Ink transport tube

The thermoplastic elastomer composition for ink transport tubes, combining SEBS/SIBS, polyolefin, and modified polyethylene, addresses surface tackiness and enhances flexibility and barrier properties, ensuring reliable operation and print quality.

JP7591435B2Active Publication Date: 2024-11-28FUKOKU CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021037956
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-11-28
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

Existing ink transport tubes for inkjet printers made of thermoplastic elastomers suffer from surface tackiness, leading to abrasion and blockage due to friction, poor shape recovery, and inadequate anti-adhesive properties, compromising flexibility, kink resistance, water vapor barrier, and gas barrier properties.

Method used

A thermoplastic elastomer composition comprising styrene-ethylene-butylene-styrene copolymer (SEBS) or styrene-isobutylene-styrene copolymer (SIBS), polyolefin resin, polybutene or polyisobutylene, and modified polyethylene with a polar structure, which reduces surface tackiness and enhances flexibility, kink resistance, and barrier properties.

Benefits of technology

The composition provides an ink transport tube with excellent kink resistance, water vapor barrier, gas barrier, and strain resistance, while maintaining permanent low surface tackiness, ensuring reliable operation and print quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591435000002
    Figure 0007591435000002
  • Figure 0007591435000003
    Figure 0007591435000003
  • Figure 0007591435000001
    Figure 0007591435000001
Patent Text Reader

Abstract

To provide an ink transportation tube formed of soft thermoplastic elastomer permanently reduced in adhesiveness of a surface, while having excellent kink resistance, steam barrier, gas barrier, and distortion resistance residual property.SOLUTION: An ink transportation tube for an ink jet printer is formed of a thermoplastic elastomer composition. The thermoplastic elastomer contains at least one kind selected from a group consisting of (A) styrene-based thermoplastic elastomer (TPS), (B) polyolefin resin, (C) polybutene, polyisobutylene and polyisoprene-isobutylene copolymer, and (D) modified polyethylene. The modified part of (D) contains a structure having polarity. An addition amount of the (D) modified polyethylene to 100 pts.wt. of the (A) styrene-based thermoplastic elastomer (TPS) is 0.1-50 pts.wt.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink transport tube for an ink jet printer, which is made of a thermoplastic elastomer. [Background technology]

[0002] Patent Document 1 discloses that a molded article obtained from a resin composition containing (a) 100 parts by mass of a hydrogenated block copolymer of an aromatic vinyl compound and a conjugated diene compound, (b) 5 to 100 parts by mass of a polypropylene resin having a melt mass flow rate of 1 to 10 g / 10 min at 230° C. and 21.18 N in accordance with JIS K7210, and (c) 50 to 120 parts by mass of a rubber softener, the resin composition having a Shore A hardness of 50 to 95 in accordance with JIS K6253 and a melt mass flow rate of 0.1 to 15 g / 10 min at 230° C. and 49 N in accordance with JIS K7210, is suitable for use as an automobile part, in particular a hose / tube material.

[0003] The thermoplastic elastomer molded product of Patent Document 1 becomes sticky on the surface when its hardness decreases. Therefore, when used as an ink transport tube for an inkjet printer, surface wear occurs due to friction between the tubes and between the tube and the outer peripheral parts of the printer when the ink head is in operation. Furthermore, in inkjet printers, the tube may be temporarily crushed. This crushing is temporary and the tube is quickly released, but if the inner surface of the tube is sticky, there is a problem that the tube will remain clogged due to adhesion between the inner surfaces even if an attempt is made to release the crushed state (poor shape recovery responsiveness). It is also described that the addition of polymers such as unmodified polyolefins and acrylic resins can impart non-stickiness (anti-blocking properties), but the non-stick effect is insufficient and does not last long. In addition, the hardness increases, making it difficult to achieve flexibility. Thus, the problems specific to ink transport tubes are not fully resolved. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-131769 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide an ink transport tube made of a flexible thermoplastic elastomer that has excellent kink resistance, water vapor barrier properties, gas barrier properties, and residual distortion resistance, while permanently reducing the tackiness of its surface. [Means for solving the problem]

