Gravure ink composition for adsorbing carboxyl group-containing compounds, printed matter adsorbing carboxyl group-containing compounds, laminate, method for producing printed matter adsorbing carboxyl group-containing compounds, method for producing laminate, packaging bag, packaging container

A gravure ink composition with zinc oxide and resins forms an adsorption layer to suppress odors from processed foods and resin deterioration, addressing inefficiencies and risks in existing methods while maintaining print suitability.

JP7591397B2Active Publication Date: 2024-11-28TOKYO PRINTING INC MFG CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020213622
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-28
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Existing methods for suppressing unpleasant odors from processed foods and resin deterioration, such as acid and oxidation odors, are inefficient and pose risks like accidental ingestion or poor print suitability, especially when using zinc compounds in gravure printing.

Method used

A gravure ink composition containing zinc oxide and specific resins is used to form a carboxyl group-containing compound adsorption layer, which can be printed and laminated to suppress odors through chemical adsorption, suitable for gravure printing.

Benefits of technology

The composition effectively suppresses odors from processed foods and resin deterioration while maintaining printability and avoiding risks associated with traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591397000001
    Figure 0007591397000001
  • Figure 0007591397000002
    Figure 0007591397000002
  • Figure 0007591397000003
    Figure 0007591397000003
Patent Text Reader

Abstract

To provide a gravure ink composition for adsorbing a carboxyl group-containing compound which can suppress an acid odor generated from processed foods such as meat products such as seafood, egg products, rice, bread, noodle, confectioneries, milk products, frozen food, instant food and fermentation food, an unpleasant acid odor generated when contents containing a fatty acid compound constituting fat contained in the processed foods are subjected to a heat treatment, an unpleasant odor such as body odor and pet odor, and an acid odor due to deterioration of a resin, and which enables manufacture of printed matter having printability with a simple process.SOLUTION: A gravure ink composition for adsorbing a carboxyl group-containing compound is used for a printed matter including a base material and a layer for adsorbing acetic acid and the like on at least one side of the base material, and comprises: zinc oxide; at least one resin of an urethane resin, a (meth)acrylic resin, a polyamide resin, nitrocellulose, a chlorinated polyolefin resin and a vinyl chloride-vinyl acetate copolymer resin; and a solvent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink composition that suppresses the acidic odors generated by processed foods such as seafood and other meat products, egg products, and cooked rice, and the unpleasant oxidized odors generated when the contents containing fatty acid compounds that constitute the lipids contained in these processed foods are heated, as well as unpleasant body odors and sweat odors containing acidic gases emitted by the human body, pet odors (unpleasant odors), and oxidized odors (carboxylic acid odors) caused by deterioration of resins. [Background technology]

[0002] The acidic components contained in processed foods such as seafood and other meat products, egg products, and cooked rice, the acidic odors resulting from the acid treatment process during processing, and the fatty acid compounds (low-molecular-weight fatty acids, unsaturated fatty acids, etc.) that compose these lipids, generate an unpleasant retort odor when they are boiled or retorted. This retort odor is caused by the odor of the fatty acid compounds that compose the lipids, and the oxidized odor caused by volatile carbonyl compounds that are generated by the oxidation of fatty acids. These acidic odors and oxidized odors affect the taste and flavor of foods, so various studies have been conducted to suppress them. Various studies have also been conducted to suppress unpleasant odors such as body odor and pet odor, and oxidized odors caused by deterioration of resins.

[0003] There are several methods to suppress acid odors and retort odors, including kneading deodorizing ingredients into the film, encapsulating desiccants with deodorizing effects, and masking the acid odor. However, there are many problems with these methods, such as the risk of accidental ingestion or consumption, increased costs, and the inability to encapsulate or mask the odor with some foods.

[0004] In Patent Document 1, a coating agent containing a zinc compound is applied to the surface of an oxygen gas barrier material, and then dried to provide a coating layer containing the zinc compound on the surface of the oxygen gas barrier material. The oxygen gas permeability measured at 20°C and 80% relative humidity (RH) is 3 cm 3 (STP) / m 2A method for producing a package has been proposed, the method including a step of obtaining a packaging material having a viscosity of 0.1-24hr-atm or less, and a step of packaging the contents by arranging a coating layer containing the zinc compound on the side of the contents rather than the oxygen gas barrier material so as to absorb the retort odor generated from the contents, the method having a function of absorbing the retort odor generated from the food, and using a zinc compound as a material having a function of absorbing the retort odor. However, the coating agent containing the zinc compound is applied by a coating method using a coating device, and is not printed by a gravure printing method using a gravure printing machine, so a coating agent application step is required, which is troublesome. In addition, since the composition of the coating agent is unknown, there is a possibility that it cannot be applied to gravure printing as it is, and there is also a possibility that the printability (blocking resistance) is poor, so further consideration is required for application to gravure printing.

[0005] Patent Document 2 describes an interior design using fabric to which multiple deodorants have been applied, and discloses zinc oxide as a deodorant that is effective against acidic gas odors such as pet odors. However, a deodorant layer is formed on the fabric, and the thickness of the layer is 60 to 160 g / m2 in terms of dry weight. 2 It is very thick, and can only be formed by coating with a coater or by textile printing, and cannot be used at all for gravure printing. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2013-018551 A [Patent Document 2] JP 2014-054754 A Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, an object of the present invention is to provide a gravure ink composition for adsorbing a carboxyl group-containing compound that can suppress unpleasant odors such as acid odors generated from processed foods such as seafood and other meat products, egg products, cooked rice, bread, noodles, confectionery, dairy products, frozen foods, instant foods, and fermented foods, and unpleasant odors such as oxidized odors, body odors, and pet odors generated when contents containing fatty acid compounds that constitute the lipids contained in these processed foods are heat-treated, as well as oxidized odors due to resin deterioration, and that can produce printed matter in a simple process. [Means for solving the problem]

[0008] The present inventors have found that the above-mentioned problems can be solved by a gravure ink composition for adsorbing a carboxyl group-containing compound, which contains zinc oxide, at least one resin selected from the group consisting of urethane resin, (meth)acrylic resin, polyamide resin, soluble nitrocellulose, chlorinated polyolefin resin, and vinyl chloride-vinyl acetate copolymer resin, and a solvent, and have thus completed the present invention.

