Barrier film, laminate, and packaging container

A sealant film with a polyolefin resin layer, surface resin layer, and adhesive resin layer, combined with a vapor deposition layer, addresses low adhesion issues, improving barrier properties and lamination strength in packaging containers.

JP7591193B2Active Publication Date: 2024-11-28DAI NIPPON PRINTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020206077
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-11
Publication Date
2024-11-28
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

The adhesion between the sealant film and the vapor deposition layer is low, leading to poor barrier properties in packaging containers.

Method used

A sealant film comprising a polyolefin resin layer, a surface resin layer with a polar group, an adhesive resin layer, and a vapor deposition layer, with specific thickness ratios and materials to enhance adhesion and barrier properties.

Benefits of technology

Improves the barrier properties of the film and laminate, enhancing oxygen and water vapor barrier, light shielding, and lamination strength while maintaining recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591193000004
    Figure 0007591193000004
  • Figure 0007591193000005
    Figure 0007591193000005
  • Figure 0007591193000006
    Figure 0007591193000006
Patent Text Reader

Abstract

To enhance barrier properties of a barrier film having a sealant film and a vapor-deposited layer.SOLUTION: A barrier film includes: a sealant film having a first face and a second face located on an opposite side of the first face; and a vapor-deposited layer located on the second face. The sealant film includes: a polyolefin resin layer composing the first face; a surface resin layer composing the second face and containing a resin material having a polar group; and an adhesive resin layer located between the polyolefin resin layer and the surface resin layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a barrier film, a laminate, and a packaging container. [Background technology]

[0002] 2. Description of the Related Art Laminates in which a plurality of films are laminated are used as components for constituting packaging containers such as pouches. The laminates include a substrate and a sealant film.

[0003] Packaging containers are sometimes required to have barrier properties against oxygen, water vapor, etc. For example, Patent Document 1 proposes forming an aluminum vapor deposition layer on the surface of a sealant film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-179878 A Summary of the Invention [Problem to be solved by the invention]

[0005] If the adhesion between the sealant film and the deposition layer is poor, the barrier properties will also be poor.

[0006] The present invention has been made in consideration of the above points, and has an object to improve the barrier properties of a barrier film including a sealant film and a deposition layer. [Means for solving the problem]

[0007] The present invention relates to A sealant film including a first surface and a second surface opposite to the first surface; a deposition layer located on the second surface, The sealant film is a barrier film comprising a polyolefin resin layer constituting the first surface, a surface resin layer constituting the second surface and containing a resin material having a polar group, and an adhesive resin layer located between the polyolefin resin layer and the surface resin layer.

[0008] In the barrier film of the present invention, the resin material may be one or more resin materials selected from ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyester, nylon 6, nylon 6,6, MXD nylon, and amorphous nylon.

[0009] In the barrier film of the present invention, the surface resin layer may contain an ethylene-vinyl alcohol copolymer and have a thickness of 3 μm or more, and the adhesive resin layer may have a thickness of 3 μm or more.

[0010] In the barrier film of the present invention, the surface resin layer may contain nylon 6, nylon 6,6 or MXD nylon and have a thickness of 2 μm or more, The adhesive resin layer may have a thickness of 2 μm or more.

[0011] In the barrier film of the present invention, the ratio of the thickness of the surface resin layer to the thickness of the sealant film may be 1% or more and 20% or less.

[0012] In the barrier film of the present invention, the polyolefin resin layer may be a polypropylene resin layer.

[0013] In the barrier film of the present invention, the polypropylene resin layer may include a first copolymer layer and a second copolymer layer, and a homopolymer layer located between the first copolymer layer and the second copolymer layer.

[0014] In the barrier film of the present invention, the vapor deposition layer may include a metal layer or an inorganic oxide layer.

[0015] In the barrier film of the present invention, a value obtained by dividing the breaking energy of the sealant film by the thickness of the sealant film may be 0.0025 J / μm or more.

[0016] The present invention is a laminate comprising the above-described barrier film and a substrate.

[0017] In the laminate of the present invention, the substrate may include a stretched plastic film. In this case, the laminate may include a printed layer located between the substrate and the barrier film.

[0018] In the laminate of the present invention, the substrate may comprise a stretched plastic film. In this case, the laminate may comprise an adhesive layer located between the substrate and the barrier film.

[0019] In the laminate of the present invention, the substrate may include paper.

[0020] The present invention is a packaging container comprising the above-described laminate. Effect of the Invention

[0021] According to the present invention, the barrier properties of a barrier film including a sealant film and a vapor deposition layer can be improved. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a barrier film in the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a barrier film in the present embodiment. [Diagram 3] FIG. 1 is a diagram illustrating an example of a deposition apparatus. [Figure 4] FIG. 1 is a diagram illustrating an example of a deposition apparatus. [Diagram 5] FIG. 2 is a cross-sectional view showing an example of a laminate according to the present embodiment. [Figure 6]FIG. 2 is a cross-sectional view showing an example of a laminate according to the present embodiment. [Figure 7] FIG. 2 is a diagram showing an example of a method for measuring laminate strength. [Figure 8] FIG. 2 is a diagram showing an example of a method for measuring laminate strength. [Figure 9] FIG. 13 is a diagram showing an example of measurement results of laminate strength. [Figure 10] FIG. 1 is a diagram showing an example of a packaging container. [Figure 11] FIG. 1 is a diagram showing an example of a packaging container. [Figure 12] FIG. 1 is a diagram showing an example of a packaging container. [Figure 13] FIG. 1 is a diagram showing the evaluation results of examples and comparative examples. [Figure 14] FIG. 1 is a diagram showing the evaluation results of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings, in which the scale and aspect ratios have been appropriately changed and exaggerated from those of the actual objects for the sake of illustration and ease of understanding.

[0024] In addition, terms used in this specification that specify shapes, geometric conditions, and the extent thereof, such as "orthogonal" and "same," as well as values ​​of length and angle, are not bound by strict meanings, but are interpreted to include a range within which similar functions can be expected.

[0025] (Barrier film) 1 is a cross-sectional view showing an example of a barrier film 10 according to the present embodiment. The barrier film 10 includes a sealant film 20 and a deposition layer 30. The sealant film 20 includes a first surface 20x and a second surface 20y. The second surface 20y is a surface located opposite to the first surface 20x. The deposition layer 30 is located on the second surface 20y.

[0026] 1, the sealant film 20 includes a polyolefin resin layer 21, an adhesive resin layer 22, and a surface resin layer 23. The polyolefin resin layer 21 constitutes a first surface 20x. The surface resin layer 23 constitutes a second surface 20y. The adhesive resin layer 22 is located between the polyolefin resin layer 21 and the surface resin layer 23.

[0027] 2 is a cross-sectional view showing another example of the barrier film 10. In the example shown in FIG. 2, the polyolefin resin layer 21 is a polypropylene resin layer. In this case, the polyolefin resin layer 21 may include a first copolymer layer 21a, a homopolymer layer 21b, and a second copolymer layer 21c. The first copolymer layer 21a may constitute the first surface 20x of the sealant film 20. The homopolymer layer 21b is located between the first copolymer layer 21a and the second copolymer layer 21c. The second copolymer layer 21c may be in contact with the adhesive resin layer 22.

