container

A container with a flange portion having uneven and smooth surfaces addresses the issue of film peeling during use by maintaining adhesion during use and enabling easy post-use removal, enhancing recycling efficiency.

JP7591468B2Active Publication Date: 2024-11-28株式会社ユポ
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021098539
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-14
Publication Date
2024-11-28
Estimated Expiration
2041-06-14

AI Technical Summary

Technical Problem

Plastic containers used for food products often require cleaning before recycling due to films peeling off during use, and improvements like strong adhesives increase manufacturing steps.

Method used

A container design with a flange portion featuring uneven and smooth surfaces, where the film adheres strongly during use but can be easily peeled off post-use, using a thermoplastic resin film and adhesive layer with controlled adhesive strength.

Benefits of technology

The design ensures the film remains intact during use, facilitating easy removal after use, thus simplifying cleaning and enabling efficient recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591468000003
    Figure 0007591468000003
  • Figure 0007591468000004
    Figure 0007591468000004
  • Figure 0007591468000005
    Figure 0007591468000005
Patent Text Reader

Abstract

To provide a container which has such a configuration that a film adhering to a tor face is difficult to tear in use of the container and easy to tear by the hand after the use thereof.SOLUTION: A container has a film formed from thermoplastic resin adhering onto a top face of a container body formed from thermoplastic resin. The container body includes a flange part. A surface of the flange part includes an uneven part with an uneven structure and a smooth part without the uneven structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a container. [Background technology]

[0002] Conventionally, plastic containers have been used as containers for selling vegetables, food such as bento boxes, etc. From the viewpoint of environmental protection, plastic containers are increasingly being recycled, but in order to be recycled, the plastic containers must be washed.

[0003] To reduce the effort required for cleaning, containers have been proposed in which a peelable film is attached to the inside of the container body (see, for example, Patent Documents 1 and 2). By peeling the film off the container body after use, dirt on the container can be removed together with the film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-225662 A [Patent Document 2] JP 2017-200744 A Summary of the Invention [Problem to be solved by the invention]

[0005] Films that can be peeled off by hand after use of the container are also likely to peel off when the container is in use. Improvements such as using an adhesive or heat seal material with strong adhesive strength to strongly attach part of the film to the container are necessary, but such improvements will increase the number of manufacturing steps.

[0006] An object of the present invention is to provide a container having a structure in which a film adhered to the upper surface is unlikely to peel off when the container is in use, but can be easily peeled off by hand after use. [Means for solving the problem]

[0007] As a result of intensive research by the present inventors to solve the above problems, they discovered that the above problems could be solved by partially providing an uneven portion on the flange portion of the container, and thus completed the present invention. That is, the present invention is as follows.

[0008] (1) A container having a film made of a thermoplastic resin bonded to the top surface of a container body made of a thermoplastic resin, The container body includes a flange portion, The flange surface includes an uneven portion having an uneven structure and a smooth portion not having the uneven structure. container.

[0009] (2) The adhesive strength of the film in the entire flange portion including the uneven portion and the smooth portion is 0.5 to 20 N / 15 mm. The container described in (1) above.

[0010] (3) The arithmetic mean roughness (Ra) of the surface of the uneven portion is 0.1 to 3.0 mm. A container according to (1) or (2) above.

[0011] (4) When the container body is rectangular, the smooth portion is located at at least one of the four corners of the flange portion. A container according to any one of (1) to (3) above.

[0012] (5) An adhesive layer is provided between the film and the container body. A container according to any one of (1) to (4) above.

[0013] (6) The adhesive strength of the film at the flat portion is less than 0.5 N / 15 mm. A container according to any one of (1) to (5) above. Effect of the Invention

[0014] According to the present invention, it is possible to provide a container having a structure in which a film adhered to the upper surface is unlikely to peel off when the container is in use, and can be easily peeled off by hand after use. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a perspective view showing a container according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a perspective view of a container from which a film is to be peeled off. [Figure 4] FIG. 13 shows a bag formed by peeling off the film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of the container of the present invention will be described in detail below. The following is one example (representative example) of the present invention, and the present invention is not limited thereto. In the following description, the term "(meth)acrylic" refers to both acrylic and methacrylic.

[0017] [container] Fig. 1 shows a container 1 of this embodiment. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. The container 1 comprises a container body 2 and a film 3. The container body 2 is a thermoformed body of a thermoplastic resin sheet 2', and the film 3 is a thermoplastic resin film. The film 3 is adhered to the upper surface of the container body 2, and constitutes a surface layer on the upper side of the container 1. From the viewpoint of adjusting the adhesive strength between the container body 2 and the film 3, it is preferable that the container 1 comprises an adhesive layer 4 between the container body 2 and the film 3.

[0018] The container 1 may be provided with a lid material that covers the upper side of the container body 2. In order to fix the lid material to the container body 2, a lid material that fits with the container body 2 or that is bonded by heat can be used. Furthermore, the lid material and the container body 2 may be integrally molded so that a part of the lid material is connected to the container body 2.

[0019] As shown in Fig. 3, the film 3 can be peeled off by hand from the container body 2. After using the container 1, the container body 2 from which the film 3 has been peeled off can be recycled as is. Even if the top surface of the container 1 becomes dirty due to the contents, the dirt can be removed together with the film 3, eliminating the need for cleaning and facilitating recycling.

[0020] The peeled film 3 can also be used as a packaging film. By squeezing the ends of the film 3 together, a bag 5 can be formed as shown in Fig. 4, and the vegetables, side dishes, leftovers from a lunch box, etc. contained in the container 1 can be stored in this bag 5.

[0021] Each component will be described in detail below. (Container body) The container body 2 includes a storage portion 21 and a flange portion 22. These are usually integrally molded from a thermoplastic resin.