[0006] The present invention encompasses the following: [1] (A) a styrene-based thermoplastic elastomer (TPS); (B) a polyolefin resin; (C) at least one selected from the group consisting of polybutene, polyisobutylene, and polyisoprene-isobutylene copolymer; (D) Modified polyethylene and Including, The modified portion of (D) contains a polar structure, The amount of modified polyethylene (D) added is 0.1 to 50 parts by weight per 100 parts by weight of styrene-based thermoplastic elastomer (A) (TPS). 1. An ink transport tube for an ink jet printer, comprising a thermoplastic elastomer composition comprising: [2] The ink transport tube for an inkjet printer according to [1], wherein (A) the styrene-based thermoplastic elastomer (TPS) is a styrene-ethylene-butylene-styrene copolymer (SEBS). [3] The ink transport tube for an inkjet printer according to [1], characterized in that (A) the styrene-based thermoplastic elastomer (TPS) is made of a styrene-ethylene-butylene-styrene copolymer (SEBS) and a styrene-isobutylene-styrene copolymer (SIBS). [4] (A) The ink transport tube for an ink jet printer according to [3], characterized in that, when the styrene-based thermoplastic elastomer is 100 parts by weight, the styrene-ethylene-butylene-styrene copolymer (SEBS) is 50 parts by weight to 99 parts by weight, and the styrene-isobutylene-styrene copolymer (SIBS) is 1 part by weight to 50 parts by weight. [5] The surfaces of two thermoplastic elastomer sheets measuring 60 (length) x 10 (width) x 2 (thickness) mm were rubbed 100 times with a 10 mm diameter polypropylene rod pressed against the thermoplastic elastomer sheets, and then the rubbed thermoplastic elastomer surfaces were pressed together with a pressure load of 1 gf / mm 2 An ink transport tube made of the thermoplastic elastomer according to any one of [1] to [4], characterized in that the maximum adhesion load (maximum adhesion load after durability; non-stickiness persistence) measured using a T-type peel tester at a peel speed of 50 mm / min after being pressed against the ink transport tube for 1 minute is 0.05 N / cm or less. [6] Two thermoplastic elastomer sheets of 60 (length) x 10 (width) x 2 (thickness) mm are pressed together with a pressure load of 1 gf / mm 2 The ink transport tube according to [5], characterized in that after being pressed for 1 minute, the maximum adhesion load (initial maximum adhesion load) measured using a T-type peel tester at a peel speed of 50 mm / min is 0.05 N / cm or less. Effect of the Invention

[0007] According to the present invention, it is possible to provide an ink transport tube made of a flexible thermoplastic elastomer having excellent kink resistance, water vapor barrier properties, gas barrier properties, and residual distortion resistance, while having permanently low surface adhesion. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram of evaluation of non-adhesiveness by a T-peel test. [Diagram 2] FIG. 2 is a schematic diagram of a method for evaluating non-stickiness persistence. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The thermoplastic elastomer composition of the present invention and its molded product are suitable for use as, for example, an ink transport tube for an ink-jet printer.

[0010] Inkjet printers can be broadly divided into two types. One is the on-carriage type, where the ink tank and ink head are integrated, and this type is mainly used in home printers. On the other hand, there is also the off-carriage type, where the ink tank and ink head are separate and connected via the ink transport tube mentioned above to transport ink from the tank to the head. This type has the advantage that the ink tank can be made large and the printing speed is fast, and large-format printers for printing A1 size and above are examples of this type.

[0011] In general, ink transport tubes for off-carriage type ink jet printers are required to have flexibility, kink resistance, water vapor barrier properties, gas barrier properties, and residual distortion resistance (details of each performance will be described later). To meet these requirements, many ink transport tubes using styrene-based thermoplastic elastomers have been invented to date. In order to use a composition containing (A) styrene-ethylene-butylene-styrene copolymer (SEBS) and (B) polypropylene resin, such as that described in Patent Document 1, for ink transport tube applications, it is necessary to add a softener to the composition to impart sufficient flexibility. Commonly used softeners added to thermoplastic elastomers are non-aromatic softeners (for example, paraffinic mineral oils, naphthenic mineral oils, polybutene, polyisobutylene, polyisoprene-isobutylene copolymers, etc., which are linear saturated hydrocarbons or branched saturated hydrocarbons). From the viewpoint of gas barrier properties and water vapor barrier properties, (C) polybutene, polyisobutylene, and polyisoprene-isobutylene copolymers are particularly suitable. However, when an ink transport tube was produced from a composition containing the components (A) to (C), the obtained ink transport tube had a sticky surface, which caused problems such as blockage inside the tube when released from a crushed state (poor shape recovery response) and surface wear due to friction between the tubes and between the tubes and the outer peripheral parts of the tube when the ink head was in operation. From the disclosure of Patent Document 1, it was known that a certain degree of non-stickiness could be imparted by adding polymers such as unmodified polyolefins and acrylic resins. However, the non-stick effect was insufficient, the effect did not last long, or the effect was traded off with a loss of flexibility, so the above-mentioned problems specific to ink transport tubes could not be completely solved.

