Method for producing photoluminescent materials
By extracting silver atoms from zeolites using a cationic aqueous solution, the method produces photoluminescent materials with reduced silver content, maintaining emission intensity and preventing discoloration, addressing the issue of high silver content materials turning colored when mixed with resins or rubbers.
Patent Information
- Application Number
- JP2020101648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-06-11
AI Technical Summary
Photoluminescent materials containing high silver atom content often turn colored when mixed with resin or rubber, leading to reduced emission intensity.
A method to produce photoluminescent materials with reduced silver atom content by extracting silver atoms from zeolites using an aqueous solution containing cations other than silver ions and ammonia, converting non-emissive silver atoms into ammine complexes and replacing them with other cations.
The method results in a photoluminescent material with maintained or enhanced emission intensity and prevents discoloration when mixed with resins or rubbers, while potentially reducing production costs by recovering silver.
Smart Images

Figure 0007591778000001 
Figure 0007591778000002 
Figure 0007591778000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a photoluminescent material. Here, the term "photoluminescent material" means a material used in applications that utilize photoluminescence (i.e., the phenomenon of emitting visible light when irradiated with light). [Background technology]
[0002] Photoluminescent materials that emit visible light when irradiated with light are used in lighting devices, backlights for liquid crystal devices, plasma displays, and the like.
[0003] Various photoluminescent materials have been developed so far. For example, Patent Document 1 discloses a photoluminescent material that is a faujasite-type zeolite containing silver atoms (silver ions). Patent Documents 2 to 4 disclose photoluminescent materials that are A-type zeolite containing silver atoms (silver ions). Patent Document 5 discloses a photoluminescent material that is a sodalite containing silver atoms. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-52102 A [Patent Document 2] JP 2014-37492 A [Patent Document 3] International Publication No. 2017 / 209033 [Patent Document 4] JP 2018-197296 A [Patent Document 5] International Publication No. 2016 / 190356 Summary of the Invention [Problem to be solved by the invention]
[0005] In photoluminescent materials containing silver atoms as described in Patent Documents 1 to 5, if the content of silver atoms is high, the mixture obtained may be colored when mixed with resin or rubber. The present invention has been made in view of such circumstances, and its purpose is to produce a photoluminescent material with a reduced content of silver atoms. [Means for solving the problem]
[0006] The present invention capable of achieving the above object is as follows. [1] A method for producing a photoluminescent material that emits visible light when irradiated with light, comprising the steps of: The method includes obtaining a photoluminescent material II having a reduced content of silver atoms by extracting silver atoms from a photoluminescent material I containing silver atoms in an aqueous solution containing cations other than silver ions and ammonia; and The method wherein the photoluminescent material I is a zeolite containing silver atoms. [2] The method according to [1] above, wherein the photoluminescent material I is at least one selected from the group consisting of faujasite-type zeolite containing silver atoms, A-type zeolite containing silver atoms, and sodalite containing silver atoms. [3] The method according to [2] above, wherein the faujasite-type zeolite containing silver atoms is a faujasite-type zeolite containing 5% by weight or more and 30% by weight or less of silver ions. [4] The method according to [2] or [3], wherein the A-type zeolite containing silver atoms is an A-type zeolite containing 2.5% by weight or more and 40% by weight or less of silver ions. [5] The method according to any one of the above [2] to [4], wherein the sodalite containing silver atoms is sodalite containing 0.25% by weight or more and 51% by weight or less of silver atoms. [6] The method according to any one of [1] to [5] above, wherein the cations other than silver ions include alkali metal ions and / or alkaline earth metal ions. [7] The method according to any one of the above [1] to [6], wherein the ratio of the silver atom content in the photoluminescent material II to the silver atom content in the photoluminescent material I (silver atom content in the photoluminescent material II / silver atom content in the photoluminescent material I) is 3 / 100 to 9 / 10. [8] A photoluminescent material produced by the method according to any one of [1] to [7] above. Effect of the Invention
[0007] According to the present invention, photoluminescent materials can be produced that have a reduced content of silver atoms. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] One of the features of the present invention is to obtain a photoluminescent material II with a reduced content of silver atoms by extracting silver atoms from a photoluminescent material I containing silver atoms in an aqueous solution containing cations other than silver ions and ammonia. It is presumed that such an operation causes silver atoms (silver ions or silver clusters) at sites in the photoluminescent material I that do not contribute to light emission to be converted into ammine complexes and dissolved in the aqueous solution, and cations other than silver ions in the aqueous solution are incorporated into the photoluminescent material in place of the dissolved silver atoms, resulting in the production of a photoluminescent material II with a reduced content of silver atoms. However, the present invention is not limited to such a presumed mechanism.