[0028] Each component of the barrier film 10 will now be described in detail.

[0029] [Sealant film] The sealant film 20 is a film produced by coextrusion. The sealant film 20 is preferably an unstretched film. The term "unstretched" refers not only to a film that is not stretched at all, but also to a film that is slightly stretched due to tension applied during film formation.

[0030] The breaking strength of the sealant film 20 in at least one direction is, for example, 100 MPa or less, and may be 50 MPa or less. For example, the breaking strength of the sealant film 20 in the machine direction and the perpendicular direction may be 100 MPa or less, and may be 50 MPa or less. The breaking elongation of the sealant film 20 in at least one direction is, for example, 300% or more, and may be 350% or more. For example, the tensile elongation of the sealant film 20 in the machine direction and the perpendicular direction may be 300% or more, and may be 350% or more.

[0031] The breaking strength is the stress applied to the sealant film 20 when it breaks. The breaking elongation is the elongation occurring in the sealant film 20 when it breaks. The breaking strength and tensile elongation of the sealant film 20 are measured in accordance with JIS K7127. As a measuring instrument, a Tensilon universal material testing machine RTC-1310 manufactured by A&D can be used. In the measurement, a rectangular film cut from the sealant film 20 with a width of 10 mm and a length of 150 mm is used as a test piece. The distance between a pair of chucks holding the test piece at the start of the measurement is 50 mm. The tensile speed of the test piece is 300 mm / min. The environment during the measurement is a temperature of 23°C and a relative humidity of 50% RH.

[0032] Next, each layer of the sealant film 20 will be described.

[0033] [Polyolefin resin layer] The polyolefin resin layer 21 includes a polymer synthesized using an olefin such as ethylene or propylene as a monomer. For example, the polyolefin resin layer 21 includes polyethylene, polypropylene, etc. The polyolefin resin layer 21 may be a polypropylene resin layer.

[0034] The polypropylene contained in the polyolefin resin layer 21 may be either a homopolymer or a copolymer. The copolymer may be either a block copolymer or a random copolymer.

[0035] A block copolymer is a copolymer having a polymer block of propylene and a polymer block of an α-olefin other than propylene. For example, a block copolymer includes a polymer block of ethylene, butene-1, 4-methyl-1-pentene, etc. in addition to a polymer block of propylene. For example, a block copolymer includes a propylene-ethylene block copolymer. The structural formula of a propylene-ethylene block copolymer is shown in formula (I).

[0036] [ka]

[0037] A random copolymer is a random copolymer containing propylene and an α-olefin other than propylene. For example, the random copolymer contains ethylene, butene-1, 4-methyl-1-pentene, etc. in addition to propylene. For example, the random copolymer includes a propylene-ethylene random copolymer. The structural formula of a propylene-ethylene random copolymer is shown in formula (II). The random copolymer may include a terpolymer.

[0038] [ka]

[0039] A homopolymer is a polymer of only propylene. The structural formula of a propylene homopolymer is shown in formula (III).

[0040] [ka]

[0041] Homopolymers have higher crystallinity than random polymers. When emphasis is placed on rigidity, heat resistance, etc., it is preferable to use homopolymers. When emphasis is placed on impact resistance, sealability, etc., it is preferable to use random copolymers or block copolymers.

[0042] The polyolefin resin layer 21 may contain biomass-derived polypropylene. The polyolefin resin layer 21 may contain mechanically recycled or chemically recycled polypropylene.

[0043] The thickness of the polyolefin resin layer 21 is, for example, 20 μm or more, and may be 40 μm or more. The thickness of the polyolefin resin layer 21 is, for example, 100 μm or less, and may be 80 μm or less.

[0044] As shown in FIG. 2, the polyolefin resin layer 21 may include a first copolymer layer 21a, a homopolymer layer 21b, and a second copolymer layer 21c. The first copolymer layer 21a and the second copolymer layer 21c include the above-mentioned polypropylene copolymer. The homopolymer layer 21b includes the above-mentioned polypropylene homopolymer. The polyolefin resin layer 21 includes the first copolymer layer 21a, thereby improving the sealing property of the sealant film 20. The polyolefin resin layer 21 includes the homopolymer layer 21b, thereby preventing defects such as pinholes and cuts from occurring in the barrier film 10 due to the flow of polypropylene during heating. The polyolefin resin layer 21 includes the second copolymer layer 21c, thereby improving the adhesion between the polyolefin resin layer 21 and the adhesive resin layer 22.

[0045] The thickness of the first copolymer layer 21a is, for example, 5 μm or more, and may be 10 μm or more. The thickness of the first copolymer layer 21a is, for example, 20 μm or less, and may be 17 μm or less.

[0046] The thickness of the homopolymer layer 21b is, for example, 10 μm or more, and may be 15 μm or more. The thickness of the homopolymer layer 21b is, for example, 50 μm or less, and may be 30 μm or less. The thickness of the homopolymer layer 21b may be greater than the thickness of the first copolymer layer 21a.

[0047] The thickness of the second copolymer layer 21c is, for example, 2 μm or more, and may be 3 μm or more. The thickness of the second copolymer layer 21c is, for example, 20 μm or less, and may be 15 μm or less, or may be 10 μm or less. The thickness of the second copolymer layer 21c may be smaller than the thickness of the first copolymer layer 21a and the thickness of the homopolymer layer 21b.

[0048] When the polyolefin resin layer 21 is a polypropylene resin layer, the polypropylene content in the polyolefin resin layer 21 is, for example, 70% by mass or more, optionally 80% by mass or more, or optionally 90% by mass or more.

[0049] The polypropylene resin layer may contain a resin material other than polypropylene. For example, the polypropylene resin layer may contain a polyolefin such as polyethylene, a (meth)acrylic resin, a vinyl resin, a cellulose resin, a polyamide resin, a polyester, an ionomer resin, or the like.

[0050] (Surface resin layer) The surface resin layer 23 contains a resin material having a polar group. Therefore, the deposition layer 30 easily adheres to the surface of the surface resin layer 23. This can improve the barrier properties of the barrier film 10.

[0051] The polar group means a group containing one or more heteroatoms. The polar group is, for example, an ester group, an epoxy group, a hydroxyl group, an amino group, an amide group, a carboxyl group, a carbonyl group, a carboxylic anhydride group, a sulfone group, a thiol group, and a halogen group. The polar group is preferably a hydroxyl group, an ester group, an amino group, an amide group, a carboxyl group, or a carbonyl group, and more preferably a hydroxyl group.

[0052] The resin material of the surface resin layer 23 is, for example, an ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyamide resin, etc. The polyamide resin is nylon 6, nylon 6,6, MXD nylon, amorphous nylon, etc. The resin material of the surface resin layer 23 is preferably an ethylene-vinyl alcohol copolymer or polyvinyl alcohol.

