Nanogap electrode structure, manufacturing method thereof, analysis device, and analysis method

The nanogap electrode structure forms stable nanogaps through electromigration, addressing the complexity of the MCBJ system by using an insulating film with nanopores and electrode parts to efficiently guide samples for analysis.

JP7591247B2Active Publication Date: 2024-11-28TEI SOLUTIONS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020090914
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-25
Publication Date
2024-11-28
Estimated Expiration
2040-05-25

AI Technical Summary

Technical Problem

The MCBJ system for forming nanogaps requires a mechanical stress mechanism, making it unstable and complex.

Method used

A nanogap electrode structure with an insulating film and nanopores, where a nanogap is formed through electromigration by applying a voltage between electrode parts, creating a stable nanogap in the nanopore upper region.

Benefits of technology

Stable formation of nanogaps using a simple method, efficiently guiding samples to the nanogap for analysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591247000001
    Figure 0007591247000001
  • Figure 0007591247000002
    Figure 0007591247000002
  • Figure 0007591247000003
    Figure 0007591247000003
Patent Text Reader

Abstract

To provide a nano-gap electrode structure, a manufacturing method therefor, an analyzer and an analysis method, with which it is possible to stably form a nano-gap by a simple method.SOLUTION: A nano-gap electrode structure 10 comprises: an insulating film 11 having a nano-pore 13 which a sample passes through; and a nano-gap electrode 12 provided to the insulating film 11 and having a nano-gap 17 between a pair of electrode parts 14a, 14b. The pair of electrode parts 14a, 14b include a nano-pore upper region 15 located at the top of the nano-pore 13 and a connection region 16 for connecting to the nano-pore upper region 15 and located at the top of the insulating film 11. The nano-gap 17 is provided inside of the nano-pore upper region 15.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nano-gap electrode structure, a manufacturing method thereof, an analysis device, and an analysis method. [Background technology]

[0002] In recent years, nanogap electrodes having a nanogap between opposing electrodes have been attracting attention, and research into electronic devices, biodevices, etc. using nanogap electrodes has been actively conducted. In the field of biodevices, for example, an analytical device has been developed that passes single-stranded DNA (deoxyribonucleic acid) through a nanogap, measures the tunnel current that flows between the electrodes when the bases of the single-stranded DNA pass through the nanogap, and identifies the bases that make up the single-stranded DNA based on the current value.

[0003] As a method for forming a nano-gap electrode, a mechanically-controllable break junction (MCBJ) system is known (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2019-525766 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the MCBJ system described in Patent Document 1 requires a mechanism for applying mechanical stress to form a nanogap, and it is desirable to form a nanogap stably in a simple manner.

[0006] An object of the present invention is to provide a nanogap electrode structure that can stably form a nanogap by a simple method, and a manufacturing method, an analytical device, and an analytical method thereof. [Means for solving the problem]

[0007] The nanogap electrode structure of the present invention comprises an insulating film having a nanopore through which a sample passes, and a nanogap electrode provided on the insulating film and having a nanogap between a pair of electrode portions, the pair of electrode portions having a nanopore upper region located above the nanopore and a connection region located on the insulating film and connecting to the nanopore upper region, and the nanogap is provided within the nanopore upper region.

[0008] The manufacturing method of the nanogap electrode structure of the present invention includes a preparation step of preparing a nanogap electrode composed of a pair of electrode portions provided on an insulating film having a nanopore and having a nanopore upper region located above the nanopore, and a nanogap formation step of applying a voltage between the pair of electrode portions to form a nanogap in the nanopore upper region by electromigration.

[0009] The analytical device of the present invention includes the above-mentioned nano-gap electrode structure, a power source that applies a voltage between the pair of electrode portions, an ammeter that detects a tunneling current flowing between the pair of electrode portions, and an analytical portion that analyzes a sample based on the current value of the tunneling current.

[0010] The analytical method of the present invention includes a first step of forming a nanogap in a nanogap electrode that is provided in an insulating film having a nanopore and is composed of a pair of electrode parts having a nanopore upper region located above the nanopore, and a second step of detecting a tunneling current when a sample passes through the nanogap and analyzing the sample based on the current value of the tunneling current. Effect of the Invention

[0011] According to the present invention, a nanogap can be stably formed by a simple method in the upper nanopore region of the pair of electrode parts located above the nanopore.

[0012] In addition, since a nanogap is formed above the nanopore, the sample to be analyzed can be efficiently guided to the nanogap. [Brief description of the drawings]

[0013] [Figure 1] 1 is a perspective view showing the appearance of a nano-gap electrode structure according to a first embodiment. [Diagram 2] FIG. 2 is an enlarged view of the vicinity of the nanopore indicated by the symbol II in FIG. [Diagram 3] FIG. 2 is an enlarged view of the vicinity of a nanopore of a nano-gap electrode structure in which a pair of electrode portions are not cut. [Figure 4A] FIG. 11 is a plan view for explaining an insulating film forming step. [Figure 4B] FIG. 4B is a cross-sectional view taken along line BB in FIG. 4A. [Figure 5A] FIG. 13 is a plan view for explaining the nanopore forming process. [Figure 5B] FIG. 5B is a cross-sectional view taken along line BB in FIG. 5A. [Figure 6A] FIG. 13 is a plan view for explaining the nanopore embedding step. [Figure 6B] FIG. 6B is a cross-sectional view taken along line BB in FIG. 6A. [Figure 7A] FIG. 11 is a plan view for explaining an electrode forming step. [Figure 7B] FIG. 7B is a cross-sectional view taken along line BB in FIG. 7A. [Figure 8A] FIG. 11 is a plan view for explaining a flow path forming step. [Figure 8B] FIG. 8B is a cross-sectional view taken along line BB in FIG. 8A. [Figure 9A] FIG. 11 is a plan view for explaining a nanogap forming step. [Figure 9B] FIG. 9B is a cross-sectional view taken along line BB in FIG. 9A. [Figure 10]FIG. 1 is an explanatory diagram for explaining an analysis device according to a first embodiment. [Figure 11] FIG. 11 is an enlarged view showing the vicinity of a nanopore of the nano-gap electrode structure according to the second embodiment. [Figure 12] FIG. 11 is an enlarged view showing a state in which the first electrode portion and the second electrode portion of the nano-gap electrode structure according to the second embodiment are not cut off. [Figure 13] 13A and 13B are explanatory views for explaining modified examples of the thin-walled portion. [Figure 14] FIG. 13 is an enlarged view showing the vicinity of a nanopore of the nano-gap electrode structure according to the third embodiment. [Figure 15] FIG. 11 is an enlarged view showing a state in which the first electrode portion and the second electrode portion of the nano-gap electrode structure according to the third embodiment are not cut off. [Figure 16] FIG. 11 is a cross-sectional view of a nano-gap electrode structure according to a fourth embodiment. [Figure 17A] FIG. 11 is a plan view for explaining an adhesive layer forming step. [Figure 17B] FIG. 17B is a cross-sectional view taken along line BB in FIG. 17A. [Figure 18A] FIG. 11 is a plan view for explaining an electrode forming step. [Figure 18B] FIG. 18B is a cross-sectional view taken along line BB in FIG. 18A. [Figure 19A] FIG. 11 is a plan view illustrating a first example of an adhesive layer removing step. [Figure 19B] FIG. 19B is a cross-sectional view taken along line BB in FIG. 19A. [Figure 20A] FIG. 11 is a plan view for explaining an adhesive layer forming step. [Figure 20B] FIG. 20B is a cross-sectional view taken along line BB in FIG. 20A. [Figure 21A] FIG. 13 is a plan view for explaining the nanopore forming process. [Figure 21B] FIG. 21B is a cross-sectional view taken along line BB in FIG. 21A. [Figure 22] FIG. 13 is an enlarged view showing the vicinity of a nanopore of the nano-gap electrode structure according to the fifth embodiment. [Diagram 23]FIG. 13 is an enlarged view showing a state in which the first electrode portion and the second electrode portion of the nano-gap electrode structure according to the fifth embodiment are not cut off. [Figure 24A] FIG. 11 is a plan view illustrating a first layer forming step. [Figure 24B] FIG. 24B is a cross-sectional view taken along line BB in FIG. 24A. [Figure 25A] FIG. 11 is a plan view illustrating a second layer forming step. [Figure 25B] FIG. 25B is a cross-sectional view taken along line BB in FIG. 25A. [Figure 26A] FIG. 11 is a plan view for explaining a flow path forming step. [Figure 26B] FIG. 26B is a cross-sectional view taken along line BB in FIG. 26A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [First embodiment] FIG. 1 is a perspective view showing the appearance of the nano-gap electrode structure 10 according to the first embodiment. In FIG. 1, the X-axis, Y-axis, and Z-axis indicate three axes of a Cartesian coordinate system. The Z-axis direction is the thickness direction (thickness direction) of the nano-gap electrode structure 10. The Y-axis direction is the width direction (width direction) of the nano-gap electrode structure 10. The X-axis direction is the direction in which a current flows, which will be described later. The positive direction of the Z-axis is the upward direction, and the negative direction of the Z-axis is the downward direction. In each member constituting the nano-gap electrode structure 10, the upper surface is the front surface, and the lower surface is the back surface. Viewing the nano-gap electrode structure 10 from above downward is called a "plan view."