[0009] The reduction in the content of silver atoms can be confirmed, for example, by measurement using a wavelength dispersive X-ray fluorescence apparatus, which can also measure the content of each atom (each cation) in the photoluminescent material.
[0010] A mixture obtained by mixing a photoluminescent material with a high content of silver atoms with a resin or rubber has a problem that the mixture turns black and the luminescence intensity decreases. On the other hand, a photoluminescent material with a reduced content of silver atoms can suppress such discoloration and the decrease in luminescence intensity. In addition, if the method of the present invention can recover the silver dissolved in the aqueous solution and use it in the production of a photoluminescent material, a reduction in production costs can be expected.
[0011] As shown in the following Examples and Comparative Examples, the emission intensity of photoluminescent material II obtained by reducing the content of silver atoms in photoluminescent material I was surprisingly equal to or greater than that of photoluminescent material I. Here, "the emission intensity of photoluminescent material II is equal to that of photoluminescent material I" means that the relative emission intensity of photoluminescent material II, calculated assuming that the emission intensity of photoluminescent material I is 1, is within the range of 0.9 to 1.1.
[0012] The photoluminescent material I used in the present invention can be produced by ion exchange of zeolite, which is a raw material. This ion exchange can be carried out by stirring and holding zeolite in a silver ion-containing aqueous solution. Examples of the silver ion-containing aqueous solution include a silver nitrate aqueous solution. If it is necessary to contain ions other than silver ions (hereinafter sometimes abbreviated as "other ions") in the photoluminescent material I, the other ions may be present in the silver ion-containing aqueous solution used for ion exchange, or ion exchange using a silver ion-containing aqueous solution and ion exchange using an aqueous solution containing other ions may be carried out sequentially. Examples of the aqueous solution containing other ions include a zinc sulfate aqueous solution, a calcium nitrate aqueous solution, a magnesium sulfate aqueous solution, and a potassium sulfate aqueous solution. In addition, the concentration of silver ions and other ions in the aqueous solution can be appropriately adjusted according to the design value of the content of silver ions and other ions in the photoluminescent material I. The ion exchange can be carried out at room temperature. The time for ion exchange (i.e., the stirring and holding time of zeolite in the ion-containing aqueous solution) is usually 30 minutes or more and 10 hours or less, and preferably 5 hours or less.
[0013] When the zeolite, which is the raw material of the photoluminescent material I, is a faujasite-type zeolite or an A-type zeolite, it is preferable to filter the ion-exchanged zeolite from the ion-containing aqueous solution, wash it with water, and then dry it. Drying can be performed in an air atmosphere, an inert gas (e.g., nitrogen gas) atmosphere, or a reduced pressure atmosphere. Among these, drying in an air atmosphere is preferable because it allows simple operation. The drying time is usually 1 hour or more and 30 hours or less, and preferably 20 hours or less. The drying temperature is preferably 300° C. or less, more preferably 200° C. or less, and preferably 50° C. or more, more preferably 100° C. or more. The drying conditions can be appropriately adjusted depending on the type of zeolite used.
[0014] The dried A-type zeolite may be further subjected to a heat treatment such as calcination. The heat treatment may be performed in an air atmosphere, an inert gas (e.g., nitrogen gas) atmosphere, or a reduced pressure atmosphere. Heat treatment in an air atmosphere is preferred because the operation can be easily performed. The heat treatment temperature is preferably 180°C or higher, more preferably 200°C or higher, and preferably 300°C or lower, more preferably 250°C or lower. The heat treatment time is preferably 1 hour or higher, more preferably 2 hours or higher, and preferably 10 hours or lower, more preferably 5 hours or lower.
[0015] When the zeolite used as the raw material of the photoluminescent material I is sodalite, it is preferable to filter the ion-exchanged sodalite from the ion-containing aqueous solution, wash it with water, and then heat-treat it. The heat treatment may be performed under an inert gas (e.g., nitrogen gas) atmosphere or under air atmosphere. The heat treatment temperature is preferably 50°C or higher and 850°C or lower, more preferably 150°C or higher and 600°C or lower, and can be appropriately adjusted depending on the type of the photoluminescent material I produced from the sodalite. The heat treatment time is preferably 1 hour or higher and 24 hours or lower, more preferably 2 hours or higher and 24 hours or lower.