[0053] The surface resin layer 23 may contain additives as long as the adhesion of the vapor deposition layer 30 to the surface resin layer 23 is not impaired. Examples of additives include crosslinking agents, antioxidants, antiblocking agents, lubricants (slip agents), UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0054] The ratio of the thickness of the surface resin layer 23 to the thickness of the sealant film 20 is, for example, 1% or more, or may be 3% or more, or may be 5% or more. This can improve the adhesion of the deposition layer 30 to the surface resin layer 23. This can improve the barrier properties of the barrier film 10. In addition, the lamination strength of the laminate including the barrier film 10 can be increased.

[0055] The ratio of the thickness of the surface resin layer 23 to the thickness of the sealant film 20 is, for example, 20% or less, may be 15% or less, or may be 10% or less. This can improve the film formability and processability of the sealant film 20. In addition, the recyclability of the barrier film 10 and the recyclability of the laminate including the barrier film 10 can be improved.

[0056] The thickness of the surface resin layer 23 is, for example, 1 μm or more, may be 2 μm or more, or may be 3 μm or more. The thickness of the surface resin layer 23 is, for example, 5 μm or less, or may be 4 μm or less.

[0057] [Adhesive resin layer] The adhesive resin layer 22 contains a resin that bonds the polyolefin resin layer 21 and the surface resin layer 23. By providing the adhesive resin layer 22, the adhesion between the polyolefin resin layer 21 and the surface resin layer 23 can be increased.

[0058] The adhesive resin layer 22 may contain an adhesive resin such as polyether, polyester, silicone resin, epoxy resin, polyurethane, vinyl resin, phenol resin, and polyolefin. Preferably, the adhesive resin layer 22 contains polyolefin and an acid-modified product thereof. When the polyolefin resin layer 21 is a polypropylene resin layer, the adhesive resin layer 22 preferably contains polypropylene and an acid-modified product thereof. This can increase the proportion of polypropylene in the barrier film 10. This can increase the recyclability of the barrier film 10 and the laminate and packaging container described below. The adhesive resin layer 22 may contain commercially available polypropylene and its acid-modified product. For example, the adhesive resin layer 22 may contain the Admer series manufactured by Mitsui Chemicals, Inc.

[0059] The thickness of the adhesive resin layer 22 is, for example, 1 μm or more, may be 2 μm or more, or may be 3 μm or more. This can further increase the adhesion between the polyolefin resin layer 21 and the surface resin layer 23. The thickness of the adhesive resin layer 22 is, for example, 15 μm or less, may be 10 μm or less, or may be 5 μm or less. This can further increase the processability of the sealant film 20.

[0060] [Vapour-deposited layer] The deposition layer 30 includes a metal layer or an inorganic oxide layer. The deposition layer 30 is difficult to pass gases such as oxygen and water vapor. Therefore, the barrier film 10 and the laminate described later can have barrier properties such as oxygen barrier property and water vapor barrier property. This can prevent the weight of the contents from decreasing in a packaging container made of the laminate. In addition, it can prevent light from passing through the laminate and reaching the contents. This can prevent oxidation of the components of the contents such as oil.

[0061] The metal layer may comprise a metal such as aluminum. For example, the metal layer may comprise a layer of aluminum vapor-deposited on the surface resin layer 23.

[0062] The inorganic oxide layer may contain inorganic oxides such as aluminum oxide (alumina), silicon oxide (silica), magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, silicon carbide oxide (carbon-containing silicon oxide), etc. Preferably, the inorganic oxide layer contains silica, silicon carbide oxide, or alumina. Silica is preferred in that no aging treatment is required after forming the vapor deposition layer.

[0063] The thickness of the deposition layer 30 is, for example, 1 nm or more, may be 5 nm or more, or may be 10 nm or more. This can further improve the barrier properties of the barrier film 10. The thickness of the deposition layer 30 may be 150 nm or less, may be 100 nm or less, or may be 50 nm or less. This can suppress the occurrence of defects such as cracks in the deposition layer 30. In addition, the recyclability of the laminate and the packaging container can be improved.

[0064] The deposition layer 30 may be composed of a single layer or may include multiple layers. A single layer is a layer formed by one deposition process. Multiple layers are formed by multiple deposition processes. The materials constituting the multiple layers may be the same or different. The methods of forming the multiple layers may be the same or different.

[0065] (Barrier film manufacturing method) Next, a method for producing the barrier film 10 will be described.

[0066] First, the sealant film 20 is produced by a co-extrusion method. Specifically, the polyolefin constituting the polyolefin resin layer 21, the adhesive resin constituting the adhesive resin layer 22, and the resin material constituting the surface resin layer 23 are extruded together using a T-die method, an inflation method, or the like. In this way, the sealant film 20 can be produced. When the polyolefin resin layer 21 includes a first copolymer layer 21a, a homopolymer layer 21b, and a second copolymer layer 21c as shown in FIG. 2, the material of each polymer layer is extruded together with the adhesive resin constituting the adhesive resin layer 22 and the resin material constituting the surface resin layer 23.

[0067] Next, a deposition layer 30 is formed by deposition on the surface resin layer 23 of the sealant film 20. In this way, the barrier film 10 including the sealant film 20 and the deposition layer 30 can be obtained.

[0068] Known methods can be used to form the deposition layer 30. For example, physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition can be used.

[0069] The surface resin layer 23 may be subjected to a surface treatment, which can improve adhesion to the deposition layer 30. The method of the surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals.

[0070] When forming the deposition layer 30 by the PVD method, a vacuum film-forming apparatus having a plasma assist function may be used as described below. For example, as shown in Figs. 3 and 4, the vacuum film-forming apparatus may include a vacuum container 101, an unwinding section 102, a film-forming drum 103, a winding section 104, a conveying roll 105, an evaporation source 106, an adhesion-preventing box 108, a deposition material 109, and a plasma gun 110. When the deposition layer 30 contains an inorganic oxide, the vacuum film-forming apparatus may include a reaction gas supply section 107. Fig. 3 is a schematic cross-sectional view of the vacuum film-forming apparatus in the XZ plane. Fig. 4 is a schematic cross-sectional view of the vacuum film-forming apparatus in the XY plane.

[0071] As shown in Fig. 3, the sealant film 20 wound around the film-forming drum 103 is arranged so that the surface resin layer 23 faces downward. An electrically grounded deposition-protection box 108 is arranged below the film-forming drum 103. An evaporation source 106 is arranged on the bottom surface of the deposition-protection box 108. The film-forming drum 103 is arranged at a position facing the upper surface of the evaporation source 106 at a certain interval in the vertical direction. Transport rolls 105 are arranged between the unwinding section 102 and the film-forming drum 103, and between the film-forming drum 103 and the winding section 104. Although not shown, the vacuum container 101 is connected to a vacuum pump.

[0072] The evaporation source 106 holds the deposition material 109. Although not shown, the evaporation source 106 is equipped with a heating device. The reactive gas supply unit 107 supplies a reactive gas that reacts with the evaporated deposition material 109. The reactive gas may be oxygen, nitrogen, helium, argon, or a mixture of these gases. When the deposition layer 30 contains an inorganic oxide, the reactive gas supply unit 107 supplies oxygen.