[0015] As shown in FIG. 1, the nanogap electrode structure 10 includes an insulating film 11 and a nanogap electrode 12 provided on the insulating film 11. The insulating film 11 has a nanopore 13 through which a sample passes. The nanogap electrode 12 is composed of a pair of electrode parts 14a, 14b to which a voltage is applied. The pair of electrode parts 14a, 14b has a nanopore upper region 15 located at the upper part of the nanopore 13 and a connection region 16 located at the upper part of the insulating film 11 and connected to the nanopore upper region 15. In this embodiment, the nanopore upper region 15 is arranged so as to block a part of the nanopore 13, but it may be arranged so as to block the entire nanopore 13. As will be described in detail later, the nanopore upper region 15 is configured to induce a disconnection due to electromigration by a current that flows when a voltage is applied between the pair of electrode parts 14a, 14b in a state where the pair is connected to each other. Due to the occurrence of a disconnection in the nanopore upper region 15, a nanogap 17 that connects to the nanopore 13 is formed between the pair of electrode portions 14a, 14b. Fig. 1 shows the nanogap electrode structure 10 in a state in which the nanogap 17 is formed between the pair of electrode portions 14a, 14b and the pair of electrode portions 14a, 14b are not connected. In the following description, when the pair of electrode portions 14a, 14b are to be distinguished from each other, they will be referred to as the first electrode portion 14a and the second electrode portion 14b.

[0016] The configuration of the nano-gap electrode structure 10 will be described in detail with reference to Figures 1 and 2. The outer shape of the nano-gap electrode structure 10 in plan view is not particularly limited, and is rectangular in this embodiment.

[0017] The insulating film 11 is formed of, for example, a SiN film (silicon nitride film) or a SiO film (silicon oxide film). In this embodiment, the insulating film 11 is formed of a SiN film. The thickness of the insulating film 11 is not particularly limited, and is 100 nm in this embodiment.

[0018] The insulating film 11 is provided on a substrate 18. In this embodiment, the substrate 18 is a silicon substrate with a (100) surface orientation, but is not limited thereto. The thickness of the substrate 18 is not particularly limited, and is 775 μm in this embodiment. A flow path 19 is provided inside the substrate 18. In FIG. 1, the flow path 19 is indicated by a two-dot chain line. The flow path 19 penetrates the substrate 18 in the thickness direction and connects to the nanopore 13. The flow path 19 also connects to the nanogap 17 via the nanopore 13. The shape of the flow path 19 is not particularly limited, and can be any shape. In this embodiment, the shape of the flow path 19 is a quadrangular pyramid shape, and the area of ​​the cross section parallel to the XY plane increases from top to bottom.

[0019] The nanopore 13 penetrates the insulating film 11 in the thickness direction. The diameter of the nanopore 13 is several nm to several hundred nm, and is 100 nm in this embodiment.

[0020] The nanogap electrode 12 is made of a material such as gold (Au) or platinum (Pt), and is made of gold in this embodiment. In this example, the nanogap electrode 12 has a single-layer structure, but may have a laminated structure in which two or more layers are laminated. When the nanogap electrode 12 has a laminated structure, each layer may be made of the same material or different materials. When each layer is made of different materials, the above materials may be used in combination.

[0021] The outer shape of the first electrode portion 14a and the second electrode portion 14b in plan view is not particularly limited, but it is preferable that the nanopore upper region 15 is narrower than the connection region 16, and it is particularly preferable that the vicinity of the center of the nanopore upper region 15 is the narrowest. In this embodiment, the outer shape of the first electrode portion 14a and the second electrode portion 14b in plan view is an isosceles triangle, and each apex angle is disposed near the center of the nanopore upper region 15. As a result, the width (length in the Y-axis direction) of the nanogap electrode 12 becomes smaller toward the center of the nanopore 13. The minimum value of the width of the first electrode portion 14a and the second electrode portion 14b is, for example, 1 nm to 100 nm. In FIG. 1, the first electrode portion 14a and the second electrode portion 14b are disposed in the X-axis direction with their apex angles facing each other. When a voltage is applied to the pair of electrodes 14a and 14b, a current flows in the X-axis direction. In this embodiment, the thickness of the pair of electrode portions 14a and 14b is 30 nm.

[0022] FIG. 2 is an enlarged view of the nanopore 13 and its vicinity indicated by the symbol II in FIG. 1. In FIG. 2, the boundary between the nanopore upper region 15 and the connection region 16 is indicated by a dashed line. The nanopore upper region 15 and the connection region 16 are provided in the first electrode portion 14a and the second electrode portion 14b, respectively. In the following description, when the nanopore upper region 15 is to be described separately, the nanopore upper region provided in the first electrode portion 14a is described as the first nanopore upper region 15a, and the nanopore upper region provided in the second electrode portion 14b is described as the second nanopore upper region 15b. When the connection region 16 is to be described separately, the connection region provided in the first electrode portion 14a is described as the first connection region 16a, and the connection region provided in the second electrode portion 14b is described as the second connection region 16b.

[0023] The nanogap 17 is provided between the pair of electrode portions 14a and 14b. The distance between the nanogap 17 is about one atomic layer, for example, 0.1 nm to 0.3 nm. In FIG. 2, the nanogap 17 is provided near the center of the nanopore upper region 15.

[0024] FIG. 3 shows the nanogap electrode structure 10 in a state where the pair of electrode parts 14a, 14b are not cut. The nanopore upper region 15 is configured to induce a disconnection due to electromigration by a current that flows when a voltage is applied between the pair of electrode parts 14a, 14b in a mutually connected state, and has a function as an EM disconnection inducing part. In this embodiment, the minimum value of the width (length in the Y-axis direction) of the nanopore upper region 15 is smaller than the minimum value of the width of the connection region 16. The thickness (length in the Z-axis direction) of the nanopore upper region 15 and the thickness of the connection region 16 are the same. Therefore, in a plane (YZ plane) perpendicular to the direction in which the current flows between the pair of electrode parts 14a, 14b (X-axis direction), the minimum value of the cross-sectional area of ​​the nanopore upper region 15 is smaller than the minimum value of the cross-sectional area of ​​the connection region 16. The smaller the cross-sectional area in the plane perpendicular to the direction in which the current flows between the pair of electrode parts 14a, 14b, the higher the current density, and the more likely it is that a disconnection due to electromigration will occur.

