Lattice modified carbons and their chemical functionalization.
Autocatalytic growth of modified carbon lattices with controlled non-hexagonal rings and functional group addition addresses the need for gentler and more controllable carbon functionalization, achieving reactive and selective functionalization without harsh chemicals, suitable for various applications.
Patent Information
- Application Number
- JP2020543477
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-10-24
- Filing Date
- 2018-10-23
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2038-10-23
AI Technical Summary
Existing methods for chemically functionalizing carbon lattices are harsh, poorly controlled, and lack specificity in terms of aspect, site, hierarchy, and group functionalities, necessitating a need for gentler and more controllable processes to achieve optimal properties for specific applications.
The use of autocatalytic growth of modified carbon lattices and lattice assemblies, allowing for selective chemical functionalization through oxidation reactions, including the introduction of non-hexagonal rings and controlled functional group addition to the basal planes, using commercially available carbons as nuclei.
This approach enables more reactive and controllable functionalization of carbon lattices, eliminating the need for aggressive processes like the Hummer method, and allows for gentler, safer, and environmentally friendly methods, achieving site-selective, region-selective, and group-selective functionalization.
Smart Images

Figure 0007591404000028 
Figure 0007591404000029 
Figure 0007591404000030
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 576,433, filed October 24, 2017, which is incorporated herein by reference in its entirety for all purposes. This application is also related to PCT / US17 / 17537, filed February 10, 2017, which is incorporated herein by reference in its entirety for all purposes.
[0002] The following disclosure relates to methods and materials used to synthesize chemically functionalized carbon-based materials. Synthesis can be accomplished by synthesizing lattice-modified carbon via self-catalyzed lattice growth and may include chemical functionalization of carbon-based materials. More specifically, the disclosure relates to the synthesis of carbon lattices and multilayer lattice assemblies with controlled concentrations of non-hexagonal rings, and the covalent attachment of functional groups to the basal planes of these lattices and assemblies. [Background technology]
[0003] "Low-dimensional carbon" 1 A common method for synthesizing polycyclic carbon polymers involves chemical vapor deposition (CVD) of polycyclic carbon polymers. Polycyclic carbon polymers, also referred to herein as "carbon lattices" or "lattices", are made up of sp 2 atoms in a multiatomic ring structure. 2 Graphene is an atomic monolayer sheet (i.e., a sheet with a thickness of a single atom) of carbon atoms bonded together through hybrid bonds. Figure 1 shows a graphene lattice, which includes carbon atoms bonded together in a hexagonal ring structure. During CVD, carbonaceous gas molecules contact a catalytic material, such as a transition metal foil, which catalyzes the decomposition of the gas molecules and deposits a carbon lattice on the catalyst. After synthesizing a lattice or a multilayer assembly of lattices, the properties of the lattice can be modified by chemically functionalizing the lattice. This method of adding functional groups often requires harsh and poorly controlled oxidation reactions, such as the Hummers process.
[0004] 1A carbon-based structure is defined herein as having at least one structural feature that is 100 nm or less in size.
[0005] There is an unmet need in the art for gentler, more controllable methods for producing chemically functionalized carbon. There is an unmet need for carbons with side-specific, site-specific, hierarchical, and group-specific functionality. In general, more sophisticated functional architectures at the lattice and particle level can be used to construct carbons with properties optimized for specific applications. Summary of the Invention
[0006] The use of commercially available carbons as lattice nuclei (e.g., carbon black or graphite) allows for the effective modification of the chemical functionality of these carbons. It has been shown that carbon black and activated carbon can be used as inexpensive catalysts to produce hydrogen from hydrocarbon gases, resulting in potentially valuable carbon by-products. However, the tiling and structure of new lattice domains synthesized with these nuclei have not been thoroughly explored, nor have chemical functionalizations been investigated. Thus, there is an unmet need in the art for chemical functionalization of carbon catalyst lattices and lattice assemblies produced via hydrocarbon reforming.
[0007] This disclosure describes, inter alia, novel methods and materials relating to the autocatalytic growth of modified carbon lattices and lattice assemblies, and the use of lattice-modified carbon as a feedstock for the formation of chemically functionalized nanostructured carbon, particularly via oxidation reactions.
[0008] Also described herein are novel methods and materials related to the autocatalytic growth of modified carbon lattices and lattice assemblies with lattice properties that enable selective chemical functionalization, including the use of these materials as feedstocks for side-selective, site-selective, region-selective, hierarchical-selective, and group-selective functionalization. In particular, the present disclosure describes the utilization of modified carbon lattices and lattice assemblies with reactive surfaces to obtain basal plane oxidation.
[0009] The methods and materials described herein offer several advantages over the prior art. For example, the lattice modified carbons described herein can be more chemically reactive than graphene or graphitic carbons. Thus, as a feedstock for chemical functionalization processes, the lattice modified carbons can be more easily and controllably functionalized. This can eliminate the need for more aggressive functionalization processes utilized with graphitic feedstocks, such as the Hummers process, allowing for the use of milder, safer, and more environmentally friendly functionalization processes.
[0010] Under certain CVD conditions, the carbon lattice can autocatalyze ("self-catalyze") its own growth in the absence of a catalyst. Modeling of this phenomenon with density functional theory predicts that, for example, a hexagonal lattice may grow without a non-carbon catalyst via dissociative adsorption of methane at the lattice edges. The carbon adatoms then bond to each other and assemble into new ring structures that are incorporated into the lattice. At the same time, the lattice edges are regenerated and can adsorb new carbon adatoms. In this autocatalytic growth regime, the carbon lattice acts as a catalyst.
[0011] Due to the catalytic role of the lattice, a "carbon lattice nucleus", "nucleus" or "seed" is required for the autocatalytic growth process. A nucleus, as defined herein and shown in FIG. 2, is the initial structural state of the lattice over any time interval during which autocatalytic lattice growth occurs. Thus, a nucleus is not defined by its size, geometry or ring structure, but only by its designation as the structural initiation point of some extended lattice structure that grows from the nucleus over the interval of autocatalytic growth. At the end of the interval, the new regions of the lattice, i.e., regions that were not present in the nucleus state, are referred to as "new growth regions" or "new regions". These regions are also shown in FIG. 2.
[0012] In an autocatalytic CVD process, pre-existing lattice nuclei are introduced into a CVD reactor and then grown via autocatalysis. Alternatively, it may nucleate and grow in situ. Nucleation may be induced by a non-carbon catalyst (e.g., metals, metal oxides, metal carbonates, metal halides). Alternatively, when nucleation occurs without a non-carbon catalyst (e.g., the nuclei are formed on the surface of another carbon lattice or by gas-phase pyrolysis of a hydrocarbon), it is referred to herein as "auto-nucleation."
[0013] Autocatalytic growth can occur in several situations. One situation is isolated - i.e., the region of the growing lattice (a "region" is defined herein as any contiguous subset of carbon atoms that make up a two-dimensional carbon lattice, as shown in FIG. 3) is not in contact with another solid molecule or particle. Another situation is on a support - i.e., one or more regions of the lattice are in contact with a larger solid molecule or particle. Another situation, similar to supported growth, is when one lattice is in overlapping contact with itself or another carbon lattice. Overlapping contact includes contact between two lattice side faces. A "side" is defined herein as the two lattice planes associated with a given region of the carbon lattice, as shown in FIG. 3. Except for certain topological anomalies, such as a Möbius strip, there are always two sides to a lattice geometry, in which case the two "sides" can be simply thought of as two localized faces formed by localized regions of the lattice. The sides of a lattice, which are a two-dimensional feature, are distinct from the "edges" of a lattice, which are one or more terminations of one dimension of the lattice.
[0014] Overlapping contact between two lattice sides may occur during CVD growth; for example, when lattices grown from multiple nearby nuclei on a common support surface encounter each other, they may subside or sink into each other to form an overlap. Alternatively, a lattice may overlap itself (e.g., in a folded configuration formed when one side contacts itself, or in a scroll configuration resulting when one side contacts the other, respectively). When a lattice overlaps with itself or another lattice, such an overlapping architecture is referred to herein as a "multilayer feature." Any carbon structure that includes one or more multilayer features is referred to herein as a "multilayer structure" ("MS"). As shown in FIG. 4, a multilayer structure may include a number of geometries.
[0015] In a multilayer structure, each overlapping lattice region is called a "layer." While it is possible for a single lattice to contain more than one layer (e.g., a folded nanoplatelet or scrolled nanotube), the most common type of multilayer structure contains multiple lattices (e.g., a graphitic stack of lattices or a multi-walled nanotube). In carbon grown via template-guided CVD, the walls grown around the template are typically multilayered. The walls may contain lattices that overlap other lattices, and lattices that wrap around themselves in three dimensions.
[0016] The lattice may contain different ring structures and different molecular patterns (herein referred to as "tilings"). 2 The crystalline arrangement of bonded carbon atoms is known as "graphene" and has regular honeycomb tiling. Some graphene lattices may incorporate a low concentration of non-hexagonal rings, e.g., pentagonal, heptagonal, octagonal rings. Non-hexagonal rings, when incorporated into the lattice at low concentrations, may only slightly locally alter the tiling of the graphene lattice. Because the incorporation of non-hexagonal rings causes a deviation from the hexagonal tiling of graphene, the non-hexagonal rings are referred to herein as "defects." The frequency or concentration of defects in a lattice, expressed as the percentage of non-hexagonal rings relative to all rings in the basal plane, is referred to herein as the "imperfections" or "defect concentrations" of the lattice.
[0017] The higher the concentration of non-hexagonal rings, the more extensive and ubiquitous the tiling can be. In fact, some lattice types may be composed entirely of non-hexagonal rings, such as pentagraphene, which has regular pentagonal tiling. Other lattice structures may contain pentagons, hexagons, and heptagons in a random glassy tiling, sometimes referred to as "amorphous graphene". These non-hexagonal tilings may have significantly different properties compared to graphene, such as higher lattice strain, different interlayer spacing and spacing distribution of multilayer lattice assemblies, and non-zero local curvature associated with topological irregularities. Controlling the introduction of non-hexagonal rings into the lattice while it is growing (e.g., by introducing them into the lattice at a controlled frequency) is referred to herein as "lattice modification". Carbon lattices created via lattice modification processes are referred to as "modified carbon lattices" or "modified lattices".
[0018] Lattice modification can allow for tuning of the chemical potential energy of the lattice, which in turn can make the addition of functional groups (referred to herein as "chemical functionalization" or "functionalization") easier and more controllable. The "functionality" (i.e., the chemical nature of the lattice or multilayer structure resulting from chemical functionalization) can affect the manner in which the particles interact with other materials and media. To the extent that non-hexagonal lattice features can be induced to form in controllable concentrations during lattice growth, the lattice modification process can facilitate the production of chemically functionalized lattices and lattice assemblies.
[0019] One of the most common functionalizations of nanostructured carbon is the covalent attachment of oxygen-based functional groups, or "oxygen groups." Oxygen groups that are preferentially attached to the basal planes of the graphene lattice include ether / epoxide (COC), hydroxyl (C-OH), and carbonyl (C=O). In lattices with localized protrusions, carboxyl and ether groups are preferentially attached to the basal planes (e.g., edge-wall carboxylation of nanotubes). Carboxylation can result in the cleavage of C-C bonds and the formation of vacancies. A sufficient level of oxidation on the graphene lattice results in what is commonly referred to as graphene oxide ("GO"). In many procedures for making graphene oxide, progressive oxidative etching of the carbon lattice can produce an adsorbed layer of organic residue on the surface of the lattice. This residue, also referred to herein as "oxidation residue" ("OD"), can be physisorbed to the GO lattice. As such, the oxygen groups of the OD may not be lattice-bonded to the underlying lattice. OD may be present on the GO unless the lattice is subsequently base washed, resulting in the OD desorbing. Another effect of the progressive oxidative etch may be to introduce or enlarge vacancies, as well as introduce other defects into the lattice.
[0020] Oxygen groups and oxidation residues on the GO lattice can affect the bonding and formation of interfaces between the lattice and other materials. For example, residues on the as-produced GO lattice have been shown to reduce the crosslink density at the interface of GO and the epoxy matrix in epoxy nanocomposites. Reducing the crosslink density between the matrix and the lattice can hinder the ability of the polymer to transfer stress to the lattice, reducing the modulus of the nanocomposite. Compared to epoxy nanocomposites made with OD-decorated GO, GO with the ODs removed can allow for a denser crosslink interface, resulting in a higher modulus.
[0021] The oxygen groups in the ODs on GO typically account for a significant percentage of the total oxygen reported for GO. XPS analysis shows that after removal of the ODs by base washing, the C:O ratio decreases from about 2:1 to 6:1. Thus, the lattice-bound oxygen may often be much lower than the reported C:O ratios associated with GO indicate. Base washing and chemical reduction can also cause significant "de-epoxidation" of the lattice by converting lattice-bound epoxides to other oxygen groups. This conversion is undesirable if epoxide moieties are required for certain applications, in which case removal of the ODs may be problematic.
