the resins that make up both of them, and are not joined using an adhesive such as a hot melt adhesive. Therefore, no adhesive is present between the nonwoven fabric 2 and the elastic filaments 3. Here, "no adhesive is present" refers not only to a case where the basis weight of the adhesive is zero, but also strictly speaking to a case where the basis weight of the adhesive is relatively small (for example, 1 g / m2 In terms of improving the bonding strength between the elastic filaments 3 and the nonwoven fabric 2, it is preferable that the elastic filaments 3 are fused to the nonwoven fabric 2 over their entire length.
[0023] The stretch sheet 1 stretches along the direction in which the elastic filaments 3 extend (longitudinal direction X). The stretchability of the stretch sheet 1 is manifested by the elasticity of the elastic filaments 3. "Elastic" means the property of being able to be stretched and contracting when the stretching force is released. When the stretch sheet 1 is stretched along the direction in which the elastic filaments 3 extend, the elastic filaments 3 and the nonwoven fabric 2 extend. When the stretch sheet 1 is released from the stretching, the elastic filaments 3 contract, and the nonwoven fabric 2 returns to its pre-stretch state. In the stretch sheet 1, the elastic filaments 3 do not cross each other, so when the stretch sheet 1 is stretched along the direction in which the elastic filaments 3 extend, the stretch sheet 1 can be stretched with almost no shrinkage in the direction perpendicular to the stretching direction, i.e., so-called width shrinkage.
[0024] The basis weight of the stretch sheet 1 is not particularly limited, but from the viewpoint of improving stretchability, it is preferable to set it as follows. The overall basis weight of the stretch sheet 1 is preferably 10 g / m 2 More preferably, 20 g / m 2 More than 70 g / m 2 Less than 50 g / m 2 The following is the result. The basis weight of the low basis weight portion 21 of the nonwoven fabric 2 is preferably 3 g / m 2 More preferably, 7 g / m 2 and preferably 20 g / m 2 Less than 15g / m 2 The following is the result. The basis weight of the high basis weight portion 23 of the nonwoven fabric 2 is preferably 5 g / m 2 More preferably, 10 g / m2 More than 50 g / m 2 Less than or equal to 30 g / m 2 The following is the result.
[0025] The thickness of the nonwoven fabric 2 is preferably 0.05 mm or more, more preferably 0.1 mm or more, even more preferably 0.15 mm or more, and is preferably 5 mm or less, more preferably 1 mm or less, even more preferably 0.5 mm or less. The thickness of the nonwoven fabric 2 is measured by the following method. A razor is applied to the stretch sheet 1 including the nonwoven fabric 2 to be measured, and the stretch sheet 1 is cut in the thickness direction by hitting the top of the razor with a hammer, etc. The cut stretch sheet 1 is sandwiched between flat plates and a tension of 0.5 cN / cm is applied to the stretch sheet 1. 2 With this load applied, the cross section of the stretch sheet 1 is observed under a microscope at a magnification of 50 to 200 times, and the thickness of the nonwoven fabric 2 is measured within the observed field of view. Measurements are taken at any three points on the cross section of the stretch sheet 1, and the average of these measurements is taken as the thickness of the nonwoven fabric 2.
[0026] The distance between adjacent elastic filaments 3 is preferably 0.4 mm or more, more preferably 0.6 mm or more, and preferably 2 mm or less, more preferably 1 mm or less, and further preferably 1 mm or less. The distance between adjacent elastic filaments 3 can be measured by cutting the stretch sheet 1 containing the elastic filaments 3 to be measured in a direction perpendicular to the extension direction of the elastic filaments 3, observing the cut surface with a microscope at a specified magnification, and measuring the distance between adjacent elastic filaments 3 in the observed field of view. Measurements are performed at 100 arbitrary locations, and the average value is taken as the distance between adjacent elastic filaments 3.
[0027] Examples of the nonwoven fabric 2 include air-through nonwoven fabric, heat-rolled nonwoven fabric, spunlace nonwoven fabric, spunbonded nonwoven fabric, meltblown nonwoven fabric, etc. These nonwoven fabrics may be nonwoven fabrics of continuous filaments or staple fibers. The fibers constituting the nonwoven fabric 2 may be, for example, inelastic fibers made of a substantially inelastic resin, and in that case, the nonwoven fabric 2 may be a stretchable fiber layer mainly made of the inelastic fibers. Examples of such inelastic fibers include fibers made of polyesters such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyamides. The fibers constituting the nonwoven fabric 2 may be short or long fibers, and may be hydrophilic or water-repellent. In addition, core-sheath or side-by-side composite fibers, split fibers, modified cross-section fibers, crimped fibers, heat-shrinkable fibers, and the like may also be used. These fibers may be used alone or in combination of two or more.
[0028] The elastic filament 3 is made of, for example, a thermoplastic elastomer or rubber. In particular, when a thermoplastic elastomer is used as a raw material, it can be melt-spun using an extruder in the same manner as a normal thermoplastic resin, and the elastic filament thus obtained is easy to heat-seal, making it suitable for a stretch sheet. Examples of thermoplastic elastomers include styrene-based elastomers such as SBS (styrene-butadiene-styrene), SIS (styrene-isoprene-styrene), SEBS (styrene-ethylene-butadiene-styrene), and SEPS (styrene-ethylene-propylene-styrene), olefin-based elastomers (ethylene-based α-olefin elastomers, propylene-based elastomers copolymerized with ethylene, butene, octene, etc.), polyester-based elastomers, and polyurethane-based elastomers, and these can be used alone or in combination of two or more. Also, core-sheath or side-by-side composite fibers made of these resins can be used.
[0029] As shown in FIG. 1, the stretch sheet 1 is characterized in that the elastic filaments 3 are exposed at the portions other than the fused portions with the nonwoven fabric 2 . In this embodiment, the stretch sheet 1 comprises a single sheet of nonwoven fabric 2 and a plurality of elastic filaments 3 arranged on one side of the single sheet of nonwoven fabric 2, and the entirety of the elastic filaments 3 is exposed except for the fused portions with the nonwoven fabric 2. Conventional stretch sheets, which have a configuration in which an elastic filament is interposed between two sheets of nonwoven fabric and in which the elastic filament is not exposed, have the problem that the nonwoven fabric tends to provide resistance during extension and contraction, and the inherent elasticity of the elastic filament is not fully utilized, but the stretch sheet 1 has the elastic filament 3 exposed, which ensures that there is a portion that does not restrict the movement accompanying the extension and contraction of the elastic filament 3, thereby resolving this problem. Therefore, the stretch sheet 1 has superior elasticity compared to the conventional stretch sheets described above, and can be stretched, for example, to the extendible length of the nonwoven fabric 2 or to the maximum elongation of the elastic filament 3. Moreover, the stretch sheet 1 has superior breathability because the number of layers of nonwoven fabric that cause airflow resistance is smaller than in conventional stretch sheets in which the elastic filament is not exposed. The stretch sheet 1 can be suitably used as a component of an absorbent article due to its excellent breathability and stretchability. For example, the stretch sheet 1 can be used as an exterior body forming the outer surface of a diaper. When such a diaper is worn, the elastic filaments 3 contract well, so that the diaper fits well to the wearer's body. The stretch sheet 1 used as an exterior body is preferably incorporated into the diaper so that its longitudinal direction X is aligned with the waist circumference direction of the diaper. When such a diaper is put on a wearer, the exterior body stretches well in the waist circumference direction, so that it can be easily opened with little force, which makes it easy to put on.
[0030] Thus, the stretch sheet 1 has excellent breathability and stretchability due to the exposed elastic filaments 3, but on the other hand, due to this, there are inherent problems that are not present in conventional stretch sheets in which elastic filaments are interposed between two sheets of nonwoven fabric. Specifically, the stretch sheet 1 has low blocking resistance due to the exposed elastic filaments 3, which may be sticky, and there are concerns about poor handling and storage stability. For example, in a stretch sheet roll in which a long stretch sheet is wound into a roll, overlapping stretch sheets may adhere to each other via the elastic filaments, which is called blocking, and there is a concern that it may become difficult to unwind the stretch sheet from the roll.
[0031] However, in the stretch sheet 1, the surface of the exposed portion of the elastic filament 3 is roughened due to the unevenness of the elastic filament 3 itself, thereby reducing the stickiness of the elastic filament 3 and resolving problems caused by the exposed elastic filament 3, such as blocking.