[0009] That is, the present invention provides (1) A gravure ink composition for adsorbing a carboxyl group-containing compound, which is used for a carboxyl group-containing compound-adsorbing printed matter having a substrate and a carboxyl group-containing compound-adsorbing layer on at least one of the substrates, The gravure ink composition for adsorbing a carboxyl group-containing compound is characterized in that it comprises zinc oxide (A), at least one resin (b1) selected from the group consisting of urethane resin, (meth)acrylic resin, polyamide resin, nitrocellulose, chlorinated polyolefin resin, and vinyl chloride-vinyl acetate copolymer resin, and a solvent (C). (2) The gravure ink composition for adsorbing a carboxyl group-containing compound according to (1), characterized in that the zinc oxide has an average particle size of 0.01 to 10 μm. (3) A carboxyl group-containing compound adsorption printed matter, characterized in that the gravure ink composition for adsorbing a carboxyl group-containing compound according to (1) or (2) forms a carboxyl group-containing compound adsorption layer on at least one surface of a substrate, the ink layer having a thickness of 0.1 to 5 μm. (4) A laminate comprising a substrate having a carboxyl group-containing compound adsorption layer formed by laminating the gravure ink composition for adsorbing a carboxyl group-containing compound according to (1) or (2) on at least one surface of the substrate, the ink layer having a thickness of 0.1 to 5 μm, and a laminate layer formed on the carboxyl group-containing compound adsorption layer or on the substrate on the opposite surface of the carboxyl group-containing compound adsorption layer. (5) The laminate according to (4), wherein the laminate layer is a sealant layer or a sealing layer. (6) The laminate according to (4), wherein the laminate layer is at least one laminate layer selected from the group consisting of dry laminate, non-solvent laminate, thermal laminate, extrusion laminate, co-extrusion laminate, and PE sandwich laminate. (7) preparing a substrate; a gravure printing step of printing the gravure ink composition for absorbing a carboxyl group-containing compound according to (1) or (2) on at least one of the substrates to form a carboxyl group-containing compound adsorption layer; (8) preparing a substrate; a gravure printing step of forming a carboxyl group-containing compound adsorption layer by printing the gravure ink composition for adsorbing a carboxyl group-containing compound according to (1) or (2) on at least one of the substrates in a film thickness of 0.1 to 5 μm; a laminating step or a coating step of forming a laminate layer on the carboxyl group-containing compound adsorption layer or on the substrate opposite to the carboxyl group-containing compound adsorption layer; A method for producing a laminate, comprising: (9) The method for producing a laminate according to (8), wherein the lamination step is a lamination step for forming a sealant layer or the coating step is a coating step for forming a seal layer. (10) The method for producing a laminate according to (8), wherein the lamination step is a lamination step for forming at least one laminate layer among a dry lamination step, a non-solvent lamination step, a thermal lamination step, an extrusion lamination step, a co-extrusion lamination step, and a PE sandwich lamination step. (11) A packaging bag essentially comprising a substrate, a carboxyl group-containing compound adsorption layer, and a sealant layer or a sealing layer, the packaging bag being characterized in that the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound according to (1) or (2). (12) A packaging container essentially comprising a substrate, a carboxyl group-containing compound adsorption layer, and an extrusion laminate layer, characterized in that the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound according to (1) or (2). This is regarding. Effect of the Invention

[0010] According to the present invention, in addition to being able to suppress the acidic odor generated from processed foods such as seafood and other meat products, egg products, and cooked rice, as well as the unpleasant oxidized odor generated when contents containing fatty acid compounds constituting the lipids contained in these processed foods are heat-treated, such as body odor and pet odor, and the oxidized odor due to resin deterioration, a gravure ink composition for adsorbing a carboxyl group-containing compound can be provided which can produce printed matter having printability in a simple process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail. Note that this embodiment is merely one embodiment of the present invention, and the present invention is not limited to this embodiment, and various modifications and embodiments are possible without departing from the gist of the present invention.

[0012] In the following description, (meth)acrylic and (meth)acrylate mean acrylic and methacrylic, acrylate and methacrylate, respectively.

[0013] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention (hereinafter also referred to simply as "adsorption ink composition") is a gravure ink composition for adsorbing a carboxyl group-containing compound used for a carboxyl group-containing compound adsorption printed matter comprising a substrate and a carboxyl group-containing compound adsorption layer on at least one side of the substrate, and the gravure ink composition for adsorbing a carboxyl group-containing compound preferably comprises zinc oxide (A), at least one resin (b1) selected from the group consisting of urethane resin, (meth)acrylic resin, polyamide resin, soluble cellulose, chlorinated polyolefin resin and vinyl chloride-vinyl acetate copolymer resin, and a solvent (C).

[0014] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention preferably contains zinc oxide (A), which is low in zinc toxicity and easily available, and which chemically adsorbs unpleasant odors such as acid odors, retort odors, body odors, and pet odors, as well as oxidized odors caused by resin deterioration.

[0015] In the present invention, the carboxyl group-containing compounds derived from acid odors, retort odors, body odors, pet odors, and oxidized odors due to resin deterioration include saturated fatty acids and sour components such as acetic acid, propionic acid, butyric acid, isobutyric acid, 3-methylbutyric acid, n-valeric acid, isovaleric acid, 3-methylvaleric acid, 4-methylvaleric acid, enanthic acid, capric acid, caproic acid, isocaproic acid, bellargonic acid, sorbic acid, benzoic acid, oxalic acid, lactic acid, sodium lactate, citric acid, trisodium citrate, adipic acid, DL-tartaric acid, L-tartaric acid, and sodium DL-tartrate. , sodium L-tartrate, azelaic acid, maleic acid, maleic anhydride, malonic acid, succinic acid, monosodium succinate, disodium succinate, sodium acetate, gluconic acid, glucono delta-lactone, fumaric acid, monosodium fumarate, DL-malic acid, sodium DL-malate, itaconic acid, α-ketoglutaric acid, and unsaturated fatty acids, such as α-linolenic acid, γ-linolenic acid, dihomo-γ-linolenic acid, linoleic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, and dipicolinic acid.

[0016] The zinc oxide (A) is preferably granular, and the average particle size is preferably 0.01 to 10 μm, more preferably 0.02 to 5 μm. By having an average particle size of 0.01 to 10 μm, the effect of adsorbing a carboxyl group-containing compound can be maintained, and there is no risk of zinc oxide settling over time. If the average particle size is smaller than 0.01 μm, the dispersibility is poor, and if the average particle size is larger than 10 μm, the transparency is poor. The average particle size here refers to the D50 particle size measured by a laser diffraction / scattering method. For example, a laser diffraction / scattering type particle size distribution measuring device LA-920 (manufactured by Horiba, Ltd.) or MICROTRAC 9320-X100 (manufactured by Honeywell) can be mentioned.

[0017] The content of zinc oxide (A) in the adsorption ink composition is preferably 1 to 70% by weight, more preferably 5 to 50% by weight. If the content of zinc oxide is less than 1% by weight, the adsorption of the carboxyl group-containing compound is poor, and if the content of zinc oxide is more than 70% by weight, the fluidity is poor.

[0018] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention preferably contains at least one resin (b1) selected from urethane resin, (meth)acrylic resin, polyamide resin, nitrocellulose, chlorinated polyolefin resin, and vinyl chloride-vinyl acetate copolymer resin. The method for preparing these resins may be any conventional method. These resins may be of one type or of two or more types. Commercially available products that can be used include LG-FK R medium (urethane-based), PULPTECC medium (polyamide-based), LRC-LAMI medium (nitrocellulose-based), SYNA-S medium (acrylic-based), NOPL-L medium (chlorinated polyolefin-based), and LAMREK medium (vinyl chloride-acetate-based) (all manufactured by Tokyo Ink Co., Ltd.).

[0019] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention may contain other thermoplastic resins (b2) in addition to the resin (b1). For example, shellacs, rosins, rosin-modified maleic acid resins, rosin-modified phenolic resins, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, polyethylene resins, polypropylene resins, vinyl chloride-vinyl acetate copolymer resins, vinyl chloride resins, ethylene-(meth)acrylic acid copolymers, polyester resins, polyvinylidene chloride resins, vinyl acetate resins, ketone resins, butyral resins, chlorinated ethylene vinyl acetate resins, ethylene vinyl acetate resins, styrene maleic acid resins, polystyrene resins, etc. Preferred are polyacetal resins, polycarbonate resins, casein, alkyd resins, acrylonitrile resins, acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, polysulfone resins, polyether resins, polyethersulfone resins, polyetherketone resins, modified polyphenylene ether resins, polyphenylenesulfone resins, polyimide resins, polyamideimide resins, amorphous polyarylate resins, polyetheretherketone resins, polyvinyl alcohol resins, ethylene-vinyl alcohol resins, polylactic acid, etc. These resins may be used alone or in combination of two or more kinds. Commercially available products that can be used include TPH medium, VESTA medium, LRC-NT medium, and KCNT medium (all manufactured by Tokyo Ink Co., Ltd.).