[0025] In the nanogap electrode structure 10 in a state where the pair of electrode portions 14a, 14b are not cut, electromigration occurs due to a current that flows when a voltage is applied between the pair of electrode portions 14a, 14b. In the process of metal atoms in the nanopore upper region 15 diffusing and / or moving due to electromigration, the first electrode portion 14a and the second electrode portion 14b are cut at a location in the nanopore upper region 15 where the current density is high, and a nanogap 17 is formed in the nanopore upper region 15 (see FIG. 2).

[0026] In the nanogap electrode structure 10, after a predetermined time (e.g., 15 minutes) has elapsed since the application of the voltage that generates electromigration was stopped, the nanogap 17 is filled in the process of the diffusion and / or migration of metal atoms in the nanopore upper region 15, and the first electrode portion 14a and the second electrode portion 14b are reconnected. In the nanogap electrode structure 10 in which the first electrode portion 14a and the second electrode portion 14b are not disconnected in this manner, a voltage is applied between the pair of electrode portions 14a and 14b, and electromigration occurs again, forming the nanogap 17 at a location of high current density in the nanopore upper region 15 (see FIG. 2).

[0027] The nanogap electrode structure 10 is configured such that, of the pair of electrode parts 14a, 14b, the nanopore upper region 15 located above the nanopore 13 induces a disconnection due to electromigration. When a voltage is applied between the pair of electrode parts 14a, 14b in a mutually connected state, a disconnection due to electromigration does not occur in the connection region 16 located above the insulating film 11, but a disconnection due to electromigration occurs near the nanopore upper region 15 where the current density is highest, so that a nanogap 17 connected to the nanopore 13 can be formed. Therefore, the nanogap electrode structure 10 can stably form the nanogap 17 by a simple method.

[0028] Next, a method for manufacturing the nanogap electrode structure will be described. The method for manufacturing the nanogap electrode structure includes a preparation step of preparing a nanogap electrode provided in an insulating film having a nanopore, the nanogap electrode being composed of a pair of electrode parts having a nanopore upper region located above the nanopore, and a nanogap formation step of applying a voltage between the pair of electrode parts to form a nanogap in the nanopore upper region by electromigration.

[0029] A manufacturing method of the nano-gap electrode structure 10 according to this embodiment will be described with reference to Figures 4A, 4B to 9A, and 9B. Figures 4A to 9A are plan views, and Figures 4B to 9B are cross-sectional views taken along line BB in Figures 4A to 9A. Note that in this embodiment, the outer shape in plan view is square, but Figures 4A to 9A only show a part of the outer shape.

[0030] First, the preparation process will be described with reference to Figures 4A, 4B to 8A, and 8B. The preparation process includes an insulating film forming process, a nanopore forming process, a nanopore embedding process, an electrode layer forming process, and a flow path forming process.

[0031] 4A and 4B, in the insulating film forming step, an insulating film 21 is formed on a substrate 20. The substrate 20 is a silicon substrate having a thickness of 775 μm and a surface orientation of (100). The insulating film 21 is formed, for example, by a chemical vapor deposition (CVD) method using DCS (dichlorosilane) as a raw material gas. In this embodiment, the insulating film 21 is formed only on the surface of the substrate 20, but the insulating film 21 may be formed on both sides of the substrate 20.

[0032] As shown in FIGS. 5A and 5B, in the nanopore formation step, a nanopore 23 is formed in an insulating film 21. First, a photoresist is applied to the insulating film 21 to form a photoresist layer (not shown), and the photoresist layer is patterned by photolithography. A resist pattern is formed in the photoresist layer, with an opening corresponding to the nanopore 23. Next, the insulating film 21 is dry-etched using the photoresist layer with the resist pattern formed thereon as a mask. As a result, the nanopore 23 is formed in the insulating film 21.

[0033] As shown in FIGS. 6A and 6B, the nanopore embedding step forms a deposit film 27 in the nanopore 23. First, a SiO film is formed on the entire surface of the insulating film 21 by, for example, a CVD method using TEOS (tetraoxysilane) as a raw material gas. Next, the surface of the SiO film is planarized by, for example, a CMP (Chemical Mechanical Polishing) method. The planarization is preferably performed so that the surface of the insulating film 21 is exposed. The SiO film on the surface of the insulating film 21 is removed by the planarization. The deposit film 27 is formed by the SiO film remaining in the nanopore 23. The deposit film 27 may be an a-Si film (amorphous silicon film) or the like. Instead of using the CMP method, the planarization may be performed by etching back the surface of the deposit film 27.

[0034] As shown in FIGS. 7A and 7B, the electrode forming step forms the nanogap electrode 22 on the insulating film 21. First, a photoresist is applied to the insulating film 21 to form a photoresist layer (not shown), and the photoresist layer is patterned by photolithography to expose the portion of the insulating film 21 where the nanogap electrode 22 is to be formed, and the portion where the nanogap electrode 22 is not to be formed is covered with the photoresist layer. Next, an Au film is formed on the photoresist layer and the exposed insulating film 21 by performing a sputtering method using Au as a target material. Next, the Au film on the photoresist layer is removed together with the photoresist layer by performing a lift-off method. The nanogap electrode 22 is formed by the Au film remaining on the insulating film 21. The Au film may be formed by a vapor deposition method. If the adhesion between the Au film and the insulating film 21 is poor, an adhesive layer of, for example, titanium (Ti) or chromium (Cr) may be provided between the Au film and the insulating film 21. The thickness of the adhesive layer is, for example, about 2 nm.

[0035] The electrode formation process is not limited to the lift-off method. For example, when Pt is used as the material for forming the nanogap electrode 22, a Pt film is formed on the insulating film 21 by a sputtering method using Pt as a target material, a photoresist is applied to the Pt film to form a photoresist layer, the photoresist layer is patterned by a photolithography technique, and the Pt film is dry-etched using the patterned photoresist layer as a mask. The nanogap electrode 22 can be formed from the Pt film remaining on the insulating film 21.

[0036] The nanogap electrode 22 is composed of a pair of electrode parts 24a, 24b (first electrode part 24a, second electrode part 24b) to which a voltage is applied. The pair of electrode parts 24a, 24b has a nanopore upper region 25 (first nanopore upper region 25a, second nanopore upper region 25b) located at the top of the nanopore 23, and a connection region 26 (first connection region 26a, second connection region 26b) located at the top of the insulating film 21 and connected to the nanopore upper region 25. In the electrode formation step, the nanogap electrode 22 is formed so that the outer shape of the first electrode part 24a and the second electrode part 24b in a plan view is an isosceles triangle. The first electrode part 24a and the second electrode part 24b are connected near the vertices of each isosceles triangle. The portion where the first electrode portion 24a and the second electrode portion 24b are connected is included in the nanopore upper region 25. The width (length in the Y-axis direction) of the portion where the first electrode portion 24a and the second electrode portion 24b are connected is, for example, 1 nm to 100 nm, which is the minimum value of the width of the entire nanogap electrode 22. As a result, the minimum value of the width of the nanopore upper region 25 is smaller than the minimum value of the width of the connection region 26. Since the thickness (length in the Z-axis direction) of the first electrode portion 24a and the thickness of the second electrode portion 24b are the same, the minimum value of the cross-sectional area of ​​the nanopore upper region 25 is smaller than the minimum value of the cross-sectional area of ​​the connection region 26 in the YZ plane. In this way, the nanopore upper region 25 is configured to induce a disconnection due to electromigration by a current that flows when a voltage is applied between the pair of electrodes 24a and 24b, and has a function as an EM disconnection inducing portion.