[0016] The photoluminescent material I used in the present invention is preferably A faujasite-type zeolite containing silver atoms (hereinafter sometimes abbreviated as "photoluminescent material I-1"); A type zeolite containing silver atoms (hereinafter sometimes abbreviated as "photoluminescent material I-2"), and Sodalite containing silver atoms (hereinafter sometimes abbreviated as "photoluminescent material I-3") It is at least one selected from the group consisting of: Photoluminescent material I-1 to photoluminescent material I-3 will be explained in order below.
[0017] First, as a photoluminescent material I-1 containing faujasite-type zeolite, for example, one described in Patent Document 1 can be mentioned. Examples of faujasite-type zeolite include synthetic zeolites X-type and Y-type zeolite, and natural zeolite faujasite. Among these, X-type zeolite is preferred.
[0018] The average particle size of the faujasite-type zeolite, the photoluminescent material I-1 obtained from the faujasite-type zeolite, and the photoluminescent material II obtained from the photoluminescent material I-1 is preferably 0.1 μm or more and 2 μm or less, more preferably 0.5 μm or more and 1.5 μm or less. These average particle sizes can be measured by laser diffraction and laser scattering methods.
[0019] Faujasite-type zeolites (faujasite, X-type zeolite and Y-type zeolite) are commercially available and are readily available.
[0020] The photoluminescent material I-1 is preferably a faujasite-type zeolite containing 5% to 30% by weight of silver ions, and more preferably, the silver ion content is 7% to 20% by weight.
[0021] In the present invention, the content of silver atoms in the photoluminescent material I or II is a value based on the entire photoluminescent material I or II. The same applies to the contents of other atoms or ions.
[0022] The photoluminescent material I-1 may contain ions other than silver ions (hereinafter, sometimes abbreviated as "other ions"). The other ions may be used alone or in combination of two or more kinds.
[0023] The other ions contained in the photoluminescent material I-1 can be introduced into the photoluminescent material I-1 by ion exchange using an aqueous metal salt solution containing the other ions.
[0024] Examples of other ions contained in the photoluminescent material I-1 include alkali metal ions such as sodium ions and potassium ions, alkaline earth metal ions such as calcium ions and magnesium ions, and zinc ions, etc. Among these, the photoluminescent material I-1 containing calcium ions is preferred because it increases the luminescence intensity.
[0025] When the photoluminescent material I-1 contains other ions, the content of each of them is preferably 1% by weight or more and 10% by weight or less.
[0026] Next, a photoluminescent material I-2 containing A-type zeolite will be described. The average particle size of the A-type zeolite, the photoluminescent material I-2 obtained from the A-type zeolite, and the photoluminescent material II obtained from the photoluminescent material I-2 is preferably 0.1 μm or more and 20 μm or less, more preferably 0.5 μm or more and 15 μm or less. Type A zeolites are commercially available and readily available.
[0027] The photoluminescent material I-2 is preferably an A-type zeolite containing 2.5% by weight to 40% by weight of silver ions, more preferably A type zeolite containing silver ions and zinc ions, the silver ion content being 2.5% by weight or more and 30% by weight or less, the zinc ion content being 0.5% by weight or more and 15% by weight or less, and the total content of silver ions and zinc ions being 5% by weight or more and 35% by weight or less (hereinafter sometimes abbreviated as "photoluminescent material I-2a"); A type zeolite containing at least one selected from the group consisting of cesium ions and rubidium ions, silver ions and zinc ions, wherein the total content of at least one selected from the group consisting of cesium ions and rubidium ions is 1% by weight or more and 25% by weight or less, the silver ion content is 2.5% by weight or more and 30% by weight or less, and the zinc ion content is 0.5% by weight or more and 15% by weight or less (hereinafter may be abbreviated as "photoluminescent material I-2b"); and A type zeolite containing silver ions and ammonium ions, the silver ion content being 5% by weight or more and 40% by weight or less, and the ammonium ion content being 0.1% by weight or more and 25% by weight or less (however, A type zeolite containing zinc ions is excluded) (hereinafter sometimes abbreviated as "photoluminescent material I-2c"); It is at least one selected from the group consisting of: Photoluminescent material I-2a to photoluminescent material I-2c will be described below in order.