[0020] In the adsorption ink composition of the present invention, the content of the thermoplastic resin (B), which is the sum of the resin (b1) and the other thermoplastic resin (b2), is preferably 1 to 30% by weight, more preferably 3 to 20% by weight, calculated as solid content. If the content of the thermoplastic resin (B) is less than 1% by weight, the film-forming property of the adsorption ink composition is poor, and if the content of the thermoplastic resin (B) is more than 30% by weight, the fluidity of the adsorption ink composition is poor, and the manufacturing suitability is poor.

[0021] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention can use a solvent that is usually used in gravure ink. Examples of the solvent include aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, cyclohexane, methylcyclohexane and ethylcyclohexane, alcohol solvents such as methanol, ethanol, isopropyl alcohol, normal propyl alcohol, 1-butanol, 2-butanol, isobutanol and tert-butanol, ester solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate and tert-butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ... Examples of the glycol ether solvents include glycol ether solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether, and esterified products thereof. As the esterified products, acetates are mainly selected, for example, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. Among them, from the viewpoint of printability and versatility, toluene, ethyl acetate, n-propyl acetate, isopropyl alcohol, propylene glycol monomethyl ether, and methyl ethyl ketone are more preferable. These can be used alone or in combination. The solvent in the adsorption ink composition is preferably within the range of 65 to 98% by weight. If it is less than 65% by weight, the solid content will be high, the fluidity will be poor, and the ink manufacturing suitability will be poor, while if it exceeds 98% by weight, the ink film thickness will become locally non-uniform, irregular shading (swim phenomenon) will occur on the printed surface, the viscosity will be low, and zinc oxide may be more likely to settle.

[0022] The adsorption ink composition may also contain coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, waxes, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, etc. Any known and commonly used agents may be appropriately selected within the range that does not impair the properties of the adsorption ink composition.

[0023] The colorant may include a pigment or a dye or a mixture thereof. Examples of pigments include inorganic pigments such as titanium dioxide, red iron oxide, barium sulfate, calcium carbonate, silica, zinc oxide, zinc sulfide, mica, talc, and pearls, organic pigments such as phthalocyanine, insoluble azo, condensed azo, dioxazine, anthraquinone, quinacridone, perylene, perinone, thioindigo, and carbon black, and various other fluorescent pigments, metal powder pigments, and extender pigments. These pigments may be used alone or in combination of two or more. As dyes, those that dissolve or disperse in a solvent are preferred, and may be used alone or in combination of two or more. Among them, it is preferable to use pigments from the viewpoint of durability.

[0024] The substrate is preferably at least one selected from paper, plastic film or sheet, and laminates thereof. For example, polyester films such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate, polyolefin films such as polyethylene, polypropylene, and ethylene-vinyl acetate, polystyrene films, alcohol-based films such as ethylene-vinyl alcohol and polyvinyl alcohol, polyamide films or barrier polyamide films with a barrier layer disposed between them, polycarbonate films, polyacrylonitrile films, polyimide films, cellophane, moisture-proof cellophane, transparent vapor-deposited polyester films or transparent vapor-deposited polyamide films in which a vapor-deposited layer of alumina or silica is provided on a PET film or polyamide film, various coating films coated with polyvinylidene chloride resin, polyvinyl alcohol resin, polyacrylic acid resin, etc., co-extruded films of PET and nylon, and polylactic acid films can be mentioned. These may be either stretched or unstretched, and one or more types may be laminated. An appropriate one can be selected in consideration of mechanical strength, dimensional stability, etc. In addition, in order to improve the adhesion of the anchor coat layer or the laminate layer, the printed surface may be subjected to corona treatment, low-temperature plasma treatment, frame treatment, solvent treatment, coating treatment, etc., or may be previously subjected to a coating treatment. Among them, PET film, polyethylene film, polypropylene film, polyamide film, coating film, transparent vapor-deposited polyester film or transparent vapor-deposited polyamide film, co-extrusion film, etc. are preferred. The thickness of the substrate is not particularly limited as long as it is within a range that does not interfere with printability, winding suitability, etc., but is preferably 5 to 300 μm, more preferably 6 to 250 μm. In addition, the substrate may be a film having heat sealability such as a polyethylene film, so that the substrate itself may function as a sealant layer.

[0025] The paper substrate preferably includes at least one selected from coated paper, uncoated paper, and paper substrates laminated with a plastic film or the like. The paper substrate may be laminated with thermoplastic resin or the like by dry lamination, non-solvent lamination, extrusion lamination, or a method of laminating via an adhesive, or may be a suitable combination of these. A laminated body to which heat sealability has been imparted can also be used as the paper substrate. Methods of imparting heat sealability include lamination of a known sealant film, resin coating by extrusion lamination, coating of a heat seal agent or hot melt, and heat sealable resin processing by coextrusion, and the layer to which heat sealability has been imparted by these methods is also called a heat seal layer. The thickness of the paper substrate is not particularly limited as long as it is within a range that does not interfere with printability and winding suitability, but is preferably 5 to 800 μm, more preferably 6 to 600 μm.

[0026] In the carboxyl group-containing compound adsorbing printed matter of the present invention, the gravure ink composition for adsorbing a carboxyl group-containing compound preferably forms a carboxyl group-containing compound adsorption layer by laminating an ink layer on at least one surface of a substrate. The thickness of the ink layer is preferably 0.1 to 5 μm, more preferably 0.3 to 3 μm. If it is thinner than 0.1 μm, the adsorption property is reduced. If it is thicker than 5 μm, the blocking resistance is poor.

[0027] The carboxyl group-containing compound adsorption layer is preferably formed by laminating an ink layer on at least one surface of a substrate. The carboxyl group-containing compound adsorption layer is preferably formed by coating using a gravure printing method. In particular, it is more preferable to form the layer by coating using a gravure printing method using a multi-color gravure printer. The carboxyl group-containing compound adsorption layer may be an ink layer formed by laminating a gravure ink composition for carboxyl group-containing compound adsorption alone, or may include the ink layer and another ink layer formed by laminating another gravure ink composition. Furthermore, since the layer is formed by coating using a gravure printing method, not only full solid printing but also partial printing and reverse printing are possible. Depending on the final packaging mode, the position of the substrate for forming the carboxyl group-containing compound adsorption layer may change, and the order of formation of the ink layer and other ink layers may change. That is, for example, a carboxyl group-containing compound adsorption layer may be formed as in substrate / ink layer / other ink layer, and then another substrate may be laminated by dry lamination or the like (substrate / ink layer / other ink layer / DL / other substrate), or a carboxyl group-containing compound adsorption layer may be formed as in substrate / other ink layer / ink layer (or ink layer / other ink layer, etc., multiple layers), and then another substrate may be laminated by dry lamination or the like (substrate / other ink layer / ink layer / (other ink layer, etc. / )DL / other substrate). In addition, by using a printing machine having a reversing mechanism, a carboxyl group-containing compound adsorption printed matter having a variety of other ink layers can be obtained. For example, a carboxyl group-containing compound adsorption layer may be formed as in substrate / ink layer / other ink layer, and then the other ink layer may be reversed, and then another substrate may be laminated by dry lamination or the like (other substrate / DL / other ink layer / substrate / ink layer / other ink layer / DL / other substrate).