[0022] <Containment Unit> The storage section 21 may be in the shape of a deep bowl or dish. The shape of the bottom surface of the storage section 21 may be, for example, a polygonal shape such as a square, a circular shape, an elliptical shape, or the like.

[0023] The size of the storage section 21 can be appropriately selected according to the size of the contents. Usually, the long side of the bottom surface of the storage section 21 (meaning the longest overall length in the case of a rectangle, the diameter in the case of a circle, and the major axis in the case of an ellipse) is 50 mm to 500 mm, and the depth is 30 mm to 300 mm.

[0024] From the viewpoint of formability and strength of the container 1, it is preferable that the bottom surface of the storage section 21 is rectangular, circular, or elliptical. Moreover, if the storage section 21 is bowl-shaped, it is easier to form the film 3 peeled off from the container body 2 into a bag body 5, which is preferable. From the same viewpoint, it is preferable that the long side or diameter of the bottom surface is longer than the depth of the storage section 21. For this reason, it is more preferable that the ratio of the long side or diameter to the depth is 1 or more, and is usually 20 or less.

[0025] The thickness of the storage section 21 can be appropriately selected, but the thickness is preferably 200 μm or more, more preferably 250 μm or more, and even more preferably 300 μm or more from the viewpoint of increasing the compressive strength of the container 1. From the viewpoint of reducing costs, the thickness is preferably 800 μm or less, and more preferably 500 μm or less.

[0026] The corners of the bottom or wall are usually rounded in an arc shape, preferably with a radius of about 5 to 20 mm. The rounded shape makes the film 3 curved after peeling, making it easier to use as a bag 5.

[0027] <Flange part> The flange portion 22 protrudes outward from the end portion of the storage portion 21. The flange portion 22 can suppress deformation of the container 1. In addition, the flange portion 22 makes it easier to grip the container 1 with the hand.

[0028] The width from the inner periphery to the outer periphery of flange portion 22 can be selected depending on the contents of container 1, but is usually 5 mm or more. The thickness of the flange portion 22 can be the same as that of the housing portion 21 .

[0029] <<Uneven and smooth areas>> The surface of the flange portion 22 includes an uneven portion 22a having an uneven structure, and a smooth portion 22b having no such uneven structure. The uneven portion 22a can be formed by providing an uneven structure to a mold used for thermoforming the container 1. Since the uneven portion 22a is formed in the process of thermoforming the container 1, the uneven portion 22a can be easily formed without increasing the number of manufacturing steps.

[0030] The end of the container 1, such as the flange portion 22, is susceptible to impacts while the container 1 is in use. In addition, since the interface between the film 3 and the container body 2 is exposed, the film 3 tends to peel off easily at the flange portion 22. However, the uneven structure of the uneven portion 22a serves to fit the film 3 into the container body 2. Therefore, the uneven portion 22a can prevent the film 3 from peeling off. On the other hand, the film 3 is likely to peel off at the smooth portion 22b, which does not have an uneven structure to prevent peeling. Therefore, the smooth portion 22b can be used as a trigger for peeling off the film 3, making it easier to peel off after use.

[0031] The adhesive strength of the film 3 of the entire flange portion 22 including the uneven portion 22a and the smooth portion 22b is preferably 0.5 N / 15 mm or more, and more preferably 2 N / 15 mm or more, from the viewpoint of preventing peeling of the film 3 during use of the container 1. From the viewpoint of facilitating peeling of the film 3 after use of the container 1, the adhesive strength is preferably 20 N / 15 mm or less, more preferably 15 N / 15 mm or less, and even more preferably 10 N / 15 mm or less. The adhesive strength can be adjusted by the material of the adhesive layer 4, the interval or depth of the recesses (or protrusions) of the uneven structure, and the like.

[0032] On the other hand, the adhesive strength of the film 3 at the smooth portion 22b is preferably 0.01 N / 15 mm or more in order to prevent unnecessary peeling during use, and is preferably less than 0.5 N / 15 mm in order to provide an opportunity for peeling of the film 3. The adhesive strength is a value measured by a 180° peel test in accordance with JIS Z 0238:1998 using a strip-shaped sample cut from the flange portion 22.

[0033] Examples of the pattern of the uneven structure include a pattern in which the unevenness is distributed in a striped, net, dotted, zigzag, or wavy pattern, etc. Depending on the application of the container 1, an uneven structure having a wood grain pattern, cloth grain pattern, or the like may be selected.

[0034] From the viewpoint of preventing unnecessary peeling during use, the arithmetic mean roughness Ra of the surface of the uneven portion 22a is preferably 0.1 mm or more, more preferably 0.3 mm or more, and even more preferably 0.5 mm or more. From the viewpoint of facilitating peeling by hand after use, the arithmetic mean roughness Ra is preferably 5.0 mm or less, more preferably 3.0 mm or less, and even more preferably 1.0 mm or less. On the other hand, the arithmetic mean roughness Ra of the surface of the smooth portion 22b is usually about 0.01 to 0.1 mm.

[0035] From the viewpoint of preventing peeling of the film 3, the distance d between the concaves (or convexities) in the concave-convex portion 22a is preferably 1.5 mm or less, and more preferably 1.2 mm or less. From the viewpoint of reducing snagging or tearing when the film 3 is peeled off, the distance d is preferably 0.2 mm or more, and more preferably 0.3 mm or more.

[0036] In order to prevent peeling of the film 3, the ratio of the spacing between recesses to the depth of the recesses (or the ratio of the spacing between protrusions to the height of the protrusions) is preferably 0.5 to 5 times.

[0037] In addition, the wall surface of the recess or protrusion may be inclined with respect to the surface of the smooth portion 22b of the flange portion 22. The inclination angle θ is preferably 45° or more, more preferably 50° or more, but is usually 110° or less, and preferably 90° or less.