[0028] Examples of the photoluminescent material I-2a include those described in Patent Document 2. The silver ion content in the photoluminescent material I-2a is more preferably 3.5% by weight or more and 20% by weight or less.
[0029] The zinc ion content in the photoluminescent material I-2a is more preferably 5% by weight or more and 7% by weight or less.
[0030] The total content of silver ions and zinc ions in the photoluminescent material I-2a is more preferably 10% by weight or more and 25% by weight or less.
[0031] The molar ratio of silver ions:zinc ions in the photoluminescent material I-2a is preferably from 1:45 to 8:1, more preferably from 1:5 to 2:1.
[0032] The photoluminescent material I-2a may contain ions other than silver ions and zinc ions (hereinafter sometimes abbreviated as "other ions"). The photoluminescent material I-2a may contain one type of other ion, or may contain two or more types of other ions.
[0033] Other ions contained in the photoluminescent material I-2a can be introduced into the photoluminescent material I-2a by ion exchange with an aqueous solution of a salt containing the other ions.
[0034] Examples of other ions contained in the photoluminescent material I-2a include alkali metal ions such as sodium ions and potassium ions, alkaline earth metal ions such as calcium ions and magnesium ions, and ammonium ions. Among these, ammonium ions are preferred.
[0035] When the photoluminescent material I-2a contains other ions (eg, ammonium ions), the content of each of these ions is preferably 1% by weight or more and 10% by weight or less.
[0036] An example of the photoluminescent material I-2b is described in Patent Document 3. The photoluminescent material I-2b contains at least one ion selected from the group consisting of cesium ions and rubidium ions, and preferably contains cesium ions.
[0037] The total content of at least one selected from the group consisting of cesium ions and rubidium ions in the photoluminescent material I-2b (when there is only one of them, the content thereof) is more preferably 2% by weight or more and 23% by weight or less.
[0038] The silver ion content in the photoluminescent material I-2b is more preferably 3.5% by weight or more and 28% by weight or less.
[0039] The zinc ion content in the photoluminescent material I-2b is more preferably 5% by weight or more and 13% by weight or less.
[0040] The photoluminescent material I-2b may contain ions other than cesium ions, rubidium ions, silver ions, and zinc ions (hereinafter sometimes abbreviated as "other ions"). The photoluminescent material I-2b may contain one type of other ion, or may contain two or more types of other ions.
[0041] Other ions contained in the photoluminescent material I-2b can be introduced into the photoluminescent material I-2b by ion exchange with an aqueous solution containing the other ions.
[0042] Examples of other ions contained in the photoluminescent material I-2b include ammonium ions, sodium ions, potassium ions, calcium ions, and magnesium ions.
[0043] Examples of photoluminescent material I-2c include those described in Patent Document 4. The silver ion content in photoluminescent material I-2c is more preferably 7% by weight or more and 35% by weight or less.
[0044] The content of ammonium ions in the photoluminescent material I-2c is preferably 0.1% by weight to 25% by weight, more preferably 1% by weight to 15% by weight.
[0045] The total content of silver ions and ammonium ions in the photoluminescent material I-2c is preferably 6% by weight or more and 40% by weight or less, more preferably 10% by weight or more and 35% by weight or less.
[0046] The photoluminescent material I-2c may contain ions other than silver ions and ammonium ions (excluding zinc ions) (hereinafter, sometimes abbreviated as "other ions"). The photoluminescent material I-2c may contain one type of other ion, or may contain two or more types of other ions.
[0047] Other ions contained in the photoluminescent material I-2c can be introduced into the photoluminescent material I-2c by ion exchange with an aqueous solution containing the other ions.
[0048] Examples of other ions contained in the photoluminescent material I-2c include alkali metal ions such as sodium ions, potassium ions, and cesium ions; alkaline earth metal ions such as calcium ions, strontium ions, and barium ions; and other metal ions such as nickel ions, copper ions, manganese ions, and aluminum ions. Among these, the cesium ion is preferred.
[0049] When the photoluminescent material I-2c contains other ions, the content thereof (when two or more kinds of other ions are contained, the total content of the other ions) is preferably 0.1% by weight or more and 40% by weight or less.