[0073] The deposition material 109 evaporated from the evaporation source 106 is directed toward the surface resin layer 23 of the sealant film 20. Plasma is irradiated from the plasma gun 110 toward the surface resin layer 23. This forms the deposition layer 30. Details of such a formation method are disclosed in, for example, JP 2011-214089 A.

[0074] Next, an example of forming an inorganic oxide deposition layer 30 by plasma enhanced chemical vapor deposition will be described. As the plasma generating device, a device that generates high frequency plasma, pulse wave plasma, microwave plasma, or the like can be used. Also, a device having two or more film formation chambers may be used. The device is preferably equipped with a vacuum pump, which allows each film formation chamber to be maintained in a vacuum. The degree of vacuum in each film formation chamber is 1×10 Pa to 1×10 -6 It is preferable that the vapor deposition layer 30 is formed at a pressure of 100 Pa. An example of a method for forming the vapor deposition layer 30 using a plasma generating device will be described below.

[0075] First, the sealant film 20 is sent into a film-forming chamber. Then, the sealant film 20 is transported onto a drum at a predetermined speed. Then, a mixed gas composition containing a film-forming monomer gas containing an inorganic oxide, oxygen gas, an inert gas, and the like is supplied from a gas supply device into the film-forming chamber. The surface resin layer 23 is irradiated with plasma generated by glow discharge to form a deposition layer 30 on the surface resin layer 23. Details of such a formation method are disclosed, for example, in JP 2012-076292 A.

[0076] As an apparatus used in the method for forming a vapor-deposited film, a continuous vapor-deposited film-forming apparatus including a plasma pretreatment chamber and a film-forming chamber may be used, as described below. First, in a plasma pretreatment chamber, plasma is irradiated from a plasma supply nozzle onto the surface resin layer 23 of the sealant film 20. Then, in a film formation chamber, a deposition layer 30 is formed on the surface resin layer 23. Details of such a formation method are disclosed, for example, in International Publication WO2019 / 087960.

[0077] The surface of the deposition layer 30 may be subjected to the above-mentioned surface treatment.

[0078] (Effect of sealant film) In this embodiment, the sealant film 20 has a surface resin layer 23 that contains a resin material having a polar group. Therefore, by forming a vapor deposition layer 30 on the surface resin layer 23, it is possible to improve the adhesion between the sealant film 20 and the vapor deposition layer 30. This makes it possible to improve the barrier properties of the barrier film 10. Furthermore, when the vapor deposition layer 30 contains a metal layer made of aluminum or the like, it is possible to improve the light blocking properties of the barrier film 10.

[0079] In the present embodiment, the sealant film 20 includes the first copolymer layer 21a, and thus the impact resistance of the sealant film 20 can be increased. The breaking energy of the sealant film 20 is, for example, 0.1 J or more, and may be 0.2 J or more, or may be 0.3 J or more. The value obtained by dividing the breaking energy of the sealant film 20 by the thickness of the sealant film 20 is, for example, 0.0025 J / μm or more, and may be 0.0050 J / μm or more, or may be 0.0075 J / μm or more. These values ​​also hold for the barrier film 10 including the sealant film 20 and the vapor deposition layer 30.

[0080] A film impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd. is used as a measuring device for measuring the breaking energy of the sealant film 20. Specifically, the hammer of the film impact tester applies an impact to a test piece of the sealant film 20 in a state in which tension is applied. The strength at which the test piece breaks is measured. A 3J hammer is used. The diameter of the impact ball at the tip of the hammer is 12.7 mm. The lifting angle of the hammer is 90°. The test piece includes an effective dimensional area consisting of a circle with a diameter of 35 mm. For example, the shape of the test piece is a square with each piece being 100 mm. In the measurement, the test piece is held by a chuck and an impact is applied to the effective dimensional area of ​​the test piece by the hammer.

[0081] The five test pieces are measured for the breaking energy of the sealant film 20. The average of the breaking energies of the five test pieces is used as the breaking energy of the sealant film 20. The measurement is performed in an environment with a temperature of 23° C. and a relative humidity of 50% RH.

[0082] The oxygen permeability of the barrier film 10 is, for example, 0.50 cc / m 2 ·day·atm or less, 0.40cc / m 2 ·day·atm or less, 0.30cc / m 2 The oxygen permeability may be less than 10 ...

[0083] The water vapor permeability of the barrier film 10 is, for example, 2.0 g / m 2 -day or less, 1.0g / m 2 · day or less, 0.50g / m 2 The water vapor permeability is measured in an environment of a temperature of 40° C. and a relative humidity of 90% RH in accordance with JIS K 7129. A water vapor permeability measuring device PERMATRAN-w 3 / 33 manufactured by MOCON is used as a measuring device for the water vapor permeability.

[0084] The total light transmittance of the barrier film 10 is, for example, 1.0% or less, may be 0.50% or less, or may be 0.20% or less. The total light transmittance is measured in an environment of a temperature of 23° C. and a relative humidity of 90% RH in accordance with JIS K 7361. A haze meter MDH4000 manufactured by Nippon Denshoku Industries Co., Ltd. is used as a measuring device for the total light transmittance.

[0085] In this embodiment, the polyolefin resin layer 21 includes the first copolymer layer 21a, the homopolymer layer 21b, and the second copolymer layer 21c. The polyolefin resin layer 21 includes the first copolymer layer 21a, which can improve the sealing property and impact resistance of the sealant film 20. The polyolefin resin layer 21 includes the homopolymer layer 21b, which can prevent defects such as pinholes and cuts from occurring in the barrier film 10 due to the flow of polypropylene during heating. In addition, the homopolymer layer 21b has a high heat resistance temperature and therefore has high rigidity. This can improve the resistance of the barrier film 10 to bending fatigue. The polyolefin resin layer 21 includes the second copolymer layer 21c, which can improve the adhesion between the polyolefin resin layer 21 and the adhesive resin layer 22.

[0086] The thickness of the barrier film 10 is, for example, 20 μm or more, and may be 40 μm or more. The thickness of the barrier film 10 is, for example, 80 μm or less, and may be 60 μm or less.

[0087] (Laminate) Next, a description will be given of a laminate including the barrier film 10. The laminate may be used as a packaging material that constitutes a packaging container.

[0088] 5 is a cross-sectional view showing an example of a laminate 50 according to the present embodiment. The laminate 50 includes a substrate 40 and a sealant film 20. The laminate 50 includes an inner surface 50x and an outer surface 50y. The inner surface 50x is formed by the polyolefin resin layer 21 of the sealant film 20. The outer surface 50y may be formed by the substrate 40.

[0089] [Base material] The substrate 40 faces the second surface 20y of the sealant film 20. The sealant film 20 and the substrate 40 may be laminated by, for example, a dry lamination method. In this case, the adhesive layer 45 is located between the substrate 40 and the sealant film 20.

[0090] The substrate 40 may include a plastic film. For example, the substrate 40 may include a polyolefin film such as a polyethylene film or a polypropylene film, a polyester film such as a polyethylene terephthalate film or a polybutylene terephthalate film, or a polyamide film such as a nylon film or a nylon 6 / metaxylylenediamine nylon 6 coextruded costretched film. The substrate 40 may include only one plastic film, or may include two or more plastic films.