[0028] In addition to the carboxyl group-containing compound adsorption layer, the carboxyl group-containing compound adsorption printed matter of the present invention may have an intermediate layer laminated thereon to impart or enhance properties such as rigidity, stiffness, gas barrier properties, aroma retention, moisture resistance, pinhole resistance, dead hole properties, light blocking properties, and straight cut properties. When an intermediate layer is provided, it is not necessary to apply the carboxyl group-containing compound adsorption layer to the substrate, and the carboxyl group-containing compound adsorption layer may be provided on the intermediate layer. However, it is preferable that the gas barrier layer for imparting gas barrier properties is not provided closer to the source of the adsorbed substance than the carboxyl group-containing compound adsorption layer.

[0029] Examples of the intermediate layer include plastic films, sheets, and laminates thereof. Examples of plastic films include polyester films such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate; polyolefin films such as polyethylene, polypropylene, and ethylene-vinyl acetate; polystyrene films, alcohol-based films such as ethylene-vinyl alcohol and polyvinyl alcohol; polyamide films or barrier polyamide films with a barrier layer disposed between them; polycarbonate films, polyacrylonitrile films, polyimide films, cellophane, moisture-proof cellophane; transparent vapor-deposited polyester films or transparent vapor-deposited polyamide films in which a vapor-deposited layer of alumina or silica is provided on a PET film or polyamide film; various coating films coated with polyvinylidene chloride resin, polyvinyl alcohol resin, polyacrylic acid resin, and the like; co-extruded films of PET and nylon; and polylactic acid films. These may be stretched or unstretched, and one or more types may be laminated. An appropriate one can be selected in consideration of mechanical strength, dimensional stability, and the like. In order to improve adhesion, the bonding surfaces may be subjected to corona treatment, low-temperature plasma treatment, frame treatment, solvent treatment, coating treatment, etc., or may be previously subjected to such treatment. Both surfaces are preferably treated. The intermediate layer may have any thickness as long as it does not impair printability or windability, and the thickness is preferably from 5 to 300 μm, and more preferably from 6 to 250 μm.

[0030] The laminate of the present invention is preferably such that the carboxyl group-containing compound adsorption printed matter has a carboxyl group-containing compound adsorption layer formed by laminating an ink layer on at least one side of a substrate, and a laminate layer is laminated on the carboxyl group-containing compound adsorption layer or on the substrate on the opposite side of the carboxyl group-containing compound adsorption layer. The thickness of the ink layer is preferably 0.1 to 5 μm, more preferably 0.3 to 3 μm. The laminate layer is preferably a sealant layer or a sealing layer. Examples of the sealant layer include a laminate provided with heat sealability, a layer formed by laminating a known sealant film, or a layer formed by resin coating by extrusion lamination, and examples of the sealing layer include a layer formed by coating a heat seal agent or a hot melt agent.

[0031] As for the sealant layer, as long as the seal strength is sufficient, the lamination method is appropriately selected according to the substrate, application, configuration, etc. For example, lamination of a known sealant film via an adhesive to the carboxyl group-containing compound adsorption layer on the substrate (dry lamination method, non-solvent lamination method, wet lamination method), lamination by heat (thermal lamination method), resin coating by extrusion lamination method (extrusion lamination method, co-extrusion lamination method, PE sandwich lamination method), etc. can be preferably used. The laminate can be manufactured by one of these methods or a combination of them. The thickness of the sealant layer is not particularly limited, but is preferably 2 to 200 μm for a sealant film and 1 to 100 μm for a resin coating by extrusion lamination.

[0032] Examples of the sealant film include polyolefin films such as polyethylene, polypropylene, ethylene-vinyl acetate, and copolymers thereof, co-extruded films and colored films thereof, polystyrene films, polyacrylonitrile films, and ethylene-vinyl alcohol resin films. These films may be stretched or unstretched, and one or more types may be laminated.

[0033] When an adhesive is used in the dry lamination method, non-solvent lamination method, wet lamination method, extrusion lamination method, etc., a commercially available adhesive may be used, for example, a two-liquid or one-liquid type urethane resin adhesive, an acrylic type, an epoxy type, a polyester type, a polyethyleneimine type, a polybutadiene type, an aqueous urethane type, an isocyanate type, an organic titanium type, a starch type water-soluble adhesive, or an aqueous adhesive such as a vinyl acetate emulsion. A known application method can be used as a method for applying the adhesive to form a sealant layer, for example, a roll coater, a reverse roll coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, a dip coater, etc. can be used. The thickness of the adhesive is not particularly limited, but is preferably in the range of about 0.001 to 10 μm, and particularly preferably in the range of 0.01 to 5 μm.

[0034] Resins that can be used for resin coating by the extrusion lamination method include thermoplastic resins such as polyethylene resins such as LDPE, LLDPE, and HDPE, polypropylene resin, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins obtained by modifying polyethylene or polypropylene with maleic acid, fumaric acid, or the like, polystyrene resin, and polybutylene terephthalate resin, and these resins may be used alone or in combination.

[0035] The method of forming the sealing layer is appropriately selected according to the substrate, application, configuration, etc., as long as sufficient sealing strength can be ensured. For example, coating of a heat-sealing agent or hot melt can be preferably used. The laminate can be manufactured by one or a combination of these methods. The thickness of the sealing layer is not particularly limited, but is preferably 1 to 50 μm for coating of a hot-melt adhesive and 0.01 to 30 μm for coating of a heat-sealing agent.

[0036] Examples of the resin of the heat sealant include thermoplastic resins such as vinylidene chloride, shellacs, rosins, rosin-modified maleic acid resins, rosin-modified phenolic resins, nitrocellulose, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, polyamide resins, vinyl chloride-vinyl acetate copolymers, polyester resins, ketone resins, butyral resins, chlorinated polypropylene resins, chlorinated polyethylene resins, chlorinated ethylene vinyl acetate resins, ethylene vinyl acetate resins, (meth)acrylic resins, urethane resins, ethylene-vinyl alcohol resins, styrene-maleic acid resins, casein, and alkyd resins, which may be used alone or in combination of two or more. Examples include types in which these resins are dissolved in a solvent, or types dispersed in water such as acrylic emulsions, urethane emulsions, ethylene-vinyl alcohol emulsions, polyethylene emulsions, polypropylene emulsions, and ethylene vinyl acetate emulsions.

[0037] In addition, the laminate layer is preferably at least one of dry lamination, non-solvent lamination, thermal lamination, extrusion lamination, co-extrusion lamination, and PE sandwich lamination. The laminate layer can be produced by at least one of dry lamination, non-solvent lamination, thermal lamination, and resin coating by extrusion lamination (extrusion lamination, co-extrusion lamination, and PE sandwich lamination).