[0050] Photoluminescent material I-3 containing sodalite is described in, for example, Patent Document 5. Photoluminescent material I-3 can be produced by ion-exchanging sodalite by stirring and holding it in an aqueous solution containing silver ions, filtering, washing with water, and then heat-treating the ion-exchanged sodalite obtained. The heat-treatment conditions vary depending on the content of silver atoms and, if necessary, the content of zinc atoms. In the production of photoluminescent material I-3, drying at a temperature higher than room temperature is included in the heat treatment. Sodalite is easily available as a by-product of A-type zeolite, which is currently mass-produced at low cost.
[0051] The average particle size of sodalite, photoluminescent material I-3 obtained from sodalite, and photoluminescent material II obtained from photoluminescent material I-3 is preferably 0.05 μm or more and 500 μm or less, more preferably 0.5 μm or more and 50 μm or less.
[0052] The photoluminescent material I-3 is preferably sodalite containing 0.25% to 51% by weight of silver atoms, more preferably Sodalite containing 0.25% by weight or more and 10% by weight or less of silver atoms (hereinafter sometimes abbreviated as "photoluminescent material I-3a"); Sodalite containing 12% by weight or more and 18% by weight or less of silver atoms, produced through a heat treatment at a temperature of less than 300°C (hereinafter sometimes abbreviated as "photoluminescent material I-3b"); Sodalite containing 20% by weight or more and 31% by weight or less of silver atoms and 7% by weight or more and 17% by weight or less of zinc atoms (hereinafter sometimes abbreviated as "photoluminescent material I-3c"); Sodalite containing 33% to 51% by weight of silver atoms and 0.5% to 11% by weight of zinc atoms, produced through heat treatment at a temperature of 300°C to 850°C (hereinafter sometimes abbreviated as "photoluminescent material I-3d"). At least one selected from the group consisting of: Preferably, neither photoluminescent material I-3a nor photoluminescent material I-3b contains an oxalate anion. Hereinafter, photoluminescent materials I-3a to I-3d will be described.
[0053] Photoluminescent material I-3b (silver atom content: 12% by weight or more and 18% by weight or less) needs to be manufactured through heat treatment at a temperature of less than 300°C. On the other hand, photoluminescent material I-3d (silver atom content: 33% by weight or more and 51% by weight or less) needs to be manufactured through heat treatment at a temperature of 300°C or more. In addition, when the silver atom content is 0.25% by weight or more and 10% by weight or less (photoluminescent material I-3a) and when the silver atom content is 20% by weight or more and 31% by weight or less (photoluminescent material I-3c), they can be manufactured through heat treatment at a temperature of 300°C or more or less than 300°C.
[0054] It is presumed that the reason why the heat treatment temperatures for producing the photoluminescent material I-3 are different is that the form of silver atoms required for luminescence differs in sodalite depending on the content of silver atoms. In sodalite obtained by low-temperature heat treatment, silver atoms exist in the form of silver ions, and in sodalite obtained by high-temperature heat treatment, silver atoms exist in the form of silver ions or silver clusters, or a part of them are in the form of silver ions and the rest are in the form of silver clusters.
[0055] The temperature of the heat treatment for producing the photoluminescent material I-3a is preferably 50° C. or more and 850° C. or less, more preferably 100° C. or more and 700° C. or less, and even more preferably 150° C. or more and 600° C. or less. The time of the heat treatment for producing the photoluminescent material I-3a is preferably 1 hour or more and 24 hours or less, more preferably 2 hours or more and 24 hours or less.
[0056] The temperature of the heat treatment for producing the photoluminescent material I-3b must be less than 300° C., and is preferably 50° C. or more and less than 300° C., more preferably 100° C. or more and 270° C. or less, and even more preferably 150° C. or more and 250° C. or less. The time of the heat treatment for producing the photoluminescent material I-3b is preferably 1 hour or more and 24 hours, and more preferably 2 hours or more and 16 hours or less.
[0057] The temperature of the heat treatment for producing the photoluminescent material I-3c is preferably 50° C. or more and 850° C. or less, more preferably 100° C. or more and 700° C. or less, and even more preferably 150° C. or more and 600° C. or less. The time of the heat treatment for producing the photoluminescent material I-3c is preferably 1 hour or more and 24 hours or less, more preferably 2 hours or more and 24 hours or less.
[0058] The temperature of the heat treatment for producing the photoluminescent material I-3d must be 300° C. or more and 850° C. or less, preferably 300° C. or more and 700° C. or less, more preferably 350° C. or more and 650° C. or less, and further preferably 400° C. or more and 600° C. or less. The time of the heat treatment for producing the photoluminescent material I-3d is preferably 1 hour or more and 12 hours or less, more preferably 2 hours or more and 8 hours or less.