[0032] The above-mentioned "roughness caused by the unevenness of the elastic filament itself" refers to the surface of the elastic filament being uneven due to fine scratches on the surface itself, which gives the surface roughness (the surface is not smooth). Therefore, for example, when the surface of an elastic filament, which has a smooth surface without unevenness, is uneven due to the adhesion of a substance other than the elastic filament, such as a fine material described below, it is not said that the surface has "roughness caused by the unevenness of the elastic filament itself."
[0033] FIG. 2 shows an electron microscope photograph of a part of the surface on which the elastic filaments are arranged in a stretch sheet having the same basic structure as the stretch sheet 1. In FIG. 2, the obliquely crossing band-like object is the exposed part of the elastic filament, and the numerous fibrous objects present above and below the exposed part are the constituent fibers of the nonwoven fabric to which the elastic filaments are fused. The irregular white pattern present on the surface of the exposed part of the elastic filament is the "irregularity of the elastic filament itself" and is scattered over the entire surface. Thus, in the stretch sheet shown in FIG. 2, the surface of each exposed part of the multiple elastic filaments is given roughness due to the irregularity of the elastic filament itself.
[0034] In an article such as a product suspected of patent infringement, whether or not the surface of the exposed part of the elastic filament in the stretch sheet of the article is provided with the above-mentioned "roughness due to the unevenness of the elastic filament itself" can be determined by observing the exposed part with an electron microscope. In that case, if an irregular pattern such as that shown in FIG. 2 can be confirmed on the surface of the elastic filament in the captured electron microscope photograph, the article is presumed to satisfy one of the constituent elements of the present invention, that is, "a part of the elastic filament other than the fusion part with the nonwoven fabric is exposed, and the surface of the exposed part of the elastic filament is provided with roughness due to the unevenness of the elastic filament itself." If the stretch sheet to be observed is fixed to another member with an adhesive or the like, the fixation is released by the above-mentioned method, and the stretch sheet is taken out and subjected to electron microscope observation. In addition, if the stretch sheet to be observed is fixed to another member by fusion such as heat sealing, and it is difficult to release the fixation, the part of the stretch sheet other than the fusion part may be observed.
[0035] In addition, when a nonwoven fabric is arranged and fixed on the surface (surface on which the exposed elastic filaments are present) of a "stretch sheet having exposed elastic filaments" such as the product of the present invention, where the elastic filaments are interposed between two sheets of nonwoven fabric, the product does not appear to have exposed elastic filaments at first glance, and the fact that a stretch sheet having exposed elastic filaments is used may be overlooked. However, whether or not the product is an embodiment of a stretch sheet having exposed elastic filaments can be determined by observing the joint between the elastic filaments and the nonwoven fabric in the stretch sheet with an electron microscope. That is, a stretch sheet having exposed elastic filaments is typically manufactured through a process of contacting a molten or softened elastic filament with one side of a raw nonwoven fabric before the elastic filaments are solidified, as in the manufacturing method of the present invention described below. In this case, heat fusion occurs between the raw nonwoven fabric and the molten or softened elastic filament due to the heat brought in by the elastic filament. In contrast, when a nonwoven fabric is fixed to the surface of the elastic filaments of a stretch sheet having exposed elastic filaments with an adhesive, the above-mentioned thermal fusion does not occur, and when fusion is performed by heat sealing or ultrasonic treatment from the surface on which the elastic filaments are not placed, the fused portion between the nonwoven fabric and the elastic filaments is formed so as to extend over the entire thickness direction of the nonwoven fabric. Whether the method of joining the elastic filaments to the nonwoven fabric is the above-mentioned thermal fusion, or whether the nonwoven fabric is placed on the surface of the elastic filaments of the product of the present invention and fixed by fusion with an adhesive, heat treatment, or ultrasonic treatment can be easily determined by observing the joint between the elastic filaments and the nonwoven fabric with an electron microscope.
[0036] In the stretch sheet shown in Fig. 2, cellulose fibers are attached as fine materials to the surfaces of the exposed parts of the elastic filaments. In this way, the surface of the exposed parts of the elastic filaments is provided with the "irregularities of the elastic filaments themselves" and has fine materials attached thereto, so that the degree of irregularity (value of surface roughness) of the surface of the exposed parts is greater than when no fine materials are attached, and therefore the blocking resistance and storage stability of the stretch sheet can be further improved.
[0037] The adhesion area ratio of the fine material on the surface of the exposed part of the elastic filament is preferably 1% or more, more preferably 3% or more, and preferably 20% or less, more preferably 10% or less. This adhesion area ratio of the fine material is the ratio of the total area of the fine material present on the exposed part to the area of the exposed part of the elastic filament, and can be measured by a method conforming to the <Method of Measuring the Roughness Ratio> described later. If the adhesion area ratio of the fine material is too low, there is little point in attaching the fine material to the surface of the exposed part of the elastic filament, and if the adhesion area ratio of the fine material is too high, the user may notice the fine material falling off when the stretch sheet is used in a stretching situation.
[0038] The means for attaching the fine material to the surface of the elastic filament is not particularly limited, and typically, the resin constituting the elastic filament is fused by melting, but the fine material may be attached to the surface of the elastic filament via an adhesive. Depending on the type of fine material, the resin constituting the fine material may be fused by melting.
[0039] The fine material may have a certain degree of hardness and abrasion resistance, and is typically a material different from the elastic filament, but may be the same material as the elastic filament. Examples of materials that can be used as the fine material include cellulose fiber, plastic, glass, ceramic, carbon, etc., and these can be used alone or in combination of two or more.
[0040] The shape of the fine material is not particularly limited, and may be, for example, elongated fiber or particulate. If particulate, it may be, for example, spherical, lump, bale-shaped, or amorphous. The average length in the longitudinal direction of the fibrous fine material (average fiber length) is preferably 1 μm or more, more preferably 100 μm or more, and preferably 10 mm or less, more preferably 5 mm or less. If the average fiber length of the fibrous fine material is too short, the effect of the fine material adhering to the surface of the elastic filament may not be fully exhibited, and conversely, if it is too long, the fine material may easily fall off from the surface of the elastic filament. For example, if fine material with a relatively long longitudinal length falls off from the surface of the elastic filament during use of the stretch sheet, it may be mistaken for the occurrence of a foreign object, which may damage the reliability of the product. The particulate fine material preferably has an average particle size of 1 μm or more, more preferably 100 μm or more, and preferably 2 mm or less, more preferably 1 mm or less.
[0041] Since the fine material is typically attached to the surface of the elastic filament by contacting it with the elastic filament in a molten or softened state, the fine material is preferably one that does not change in quality when it comes into contact with the elastic filament in a molten or softened state, and specifically, a material that does not melt or thermally decompose at 200°C is preferable. Examples of such materials include cellulose fibers, glass fibers, etc., and these can be used alone or in combination of two or more. Examples of cellulose fibers include bleached wood pulp such as softwood bleached kraft pulp (NBKP), softwood bleached sulfite pulp (NBSP), and hardwood bleached kraft pulp (LBKP), natural cellulose fibers such as cotton and hemp, and regenerated cellulose fibers such as rayon, lyocell, and cupra.
[0042] The "roughening ratio" can be used as an index of the surface roughness of the exposed part of the elastic filament. The roughening ratio is the ratio of the total area of the irregularities present in the exposed part to the area of the exposed part of the elastic filament, and is measured by the following method. The "irregularities present in the exposed part" referred to here include both the "irregularities of the elastic filament itself" and the "irregularities due to the attachment of fine materials". In other words, the roughening ratio of the exposed part of the elastic filament reflects the "roughness due to the irregularities of the elastic filament itself" when no fine material is attached to the exposed part, and reflects both the "roughness due to the irregularities of the elastic filament itself" and the "roughness due to the irregularities due to the attachment of fine materials" when a fine material is attached to the exposed part.