[0037] As shown in FIGS. 8A and 8B, in the flow path forming step, a flow path 29 that connects to the nanopore 23 is formed in the substrate 20. First, a protective film (not shown) is formed on the surface of the insulating film 21, the surface of the nanogap electrode 22, and the back surface of the substrate 20. The protective film is preferably made of a material that has a large etching rate selection ratio to a wet etching solution in anisotropic wet etching, which will be described later. The protective film is, for example, a SiO film formed by a CVD method using TEOS as a raw material gas. Next, a photoresist layer (not shown) is formed on the protective film provided on the back surface of the substrate 20, patterned by photolithography technology, and the protective film on the back surface of the substrate 20 is dry-etched using the photoresist layer on which the resist pattern is formed as a mask. As a result, an opening is formed in a portion of the protective film provided on the back surface of the substrate 20 that corresponds to the flow path 29. The back surface of the substrate 20 is exposed from the opening of the protective film. Next, the substrate 20 is immersed in a wet etching solution to perform anisotropic wet etching. As the wet etching solution, an alkaline aqueous solution such as KOH (potassium hydroxide) or TMAH (tetramethylammonium hydroxide) is used. The protective film functions as a mask for anisotropic wet etching. Therefore, only a part of the back surface of the substrate 20 exposed from the opening of the protective film is etched. After forming the flow path 29 in the substrate 20, the protective film, which is a SiO film, and the deposit film 27 are removed by wet etching using, for example, HF (hydrofluoric acid) as a wet etching solution. This results in the nanogap electrode structure precursor 30 shown in Figures 8A and 8B.

[0038] As described above, the nanogap electrode structure precursor 30 can be manufactured by the insulating film forming step, the nanopore forming step, the nanopore filling step, the electrode layer forming step, and the flow path forming step. The nanogap electrode structure precursor 30 has the same configuration as the nanogap electrode structure 10, except that it does not have the nanogap 17.

[0039] Next, the nanogap forming process will be described with reference to Figures 9A and 9B. First, the pair of electrodes 24a, 24b of the nanogap electrode structure precursor 30 are electrically connected to the power source 31 using the wiring 35. Note that the wiring 35 and the power source 31 are not shown in Figure 9A. The power source 31 is turned on, and a voltage is applied between the pair of electrodes 24a, 24b. Since the cross-sectional area of ​​the nanopore upper region 25 is smaller than that of the connection region 26, the current density is larger than that of the connection region 26, and a disconnection due to electromigration occurs. The disconnection of the nanopore upper region 25 disconnects the first electrode portion 24a and the second electrode portion 24b, and a nanogap 17 is formed in the nanopore upper region 25. The nanogap electrode structure precursor 30 in which the nanogap 17 is formed becomes the nanogap electrode structure 10 (see Figure 1).

[0040] As shown in FIG. 10, the nano-gap electrode structure 10 is used in an analysis device 40 that analyzes a small amount of sample. The analysis device 40 analyzes the sample by detecting a change in a tunnel current flowing between a pair of electrodes 14a, 14b when the sample passes through the nano-gap 17 of the nano-gap electrode structure 10. Examples of the sample include DNA, proteins, pollen, viruses, cells, organic particles or inorganic particles, and particulate matter such as PM (Particulate Matter) 2.5. The sample is dispersed in a solution containing an electrolyte, and the obtained sample liquid is provided to the analysis device 40. Examples of the solution in which the sample is dispersed include phosphate buffered saline (PBS).

[0041] The analysis device 40 includes the nano-gap electrode structure 10, a power source 41, a control unit 42, an ammeter 43, and an analysis unit 44. The nano-gap electrode 12 of the nano-gap electrode structure 10, the power source 41, and the ammeter 43 are connected using wiring 45.

[0042] The power source 41 is electrically connected to the pair of electrodes 14a, 14b. The power source 41 applies a voltage between the pair of electrodes 14a, 14b. The voltage of the power source 41 is controlled by the control unit .

[0043] The control unit 42 is electrically connected to the power source 41. The control unit 42 performs a first control of setting the voltage of the power source 41 to a first voltage and forming the nanogap 17 between the pair of electrode units 14a, 14b, and a second control of setting the voltage of the power source 41 to a second voltage different from the first voltage and generating a tunnel current between the pair of electrode units 14a, 14b facing each other via the nanogap 17.

[0044] The first control is performed in a state where the first electrode portion 14a and the second electrode portion 14b are not disconnected. The second control is performed in a state where the nanogap 17 is formed between the pair of electrodes 14a, 14b. The control portion 42 is configured to enable switching between the first control and the second control, for example, by operating an operation portion (not shown).

[0045] The ammeter 43 is electrically connected to the pair of electrode units 14a, 14b. The ammeter 43 detects a tunnel current flowing between the pair of electrode units 14a, 14b facing each other across the nanogap 17 when the control unit 42 is performing a second control. Note that the ammeter 43 may detect a current flowing between the pair of electrode units 14a, 14b connected to each other when the control unit 42 is performing a first control.

[0046] The analysis unit 44 is electrically connected to the ammeter 43. The analysis unit 44 analyzes the sample based on the current value of the tunneling current detected by the ammeter 43. The current value of the tunneling current changes depending on the electrical resistance of the sample passing through the nanogap 17. For this reason, for example, when single-stranded DNA passes through the nanogap 17, the analysis unit 44 can identify the bases and analyze the base sequence, etc., based on the current value of the tunneling current that changes depending on the type of base that constitutes the single-stranded DNA.

[0047] Although not shown, the analysis device 40 may include a pair of electrodes for electrophoresis of the sample and a power source for applying a voltage to the pair of electrodes. When a voltage is applied from the power source to the pair of electrodes, electrophoresis of the sample is performed, and the sample passes through the nanogap 17 and the nanopore 13. The analysis device 40 may be configured to flow the sample by pressure, or may be configured to flow the sample by using both electrophoresis and pressure.

[0048] The analysis device 40 analyzes the sample by applying a first voltage between the pair of electrode portions 14a, 14b to form a nanogap 17 in the nanopore upper region 15, and then applying a second voltage between the pair of electrode portions 14a, 14b to detect a tunnel current when the sample passes through the nanogap 17. Thus, the analysis device 40 can continuously form the nanogap 17 and analyze the sample.

[0049] The nanogap electrode structure precursor 30 may be provided to the analysis device 40. A voltage is applied between the pair of electrode parts 24a, 24b to form a nanogap 17 in the nanopore upper region 25, thereby obtaining the nanogap electrode structure 10.

[0050] Next, an analysis method will be described. The analysis method includes a first step of forming a nanogap in a nanogap electrode provided in an insulating film having a nanopore, the nanogap electrode being composed of a pair of electrode parts having a nanopore upper region located above the nanopore, and a second step of detecting a tunnel current when a sample passes through the nanogap and analyzing the sample based on the current value of the tunnel current. In this embodiment, an analysis method using an analysis device 40 will be described.

[0051] In the first step, the nanogap electrode structure 10 in a state in which the first electrode portion 14a and the second electrode portion 14b are not disconnected is first provided to the analysis device 40. The control portion 42 performs a first control to set the voltage of the power source 41 to a first voltage. Electromigration occurs due to a current that flows as a result of the first voltage being applied between the pair of electrodes 14a, 14b, and a nanogap 17 is formed in the nanopore upper region 15. In this way, the analysis method according to this embodiment can stably form the nanogap 17 by a simple method.