[0038] Resins that can be used for resin coating by the extrusion lamination method include polyethylene resins such as LDPE, LLDPE, and HDPE, polypropylene resins (homopolypropylene, random polypropylene, etc.), ethylene-vinyl acetate copolymers, ionomer resins, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl methacrylate copolymers, ethylene-propylene copolymers, methylpentene polymers, acid-modified polyolefin resins obtained by modifying polyethylene or polypropylene with maleic acid, fumaric acid, etc., polystyrene resins (general-purpose polystyrene (GPPS), high impact polystyrene (HIPS), expanded polystyrene (PSP), heat-resistant PSP, etc.), and thermoplastic resins such as polybutylene terephthalate resins, and these resins may be used alone or in combination.

[0039] The carboxyl group-containing compound-adsorbed printed matter of the present invention is preferably used for packaging, food preservation, retort, microwave oven, agriculture, civil engineering, fishing, automobile interior / exterior, marine, daily necessities, building material interior / exterior, housing equipment, medical / medical equipment, pharmaceutical, home appliances, furniture, stationery / office supplies, sales promotion, commercial, electrical / electronic industry, industrial materials, etc. Among these, it is more preferably used for packaging.

[0040] The method for producing a carboxyl group-containing compound adsorbing printed matter of the present invention preferably includes a step of preparing a substrate, and a gravure printing step of forming a carboxyl group-containing compound adsorption layer by printing the gravure ink composition for adsorbing a carboxyl group-containing compound on at least one of the substrates. The thickness of the carboxyl group-containing compound adsorption layer is preferably 0.1 to 5 μm, more preferably 0.3 to 3 μm. If it is less than 0.1 μm, the adsorption property of the carboxyl group-containing compound decreases. If it is more than 5 μm, the blocking resistance is poor.

[0041] The method for producing the carboxyl group-containing compound adsorbed printed matter may be a carboxyl group-containing compound adsorption layer formed by printing the gravure ink composition for adsorbing a carboxyl group-containing compound alone, or may include a gravure printing step for forming the carboxyl group-containing compound adsorption layer and another printed layer formed by printing another gravure ink composition, and is more preferably produced by a gravure printing step using a multicolor gravure printer. Furthermore, a gravure printer having a reversing mechanism may be used.

[0042] In addition to the carboxyl group-containing compound adsorption layer, a step of forming an intermediate layer for imparting or enhancing properties such as rigidity, stiffness, gas barrier properties, aroma retention, moisture resistance, pinhole resistance, dead hole resistance, light blocking properties, and straight line cutting properties may be included.

[0043] The method for producing the laminate of the present invention preferably includes a step of preparing a substrate, a gravure printing step of forming a carboxyl group-containing compound adsorption layer by printing the gravure ink composition for adsorbing a carboxyl group-containing compound on at least one side of the substrate with a thickness of 0.1 to 5 μm, and a lamination step or coating step of forming a laminate layer on the carboxyl group-containing compound adsorption layer or on the substrate on the opposite side of the carboxyl group-containing compound adsorption layer, and more preferably the lamination step is a lamination step of forming a sealant layer or the coating step is a coating step of forming a seal layer. The lamination step may also be a lamination step of forming at least one laminate layer among a dry lamination step, a non-solvent lamination step, a thermal lamination step, an extrusion lamination step, a co-extrusion lamination step, and a PE sandwich lamination step.

[0044] The lamination step for forming the sealant layer may be, for example, a step of laminating a laminate having heat sealability or a known sealant film, or a step of resin coating by extrusion lamination, and the coating step for forming the sealant layer may be a step of coating a heat seal agent or a hot melt agent.

[0045] The packaging bag of the present invention essentially comprises a substrate, a carboxyl group-containing compound adsorption layer, and a sealant layer or a sealing layer, and it is preferable that the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound.

[0046] The packaging bag may be of any known type, such as two-sided sealed, three-sided sealed, four-sided sealed, pillow sealed, standing pouch, envelope sealed, gusseted, or heat-cut sealed.

[0047] The packaging container of the present invention is a packaging container essentially comprising a substrate, a carboxyl group-containing compound adsorption layer, and an extrusion laminate layer, and it is preferable that the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound.

[0048] The packaging container may be any of the well-known forms used for packaging purposes, such as cups, trays, bottles, containers, boxes, cases, food containers, covers, lids, caps, labels, and in-mold cups.

[0049] The gravure ink composition for adsorbing a carboxyl group-containing compound of the present invention can be produced by a known method by uniformly dissolving or dispersing zinc oxide, a thermoplastic resin, a coloring material, various additives, etc. in a solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, a homomixer, etc. may be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the adsorption ink composition, they are preferably removed using a known filter or centrifuge, etc., since they deteriorate the printability and the quality of the printed matter.

[0050] The viscosity of the gravure ink composition for adsorbing a carboxyl group-containing compound is not particularly limited as long as it does not interfere with printing. In consideration of the manufacturability and handling of the ink composition used in gravure printing, it is preferably 10 to 1,000 mPa·s at 25°C. If it is less than 10 mPa·s, the viscosity is too low and zinc oxide tends to settle, and if it is more than 1,000 mPa·s, the fluidity is poor, causing problems during ink production and making it difficult to fill the container. In this case, it can be measured using a commercially available viscometer such as a Brookfield viscometer or a cone-plate viscometer.

[0051] The adsorption ink composition is preferably used in gravure printing, and may be applied as is, but may be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it tends to swim, and if it is more than 40 seconds, transferability during printing becomes poor.

[0052] The dilution solvent may be any solvent that can adjust the viscosity of the adsorption ink composition, and examples of the dilution solvent include organic solvents. Commercially available solvents are also available, and are not particularly limited. Examples of commercially available solvents include TA52 solvent (alcohol-based solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-based solvent), SL9155 solvent (non-toluene-based solvent), CN104 solvent (non-toluene-based solvent), AC372 solvent (non-toluene-based solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).

[0053] During printing, if necessary, a curing agent can be added to the adsorption ink composition. For example, polyisocyanate-based curing agents such as aromatic diisocyanates such as tolylene diisocyanate and 4,4'-diphenylmethane diisocyanate, aliphatic diisocyanates such as hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexyl diisocyanate, and pentane-1,5-diisocyanate (Stabio PDI), and modified forms such as trimethylolpropane trimer, isocyanurate, biuret, and allophanate can be used alone or in combination of two or more. Commercially available products include 24A-100, 22A-75, TPA-100, TSA-100, TSS-100, TAE-100, TKA-100, P301-75E, E402-808, E405-70B, AE700-100, D101, D201, A201H (manufactured by Asahi Kasei Corporation), Mytech Y260A (manufactured by Mitsubishi Chemical Corporation), Coronate HX, Coronate HL, Coronate L (manufactured by Tosoh Corporation), Desmodur N75MPA / X (manufactured by Covestro Japan Co., Ltd.), and LG Hardener C (manufactured by Tokyo Ink Co., Ltd.). EXAMPLES

[0054] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by weight."

[0055] [Preparation of gravure ink composition for adsorbing carboxyl group-containing compounds] Example 1 60 parts of LG-FK R medium (solid content 20%, manufactured by Tokyo Ink Co., Ltd.), 20 parts of zinc oxide (fine particle zinc oxide, solid content 100%, D50 average particle size 0.025 μm, manufactured by Teika Co., Ltd.), 15 parts of n-propyl acetate, 5 parts of isopropyl alcohol, and 100 parts of ceramic beads were charged and dispersed for 1 hour using a paint shaker to prepare a gravure ink composition G1 for adsorbing a carboxyl group-containing compound (abbreviation: adsorption ink G1). Similarly, the adsorption inks of Examples 2 to 9 were prepared according to the formulations in Table 1.