[0043] <Method for measuring surface roughness> In this measurement method, the area of the projected image when the exposed portion of the elastic filament in the sheet to be measured is projected in the thickness direction of the sheet is measured, and the total area of the unevenness present in the projected image is measured, and the ratio of the latter to the former is calculated as the roughening rate of the exposed portion. Specifically, a scanning electron microscope (SEM) is used to observe and capture the exposed portion of the elastic filament in the sheet to be measured from the thickness direction of the sheet, and the captured image is processed by image processing software. The observation magnification by SEM is such that the area of the unevenness in the exposed portion of the elastic filament to be observed can be analyzed, and is, for example, about 150 times. FIG. 2 shows an image that can analyze the area of the uneven portion in the exposed portion of the elastic filament. As the image processing software, for example, GIMP (GNU Image Manipulation Program), which is a general-purpose image editing and processing software, can be used. The image processing includes a task of coloring the unevenness (unevenness of the elastic filament itself, unevenness due to the adhesion of fine materials) present in the exposed portion of the elastic filament in the captured image with a predetermined color. The number of pixels in the colored portion in the image is counted, and the number of pixels in the entire exposed portion of the elastic filament including the colored portion is counted, and the roughening rate is calculated by dividing the former by the latter. For example, if the number of pixels in the colored portion (i.e., the unevenness) in an SEM image is 21,528 pixels and the number of pixels in the entire exposed portion of the elastic filament including the colored portion is 67,974 pixels, the roughening rate of the exposed portion is 32% [= (21,528 / 67,974) × 100].
[0044] The roughening ratio of the exposed part of the elastic filament is preferably 10% or more, more preferably 20% or more, from the viewpoint of more reliably solving problems caused by the exposed part such as blocking. There is no particular upper limit to the roughening ratio of the exposed part of the elastic filament, but if the roughening ratio is too high, the elastic filament may be entangled from the nonwoven fabric during the roughening process of the exposed part, so the roughening ratio is preferably 75% or less, more preferably 65% or less.
[0045] The method for measuring the adhesion area ratio of the fine material may be obtained by replacing the "irregularities" of the exposed part of the elastic filament with "fine material" in the above <Method for measuring roughness ratio>. That is, in the above "operation for coloring the irregularities present in the exposed part of the elastic filament with a predetermined color", the "irregularities of the elastic filament itself" are not colored, and only the "irregularities due to the adhesion of the fine material" are colored to form the colored part. Other than this, the adhesion area ratio of the fine material can be measured in a manner similar to that of the above <Method for measuring roughness ratio>.
[0046] Next, a manufacturing method for the stretch sheet for absorbent articles of the present invention will be explained using as an example the manufacturing method for the stretch sheet 1 described above (a stretch sheet for absorbent articles in which a plurality of elastic filaments 3 in an exposed, unstretched state are arranged to extend in one direction without crossing each other and are bonded to one side of a stretchable nonwoven fabric 2).
[0047] The method for producing the stretch sheet 1 includes a step (composite nonwoven fabric production step) of bringing multiple elastic filaments 3 in a molten or softened state spun from multiple spinning nozzles 11a into contact with one side of an original nonwoven fabric 4 before the elastic filaments 3 solidify, as shown in FIG. 3, to obtain a composite nonwoven fabric 5 in which the elastic filaments 3 are exposed and fused to one side of the original nonwoven fabric 4, and a step (stretching step) of stretching the composite nonwoven fabric 5 in the MD, as shown in FIG. 4. The desired stretch sheet 1 is produced by passing through the stretching step.
[0048] The raw nonwoven fabric 4 differs from the nonwoven fabric 2 that constitutes the stretch sheet 1 in that it does not inherently have extensibility in the MD (it does not have low basis weight portions 21 and high basis weight portions 22), but the composition of the constituent fibers is the same as that of the nonwoven fabric 2.
[0049] As shown in FIG. 3, the spinning apparatus 10 used in the composite nonwoven fabric manufacturing process includes a spinning head 11 that spins molten resin from a spinning nozzle 11a to form elastic filaments 3 in a molten or softened state, and a pair of rolls 12, 13 that take up the multiple elastic filaments 3 spun from the spinning nozzle 11a together with the raw nonwoven fabric 4. The spinning nozzle 11a is intermittently arranged along the CD at the lower end of the spinning head 11. The spinning head 11 is connected to a melt extruder (not shown) that melts chips of elastic resin, which is the raw material of the elastic filaments 3, and sends them to the spinning head 11. The basic configuration of the spinning process part in the spinning apparatus 10, including the spinning head 11, is the same as the configuration of a known melt-blow type spinning apparatus with the hot air injection mechanism removed. The first roll 12, one of the pair of rolls 12, 13, has a larger diameter than the second roll 13. The spinning head 11 and the pair of rolls 12, 13 are electrically connected to a control unit (not shown), which is capable of adjusting the resin extrusion speed by the spinning head 11 and the take-up speed by the pair of rolls 12, 13.
[0050] In the composite nonwoven fabric manufacturing process, a plurality of elastic filaments 3 in a molten or softened state spun from the spinning nozzle 11a are supplied between a pair of rolls 12, 13 together with the original nonwoven fabric 4. The pair of rolls 12, 13 take up the elastic filaments 3 before solidification together with the original nonwoven fabric 4, thereby stretching the elastic filaments 3 in the MD. The elastic filaments 3 before solidification are brought into contact with one side of the original nonwoven fabric 4 between the pair of rolls 12, 13, so that the elastic filaments 3 are fused to the original nonwoven fabric 4. Such fusion is caused by the melting heat of the elastic filaments 3 before solidification. The constituent fibers of the original nonwoven fabric 4 are melted by this melting heat, and the elastic filaments 3 and the original nonwoven fabric 4 are joined. Specifically, only the fibers present around the elastic filaments 3 in the original nonwoven fabric 4 are fused to the elastic filaments 3, and the fibers present at a position further away are not fused. In this manner, at least a portion of the constituent fibers of the original nonwoven fabric 4 is fused to the elastic filament 3. From the viewpoint of further improving the bonding strength, it is preferable that both the elastic filament 3 and at least a portion of the constituent fibers of the original nonwoven fabric 4 are fused.
[0051] In the composite nonwoven fabric manufacturing process, the elastic filaments 3 in a molten or softened state are stretched and the molecules are oriented in the stretching direction until they come into contact with the raw nonwoven fabric 4. This stretching reduces the diameter. From the viewpoint of sufficiently stretching the elastic filaments 3 and preventing thread breakage of the elastic filaments 3, the temperature of the elastic filaments 3 may be adjusted by blowing air of a predetermined temperature (hot air or cold air) onto the spun elastic filaments 3. The stretching of the elastic filaments 3 may be not only stretching in a molten state of the resin composition (elastic resin) constituting the elastic filaments 3 (melt stretching), but also stretching in a softened state during the cooling process (softening stretching).
[0052] From the viewpoint of ensuring fiber fusion and maintaining the shape of the elastic filament 3 to further improve stretchability, the temperature of the elastic filament 3 when it is brought into contact with the original nonwoven fabric 4 is preferably 100° C. or higher, more preferably 120° C. or higher, and also preferably 180° C. or lower, more preferably 160° C. or lower. The temperature of the elastic filament 3 when it is brought into contact with the original nonwoven fabric 4 is measured by observing the bonding state using a film having a melting point different from that of the resin composition constituting the elastic filament 3. If the elastic filament 3 and the film are fused together, it is understood that the bonding temperature is equal to or higher than the melting point of the film.
[0053] In the embodiment shown in FIG. 3, the elastic filaments 3 in a molten or softened state are brought into contact with the original nonwoven fabric 4 by winding the original nonwoven fabric 4, which is continuous in one direction, around the first roll 12 of a pair of rolls 12 and 13, while supplying a plurality of elastic filaments 3 between the pair of rolls 12 and 13. The elastic filaments 3 in a molten or softened state spun from the spinning nozzle 11a are supplied between the pair of rolls 12 and 13 arranged opposite to each other in a state of being arranged in one direction without intersecting with each other, and both the elastic filaments 3 and the original nonwoven fabric 4 are clamped by the pair of rolls 12 and 13. If the clamping pressure is too large, the elastic filaments 3 are likely to be embedded in the original nonwoven fabric 4, which may impair the texture. The clamping pressure is sufficient to bring the elastic filaments 3 into contact with the original nonwoven fabric 4, and an excessively high clamping pressure is not required.
[0054] In the embodiment shown in Fig. 3, the composite nonwoven fabric 5 produced in the composite nonwoven fabric production process, which is continuous in one direction, is wound into a roll to form a composite nonwoven fabric roll 5R, which is used in the next step, the stretching step. In the stretching step, the composite nonwoven fabric 5 produced in the composite nonwoven fabric production process, more specifically, the raw nonwoven fabric 4 constituting the composite nonwoven fabric 5, is stretched in MD to impart MD stretchability to the raw nonwoven fabric 4, thereby producing the desired stretch sheet 1. Fig. 4 shows a stretching step using a stretching device 30 as an example of the stretching step.