[0038] The uneven portion 22a may be provided in the flange portion 22 in an area other than a part that may cause peeling. The smooth portion 22b that may cause peeling may be provided in any position on the flange portion 22.

[0039] When the storage section 21 is rectangular, the smooth portion 22b is preferably located at at least one of the four corners of the flange section 22. The four corners make it easy to create an opening for peeling with the hand and to easily pinch the film 3 after peeling, making peeling easy. In this embodiment, the smooth portion 22b is provided at all four corners, and peeling can be done from any of the corners.

[0040] The uneven portion 22a may be disposed on the outer periphery side of the flange portion 22, and the smooth portion 22b may be disposed on the inner periphery side. When a lid material is provided on the container 1, the lid material is disposed so as to come into contact with the smooth portion 22b. In this case, the uneven portion 22a prevents the film 3 from peeling off during normal use, and the smooth portion 22b can provide a trigger for peeling after the lid material is removed.

[0041] <Thermoplastic resin> Examples of thermoplastic resins that can be used for the container body 2 include olefin-based resins, ester-based resins, and styrene-based resins.

[0042] Examples of olefin-based resins that can be used for the container body 2 include propylene-based resins with a density of 0.942 g / cm 3 More than 0.965g / cm 3 Examples of the resin include ethylene-based resins such as the following high-density polyethylene. From the viewpoint of suppressing drawdown, it is also preferable to blend 5 to 25% by mass of long-chain branched polypropylene in the polyolefin.

[0043] From the viewpoint of controlling thickness unevenness during molding of the container body forming sheet 2', the melt flow rate of the olefin resin is preferably 0.2 g / 10 min or more, more preferably 0.5 g / 10 min or more. On the other hand, from the viewpoint of suppressing drawdown, the melt flow rate is preferably 5.0 g / 10 min or less, more preferably 3.0 g / 10 min or less. The melt flow rate is a value measured in accordance with JIS K7210 under conditions of a heating temperature of 230°C and a load of 2.16 kgf.

[0044] Examples of ester-based resins that can be used for the container body 2 include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polylactic acid (PLA). Copolymers in which some of the monomers of these resins are replaced with comonomers such as isophthalic acid, naphthalene-2,6-dicarboxylic acid, adipic acid, trimethylene glycol, and 1,4-cyclohexanedimethanol can also be used. These comonomer-derived components may be contained in the ester-based resin in an amount of 1 to 25% by mass.

[0045] From the viewpoint of stable molding of the container body forming sheet 2', the intrinsic viscosity of the ester resin is preferably 0.5 dl / g or more, more preferably 0.6 dl / g or more. On the other hand, from the viewpoint of suppressing drawdown, the intrinsic viscosity is preferably 1.3 dl / g or less, more preferably 1.1 dl / g or less. The intrinsic viscosity is a value measured at a temperature of 30°C after dissolving 1.0 g of a sample in 100 ml of a mixed solvent in which phenol and tetrachloroethane are mixed in a weight ratio of 50:50.

[0046] From the viewpoint of moldability, the glass transition point (Tg) of the ester resin is preferably 40 to 110° C., and more preferably 50 to 100° C. The above glass transition point (Tg) is a value obtained by taking 5 mg of a sample from the container body-forming sheet 2′, melting it in nitrogen at 285° C. for 5 minutes, and then quenching the quenched material, and subjecting the quenched material to differential scanning calorimetry at a heating rate of 20° C. / min.

[0047] Examples of styrene-based resins that can be used for the container body 2 include general purpose polystyrene resins (GPPS: General Purpose PolyStyrene), rubber-modified polystyrene resins, and mixtures thereof. The general purpose polystyrene resins are usually styrene homopolymers. The rubber-modified polystyrene resins are also called high impact polystyrene (HIPS: High Impact Polystyrene).

[0048] The container body 2 may contain a filler. The content of the filler in the container body 2 is preferably 5% by mass or more, and more preferably 10% by mass or less, from the viewpoint of reducing the resin material in the container body 2. On the other hand, from the viewpoint of increasing the compression strength during molding, the content of the filler is preferably 60% by mass or less, and more preferably 50% by mass or less. As the filler, the same filler as that used in the film 3 described later can be used.

[0049] The container body 2 may be a foam. Examples of the foaming method include known methods such as chemical foaming, physical foaming, and supercritical foaming. From the viewpoint of reducing the weight of the container body 2, the foaming ratio is preferably 1.1 times or more, and more preferably 1.5 times or more. On the other hand, from the viewpoint of suppressing deformation, the foaming ratio is preferably 3 times or less, and more preferably 2 times or less.

[0050] The container body 2 may have a single-layer structure or a multi-layer structure. A multi-layer structure is preferable because the adhesive strength of the film 3 can be adjusted depending on the type of thermoplastic resin in the outermost layer.

[0051] (film) Since the film 3 is a thermoplastic resin film having excellent mechanical strength, it is easily adhered to the container body 2 and has excellent handleability as a packaging film after being peeled off.

[0052] <Thermoplastic resin> Examples of thermoplastic resins that can be used for the film 3 include olefin resins, ester resins, styrene resins, amide resins such as nylon-6, nylon-6,6, nylon-6,10, and nylon-6,12, vinyl chloride resins, and polycarbonate resins. These can be used alone or in combination of two or more. From the viewpoint of mechanical strength, the film 3 is preferably composed mainly of an olefin resin or an ester resin, and more preferably composed mainly of an olefin resin. The term "main component" means that the content in the film is more than 50% by mass.

[0053] Examples of olefin-based resins that can be used for the film 3 include propylene-based resins and ethylene-based resins. Among these, propylene-based resins are preferred from the viewpoints of formability and mechanical strength.