[0056] [Table 1]

[0057] [Preparation of printed matter adsorbing carboxyl-containing compounds] Example 10 Using a solid plate on a gravure proofing machine GRAVO-PROOF (product number: CM-W, manufactured by Nissho Gravure Co., Ltd.), the adsorption ink G1 of Example 1 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 1.0 μm on a 20 μm-thick stretched polypropylene film Pylen P-2161 (abbreviation: OPP, manufactured by Toyobo Co., Ltd.) to obtain an adsorption print PR1. Similarly, the adsorption ink and film thickness were changed as shown in Table 2, and adsorption prints PR10 to PR14 were obtained, respectively.

[0058] Example 11 Furthermore, the substrate was replaced with a 12 μm-thick polyethylene terephthalate film E-5102 (abbreviation: PET, manufactured by Toyobo Co., Ltd.), and the adsorption ink G1 was printed in a film thickness of 1.1 μm to obtain an adsorption print PR2.

[0059] Example 12 Furthermore, the substrate was replaced with Emblem ON-RT (abbreviation: NY, manufactured by Unitika Ltd.) made of a 15 μm-thick nylon film, and the adsorption ink G1 was printed in a film thickness of 0.9 μm to obtain an adsorption print PR3.

[0060] (Example 13) Furthermore, the substrate was replaced with a 12 μm thick vapor-deposited polyethylene terephthalate film, Barrilox 1011HGCR (abbreviation: vapor-deposited PET, manufactured by Toray Film Processing Co., Ltd.), and the adsorption ink G1 was printed at a film thickness of 1.0 μm to obtain an adsorption print PR4.

[0061] Example 14 Furthermore, the substrate was replaced with a 40 μm-thick unstretched linear low-density polyethylene film L-4102 (abbreviation: PE, manufactured by Toyobo Co., Ltd.), and the adsorption ink G2 was printed with a film thickness of 0.9 μm to obtain the adsorption print PR5. Similarly, the film thickness was changed as shown in Table 2 to obtain the adsorption prints PR15 to PR16.

[0062] Example 15 Furthermore, the base material is 50 g / m 2 Instead of the gravure paper, one-sided gloss bleached kraft paper (abbreviation: paper, manufactured by Oji Materia Co., Ltd.), the adsorption ink G3 was printed at a film thickness of 1.2 μm to obtain the adsorption print PR6. Similarly, the film thickness was changed as shown in Table 2 to obtain the adsorption prints PR17 to PR18.

[0063] (Example 16) Furthermore, the substrate was replaced with Styrophane SPH (abbreviation: CPS, manufactured by Oishi Sangyo Co., Ltd.), a non-oriented polystyrene film with a thickness of 18 μm, and the adsorption ink G4 was printed with a film thickness of 1.0 μm to obtain the adsorption print PR7. Similarly, the film thickness was changed as shown in Table 2 to obtain the adsorption print PR19 to PR20.

[0064] (Example 17) Furthermore, the substrate was replaced with a 25 μm-thick unstretched polypropylene film KT (abbreviation: CPP, manufactured by Sun-Tox Co., Ltd.), and the adsorption ink G5 was printed at a film thickness of 1.0 μm to obtain an adsorption print PR8. Similarly, the film thickness was changed as shown in Table 2 to obtain adsorption prints PR21 to PR22, respectively.

[0065] (Example 18) Furthermore, the substrate was replaced with a 12 μm thick polyethylene terephthalate film E-5102 (abbreviation: PET, manufactured by Toyobo Co., Ltd.), and the adsorption ink G6 was printed with a film thickness of 0.9 μm to obtain the adsorption print PR9. Similarly, the film thickness was changed as shown in Table 2 to obtain the adsorption prints PR23 to PR24.

[0066] Comparative Example 1 The LG-FK R medium used in Example 1 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed to a film thickness of 0.9 μm on a 20 μm-thick stretched polypropylene film, Pylen P-2161 (abbreviation: OPP, manufactured by Toyobo Co., Ltd.) to obtain an adsorption print PR25.

[0067] Comparative Example 2 Furthermore, the substrate was changed to a 12 μm-thick polyethylene terephthalate film E-5102 (abbreviation: PET, manufactured by Toyobo Co., Ltd.), and printing was performed in a film thickness of 1.1 μm in the same manner as in Comparative Example 1, to obtain an adsorption print PR26.

[0068] Comparative Example 3 Furthermore, the substrate was changed to a 15 μm-thick nylon film Emblem ON-RT (abbreviation: NY, manufactured by Unitika Ltd.), and printing was performed in a film thickness of 1.0 μm in the same manner as in Comparative Example 1 to obtain an adsorption print PR27.

[0069] Comparative Example 4 Furthermore, the substrate was changed to a 12 μm thick vapor-deposited polyethylene terephthalate film, Barrilox 1011HGCR (abbreviation: vapor-deposited PET, manufactured by Toray Film Processing Co., Ltd.), and printing was performed with a film thickness of 1.1 μm in the same manner as in Comparative Example 1, to obtain an adsorption print PR28.

[0070] Comparative Example 5 Furthermore, the substrate was changed to a 40 μm-thick unstretched linear low-density polyethylene film L-4102 (abbreviation: PE, manufactured by Toyobo Co., Ltd.), and the PULPTECC medium used in Example 2 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 1.1 μm to obtain an adsorption print PR29.

[0071] Comparative Example 6 Furthermore, the base material is 50 g / m 2 Instead of the gravure paper, one-sided gloss bleached kraft paper (abbreviation: paper, manufactured by Oji Materia Co., Ltd.), the LRC-LAMI medium used in Example 3 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 1.1 μm to obtain an adsorption print PR30.

[0072] Comparative Example 7 Furthermore, the substrate was changed to Styrophane SPH (abbreviation: CPS, manufactured by Oishi Sangyo Co., Ltd.), an unstretched polystyrene film with a thickness of 18 μm, and the SYNA-S medium used in Example 4 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 1.0 μm to obtain an adsorption print PR31.

[0073] Comparative Example 8 Furthermore, the substrate was changed to a 25 μm-thick unoriented polypropylene film KT (abbreviation: CPP, manufactured by Sun-Tox Co., Ltd.), and the NOPL-L medium used in Example 5 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 1.0 μm to obtain an adsorption print PR32.

[0074] Comparative Example 9 Furthermore, the substrate was changed to a 12 μm-thick polyethylene terephthalate film E-5102 (abbreviation: PET, manufactured by Toyobo Co., Ltd.), and the LAMREK medium used in Example 6 was adjusted to a viscosity of 17 seconds using a Zahn cup No. 3 with a dilution solvent (40 parts MEK, 40 parts propyl acetate, 20 parts isopropyl alcohol), and then printed at a film thickness of 0.9 μm to obtain an adsorption print PR33.

[0075] Comparative Example 10 As in Example 10, the adsorption ink G1 was used as shown in Table 3, and the film thickness was changed to 0.05 μm to obtain an adsorption print PR34.

[0076] Comparative Example 11 As in Example 10, the adsorption ink G1 was used and the film thickness was changed to 6.0 μm as shown in Table 3, to obtain the adsorption printed matter PR35.

[0077] The adsorptive printed matter of Examples 10 to 33 and Comparative Examples 1 to 11 was evaluated for blocking resistance, and the results are shown in Tables 2 and 3.