[0055] The stretching device 30 includes a pair of grooved rolls 31a, 31b, a roll support shaft 32 disposed upstream of the grooved rolls 31a, 31b in the MD and to which the composite nonwoven fabric roll 5R is attached, a pair of in-feed rolls 33a, 33b disposed between the roll support shaft 32 and the grooved rolls 31a, 31b, and a pair of out-feed rolls 34a, 34b disposed downstream of the grooved rolls 31a, 31b in the MD. The roll support shaft 32 is driven to rotate, whereby the composite nonwoven fabric 5 is unwound from the composite nonwoven fabric roll 5R, and the unwound composite nonwoven fabric 5 is supplied between the grooved rolls 31a, 31b by the pair of in-feed rolls 33a, 33b. The pair of out-feed rolls 34a, 34b pull out the composite nonwoven fabric 5 (stretch sheet 1) stretched between the grooved rolls 31a, 31b from the grooved rolls 31a, 31b and transport it to the next process. The stretching device 30 includes a drive unit (not shown) for driving at least one of the pair of in-feed rolls 33a, 33b and the pair of out-feed rolls 34a, 34b to rotate.
[0056] The pair of tooth-groove rolls 31a, 31b may be so-called co-rotating rolls in which both are driven by a driving source, or so-called co-rotating rolls in which only one is driven by a driving source. On the peripheral surface of each of the pair of tooth-groove rolls 31a, 31b, teeth and tooth bottoms extending along the roll axis direction are alternately formed along the circumferential direction. As the tooth profile of the tooth-groove rolls 31a, 31b, a general involute tooth profile or a cycloid tooth profile is used, and in particular, those with a narrow tooth width are preferable. The pair of tooth-groove rolls 31a, 31b are combined so that the teeth of one are loosely inserted between the teeth of the other and the teeth of the other are loosely inserted between the teeth of the other, that is, so that meshing portions of the tooth grooves of both rolls 31a, 31b are formed. The stretching device 30 has a known lifting mechanism (not shown) that displaces one or both roll axes of a pair of grooved rolls 31a, 31b up and down, and the lifting mechanism makes it possible to adjust the distance between the grooved rolls 31a, 31b.
[0057] In the stretching step, the composite nonwoven fabric 5 is supplied to the meshing portion of the pair of grooved rolls 31a, 31b while the pair of rolls 31a, 31b are rotating, so that the raw nonwoven fabric 4 of the composite nonwoven fabric 5 is stretched along the MD (the extension direction of the elastic filaments 3). As a result, the raw nonwoven fabric 4 is formed with a low basis weight portion 21 and a high basis weight portion 22 (see FIG. 1) to impart extensibility along the MD, and the composite nonwoven fabric 5 becomes a stretch sheet 1 having elasticity in the MD. The low basis weight portion 21 is a region in the meshing portion where the degree of stretching is relatively large, and the high basis weight portion 22 is a region in the meshing portion where the degree of stretching is relatively small (typically, hardly stretched). The degree of stretching of the composite nonwoven fabric 5 can be adjusted by appropriately adjusting the rotation speed (conveying speed of the workpiece) of the pair of in-feed rolls 33a, 33b and the pair of out-feed rolls 34a, 34b. For the stretching step, the technique described in JP-A-2008-179128 can be appropriately used.
[0058] The method for producing the stretch sheet 1 is characterized in that, in addition to the composite nonwoven fabric production step and stretching step, it further includes a surface roughening step of forming irregularities on the surfaces of the elastic filaments 3 in the areas not in contact with the original nonwoven fabric 4. By carrying out the surface roughening step, the surface of each exposed portion of the plurality of elastic filaments 3 in the stretch sheet 1 is given the "roughness caused by the irregularities of the elastic filaments 3 themselves."
[0059] The surface roughness imparting step is typically carried out simultaneously with the composite nonwoven fabric production step, or after the composite nonwoven fabric production step and before the stretching step. A method of transferring the surface roughness of another object to the elastic filaments 3 in a molten or softened state (see Figs. 5 to 8) described later is a specific example of the former. A specific example of the latter is a method of imparting fine irregularities (scratches) to the surface of the exposed part of the elastic filaments 3 fused in an exposed state to one side of the raw nonwoven fabric 4 in the composite nonwoven fabric 5 produced through the composite nonwoven fabric production step, for example, by rubbing the surface of the exposed part with an object having a predetermined surface roughness. Regardless of the method, the "roughness caused by the irregularities of the elastic filaments 3 themselves" is imparted to the surface of the exposed part of the elastic filaments 3 in the composite nonwoven fabric roll 5R (see Fig. 3) produced through the surface roughness imparting step. Therefore, the composite nonwoven fabric roll 5R has blocking resistance and excellent storage stability, and is less susceptible to problems such as difficulty in unwinding the composite nonwoven fabric 5 from the roll 5R as shown in FIG.
[0060] A preferred embodiment of the surface roughness imparting step includes a method in which an object having a predetermined surface roughness is brought into contact with the elastic filament 3 in a molten or softened state, thereby transferring the surface roughness of the object to the elastic filament 3. Such a method of transferring the surface roughness of another object to the elastic filament 3 in a molten or softened state can solve problems that arise when manufacturing a stretch sheet such as the stretch sheet 1 in which the elastic filaments are exposed. That is, since the elastic filaments 3 are exposed in the stretch sheet 1, not only the problems after production (such as poor handling and storage stability) described above are inherent, but also problems during production. Specifically, for example, there is a concern that the elastic filaments 3 in a molten or softened state expanded from the spinning nozzle 11a will stick to and be entangled with the roll that comes into contact with the elastic filaments 3 (the second roll 13 in the embodiment shown in FIG. 3) out of a pair of rolls 12, 13 that are part of the spinning device 10. By utilizing the above-mentioned method of transferring surface roughness and using a roll having a predetermined surface roughness on its circumferential surface as the roll that comes into contact with the elastic filaments 3 in a molten or softened state, the contact area between the elastic filaments 3 and the circumferential surface of the roll is reduced, and the van der Waals force that causes the elastic filaments 3 to stick to the circumferential surface of the roll is reduced, making it difficult for the elastic filaments 3 to stick to the circumferential surface of the roll. Furthermore, even if the elastic filaments 3 stick to the circumferential surface of the roll, they can be peeled off relatively easily. This makes it possible to efficiently produce the stretch sheet 1 while imparting roughness to the elastic filaments 3 due to the unevenness of the elastic filaments 3 themselves.
[0061] 5 shows a case where a first roll 12A having a predetermined surface roughness is used instead of the first roll 12 having a smooth peripheral surface in the spinning apparatus 10 shown in FIG. 3. In the method for producing a stretch sheet 1 in this case, in the composite nonwoven fabric production step, the raw nonwoven fabric 4 is wound around the second roll 13 of a pair of opposing rolls 12A and 13 and supplied between the pair of rolls 12A and 13, and multiple elastic filaments 3 in a molten or softened state spun from multiple spinning nozzles 11a are supplied between the raw nonwoven fabric 4 and the first roll 12A of the other pair of rolls 12A and 13, and in the surface roughness imparting step, the roll peripheral surface of the first roll 12A having a predetermined surface roughness is brought into contact with the non-contact portions of the surfaces of the elastic filaments 3 in a molten or softened state that do not contact the raw nonwoven fabric 4 before the elastic filaments 3 in a molten or softened state are solidified. This effectively prevents the elastic filaments 3 from sticking to the peripheral surface of the first roll 12A and becoming entangled, while imparting roughness due to the unevenness of the elastic filaments 3 themselves to the surface of the exposed portions of the elastic filaments 3 in the composite nonwoven fabric 5 produced through the composite nonwoven fabric production process.
[0062] 6 shows a case where a second roll 13A having a predetermined surface roughness is used instead of the second roll 13 having a smooth peripheral surface in the spinning apparatus 10 shown in FIG. 3. In this case, in the method for producing a stretch sheet 1, in the composite nonwoven fabric production step, the raw nonwoven fabric 4 is wound around the first roll 12, one of a pair of opposing rolls 12, 13A, and supplied between the pair of rolls 12, 13A, while a plurality of elastic filaments 3 in a molten or softened state spun from a plurality of spinning nozzles 11a are supplied between the raw nonwoven fabric 4 and the second roll 13A, the other of the pair of rolls 12, 13A, and in the surface roughness imparting step, the roll peripheral surface of the second roll 13A having a predetermined surface roughness is brought into contact with the non-contact portions of the surfaces of the elastic filaments 3 in a molten or softened state that do not contact the raw nonwoven fabric 4 before the elastic filaments 3 in a molten or softened state are solidified. This effectively prevents the elastic filaments 3 from sticking to the peripheral surface of the second roll 13A and becoming entangled, while imparting roughness due to the unevenness of the elastic filaments 3 themselves to the surface of the exposed portions of the elastic filaments 3 in the composite nonwoven fabric 5 produced through the composite nonwoven fabric production process.