[0022] In addition to the problems of lattice decomposition and residue generation, the most common methods of oxidizing graphitic carbon, such as the Brody, Staudenmeyer, Hoffman, and Hummer processes, as well as their variations, have other significant drawbacks. First, they generally offer little control over the process, both in terms of the location and extent of oxidation. These methods oxidize by reaction of the graphitic carbon feedstock with strong acids (usually H2SO4, HNO3, or some combination thereof) and strong oxidizing agents (KMnO0, KClO3, NaNO3, etc.) that intercalate into the graphite. However, these materials are not completely consumed and can generate corrosive waste streams. Second, they require hazardous chemicals and generate explosive and toxic gases (ClO2, NO2, N2O4, etc.). Thus, they require production, storage, and consumption of hazardous reagents and can generate hazardous waste.
[0023] A milder and more controllable process to form GO using defective graphene lattices as a source of oxidation has been explored. However, it has been shown in the literature that this can only be performed with limited controllability and little industrial scalability. In one example, reactive defects were introduced into pretreated graphite via electron beam irradiation, resulting in the oxidation of the defective graphite. However, the use of electron beam radiation and other aspects of the process may not be easily scalable for mass production, and control of the oxidation was limited. Furthermore, electron beam irradiation may not penetrate certain layers of the multilayer lattice assembly. Thus, there remains an unmet need for a controllable and mild process to generate carbon lattices with basal plane oxidation.
[0024] Lattice modification methods can provide new functionalization capabilities due to the ability to form more highly modified lattice raw materials that make functionalization more selective. For example, common raw materials such as graphite or graphite nanoplatelets used to make graphene oxide can include carbon lattices with planar sides. Thus, the overall chemical reactivity of either side of the lattice can be the same. In contrast, single-walled nanotubes have a concave inner surface and a convex outer surface. It has been shown that the convex side of a nanotube lattice with a hexagonal tiling is more chemically reactive than the planar lattice of a hexagonal tiling due to its distortion, whereas the concave side of a nanotube lattice with a hexagonal tiling is less chemically reactive than the planar lattice of a hexagonal tiling. Thus, functionalization of single-walled nanotubes tends to be substantially one-sided, which is described herein as "monotopic" or "side-selective" functionalization. Double-sided functionalization is described herein as "ditopic" functionalization.
[0025] Unlike the specific case of nanotubes, where each side is 100% concave or convex, there may be other lattices where each side exhibits localized concave and convex topographical features, or "sites." Thus, the difference in reactivity of concave and convex lattice curvatures may not only allow for side-selective functionalization, but also "site-selective" functionalization (i.e., topographical site-specific functionalization effects). For example, an amorphous graphene lattice may have a pleated topography, where each side exhibits a large number of both concave and convex sites. When exposed to an oxidizing agent, these nanoscale sites may be selectively unfunctionalized or functionalized based on their curvature, resulting in a mapping of functional groups that substantially correspond to the topography of the lattice.
[0026] Another type of selectivity can be based on the region(s) of the lattice that is / are functionalized. For example, a modified lattice may contain a hexagonal planar lattice core around which one or more amorphous, pleated new lattice regions are grown concentrically. The core region and the new region(s) may have different chemical reactivities such that the lattice may be selectively functionalized at the planar core region but not at the pleated new lattice region. This may result in mapping of functional groups to correspond to the region properties of the lattice, or "region-selective" functionalization.
[0027] Another type of site selectivity may relate to specific functionally distinct "hierarchies" (a "hierarchy" is defined herein as a distinct band within a multilayer structure that includes one or more adjacent layers). For example, in a multilayer structure synthesized on a template or support, cell wall development typically proceeds from the inside out, i.e., the inner band of the lattice grows first next to the template, then the middle band of the lattice grows above the inner band, and finally the outer band. Once the walls are formed, lattice modifications can be exploited to form distinct tilings associated with each hierarchical level. This can be exploited to form functional surfaces (a "surface" is defined herein as the outer face of the external lattice region) that change how the particle interacts with other media but do not affect the internal chemistry of the particle. For example, the internal lattice of the particle may remain conductive while the oxidized surface becomes non-conductive. Hierarchical selective oxidation is not possible with oxidation methods such as the Hummers method, where an oxidizing agent is intercalated into the multilayer structure, and not only the surface of the particle but also its internal lattice is oxidized.
[0028] In addition to site-selective functionalization, lattice modification may allow for "group-selective" functionalization, where certain types of functional groups are preferentially formed. When functionalizing lattices with dense, small topographical features, carboxyls and ethers may be preferentially formed due to the predominance of convex-specific functionality and concave-specific non-functionality, with a relative paucity of planar functionality. Highly carboxylated basal faces may result in a more polar and hydrophilic surface, improving dispersibility in polar media.
[0029] Lattice-modified carbon can be utilized as a source of material for selective functionalization. This can be particularly beneficial for selectively oxidizing the surface of templated carbon particles. Selective surface oxidation can make the particles more dispersible while leaving the internal lattice structure intact and remaining unoxidized.
[0030] Additional advantages and applications will become readily apparent to those skilled in the art from the detailed description that follows. The examples and descriptions herein are to be regarded as illustrative in nature and not as limiting.
[0031] Exemplary embodiments are described with reference to the accompanying drawings. [Brief description of the drawings]
[0032] [Figure 1] Illustrative illustration of the hexagonal lattice structure of graphene. The lattice is a single atom thick and contains multi-atom ring structures. The ring structures form tilings of the lattice, which can be regular or irregular based on the type of rings present. [Diagram 2] Illustrates carbon lattice nuclei and new growth regions formed from the edges of the nuclei over a period of autocatalytic lattice growth, which together constitute a modified lattice structure that may have locally altered tiling. [Diagram 3] Illustration of the basic features of a lattice, including the edges of the lattice, which comprise the one-dimensional terminations of the lattice, the sides of the lattice, which comprise the two surfaces formed by any domain, and the lattice regions, which are some localized subset of the carbon atoms of the lattice. [Figure 4] 1 is an illustration of several hypothetical multi-layer structures, each featuring two or more layers. The templated multi-layer structure shows a cross-section of a template and a multi-layer wall formed around the template. [Diagram 5] 13A-13D are scanning electron microscope (SEM) images of samples A1-A4 after extraction of the MgO template. [Figure 6] FIG. 13 Transmission electron microscope (TEM) images of samples A1, A3, and A4 after extraction of the MgO template, showing the cross-section or wall thickness of the multilayer structure. [Figure 7] 1 shows Raman spectra of samples A1 to A4 before extraction of the MgO template. [Figure 8]Thermogravimetric analysis (TGA) curves of the oxidized samples A1-A4. Two oxidation protocols were performed: 20 h and 40 h. All TGA curves were performed in argon (at a heating rate of 20 °C / min). [Figure 9] C / O ratios extracted from X-ray photoelectron spectroscopy (XPS) analysis of samples A3, A3 80xBT-2h, and A3 80xBT-20h, showing the O / C ratio (A) and the decomposition of carbon-oxygen moieties (B). [Figure 10] 14 is SEM images of sample A3 and its oxidized form for different oxidation times of 2 h and 20 h. [Figure 11] 1 shows Raman spectra of samples A1, A3, and B1 before and after extraction of the MgO template. [Figure 12] 14 SEM images of samples A1, A3, and B1 after extraction of the MgO template. [Figure 13] 13A-13D are transmission electron microscope (TEM) images of samples A1, A3, and B1 after extraction of the MgO template, showing the cross-section or wall thickness of the multilayer structure. [Figure 14] TGA curves of the oxidized variants of samples A1, A3, and B. Two oxidation protocols were used: 20 h and 40 h. All TGA curves were performed in argon (at a heating rate of 20° C. / min). [Figure 15] 13A-13C are images showing the difference in wetting behavior of B2-Ox and B3-Ox after resuspension in water. [Figure 16] FIG. 1 is a schematic diagram showing a typical reaction between a silane and a hydroxyl group via a two-step hydrolysis and condensation reaction mechanism. [Figure 17] 13A-13D are images of CO-Ox and CO-Ox-OTES (before and after agitation) showing the change in wetting behavior of the functionalized carbon. [Figure 18] Figure 1 shows the TGA curves of CO-Ox and CO-Ox-OTES. All TGA curves were performed in argon (at a heating rate of 20°C / min). [Figure 19]1A-1D are SEM images of samples carbon black control (D0) and autocatalytically grown carbon at low (D1) and high (D2) temperatures, respectively. [Figure 20] TGA curves of samples D0, D1, and D2 (A), showing the different thermal properties of the additional carbon grown on the carbon black. Also shown are the oxidized forms D1-Ox and D2-Ox (B), showing the different behavior after oxidation. All TGA curves were performed in air (at a heating rate of 10 °C / min). [Figure 21] Figure 1 shows TGA curves of sample E2 40xABT-20h (control, BW and BW-RA) showing the percentage mass loss (A) and normalized differential weight (B). All TGA curves were performed in argon (at a heating rate of 20°C / min). [Figure 22] 3 shows the TGA curves of samples E0, E1 and E2 after 24 hours of piranha treatment showing the percentage of mass loss. All TGA curves were performed in argon (at a heating rate of 20° C. / min). [Figure 23] 3 shows the TGA curves of samples E0, E1 and E2 after 24 hours of piranha treatment showing the normalized differential weight. All TGA curves were performed in argon (at a heating rate of 20° C. / min). [Figure 24] 3 shows the TGA curves of samples E1 and E2 after 24 hours of piranha treatment and base washing, showing the normalized differential weight. All TGA curves were performed in argon (at a heating rate of 20° C. / min). [Diagram 25] 1 shows the TGA curves of samples E0 and E2 after 60 hours of APS treatment showing the percentage of mass loss. All TGA curves were performed in argon (at a heating rate of 20° C. / min). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The following discussion, including the experimental results described, demonstrates the use of autocatalytic lattice growth to modify lattices of non-hexagonal rings of controllable density, and of locally altered molecular tilings. The resulting lattice-modified lattices can then be chemically functionalized. Such autocatalytic lattice growth can be obtained under a number of different conditions without substantially departing from the essence of the process described herein.
[0034] Described herein is a chemically functionalized carbon lattice formed by a method that includes heating carbon lattice nuclei in a reactor to a temperature between room temperature and 1500° C. The method also includes exposing the carbon lattice nuclei to a carbonaceous gas to cause carbon atoms in the carbonaceous gas to adsorb onto the edges of the carbon lattice nuclei and to covalently bond the adsorbed carbon atoms to one another in the polyatomic rings, a portion of which includes a non-hexagonal ring, and to cause the polyatomic rings to covalently bond to one another at one or more new lattice regions extending from the carbon lattice nuclei, thereby forming a modified lattice incorporating non-hexagonal rings, and exposing a portion of the modified lattice to one or more chemicals to attach at least one of a functional group and a molecule to the modified lattice.
[0035] In some embodiments, the method may further include nucleating carbon lattice nuclei in the reactor. The carbon lattice nuclei may be placed on a template or support during the method. The template or support may include an inorganic salt. The template or support may include an internal carbon lattice of at least one of template carbon, carbon black, graphitic carbon, and activated carbon particles. The template or support may induce the formation of a modified lattice. The carbonaceous gas may include organic molecules. The modified lattice may include a portion of a multilayer lattice assembly. The non-hexagonal ring may include at least one of a 3-membered ring, a 4-membered ring, a 5-membered ring, a 7-membered ring, an 8-membered ring, and a 9-membered ring. The functionalized non-hexagonal ring may form an amorphous or haeckelite lattice structure with non-planar lattice characteristics.
[0036] The method may further include adjusting at least one of the frequency and tiling of non-hexagonal rings formed in the modified lattice by selecting conditions under which the rings are formed. The selected conditions may include at least one of the species of carbonaceous gas, partial pressure of the carbonaceous gas, total gas pressure, temperature, and lattice edge geometry. The method may include substantially maintaining the conditions while the new lattice regions are formed. The method may include substantially altering the conditions while the new lattice regions are formed. Altering the conditions may include heating or cooling the new lattice regions while the new lattice regions are formed. Altering the conditions may include conveying the modified lattice through two or more separate reactor zones, each separate reactor zone having a separate local condition while the new lattice regions are formed. Conveying the modified lattice through two or more separate local conditions may include conveying the modified lattice through a gradient of local conditions while the new lattice regions are formed. The separate local conditions may include separate levels of thermal energy. The separate local conditions may include separate local temperatures in the range of 300°C to 1100°C. Conveying the modified lattice may include conveying the modified lattice in a moving or fluidized bed. The concentration of non-hexagonal ring structures may be substantially the same throughout the modified lattice.