[0012] First, various characteristics required for an ink transport tube, particularly an ink transport tube for an ink jet printer, will be described.

[0013] - Non-stickiness and non-stickiness persistence Considering the above-mentioned problems caused by the stickiness of the surface of the ink transport tube, the initial maximum sticking load and the maximum sticking load after durability testing, which are measured in the non-stickiness evaluation method and the non-stickiness durability evaluation method described below, are preferably 0.10 N / cm or less, and more preferably 0.05 N / cm or less. From another viewpoint, when the initial maximum sticking load and the maximum sticking load after durability of a composition containing the above components (A) to (C) but not the component (D) are xN / cm and yN / cm, respectively, the initial maximum sticking load and the maximum sticking load after durability of a composition containing the components (A) to (D) of the present invention are preferably 0.59xN / cm or less and 0.67yN / cm or less, respectively, and more preferably 0.29xN / cm or less and 0.33yN / cm or less.

[0014] Flexibility In an off-carriage type inkjet printer, the ink transport tube connecting the ink tank and the ink head is pulled along with the drive of the ink head, and the ink transport tube is subjected to a large bending deformation. Therefore, if the ink transport tube has a high hardness, there is a risk that an excessive load is applied to the motor when the ink head is driven, or that the tube may be fatigued and broken. Therefore, the ink transport tube needs to have flexibility that can withstand the drive operation of the ink head. From these points of view, the hardness of the thermoplastic elastomer of the present invention, as measured by the hardness evaluation method described below, is preferably 65 or less, more preferably 50 or less.

[0015] Kink resistance The ink transport tube is subjected to a large bending deformation with a large curvature when the ink head is driven. If the ink transport tube buckles (kinks) at this time, the ink flow path will be blocked and the supply of ink to the ink head will be hindered. Therefore, the ink transport tube needs to have excellent kink resistance.

[0016] -Water vapor barrier properties Since ink is present inside the ink transport tube, if the water in the ink evaporates outside the tube, the viscosity of the ink increases, leading to poor ink ejection and reduced print quality. To avoid this, the ink transport tube needs to have excellent water vapor barrier properties.

[0017] Gas barrier properties When outside gases such as air permeate into the ink transport tube, the outside gas dissolves in the ink inside the tube. As a result, air bubbles form in the ink, causing ink discharge abnormalities and reduced print quality. To avoid this, the ink transport tube needs to have excellent gas barrier properties.

[0018] -Distortion resistance If the ink transport tube has poor resistance to residual distortion, the entire tube is likely to be permanently deformed, which may adversely affect the operation of the ink head. In addition, the tube's ability to recover its shape when released from compression is also poor, making the inside of the tube more likely to become clogged. For this reason, the ink transport tube needs to have excellent resistance to residual distortion.

[0019] Next, the composition of the thermoplastic elastomer composition suitable for producing an ink transport tube, particularly an ink transport tube for an ink jet printer, will be described.

[0020] <Component composition> The thermoplastic elastomer composition of the present invention has the following component configuration. (A) a styrene-based thermoplastic elastomer (TPS); (B) a polyolefin resin; (C) at least one selected from the group consisting of polybutene, polyisobutylene, and polyisoprene-isobutylene copolymer; (D) Modified polyethylene and Including, The modified portion of (D) contains a polar structure, The amount of the modified polyethylene (D) added is 0.1 to 50 parts by weight per 100 parts by weight of the styrene-based thermoplastic elastomer (TPS) (A).

[0021] (A) Thermoplastic styrene elastomer (TPS) (A) Styrene-based thermoplastic elastomer (TPS) is the main component of the thermoplastic elastomer of the present invention, and is capable of satisfying the performance requirements of the ink transport tube, such as flexibility, kink resistance, water vapor barrier properties, gas barrier properties, and residual strain resistance, in a well-balanced manner, and examples thereof include styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-ethylene-propylene-styrene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), styrene-isobutylene-styrene copolymer (SIBS), styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), etc. However, in consideration of gas barrier properties and water vapor barrier properties, it is preferable to use styrene-ethylene-butylene-styrene copolymer (SEBS) or styrene-isobutylene-styrene copolymer (SIBS). Examples of such raw materials include Septon 8004, 8006, and 8007L (all manufactured by Kuraray Co., Ltd.), and SIBSTAR 073T, 102T, and 103T (all manufactured by Kaneka Co., Ltd.). These may be used alone or in combination. The styrene-based thermoplastic elastomer (TPS) preferably has an MFR of 2.0 g / 10 min or less, measured, for example, in accordance with JIS K 7210 at 230° C. and 2.16 kgf.