[0063] An example of the rolls 12A and 13A having a predetermined surface roughness on the roll peripheral surface is a roll having a surface treatment applied thereto to increase the frictional force on the roll peripheral surface. Examples of the surface treatment include attaching a material having a high friction coefficient to the roll peripheral surface, and applying a surface treatment such as a thermal spraying treatment or a blasting treatment to the roll peripheral surface itself. The surface roughness of the roll peripheral surface that has been subjected to the surface treatment is preferably 5 μm or more, more preferably 10 μm or more, and preferably 50 μm or less, more preferably 30 μm or less, when the arithmetic mean roughness Ra is used as an index. If the Ra of the roll peripheral surface is too small, it is not possible to impart a sufficient uneven shape to the surface of the exposed part of the elastic filament, and conversely, if the Ra is too large, the elastic filament may be mechanically entangled between the projections of the roughness, which may cause problems in the production of the stretch sheet. The Ra of the roll peripheral surface can be measured using a general-purpose surface roughness measuring device (for example, Surftest SJ-500, manufactured by Mitutoyo Corporation).
[0064] Another example of the rolls 12A and 13A having a predetermined surface roughness applied to the roll peripheral surface is a roll having the above-mentioned fine material applied to the roll peripheral surface. By contacting the roll peripheral surface having such fine material applied to the elastic filaments in a molten or softened state in the surface roughness application process, it is possible to manufacture a stretch sheet having the fine material applied to the surface of the exposed part of the elastic filaments, such as the stretch sheet shown in FIG. 2, in which the "unevenness of the elastic filaments themselves" is applied to the surface of the exposed part of the elastic filaments. In the stretch sheet manufactured in this way, the "unevenness of the elastic filaments themselves" on the surface of the exposed part of the elastic filaments is formed by transferring the unevenness of the roll peripheral surface to which the fine material is applied, and the fine material applied to the surface of the exposed part of the elastic filaments is dropped off from the roll peripheral surface.
[0065] A specific example of the "roll having a fine material attached to its peripheral surface" is a roll containing the above-mentioned material that does not melt or pyrolyze at 200°C on its peripheral surface. A specific example of such a roll is a cotton roll whose peripheral surface is made of cellulose fiber (a material that does not melt or pyrolyze at 200°C). The cotton roll may be any roll in which at least the outermost layer forming the peripheral surface of the roll is made of a cotton layer, and for example, a metal roll or a rubber roll whose peripheral surface is covered with a cotton layer can be used. The cotton roll preferably has a Shore D hardness (JIS K7215) of 75 to 85 degrees, particularly 77 to 83 degrees.
[0066] 7 shows the main parts of another embodiment of the method for producing the stretch sheet 1. In the embodiments described below, configurations different from the above-mentioned embodiment (spinning device 10, stretching device 30) will be described, and configurations similar to those in the above-mentioned embodiment will be given the same reference numerals and description will be omitted. For configurations not specifically described in the embodiments described below, the description of the above-mentioned embodiment will be applied as appropriate.
[0067] The method for producing the stretch sheet 1 shown in Fig. 7 includes a step of contacting a plurality of elastic filaments 3 in a molten or softened state spun from a plurality of spinning nozzles 11a (see Fig. 3) with one side of an original nonwoven fabric 4 before the elastic filaments 3 are solidified to obtain a composite nonwoven fabric 5 in which the elastic filaments 3 are fused to one side of the original nonwoven fabric 4, and a step of contacting a release sheet 6 with the non-contact portion of the surface of the elastic filaments 3 with the original nonwoven fabric 4 to obtain a laminated sheet 7 in which the elastic filaments 3 are interposed between the original nonwoven fabric 4 and the release sheet 6 (laminate sheet production step), a step of removing the release sheet 6 from the laminated sheet 7, and a step of stretching the composite nonwoven fabric 5 (stretching step). Fig. 7 shows the laminated sheet production step.
[0068] In the laminated sheet manufacturing process shown in Fig. 7, a raw nonwoven fabric 4 continuous in one direction is wound around one of a pair of opposing rolls 12, 13 and supplied between the pair of rolls 12, 13, and a release sheet 6 continuous in one direction is wound around the other of the pair of rolls 12, 13 and supplied between the pair of rolls 12, 13, and further, a plurality of elastic filaments 3 in a molten or softened state spun from a plurality of spinning nozzles 11a (see Fig. 3) are supplied between the raw nonwoven fabric 4 and the release sheet 6, and the raw nonwoven fabric 4, the elastic filaments 3 (composite nonwoven fabric 5), and the release sheet 6 are sandwiched and pressed by the pair of rolls 12, 13 to produce a laminated sheet 7 continuous in one direction. The raw nonwoven fabric 4 and the release sheet 6 are fused to the elastic filaments 3 before solidification by contacting them between the pair of rolls 12, 13. The laminated sheet 7 thus produced has a configuration in which the entire surface of the composite nonwoven fabric 5 on which the elastic filaments 3 are disposed is covered with the release sheet 6. In addition, the original nonwoven fabric 4 may be wound around the first roll 12 and the release sheet 6 may be wound around the second roll 13, which is the opposite to the configuration shown in FIG.
[0069] Since the release sheet 6 comes into contact with the multiple elastic filaments 3 in a molten or softened state, it is preferable that the release sheet 6 is mainly made of a material that does not melt even when it comes into contact with such high-temperature elastic filaments 3 and that allows easy removal from the laminate sheet 7, and from this viewpoint, the release sheet 6 is mainly made of a material that does not melt or thermally decompose at 200°C, which is one of the fine materials mentioned above. Here, "mainly made of" means that the content of the material that does not melt or thermally decompose at 200°C in the release sheet 6 exceeds 85% by mass with respect to the total mass of the release sheet 6. The content of the material that does not melt or thermally decompose at 200°C in the release sheet 6 may be 100% by mass.
[0070] A specific example of the release sheet 6 is paper mainly composed of cellulose fibers (a material that does not melt or thermally decompose at 200° C.). As the cellulose fibers contained in the release sheet 6, those usable as the fine material described above can be used. The basis weight of the release sheet 6 made of paper containing cellulose fibers is preferably 9 g / m from the viewpoint of imparting necessary and sufficient strength to the release sheet 6. 2 More preferably, 12 g / m 2 More than 100 g / m 2 Less than 70 g / m 2 The following is the result.
[0071] There is no particular restriction on the timing for removing the release sheet 6 from the laminated sheet 7, and it may be after the elastic filaments 3, which were in a molten or softened state when the release sheet 6 was brought into contact with the laminated sheet 7, have cooled and solidified.
[0072] From the viewpoint of smoothly removing the release sheet 6 from the laminated sheet 7 (a laminate of the composite nonwoven fabric 5 and the release sheet 6), the peel strength between the surface of the composite nonwoven fabric 5 on which the elastic filaments 3 are arranged and the release sheet 6 is preferably 0.19 N / 25 mm or less, more preferably 0.1 N / 25 mm or less. There is no particular lower limit to the peel strength, but it is preferably 0.005 N / 25 mm or more. The peel strength can be adjusted by appropriately adjusting the type of release sheet 6, the clamping pressure applied by the pair of rolls 12, 13, etc. The peel strength is measured by the following method.
[0073] <Method for measuring peel strength> A test piece is cut out from the laminated sheet 7 (a laminate of a composite nonwoven fabric 5 and a release sheet 6) to be evaluated, in a plan view, in a rectangular shape with a length of 150 mm in MD and a length of 25 mm in CD. Next, at one end of the longitudinal direction of the test piece, the layer between the composite nonwoven fabric 5 and the release sheet 6 is peeled off in the MD by 30 mm to separate the composite nonwoven fabric 5 side and the release sheet 6 side, and the longitudinal ends of each of the two separated parts (parts to be supported by the chucks of the tensile tester) are clamped by 10 mm between a pair of chucks of the tensile tester, and the test piece is set in a T-shape. The distance between the chucks is 30 mm. Then, peeling is performed at a tensile speed of 50 mm / min, and the maximum strength is measured. The measurement is performed three times, and the average value of the maximum strength is the peel strength (unit: N / 25 mm) to be evaluated. If the CD length of the test piece is less than 25 mm, a test piece is prepared with an appropriate length, and the average value of the maximum strength after the test is converted to a 25 mm width. The support portion of the test piece may be appropriately changed depending on the size of the test piece, and may be reduced from the above-mentioned 30 mm. As the tensile tester, for example, "Autograph AG-X" manufactured by Shimadzu Corporation can be used.