[0078] <Blocking resistance> The printed material was cut into pieces measuring 3cm x 3cm, the printed surface was placed over the non-printed surface, and the material was then subjected to a 500g / cm2 test at 50°C for 24 hours. 2 After applying a load of 1000 mm, the overlapping portion of the printed and non-printed surfaces was peeled off, and the state of ink peeling was observed, and the peeling resistance at that time was evaluated. Those that showed no ink peeling or peeling resistance were judged to have good blocking resistance. Ink peeling and peeling resistance were evaluated on a three-point scale: ○: no ink peeling or peeling resistance, △: slight ink peeling was observed and there was peeling resistance (no practical problems), ×: ink peeling was observed over the entire surface and there was considerable peeling resistance.

[0079] [Laminated body production] Takelac A-969V / A-5 (abbreviation: DL, manufactured by Mitsui Chemicals, Inc.) was applied onto the adsorption ink layer of the adsorption printed matter PR1 using A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and a 30 μm-thick unstretched polypropylene film, Pylen P-1128 (abbreviation: CPP, manufactured by Toyobo Co., Ltd.), was then laminated thereon, and the resulting product was aged at 40° C. for 24 hours to obtain a laminate LAM1 of PR1 / DL / CPP. Similarly, the adsorption printed matter PR1 was replaced with the adsorption printed matters PR10 to PR14, PR25 and PR34 to obtain laminates LAM11 to LAM15, LAM26 and LAM36.

[0080] Similarly, instead of the adsorption printed material PR1, the adsorption printed material PR2 was coated with Takelac A-525 / Takenate A-52 (manufactured by Mitsui Chemicals, Inc.) and A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and a 60 μm thick unstretched polypropylene film, Torayfan NO ZK93KM (abbreviation: Reto CPP, manufactured by Toray Film Processing Co., Ltd.), was then laminated, and the resulting laminate was aged at 40°C for 24 hours to obtain a PR2 / DL / Reto CPP laminate LAM2. Similarly, the adsorption printed matter PR1 was replaced with the adsorption printed matter PR26 to obtain a laminate LAM27.

[0081] Similarly, Takelac A-969V / A-5 (abbreviation: DL, manufactured by Mitsui Chemicals, Inc.) was applied onto the adsorption ink layer of the adsorption printed matter PR2 using A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and aging was carried out for 24 hours at 40°C, thereby obtaining a PR2 / DL / LLDPE laminate LAM3, in place of Takelac L-4102 (abbreviation: LLDPE, manufactured by Toyobo Co., Ltd.), a 40 μm-thick unstretched polyethylene film. Similarly, the adsorption printed matter PR2 was replaced with the adsorption printed matter PR26 to obtain a laminate LAM28.

[0082] Similarly, instead of the adsorption printed material PR1, the adsorption printed material PR3 was coated with Takelac A-969V / A-5 (manufactured by Mitsui Chemicals, Inc.) and A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and a 40 μm thick unstretched polyethylene film, Rix L-4102 (abbreviation: LLDPE, manufactured by Toyobo Co., Ltd.), was laminated, and then aging was performed at 40°C for 24 hours to obtain a PR3 / DL / LLDPE laminate LAM4. Similarly, the adsorption printed matter PR1 was replaced with the adsorption printed matter PR27 to obtain a laminate LAM29.

[0083] Similarly, the adsorption printed material PR1 was replaced with the adsorption printed material PR4, and Takelac A-525 / Takenate A-52 (manufactured by Mitsui Chemicals, Inc.) was coated with A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and a 60 μm thick unstretched polypropylene film, Torayfan NO ZK93KM (abbreviation: Reto CPP, manufactured by Toray Film Processing Co., Ltd.), was used instead. The resulting film was aged at 40°C for 24 hours to obtain a laminate LAM5 of PR4 / DL / Reto CPP. Similarly, the adsorption printed matter PR1 was replaced with the adsorption printed matter PR28 to obtain a laminate LAM30.

[0084] The PE layer of the substrate of the adsorption printed matter PR5 functions as a heat seal layer, so that the PE layer was used as it is to form the laminate LAM6. Similarly, the adsorption printed matter PR29 was directly used as a laminate LAM31.

[0085] The opposite side (on the paper) of the adsorption ink layer of the adsorption print PR6 was subjected to a corona treatment, and low-density polyethylene resin Petrothene 204 (abbreviation: LDPE40, manufactured by Tosoh Corporation) was melt-extruded and laminated at 40 μm using an extrusion laminator at a line speed of 100 m / min. Further, the adsorption ink layer was subjected to a corona treatment, and low-density polyethylene resin Petrothene LW01 (abbreviation: LDPE20, manufactured by Tosoh Corporation) was melt-extruded and laminated at 20 μm to obtain a laminate LAM7 of LDPE20 / / PR6 / / LDPE40. (" / / " indicates extrusion laminate.)

[0086] Similarly, the adsorption printed matter PR6 was replaced with the adsorption printed matters PR17 to PR18 and PR30 to obtain laminates LAM18 to LAM19 and LAM32 of LDPE20 / / PR17 / / LDPE40.

[0087] Impact-resistant polystyrene resin E640N (abbreviation: HIPS, manufactured by Toyo Polystyrene Co., Ltd.) was melt-extruded onto the adsorption ink layer of the adsorption printed matter PR7 using an extrusion laminator at a line speed of 100 m / min, and laminated at a thickness of 200 μm to obtain a PR7 / / HIPS laminate LAM8.

[0088] Similarly, the adsorption printed matter PR7 was replaced with the adsorption printed matters PR19 to PR20 and PR31 to obtain PR19 / / HIPS laminates LAM20 to LAM21 and LAM33.

[0089] Homopolypropylene resin E111G (abbreviation: PP, MFR = 0.5 g / 10 min, manufactured by Prime Polymer Co., Ltd.) was melt-extruded onto the adsorbent ink layer of the adsorbent printed matter PR8 using an extrusion laminator at a line speed of 100 m / min, and laminated at a thickness of 600 μm to obtain a PR8 / LD / / PP laminate LAM9.

[0090] Similarly, the adsorption printed matter PR8 was replaced with the adsorption printed matters PR21 to PR22 and PR32 to obtain laminates LAM22 to LAM23 and LAM34 of PR21 / LD / / PP.

[0091] Takelac A-525 / Takenate A-52 (manufactured by Mitsui Chemicals, Inc.) and A-Bar OSP-10 (manufactured by OSG System Products, Inc.) were applied onto the adsorption ink layer of the adsorption printed matter PR9, and a 60 μm-thick unstretched polypropylene film, Torayfan NO ZK93KM (abbreviation: CPP, manufactured by Toray Film Processing Co., Ltd.), was then laminated thereon, and the resulting product was aged at 40° C. for 24 hours to obtain a PR9 / DL / CPP laminate LAM10.

[0092] Similarly, the adsorption printed matter PR9 was replaced with the adsorption printed matters PR23 to PR24 and PR33 to obtain laminates LAM24 to LAM25 and LAM35 of PR23 / DL / CPP.

[0093] The adsorptivity of the laminates LAM1 to LAM36 was evaluated, and the results are shown in Tables 2 and 3. Note that adsorptivity was not evaluated for Comparative Example 11 (PR35), which was rated as "x" for blocking resistance. In Table 3, this is indicated by "-".