[0022] When styrene-ethylene-butylene-styrene copolymer (SEBS) and styrene-isobutylene-styrene copolymer (SIBS) are used in combination, the gas barrier property and water vapor permeability improve as the ratio of the latter increases, but the residual strain resistance tends to deteriorate. Therefore, when styrene-ethylene-butylene-styrene copolymer (SEBS) and styrene-isobutylene-styrene copolymer (SIBS) are used in combination, it is preferable to use 50 to 99 parts by weight of the former and 1 to 50 parts by weight of the latter, based on 100 parts by weight of the total of (A) styrene-based thermoplastic elastomer (TPS) (or the weight ratio of SEBS:SIBS is preferably in the range of 50:50 to 99:1). If the former is less than 50 parts by weight and the latter is more than 50 parts by weight, the residual strain resistance deteriorates, and the tube may be adversely affected by being easily permanently deformed.

[0023] (B) Polyolefin resin The thermoplastic elastomer composition of the present invention contains a polyolefin resin that is compatible with the (A) component. Polyolefin is a resin made of a polymer synthesized from a simple alkene having a double bond between carbon and carbon as a monomer, and corresponds to polyethylene resin and polypropylene resin. The incorporation of this component improves the flowability at high temperatures and improves moldability. Among them, polypropylene resin is particularly suitable in the present invention because it has little deterioration in gas barrier properties. Examples of raw materials that correspond to this include trade names: Novatec PP EA7A, Novatec PP BC05B, Novatec LD LJ803 (all manufactured by Japan Polypropylene Corporation), PM600A, PL400A (all manufactured by Sun Allomer Corporation). This component is preferably contained in an amount of 10 to 50 parts by weight per 100 parts by weight of the (A) component. The incorporation of this component in an amount of 10 parts by weight or more makes it easier to improve moldability. In addition, the incorporation of this component in an amount of 50 parts by weight or less makes it easier to suppress the deterioration of flexibility and kink resistance and the deterioration of residual strain resistance. The polyolefin resin preferably has an MFR of 0.3 to 2.5 g / 10 min, measured according to JIS K 7210 at 230° C. and 2.16 kgf.

[0024] (C) Polybutene, polyisobutylene, polyisoprene-isobutylene copolymer The component (C) used in the present invention is a component that can increase the flexibility of an ink transport tube made of a thermoplastic elastomer without decreasing its gas barrier property or water vapor barrier property. Component (C) is available in a range of viscosities from low to high. When a low viscosity product is used, the adhesion is low, but the gas barrier property and water vapor barrier property of the ink transport tube may be decreased compared to a high viscosity product. On the other hand, a high viscosity product has high surface adhesion, but has high gas barrier property and water vapor barrier property, and is therefore more suitable for use as an ink transport tube. The problem of surface adhesion caused by component (C) can be solved by adding modified polyethylene (D). Therefore, the kinetic viscosity of component (C) at 40°C is preferably 500 mm 2 / s or more, preferably 1,000 mm 2 Examples of raw materials that fall into this category include trade names such as Nippon Oil Polybutene HV-15, HV-35, HV-50, and HV-100 (all manufactured by Nippon Petrochemicals), Tetrax 3T, 4T, 5T, and 6T (all manufactured by JXTG Nippon Oil & Energy), JSR BUTYL065, JSR BUTYL268, and JSR BUTYL365 (all manufactured by JSR). Preferred polybutenes, polyisobutylenes, and polyisoprene-isobutylene copolymers have, for example, MLs of 50 to 90. (1+4) At 100°C, it has a weight average molecular weight of 1,000 to 100,000, or a number average molecular weight of 100 to 10,000. From the viewpoint of improving the print quality of the printer, the upper limit of the amount of this component added is preferably 300 parts by weight or less, more preferably 150 parts by weight or less, per 100 parts by weight of component (A), while the lower limit is preferably 30 parts by weight or more, more preferably 50 parts by weight or more, from the viewpoint of improving flexibility.