[0074] When the release sheet 6 is removed from the laminated sheet 7, the exposed portion of the elastic filament 3 fused to the original nonwoven fabric 4 appears. The surface of the exposed portion of the elastic filament 3 is typically provided with the "irregularities of the elastic filament 3 itself" and has "a material that does not melt or thermally decompose at 200°C" (fine material) attached thereto. The former is formed by transferring the irregularities that existed on the contact surface of the release sheet 6 with the elastic filament 3, and the latter is a material that fell off the release sheet 6 when the release sheet 6 was removed from the laminated sheet 7. The stretch sheet shown in FIG. 2 was manufactured using paper containing cellulose fibers as the release sheet 6, and the fine material attached to the surface of the elastic filament in FIG. 2 is cellulose fiber derived from paper.
[0075] The method for producing a stretch sheet using a release sheet 6 as shown in FIG. 7 can efficiently produce a stretch sheet that is resistant to blocking and has excellent storage stability, while effectively preventing the elastic filaments 3 from sticking to and becoming entangled on the peripheral surfaces of the pair of rolls 12, 13 during production, just like the method for producing a stretch sheet using rolls 12A, 13A having a predetermined surface roughness imparted to the peripheral surfaces of the rolls as shown in FIGS. 5 and 6.
[0076] Fig. 8 shows another example of a method for producing a stretch sheet using a release sheet 6. In the embodiment shown in Fig. 8, a third roll 14 is disposed downstream in the MD from the second roll 13 such that the peripheral surface of the third roll 14 faces the peripheral surface of the first roll 12, and an endless release sheet 6 is stretched across both rolls 13, 14 so that the release sheet 6 rotates between both rolls 13, 14. At least one of the rolls 13, 14 is a drive roll.
[0077] In the embodiment shown in FIG. 8, the release sheet 6, the elastic filament 3, and the original nonwoven fabric 4 are transported to the MD as a laminated sheet 7 in close contact with each other between the two rolls 13 and 14 (laminated sheet manufacturing process), and when the release sheet 6 leaves the first roll 12 at the position of the third roll 14 and enters a predetermined orbit, the release sheet 6 is removed from the laminated sheet 7, and the remaining composite nonwoven fabric 5 (elastic filament 3 and original nonwoven fabric 4) is transported to the MD. In the embodiment shown in FIG. 7, the portion where the elastic filament 3 and the original nonwoven fabric 4 are pressed from both sides in the thickness direction in a state where they are overlapped is only between the pair of rolls 12 and 13, whereas in the embodiment shown in FIG. 8, the portion is between the release sheet 6 and the first roll 12, which are stretched from the second roll 13 to the third roll 14, so that the embodiment shown in FIG. 8 maintains the elastic filament 3 in a molten or softened state in close contact with the original nonwoven fabric 4 for a longer period of time than the embodiment shown in FIG. 7. Therefore, for example, even if the processing speed is relatively fast and it is difficult to sufficiently solidify the elastic filament 3 in a molten or softened state in the configuration shown in Figure 7, the elastic filament 3 in a molten or softened state can be sufficiently solidified in the configuration shown in Figure 8.
[0078] The present invention can effectively prevent problems such as blocking caused by the exposed portions of the elastic filaments by adopting the aforementioned characteristic configurations such as "giving roughness to the surface of the exposed portions of the elastic filaments due to the unevenness of the elastic filaments themselves" and "adhering a fine material to the surface of the exposed portions of the elastic filaments." An anti-blocking agent may also be used in combination. One example of a method for using an anti-blocking agent is to apply the anti-blocking agent to the entire surface of the composite nonwoven fabric 5 on which the elastic filaments 3 are disposed or the surface opposite thereto, after the composite nonwoven fabric production step and the surface roughening step and before the stretching step in the above-mentioned method for producing the stretch sheet 1. In such a method, the anti-blocking agent is preferably applied by spraying. Another example of a method for using an anti-blocking agent is to incorporate fibers with an anti-blocking agent kneaded into the raw nonwoven fabric 4. Such fibers can be obtained by kneading the anti-blocking agent into the constituent resin of the fibers. When an anti-blocking agent is used in the production of a stretch sheet, the amount of anti-blocking agent used (the content of anti-blocking agent in the stretch sheet) is preferably 0.3 parts by weight or more, more preferably 0.5 parts by weight or more, and preferably 2 parts by weight or less, more preferably 1.5 parts by weight or less, per 100 parts by weight of the original nonwoven fabric.
[0079] As the blocking inhibitor, amide compounds, silicone compounds, modified silicone compounds, fluorocarbon compounds, hydrocarbon compounds having side chains, mineral oils, waxes, and the like can be used. Examples of the amide compound include compounds having a structure consisting of amine and carboxylic acid, and polyamide compounds. The amide compound may be either a compound in which the amino group and the carbonyl group end remain in the molecule, or a compound blocked in the form of an amide group. Specific examples include stearic acid amide, behenic acid amide, hexamethylene bisstearic acid amide, trimethylene bisoctyl acid amide, hexamethylene bishydroxystearic acid amide, trioctatrimellitic acid amide, distearyl urea, butylene bisstearic acid amide, xylylene bisstearic acid amide, distearyl adipic acid amide, distearyl phthalic acid amide, distearyl octadecanedioic acid amide, epsilon caprolactam, and derivatives thereof. Examples of the silicone-based compound include dimethyl silicone, methyl phenyl silicone, and methyl hydrogel silicone. The modified silicone compound may include modified silicone polymers, silicone polymers, etc. Among them, amino-modified silicone, diamino-modified silicone, polyether-modified silicone, etc. From the viewpoint of further improving the feel on the skin, amino-modified silicone or diamino-modified silicone is preferred. Examples of fluorocarbon compounds include fluorinated polymers such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF).
[0080] While the present invention has been described above based on its preferred embodiments, the present invention is not limited to the above-described embodiments and can be modified as appropriate without departing from the spirit of the present invention.
[0081] The following supplementary notes are further disclosed regarding the above-described embodiment of the present invention. <1> A plurality of elastic filaments in an unstretched state are arranged so as to extend in one direction without intersecting each other and are bonded by fusion to one surface of an extensible nonwoven fabric; A stretch sheet for absorbent articles, in which the elastic filaments are exposed at portions other than the fused portions with the nonwoven fabric, and the surfaces of the exposed portions of the elastic filaments are provided with roughness due to the unevenness of the elastic filaments themselves. <2> The roughening rate of the exposed portion of the elastic filament is 10% or more. <1> The stretch sheet for absorbent articles according to claim 1. <3> The roughness ratio of the exposed portion of the elastic filament is preferably 20% or more, and preferably 75% or less, more preferably 65% or less. <1> or <2> The stretch sheet for absorbent articles according to claim 1. <4> There is no adhesive between the nonwoven fabric and the elastic filaments. <1> ~ <3> 13. The stretch sheet for absorbent articles according to claim 12. <5> The elastic filaments are fused to the nonwoven fabric over the entire length of the elastic filaments in the longitudinal direction. <1> ~ <4> 13. The stretch sheet for absorbent articles according to claim 12.
[0082] <6> A fine material is attached to the surface of the exposed portion of the elastic filament. <1> ~ <5> 13. The stretch sheet for absorbent articles according to claim 12. <7> The fine material includes a material that does not melt or thermally decompose at 200° C. <6> The stretch sheet for absorbent articles according to claim 1. <8> The fine material includes a fibrous fine material, and the average fiber length of the fibrous fine material is preferably 1 μm or more, more preferably 100 μm or more, and preferably 10 mm or less, more preferably 5 mm or less. <6> or <7> The stretch sheet for absorbent articles according to claim 1. <9> The fine material includes cellulose fibers. <6> ~ <8> 13. The stretch sheet for absorbent articles according to claim 12. <10> The fine material includes a particulate fine material, and the particulate fine material has an average particle size of preferably 1 μm or more, more preferably 100 μm or more, and preferably 2 mm or less, more preferably 1 mm or less. <6> ~ <9> 13. The stretch sheet for absorbent articles according to claim 12. <11> The adhesion area ratio of the fine material on the surface of the exposed part of the elastic filament is preferably 1% or more, more preferably 3% or more, and is preferably 20% or less, more preferably 10% or less. <6> ~ <10> 13. The stretch sheet for absorbent articles according to claim 12.