[0052] In the second step, the control unit 42 performs a second control to set the voltage of the power supply 41 to a second voltage. When the second voltage is applied between the pair of electrodes 14a, 14b, a tunnel current is generated between the pair of electrodes 14a, 14b facing each other across the nanogap 17. The ammeter 43 detects the tunnel current. The analysis unit 44 analyzes the sample based on the current value of the tunnel current detected by the ammeter 43 when the sample passes through the nanogap 17. Since the nanogap 17 is formed on the nanopore 13, the sample to be analyzed can be efficiently guided to the nanogap.

[0053] [Second embodiment] 11 is an enlarged view of the vicinity of the nanopore 13 of the nano-gap electrode structure 50 according to the second embodiment. In the following description, the same members as those in the first embodiment are denoted by the same reference numerals and description thereof will be omitted.

[0054] The nanogap electrode structure 50 includes an insulating film 11 and a nanogap electrode 52 provided in the insulating film 11. The nanogap electrode 52 has a pair of electrode portions 54a, 54b. The pair of electrode portions 54a, 54b has a nanopore upper region 55 (first nanopore upper region 55a, second nanopore upper region 55b) located above the nanopore 13, and a connection region 56 (first connection region 56a, second connection region 56b) located above the insulating film 11 and connected to the nanopore upper region 55. The nanopore upper region 55 is provided with a nanogap 17 that connects to the nanopore 13.

[0055] The nanogap electrode 52, like the nanogap electrode 12 according to the first embodiment, has a width (length in the Y-axis direction) that decreases toward the center of the nanopore 13. The nanogap electrode 52 is different from the nanogap electrode 12 in that it has a thin-walled portion 57 near the nanopore 13. The thin-walled portion 57 is a portion in which at least one of the front surface and the back surface of the nanogap electrode 52 is recessed, and in FIG. 11, it is a portion in which the back surface of the nanogap electrode 52 is recessed. The thin-walled portion 57 has a smaller thickness (length in the Z-axis direction) than other portions of the nanogap electrode 52. The thin-walled portion 57 is provided at least in the nanopore upper region 55, and in FIG. 11, it is provided in the entire nanopore upper region 55 and a part of the connection region 56. The thin-walled portion 57 shown in FIG. 11 has a shape in which the side surface as well as the back surface of the nanogap electrode 52 are recessed, and has a smaller width (length in the Y-axis direction) than other portions of the nanogap electrode 52.

[0056] As described above, the nanogap electrode 52 has a width that decreases toward the center of the nanopore 13, and has a thin portion 57 near the nanopore 13. Therefore, in a plane (YZ plane) perpendicular to the direction in which current flows between the pair of electrode portions 54a, 54b (X-axis direction), the minimum value of the cross-sectional area of ​​the nanopore upper region 55 is smaller than the minimum value of the cross-sectional area of ​​the connection region 56. In the nanopore upper region 55, which has a smaller thickness than the connection region 56, the current density is higher than in the connection region 56, and disconnection due to electromigration is more likely to occur, so that the nanogap 17 is reliably formed.

[0057] 12 is an enlarged view showing a state in which the first electrode portion 54a and the second electrode portion 54b of the nanogap electrode structure 50 are not disconnected. By applying a voltage between the pair of electrode portions 54a and 54b that are connected to each other, a disconnection due to electromigration occurs in the nanopore upper region 55, and a nanogap 17 can be formed in the nanopore upper region 55 (see FIG. 11).

[0058] Next, a method for manufacturing the nanogap electrode structure 50 will be described. In the method for manufacturing the nanogap electrode structure 50, first, as in the first embodiment, an insulating film forming step (see FIGS. 4A and 4B), a nanopore forming step (see FIGS. 5A and 5B), a nanopore embedding step (see FIGS. 6A and 6B), an electrode forming step (see FIGS. 7A and 7B), and a flow path forming step (see FIGS. 8A and 8B) are performed. After the flow path forming step, a wet etching solution is poured from the nanopore 23 to wet etch the back surface of the nanopore upper region 25 of the nanogap electrode 22, thereby partially removing the back surface of the nanopore upper region 25 in the thickness direction and thinning the nanopore upper region 25. When removing the back surface of the nanopore upper region 25 by wet etching, the nanogap electrode 22 is isotropically etched, so that the back surface of the connection region 26 is also partially removed in the thickness direction, and the side surface of the nanopore upper region 25 and the side surface of the connection region 26 are also partially removed in the width direction. As a result, a recess is formed on the back surface and side surface of the nanogap electrode 22 near the nanopore 23. The nanogap electrode 22 with a recess formed on the back surface and side surface near the nanopore 23 is a nanogap electrode 52 having a thin portion 57 (see FIG. 12).

[0059] The thin portion 57 is not limited to a shape in which the back surface and the side surface of the nano-gap electrode 52 are recessed. Modified examples of the thin portion 57 will be described below.

[0060] As shown in FIG. 13, the thin portion 58 is a portion where only the back surface of the nanogap electrode 52 is recessed, without recessing the side surface of the nanogap electrode 52. When only the back surface of the nanogap electrode 52 is recessed, without recessing the side surface, anisotropic etching by dry etching is performed on the back surface of the nanopore upper region 25 (see FIGS. 8A and 8B) of the nanogap electrode 22 after the flow path forming process, for example. Also, instead of forming a recess on the back surface of the nanogap electrode 52, a recess may be formed on the front surface of the nanogap electrode 52, or a recess may be formed on both the front surface and the back surface of the nanogap electrode 52. Instead of performing wet etching or dry etching, an electron beam may be irradiated. When an electron beam is used, a nanopore upper region 55 having a fine groove can also be formed. Since the cross-sectional area of ​​the groove of the nanopore upper region 55 is smaller than that of the connection region 56, disconnection due to electromigration is likely to occur.

[0061] [Third embodiment] FIG. 14 is an enlarged view of the vicinity of the nanopore 13 of the nano-gap electrode structure 60 according to the third embodiment.

[0062] The nanogap electrode structure 60 includes an insulating film 11 and a nanogap electrode 62 provided in the insulating film 11. The nanogap electrode 62 has a pair of electrode portions 64a, 64b. The pair of electrode portions 64a, 64b has a nanopore upper region 65 (first nanopore upper region 65a, second nanopore upper region 65b) located above the nanopore 13, and a connection region 66 (first connection region 66a, second connection region 66b) located above the insulating film 11 and connected to the nanopore upper region 65. The nanopore upper region 65 is provided with a nanogap 17 that connects to the nanopore 13.

[0063] In the third embodiment, the configuration of the nanopore upper region 65 is different from the nanopore upper region 15 according to the first embodiment and the nanopore upper region 55 according to the second embodiment. In the third embodiment, for example, after the flow channel forming process shown in Figs. 8A and 8B, ion implantation is performed on the nanopore upper region 25 of the nanogap electrode 22 to alter the material of the nanopore upper region 25. Examples of elements to be implanted into the nanopore upper region 25 include Si, Ni, Ti, and Cr. The altered nanopore upper region 25 is the nanopore upper region 65 according to the third embodiment. The method of altering the nanopore upper region 25 is not limited to the above ion implantation method. For example, a plasma treatment or an annealing treatment such as laser annealing or electron beam annealing may be performed using the substrate 20 and the insulating film 21 as a mask.

[0064] The nanopore upper region 65 includes an altered material that is the altered material of the connection region 66. In the altered nanopore upper region 65, disconnection due to electromigration is more likely to occur than in the unaltered connection region 66, and therefore the nanogap 17 is reliably formed.