[0037] The concentration of non-hexagonal ring structures in one region of the modified lattice may be substantially different from the concentration of non-hexagonal ring structures in another region of the modified lattice. The modified lattice may include a surface of a multi-layer assembly of the modified lattice. Non-planar features in the modified lattice may increase the chemical reactivity of the lattice. A Raman spectrum of the modified lattice or the multi-layer assembly of the modified lattice may exhibit an IT / IG peak intensity ratio of less than 0.25. A Raman spectrum of the modified lattice or the multi-layer assembly of the modified lattice may exhibit an IT / IG peak intensity ratio of 0.25 to 0.50. A Raman spectrum of the modified lattice or the multi-layer assembly of the modified lattice may exhibit an IT / IG peak intensity ratio of 0.50 to 0.75. A Raman spectrum of the modified lattice or the multi-layer assembly of the modified lattice may exhibit an IT / IG peak intensity ratio of greater than 0.75. The d-spacing of the interlayer as determined by XRD may exhibit a peak intensity at 3.45 Å to 3.55 Å. The d-spacing of the interlayer as determined by XRD may show a peak intensity at 3.55 Å to 3.65 Å. Exposing a portion of the modified lattice to one or more chemicals may include exposing at least two sides of the exposed portion of the modified lattice. Exposing a portion of the modified lattice to one or more chemicals may include exposing only one side of the exposed portion of the modified lattice. The unexposed side of the modified lattice may be physically blocked by an adjacent carrier. The adjacent carrier may include one or more carbon lattices. Exposing a portion of the modified lattice to one or more chemicals may include covalently attaching a functional group to the exposed portion of the modified lattice. Exposing a portion of the modified lattice to one or more chemicals may include mechanically agitating the modified lattice in the presence of the chemicals. Attaching at least one of the functional groups and molecules to the modified lattice may include forming a covalent bond between a lattice-bonded carbon atom and at least one of an oxygen atom, a nitrogen atom, a sulfur atom, a hydrogen atom, and a halogen atom. The step of attaching at least one of the functional group and the molecule to the modified lattice may include forming a covalent bond between a lattice-bonding carbon atom and an oxygen atom.The step of attaching at least one of the functional group and the molecule to the modified lattice may include forming a covalent bond between a lattice-bonded carbon atom and a nitrogen atom in the form of a quaternary nitrogen cation.
[0038] At least one of the one or more chemicals may include an acid. The acid may include oleum, sulfuric acid, oleum, nitric acid, hydrochloric acid, chlorosulfonic acid, fluorosulfonic acid, alkylsulfonic acid, hypophosphorous acid, perchloric acid, perbromic acid, periodic acid, and combinations thereof. The acid may include an intercalating agent that intercalates into two or more lattices of the multilayer lattice assembly. At least one of the one or more chemicals may be an oxidizing agent. The oxidizing agent may include at least one of the group consisting of peroxides, peracids, tetroxides, chromates, dichromates, chlorates, perchlorates, nitrogen oxides, nitrates, nitric acid, persulfate ion-containing compounds, hypochlorites, hypochlorous acid, chlorine, fluorine, steam, oxygen gas, ozone, and combinations thereof. The oxidizing agent may include at least one of peroxides, hypochlorites, and hypochlorous acid. The oxidizing agent may include an acidic solution. The oxidizing agent may include a basic solution. The method may include forming at least one of carboxyl, carbonate, hydroxyl, carbonyl, ether, and epoxide functional groups in the basal plane of the exposed portion of the modified lattice. The method may include selectively forming one or more types of functional groups based on at least one of the following factors: local defect structure of the exposed lattice, local curvature of the exposed lattice, pH of the oxidizing solution, concentration of the oxidizing solution, temperature of the oxidizing solution, oxidizing species in the oxidizing solution, time the lattice is exposed to the oxidizing solution, ion concentration of the oxidizing solution. The step of selectively forming one or more types of functional groups may include selectively forming carboxyl functional groups. Forming carboxyl functional groups may introduce vacancies in the basal plane of the carbon lattice. The method may include etching the vacancies to form nanoscale holes in the basal plane. The step of exposing a portion of the modified lattice to one or more chemicals may include a progressive oxidative etch. The progressive oxidative etch of the lattice may generate organic residues. The organic residues may be adsorbed onto the surface of the multilayer lattice assembly. The progressive oxidative etching of the lattice may produce substantially no organic debris. The atomic ratio of carbon to oxygen on the exposed side of the modified lattice may be from 1:1 to 2:1. The atomic ratio of carbon to oxygen on the exposed side of the modified lattice may be from 2:1 to 4:1.The atomic ratio of carbon to oxygen on the exposed side of the modified lattice may be between 4:1 and 6:1. The atomic ratio of carbon to oxygen on the exposed side of the modified lattice may be between 6:1 and 8:1. The atomic percentage of nitrogen in the modified lattice may be greater than 5%. The atomic percentage of nitrogen in the modified lattice may be between 1% and 5%. The atomic percentage of sulfur in the modified lattice may be greater than 5%. The atomic percentage of sulfur in the modified lattice may be between 1% and 5%.
[0039] The method may include exposing the modified lattice to a basic solution after exposing it to an oxidizing agent. The method may include exposing the modified lattice to a basic solution to increase the total mass of labile groups by more than 50% as determined by thermogravimetric analysis of the functionalized carbon in an argon atmosphere. The total mass of labile groups on the oxidized carbon may increase by 25% to 50% as determined by thermogravimetric analysis of the functionalized carbon in an argon atmosphere after exposure to the basic solution. The step of exposing the carbon to a basic solution may include deprotonating carboxyl groups to form carboxylate groups. The method may include exposing the modified lattice to an acidic solution. The step of exposing the modified lattice to an acidic solution may include protonating carboxylate groups to form carboxyl groups. The method may include covalently bonding a molecule to the chemically functionalized carbon lattice. The molecule may include a coupling agent. The coupling agent may include a siloxane or a polysiloxane.
[0040] Some embodiments include a method of forming a chemically functionalized carbon lattice, the method comprising heating carbon lattice nuclei in a reactor to a temperature between room temperature and 1500° C. The method includes exposing the carbon lattice nuclei to a carbonaceous gas to adsorb carbon atoms in the carbonaceous gas onto the edges of the carbon lattice nuclei, covalently bonding the adsorbed carbon atoms to one another in polyatomic rings where a portion of the polyatomic rings incorporate non-hexagonal rings, and covalently bonding the polyatomic rings to one another at one or more new lattice regions extending from the carbon lattice nuclei, thereby forming a modified lattice including non-hexagonal rings. The method further comprises exposing a portion of the modified lattice to one or more chemicals to attach at least one of a functional group and a molecule to the modified lattice.
[0041] In the experiments disclosed herein, CVD was performed under ambient pressure. Gases used during CVD included methane (CH4), propylene (C3H6), and argon (Ar). In some experiments, MgO templates were used. Such templates were formed from magnesium carbonate (Light Magnesium Carbonate or L-MgCO3) supplied by Akrochem. Hydrochloric acid (HCl) supplied by Shape Chemicals was used for acid extraction of the MgO templates.
[0042] An MTI rotary tube furnace and quartz tube with a programmable maximum temperature of 1200° C. was used for all CVD experiments. The furnace was equipped and operated according to the numbered scheme described below.
[0043] In Scheme 1, the furnace was maintained horizontally. The sample powder was loaded directly into a quartz tube with an outer diameter of 100 mm and pushed into the central area within the heating zone of the furnace. Ceramic blocks were inserted into the tube and placed on either side of the heating zone. Glass wool was used to fix the position of the ceramic blocks. The tube was equipped with a stainless steel flange, an upstream gas supply inlet, and a downstream gas outlet. The quartz tube was rotated at 2.5 or 10 RPM during furnace heating, CVD process, and furnace cooling.
[0044] In scheme 2, both the furnace and the quartz tube (60 mm outer diameter) were tilted / inclined. The tube was rotated. A "Schenk Accurate" reciprocating auger feeder was inserted into the high end of the tube and the air gap between the feeder's outer diameter and the quartz tube's inner diameter was sealed with a freely rotating silicone foam washer. The auger feeder continuously metered the powder into the high end of the quartz tube. The downstream end of the tube remained open to atmosphere. To flow process gas through the auger feeder, the auger feeder was modified upstream of the quartz tube with a gas supply inlet upstream.
[0045] In Scheme 3, the furnace was maintained horizontally. The powder was placed in a ceramic boat. The boat was then placed in a quartz tube (outer diameter 60 mm) and pushed into the central region of the tube (i.e., within the heating zone of the furnace). The quartz tube was not rotated. One end of the tube was equipped with a stainless steel flange and a gas supply inlet. The opposite end of the tube remained open to the atmosphere.
[0046] All Raman spectroscopic characterizations were performed using a ThermoFisher DXR Raman microscope equipped with a 532 nm excitation laser, and all TGA characterizations were performed on a TA Instruments Q600 TGA / DSC.
[0047] Raman spectroscopy is commonly used to characterize the lattice structure of carbon. Three main spectral features are typically observed: 2 Associated with bonded carbon: G band (1585 cm -1 ), G' band (alternatively called the "2D band"; 2500-2800 cm -1 ), and the "D band" (1200-1400 cm -1 The G band is sp 2 sp 2 It can provide Raman characteristics of carbon crystals. In contrast, the D band arises from out-of-plane vibrations caused by structural defects in carbon. The higher the D band, the more broken sp 2 High bond ratio, sp3 It indicates a high degree of bonding. Thus, the D band is associated with lattice disorder, and the ratio of the intensity of the D band to the G band is a measure of defects. However, as disorder increases beyond a certain threshold, accurate D band measurements become difficult to obtain because the D peak broadens and decreases in height. As this broadening occurs, the valley between the D and G peaks becomes shallower. For this reason, the present disclosure defines and uses a fourth feature, the "T band," which is the valley between the D and G peaks, to identify disorder instead of the D band. The depth of the T band valley is related to the degree of order. The T band valley intensity, referred to herein as "T band intensity," can be measured to indicate the broadening of the D peak. As used herein, the T band intensity is defined as the local minimum intensity value that occurs between the wavenumber associated with the D peak and the wavenumber associated with the G peak.
[0048] The intensities of G, 2D, D, and T bands are herein denoted as I, G , I G’ (or I 2D ), I D , and I T It is specified as I G’ / I G (or I 2D / I G ) peak ratio is the sp 2 As mentioned above, I D / I G The ratio is sp 2 Non-sp for carbon 2 It can be understood as a measure of the carbon fraction and can be related to the defect concentration. In the case of highly disordered carbon, I T / I G The ratio reflects the broadening of the D peak and is related to the defect concentration, so I D / I G It has the same physical interpretation as
[0049] For each sample, the Raman spectrum of 25 different points was measured. The measurements were made on a rectangular grid of 5 x 5 points with a spacing between the points of 20 μm. The spectra of the 25 different points were then averaged to create a composite spectrum. All peak intensity ratios reported for each sample are derived from the composite spectrum of the sample.
[0050] To investigate the control and influence of defect concentration, as well as the oxidation of defects, experiments A to E were performed. Details of each experiment are described below.
[0051] Experiment A - Procedure In experiment A, the influence of the metal oxide template (MgO) and other parameters such as hydrocarbon type and reactor temperature on the lattice structure and reactivity is investigated.
[0052] The metal oxide powder catalyzes the pyrolysis of the carbonaceous gas, resulting in the in-situ nucleation of multi-ring (i.e., "polycyclic") carbon structures on the surface of the metal oxide particles. The lattice nuclei can provide seeds for self-catalyzed lattice growth, as disclosed in PCT / US17 / 17537. If growth continues long enough, the carbon lattice can form a multilayer structure that at least partially covers the surface of the metal oxide particle, which can act as a template and / or catalyst. The metal oxide template can then be extracted from the carbon shell to obtain the templated multilayer structure.
[0053] In experiment A, four carbon samples (A1-A4) were synthesized by MgO template-induced CVD process using the furnace Scheme 1 described above. All gases used in the synthesis were supplied by Praxair. The MgO template was prepared by calcining L-MgCO3 at a temperature of 1050 °C for 2 h, resulting in a powder of polyhedral particles (PH-MgO).
[0054] For sample A1, a mixture of CH4 and Ar was used as the feed gas. A quartz tube was loaded with 300 g of PH-MgO powder. The tube was then closed and rotated at 2.5 RPM. After starting an Ar flow of 500 sccm, the temperature of the furnace was ramped from room temperature to 1050°C over 50 minutes. It was then held at 1050°C for 30 minutes. The Ar gas flow was maintained during heating. Then, a CH4 flow of 160 sccm was started while the Ar flow was maintained for 60 minutes. The CH4 flow was then stopped and the furnace was cooled to room temperature under continuous Ar flow. The MgO was then extracted by acid etching with HCl to obtain a slurry of carbon in an aqueous magnesium chloride (MgCl2) brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (A1-Aq). The water was replaced with acetone by a solvent exchange process to obtain an acetone paste.
[0055] The acetone paste was then evaporated to dryness to form dry carbon powder A1.