[0025] (D) Modified polyethylene The modified polyethylene component (D) used in the present invention is a component added to reduce the tackiness of the surface of the ink transport tube made of a thermoplastic elastomer, and the modified portion includes a structure having polarity. Examples of the structure having polarity include functional groups such as epoxy groups, ether groups, sulfide groups, carboxy groups, ester groups, carbonate groups, alkoxy groups, hydroxy groups, imide groups, amide groups, acrylic groups, methacrylic groups, nitrile groups, nitro groups, amino groups, and sulfonyl groups, as well as structures such as epoxy resins, acrylic resins, polyacrylonitrile, polyesters, styrene-styrene-acrylonitrile acrylic resins, acrylonitrile-butadiene-styrene resins, acrylonitrile butadiene resins, polyurethanes, polyamide resins, and polyimide resins. Examples of raw materials that fall under this category include styrene-acrylonitrile modified polyethylene (trade name: Modiper A1401, manufactured by NOF Corporation) and maleic acid modified polyethylene (trade name: Adtex DU6310, manufactured by Japan Polyethylene Co., Ltd.). Among these, those containing a styrene structure in the modified portion, which has an attractive interaction with the hard segment (styrene unit) of component (A), have particularly high durability of the adhesion prevention effect. That is, the modified portion of the particularly preferred component (D) contains a polar structure and a styrene structure. The lower limit of the amount of component (D) added must be 0.1 parts by weight or more, preferably 0.5 parts by weight or more, and more preferably 1.0 parts by weight or more, per 100 parts by weight of component (A) from the viewpoint of anti-tack effect, while the upper limit of the amount added is preferably 50 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 15 parts by weight or less, from the viewpoints of flexibility, kink resistance, and residual strain resistance.

[0026] As a method for modifying polyethylene, a modification method in which the raw polyethylene is contacted with the compound having the above functional group or the above resin at high temperature by a known method such as a solution method, a slurry method, or a melt kneading method is particularly suitable. Other modification methods include a method in which a high molecular weight polyethylene is graft-modified by the above method, and then thermally decomposed or oxidatively decomposed, and a method in which a high molecular weight polyethylene is oxidatively decomposed in an oxidizing atmosphere to introduce a carboxyl group as a structure having polarity. By allowing styrene to coexist during the reaction, a component (D) having both a structure having polarity and a styrene structure in the modified part can be obtained. The modified polyethylene preferably has an MFR of 0.1 to 1.2 g / 10 min, measured, for example, in accordance with JIS K 7210 at 190° C. and 2.16 kgf.

[0027] <Mechanism of anti-adhesive effect> Without being bound by theory, the mechanism by which the anti-tack effect of the present invention is exhibited is presumed to be as follows. In the case of an ink transport tube for an ink jet printer, which is made of a thermoplastic elastomer containing components (A), (B), and (C), the surface of the tube becomes sticky due to the bleed-out of component (B) onto the surface and the high flexibility of the thermoplastic elastomer. When modified polyethylene (D) is added to such a thermoplastic elastomer composition, the polar structure of the modified portion, which has poor compatibility with the main component (A), causes component (D) to precipitate on the surface of the ink transport tube, which results in the surface being covered with non-adhesive component (D) and the highly adhesive components such as component (B) not being exposed to the surface, thereby reducing the adhesiveness. On the other hand, the polyethylene structure of component (D) has excellent compatibility with component (A) and can be fully compatible and alloyed with each other. Therefore, even if the tubes are repeatedly brought into contact with and peeled off from each other or rub against each other, they do not easily peel off from the surface, and therefore the non-adhesive effect is maintained permanently. Furthermore, when a styrene structure is present in the modified portion of component (D), this styrene structure and the hard segment (styrene unit) of component (A) create an attractive interaction, resulting in particularly excellent lasting non-stick properties. EXAMPLES

[0028] The present invention will be described in detail below with reference to examples and comparative examples. The methods for producing compositions and molded products, the various evaluation methods, and the raw materials used in the examples are as follows.

[0029] ·Method of manufacturing thermoplastic elastomer composition First, components (A) to (C) were melt-kneaded at a rotation speed of 20 rpm using a Labo Plastomill 10C100-B600 mixer (manufactured by Toyo Seiki) set at 170°C. Next, when the temperature of the thermoplastic elastomer inside reached 165°C, component (D) was added and kneaded at a rotation speed of 20 rpm for an additional 5 minutes. The temperature of the mixer was then increased to 200°C, and the mixture was further kneaded until the internal thermoplastic elastomer temperature reached 195°C, and then removed.

[0030] -Method of manufacturing thermoplastic elastomer test specimens The thermoplastic elastomer composition obtained by the above-mentioned manufacturing method was placed in a sheet mold of any size heated to 195°C and heated for 10 minutes without applying pressure. Then, the composition was heated for another 10 minutes with sufficient molding pressure, and the sheet mold was then cooled to 25°C to obtain a thermoplastic elastomer sheet.

[0031] -Method of manufacturing thermoplastic elastomer tube and method of evaluating moldability The thermoplastic elastomer composition obtained by the above-mentioned manufacturing method was extruded using a Labo Plastomill 10C100-single tube extruder D2025N set at 195°C, and then instantly cooled with water to obtain a tubular molded product having an outer diameter of 4.0 mm and an inner diameter of 1.5 mm.