[0065] 15 is an enlarged view showing a state in which the first electrode portion 64a and the second electrode portion 64b of the nanogap electrode structure 60 are not disconnected. By applying a voltage between the pair of electrode portions 64a, 64b that are connected to each other, a disconnection due to electromigration occurs in the nanopore upper region 65, and a nanogap 17 can be formed in the nanopore upper region 65 (see FIG. 14).

[0066] Alternatively, the nanopore upper region, which is thinner than the connection region, may be altered as in the second embodiment. That is, the nanopore upper region may be thinner than the connection region and may include an altered material that is the alteration of the material that constitutes the connection region.

[0067] [Fourth embodiment] 16, a nano-gap electrode structure 70 according to the fourth embodiment includes an adhesive layer 71 for adhering the nano-gap electrode 12 to the insulating film 11. The same members as those in the first embodiment are denoted by the same reference numerals and will not be described.

[0068] The adhesive layer 71 is provided between the insulating film 11 and the nanogap electrode 12. The adhesive layer 71 is in contact with the connection region 16 of the nanogap electrode 12 and is not in contact with the nanopore upper region 15. The adhesive layer 71 has an opening in a portion corresponding to the nanopore 13. The material of the adhesive layer 71 is, for example, Ti or Cr. The thickness of the adhesive layer 71 is, for example, 2 nm. The outer shape of the adhesive layer 71 in a plan view is not particularly limited, but is preferably the same shape as the nanogap electrode 12 or a similar shape larger than the nanogap electrode 12.

[0069] An example of a method for forming the adhesive layer 71 is described below. After performing an insulating film forming step (see FIGS. 4A and 4B), a nanopore forming step (see FIGS. 5A and 5B), and a nanopore embedding step (see FIGS. 6A and 6B), an adhesive layer forming step, an electrode forming step, a flow path forming step, and an adhesive layer removing step are performed. The insulating film forming step, the nanopore forming step, and the nanopore embedding step are the same as those in the first embodiment, and therefore descriptions thereof are omitted.

[0070] As shown in FIGS. 17A and 17B, in the adhesive layer forming step, an adhesive layer 72 is formed on the insulating film 21. First, a photoresist is applied to the insulating film 21 to form a photoresist layer (not shown), and the photoresist layer is patterned by photolithography. In this example, a resist pattern is formed on the photoresist layer so that the outer shape of the adhesive layer 72 in a plan view is the same as that of the nanogap electrode 12 of the nanogap electrode structure 70. A portion of the insulating film 21 where the adhesive layer 72 is to be formed is exposed, and a portion where the adhesive layer 72 is not to be formed is covered with the photoresist layer. Next, a Ti film is formed on the photoresist layer and the exposed insulating film 21 by performing a sputtering method using, for example, Ti as a target material. An adhesive layer 72 having a portion corresponding to the nanopore upper region 25 of the nanogap electrode 22 and a portion corresponding to the connection region 26 is formed.

[0071] 18A and 18B, in the electrode formation process, a sputtering method is performed using Au as a target material to form an Au film on the adhesive layer 72. Next, a lift-off method is performed to remove the adhesive layer 72 and the Au film on the photoresist layer together with the photoresist layer. The nanogap electrode 22 is formed by the Au film remaining on the adhesive layer 72.

[0072] Next, a flow path forming step (see FIGS. 8A and 8B) is performed. The flow path forming step is the same as that in the first embodiment, so a detailed description will be omitted. However, a protective film is formed, a flow path 29 is formed, and a deposit film 27 is removed.

[0073] As shown in FIGS. 19A and 19B, the adhesive layer removal step removes a portion of the adhesive layer 72 that contacts the nanopore upper region 25 of the nanogap electrode 22. In the adhesive layer removal step, a portion of the adhesive layer 72 is sputter-etched from the rear surface of the substrate 20. As a result, the portion of the adhesive layer 72 that contacts the nanopore upper region 25 of the nanogap electrode 22 is removed, and a portion that contacts the connection region 26 of the nanogap electrode 22 remains. The adhesive layer 72 has an opening at a portion corresponding to the nanopore 23. The portion of the adhesive layer 72 that contacts the connection region 26 becomes the adhesive layer 71 (see FIG. 16). Note that the method for removing a portion of the adhesive layer 72 is not limited to the above-mentioned sputter etching, and wet etching may be performed, for example.

[0074] As described above, by performing the insulating film forming process, nanopore forming process, nanopore filling process, adhesive layer forming process, electrode forming process, flow path forming process, and adhesive layer removing process, a nanogap electrode structure 70 having an adhesive layer 71 is obtained (see Figure 16).

[0075] The adhesive layer 71 is not limited to being in contact with the nanopore upper region 15 of the nanogap electrode 12, and may be in contact with the nanopore upper region 15. When obtaining an adhesive layer 71 in contact with the nanopore upper region 15, the adhesive layer removal step (see FIGS. 19A and 19B) is not performed, or a part of the adhesive layer 72 is removed so that the adhesive layer 72 remains on the back surface of the nanopore upper region 25 in the adhesive layer removal step.

[0076] The adhesive layer forming step may be carried out as a step subsequent to the insulating film forming step (see FIGS. 4A and 4B). The case where the adhesive layer forming step is carried out as a step subsequent to the insulating film forming step will be described below.

[0077] As shown in FIGS. 20A and 20B, in the adhesive layer forming step, an adhesive layer 73 is formed on the insulating film 21. First, a photoresist is applied to the insulating film 21 to form a photoresist layer (not shown), and the photoresist layer is patterned by photolithography. In this example, a resist pattern is formed on the photoresist layer so that the outer shape of the adhesive layer 73 in a plan view is a similar shape to the nanogap electrode 12 of the nanogap electrode structure 70 but larger than the nanogap electrode 12. In FIG. 20A, a portion corresponding to the outer shape of the nanogap electrode 12 of the nanogap electrode structure 70 is shown by a dotted line. The portion of the insulating film 21 where the adhesive layer 73 is to be formed is exposed, and the portion where the adhesive layer 73 is not to be formed is covered with a photoresist layer. Next, a Ti film is formed on the photoresist layer and on the exposed insulating film 21 by performing a sputtering method using, for example, Ti as a target material. An adhesive layer 73 having a portion corresponding to the nanopore upper region 25 of the nanogap electrode 22 and a portion corresponding to the connection region 26 of the nanogap electrode 22 is formed.

[0078] As shown in FIGS. 21A and 21B, the nanopore forming step forms the nanopore 23 in the insulating film 21. A photoresist is applied to the adhesive layer 73 and the insulating film 21 to form a photoresist layer, the photoresist layer is patterned by photolithography, and the adhesive layer 73 and the insulating film 21 are dry-etched using the patterned photoresist layer as a mask. This forms the nanopore 23 in the insulating film 21. Since the adhesive layer 73 has an opening in a portion corresponding to the nanopore 23, it does not have a portion in contact with the nanopore upper region 25 of the nanogap electrode 22 formed in the next electrode forming step. Therefore, the nanopore forming step includes an adhesive layer removing step of removing the portion of the adhesive layer 73 in contact with the nanopore upper region 25 of the nanogap electrode 22.

[0079] After the nanopore forming step, a nanopore embedding step, an electrode forming step, and a flow path forming step are performed in the same manner as in the first embodiment, thereby obtaining a nanogap electrode structure 70 having an adhesive layer 71 (see FIG. 16).

[0080] [Fifth embodiment] FIG. 22 is an enlarged view of the vicinity of the nanopore 13 of the nano-gap electrode structure 80 according to the fifth embodiment.