[0056] For sample A2, a mixture of CH4 and Ar was used as the feed gas. A quartz tube was filled with 300 g of PH-MgO powder, which was then closed and the tube started to rotate at 2.5 RPM. After starting an Ar flow of 500 sccm, the furnace was heated from room temperature to 1050°C over 50 minutes. It was then held at 1050°C for 30 minutes. The Ar flow was maintained during the entire heating. Next, a CH4 flow of 1920 sccm was started while maintaining the Ar flow. This was continued for 15 minutes. The CH4 flow was then stopped and the furnace was cooled to room temperature while continuing the Ar flow. The MgO was extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in an aqueous MgCl2 brine solution. The carbon was filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (A2-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone / carbon paste. The acetone paste was then evaporated to dryness to form dry carbon powder A2.
[0057] For sample A3, a mixture of C3H6 and Ar was used as the feed gas. A quartz tube was loaded with 300 g of PH-MgO, which was then closed and the tube started to rotate at 2.5 RPM. After starting an Ar flow of 500 sccm, the furnace was heated from room temperature to a set temperature of 750° C. over 30 minutes and maintained at 750° C. for 30 minutes while maintaining the Ar flow. Next, a C3H6 flow of 270 sccm was started without changing the Ar flow. This was continued for 30 minutes. The C3H6 flow was then stopped and the furnace was cooled to room temperature while continuing the Ar flow. The MgO was extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in an aqueous MgCl2 brine solution. The carbon was filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (A3-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone / carbon paste. The acetone paste was then evaporated to dryness to form dry carbon powder A3.
[0058] For sample A4, a mixture of C3H6 and Ar was used as the feed gas. A quartz tube was loaded with 300 g of PH-MgO, which was then closed and rotated at 2.5 RPM. After starting an Ar flow of 500 sccm, the furnace was heated from room temperature to a set temperature of 650° C. over 30 minutes and maintained at 650° C. for 30 minutes while maintaining the Ar flow. Then, a C3H6 flow of 270 sccm was started without changing the Ar flow. This was continued for 60 minutes. The C3H6 flow was then stopped and the furnace was cooled to room temperature while continuing the Ar flow. The MgO was extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in an aqueous MgCl2 brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (A4-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone / carbon paste. The paste was then evaporated to dryness to form dry carbon powder A4.
[0059] Each aqueous paste was then subjected to a series of measurements to evaluate the effect of mild oxidation on the carbon. Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidizing agent. In each reaction, a concentration of 0.5 wt% carbon and approximately 5.3 wt% NaOCl were used, as shown in Table 1 below. [Table 1]
[0060] After the reaction was run for 20 hours, a 24 gram aliquot (containing approximately 0.12 grams of sampled carbon) was collected. The remaining solution was allowed to react for an additional 20 hours (total reaction time 40 hours). The solutions sampled at 20 and 40 hours were filtered, followed by washing the carbon retentate with DI water and resuspending it in 0.2M HCl solution. The acidic solution was stirred for 10 minutes, then filtered and washed with DI water to obtain an aqueous paste of oxidized carbon. A solvent exchange process was then used to replace the water with acetone to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form oxidized carbon powder. Carbon oxidized using this protocol was labeled as "80xBT-20 hr" or "80xBT-40 hr" based on whether it was run for 20 or 40 hours.
[0061] Experiment A - Materials characterization and analysis Carbon yield, defined herein as the weight percent of carbon in the as-synthesized powders of MgO and C, was measured by performing an ash test on the dark gray powders recovered after the CVD process. The yield was measured after CVD turned the originally white MgO powder dark gray, the color change indicating the formation of carbon. By varying the temperature, flow rate, growth time, and hydrocarbon species, similar yields ranging from 1.71% to 2.31% were obtained for each carbon synthesis procedure. SEM images of samples A1-A4 are shown in Figure 5, and TEM images of A1, A3, and A4 are shown in Figure 6. In the TEM images, it can be observed that the lattice fringes of sample A1 are flatter and more aligned than those of A3 and A4. This is due to the nearly hexagonal splines with relatively less out-of-plane deformation due to defects. 2The results show a tiling of the lattice structure. Of the three samples, A4 is the most nonplanar and has the highest concentration of defects throughout the basal planes, which induces out-of-plane deformations that give the sp triangular bonds some tetrahedral character. This distortion should increase the potential energy and chemical reactivity of the lattice. The yields are summarized in Table 2. [Table 2]
[0062] The defect concentration of the carbon before template extraction was analyzed by Raman spectroscopy. The spectra of these samples are shown in Figure 7, and the spectral peak ratios are given in Table 3 below. [Table 3]
[0063] Raman spectroscopy is T / I G (approximate defect concentration) is significantly higher for samples A3 and A4 grown at 750°C and 650°C, respectively, than for samples A1 and A2 grown at 1050°C. This indicates that, all other things being equal, samples grown at higher temperatures (i.e., A1 and A2 grown at 1050°C) have lower defect concentrations (i.e., I T / I G This is consistent with the TEM analysis. Comparing the Raman analysis of A1 and A2, for samples produced at the same temperature (i.e., 1050 °C), the lower gas flow rate leads to a lower defect concentration (i.e., I for sample A1 with lower flow rate). T / I GIt is shown that the rate of self-nucleation (i.e., the nucleation of new carbon lattices by the carbon catalyst) increases with increasing hydrocarbon flow rate. This reduces the average lattice size, increases the density of edge states, and reduces the orders in the Raman spectrum. When filled with hydrocarbon molecules, the rate of lattice edge growth may accelerate to a point where the formation of non-hexagonal rings increases. This may reduce the ordering of the basal planes.
[0064] Carbons synthesized via template-induced CVD often exhibit Raman spectra indicative of high defect concentrations. High defect concentrations can be caused by the high nucleation density that typically occurs with templates. Lattice assemblies formed with many lattice nuclei of hexagonal tiling generally exhibit highly defective spectra due to the high density of edges. Large lattices of non-hexagonal tiling may have defective spectra due to the significant concentration of non-hexagonal rings in the basal planes. For these reasons, the high defect concentrations exhibited by the Raman spectra associated with most samples in experiment A do not independently prove the presence of lattices with non-hexagonal rings. To confirm non-hexagonal lattice tiling, the Raman results can be compared to the results of other characterization methods, such as TGA.
[0065] The TGA of the sodium hypochlorite oxidized samples shown in Figure 8 confirms the level of oxygen moieties in the samples. When exposed to heat under Ar, the oxidized carbon samples exhibit mass loss, primarily due to the evolution of oxygen-containing moieties. The TGA mass loss for each of the oxidized carbon samples at temperatures between 100 °C and 750 °C is shown in Table 4. [Table 4]
[0066] In sample A1, the Raman spectrum indicated a relatively low defect concentration and thus a high degree of hexagonal tiling. Thus, oxidation upon exposure to sodium hypochlorite solution was minimal. As with other graphitic carbon nanostructures, the chemical stability of the hexagonal basal planes and the lack of accessible lattice edges prevented extensive oxidation during the relatively mild oxidation process used to fabricate the sample. In sample A2, the oxidation measured by TGA was slightly greater. This can be attributed to a smaller lattice size distribution and a higher number of accessible edge defects resulting from the self-nucleation of small lattices on the surface of the lattice assembly.
[0067] TEM analysis and Raman spectra were obtained (Table 3I T / I G The TGA data indicate that samples A3 and A4 are significantly more defective than samples A1 and A2 (as evidenced by the higher .DELTA..Oxidation.. The TGA data correspondingly indicate that A3 and A4 also exhibit a higher degree of oxidation (greater mass loss as shown in Table 4). The increased oxidation was surprising given the higher yields of these carbon shells compared to samples A1 and A2 (Table 2). Since the MgO template was essentially identical in each of the four samples (A1-A4), the higher yields of A3 and A4 suggest a thicker multilayer structure with proportionately less surface area exposed to the oxidizing agent. In the absence of intercalation by the oxidizing agent, oxidation occurs only at the surface of the multilayer structure. Thus, a reduction in surface area typically suggests a lower degree of oxidation (i.e., less oxygen per unit mass of structure). Even if the multilayer structures of samples A3 and A4 contain highly reactive lattice structures, no intercalation by sodium hypochlorite solution is presumed, leading to lower oxidation of the aggregate surface.
[0068] The relatively high degree of mass loss of samples A3 and A4 shown in Table 4 indicates that the basal planes of the lattice were oxidized. To verify the oxidation of the basal planes, sample A3 was analyzed by XPS both before oxidation and after 2 and 20 hours of oxidation. Figure 9A shows that the A3 sample before functionalization showed very little oxygen (0.7%), whereas the 2 and 20 hour samples showed 10% and 17% oxygen, respectively. In the absence of intercalation, this suggests that the multilayer lattice assembly is gradually etched from the outside. As the mass of carbon decreases, its proportion of the total mass of carbon and oxygen also decreases. Figure 5A also shows the O / C ratio of all three samples. The O / C ratio of sample A3 80xBT-20 hours is 0.21, which is a typical level for the reduction of GO.
[0069] The XPS concentrations (atomic %) of various oxygen-containing species in the 2-hour and 20-hour samples (A3 80xBT-2 hours and A3 80xBT-20 hours, respectively) are shown in Figure 9B. The data in Figure 9B indicates that oxidation of both the 2-hour and 20-hour samples occurs not only at the edges of the lattice, but also within the basal planes. This is because the XPS results for both the 2-hour and 20-hour samples show significant amounts of epoxide, carbonyl, and hydroxyl moieties, which are indicative of oxidation of the basal planes. A stronger oxidizing agent is generally required to obtain a significant presence of these functional groups on the basal planes of the hexagonal tiling lattice.
[0070] The introduction of non-hexagonal rings into the lattice results in a non-planar surface that does not stack regularly. The pleated regions can increase the interstitial spacing over a range of hundreds of rings. XRD analysis of sample A1 showed a d-spacing of 3.45A, which is typical of a planar turbostratic stacked graphene lattice. In comparison, the d-spacings of samples A3 and A4 were larger at 3.57A and 3.53A, respectively. Although oxygen intercalation typically increases the interstitial d-spacing, the d-spacings of samples A3 and A4 after oxidation are not as large, further suggesting a lack of intercalation. This is further evidenced by SEM analysis of these samples (Figure 10), which confirms that the multilayer lattice assemblies retain the original template geometry, a desirable attribute of template-generated porous carbon that can be degraded if the interlayer spacing within the assemblies is expanded as in graphite oxide structures.
[0071] This process has several other distinct advantages. First, no base wash or chemical reduction steps are required (although they can be incorporated). Unlike the Hummers process, tunable oxidation is easy, and one only needs to set the conditions for the autocatalytic ring formation so that the required defect concentration is obtained and a corresponding amount of oxygen groups are attached to the carbon. Furthermore, the by-product of the reaction is dissolved sodium chloride (NaCl), and the reaction can be continued until all the sodium hypochlorite is consumed and converted, allowing functionalization to make a non-toxic, neutral pH brine for easy disposal. If a different brine is preferred, e.g., lithium chloride brine, a hypochlorite species related to the desired cation can be utilized.
[0072] The results of experiment A show that lattice nuclei can be nucleated in the reactor and that autocatalytic growth can be utilized to grow new lattice domains with a controllable concentration of non-hexagonal rings. One simple way to induce the formation of non-hexagonal rings is to modulate the average temperature associated with the formation of modified carbon lattices. Different hydrocarbon feedstocks can be utilized with different lattice growth rates. In experiment A, a template was utilized, but other embodiments of the process could exclude the use of a template. The functionalized carbon produced in experiment A includes both individual functionalized lattices and multilayer assemblies of functionalized lattices. The controllable level of basal plane functionality obtained with the mild oxidation process indicates increased reactivity of the defective lattice formed. The lack of intercalation indicates that side selective functionalization can be obtained by exposing only one side of the lattice domains, and the increased O:C ratio as a function of time indicates that the oxidation process utilized involves a gradual oxidative etch. This was supported by the amber color of the filtrate after filtering the oxidized carbon. The amber color of the filtrate indicates OD generated by lattice etching.
[0073] Experiment B Experiment B shows the synthesis of templated multilayer lattice assemblies with different functionality hierarchies. In part 1 of experiment B, a multilayer structure is shown that contains an interior unfunctionalized hierarchies and two functionalized surface hierarchies. The distinct lattice characteristics of each hierarchies were obtained by using a three-step template-induced CVD process. In part 2 of experiment B, a multilayer structure is shown that contains one unfunctionalized hierarchies and one functionalized hierarchies. The distinct lattice characteristics of each hierarchies were obtained by using a two-step template-induced CVD process. Unlike the procedure in part 1, where the template was extracted after the completion of the three CVD steps, in the procedure in part 2, the template was extracted between the first and second CVD steps.