[0083] <12> A method for producing a stretch sheet for absorbent articles, comprising bonding a plurality of elastic filaments in an exposed state, the elastic filaments being arranged so as to extend in one direction without crossing each other, to one surface of a stretchable nonwoven fabric, the method comprising the steps of: a composite nonwoven fabric production process in which a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are brought into contact with one side of an original nonwoven fabric before the elastic filaments are solidified, thereby obtaining a composite nonwoven fabric in which the elastic filaments are fused in a state of being exposed on one side of the original nonwoven fabric; a surface roughening step of forming irregularities on the surface of the elastic filament in a portion that does not contact the raw nonwoven fabric; and stretching the composite nonwoven fabric. <13> In the composite nonwoven fabric manufacturing step, the elastic filaments are fused to at least a part of the constituent fibers of the raw nonwoven fabric. <12> A method for producing the stretch sheet for absorbent articles according to claim 1.
[0084] <14> In the composite nonwoven fabric manufacturing process, the raw nonwoven fabric is wound around one of a pair of opposing rolls and supplied between the pair of rolls, and a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are supplied between the raw nonwoven fabric and the other of the pair of rolls, a predetermined surface roughness is imparted to the peripheral surface of the other of the pair of rolls, In the surface roughening step, the non-contact portion of the elastic filament is brought into contact with the peripheral surface of the other roll before the elastic filament is solidified. <12> or <13> A method for producing the stretch sheet for absorbent articles according to claim 1. <15> The other roll (the roll having a predetermined surface roughness on the peripheral surface) is a roll having a surface treatment applied thereto so as to increase frictional force on the peripheral surface of the roll. <14> A method for producing the stretch sheet for absorbent articles according to claim 1. <16> The arithmetic mean roughness Ra of the other roll (the roll having a predetermined surface roughness on its peripheral surface) is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 50 μm or less, more preferably 30 μm or less. <14> or <15> A method for producing the stretch sheet for absorbent articles according to claim 1. <17> A roll having a fine material attached to its peripheral surface is used as the other roll (the roll having a predetermined surface roughness imparted to its peripheral surface). <14> ~ <16> 13. A method for producing the stretch sheet for absorbent articles according to claim 12. <18> The peripheral surface of the other roll contains a material that does not melt or thermally decompose at 200°C. <14> ~ <17> 13. A method for producing the stretch sheet for absorbent articles according to claim 12. <19> The peripheral surface of the other roll contains cellulose fibers. <14> ~ <18> 13. A method for producing the stretch sheet for absorbent articles according to claim 12. <20> The other roll (the roll having a predetermined surface roughness on the peripheral surface) is a cotton roll having a peripheral surface made of cellulose fiber (a material that does not melt or thermally decompose at 200° C.). <14> ~ <19> 13. A method for producing the stretch sheet for absorbent articles according to claim 12. <21> The cotton roll used has a Shore D hardness (JIS K7215) of preferably 75 to 85 degrees, more preferably 77 to 83 degrees. <20> A method for producing the stretch sheet for absorbent articles according to claim 1.
[0085] <22> A method for producing a stretch sheet for absorbent articles, comprising bonding a plurality of elastic filaments in an exposed state, the elastic filaments being arranged so as to extend in one direction without crossing each other, to one surface of a stretchable nonwoven fabric, the method comprising the steps of: a step of contacting a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles with one side of an original nonwoven fabric before the elastic filaments are solidified to obtain a composite nonwoven fabric in which the elastic filaments are fused to one side of the original nonwoven fabric, and contacting a release sheet with the portions of the surfaces of the elastic filaments that are not in contact with the original nonwoven fabric to obtain a laminated sheet in which the elastic filaments are interposed between the original nonwoven fabric and the release sheet; removing the release sheet from the laminate sheet; and stretching the composite nonwoven fabric. The release sheet is mainly made of a material that does not melt or thermally decompose at 200°C. <23> The basis weight of the release sheet is preferably 9 g / m 2 More preferably, 12 g / m 2 More than 100 g / m 2 Less than 70 g / m 2The above-mentioned <22> A method for producing the stretch sheet for absorbent articles according to claim 1. <24> The step of removing the release sheet from the laminated sheet is performed after the elastic filaments, which were in a molten or softened state when the release sheet was brought into contact with the laminated sheet, have cooled and solidified. <22> or <23> A method for producing the stretch sheet for absorbent articles according to claim 1. <25> The peel strength between the surface of the composite nonwoven fabric on which the elastic filaments are arranged and the release sheet is preferably 0.19 N / 25 mm or less, more preferably 0.1 N / 25 mm or less, and preferably 0.005 N / 25 mm or more. <22> ~ <24> 13. A method for producing the stretch sheet for absorbent articles according to claim 12.
[0086] <26> Using an antiblocking agent, <14> ~ <25> 13. A method for producing the stretch sheet for absorbent articles according to claim 12. <27> The amount of the anti-blocking agent used (the content of the anti-blocking agent in the stretch sheet) is preferably 0.3 parts by weight or more, more preferably 0.5 parts by weight or more, and preferably 2 parts by weight or less, more preferably 1.5 parts by weight or less, based on 100 parts by weight of the raw nonwoven fabric. <26> A method for producing the stretch sheet for absorbent articles according to claim 1. <28> The blocking inhibitor is at least one selected from the group consisting of an amide compound, a silicone compound, and a modified silicone compound. <26> or <27> A method for producing the stretch sheet for absorbent articles according to claim 1. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to such examples.
[0088] [Examples 1 to 5 and Comparative Examples 1 to 3: Production of stretch sheets with exposed elastic filaments] First, using a spinning apparatus with a configuration similar to that of the spinning apparatus 10 described above, and a manufacturing method having a laminate sheet manufacturing step using the release sheet described above, a laminate sheet with a configuration similar to that of laminate sheet 7, which is an intermediate product of the stretch sheet 1 shown in Figure 1, was manufactured, i.e., a laminate sheet consisting of an unstretched composite nonwoven fabric and a release sheet fused to the surface of the composite nonwoven fabric on which the elastic filaments are arranged, and in which a plurality of unstretched elastic filaments are fused to one surface of the nonwoven fabric in an exposed state, the filaments being arranged so as to extend in one direction without crossing each other. Specifically, the raw material resin of the elastic filament was spun out from the spinning nozzle in a molten state, and as shown in Fig. 7, the elastic filament was brought into contact with one side of the original nonwoven fabric before solidification to obtain a composite nonwoven fabric in which the elastic filament was fused to one side of the original nonwoven fabric, and a release sheet was brought into contact with the non-contact part of the surface of the elastic filament with the original nonwoven fabric to obtain a laminated sheet in which the elastic filament was interposed between the original nonwoven fabric and the release sheet (laminate sheet manufacturing process). However, in this laminated sheet manufacturing process, the original nonwoven fabric was wound around the first roll 12 and the release sheet was wound around the second roll 13, in the opposite manner to the form shown in Fig. 7. The resin discharge speed from the spinning nozzle was 10 g / min, and the take-up speed of the elastic filament by the pair of rolls 12 and 13 was 150 m / min. The interval between adjacent elastic filaments in the obtained composite nonwoven fabric was 0.5 mm. Next, the release sheet was removed from the laminated sheet obtained in each Example and Comparative Example to obtain a composite nonwoven fabric, and the composite nonwoven fabric was stretched in MD using a stretching device having a configuration similar to that of the above-mentioned stretching device 30 to obtain a stretch sheet having elasticity in MD.
[0089] Styrene-ethylene-propylene-styrene (SEPS) was used as the raw resin for the elastic filament. The following materials were used as the raw nonwoven fabric and release sheet. None of the following contained an anti-blocking agent. SB nonwoven fabric 1: Hydrophobic spunbond nonwoven fabric, basis weight 18g / m 2 Raw material resin: polypropylene (melting point 140-170℃), fiber diameter 17μm ·SB nonwoven fabric 2: Hydrophilic spunbond nonwoven fabric, basis weight 18g / m 2 Raw material resin: polypropylene (melting point 140-170℃), fiber diameter 17μm ·AT non-woven fabric: Hydrophilic air-through non-woven fabric, basis weight 20g / m 2 Core raw material resin: PET, Sheath raw material resin: polyethylene (melting point 130℃), fiber diameter 16μm ·Paper: basis weight 16g / m 2 , Cellulose fiber (wood pulp) 100% by mass ·Resin compound paper: basis weight 15g / m 2 , cellulose fiber (wood pulp) 90% by mass, synthetic fiber (core raw material resin: PET, sheath raw material resin: low-melting point PET (melting point 120°C) core-sheath type composite fiber not hydrophilized) 10% by mass
[0090] [Comparative Examples 4 and 5: Production of stretch sheets with non-exposed elastic filaments] In the manufacturing method of the above-mentioned elastic filament exposed type stretch sheet, a stretch sheet was produced in the same manner as the above-mentioned manufacturing method, except that a raw nonwoven fabric was used instead of a release sheet, in which an elastic filament was interposed between two nonwoven fabrics and no exposed portion of the elastic filament was produced.