[0032] Hardness evaluation method Hardness, which is an index of flexibility, was measured using a Type A hardness tester in accordance with JIS K 6253-3. The hardness value in this evaluation was the value 15 seconds after the indenter contacted the test piece. Considering the motor load when the ink head is driven and fatigue destruction due to continuous driving, the hardness is preferably 65 or less, and more preferably 50 or less.

[0033] Kink resistance evaluation method The tube produced by the above method was cut to a length of 300 mm, and both ends of the tube were aligned in the same direction and clamped with a clip. The clamped tube was slowly pressed with a finger and traced from both ends toward the center of the tube so that the two ends were in contact and parallel, and the finger was stopped at the point where the center of the tube buckled, and the distance from the center of the tube was measured to evaluate kink resistance. Considering the maximum curvature caused by driving the ink head, it is preferable that the distance from the center of the tube at the time of buckling is 70 mm or less.

[0034] -Elongation and tensile strength evaluation method The elongation and tensile strength were measured in accordance with JIS K 6251 at a tensile speed of 500 mm / min using a dumbbell-shaped No. 3 test piece.

[0035] Water vapor barrier property evaluation method The water vapor barrier property was measured using the thermoplastic elastomer sheet having a thickness of 0.5 mm produced by the above method in accordance with JIS Z 0208. The test conditions were Condition A (temperature 25±0.5°C, relative humidity 90±2%). Considering the deterioration of print quality due to evaporation of water from the ink in the tube, a printing pressure of 10 g / m 2 -24 hours or less is preferable.

[0036] Gas barrier property evaluation method The air permeability coefficient was measured in accordance with JIS K 7126-1 using the thermoplastic elastomer sheet having a thickness of 0.5 mm produced by the above method. The test temperature was 23°C and the differential pressure was 100 kPa. Considering the degradation of print quality due to dissolution of external gas into the ink in the tube, the -10 cm 3 cm / cm 2 ·s·cmHg or less is preferable.

[0037] -Distortion resistance remaining evaluation method The thermoplastic elastomer sheet with a thickness of 2 mm produced by the above method was punched out into a disk shape with a diameter of 29.0±0.5 mm, and three of these were stacked. Using these three-ply test pieces, the compression set rate was evaluated using a method similar to JIS K 6262 Method A, and this was used as an index of residual strain resistance. The test conditions were a temperature of 70°C, a time of 24 hours, and a compression rate of 25%. Considering the permanent deformation of the tube and the shape recovery when released from crushing, it is preferable that the deformation be 50% or less.

[0038] Non-adhesiveness evaluation method The thermoplastic elastomer sheet with a thickness of 2 mm produced by the above method was punched out into a strip of 60 x 10 mm. The two test pieces were completely overlapped and lightly pasted together with fingers to avoid trapping air, and a load of 500 gf was applied to the 50 x 10 mm part of the longitudinal end and pressed for 1 minute. Next, while lightly pressing the pressed side so as not to peel off, a portion of about 20 mm was peeled off from the other end, and this portion was chucked in a precision universal testing machine (Autograph AGS-X (manufactured by Shimadzu Corporation)). Thereafter, a T-type peel test was performed to peel off the two test pieces pressed together at a peel speed of 50 mm / min, and the maximum adhesion load of the pressed part (hereinafter, this load is referred to as the initial maximum adhesion load) was measured, and the value was used as an index of non-adhesiveness (see Figure 1). The test conditions were: pressure load: 1 gf / mm 2 , compression time: 1 minute, peeling speed: 50 mm / min. Considering blockage of the tube, the motor load when driving the ink head, and wear on the tube surface, the pressure is preferably 0.10 N / cm or less, and more preferably 0.05 N / cm or less.

[0039] -Non-sticky durability evaluation method The thermoplastic elastomer sheet with a thickness of 2 mm produced by the above method was punched out into a rectangular shape of 60 x 10 mm, and the side of a polypropylene cylindrical rod with a diameter of 10 mm was pressed against it with a load of 1 kgf / cm, and the entire surface was rubbed 100 times (see Figure 2). Then, two test pieces that had been subjected to this operation were completely overlapped, and a load of 500 gf was applied to the 50 x 10 mm part of the longitudinal end and pressed for 1 minute. Then, the maximum adhesion load of the pressed part (hereinafter, this load is referred to as the maximum adhesion load after durability) was measured using the same evaluation method as the above "Non-adhesive Evaluation Method", and the value was used as an index of non-adhesive durability. For the same reasons as in the above "Non-tackiness evaluation method," the strength is preferably 0.10 N / cm or less, and more preferably 0.05 N / cm or less.