[0074] In part 1 of experiment B, a single sample (sample B1) was synthesized via a MgO template-induced CVD process using furnace Scheme 1. The PH-MgO template was generated by calcining L-MgCO3 at 1050 °C for 2 h. A methane / propylene / argon mixture was used as the feed gas. 300 g of PH-MgO was loaded into a quartz tube (100 mm outer diameter) in the heating zone of the furnace. The tube was rotated at a speed of 2.5 RPM during the temperature ramp, growth, and cooling stages. The temperature was ramped from room temperature to 750 °C over 30 min and maintained at 750 °C for 30 min under 500 sccm Ar flow. Then, a C3H6 flow of 270 sccm was started while keeping the Ar flow constant. This was continued for 5 min (CVD "Stage 1"). The C3H6 flow was then stopped and the reactor was heated to 1050°C for 15 minutes and maintained at that temperature for another 30 minutes under an Ar flow of 500 sccm. A CH4 flow of 160 sccm was then started while the Ar flow was kept constant. This was continued for 60 minutes (CVD "phase 2"). The CH4 flow was then stopped and the reactor was cooled to 750°C over 30 minutes and maintained at that temperature for 30 minutes under an Ar flow of 500 sccm. A C3H6 flow of 270 sccm was then started without changing the Ar flow. This was continued for 5 minutes (CVD "phase 3"). The C3H6 flow was then stopped and the reactor was cooled to room temperature while the Ar flow was continued.
[0075] The MgO was extracted by acid etching with HCl to obtain a slurry of carbon in aqueous MgCl2 brine. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (B1-Aq). A solvent exchange process was then used to replace the water with acetone to obtain an acetone / carbon paste. The paste was then evaporated to dryness to form dry carbon powder B1.
[0076] Next, the effect of a mild oxidation reaction on carbon was evaluated using an aqueous paste ("B1-Aq"). Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidant. In each reaction, a concentration of 0.5 wt% carbon and approximately 5.3 wt% NaOCl were used, as shown in Table 5. [Table 5]
[0077] The reaction was carried out for 20 hours after which a 24 gram aliquot (containing approximately 0.12 grams of sample carbon) was collected. The remaining solution was allowed to react for an additional 20 hours (total reaction time 40 hours). The solution sampled at 20 and 40 hours was filtered, followed by washing the carbon retentate with DI water and resuspending it in 0.2M HCl solution. The acidic solution was stirred for 10 minutes, then filtered and washed with DI water to obtain an aqueous paste of oxidized carbon. A solvent exchange process was then used to replace the water with acetone to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form oxidized carbon powder. Carbon oxidized using this protocol was labeled as "B1 80xBT-20 hours" or "B1 80xBT-40 hours" based on whether it was run for 20 or 40 hours.
[0078] In part 2 of experiment B, to demonstrate a two-step CVD process, in the first step, sample B2 was synthesized via a MgO template-induced CVD process using furnace scheme 1, followed by removal of the template. Sample B2 was used in the second step of a self-catalytic lattice growth CVD process to synthesize sample B3 using furnace scheme 3. All process gases were supplied by Praxair.
[0079] For sample B2, a mixture of CH4 and Ar was used as the feed gas. A quartz tube was loaded with 500 g of Elastomag 170 (EL-170) grade MgO. It was then closed and rotated at 10 RPM. After starting an Ar flow of 500 sccm, the temperature of the furnace was ramped from room temperature to 1050°C over 50 minutes. It was then held at 1050°C for 30 minutes. The Ar gas flow was maintained during both the ramp and steady state. Next, a CH4 flow of 1200 sccm was started without changing the Ar flow. This was continued for 45 minutes. The CH4 flow was then stopped and the furnace was cooled to room temperature while the Ar flow continued. The MgO was extracted by acid etching with hydrochloric acid (HCl) under excess acidic conditions to obtain a slurry of carbon in an aqueous magnesium chloride (MgCl2) brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (B2-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste, which was then evaporated to dryness to form dry carbon powder B2.
[0080] For sample B3, a mixture of C3H6 and Ar was used as the feed gas and a quartz tube was used for the experiment. After starting the Ar flow of 4700 sccm, the furnace was heated from room temperature to the set temperature of 750 °C over 20 minutes and maintained at 750 °C for 30 minutes while maintaining the Ar flow. An alumina boat containing 0.302 g of B2 dried powder was then placed in the cold zone of the tube for 10 minutes and the air was removed under high argon flow. The boat was then slid into the heated zone and held there for 5 minutes to allow the temperature to equilibrate. Next, a C3H6 flow of 750 sccm was started without changing the Ar flow. This was continued for 23 minutes. The C3H6 flow was then stopped and the boat was left in the heated zone for 5 minutes. The boat was then slid into the cold zone and held there for 10 minutes to reduce the temperature under a high flow argon blanket. Sample B3 was weighed after cooling to room temperature.
[0081] Samples B2 and B3 were then oxidized using sodium hypochlorite solution (about 13 wt% NaOCl). In each reaction, a carbon concentration of 0.6 wt% and a NaOCl concentration of about 3.1 wt% were used, as shown in Table 6 below. [Table 6]
[0082] The reaction was allowed to proceed for 30 minutes. After this, the contents were filtered to obtain a carbon retentate, which was washed with DI water and resuspended in 0.2 M HCl solution. The acidic solution was stirred for 10 minutes. The acidic solution was subsequently filtered and washed with DI water to obtain an aqueous paste of carbon oxide. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was evaporated to dryness at 60° C. to form a carbon oxide powder. The carbon oxidized using this protocol was designated B2-Ox and B3-Ox.
[0083] Experiment B - Materials characterization and analysis The carbon yield (after CVD turned the MgO powder dark grey due to carbon deposition) was measured by ash test and was 2.25%, which was similar to the carbon sample from experiment A. Table 7 below summarizes the process parameters and yields. [Table 7]
[0084] Prior to template extraction, the carbon was analyzed for defects using Raman spectroscopy. The spectrum of sample B1 is shown in Figure 11, and the spectral peak ratios are shown in Table 8 below. [Table 8]
[0085] The Raman spectrum of sample B1 shows an intermediate level of two-dimensional order (i.e., I between A1 and A3). 2D / I G ) and defects (i.e., I between A1 and A3 T / IG ) in the hybrid layer. The hybrid Raman results indicate the presence of three layers, two of which are similar to A1 and one to A3. The modified carbon lattice in the layer grown at 1050□ is relatively hexagonal, as in sample A1, while the modified carbon lattice in the layer grown at 750□ is significantly more defective, as in sample A3. SEM images of samples A1, A3 and B1 are shown in Figure 12, which indicates the hybrid nature of sample B1, which not only retains the curved shape of the template well (as in A3), but also has few broken junctions (as in A1) since the entire particle is coated. TEM images of samples A1, A3 and B1 in Figure 13 show the cross-section or wall thickness of the multilayer structure.
[0086] The concentric development of multilayer structures during template-guided growth, in combination with adjustments to the reactor settings and the accompanying growth conditions, allows the formation of different layers. The surface layers are the first and last layers synthesized on the template, corresponding to stages 1 and 3 of the CVD process, respectively. The inner layers formed during CVD stage 2 are less defective and more chemically inert, due to the presence of carbon grown at higher temperatures.
[0087] The TGA of the sodium hypochlorite oxidized samples shown in Figure 14 provides more information. When exposed to heat under Ar, the oxidized carbon samples exhibited mass loss due to removal of oxygen moieties. The TGA mass loss of each oxidized carbon sample at temperatures between 100 °C and 750 °C is shown in Table 9. [Table 9]
[0088] Comparison of the Raman and mass loss data between samples B1, A1, and A3 provides further insight into the structure of sample B1. For sample A1, the Raman spectrum shows a relatively high degree of order, corresponding to a high degree of hexagonal tiling. For sample A3, the Raman spectrum showed significantly more defects. The yield of sample A1 was 1.7% (Table 2), and the exact growth conditions were used to produce the inner core of sample B1, which had a yield of 2.25% (Table 7). Thus, sample B1 is composed primarily of a sample A1 type lattice, with a relatively thin surface hierarchy of sample A3 type lattice. TGA confirms that the mass loss (proxy for oxidation level) of sample B1 (15%) is more indicative of a sample A1 (12%) type lattice structure, with slightly higher oxidation, possibly from the presence of a defective surface hierarchy (see Table 9).
[0089] The growth conditions for B2 produced a relatively high degree of hexagonal tiling based on the observed Raman spectrum showing a 2D peak. The conditions selected for B3 were such that a thin layer of defective carbon (~14% of the total mass) grows over B2, but also produces a dramatic change in hydrophilicity. Thus, sample B3 is a hierarchical multilayer structure consisting of a reactive "skin" formed on top of an inert layer. This structure allows for hierarchically selective functionalization of the surface to more effectively disperse hydrophobic carbon nanoparticles.
[0090] Table 10, shown below, summarizes the mass increase of B3 based on the combination of parameters used to grow B2. [Table 10]
[0091] Unlike experiment A, where oxidation was shown to gradually etch the multilayer structure and generate OD over an extended period of time, experiment B used a much shorter oxidation time with the goal of limiting etching. Reducing the oxidation time to approximately 30 min oxidized the carbon surface, increasing the hydrophilicity of the carbon (as shown in Figure 15), and eliminating observable OD generation.
[0092] Experiment C Experiment C illustrates the role that controllable chemical reactivity plays in attaching other molecules to nanocarbons. It builds on the results of experiments A and B and demonstrates side- and hierarchically selective functionalization of modified lattices and multilayer lattice assemblies. It also demonstrates an embodiment of a lattice modification process in which lattice nuclei are transported through the reaction zone simultaneously with the growth of new lattice domains.
[0093] In experiment C, one carbon sample (CO) was synthesized via an MgO template-induced CVD process using the furnace configuration in Scheme 2 in two steps (described below). The MgO template was fabricated by calcining Elastomag-170 (EL-170) at a temperature of 1050 °C for 1 h, resulting in a powder of ovoid particles (Ov-MgO).
[0094] In step 1, the 60 mm OD quartz tube and the furnace were both tilted at a 0.6 degree incline. The tube was rotated at approximately 6 RPM. A mixture of C3H6 and Ar was used as the feed gas. 2718 g of Ov-MgO was loaded into the hopper, which was then sealed and maintained under a slight positive pressure using 4720 sccm argon flow to prevent air from entering the system.
[0095] After starting a second Ar flow at 4720 sccm in the quartz tube, the furnace was heated from room temperature to two set temperatures, 850 °C in zone 1 (upstream) and 750 °C in zone 2 (downstream), over 30 min. This reactor configuration, when established and maintained throughout the course of the CVD process, creates multiple gradients through which carbon lattice nuclei and new lattice domains are transported simultaneously with autocatalytic carbon growth. The first gradient was the increase from the temperature at which in-situ lattice nucleation occurs to about 850 °C. The second temperature gradient through which the growing carbon lattice traveled was the cool down from the temperature in zone 1 to the temperature in zone 2 (i.e., from 850 °C to 750 °C). The third temperature gradient through which the carbon lattice traveled was the cool down from the temperature in zone 2 to the temperature at which autocatalytic lattice growth terminates. Additionally, the use of a CVD furnace according to Scheme 2 also creates other parameter gradients, such as the partial pressure of the carbonaceous feed gas and the various hydrocarbon and hydrogen decomposition products resulting from deposition.
[0096] Once the furnace zones reached the set temperatures, the system was maintained at those temperatures for 30 minutes under Ar flow. The MgO powder feed system was started with the auger screw set at approximately 7%, corresponding to a weight feed rate of approximately 8 g / min of MgO powder. The depth was set at a low setting to allow a shallow bed to move through the feed tube while the paddle agitation was set at 10%, ensuring that the powder did not pack or densify. The powder had a residence time of approximately 14 minutes in the furnace heating zone. It took approximately 20 minutes (from the start of the initial material feed) to achieve a steady-state bed (i.e., a bed where the mass entering the heating zone and the mass exiting the heating zone are approximately the same). After a steady-state bed was reached, a C3H6 flow of 250 sccm was started without changing the Ar flow. Powder exiting the tube during the first 25 minutes (from the start of the hydrocarbon gas flow) was discarded. Collection began at the 25 minute mark (from the start of the hydrocarbon gas flow). The reaction took about 4 hours and 45 minutes to complete, yielding 2203 g of product.
[0097] In step 2, the quartz tube (60 mm outer diameter) and the furnace were both tilted at a 0.6 degree incline. Again, the tube was rotated at approximately 6 RPM. A mixture of C3H6 and Ar was used as the feed gas. 2181 g of the powder recovered in step 1 was loaded into the hopper, which was then sealed and maintained under a slight positive pressure using an Argon flow of 4720 sccm to prevent air from entering the system. After starting a second Ar flow at 4720 sccm in the quartz tube, the furnace was heated from room temperature to the set temperatures of 750°C (Zone 1-upstream) and 750°C (Zone 2-downstream) over 30 minutes. Thus, the furnace had two temperature gradients (up to and down from 750°C).