[0091] Preferably, the substrate 40 includes a polyolefin film. When the polyolefin resin layer 21 of the sealant film 20 is a polypropylene resin layer, the substrate 40 preferably includes a polypropylene film. This can increase the proportion of polypropylene in the laminate 50. This can increase the recyclability of the laminate 50 and the packaging container.

[0092] The plastic film may be stretched in a predetermined direction. In the following description, the stretched plastic film is also referred to as a stretched plastic film. The plastic film may be a uniaxially stretched film stretched in one predetermined direction, or a biaxially stretched film stretched in two predetermined directions. The stretching ratio may be 2 times or more, or 5 times or more. The stretching ratio may be 15 times or less, or 13 times or less.

[0093] The thickness of the stretched plastic film is, for example, 10 μm or more, and may be 15 μm or more. This can increase the strength and heat resistance of the laminate 50. The thickness of the stretched plastic film is, for example, 50 μm or less, and may be 40 μm or less. This can increase the film-forming property and processability of the substrate 40.

[0094] When the substrate 40 includes a plastic film, the laminate 50 may include a printed layer 41 located between the substrate 40 and the adhesive layer 45, as shown in FIG. 6. The printed layer 41 is a layer for displaying product information and imparting aesthetic appeal to the packaging container. The printed layer 41 expresses letters, numbers, symbols, figures, pictures, and the like. As a material for forming the printed layer 41, ink for gravure printing or ink for flexographic printing can be used. A specific example of an ink for gravure printing is Finart manufactured by DIC Graphics Corporation.

[0095] When the vapor-deposited layer 30 includes a metal layer made of aluminum or the like, the printed layer 41 becomes invisible when the vapor-deposited layer 30 is formed on the substrate 40. In the present embodiment, the vapor-deposited layer 30 is formed on the sealant film 20, and therefore the printed layer 41 can be visually recognized from the outer surface 50y side of the laminate 50.

[0096] The substrate 40 may include paper. The basis weight of the paper is, for example, 20 g / m 2 More than 40g / m 2 or more, and 2 The basis weight of the paper may be, for example, 150 g / m 2 Less than or equal to 100 g / m 2 or less, 80 g / m 2 The paper may be kraft paper, art paper, coated paper, glassine paper, pure white roll paper, bleached kraft paper, high-quality paper, or the like.

[0097] The adhesion of the vapor-deposited layer 30 to paper is low. Therefore, when the vapor-deposited layer 30 is formed on paper, the laminate 50 has low lamination strength. According to the present embodiment, the vapor-deposited layer 30 is formed on the sealant film 20. Therefore, even when the laminate 50 includes paper and the vapor-deposited layer 30, the laminate strength of the laminate 50 can be increased.

[0098] [Adhesive layer] The adhesive layer 45 is a layer for bonding the substrate 40 and the sealant film 20 by a dry lamination method. The adhesive layer 45 is formed by applying an adhesive to the substrate 40 or the surface of the substrate 40 and drying it. As the adhesive constituting the adhesive layer 45, for example, one-component or two-component curing or non-curing type vinyl, (meth)acrylic, polyamide, polyester, polyether, polyurethane, epoxy, rubber, and other solvent-based, water-based, or emulsion-type adhesives can be used. As the two-component curing adhesive, a cured product of polyol and an isocyanate compound can be used. For example, the two-component curing adhesive may contain a cured product of polyester polyol and an isocyanate compound. For example, the two-component curing adhesive may contain an oxygen barrier adhesive PASLIM manufactured by DIC Corporation. The oxygen barrier adhesive PASLIM contains a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound. An example of the oxygen barrier adhesive PASLIM is PASLIM VM001 / VM102CP. PASLIM VM001 / VM102CP contains a polyester-based main skeleton and a curing agent having two or more isocyanate groups. The adhesive can be applied by, for example, a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fountain method, a transfer roll coating method, or other methods.

[0099] The thickness of the adhesive layer 45 is, for example, 1 μm or more, and may be 2 μm or more. The thickness of the adhesive layer 45 is, for example, 5 μm or less, and may be 4 μm or less.

[0100] (Effect of laminate) In this embodiment, the sealant film 20 includes a surface resin layer 23 containing a resin material having a polar group. Therefore, by forming a deposition layer 30 on the surface resin layer 23, it is possible to improve the adhesion between the sealant film 20 and the deposition layer 30. This makes it possible to increase the lamination strength of the laminate 50.

[0101] The laminate strength of the laminate 50 is, for example, 0.5 N / 15 mm or more, may be 1.5 N / 15 mm or more, may be 2.0 N / 15 mm or more, or may be 2.5 N / 15 mm or more. The laminate strength of the laminate 50 is, for example, 5.0 N / 15 mm or less, may be 4.0 N / 15 mm or less. The laminate strength is measured in accordance with JIS K 6854-2 under an environment of a temperature of 23° C. and a relative humidity of 90% RH. A&D Tensilon universal material testing machine RTC-1310 is used as a measuring device for the laminate strength.

[0102] A method for measuring the laminate strength will be described with reference to Figs. 7 to 9. First, the laminate 50 was cut out to prepare a rectangular test piece including a long side and a short side. The length of the short side was 15 mm. Next, as shown in Fig. 7, the sealant film 20 and the substrate 40 were peeled off over 15 mm in the direction of the long side. Next, as shown in Fig. 8, the peeled parts of the test piece were gripped by the gripper 56 and the gripper 57. Next, the gripper 56 and the gripper 57 were pulled at a speed of 50 mm / min in opposite directions perpendicular to the surface direction of the test piece. The tensile stress applied to the gripper 56 and the gripper 57 was measured. When the pulling started, the distance S between the gripper 56 and the gripper 57 was 30 mm. When the pulling ended, the distance S between the gripper 56 and the gripper 57 was 60 mm.

[0103] Fig. 9 is a diagram showing an example of the measurement results of the tensile stress. In Fig. 9, the horizontal axis represents the distance S between the gripping tools 56, 57, and the vertical axis represents the tensile stress F applied to the gripping tools 56, 57. The change in the tensile stress F relative to the distance S passes through a first region R1 and enters a second region R2 where the rate of change of the tensile stress is smaller than that of the first region R1. The second region R2 is also called a stable region.

[0104] The tensile stress F in the second region R2 is measured for the five test pieces. Then, the average value of the tensile stress F in the second region R2 is calculated for each of the five test pieces. The average of the five average values ​​is used as the laminate strength of the laminate 50. The measurement was performed in an environment with a temperature of 23°C and a relative humidity of 50% RH.

[0105] In the present embodiment, the laminate 50 includes the barrier film 10, and thus the barrier property of the laminate 50 can be improved. In addition, when the deposition layer 30 includes a metal layer made of aluminum or the like, the light blocking property of the laminate 50 can be improved.

[0106] The oxygen permeability of the laminate 50 is, for example, 0.50 cc / m 2 ·day·atm or less, 0.40cc / m 2 ·day·atm or less, 0.30cc / m 2 The oxygen permeability is measured in the same manner as in the sealant film 20, in accordance with JIS K 7126, at a temperature of 23° C. and a relative humidity of 90%.