[0054] Examples of propylene-based resins include propylene homopolymers such as isotactic homopolypropylene and syndiotactic homopolypropylene obtained by homopolymerizing propylene, and propylene copolymers mainly composed of propylene and copolymerized with α-olefins such as ethylene, 1-butene, 1-hexene, 1-heptene, 1-octene, and 4-methyl-1-pentene, etc. The propylene copolymer may be a binary system or a multi-component system of ternary or higher components, and may be a random copolymer or a block copolymer.

[0055] Examples of ester-based resins that can be used for the film 3 include polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate.

[0056] <Filler> The film 3 may contain a filler. Examples of the filler include inorganic fillers and organic fillers. The inclusion of a filler facilitates the formation of a porous resin film. In addition, the whiteness or opacity of the film 3 may be increased. The filler contained in the film 3 may be one of the inorganic fillers or organic fillers described above, or a combination of two or more of them.

[0057] Among these, inorganic fillers are preferred from the viewpoints of cost and ease of particle size selection. Examples of inorganic fillers include inorganic particles such as heavy calcium carbonate, light calcium carbonate, titanium oxide such as rutile titanium dioxide, calcined clay, silica, diatomaceous earth, white earth, and talc. Among these, heavy calcium carbonate, clay, and diatomaceous earth are preferred because they have good pore formability and are inexpensive. In addition, for the purpose of improving dispersibility, the surface of the inorganic filler may be surface-treated with a surface treatment agent such as a fatty acid.

[0058] From the viewpoint of increasing the whiteness or opacity of the film 3, the filler content in the film 3 is preferably 10% by mass or more, and more preferably 15% by mass or more. Furthermore, from the viewpoint of increasing the uniformity of the molding of the film 3, the filler content in the film 3 is preferably 70% by mass or less, and more preferably 50% by mass or less.

[0059] From the viewpoint of easiness of forming pores, the average particle size of the filler is preferably 0.01 μm or more, more preferably 0.1 μm or more. From the viewpoint of imparting mechanical strength such as tear resistance, the average particle size of the filler is preferably 15 μm or less, more preferably 5 μm or less.

[0060] The average particle size of the inorganic filler is the volume average particle size corresponding to 50% cumulative volume (cumulative 50% particle size) measured with a particle measuring device, for example, a laser diffraction type particle size distribution measuring device (Microtrac, manufactured by Nikkiso Co., Ltd.).

[0061] <Other additives> If necessary, the film 3 may contain additives commonly used in the polymer field, such as an antifogging agent, a lubricant, an antiblocking agent, an antistatic agent, an antioxidant, a heat stabilizer, a light stabilizer, a weathering stabilizer, or an ultraviolet absorber, etc. The content of these additives in the film 3 is usually 0.01 to 5 mass % for each type of additive independently.

[0062] <Thickness and structure> From the viewpoint of preventing wrinkling or tearing during peeling, the thickness of the film 3 is preferably 20 μm or more, and more preferably 40 μm or more, while from the viewpoint of weight reduction, the thickness of the film 3 is preferably 200 μm or less, and more preferably 150 μm or less.

[0063] The film 3 may have a single layer structure or a multilayer structure. In the case of a multilayer structure, each layer can impart various functions such as white opacity, adhesion to the ink used in the printing layer, adhesion between the film 3 and the adhesive layer 4, and heat insulation.

[0064] The film 3 may be a non-stretched film or a stretched film. From the viewpoint of mechanical strength, the film 3 is preferably a stretched film, and more preferably a biaxially stretched film.

[0065] The surface of the film 3 may be activated by an activation treatment from the viewpoint of enhancing adhesion to adjacent layers. Examples of the activation treatment include corona discharge treatment, frame treatment, plasma treatment, glow discharge treatment, and ozone treatment. Among these, corona discharge treatment or frame treatment is preferred, and corona treatment is more preferred.

[0066] (adhesive layer) The adhesive layer 4 pseudo-adheres the film 3 to the container body 2. "Pseudo-adhesion" means that the adhesive strength is such that the film 3 does not peel off from the container body 2 during normal use, but the adhesive strength is such that the film 3 can be peeled off by hand when peeling it off.

[0067] Due to the pseudo-adhesion, the film 3 peels off at the interface between the film 3 and the adhesive layer 4 or at the interface between the adhesive layer 4 and the container body 2. Alternatively, the adhesive layer 4 undergoes cohesive failure, causing the film 3 to peel off.

[0068] The adhesive layer 4 can be formed by using a thermoplastic resin as its material and extruding the resin composition. Alternatively, the adhesive layer 4 can be formed by using a pressure-sensitive adhesive as its material and coating the pressure-sensitive adhesive.

[0069] <Thermoplastic resin> Thermoplastic resins that can be used for the adhesive layer 4 include the same thermoplastic resins as those used for the film 3.

[0070] From the viewpoint of sufficient adhesion between the film 3 and the container body 2, the thermoplastic resin of the adhesive layer 4 should have a density of 0.900 to 0.935 g / cm 3Preferred examples of such ethylene resins include low- or medium-density polyethylenes having a density of 0.880 to 0.940 g / cm3, linear low-density polyethylenes having a density of 0.880 to 0.940 g / cm3, metallocene-based polyethylenes produced using a metallocene catalyst, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid alkyl ester copolymers, ethylene-methacrylic acid alkyl ester copolymers having an alkyl group with a carbon number of 1 to 8, and metal salts of ethylene-methacrylic acid copolymers such as Zn, Al, Li, K, Na, etc., each having a melting point of 60 to 130° C. Among these, low- or medium-density polyethylenes having a crystallinity of 10 to 60% measured by an X-ray method and a number average molecular weight of 10,000 to 40,000, or linear low-density polyethylenes, are more preferred.