[0081] The nanogap electrode structure 80 includes an insulating film 11 and a nanogap electrode 82 provided in the insulating film 11. The nanogap electrode 82 has a pair of electrode portions 84a, 84b. The pair of electrode portions 84a, 84b has a nanopore upper region 85 (first nanopore upper region 85a, second nanopore upper region 85b) located above the nanopore 13, and a connection region 86 (first connection region 86a, second connection region 86b) located above the insulating film 11 and connected to the nanopore upper region 85. The nanopore upper region 85 is provided with a nanogap 17 that connects to the nanopore 13.

[0082] The nanogap electrode 82 has a single-layer structure in the nanopore upper region 85 and a laminated structure in the connection region 86, so that the thickness of the nanopore upper region 85 is smaller than the thickness of the connection region 86. The boundary between the single-layer structure and the laminated structure is located at the same position as the boundary between the nanopore upper region 85 and the connection region 86 in FIG.

[0083] The nanogap electrode 82 is composed of a first layer 82a provided on the insulating film 11, and a second layer 82b provided on the first layer 82a and on the nanopore 13. The first layer 82a is provided only on the insulating film 11, and is not provided on the nanopore 13. The second layer 82b has a stepped shape, and the position (height) in the Z-axis direction of the part provided on the first layer 82a is different from that of the part provided on the nanopore 13. The outer shape of the second layer 82b in a plan view is the same as that of the first layer 82a in this example, but may be a similar shape.

[0084] In the nanogap electrode 82, the nanopore upper region 85 is composed of the second layer 82b, and the connection region 86 is composed of the first layer 82a and the second layer 82b. In other words, the nanogap electrode 82 has a single-layer structure in the nanopore upper region 85 and a laminated structure in the connection region 86, and the thickness of the nanopore upper region 85 is smaller than the thickness of the connection region 86. Specifically, the minimum value of the thickness of the nanopore upper region 85 is smaller than the minimum value of the thickness of the connection region 86. Therefore, in a plane (YZ plane) perpendicular to the direction in which the current flows between the pair of electrode parts 84a, 84b (X-axis direction), the minimum value of the cross-sectional area of ​​the nanopore upper region 85 is smaller than the minimum value of the cross-sectional area of ​​the connection region 86. In the nanopore upper region 85, which is thinner than the connection region 86, the current density is higher than that in the connection region 86, and disconnection due to electromigration is more likely to occur, so that the nanogap 17 is reliably formed.

[0085] As long as the nanopore upper region 85 has at least a single-layer structure, the nanogap 17 can be formed in the nanopore upper region 85. Therefore, the boundary between the single-layer structure and the laminated structure is not limited to being located at the same position as the boundary between the nanopore upper region 85 and the connection region 86 as described above, and may be located within the nanopore upper region 85 or the connection region 86.

[0086] In this example, the first layer 82a and the second layer 82b are formed of the same material (e.g., Au), but they may be formed of different materials. When the first layer 82a and the second layer 82b are formed of different materials, for example, Ti or Cr may be used as the first layer 82a, and Au, Pt, etc. may be used as the second layer 82b. In this case, the surface of the first layer 82a may be cleaned before the second layer 82b is formed.

[0087] 23 is an enlarged view showing a state in which the first electrode portion 84a and the second electrode portion 84b of the nanogap electrode structure 80 are not disconnected. By applying a voltage between the pair of electrode portions 84a, 84b that are connected to each other, a disconnection due to electromigration occurs in the nanopore upper region 85, and a nanogap 17 can be formed in the nanopore upper region 85 (see FIG. 22).

[0088] Next, a method for manufacturing the nanogap electrode structure 80 will be described. In the method for manufacturing the nanogap electrode structure 80, first, an insulating film forming step (see FIGS. 4A and 4B), a nanopore forming step (see FIGS. 5A and 5B), and a nanopore embedding step (see FIGS. 6A and 6B) are performed, as in the first embodiment. Then, after the nanopore embedding step, an electrode forming step and a flow path forming step are performed.

[0089] The electrode formation step includes a first layer formation step and a second layer formation step. The electrode formation step according to the fifth embodiment will be described with reference to Figures 24A and 24B to Figures 25A and 25B.

[0090] As shown in FIGS. 24A and 24B, in the first layer forming step, a first layer 92a is formed on the insulating film 21. First, a photoresist is applied to the insulating film 21 to form a photoresist layer (not shown). The photoresist layer is patterned by photolithography to expose the portion of the insulating film 21 where the first layer 92a is to be formed, and the portion where the first layer 92a is not to be formed is covered with the photoresist layer. In the first layer forming step, since the first layer 92a is not formed on the nanopore 23, the deposit film 27 in the nanopore 23 is covered with the photoresist layer. Next, an Au film is formed on the photoresist layer and on the exposed insulating film 21 by performing a sputtering method using Au as a target material. Next, the Au film on the photoresist layer is removed together with the photoresist layer by performing a lift-off method. The first layer 92a is formed by the Au film remaining on the insulating film 21.

[0091] As shown in FIGS. 25A and 25B, the second layer forming step forms the second layer 92b on the first layer 92a and the nanopore 23. First, a photoresist is applied to the insulating film 21 and the first layer 92a to form a photoresist layer (not shown). The photoresist layer is patterned by photolithography to expose the portion where the second layer 92b is to be formed, and the portion where the second layer 92b is not to be formed is covered with the photoresist layer. In the second layer forming step, the second layer 92b is partially formed on the nanopore 23 so that the width becomes smaller toward the center of the nanopore 23. For this reason, the portion of the deposit film 27 in the nanopore 23 where the second layer 92b is not to be formed is covered with the photoresist layer. Next, an Au film is formed on the first layer 92a and on the photoresist layer by performing a sputtering method using Au as a target material. Next, the Au film on the photoresist layer is removed together with the photoresist layer by performing a lift-off method. The Au film remaining on the first layer 92a and the deposit film 27 forms a second layer 92b.

[0092] 26A and 26B, in the flow path forming step, a flow path 29 connected to the nanopore 23 is formed in the substrate 20 by, for example, a method similar to that of the first embodiment. After the flow path 29 is formed in the substrate 20, the deposit film 27 is removed by wet etching using, for example, HF as a wet etching solution.

[0093] As described above, a nanogap electrode structure 80 is obtained by performing the insulating film formation process, the nanopore formation process, the nanopore filling process, the electrode formation process having the first layer formation process and the second layer formation process, and the flow path formation process (see FIG. 23).

[0094] The nanogap electrode 82 is not limited to the above-described configuration in which the second layer 82b has a stepped shape, and the portion provided on the first layer 82a and the portion provided on the nanopore 13 are different in position (height) in the Z-axis direction. For example, the second layer 82b may have a portion provided on the first layer 82a and a portion provided on the nanopore 13 at the same position in the Z-axis direction. After the first layer formation step (see FIGS. 24A and 24B) is performed, a deposit film is further formed on the deposit film 27, and the second layer formation step (FIGS. 25A and 25B) is performed. This allows the second layer 82b to be formed without a stepped shape.

[0095] The size of the outer shape of the first layer 82a in plan view can be changed by changing the area in which the first layer 92a is formed in the first layer forming process. The size of the outer shape of the second layer 82b in plan view can be changed by changing the area in which the second layer 92b is formed in the second layer forming process.

[0096] The nanogap electrode 82 is not limited to the above-described configuration in which the first layer 82a is provided only on the insulating film 11 and not on the nanopore 13. Although not shown, the first layer 82a may be provided on the insulating film 11 and the nanopore 13. When the first layer 82a is provided on the nanopore 13, the second layer 82b is provided only on the first layer 82a and not on the nanopore 13. In this way, the nanopore upper region 85 is formed by the first layer 82a, and the connection region 86 is formed by the first layer 82a and the second layer 82b, and the thickness of the nanopore upper region 85 can be made smaller than the thickness of the connection region 86.