[0107] The water vapor permeability of the laminate 50 is, for example, 2.0 g / m 2 -day or less, 1.0g / m 2 · day or less, 0.50g / m 2 The water vapor permeability is measured in the same manner as in the sealant film 20, in accordance with JIS K 7129, at a temperature of 40° C. and a relative humidity of 90% RH.

[0108] The total light transmittance of the laminate 50 is, for example, 1.0% or less, may be 0.50% or less, or may be 0.20% or less. The total light transmittance is measured in an environment of a temperature of 23° C. and a relative humidity of 90% RH in accordance with JIS K 7361, as in the case of the sealant film 20.

[0109] The thickness of the laminate 50 is, for example, 20 μm or more, may be 30 μm or more, or may be 50 μm or more. The thickness of the laminate 50 is, for example, 100 μm or less, may be 90 μm or less, or may be 80 μm or less.

[0110] (packaging container) The packaging container of the present invention includes the above-mentioned laminate 50. When the substrate 40 includes a plastic film, the packaging container is, for example, a pouch, a lid material, a laminated tube, etc. When the substrate 40 includes paper, the packaging container is, for example, a paper container, etc.

[0111] Examples of packaging bags include packaging bags of various shapes, such as standing pouch type, side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, grommet seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, and gusset type.

[0112] As an example of the pouch, a standing pouch will be described. FIG. 10 is a diagram showing a simplified example of the configuration of a standing pouch. The packaging container 60 includes a body portion (side sheet) 61 and a bottom portion (bottom sheet) 62. The side sheet 61 and the bottom sheet 62 of the packaging container 60 may be made of the same material, or may be made of different materials. For example, both the side sheet 61 and the bottom sheet 62 may be the laminate 50 described above. Alternatively, either the side sheet 61 or the bottom sheet 62 may be the laminate 50 described above.

[0113] FIG. 11 is a diagram showing another example of a pouch. In the manufacturing process of the pouch of FIG. 11, two laminates 50 are prepared and stacked so that the polyolefin resin layers 21 face each other. Next, two other laminates folded in a V-shape are inserted between the two laminates 50 at one side end and the other side end of the two laminates 50. At this time, the sealant layers of the other two laminates face outward. Next, Ox sealing is performed along one side end and the other side end and the bottom end of the two laminates 50. This makes it possible to produce a side-set pouch as shown in FIG. 11.

[0114] Fig. 12 is a diagram showing another example of a pouch. As shown in Fig. 12, the packaging container 60 may be a pouch that does not have a gusset portion.

[0115] As the heat sealing method, for example, a known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc. can be used.

[0116] The contents filled in the packaging container are not particularly limited. The contents may be liquid, powder, or gel. The contents may be food or non-food. EXAMPLES

[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0118] Example 1 A sealant film 20 including a surface resin layer 23, an adhesive resin layer 22, a second copolymer layer 21c, a homopolymer layer 21b, and a first copolymer layer 21a was produced by a co-extrusion method. The surface resin layer 23 was made of nylon 6 Ultramid (registered trademark) B36LN manufactured by BASF. The adhesive resin layer 22 was made of maleic anhydride modified polypropylene QF551 manufactured by Mitsui Chemicals. The second copolymer layer 21c was made of polypropylene random copolymer PC630A manufactured by SunAllomer. The homopolymer layer 21b was made of polypropylene homopolymer PC600A manufactured by SunAllomer. The first copolymer layer 21a was made of polypropylene random copolymer PC630A manufactured by SunAllomer. The thicknesses of the surface resin layer 23, the adhesive resin layer 22, the second copolymer layer 21c, the homopolymer layer 21b and the first copolymer layer 21a were 3 μm, 4 μm, 3 μm, 17 μm and 13 μm, respectively. The viscosity number of the surface resin layer 23 was 218 ml / g (ISO307) and the density was 1.15 g / cm 3 The adhesive resin layer 22 had a melting point of 220° C. The MFR of the adhesive resin layer 22 was 5.7 g / 10 min (ASTM D1238) and a density of 0.890 g / cm 3 The MFR and density of the copolymer layers 21a and 21c were 7.5 g / 10 min and 0.9 g / cm 3 The MFR and density of the homopolymer layer 21b were 7.5 g / 10 min and 0.9 g / cm 3 The overall thickness of the sealant film 20 was 40 μm. The ratio of the thickness of the surface resin layer 23 to the thickness of the sealant film 20 was 7.5%.

[0119] An aluminum vapor deposition layer 30 was formed by wire vapor deposition on the surface resin layer 23 of the sealant film 20. This resulted in a barrier film 10 including the sealant film 20 and the vapor deposition layer 30. The vapor deposition layer 30 had a thickness of 45 nm.

[0120] Next, the substrate 40 made of a plastic film and the sealant film 20 were bonded by a dry lamination method. In this way, a first laminate 50 was obtained. As the plastic film, a biaxially oriented polypropylene film U1 manufactured by Mitsui Chemicals Tohcello was used. The thickness of the substrate 40 was 20 μm. As the adhesive, PASLIM VM001 / VM108CP manufactured by DICG was used. The amount of adhesive applied was 4 g / m 2 It was.

[0121] The base material 40 made of paper and the sealant film 20 were bonded by dry lamination. This produced a second laminate 50. The paper used was Tokai Kraft C, a kraft paper manufactured by Tokushu Tokai Paper Co., Ltd. The basis weight of the base material 40 was 50 g / m 2 The adhesive used was PASLIM VM001 / VM108CP manufactured by DICG. The amount of adhesive applied was 4 g / m 2 It was.

[0122] The layer structure of the first laminate is expressed as follows. OPP20 / DL / AL / Ny3 / Adhesive 4 / Random PP3 / Homo PP17 / Random PP13 The layer structure of the second laminate is expressed as follows. Paper / DL / AL / Ny3 / Adhesive 4 / Random PP3 / Homo PP17 / Random PP13 The " / " indicates the boundary between layers. The leftmost layer is the layer that constitutes the outer surface 50y of the laminate 50. The rightmost layer is the layer that constitutes the inner surface 50x of the laminate 50. "OPP" means biaxially oriented polypropylene film. "DL" means adhesive layer. "AL" means aluminum vapor deposition layer. "Ny" means nylon 6. "Adhesive" means adhesive resin layer. "Random PP" means random copolymer of polypropylene. "Homo PP" means homopolymer of polypropylene. The numbers mean the thickness of the layer. The unit of thickness is μm.

[0123] Example 2 An ethylene-vinyl alcohol copolymer E171B manufactured by Kuraray was used as the surface resin layer 23. The ratio of ethylene copolymer in the surface resin layer 23 was 44 mol %. The MFR and density of the surface resin layer 23 were 1.7 g / 10 min and 1.14 g / cm 3 The adhesive resin layer 22 was made of maleic anhydride modified polypropylene AT3351 manufactured by Mitsui Chemicals. The adhesive resin layer 22 had an MFR of 11 g / 10 min (ASTM D1238) and a density of 0.890 g / cm. 3 The thicknesses of the surface resin layer 23 and the adhesive resin layer 22 were 3 μm and 4 μm, respectively. Except for these points, the first laminate 50 and the second laminate 50 were produced in the same manner as in Example 1. The total thickness of the sealant film 20 was 40 μm. The ratio of the thickness of the surface resin layer 23 to the thickness of the sealant film 20 was 7.5%.