[0071] From the viewpoint of peelably adhering the film 3, it is preferable to use a thermoplastic resin that is incompatible with the surface layer of the container body 2 for the adhesive layer 4. Specifically, when the container body 2 is made of an olefin-based resin, it is preferable to use an ester-based resin, a styrene-based resin, or the like for the adhesive layer 4. Also, when the container body 2 is made of an ester-based resin or a styrene-based resin, it is preferable to use an olefin-based resin for the adhesive layer 4.

[0072] From the viewpoint of adjusting the adhesive strength, a compatible thermoplastic resin can be used in combination with a thermoplastic resin that is incompatible with the surface layer of the container body 2. For example, if sufficient adhesive strength cannot be obtained by using an olefin-based resin for the surface layer of the container body 2 and a styrene-based resin for the adhesive layer 4, the adhesive strength of the adhesive layer 4 to the container body 2 can be increased by using an olefin-based resin in combination with a styrene-based resin. From the viewpoint of pseudo-adhesion, the blending amount of the compatible thermoplastic resin used in combination with the incompatible thermoplastic resin is preferably 30 mass % or less, more preferably 20 mass % or less, of the total.

[0073] The melting point of the thermoplastic resin used in the adhesive layer 4 may be lower than that of the thermoplastic resin in the film 3. When the film 3, the adhesive layer 4, and the container body-forming sheet 2' are laminated by applying heat and pressure, lamination is possible without melting the film 3. In addition, when the container 1 is heated after use, the adhesive layer 4, which has a low melting point, melts, making it easier to peel off the film 3.

[0074] From the viewpoint of easily controlling the adhesive strength, the adhesive layer 4 may contain a tackifier or plasticizer. Examples of the tackifier include hydrogenated petroleum resins, aromatic hydrocarbon resins, and aliphatic hydrocarbon resins. Examples of the hydrogenated petroleum resins include partially hydrogenated petroleum resins. Examples of the aromatic hydrocarbon resins include terpene resins, rosin resins, and styrene resins. The tackifiers or plasticizers may be used alone or in combination of two or more kinds, but from the viewpoint of suppressing peeling of the adhesive layer 4 during normal use, it is preferable that they are highly compatible with the thermoplastic resin used in the adhesive layer 4.

[0075] When a thermoplastic resin is used, the thickness of the adhesive layer 4 is preferably 0.5 μm or more, more preferably 0.7 μm or more, and even more preferably 1 μm or more from the viewpoint of enhancing adhesiveness. From the viewpoint of suppressing cohesive failure inside the adhesive layer 4, the thickness is preferably 10 μm or less, and more preferably 6 μm or less.

[0076] <Adhesive> Examples of adhesives that can be used for the adhesive layer 4 include acrylic adhesives, silicone adhesives, urethane adhesives, and rubber adhesives. These can be used alone or in combination of two or more. Among them, acrylic adhesives and silicone adhesives are preferred because they are less likely to deteriorate or emit odors due to heat during thermoforming.

[0077] When a pressure-sensitive adhesive layer is used, the thickness of the adhesive layer 4 is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more from the viewpoint of enhancing adhesiveness. From the viewpoint of suppressing cohesive failure inside the adhesive layer 4, the thickness of the adhesive layer 4 is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less.

[0078] <Other additives> If necessary, the adhesive layer 4 may contain the same additives as the film 3 .

[0079] (Printing layer) The container 1 may be provided with a printed layer by printing on the container body 2 or the film 3. From the viewpoint of facilitating recycling of the container body 2, it is preferable that the film 3 is printed and the container body 2 is not printed.

[0080] Any surface of the container body 2 can be printed, but from the standpoint of avoiding contact with the contents, particularly food, it is preferable that the printed layer be provided below the surface layer. When printing is applied to the film 3, from the viewpoint of stabilizing the peel strength of the film 3, printing can be applied to the surface of the film 3 opposite the adhesive layer 4. From the viewpoint of avoiding contact with the contents, particularly food, it is preferable to apply a printed layer to the surface of the film 3 on the adhesive layer 4 side.

[0081] Examples of the printed information include product names, product indications such as logos, manufacturer names, sales company names, usage instructions, bar codes, etc. Examples of the printing method include gravure printing, offset printing, flexographic printing, seal printing, screen printing, etc.

[0082] [Container manufacturing method] (One-piece molding manufacturing method) The manufacturing method of the container 1 is not particularly limited, but it can be manufactured, for example, by laminating an adhesive layer 4, which is a thermoplastic resin film, and a film 3 in that order on a sheet 2' for forming the container body, and then thermoforming the laminate as a whole.

[0083] <Forming of film or sheet> Examples of methods for forming a monolayer film or sheet include cast molding, in which a molten resin is extruded into a sheet shape using a monolayer or multilayer T-die, I-die, or the like connected to a screw-type extruder, calendar molding, rolling molding, inflation molding, etc. A film or sheet may be formed by casting or calendar molding a mixture of a resin and an organic solvent or oil, and then removing the solvent or oil.

[0084] Examples of the method for laminating the film or sheet include a coextrusion method, an extrusion lamination method, a coating method, a thermal lamination method, and the like, and these methods can also be combined. In the co-extrusion method, the resin compositions of each layer are melt-kneaded in separate extruders and then laminated and extruded in a feed block or multi-manifold, and film formation and lamination are performed in parallel. In the extrusion lamination method, a resin composition is extruded onto a pre-formed film to form and laminate another film. In the coating method, a resin solution, emulsion or dispersion is coated onto a film and dried to form and laminate another film. In the thermal lamination method, a film of the adhesive layer 4 is sandwiched between a film and a sheet, heated, and bonded together.

[0085] <Stretching> Each film and sheet may be stretched individually before lamination, or may be stretched together after lamination, or the unstretched film and the stretched film may be stretched again after lamination.