[0097] The present invention is not limited to the above-described embodiments as they are, and in the implementation stage, the components can be modified and embodied without departing from the gist of the invention. In addition, various inventions can be formed by appropriately combining multiple components disclosed in the above-described embodiments. For example, a configuration in which some components are deleted from all the components shown in each embodiment can also be considered. Furthermore, the components described in different embodiments may be appropriately combined.

[0098] The present invention is not limited to the case where the nanogap electrode structure 10 or the nanogap electrode structure precursor 30 according to the first embodiment is provided to the analytical device 40; the nanogap electrode structure 50 according to the second embodiment, the nanogap electrode structure 60 according to the third embodiment, the nanogap electrode structure 70 according to the fourth embodiment, and the nanogap electrode structure 80 according to the fifth embodiment may also be provided to the analytical device 40. [Explanation of symbols]

[0099] 10,50,60,70,80 Nano gap electrode structure 11,21 Insulating film 12,22,52,62,82 Nanogap electrode 13,23 Nanopore 14a, 24a, 54a, 64a, 84a: Electrode portion (first electrode portion) 14b, 24b, 54b, 64b, 84b Electrode portion (second electrode portion) 15,25,55,65,85 Nanopore upper region 15a, 25a, 55a, 65a, 85a First nanopore upper region 15b, 25b, 55b, 65b, 85b Second nanopore upper region 16,26,56,66,86 Connection area 16a, 26a, 56a, 66a, 86a First connection region 16b, 26b, 56b, 66b, 86b Second connection area 17 Nanogap 18,20 PCB 19,29 Flow path 30 Nanogap electrode structure precursor 40 Analyzer 31,41 Power supply 42 Control section 43 Ammeter 44 Analysis Department 71,72,73 Adhesive layer

Claims

1. An insulating film having a nanopore through which a sample passes; a nano-gap electrode provided on the insulating film and having a pair of electrode portions connected to each other; Equipped with the pair of electrode portions each having a nanopore upper region located above the nanopore and a connection region located above the insulating film and connected to the nanopore upper region; The nanopore upper region is configured such that a current flowing when a voltage is applied between the pair of electrodes induces a disconnection due to electromigration to form a nanogap; In a plane perpendicular to a direction in which a current flows between the pair of electrodes, a minimum value of a cross-sectional area of ​​the nanopore upper region is smaller than a minimum value of a cross-sectional area of ​​the connection region; The nanopore upper region is formed by a thin-walled portion that is recessed so as to form a step in at least one of the front surface, which is the upper surface of the nanogap electrode, and the back surface, which is the lower surface of the nanogap electrode, and the thickness of the nanopore upper region is smaller than the thickness of the connection region. Nanogap electrode structure.

2. A nanogap electrode structure as described in claim 1, wherein the nanopore upper region is composed of a thin-walled portion with a recessed back surface.

3. The nanopore upper region is composed of a thin-walled portion recessed into the surface, The nanogap electrode structure according to claim 1 , wherein the nanogap electrode is composed of a first layer provided on the insulating film and a second layer provided on the first layer and on the nanopore.

4. An insulating film having a nanopore through which a sample passes; a nano-gap electrode provided on the insulating film and having a pair of electrode portions connected to each other; Equipped with the pair of electrode portions each having a nanopore upper region located above the nanopore and a connection region located above the insulating film and connected to the nanopore upper region; The nanopore upper region is configured such that a current flowing when a voltage is applied between the pair of electrodes induces a disconnection due to electromigration to form a nanogap; the nanopore upper region is made of a material obtained by altering a material constituting the connection region, The nanopore upper region made of the altered substance has a shape conforming to the nanopore in a plan view. Nanogap electrode structure.

5. The nanogap electrode structure of claim 4, wherein the upper region of the nanopore is altered by ion implantation, plasma treatment, laser annealing, or electron beam annealing.

6. An insulating film having a nanopore through which a sample passes; a nano-gap electrode provided on the insulating film and having a pair of electrode portions connected to each other; Equipped with the pair of electrode portions each having a nanopore upper region located above the nanopore and a connection region located above the insulating film and connected to the nanopore upper region; The nanopore upper region is configured such that a current flowing when a voltage is applied between the pair of electrodes induces a disconnection due to electromigration to form a nanogap; an adhesive layer provided between the insulating film and the nano-gap electrode; The adhesive layer is in contact with the connection region and is not in contact with the nanopore upper region, and has an opening in a portion corresponding to the nanopore. Nanogap electrode structure.

7. A preparation step of preparing a nanogap electrode including a pair of electrode portions connected to each other, the electrode portion being provided in an insulating film having a nanopore and having a nanopore upper region located above the nanopore; A nanogap forming step of applying a voltage between the pair of electrodes to form a nanogap in the upper region of the nanopore by electromigration, The preparation step includes: an insulating film forming step of forming the insulating film on a substrate; a nanopore forming step of forming the nanopore in the insulating film; an electrode forming step of forming the nano-gap electrode on the insulating film; a flow channel forming step of forming a flow channel in the substrate by etching from the back side of the substrate, the flow channel connecting to the nanopore; and etching the nanopore side to partially remove the back surface of the nanopore upper region in a thickness direction, and thinning the nanopore upper region by recessing it so as to form a step. A method for manufacturing a nanogap electrode structure having a nanogap.

8. A preparation step of preparing a nanogap electrode comprising a pair of electrode parts connected to each other, the electrode parts being provided in an insulating film having a nanopore and having a nanopore upper region located above the nanopore; A nanogap forming step of applying a voltage between the pair of electrodes to form a nanogap in the upper region of the nanopore by electromigration, The preparation step includes: an insulating film forming step of forming the insulating film on a substrate; a nanopore forming step of forming the nanopore in the insulating film; an electrode forming step of forming the nano-gap electrode on the insulating film; a flow channel forming step of forming a flow channel in the substrate by etching from the back side of the substrate, the flow channel connecting to the nanopore; and performing ion implantation, plasma treatment, laser annealing, or electron beam annealing on the upper region of the nanopore using the substrate on which the flow channel is formed and the insulating film on which the nanopore is formed as a mask, thereby altering the material of the upper region of the nanopore. A method for manufacturing a nanogap electrode structure having a nanogap.

9. The nano-gap electrode structure according to any one of claims 1 to 6, A power source that applies a voltage between the pair of electrodes; an ammeter for detecting a tunnel current flowing between the pair of electrodes in which the nanogap is formed; and an analysis unit that analyzes a sample based on the current value of the tunneling current.

10. The analytical apparatus of claim 9, further comprising a control unit that performs a first control of setting the voltage of the power supply to a first voltage and forming the nanogap between the pair of electrode units, and a second control of setting the voltage of the power supply to a second voltage different from the first voltage and generating the tunnel current between the pair of electrode units in which the nanogap is formed.

11. An analysis method using the analysis device according to claim 9 or 10, A first step of forming the nanogap; and a second step of detecting a tunneling current when the sample passes through the nanogap and analyzing the sample based on the current value of the tunneling current.

Citation Information

Patent Citations

  • Electrode systems and electrode systems used for molecular characterization

    JP2010513853A

  • Nanostructure device and manufacturing method therefor

    JP2012190840A

  • Nanopore sensors for characterizing biomolecules

    JP2014521956A

  • Method and system for nucleic acid sequencing by tunnel recognition

    JP2019518954A

  • Device and method for fabricating and calibrating nanoelectrode pairs

    JP2019525766A