[0040] ·Raw materials used Details of the raw materials used in the examples and comparative examples described below are as follows. [(A) Styrene-based thermoplastic elastomer] Product name: Septon 8007L (Kuraray) SIBSTAR 103T (Kaneka) [(B) Polyolefin resin] Product name: Novatec PP EA7A (Japan Polypropylene) [(C) Polybutene] Product name: Nippon Oil Polybutene HV-50 (manufactured by Nippon Petrochemicals) Tetrax 4T (manufactured by JXTG Energy) JSR BUTYL365 (manufactured by JSR) [(D) Modified polyethylene] Styrene-acrylonitrile modified polyethylene, product name: Modiper A1401 (manufactured by NOF Corporation) [Unmodified polyethylene (for comparison)] High density polyethylene, product name: Nipolon Hard 6000 (manufactured by Tosoh Corporation)

[0041] <Example 1> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 0.1 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0042] <Example 2> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 0.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0043] <Example 3> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 1.0 part by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0044] <Example 4> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 2.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0045] <Example 5> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 15.0 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0046] <Example 6> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 30.0 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0047] <Example 7> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 50.0 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0048] <Example 8> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polyisobutylene (Tetrax T4), and 2.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0049] <Example 9> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polyisoprene-isobutylene copolymer (JSR BUTYL365), and 2.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0050] <Example 10> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 50 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 50 parts by weight of styrene-isobutylene-styrene copolymer (SIBSTAR 103T), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 2.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0051] <Example 11> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 80 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of styrene-isobutylene-styrene copolymer (SIBSTAR 103T), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 2.5 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0052] <Comparative Example 1> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), and 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50).

[0053] <Comparative Example 2> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 0.05 parts by weight of styrene-acrylonitrile modified polyethylene (Modiper A1401).

[0054] <Comparative Example 3> According to the above-mentioned manufacturing method, a thermoplastic elastomer composition was obtained using 100 parts by weight of styrene-ethylene-butylene-styrene copolymer (Septon 8007L), 20 parts by weight of polypropylene resin (Novatec PP EA7A), 80 parts by weight of polybutene (Nippon Oil Polybutene HV-50), and 2.5 parts by weight of high-density polyethylene (Nipolon Hard).

[0055] Detailed compositional information and physical property information of the thermoplastic elastomer compositions and molded products produced in Examples 1 to 11 and Comparative Examples 1 to 3 are shown in Table 1. In addition, phr in Table 1 is parts by weight per 100 parts by weight of component (A).

[0056] [Table 1]

[0057] The "Judgment" column in Table 1 shows the results of judging whether a material is suitable for use as an ink transport tube, based on the following criteria. Flexibility, non-stickiness, and non-stickiness persistence were evaluated on a three-level scale. (1) Flexibility: A rating of 66 or above was categorized as “poor,” 65 to 51 as “good,” and 50 or below as “better.” (2) Kink resistance: If the kink resistance is 70 mm or less, it is suitable as an ink transport tube material. (3) Water vapor barrier property: 10g / m 2 -Suitable for use as ink transport tube material if the life is less than 24 hours. (4) Gas barrier property: 7.0×10 -10 cm 3 cm / cm2 If the resistance is less than 1.0scmHg, it is suitable for use as an ink transport tube material. (5) Distortion resistance: If it is 50% or less, it is suitable as an ink transport tube material. (6) Non-adhesiveness: 0.11 N / cm or more was categorized as “poor,” 0.1 to 0.06 N / cm was categorized as “good,” and 0.05 N / cm was categorized as “better.” (7) Non-stickiness durability: 0.11 N / cm or more was categorized as “poor,” 0.1 to 0.06 N / cm as “good,” and 0.05 N / cm as “better.”

[0058] (1), (6), and (7) were all rated “better,” and (2) through (5) met the criteria, so they were marked with an “◎.” A rating of “good” was given to a condition that satisfied at least one of items (1), (6), or (7) and criteria (2) through (5). At least one of items (1), (6), or (7) was marked as “poor,” or items not meeting the criteria in (2) through (5) were marked as “×.”

[0059] Examples 1 to 11 and Comparative Example 2 are thermoplastic elastomers using styrene-acrylonitrile modified polyethylene as the (D) component. The thermoplastic elastomers of Examples 1 to 11 (addition amount of (D) component is 0.1 to 50.0 parts by weight) exhibit excellent non-stickiness and non-stickiness durability. However, as the addition amount of (D) component decreases, the non-stickiness and non-stickiness durability gradually deteriorate, while as the addition amount increases, the flexibility, kink resistance, and residual strain resistance tend to gradually deteriorate. Considering these effects, among the above examples, Examples 3 to 5 and 8 to 11 (addition amount of (D) component is 1.0 to 15.0 parts by weight) are thermoplastic elastomers with better balance of all physical properties. On the other hand, Comparative Example 2 (addition amount of (D) component is 0.05 parts by weight) has a high maximum sticking load after durability and insufficient non-stickiness durability.