[0086] Examples of the stretching method that can be used include a longitudinal stretching method that utilizes the difference in peripheral speed between a group of rolls, a transverse stretching method that utilizes a tenter oven, a sequential biaxial stretching method that combines these, a rolling method, a simultaneous biaxial stretching method that utilizes a combination of a tenter oven and a pantograph, a simultaneous biaxial stretching method that utilizes a combination of a tenter oven and a linear motor, etc. Also usable is a simultaneous biaxial stretching (inflation molding) method in which a molten resin is extruded into a tube shape using a circular die connected to a screw-type extruder and then air is blown into the extruded resin.

[0087] From the viewpoint of suppressing distortion or sinking of the container body 2 after thermoforming, it is preferable to heat the laminate before thermoforming to relieve stress.

[0088] <Thermoforming> Examples of the thermoforming method include known techniques using a general vacuum forming machine, a pressure forming machine, or a vacuum pressure forming machine. For example, in a vacuum forming machine, a laminate of a container body forming sheet 2', an adhesive layer 4, and a film 3 is heated and then placed in a mold with holes. The laminate is molded by adhering it to the mold by sucking through the holes. In a pressure forming machine, a pressure box is provided to pressurize the inside, or the laminate is sandwiched between two pieces of laminate and pressed against the mold using both vacuum and pressure. This transfers the mold shape to the softened laminate. The laminate is then cooled by blowing air on it for a few seconds. In a vacuum pressure forming machine, one side of the laminate is heated with a hot plate and compressed.

[0089] The thermoforming conditions can be ordinary thermoforming conditions. Examples of the heating method include radiant heat from a heater, steam heating, and the like. Heating may be performed from one side of the laminate, or from both sides of the container body forming sheet 2'. Among them, the method of heating from both sides of the container body forming sheet 2' is preferred because it allows stable molding of complex shapes. The sheet temperature is preferably, for example, 10 to 30°C lower than the melting point of the material of the container body forming sheet 2'. For example, polypropylene is heated to about 160°C, and polyethylene terephthalate (PET) is heated to about 250°C.

[0090] After the molded container 1 is removed from the mold, unnecessary portions are removed by punching with a punching blade if necessary. The removed unnecessary portions can be crushed and reused.

[0091] (Manufacturing method by bonding) The container 1 can also be produced by thermoforming the container body 2 alone, applying an adhesive to the surface of the film 3 to form the adhesive layer 4, and then bonding the container body 2 and the film 3 together.

[0092] <Adhesive coating> After forming the film 3, an adhesive is applied to the film 3 to form the adhesive layer 4. The adhesive can be applied using a coating device such as a roll coater, a blade coater, a bar coater, an air knife coater, a size press coater, a gravure coater, a die coater, a lip coater, or a spray coater.

[0093] <Film bonding> The film 3 coated with an adhesive is heated and placed so as to cover the opening of the container body 2. Air pressure is then applied to make the film 3 adhere to the container body 2. This allows the film 3 to be bonded in close contact with the top surface of the container body 2. Alternatively, a vacuum hole may be provided in the container body 2, and the film 3 may be adhered to the container body 2 by suction from the container body 2 side.

[0094] [Container use] The use of the container 1 is not particularly limited, and it can be used, for example, as a packaging container for food such as prepared foods and boxed lunches sold in stores, parts used at manufacturing sites, transport trays for semiconductors and the like, sales containers, etc. In particular, the container 1 in which the bag body 5 can be formed from the peeled film 3 is suitable for use as food. When storing or disposing of the food in the container 1, the food can be protected by the bag body 5, and can be disposed of without getting the hands dirty.

[0095] [Packaging film or bag] The film 3 peeled off from the container 1 can be used as a packaging film to protect the contents of the container 1. The film 3 can also be used as a bag 5 by bundling the ends of the film 3. For example, leftover food in the container 1 can be stored in the bag 5, or unused parts on the container 1 can be stored in the bag 5, which is highly convenient. The opening of the bag 5 can be closed with a fastener such as a rubber band, a string, or a closure. The bottom of the bag 5 has a smaller area than the bottom of the container 1, allowing it to be stored compactly. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the terms "parts", "%", and the like are based on mass unless otherwise specified.

[0097] [Laminated film (a1)] 84% by mass of propylene homopolymer (manufactured by Japan Polypropylene Corporation, product name: Novatec PP MA4, MFR (230°C, 2.16 kg load): 5 g / 10 min, melting point: 167°C), 15% by mass of heavy calcium carbonate fine powder (manufactured by Bihoku Funka Kogyo Co., Ltd., product name: Softon #1800, volume average particle size: 1.8 μm), and 1% by mass of rutile-type titanium dioxide fine powder (manufactured by Ishihara Sangyo Co., Ltd., product name: Typaque CR-60, volume average particle size: 0.2 μm) were mixed in a mixer. Next, the mixture was melt-kneaded at 230°C using an extruder to prepare a resin composition for film.

[0098] The resin composition for the film was melt-kneaded in an extruder set at 240° C. Meanwhile, 100% by mass of high impact polystyrene (manufactured by PS Japan, product name: H9152, MFR (200° C., 5 kg load): 5.5 g / 10 min) was melt-kneaded in a separate extruder set at 240° C. to prepare a resin composition for the adhesive layer.

[0099] Each melt-kneaded resin composition was fed to one co-extrusion T-die, laminated in two layers in the T-die, and extruded from the T-die at 240°C into a film. As a result, a two-layer film was obtained in which a film made of polypropylene and a filler and an adhesive layer made of high impact polystyrene were laminated. The two-layer film was cooled by a cooling device to obtain a two-layer non-stretched film. The obtained non-stretched film was heated to 150°C and stretched 5 times in the longitudinal direction by utilizing the peripheral speed difference between a plurality of roll groups. Next, after cooling to a temperature of 60°C, it was heated again to a temperature of 150°C and stretched 8 times in the transverse direction by using a tenter. After annealing at a temperature of 160°C, it was cooled to a temperature of 60°C to obtain a two-layer structure white opaque laminated film (a1). The total thickness of the laminated film (a1) was 80μm (5μm / 75μm).