[0098] Once the furnace zones reached the set temperature, the system was held for 30 minutes to equilibrate while maintaining the Ar flow. The powder feed system was started with the auger screw set at approximately 7%, corresponding to a weight feed rate of approximately 8 g / min of MgO powder. The depth was set at a low setting to allow a shallow bed to move through the feed tube while the paddle agitation was set at 10%, ensuring that the powder did not pack or densify. The powder had a residence time of 15 minutes in the heated zone. It took approximately 20 minutes (from the start of the initial material feed) to achieve a steady-state bed (i.e., a bed where the mass entering the heated zone is approximately the same as the mass exiting the heated zone). After the steady-state bed was reached, a C3H6 flow of 500 sccm was started without changing the Ar flow. Powder exiting the tube during the first 25 minutes (from the start of the hydrocarbon gas flow) was discarded. Collection began at the 25 minute mark (from the start of the hydrocarbon gas flow). The reaction took approximately 4 hours and 50 minutes to complete, yielding 1925 g of product.
[0099] Due to the formation of heavier molecular weight hydrocarbon condensates in the downstream portion of the quartz tube, the powder from the second CVD step was heated at 300 °C overnight to remove volatile materials deposited during synthesis. The MgO was then extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in aqueous MgCl2 brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (CO-Aq) with a carbon content of 45.10 g. A portion of this aqueous paste (50 mg of carbon) was used to generate an isopropyl alcohol paste (CO-IPA) using a solvent exchange process.
[0100] A portion of the remaining aqueous paste was converted to the oxide form (CO-Ox) to evaluate its effect in epoxy formulations. Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidizer. Carbon at a concentration of 0.74 wt% and NaOCl at a concentration of approximately 5.5 wt% were used, as shown in Table 11 below. [Table 11]
[0101] The reaction was carried out for 120 minutes and upon completion the solution was filtered. The carbon retentate was washed with DI water and resuspended in 0.2 M HCl solution. The acidic solution was stirred for 10 minutes and then filtered and washed with DI water to obtain an aqueous paste of carbon oxide (CO-Ox-Aq).
[0102] CO-Ox was reacted with octyltriethoxysilane as shown in Table 12. A portion of the CO-Ox-Aq batch was mixed with DI water and sonicated using a Branson 8510DTH bath sonicator to produce a suspension of CO-Ox in water. Octyltriethoxysilane (OTES) was dissolved in IPA and added to the CO-Ox aqueous solution, and the mixture was stirred on a magnetic stir plate at room temperature for 1 hour. It was then filtered and washed with IPA to remove excess OTES. The filtered residue was heated at 110° C. for 2 hours to complete the reaction. After the heating step, the residue was subsequently thoroughly rinsed with IPA for a second time to wash off unreacted OTES from the carbon surface, and the product was dried at 110° C. for 2 hours and named CO-Ox-OTES. These carbons, namely CO, CO-Ox and CO-Ox-OTES, were characterized using their wetting behavior in water and TGA. [Table 12]
[0103] Experiment C - Materials characterization and analysis TGA analysis of samples CO and CO-Ox was performed to confirm the oxygen functionalization of sample CO-Ox. As shown in Table 13, when exposed to a heating rate of 20 °C / min from room temperature to 750 °C under argon flow, the mass loss number from 100 to 750 °C of CO-Ox was about 5% in contrast to the negligible mass loss of sample CO. [Table 13]
[0104] As detailed in the XPS results in Experiment A, two of the basal plane functional groups after oxidation include a hydroxyl group and a carboxyl group, both of which have -OH moieties. A wide range of other useful functional groups, such as glycidyl (epoxy), amine, vinyl, and aliphatic chains, can be added to these groups via silane coupling reactions. The addition of other functional groups will be useful for incorporating these oxidized carbon structures into various polymer systems in a manner that makes them compatible with the polymer matrix.
[0105] In this experiment, octyltriethoxysilane (OTES) was chosen as the silane. OTES has an aliphatic chain attached to the silicon atom. A schematic diagram of the silane functionalization of hydroxyl groups on a carbon surface is shown in Figure 16. Step 1 involves hydrolyzing the silane and "activating" it to form silanols, a process that is carried out in the presence of water. Step 2 involves the formation of hydrogen bonds between silanols and hydroxyl groups on the CO-Ox surface, which is carried out under stirring at room temperature. Step 3 involves the conversion of the hydrogen bonds to permanent covalent bonds by a condensation reaction in which an H2O molecule is removed, which is typically carried out under heating at about 110 °C for 1 h.
[0106] Functionalization with silane was evident as the wetting behavior of sample CO-Ox changed dramatically after silane treatment, with the hydrophilic carbon oxide surface becoming hydrophobic. As shown in Figure 17, the CO-Ox sample is hydrophilic and disperses instantly in water with minimal agitation, but forms a stable suspension upon agitation. However, CO-Ox-OTES after silane treatment is hydrophobic and does not disperse even with agitation. This hydrophilic to hydrophobic transformation is due to the long hydrophobic aliphatic chains that contain part of the silane molecule.
[0107] The TGA curves in Figure 18 for samples CO-Ox, CO-Ox-OTES run in argon show that the hydrophilic to hydrophobic transition is not the removal of oxygen functional groups (i.e., conversion to reduced graphene oxide). Higher mass loss is higher for sample CO-Ox-OTES, indicating new chemistry on the surface that converted the hydrophilic CO-Ox to hydrophobic CO-Ox-OTES. The TGA profile used was a 20°C / min ramp from room temperature to 800°C under 100 mL / min air flow. Also in Figure 18, there is a significant mass loss event starting at 425°C, which could be the removal of long chain aliphatic groups attached to silicon.
[0108] Experiment C shows that initial oxidative functionalization of modified carbon lattices and aggregates can serve as a platform for forming various functionalities. To the extent that the carbon feedstock can be selectively functionalized in the initial functionalization step, further functionalization can also be selectively applied based on the initial functionalization. Furthermore, experiment C illustrates a CVD process in which lattice nuclei and new lattice regions are transported through one or more parameter gradients in the reactor. This is distinguished herein from CVD processes such as those utilized in experiments A and B, in which each CVD step is performed at constant conditions. One of the capabilities enabled by parameter gradients is the ability to obtain a continuous gradient of lattice features, and the functionality associated with those features after functionalization. Parameter gradients allow for a more finely tuned and dynamic CVD procedure than can actually be modified through multiple CVD steps. Furthermore, by transporting the growing lattice through parameter gradients simultaneously with growth, a wide range of lattice properties can be engineered into the lattice (e.g., growing completely amorphous new lattice regions from hexagonal lattice nuclei) without the need for sudden, stepwise re-modification of the lattice tiling. Such sudden changes in lattice structure may not be ideal for certain properties, such as mechanical stress transfer and strength.
[0109] Test D Experiment D was performed to generally demonstrate that modified carbon lattices can be synthesized on carbon lattice nuclei without the need for non-carbon catalysts, templates, or supports. Furthermore, experiment D specifically demonstrates that carbon black lattice nuclei can be utilized as an inexpensive CVD feedstock, and that new lattice domains autocatalytically grown with various carbon feedstocks can also be tuned for reactivity and functionality. Finally, experiment D illustrates a process embodiment in which pre-nucleated carbon lattice nuclei are introduced into the reactor, as opposed to a process embodiment in which both nucleation and CVD growth are performed in-situ.
[0110] In experiment D, two carbon samples (D1 and D2) were synthesized by autocatalytic lattice growth using a typical conductive grade carbon black (D0) as the substrate. All process gases were supplied by Praxair. Conductive grade carbon black VULCAN XC72R was supplied by Cabot. In experiment D, D1 and D2 were synthesized by autocatalytic lattice growth using the furnace configuration in Scheme 3.
[0111] For sample D1, a mixture of C3H6 and Ar was used as the feed gas and a quartz tube was used for the experiment. After starting the Ar flow of 4700 sccm, the furnace was heated from room temperature to the set temperature of 750°C over 20 minutes and maintained at 750°C for 30 minutes while maintaining the Ar flow. An alumina boat containing 1 g of carbon black (D0) was then placed in the cold zone of the tube for 10 minutes to remove the air under high argon flow. The boat was then slid into the heated zone and maintained there for 5 minutes to allow the temperature to equilibrate. Next, a C3H6 flow of 750 sccm was started without changing the Ar flow. This was continued for 60 minutes. The C3H6 flow was then stopped and the boat was left in the heated zone for 5 minutes. The boat was then slid into the cold zone and maintained there for 10 minutes to reduce the temperature under a high flow argon blanket. Sample D1 was weighed after cooling to room temperature.
[0112] For sample D1, a mixture of CH4 and Ar was used as the feed gas and a quartz tube was used for the experiment. After starting the Ar flow of 4700 sccm, the furnace was heated from room temperature to the set temperature of 1050°C over 50 minutes and maintained at 1050°C for 30 minutes while maintaining the Ar flow. An alumina boat containing 1 g of carbon black (D0) was then placed in the cold zone of the tube for 10 minutes to remove the air under high argon flow. The boat was slid into the heated zone and maintained there for 5 minutes to allow the temperature to equilibrate. Then, a CH4 flow of 130 sccm was started without changing the Ar flow. This was continued for 30 minutes. The CH4 flow was then stopped and the boat was left in the heated zone for 5 minutes. The boat was then slid into the cold zone and maintained there for 10 minutes to reduce the temperature under high flow argon. Sample D1 was weighed after cooling to room temperature.
[0113] Table 14 summarizes the mass gain resulting from the CVD procedure for experiment D on carbon black seeds and also outlines the relevant process parameters. [Table 14]
[0114] Samples D1 and D2 were then oxidized using mild oxidation with sodium hypochlorite solution (about 13 wt% NaOCl). In each reaction, a carbon concentration of 0.4 wt% and a NaOCl concentration of about 4.2 wt% were used, as shown in Table 15 below. [Table 15]
[0115] The reaction was carried out for a total of 20 hours before filtering, followed by washing the carbon retentate with DI water and resuspending it in 0.2M HCl solution. The acidic solution was stirred for 10 minutes, then filtered and washed with DI water to obtain an aqueous paste of carbon oxide. A solvent exchange process was then used to replace the water with acetone to obtain an acetone paste. The paste was then evaporated to dryness at 60□ to form carbon oxide powder. Carbon oxidized using this protocol was designated D1-Ox and D2-Ox.
[0116] Experiment D - Materials characterization and analysis SEM images of samples D0, D1, and D2 are shown in Figure 19. The appearance of the particles of samples D2 and D0 is very similar, indicating conformal carbon growth. However, the particles of D1 appear to have rough carbon surfaces, possibly due to tangential or non-conformal growth. Such growth indicates a higher degree of hexagonal tiling, forming planar lattice regions with less freedom to accommodate complex surfaces.
[0117] The TGA curves of samples D0, D1, and D2 (Figure 20A) show the different thermal properties of the new lattice regions grown on DO. For sample D1, the onset of mass loss associated with carbon combustion starts at a lower temperature than D0. For sample D2, the onset is higher. This is consistent with D1 having a non-hexagonal lattice, while the more hexagonal lattice arrangement of D2 provides for higher thermal stability. The post-oxidation TGA curves of D1-Ox and D2-Ox are shown in Figure 20B. Again, different behavior between the samples can be observed, resulting in a complex thermal event. The sharp peak seen for D1-Ox is characteristic of the rapid combustion of highly oxidized carbon, while the slower combustion of D2-Ox is characteristic of less oxidized carbon.
[0118] Experiment E Experiment E demonstrates the ability to obtain group-selective functionalization and oxidation with a variety of oxidizing agents, as well as oxidation involving combinations of oxidizing agents and acids. Experiment E also demonstrates the ability to attach functional groups between the lattice layers of a multilayer lattice assembly. Experiment E further demonstrates the ability to utilize base washes or acidification treatments to modify the attached oxygen groups. Finally, Experiment E demonstrates the ability to attach non-oxygen atoms, such as sulfur or nitrogen, to the modified carbon lattice.
[0119] Three alternative oxidation protocols were tested with autocatalytically grown carbon. The first alternative oxidation protocol was a simple variation of the sodium hypochlorite treatment protocol in which the treatment was carried out in the low pH (~4) region. The second and third protocols used solutions of sulfuric acid (H2SO4) along with either hydrogen peroxide (H2O2) and ammonium persulfate ((NH4)2S2O8), respectively, to create stronger oxidizing solutions for carbon oxidation.
[0120] Similar to the carbon used in experiment A, three carbon samples (E0, E1 and E2) were synthesized by MgO template-induced CVD process using furnace Scheme 1 above. All gases used in the synthesis were supplied by Praxair. The MgO template was prepared by calcining L-MgCO3 at a temperature of 1050°C for 2 hours to obtain a powder of polyhedral particles (PH-MgO).
[0121] For sample E0, a mixture of CH4 and Ar was used as the feed gas. A quartz tube was loaded with 300 g of PH-MgO powder. The tube was then closed and rotated at 2.5 RPM. After starting an Ar flow of 500 sccm, the temperature of the furnace was ramped from room temperature to 1050°C over 50 minutes. It was then held at 1050°C for 30 minutes. The Ar gas flow was maintained during heating. Then, a CH4 flow of 160 sccm was started while the Ar flow was maintained for 60 minutes. The CH4 flow was then stopped and the furnace was cooled to room temperature under continuous Ar flow. The MgO was then extracted by acid etching with HCl to obtain a slurry of carbon in an aqueous magnesium chloride (MgCl2) brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (E0-Aq). The water was replaced with acetone by a solvent exchange process to obtain an acetone paste.