[0060] Examples 10 and 11 are thermoplastic elastomers that use a combination of styrene-ethylene-butylene-styrene copolymer (SEBS) and styrene-isobutylene-styrene copolymer (SIBS), and exhibit excellent non-stickiness and non-stickiness durability.

[0061] Comparative Example 1 is a thermoplastic elastomer that does not contain modified polyethylene (D). Compared with Examples 1 to 11, the non-stickiness and non-stickiness durability are poor, and it is not suitable for practical use as an ink transport tube for an inkjet printer.

[0062] Comparative Example 3 is a thermoplastic elastomer in which unmodified polyethylene having no polar structure is used instead of modified polyethylene (D). Compared with Example 4, the non-stickiness and non-stickiness durability are significantly inferior, and the comparative example is not suitable for practical use as an ink transport tube for an inkjet printer. [Industrial Applicability]

[0063] According to the present invention, it is possible to provide an ink transport tube made of a flexible thermoplastic elastomer that has excellent kink resistance, water vapor barrier properties, gas barrier properties, and residual distortion resistance, while permanently reducing the tackiness of its surface.

Claims

1. (A) a styrene-based thermoplastic elastomer (TPS); (B) a polyolefin resin; and (C) at least one selected from the group consisting of polybutene, polyisobutylene, and polyisoprene-isobutylene copolymer; (D) Styrene-acrylonitrile modified polyethylene; Including, The amount of the polyolefin resin (B) added relative to 100 parts by weight of the styrene-based thermoplastic elastomer (TPS) (A) is 10 to 50 parts by weight, the amount of at least one selected from the group consisting of polybutene, polyisobutylene, and polyisoprene-isobutylene copolymer (C) is 30 parts by weight or more and 300 parts by weight or less, and the amount of the styrene-acrylonitrile modified polyethylene (D) is 1.0 part by weight or more and 15 parts by weight or less.

1. An ink transport tube for an ink jet printer, comprising a thermoplastic elastomer composition comprising:

2. 2. The ink transport tube for an ink jet printer according to claim 1, wherein the styrene-based thermoplastic elastomer (TPS) (A) is a styrene-ethylene-butylene-styrene copolymer (SEBS).

3. 2. The ink transport tube for an ink-jet printer according to claim 1, wherein the styrene-based thermoplastic elastomer (TPS) (A) comprises a styrene-ethylene-butylene-styrene copolymer (SEBS) and a styrene-isobutylene-styrene copolymer (SIBS).

4. 4. The ink transport tube for an ink jet printer according to claim 3, wherein, when the styrene-based thermoplastic elastomer (A) is 100 parts by weight, the styrene-ethylene-butylene-styrene copolymer (SEBS) is 50 to 99 parts by weight, and the styrene-isobutylene-styrene copolymer (SIBS) is 1 to 50 parts by weight.

5. The surfaces of two thermoplastic elastomer sheets measuring 60 (length) x 10 (width) x 2 (thickness) mm were rubbed 100 times with a 10 mm diameter polypropylene rod pressed against the thermoplastic elastomer sheets, and the rubbed thermoplastic elastomer surfaces were then pressed together with a pressure load of 1 gf / mm. 2 5. An ink transport tube comprising the thermoplastic elastomer according to claim 1, characterized in that the maximum adhesion load (maximum adhesion load after durability test; non-adhesion durability) measured using a T-type peel tester under the condition of a peel speed of 50 mm / min after being pressed at 0.5 V for 1 minute is 0.05 N / cm or less.

6. Two thermoplastic elastomer sheets of 60 (length) x 10 (width) x 2 (thickness) mm were pressed together with a pressure load of 1 gf / mm. 2 6. The ink transport tube according to claim 5, wherein the maximum sticking load (initial maximum sticking load) measured using a T-type peel tester at a peeling speed of 50 mm / min after being pressed at 1000 V for 1 minute is 0.05 N / cm or less.

Citation Information

Patent Citations

  • Resin composition and container composed thereof

    JP2005200464A

  • Ink contacting thermoplastic elastomer composition for inkjet printer

    JP2010274627A

  • High gas-barrier composition and liquid transmission member

    JP2011219567A

  • Resin composition for ink supply tube, and ink supply tube

    JP2012051368A

  • Styrenic thermoplastic elastomer composition and application thereof

    JP2019131769A