[0100] [Laminated film (a2)] A laminate film (a2) having a total thickness of 80 μm (5 μm / 75 μm) was obtained in the same manner as laminate film (a1), except that the adhesive layer was formed by mixing high impact polystyrene (HIPS) used as the resin for the adhesive layer in laminate film (a1) and propylene homopolymer (manufactured by Japan Polypropylene, product name: Novatec PP MA4) in a ratio of 95% by mass:5% by mass.

[0101] [Laminated film (a3)] A laminate film (a3) ​​having a total thickness of 80 μm (5 μm / 75 μm) was obtained in the same manner as laminate film (a1), except that the high impact polystyrene (HIPS) used as the resin for the adhesive layer in laminate film (a1) and a propylene homopolymer (manufactured by Japan Polypropylene, product name: Novatec PP MA4) were mixed in a ratio of 50% by mass:50% by mass to form an adhesive layer.

[0102] [Laminated film (a5)] A resin composition for a film was prepared by melt-kneading 100% by mass of polypropylene (manufactured by Japan Polypropylene Corporation, product name: MA3U, MFR (230° C., 2.16 kg load): 15 g / 10 min) at 230° C. using an extruder. On the other hand, an ethylene-methyl methacrylate copolymer (manufactured by Sumitomo Chemical Co., Ltd., product name: Acryft WH206-F, MMA content 20 wt%, MFR: 2 g / 10 min) was mixed as the resin for the adhesive layer in a ratio of 70% by mass:30% by mass with a tackifier (manufactured by Harima Chemical Co., Ltd., product name: Haritac SE10, stabilized rosin ester, softening point: 78-87°C, acid value: 2-10 g KOH). This was melted in an extruder heated to 150°C to prepare a composition for the adhesive layer.

[0103] Each melt-kneaded resin composition was fed to one co-extrusion T-die, laminated in two layers in the T-die, and extruded from the T-die at 240°C to obtain a two-layer film. The two-layer film was cooled by a cooling device to obtain a two-layer non-stretched film. The obtained non-stretched film was heated to 150°C and stretched 5 times in the longitudinal direction by utilizing the peripheral speed difference between a plurality of roll groups. After cooling to a temperature of 60°C, it was heated again to a temperature of 150°C and stretched 8 times in the transverse direction by using a tenter. After annealing at a temperature of 160°C, it was cooled to a temperature of 60°C to obtain a two-layer white opaque laminated film (a5). The total thickness of the laminated film (a5) was 80μm (5μm / 75μm).

[0104] [Sheet for forming container body (b1)] 70% by mass of propylene homopolymer (manufactured by Japan Polypropylene Corporation, product name: Novatec PP EA9, MFR (230°C, 2.16 kg load): 0.5 g / 10 min, melting point: 167°C), 28% by mass of heavy calcium carbonate fine powder (manufactured by Bihoku Funka Kogyo Co., Ltd., product name: Softon #1800, volume average particle size: 1.8 μm), and 2% by mass of rutile-type titanium dioxide fine powder (manufactured by Ishihara Sangyo Co., Ltd., product name: Typaque CR-60, volume average particle size: 0.2 μm) were mixed in a mixer. Next, the mixture was melt-kneaded at 230°C using an extruder to prepare a resin composition for the base layer. Meanwhile, 100% by mass of propylene homopolymer (manufactured by Japan Polypropylene Corporation, product name: Novatec PP EA9) was melt-kneaded at 230°C using another extruder to prepare a resin composition for the skin layer.

[0105] The melt-kneaded resin composition for the base layer and the resin composition for the skin layer were fed to one co-extrusion T-die, laminated in the T-die to form a three-layer structure of skin layer / base layer / skin layer, and extruded from the T-die into a sheet at 240°C. This three-layer sheet was guided between a semi-mirror chill roll and a matte rubber roll, and cooled while being pinched (linear pressure of about 15 N / cm). After cutting off the edge portions, the sheet was wound up by a winder to obtain a container body forming sheet (b1). The container body forming sheet (b1) was a three-layered white polyolefin resin sheet with a total thickness of 250 μm (10 μm / 230 μm / 10 μm).

[0106] [Sheet for forming container body (b2)] An A-PET sheet (transparent amorphous polyethylene terephthalate resin sheet, manufactured by RP Toho Plastics, product name: NOACRYSTAL-V, thickness 300 μm) was used as the container body forming sheet (b2).

[0107] [Raw materials] Table 1 shows the list of raw materials used in the above preparation. [Table 1]

[0108] [Example 1] The chrome-plating drum dryer was heated to 95°C with steam, and the laminated film (a1) and the container body forming sheet (b1) were passed through the drum dryer side in the order of container body forming sheet / laminated film. The laminated film was heated from the side with an infrared heater, and the sheet surface temperature measured with a radiation thermometer was controlled to be about 140°C. The laminate was then nipped with a water-cooled chill roll at a linear pressure of about 20 N / cm and air-cooled to room temperature, and the resulting laminate was wound up.

[0109] The laminate was then unwound, heated, and vacuum molded using a thermoforming die. For the vacuum molding, a small vacuum molding machine with an upper heater heating system and a molding area of ​​500 mm x 500 mm was used. (Thermoforming mold) As the thermoforming mold, a vacuum forming mold was used with a square bottom surface measuring 140 mm x 58 mm and a depth of 35 mm. The bottom surface was an approximately rectangular shape with four corners in the shape of an arc with a radius of 5 mm, and the taper angle of the inner wall surface relative to the bottom surface was 30 degrees. The four corners of the outer periphery of the mold part forming the flange portion were formed in an arc shape with a radius of 15 mm. In addition, a concave-convex structure having a diamond-shaped pattern with inner angles of 30 degrees and 60 degrees was provided on the surface of the mold part forming the flange portion. The interval between the concaves in this concave-convex structure was 1 mm, and the depth of the concaves was 0.5 mm.