[0122] The acetone paste was then evaporated to dryness to form dry carbon powder E0.
[0123] For sample E1, a mixture of C3H6 and Ar was used as the feed gas. A quartz tube was loaded with 300 g of PH-MgO, which was then closed and the tube started to rotate at 2.5 RPM. After starting an Ar flow of 500 sccm, the furnace was heated from room temperature to a set temperature of 750° C. over 30 minutes and maintained at 750° C. for 30 minutes while maintaining the Ar flow. Next, a C3H6 flow of 270 sccm was started without changing the Ar flow. This was continued for 30 minutes. The C3H6 flow was then stopped and the furnace was cooled to room temperature while continuing the Ar flow. The MgO was extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in an aqueous MgCl2 brine solution. The carbon was filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (E1-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone / carbon paste. The acetone paste was then evaporated to dryness to form a dry carbon powder, E1.
[0124] For sample E2, a mixture of C3H6 and Ar was used as the feed gas. 300 g of PH-MgO was placed in a quartz tube, which was then closed and rotated at 2.5 RPM. After starting an Ar flow of 500 sccm, the furnace was heated from room temperature to a set temperature of 650°C over 30 minutes and maintained at 650°C for 30 minutes while maintaining the Ar flow. Next, a C3H6 flow of 270 sccm was started without changing the Ar flow. This was continued for 60 minutes. The C3H6 flow was then stopped and the furnace was cooled to room temperature while continuing the Ar flow. The MgO was extracted by acid etching with HCl under excess acidic conditions to obtain a slurry of carbon in an aqueous MgCl2 brine solution. The carbon was then filtered from the brine, rinsed three times with deionized water, and collected as an aqueous paste (E2-Aq). The water was then replaced with acetone using a solvent exchange process to obtain an acetone / carbon paste. The paste was then evaporated to dryness to form dry carbon powder E2.
[0125] The first oxidation protocol evaluated an acidic form of sodium hypochlorite treatment. Carbon oxides produced using this protocol were in three forms: acid bleach-control, acid bleach-base wash, and acid bleach-base wash followed by acidification.
[0126] The "control" variation was subjected only to the acidic bleaching protocol as described herein. Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidant and the pH was adjusted using 2M HCl. A concentration of 0.29 wt% carbon was used in the reaction, as shown in Table 16 below. [Table 16]
[0127] The reactions were carried out for 20 hours at the end of which they were filtered and the carbon retentate was subsequently washed with DI water to obtain an aqueous paste of carbon oxide. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form a carbon oxide powder. The carbon oxidized using this protocol was labeled "E2 40xABT-20 hr control."
[0128] A variation of the "acid bleach-base wash" was subjected to an acid bleach protocol followed by a base wash process as described here. Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidant and 2M HCl was used to adjust the pH of the reaction. 6M NaOH was used as the base wash. Carbon was used at a concentration of 0.29 wt% as shown in Table 17 below. [Table 17]
[0129] The reaction was run for 20 hours at the end of which it was filtered followed by washing the carbon retentate with DI water. The carbon retentate was resuspended in 10 g of 6M NaOH solution for the base wash step, which included 30 minutes of magnetic stirring followed by 30 minutes of bath sonication. This highly basic solution was diluted with 90 g of water, then filtered and washed with DI water to obtain an aqueous paste of carbon oxide. A solvent exchange process was then used to replace the water with acetone to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form a carbon oxide powder. Carbon oxidized using this protocol was labeled as "E2 40xABT-20 hr BW".
[0130] A variation of the "Acid bleach - Base wash followed by acidification" was subjected to an acid bleach protocol, followed by a base wash process, followed by an acidification step, as described here. Sodium hypochlorite solution (approximately 13 wt% NaOCl) was selected as the oxidant, and 2M HCl was used to adjust the pH of the reaction. 6M NaOH was used as the base wash, and after the base wash, concentrated HCl was used to acidify the solution. Carbon was used at a concentration of 0.29 wt%, as shown in Table 18 below. [Table 18]
[0131] The reaction was run for 20 hours at the end of which it was filtered followed by washing the carbon retentate with DI water. The carbon retentate was resuspended in 10 g of 6M NaOH solution for the base wash step. The base wash step included 30 minutes of magnetic stirring followed by 30 minutes of bath sonication. This highly basic solution was diluted with 90 g of water, then filtered and washed with DI water to obtain an aqueous paste of carbon oxide. The carbon retentate was resuspended in 10 g of DI water and acidified using concentrated HCl until the pH was less than 2 for the acidification step. The acidification step included 30 minutes of magnetic stirring followed by 30 minutes of bath sonication. This highly acidic solution was diluted with 90 g of water, then filtered and washed with DI water to obtain an aqueous paste of carbon oxide. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form a carbon oxide powder. The carbon oxidized using this protocol was labeled as “E2 40xABT-20hr BW-RA”.
[0132] In the second alternative oxidation protocol, concentrated sulfuric acid (more commonly referred to as piranha solution) containing hydrogen peroxide (H2O2) was used as the oxidizing medium to oxidize carbons E0, E1, and E2.
[0133] Carbons E0, E1 and E2 were used as dry powders and subjected to the piranha treatment as shown in Table 19 below. The piranha solution was a mixture of concentrated sulfuric acid and 30 wt% hydrogen peroxide in a weight ratio of 7:1. The carbon was added to the concentrated sulfuric acid and magnetically stirred for 10 minutes, after which the carbon-acid solution was placed in an ice bath and cold hydrogen peroxide was added dropwise over 5 minutes. The piranha solution containing the carbon was magnetically stirred at room temperature for 24 hours. [Table 19]
[0134] The reaction was carried out for 24 hours, at the end of which it was stopped by slowly adding the carbon-piranha solution to excess water (100 mL) without a significant exotherm. This was followed by filtration and washing of the carbon retentate with DI water. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form the oxidized carbon powder. The carbon oxidized using this protocol was labeled as "E0 PrT 24 hr", "E1 PrT 24 hr" and "E2 PrT 24 hr".
[0135] Samples E1 PrT 24h and E2 PrT 24h were subjected to a base washing protocol using 6M NaOH solution to generate E1 PrT 24h BW and E2 PrT 24h BW. The complete procedure for this synthesis is shown below.
[0136] Carbons E1 and E2 were used as dry powders and subjected to the piranha treatment as described in Table 19. The piranha solution was a mixture of concentrated sulfuric acid and 30 wt% hydrogen peroxide in a weight ratio of 7:1. The carbon was added to the concentrated sulfuric acid and magnetically stirred for 10 minutes, after which the carbon-acid solution was placed in an ice bath and cold hydrogen peroxide was added dropwise over 5 minutes. The piranha solution containing the carbon was magnetically stirred at room temperature for 24 hours.
[0137] The reaction was run for 24 hours, at the end of which it was stopped by slowly adding the carbon-piranha solution to excess water (100 mL) without a significant exotherm. This was followed by filtration and washing of the carbon retentate with DI water. The carbon retentate was resuspended in 10 g of 6M NaOH solution for a base wash step, which included 30 minutes of magnetic stirring followed by 30 minutes of bath sonication. This highly basic solution was diluted with 90 g of water, then filtered and washed with DI water to obtain an aqueous paste of carbon oxide. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form a carbon oxide powder. Carbon oxidized using this protocol was labeled as “E1 PrT 24 hr BW” and “E2 PrT 24 hr BW”.
[0138] In a third alternative oxidation protocol, referred to here as the APS treatment, concentrated sulfuric acid containing the oxidant ammonium persulfate ((NH4)2S2O8) was used as the oxidation medium to oxidize carbons E0 and E2.
[0139] Carbons E0 and E2 were used as dry powders and subjected to APS treatment as shown in Table 20 below. The APS solution was a 10:1 mixture by weight of concentrated sulfuric acid and ammonium persulfate. The carbon was added to the concentrated sulfuric acid and magnetically stirred for 10 minutes, after which the ammonium persulfate was added slowly over 5 minutes while the carbon-acid solution was placed in an ice bath. The carbon-containing APS solution was magnetically stirred at room temperature for 60 hours. [Table 20]
[0140] The reaction was carried out for 60 hours, at the end of which it was stopped by slowly adding the carbon-APS solution to excess water (100 mL) without a significant exotherm. This was followed by filtration and washing of the carbon retentate with DI water. The water was then replaced with acetone using a solvent exchange process to obtain an acetone paste. The paste was then evaporated to dryness at 60° C. to form an oxidized carbon powder. Carbon oxidized using this protocol was labeled "E0 APS 60 hr" and "E2 APS 60 hr."
[0141] Experiment E - Materials characterization and analysis Three alternative oxidation protocols were tested, demonstrating that all three were capable of oxidizing autocatalytically grown carbon to varying degrees and with varying degrees of group selectivity.
[0142] The first alternative oxidation protocol was a simple variation of the NaOCl treatment protocol carried out in the low pH (approximately 4) region. It is known that the active oxidizing species in hypochlorite solutions depend on the pH region, with the amount of undissociated hypochlorous acid (HOCl) being highest at approximately pH 4, and above pH 7 only hypochlorite (OCl) ions being present. This treatment protocol was used to compare the oxidation properties of the bleach in two different regions. It was observed that the degree of group selectivity increased with the lower pH region oxidation protocol, as evident from the TGA curves. To understand the phenomenon of selectivity of the groups produced, experiments involving sequential base washing and acidification were carried out, as these steps preferentially induce the transformation of some oxygen functional groups present. [Table 21]
[0143] As shown in Table 21 and Figure 21A, sample E2 40xABT-20hr Control has the highest percentage of mass loss between 100 °C and 750 °C (24.3%), which decreases to about 18-19% upon base washing for both E2 40xABT-20hr BW and E2 40xABT-20hr BW-RA samples. This drop is attributed to the removal of OD present on the carbon surface. It is important to note that even after removing the OD, the percentage of mass loss is still about 18%, of which 2-3% is attributed to water. [Table 22]
[0144] Based on the TEM images (Figure 6), it can be seen that E2 type carbon has cell walls containing approximately 10-15 layers. Of these layers, only the outermost layer of the wall is oxidized on the outside. There is no oxidation in the interstitials within the walls, including inside the outermost layer of the wall, as evidenced by the slight change in interlayer d-spacing after oxidation (as confirmed by XRD analysis of wall thickness measurements and TEM analysis). If we assume a conservative model in which the average number of layers in the walls is 10, and only 2 of the 10 layers are oxidized, then all of the oxygen present in the sample is present in 2 of the 10 layers, or one-fifth of the layers of each particle. To determine the true C:O ratio of only the oxidized layers, the total C:O ratio of the sample is divided by 5, since oxygen is only present in one-fifth of the layers. XPS data for samples E2 40xABT-20hr BW and E2 40xABT-20hr BW-RA (Table 22) reveal that the total oxygen content is between 14.9% and 16.0%, corresponding to total sample C:O ratios of 5.50 and 5.20, respectively. The true C:O ratios of the oxide layers (OD desorbed by base washing) are 1.04-1.1, which is dramatically lower than the typical base-washed graphene oxide C:O ratio values of 4-7.
[0145] Furthermore, while the oxygen groups on graphene oxide are divided evenly between each side, in experiment E, all lattice-bound oxygen groups are attributable only to the respective outsides of the oxidized lattice. Thus, for a given C:O ratio on a lattice where only one side is oxidized, the functional group density on the oxidized side is approximately twice the functional group density on the oxidized side of a lattice where both sides are oxidized and have the same C:O ratio. This suggests that, in combination with the surface-specific C:O ratio of the lattice-modified oxidized carbon, one can obtain a much higher functional group density on its surface compared to conventional oxidized nanocarbons such as GO.
[0146] The ability to add dramatically more oxygen onto the surface of carbon nanoparticles is a major advantage of the defect-induced oxidation process, which proves extremely useful in forming tailored interfaces between carbon nanoparticles and any system to which they are added.
[0147] The second and third protocols used a concentrated sulfuric acid (H2SO4) medium with the addition of oxidizers such as hydrogen peroxide-H2O2 (i.e. piranha solution) and ammonium persulfate-(NH4)2S2O8, respectively. Concentrated sulfuric acid in combination with an oxidizer has been shown to intercalate and bond interlayer oxygen groups to graphite, and this phenomenon was the rationale behind the second and third alternative treatment protocols.
[0148] The Raman data for samples E0, E1, E2 are shown in Table 23. Note that samples E0, E1 and E2 are of the same carbon type as those produced in experiment A (designated A1, A3 and A4, respectively). [Table 23]
[0149] Similar to A1, sample E0 is a high temperature grown carbon and has a relatively high I as seen in the Raman data in Table 23. 2D / I G ratio, which indicates a higher degree of two-dimensional order than the other samples, and I T / I GThe peak ratio is relatively low, indicating a low defect density. Samples E1 and E2 are low temperature grown carbons, and both have I 2D / I G The ratio is low (E2 is the lowest), which indicates low two-dimensional order, or I T / I G is high, indicating a high defect density.