[0124] The layer structure of the first laminate is expressed as follows. OPP20 / DL / AL / EVOH3 / Adhesive 4 / Random PP3 / Homo PP17 / Random PP13 The layer structure of the second laminate is expressed as follows. Paper / DL / AL / EVOH3 / Adhesive4 / RandomPP3 / HomoPP17 / RandomPP13 "EVOH" means ethylene-vinyl alcohol copolymer.

[0125] Comparative Example 1 As the sealant film 20, an unstretched polypropylene film 2703 manufactured by Toray Film Processing Co., Ltd. was used. The unstretched polypropylene film 2703 includes an aluminum deposition layer formed on the surface of a polypropylene resin layer. The thickness of the sealant film 20 was 40 μm. The thickness of the deposition layer was 45 nm. Except for these points, the first laminate 50 and the second laminate 50 were produced in the same manner as in Example 1.

[0126] The layer structure of the first laminate is expressed as follows. OPP20 / DL / AL / CPP40 The layer structure of the second laminate is expressed as follows. Paper / DL / AL / CPP40 "CPP" means unoriented polypropylene film.

[0127] Comparative Example 2 The first laminate 50 and the second laminate 50 were produced in the same manner as in Example 1, except that the adhesive resin layer 22 had a thickness of 1 μm and the second copolymer layer 21c had a thickness of 6 μm.

[0128] The layer structure of the first laminate is expressed as follows. OPP20 / DL / AL / Ny3 / Adhesive 1 / Random PP6 / Homo PP17 / Random PP13 The layer structure of the second laminate is expressed as follows. Paper / DL / AL / Ny3 / Adhesive 1 / Random PP6 / Homo PP17 / Random PP13

[0129] It has been difficult to stably form the first laminate 50 and the second laminate 50 having the above layer configuration. Surface resin layer 23 When the adhesive resin layer 22 contains a polyamide resin such as nylon, it is considered preferable that the thickness of the adhesive resin layer 22 is 2 μm or more in order to stably produce the barrier film 10 and the laminate 50 .

[0130] Comparative Example 3 The first laminate 50 and the second laminate 50 were prepared in the same manner as in Example 2, except that the thickness of the surface resin layer 23 was 2 μm, the thickness of the adhesive resin layer 22 was 2 μm, and the thickness of the second copolymer layer 21c was 6 μm.

[0131] The layer structure of the first laminate is expressed as follows. OPP20 / DL / AL / EVOH2 / Adhesive2 / RandomPP6 / HomoPP17 / RandomPP13 The layer structure of the second laminate is expressed as follows. Paper / DL / AL / EVOH2 / Adhesive2 / Random PP6 / Homo PP17 / Random PP13

[0132] The first laminate 50 and the second laminate 50 having the above-mentioned layer configuration were confirmed to have a white appearance. When the surface resin layer 23 contains an ethylene-vinyl alcohol copolymer, it is considered that the thickness of the surface resin layer 23 is preferably 3 μm or more in order to prevent the appearance from becoming white. When the surface resin layer 23 contains an ethylene-vinyl alcohol copolymer, it is considered that the thickness of the adhesive resin layer 22 is preferably 3 μm or more in order to ensure the laminate strength of the laminate 50.

[0133] [Measurement of Laminate Strength] The laminate strength of the first laminate 50 of Examples 1 and 2 and Comparative Example 1 was measured in accordance with JIS K 6854-2 under an environment of a temperature of 23°C and a relative humidity of 90%RH. A&D Tensilon universal material testing machine RTC-1310 was used as a measuring device for the laminate strength. Specifically, the laminate strength was measured by the method shown in Figs. 7 to 9 above. The laminate strengths in Example 1, Example 2 and Comparative Example 1 were 3.0 N / 15 mm, 2.9 N / 15 mm and 0.5 N / 15 mm, respectively. The measurement results represent the laminate strength between the layers having the lowest adhesion. In Figs. 7 to 9, the test pieces are peeled off between the adhesive layer 45 and the vapor deposition layer 30, but the measurement results do not necessarily represent the laminate strength between the adhesive layer 45 and the vapor deposition layer 30.

[0134] [Measurement of oxygen permeability] The oxygen permeability of the first laminate 50 of Examples 1 and 2 and Comparative Example 1 was measured in an environment of a temperature of 23° C. and a relative humidity of 90% RH in accordance with JIS K 7126. An oxygen permeability measuring device OX-TRAN2 / 20 manufactured by MOCON was used as the device for measuring the oxygen permeability. In the measurement, a sample of the first laminate 50 was placed so that the substrate 40 was located on the oxygen supply side. The oxygen permeability in Example 1, Example 2 and Comparative Example 1 was 0.20 cc / m2 ·day·atm, 0.01cc / m 2 ·day·atm and 4.0cc / m 2 ·day·atm.

[0135] [Measurement of water vapor permeability] The water vapor permeability of the first laminate 50 of Examples 1 and 2 and Comparative Example 1 was measured in an environment of a temperature of 40° C. and a relative humidity of 90% RH in accordance with JIS K 7129. A water vapor permeability measuring device PERMATRAN-w 3 / 33 manufactured by MOCON was used as the device for measuring the water vapor permeability. In the measurement, a sample of the first laminate 50 was placed so that the substrate 40 was located on the water vapor supply side. The water vapor permeability in Example 1, Example 2 and Comparative Example 1 was 0.10 g / m 2 day, 0.10g / m 2 day and 0.5g / m 2 ·day.

[0136] [Evaluation of Heat Shrinkage] The first laminates 50 of Examples 1 and 2 and Comparative Example 1 were evaluated for whether or not they had shrinkage due to heat. Specifically, first, two sheets of the first laminates 50 were prepared. Then, the two sheets of the first laminates 50 were stacked so that the polyolefin resin layers 21 were in contact with each other. Then, the two sheets of the first laminates 50 were heat-sealed in a temperature range of 120°C to 170°C under conditions of 1 kg and 1 second. It was visually confirmed whether or not heat shrinkage had occurred in the first laminates 50. In the temperature range of 120°C to 150°C, no thermal shrinkage occurred in any of Examples 1 and 2 and Comparative Example 1. At 160° C., slight thermal shrinkage occurred in Examples 1 and 2. In Comparative Example 1, greater thermal shrinkage occurred than in Examples 1 and 2. At 170° C., greater thermal shrinkage occurred in Examples 1 and 2 than at 160° C. in Examples 1 and 2. In Comparative Example 1, greater and more significant thermal shrinkage occurred than at 170° C. in Examples 1 and 2.