[0110] During thermoforming, the uneven structure of the mold part forming the four corners of the flange part was filled with silicone resin. As a result, uneven parts were formed in the area of ​​the flange part except for the four corners. The thermoformed body was removed from the vacuum forming machine, and the outer periphery of the flange part was trimmed to produce the container of Example 1. The arithmetic mean roughness Ra of the uneven part of the flange part was measured by a surface roughness meter and found to be 0.52 mm.

[0111] [Example 2] A container of Example 2 was produced in the same manner as in Example 1, except that the laminate film (a1) used in Example 1 was changed to the laminate film (a2).

[0112] [Comparative Example 1] The container of Comparative Example 1 was manufactured in the same manner as in Example 1, except that the laminate film (a1) was replaced with the laminate film (a3) ​​and the uneven structure of the mold was not filled during thermoforming but was used as is to form an uneven portion over the entire flange portion.

[0113] [Comparative Example 2] The container of Comparative Example 2 was manufactured in the same manner as in Example 1, except that the laminated film (a1) was replaced with the laminated film (a5), the container body forming sheet (b1) was replaced with the container body forming sheet (b2), and the uneven structure of the mold was not filled during thermoforming but was used as it was to form uneven portions over the entire flange portion.

[0114] [Comparative Example 3] The container of Comparative Example 3 was manufactured in the same manner as in Example 1, except that the uneven structure on the surface forming the flange portion of the thermoforming mold used in Example 1 was filled with silicone resin and then thermoformed, and no uneven portion was formed on the flange portion.

[0115] [evaluation] The containers of each of the Examples and Comparative Examples were evaluated as follows.

[0116] (Adhesive strength) A test piece of 60 mm x 15 mm was cut out from the flange of the molded container. When the flange had a concave-convex portion 22a, the test piece was cut out so as to include a portion with the concave-convex portion 22a and a portion without the concave-convex portion 22a. Three test pieces were taken from one container. Using this test piece, a 180-degree peel test was performed in accordance with JISZ 0238:1998 (Test method for heat-sealed soft packaging bags and semi-rigid containers).

[0117] One end of the test piece was peeled off by 10 mm to separate it into a film and a sheet, and an auxiliary piece of 80 mm x 15 mm was attached to the film with cellophane tape. One end of the separated sheet side of the test piece was fixed to the lower chuck of a universal testing machine (manufactured by Shimadzu Corporation, model: AG-100kNXplus), and the auxiliary piece was fixed to the upper chuck. Next, peeling was performed at a tensile speed of 300 mm / min and an angle of 180 degrees, and the maximum load was recorded. The average value of the measured values ​​for the three test pieces was evaluated as the adhesive strength of the film (N / 15 mm). The adhesive strength of the test piece partially provided with the uneven portion 22a is the adhesive strength of the entire flange portion 2 including the uneven portion 22a and the smooth portion 22b.

[0118] (Manual peel test) The difficulty of starting to peel off the surface film from the containers of each Example and Comparative Example was evaluated sensorily as follows. Excellent: Already peeled off and can be peeled off without using fingernails Possible: Can be peeled off by using a fingernail Not possible: Cannot be peeled off even with a fingernail

[0119] (Actual use test) Two apples were placed in each of the containers of the Examples and Comparative Examples, and the tops of the samples were covered with plastic wrap. The samples were packed in cardboard boxes as a set of two and transported by courier. After arrival, the containers were opened, and it was visually confirmed that the film had risen from the container body at the flange. Excellent: No bumps on uneven areas, bumps on smooth areas Good: The floating area on the smooth surface has spread, and there is also floating on the uneven surface, but there is no floating on the inner surface of the housing part inside the flange. Unacceptable: The floating has progressed to the inner surface of the housing part inside the flange part.

[0120] Table 2 shows the evaluation results. [Table 2]

[0121] As shown in Table 2, according to Examples 1 and 2, by providing the flange of the container with an uneven portion, it is difficult to peel off in actual use, but can be easily peeled off by hand. On the other hand, in Comparative Examples 1 and 2, in which the entire flange is provided with an uneven portion, the adhesive strength was strong and it was difficult to peel off by hand. Comparative Example 3, which has no uneven portion, was easy to peel off, but peeled off during use. [Explanation of symbols]

[0122] 1 container, 2 container body, 22 flange portion, 22a uneven portion, 22b smooth portion, 3 film, 4 adhesive layer

Claims

1. A container having a film made of a thermoplastic resin bonded to the top surface of a container body made of a thermoplastic resin, The container body is rectangular and has a flange portion, The flange surface includes an uneven portion having an uneven structure and a smooth portion not having the uneven structure, The smooth portion is located at at least one of the four corners of the flange portion, The arithmetic mean roughness (Ra) of the surface of the uneven portion is 0.1 to 3.0 mm. container.

2. The adhesive strength of the film in the entire flange portion including the uneven portion and the smooth portion is 0.5 to 20 N / 15 mm.

2. The container of claim 1.

3. An adhesive layer is provided between the film and the container body.

3. A container according to claim 1 or 2.

4. The adhesive strength of the film at the flat portion is less than 0.5 N / 15 mm. A container according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • The composite structure of synthetic resin article

    JP1992111429U

  • Container

    JP1995187192A

  • Multi-layer container

    JP1996258830A

  • Easy recycling container

    JP2000225662A

  • Biodegradable resin film laminate and container using the same

    JP2002187241A