[0150] After piranha treatment, samples E0, E1, and E2 had mass losses (100-750 °C) of 6%, 14.2%, and 14.9%, respectively, as can be seen in Table 24 and Figure 22 of the TGA data. Consistent with experiment A, E1 and E2 were more susceptible to oxidation than their more hexagonal counterparts, E0, and this was true for a variety of oxidizing agents. [Table 24]
[0151] A closer look at the oxidation between E1 and E2 reveals notable differences. While the total mass loss for E1 and E2 over the range of 100°C to 750°C is similar (approximately 14-15%), closer inspection (Figure 23 and Table 25) reveals that sample E1 drops 9.6% in the range of 100°C to 300°C, while sample E2 drops 9.0% in the range of 300°C to 750°C. This indicates group-selective functionalization, where E1 may be favored for less stable groups and E2 for more stable groups. To further explore the phenomenon of group selectivity, a base wash was used to try and understand the exact nature of the groups present in each of the carbon oxidized samples. [Table 25]
[0152] By closely examining the mass loss over various temperature ranges, it is possible to glean information about the specific functional groups present on the carbon surface. Typically, the mass loss of carbon oxides can be broadly classified into four regions based on temperature: below 100°C, 100-300°C, 300-600°C, and 600-750°C.
[0153] The mass loss peak centered at 100°C is associated with water. The second peak centered at about 200°C (100-300°C) is associated with more unstable oxygen groups including epoxides, carboxyls, carbonates, and some hydroxyl groups. The third broad peak centered at 450°C (300-600°C) is associated with more stable oxygen functional groups including carbonyl groups and some hydroxyl groups. The final peak centered at 720°C (600-750°C) is associated with groups containing carboxylic acid / sodium carbonate groups.
[0154] Table 26 and Figure 24 provide information on the TGA mass loss before and after the base wash. [Table 26]
[0155] Most of the mass loss of sample E1 PrT 24 h (9.58% of the total 14.24%) occurs in the range of 100-300 °C. However, after base washing, sample E1 PrT 24 h BW showed only 2.2% mass loss over the range of 100-300 °C, with a higher mass loss of 3.4% in the range of 300-600 °C. Given the significant reduction in total mass loss after base washing (from 14.2% to 7%), it is explained that E1 PrT 24 h had a significant amount of OD removed by the base washing, and the groups on OD were responsible for the majority of the mass loss observed in the range of 100-300 °C. However, no OD was observed in the filtrate after base washing, indicating that OD was not responsible for the mass loss.
[0156] Surprisingly, the XPS results for sample E1 PrT 24 hours showed an atomic concentration of nitrogen of 5.3% and an atomic concentration of sulfur nearly equal to 5.5%. The nitrogen present is substantially all in the form of quaternary nitrogen cations and the sulfur is substantially all in the form of sulfate anions. With a combined atomic concentration of nitrogen and sulfur of approximately 11% and oxygen exceeding 22%, it is clear from the XPS that the quaternary nitrogen cations and sulfate anions constitute the intercalated species.
[0157] This is surprising considering the absence of nitrogen compounds in the chemistry used. Instead, it appears that the lattice expands during oxidant intercalation, trapping atmospheric nitrogen dissolved in solution. When dissolved gas molecules are introduced between the lattice, they are induced to react due to the extreme confinement. Confinement has been shown to increase the reactivity of certain species and the reaction rates of certain reactions by many orders of magnitude, giving rise to the concept of using nanopores as "nanoreactors". The presence of quaternary nitrogen cations and sulfate anions explains the difference in mass loss in TGA, indicating that a base wash is effective in removing intercalated compounds.
[0158] For sample E2 PrT 24h, most of the total mass loss occurs in the ranges of 100-300°C and 300-600°C. The mass loss across these two ranges is fairly evenly split at 5.9% and 6.1%, respectively, with only 2.9% lost in the range of 600-750°C. However, for sample E2 PrT 24h BW, almost half of the total mass loss occurs in the range of 600-750°C, with the mass loss in the ranges of 100-300°C and 300-600°C decreasing to 4.4% and 5.6%, respectively. It is estimated that the base wash reduces the mass loss numbers if there was a large amount of OD. However, the total mass loss after the base wash increases significantly (from 14.93% to 19.35%). This indicates that the carboxylic acid groups on the carbon oxides are neutralized and sodium salts are formed when exposed to NaOH.
[0159] The addition of sodium cations to the carboxylic acid groups increases the total labile mass of sample E2 PrT 24h BW by about 30% (net of loss due to OD removal) relative to the total labile mass of sample E2 PrT 24h. Conversion of the COOH groups to salts (COONa) increases the theoretical mass by 56%, and if the oxygen groups on the carbon surface are 100% carboxylic acids (and no OD is present), the total labile mass should increase by about 56% after base washing. Thus, the empirically observed 30% increase in labile mass suggests that about 54% of the total labile mass is composed of carboxylic acids, and possibly more depending on the extent to which the OD-related labile mass was reduced by base washing.
[0160] Further support for this assertion is the large atomic % of sodium, about 4.6%, observed for E2 PrT 24h BW in the XPS results, and the significant shift in the thermal stability of the formed salts compared to the carboxylic acids. The TGA curves clearly show the predominance of stabilized species, which are volatile only in the temperature range of 600-750 °C, with a reduction in the more unstable carboxylic species. Furthermore, the TGA curves of E2 PrT 24h BW-RA show that, as presumed, acidifying the base-washed sample restores the more unstable species. Removal of the stabilized salts eliminates the observed shift in mass loss towards the temperature range of 600-750 °C.
[0161] Such a high level of initial carboxylic acid indicates that the carboxylic acid groups are located on the basal planes. This is rare for planar lattice materials such as graphene, but is preferred for convex lattice materials such as the outer surface of a CNT. Examination of TEM images of E2 type carbon versus E1 type carbon reveals that the E2 type lattice is much more curved and non-planar. The wrinkled fringes are less coherent and harder to track. In contrast, the E1 type lattice is more planar. This explains the group-selective carboxylation of the E2 type lattice, whereas the E1 type lattice does not appear to be selectively carboxylated. That is, the E2 type lattice contains convex and concave sites. When the E2 type lattice is exposed to an oxidant on one of its sides, it is site-selectively and group-selectively carboxylated at the convex sites due to local lattice distortion (similar to the outer surface of a nanotube). In contrast, the concave sites are speculated to be less reactive and therefore contribute fewer oxygen groups. The result is a carbon that, although distinct from nanotubes (e.g., each of its lattice planes has both concave and convex features, rather than just one or the other), resembles a nanotube because its functional groups are substantially all located on the convex sites, resulting in a high degree of carboxylation.
[0162] APS treatment was chosen as an additional method to demonstrate the difference in the chemical oxidation potential of the modified lattices for various oxidation protocols. After APS treatment, E0 and E2 had a mass loss (100-750 °C) of 12.1% and 21.9%, respectively, as seen in the TGA data in Table 27 and Figure 25. Note that APS treatment as an oxidation protocol did not produce any observable OD. [Table 27]
[0163] Similar to other oxidation treatments in previous experiments, experiment E further verifies the ability to expose the lattice modified carbon to various types of chemicals, specifically various types of oxidizing agents, to induce chemical functionalization. Experiment E further demonstrates the ability to generate lattice and multi-layer lattice assemblies in which the lattice carbon is bonded to nitrogen or sulfur atoms. Interstitial confinement is shown to induce certain reactions that are not predicted under normal conditions. Furthermore, it is shown that functional groups can be added between the lattices of multi-layer structures. Experiment E also shows that in the case of single-sided oxidation, the functional group density of the oxygen groups on the exposed side can be significantly higher than the functional group density of the oxygen groups on graphene oxide. Group-selective and site-selective functionalization utilizing modified lattice structures with both concave and convex features on both sides is also demonstrated.
[0164] This application discloses several numerical ranges in the text and figures. Since the disclosure can be practiced over the disclosed numerical ranges, the disclosed numerical ranges encompass ranges or values within the disclosed numerical ranges even if an exact range limit is not literally stated herein.
[0165] The above description is provided to enable those skilled in the art to make and use the present disclosure. Various modifications to the embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present disclosure. Thus, the present disclosure is not intended to be limited to the embodiments shown, but should be accorded the widest scope consistent with the principles and features disclosed herein. Finally, the entire disclosures of the patents and publications referenced in this application are incorporated herein by reference.
Claims
1. 1. A method for forming oxidized carbon particles, comprising: growing a wall of carbon on a surface of each template particle in a powder of template particles via template-induced chemical vapor deposition at a temperature of 850° C. or less, each carbon wall at least partially covering a surface of each template particle, said growth comprising autocatalytic growth of a carbon lattice comprising non-hexagonal rings, said carbon wall comprising: The wall thickness is at most 100 nm, The Raman spectrum at 532 nm has a maximum I of 0.
25. 2D / I G Ratio and I of at least 0.2 T / I G having a ratio an XRD diffraction pattern characterized in that it exhibits a peak diffraction angle corresponding to an interlayer d-spacing of 3.45 Å to 3.65 Å; extracting each template particle from the carbon walls formed on its surface to form a templated pore structure, each carbon wall and the templated pore structure together constituting a porous templated carbon particle; and After growth, exposing the carbon walls to an oxidizing agent to covalently bond functional groups to the surface; A method comprising:
2. The method of claim 1, wherein the carbon wall comprises multi-layer features.
3. The method of claim 1 , wherein the carbon walls have a wall thickness of less than 10 nm.
4. The method of claim 3 , wherein the carbon walls have a wall thickness of less than 10 nm.
5. 2. The method of claim 1, wherein the 532 nm Raman spectrum is derived by averaging a 25 point spectrum, the 25 point spectrum being measured on a 5x5 grid with 20 μm spacing between points.
6. The 532 nm Raman spectrum further has an I of at least 0.
4. T / I G The method of claim 5 comprising an intensity ratio.
7. The 532 nm Raman spectrum further exhibits a maximum I of 1.
0. D / I G The method of claim 5 comprising an intensity ratio.
8. 1. A method for forming oxidized carbon particles, comprising: growing a wall of carbon on a surface of each template particle in a powder of template particles via template-induced chemical vapor deposition at a first temperature of 850° C. or less, each carbon wall at least partially covering a surface of each template particle, said growth comprising autocatalytic growth of a carbon lattice comprising non-hexagonal rings, said carbon wall comprising: The wall thickness is at most 100 nm, The Raman spectrum at 532 nm has a maximum I of 0.
282. 2D / I G Ratio and I of at least 0.2 T / I G having a ratio an XRD diffraction pattern characterized in that it exhibits a peak diffraction angle corresponding to an interlayer d-spacing of 3.45 Å to 3.65 Å; after growing the carbon wall at the first temperature, heating the carbon wall to a second temperature higher than the first temperature; extracting each template particle from the carbon walls formed on its surface to form a templated pore structure, each carbon wall and the templated pore structure together constituting a porous templated carbon particle; and exposing the carbon wall to an oxidizing agent after heating to the second temperature to covalently bond functional groups to the surface thereof, wherein the oxidized carbon wall comprises multi-layer features; A method comprising:
9. The method of claim 8, wherein the second temperature is between 750°C and 1050°C.
10. The method of claim 1 , wherein the wall of carbon is conveyed through at least one of a moving bed and a fluidized bed.
11. The method of claim 1 , wherein the template particles comprise at least one of an inorganic salt and a metal oxide.
12. The method further comprises: calcining particles comprising magnesium carbonate to form said template particles comprising magnesium oxide; The method of claim 1 , comprising:
13. The method of claim 1 , wherein the oxidation comprises lateral selective functionalization.
14. The method of claim 1 , wherein the oxidation comprises covalently bonding oxygen groups to carbon atoms in the basal planes of the carbon lattice in the carbon walls.
15. The method of claim 14 , wherein the oxygen groups include at least one of hydroxyl, carboxyl, and carboxylate.
16. The method of claim 14 , wherein the oxygen group comprises an epoxide.
17. The method of claim 1 , wherein the oxidation comprises etching nanoscale holes in a carbon lattice in the carbon walls.
18. The method of claim 1 , wherein the oxidation does not produce an oxidation residue.
19. The method of claim 1 , wherein the oxidation comprises intercalating an acid into multi-layer features in the carbon wall.
20. 10. The method of claim 1, wherein the method excludes the use of strong acids and strong oxidizing agents.
Citation Information
Patent Citations
Preparation method for graphene material with porous structure
CN102583337A
Method for largely preparing amorphous carbon nanocage by taking phenol as precursor
CN104118859A
Preparation method of boron and nitrogen co-doped hollow carbon nanocage
CN104961119A
Method for preparing asphalt-based hierarchical porous carbon sheet based on sheet-shaped magnesium oxide template and application thereof
CN106430144A
Method for modifying surface of carbonaceous powder and granule
JP1993078110A