[0091] [Evaluation test] Regarding the elastic filament exposed type stretch sheet, the peel strength when removing the release sheet from the laminated sheet, which is the intermediate product of each example and comparative example, was measured by the above method. In addition, the surface roughness of the exposed part of the elastic filament in the elastic filament exposed type stretch sheet obtained in each example and comparative example was measured by the above method, and the surface of the exposed part was observed to confirm the presence or absence of unevenness of the elastic filament itself and the presence or absence of adhesion of fine material originating from the release sheet. In addition, the air flow resistance of the stretch sheet obtained in each example and comparative example was measured by the following method. The results are shown in Table 1 below.
[0092] <Method of measuring airflow resistance> This measurement method can be carried out using an air permeability tester "KES-F8-AP1 AIR PERMEABILITY TESTER" (product name) manufactured by Kato Tech Co., Ltd. Specifically, the sheet to be measured is stretched to a maximum elongation in the stretching direction, and the air permeability resistance of the stretched sheet is measured at any 12 points using the air permeability tester according to a conventional method, and the arithmetic average value is the air permeability resistance of the sheet. The "maximum elongation" basically means 100% elongation of the sheet, and in the case where the sheet breaks at 100% elongation, it means the largest elongation within the range where the sheet does not break. The larger the air permeability resistance value, the larger the air permeability resistance of the sheet and the lower the air permeability.
[0093] [Table 1]
[0094] As shown in Table 1, in each Example, the release sheet used was mainly made of a material (cellulose fiber) that does not melt or thermally decompose at 200°C, and therefore the peel strength was smaller than in Comparative Examples 2 and 3, which used release sheets that did not contain this material, and the release sheet was able to be peeled off smoothly from the laminate sheet. Furthermore, the stretch sheets obtained in each Example have unevenness on the surface of the exposed parts of the elastic filaments themselves, and fine material (cellulose fiber) derived from the release sheet is attached, giving them a certain level of surface roughness, and therefore they clearly have excellent blocking resistance and storage stability. In Comparative Examples 2 and 3, it is presumed that the release sheet could not be peeled off from the laminated sheet because the content of the low melting point material (e.g., a material with a melting point of less than 200°C, preferably 170°C or less) in the release sheet was relatively high, and the proportion of the low melting point material that was heat fused to the elastic filaments in the total mass of the low melting point material (heat fusion ratio) was too high. Considering the results of this study, it can be said that the content of the low melting point material in the release sheet is preferably 10% by mass or less with respect to the total mass of the release sheet. In addition, it can be said that paper mainly made of cellulose fiber and resin-blended paper with a resin content of 10% by mass or less are preferable as the release sheet, rather than nonwoven fabric mainly made of synthetic fiber. Furthermore, a comparison between Example 2 and Comparative Example 4, and a comparison between Examples 3 and 5 and Comparative Example 5 (comparisons between the same type of nonwoven fabric) makes it clear that a stretch sheet with one layer of exposed elastic filaments has lower air resistance and is more breathable than a stretch sheet with two layers of nonwoven fabric with no exposed elastic filaments. [Explanation of symbols]
[0095] 1 Stretch Sheet 2. Nonwoven fabric 21 Low weight part 22 High-weighted part 3 Elastic filament 4. Raw nonwoven fabric 5 Composite nonwoven fabric 5R Composite nonwoven roll 6 Release sheet 7 Laminated Sheet 10 Spinning equipment 11 Spinning head 11a Spinning nozzle 12,12A 1st roll 13,13A 2nd roll 14 Third Roll 30 Stretching device 31a, 31b Tooth groove roll 32 Roll support shaft 33a, 33b Infeed roll 34a, 34b Outfeed roll
Claims
1. A plurality of elastic filaments in an unstretched state are arranged so as to extend in one direction without intersecting each other and are bonded by fusion to one surface of an extensible nonwoven fabric; A portion of the elastic filament other than the fused portion with the nonwoven fabric is exposed, and a roughness is imparted to the surface of the exposed portion of the elastic filament due to the unevenness of the elastic filament itself, The elastic filaments are exposed at a roughness ratio of 10% or more.
2. The stretch sheet for absorbent articles according to claim 1 , wherein a fine material is attached to the surface of the exposed portion of the elastic filaments.
3. A nonwoven fabric having extensibility, on one side of which are joined by fusion a plurality of elastic filaments in an unstretched state arranged so as to extend in one direction without crossing each other, A portion of the elastic filament other than the fused portion with the nonwoven fabric is exposed, and a roughness is imparted to the surface of the exposed portion of the elastic filament due to the unevenness of the elastic filament itself, A stretch sheet for absorbent articles, wherein a fine material is attached to the surface of the exposed portion of the elastic filaments.
4. The stretch sheet for absorbent articles according to claim 3 , wherein the exposed portions of the elastic filaments have a roughness ratio of 10% or more.
5. The stretch sheet for absorbent articles according to claim 3 or 4, wherein the fine material includes a material that does not melt or thermally decompose at 200°C.
6. The stretch sheet for absorbent articles according to any one of claims 3 to 5, wherein the fine material comprises cellulose fibers.
7. A method for producing a stretch sheet for absorbent articles, comprising bonding a plurality of elastic filaments in an exposed state, the elastic filaments being arranged so as to extend in one direction without crossing each other, to one surface of a stretchable nonwoven fabric, the method comprising the steps of: a composite nonwoven fabric production process in which a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are brought into contact with one side of an original nonwoven fabric before the elastic filaments are solidified, thereby obtaining a composite nonwoven fabric in which the elastic filaments are fused in a state of being exposed on one side of the original nonwoven fabric; a surface roughening step of forming irregularities on the surface of the elastic filament in a portion that does not contact the raw nonwoven fabric; and stretching the composite nonwoven fabric. In the composite nonwoven fabric manufacturing process, the raw nonwoven fabric is wound around one of a pair of opposing rolls and supplied between the pair of rolls, and a plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are supplied between the raw nonwoven fabric and the other of the pair of rolls, a predetermined surface roughness is imparted to the peripheral surface of the other of the pair of rolls, In the surface roughening step, the non-contact portion of the elastic filament is brought into contact with the peripheral surface of the other roll before the elastic filament is solidified, The outer surface of the other roll comprises a material that does not melt or thermally decompose at 200°C.
8. The method for producing a stretch sheet for absorbent articles according to claim 7 , wherein the peripheral surface of the other roll contains cellulose fibers.
9. A method for producing a stretch sheet for absorbent articles, comprising bonding a plurality of elastic filaments in an exposed state, the elastic filaments being arranged so as to extend in one direction without crossing each other, to one surface of a stretchable nonwoven fabric, the method comprising the steps of: A plurality of elastic filaments in a molten or softened state spun from a plurality of spinning nozzles are subjected to the elastic a step of contacting the elastic filaments with one side of an original nonwoven fabric before solidification to obtain a composite nonwoven fabric in which the elastic filaments are fused to one side of the original nonwoven fabric, and contacting a release sheet with a portion of the surface of the elastic filaments that is not in contact with the original nonwoven fabric to obtain a laminated sheet in which the elastic filaments are interposed between the original nonwoven fabric and the release sheet; removing the release sheet from the laminate sheet; and stretching the composite nonwoven fabric. The release sheet is mainly made of a material that does not melt or thermally decompose at 200°C.
Citation Information
Patent Citations
Elastic filament nonwoven fabric and fiber product using the same
JP2004250795A
Elastic filament and stretchable sheet using the same
JP2009030182A
Super-elastic fabric and method for manufacturing the same
JP2014503713A
Method for producing stretch sheet
JP2015112819A
Nonwoven fabric and manufacturing method thereof and absorbent article
JP2016108714A