[0137] [Measurement of optical density and total light transmittance] The optical density and total light transmittance of the first laminate 50 of Examples 1 and 2 and Comparative Example 1 were measured in an environment of a temperature of 23° C. and a relative humidity of 90% RH in accordance with JIS K 7361. A haze meter MDH4000 manufactured by Nippon Denshoku Industries Co., Ltd. was used as a device for measuring the total light transmittance. The optical densities in Example 1, Example 2 and Comparative Example 1 were 3.4, 3.0 and 2.0, respectively. The total light transmittances in Example 1, Example 2 and Comparative Example 1 were 0.04%, 0.1% and 1.0%, respectively.

[0138] [Evaluation of Surface Gloss] The surface gloss of the first laminate 50 of Examples 1 and 2 and Comparative Example 1 was evaluated. Specifically, the first laminate 50 was visually observed from the substrate 40 side to confirm whether the gloss of the aluminum vapor-deposited layer 30 was apparent. Gloss appeared in Example 1. In Example 2 and Comparative Example 1, the degree of gloss was smaller than that in Example 1.

[0139] [Seal leak evaluation] The seal leak of the second laminate 50 of Examples 1-2 and Comparative Example 1 was evaluated. First, the second laminate 50 was heat-sealed to produce a pillow pouch. As a heat-sealing device, a vertical pillow filling machine TYTT type manufactured by Tokyo Automotive Machinery Works was used. The number of shots was 85 rpm, the sealing temperature of the vertical seal was 150°C, and the sealing temperature of the horizontal seal was 160°C. Next, the inside of the pillow pouch was filled with a check liquid through the opening at the top of the pillow pouch. As the check liquid, an edgeless seal check liquid manufactured by Mitsubishi Gas Chemical Company was used. After filling with the check liquid, the pillow pouch was placed in an environment of a temperature of 23°C and a relative humidity of 50% RH for 24 hours. Then, it was confirmed whether or not the check liquid had leaked. No leakage of the check liquid occurred in Examples 1 and 2. In Comparative Example 1, leakage of the check liquid occurred.

[0140] The measurement results and evaluation results are shown in Fig. 13. The laminates 50 of Examples 1 and 2 show better results than the laminates 50 of Comparative Examples 1 to 3.

[0141] [Evaluation of breaking strength and breaking elongation] The breaking strength and breaking elongation of the sealant films 20 of Example 1 and Comparative Example 1 were measured in accordance with JIS K7127 under an environment of a temperature of 23°C and a relative humidity of 50%RH. A&D Tensilon universal material testing machine RTC-1310 was used as a measuring device for breaking strength and breaking elongation. In the measurement, a rectangular film of 10 mm width and 150 mm length cut from the sealant film 20 was used as a test piece. The distance between the pair of chucks holding the test piece at the start of the measurement was 50 mm. The tensile speed of the test piece was 300 mm / min. The breaking strength of the sealant film 20 of Example 1 in the machine direction (MD) and the perpendicular direction (TD) was 46.1 MPa and 26.5 MPa. The breaking elongation of the sealant film 20 of Example 1 in the machine direction (MD) and the perpendicular direction (TD) was 372.8% and 403.8%. The breaking strength of the sealant film 20 of Comparative Example 1 in the machine direction (MD) and the perpendicular direction (TD) was 32.3 MPa and 28.3 MPa. The breaking elongation of the sealant film 20 of Comparative Example 1 in the machine direction (MD) and the perpendicular direction (TD) was 340.9% and 458.3%. The measurement results are shown in FIG. 14.

[0142] [Measurement of Breaking Energy] The breaking energy of the sealant films 20 of Example 1 and Comparative Example 1 was measured in an environment of a temperature of 23° C. and a relative humidity of 90% RH. A film impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd. was used as a breaking energy measuring device. The breaking energy of the sealant film 20 in Example 1 and Comparative Example 1 was 0.389 J and 0.054 J, respectively. The value obtained by dividing the breaking energy of the sealant film 20 by the thickness of the sealant film 20 was 0.00972 J / μm and 0.00135 J / μm, respectively, in Example 1 and Comparative Example 1. The measurement results are shown in FIG. [Explanation of symbols]

[0143] 10. Barrier Film 20 Sealant Film 20x 1st side 20y 2nd side 21 Polyolefin resin layer 21a First Copolymer Layer 21b Homopolymer layer 21c Second Copolymer Layer 22 Adhesive resin layer 23 Surface resin layer 30 Deposited layer 40 Base material 41 Printing layer 45 Adhesive layer 50 Laminate 50x inner surface 50y external surface 60 Packaging containers

Claims

1. A sealant film including a first surface and a second surface located opposite the first surface; a deposition layer located on the second surface, The sealant film comprises a polyolefin resin layer constituting the first surface, a surface resin layer constituting the second surface and containing a resin material having a polar group, and an adhesive resin layer located between the polyolefin resin layer and the surface resin layer, the surface resin layer contains an ethylene-vinyl alcohol copolymer and has a thickness of 3 μm or more; The adhesive resin layer has a thickness of 3 μm or more, A barrier film, wherein a value obtained by dividing the breaking energy of the sealant film by the thickness of the sealant film is 0.0025 J / μm or more.

2. A sealant film including a first surface and a second surface located opposite the first surface; a deposition layer located on the second surface, The sealant film comprises a polyolefin resin layer constituting the first surface, a surface resin layer constituting the second surface and containing a resin material having a polar group, and an adhesive resin layer located between the polyolefin resin layer and the surface resin layer, The surface resin layer contains nylon 6, nylon 6,6 or MXD nylon and has a thickness of 2 μm or more and 5 μm or less, The adhesive resin layer has a thickness of 2 μm or more.

3. 3. The barrier film according to claim 1, wherein a ratio of a thickness of the surface resin layer to a thickness of the sealant film is 1% or more and 20% or less.

4. The barrier film according to claim 1 , wherein the polyolefin resin layer is a polypropylene resin layer.

5. 5. The barrier film of claim 4, wherein the polypropylene resin layer comprises a first copolymer layer and a second copolymer layer, and a homopolymer layer located between the first copolymer layer and the second copolymer layer.

6. The barrier film according to claim 1 , wherein the deposition layer comprises a metal layer or an inorganic oxide layer.

7. 3. The barrier film according to claim 2, wherein a value obtained by dividing the breaking energy of the sealant film by a thickness of the sealant film is 0.0025 J / μm or more.

8. A barrier film according to any one of claims 1 to 7, A laminate comprising a substrate.

9. The substrate comprises a stretched plastic film; The laminate of claim 8 comprising a printed layer located between the substrate and the barrier film.

10. The substrate comprises a stretched plastic film; 10. The laminate of claim 8 or 9, comprising an adhesive layer located between the substrate and the barrier film.

11. The laminate of claim 8 , wherein the substrate comprises paper.

12. A packaging container comprising the laminate according to any one of claims 8 to 11.

Citation Information

Patent Citations

  • Package of high sealinggup property

    JP1980091665A

  • JP1989115539U

  • Aluminum vapor deposited polyethylene film and method of manufacturing the same

    JP2001179878A

  • Pouch for retort

    JP2002308286A

  • Paper-made liquid container

    JP2004042937A