[0094] <Adsorption properties of laminate> A sample piece cut from the laminate to a size of 10 cm x 10 cm was placed in a polyvinyl fluoride bag with a rubber stopper and sealed by heat sealing, after which 3 L of air was sealed in through the rubber stopper, and further test gas (acetic acid) was added so that the gas concentration was 50 ppm, and this was left to stand at room temperature. The gas concentration in the bag was measured using a detector tube through the rubber stopper at regular intervals (10 minutes, 1 hour, 3 hours, 6 hours, 24 hours). When the gas concentration became equal to or less than the lower limit of quantification (1 ppm), the measurement was terminated at that point. In addition, a blank test was performed by carrying out the same operation as above without putting in the sample piece. The measured gas concentration after 24 hours was compared to evaluate the adsorption. The gas concentration after 24 hours was also evaluated for the sample that became equal to or less than the lower limit of quantification before 24 hours and the measurement was terminated. The lower the gas concentration after 24 hours, the better the adsorption was judged to be. The test was evaluated on a two-point scale: Good: Gas concentration after 24 hours was less than 50 ppm; Bad: Gas concentration after 24 hours remained at 50 ppm.

[0095] <Ammunition Test> The laminate LAM1 was laminated so that the sealant layer or seal layer was on the innermost surface, and bonded by heat sealing at 190°C for 1 second to obtain a bag-shaped packaging bag with an opening, and vinegared rice was placed in this packaging bag as the contents, and the opening was sealed by heat sealing at 190°C for 1 second. At this time, as a comparative control, a packaging bag was obtained in the same manner using laminate LAM26 (the same substrate as laminate LAM1, but without adsorbent ink printing), and vinegared rice was placed in it and sealed. In Table 3, this is indicated as "-". Furthermore, packaging bags were obtained in the same manner for laminates LAM11 to 13 (different adsorbed inks), LAM14 to 15, and LAM36 (same substrate as laminate LAM1 but different adsorbed ink film thicknesses), and vinegared rice was placed inside and sealed. These were placed in a constant temperature bath at 50°C and left to stand for 24 hours, after which they were opened and the acetic acid odor was checked and compared. Those that had a reduced acetic acid odor compared to the control that was not printed with the adsorbent ink were judged to have good adsorption properties. Eight testers rated the product on a two-point scale: Good: All eight testers felt that the acetic acid odor had been reduced, and Bad: At least one tester felt that the acetic acid odor was the same. Similarly, the laminates LAM3 and LAM28, LAM4 and LAM29, LAM5 and LAM30, and LAM6 and LAM31 were also evaluated in the same manner.

[0096] [Table 2]

[0097] [Table 3]

[0098] From Tables 2 and 3, it is clear that the adsorption inks 1 to 9 of Examples 1 to 9 have better adsorption properties than the results of Examples 10 to 33. It is also clear that the adsorption printed matter PR1 to PR24 has good blocking resistance. It is clear from the results of Comparative Examples 1 to 9, which do not use the adsorption ink of the present invention, that the effect of adsorption is not achieved. It is clear that even if the adsorption ink of the present invention is used, if the printing film thickness is smaller than the appropriate range (PR34), the effect of adsorption is not achieved, and if the printing film thickness is large, blocking resistance is poor and, although there may be an effect of adsorption, it is clear that it cannot be used as a printed matter (PR35). In addition, in the live ammunition test using the adsorbent ink of the present invention, it is clear that the acetic acid odor is reduced compared to that of the case where no adsorbent ink is used. Furthermore, it is clear that the adsorbent effect is not achieved if the printing film thickness is smaller than the appropriate range. Therefore, in addition to being able to suppress the acidic odors that arise from processed foods such as seafood and other meat products, egg products, cooked rice, bread, noodles, sweets, dairy products, frozen foods, instant foods, and fermented foods, as well as the unpleasant oxidized odors that arise when the contents containing the fatty acid compounds that make up the lipids contained in these processed foods are heat-treated, such as body odor, pet odors, and oxidized odors due to resin deterioration, it is also possible to produce printed materials and packaging materials that are suitable for printing using a simple process.

Claims

1. A gravure ink composition for adsorbing a carboxyl group-containing compound, which is used for a carboxyl group-containing compound-adsorbing printed matter having a substrate and a carboxyl group-containing compound-adsorbing layer having a thickness of 0.1 to 3 μm on at least one of the substrates, The gravure ink composition for adsorbing a carboxyl group-containing compound is characterized by comprising zinc oxide (A) having an average particle size of 0.01 to 0.025 μm, at least one resin (b1) selected from urethane resins, chlorinated polyolefin resins, and vinyl chloride-vinyl acetate copolymer resins, and a solvent (C).

2. A carboxyl group-containing compound adsorption printed matter, characterized in that the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1 is laminated on at least one surface of a substrate to form a carboxyl group-containing compound adsorption layer having an ink layer thickness of 0.1 to 3 μm.

3. A laminate comprising: a carboxyl group-containing compound adsorption layer formed by laminating the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1 on at least one surface of a substrate, the ink layer having a thickness of 0.1 to 3 μm; and a laminate layer formed on the carboxyl group-containing compound adsorption layer or on the substrate on the opposite surface of the carboxyl group-containing compound adsorption layer.

4. 4. The laminate according to claim 3, wherein the laminate layer is a sealant layer or a sealing layer.

5. 4. The laminate according to claim 3, wherein the laminate layer is at least one of a dry laminate, a non-solvent laminate, a thermal laminate, an extrusion laminate, a co-extrusion laminate, and a PE sandwich laminate.

6. Providing a substrate; and a gravure printing step of printing the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1 on at least one of the substrates to form an ink layer having a thickness of 0.1 to 3 μm to form a carboxyl group-containing compound adsorption layer.

7. Providing a substrate; a gravure printing step of forming a carboxyl group-containing compound adsorption layer by printing the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1 on at least one of the substrates in a thickness of 0.1 to 3 μm; a laminating step or a coating step of forming a laminate layer on the carboxyl group-containing compound adsorption layer or on the substrate opposite to the carboxyl group-containing compound adsorption layer; A method for producing a laminate, comprising:

8. The method for producing a laminate according to claim 7, wherein the laminating step is a laminating step for forming a sealant layer, or the coating step is a coating step for forming a sealing layer.

9. 8. The method for producing a laminate according to claim 7, wherein the lamination step is a lamination step for forming at least one laminate layer among a dry lamination step, a non-solvent lamination step, a thermal lamination step, an extrusion lamination step, a co-extrusion lamination step, and a PE sandwich lamination step.

10. A packaging bag essentially comprising a substrate, a carboxyl group-containing compound adsorption layer having a thickness of 0.1 to 3 μm, and a sealant layer or a sealing layer, wherein the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1.

11. A packaging container comprising a substrate, a carboxyl group-containing compound adsorption layer having a thickness of 0.1 to 3 μm, and an extrusion laminate layer, the packaging container being characterized in that the carboxyl group-containing compound adsorption layer is formed from the gravure ink composition for adsorbing a carboxyl group-containing compound according to claim 1.

Citation Information

Patent Citations

  • Deodorizing composition

    JP1990080050A

  • Heat exchanger made of aluminum

    JP1992254196A

  • Method for manufacturing package

    JP2013018551A

  • Interior using deodorant functionality fabric, and deodorant functionality fabric

    JP2014054754A

  • Acetic acid adsorption film

    JP2017171738A