[0059] In the photoluminescent material I-3a and the photoluminescent material I-3b, in which the content of silver atoms is 18% by weight or less, zinc atoms are not necessary for emission. However, the photoluminescent material I-3a and the photoluminescent material I-3b may also contain zinc atoms. On the other hand, in the photoluminescent material I-3c and the photoluminescent material I-3d, in which the content of silver atoms is 20% by weight or more, zinc atoms are necessary in addition to silver atoms for emission. It is presumed that the reason why zinc atoms are necessary when the content of silver atoms is high is that the form of silver atoms necessary for emission differs in sodalite depending on the content of silver atoms as described above.
[0060] The photoluminescent material I-3 may contain atoms (hereinafter referred to as "other atoms") and / or ions (hereinafter referred to as "other ions") other than silver and zinc atoms. Examples of the other atoms include transition metal atoms other than silver and zinc, alkali metal atoms, alkaline earth metal atoms, halogen atoms, etc. Examples of the other ions include ammonium ions, halide ions, etc. However, it is preferable that the photoluminescent material I-3a and the photoluminescent material I-3b do not contain oxalate anions.
[0061] The content of silver atoms in the photoluminescent material I-3a is preferably 2.5% by weight or more and 10% by weight or less, more preferably 3.5% by weight or more and 8% by weight or less. The photoluminescent material I-3a may contain zinc atoms. The content of zinc atoms in the photoluminescent material I-3a is preferably 25% by weight or less, more preferably 5% by weight or more and 25% by weight or less.
[0062] The content of silver atoms in the photoluminescent material I-3b is preferably 12% by weight or more and 18% by weight or less, more preferably 13% by weight or more and 17% by weight or less. The photoluminescent material I-3b may contain zinc atoms. The content of zinc atoms in the photoluminescent material I-3b is preferably 0% by weight or more and 21% by weight or less, more preferably 5% by weight or more and 21% by weight or less.
[0063] The content of silver atoms in the photoluminescent material I-3c is preferably 20% by weight or more and 31% by weight or less, more preferably 22% by weight or more and 31% by weight or less.The content of zinc atoms in the photoluminescent material I-3c is preferably 7% by weight or more and 17% by weight or less, more preferably 8.5% by weight or more and 17% by weight or less.
[0064] The content of silver atoms in the photoluminescent material I-3d is preferably 33% by weight or more and 50.5% by weight or less, more preferably 35% by weight or more and 49% by weight or less. The content of zinc atoms in the photoluminescent material I-3d is preferably 0.5% by weight or more and 11% by weight or less, more preferably 0.8% by weight or more and 11% by weight or less.
[0065] The aqueous solution for extracting silver atoms from the photoluminescent material I (hereinafter sometimes abbreviated as "aqueous extraction solution") contains ammonia and cations other than silver ions. The cations other than silver ions may be nonmetallic ions such as ammonium ions, or metal ions such as alkali metal ions, alkaline earth metal ions, and zinc ions.
[0066] The cations other than silver ions preferably include alkali metal ions and / or alkaline earth metal ions. The alkali metal ions are preferably lithium ions, sodium ions, potassium ions, and cesium ions. The alkaline earth metal ions are preferably strontium ions and barium ions. The cations other than silver ions more preferably include at least one selected from the group consisting of lithium ions, sodium ions, potassium ions, cesium ions, strontium ions, and barium ions, even more preferably include at least one selected from the group consisting of sodium ions, potassium ions, cesium ions, strontium ions, and barium ions, particularly preferably include at least one selected from the group consisting of sodium ions, potassium ions, and strontium ions, and most preferably include sodium ions and / or strontium ions.
[0067] The cations other than the silver ion may be used alone or in combination. For example, two or more alkali metal ions may be used as the cations other than the silver ion, or alkali metal ions and other cations (e.g., zinc ions) may be used.
[0068] In the photoluminescent material I-2a or I-2b containing silver and zinc, if zinc ions are extracted together with silver ions, the luminescence intensity may decrease. Therefore, when using the photoluminescent material I-2a or I-2b, it is preferable that the cation other than silver ions contains zinc ions. By using zinc ions, the decrease in the luminescence intensity of the photoluminescent material II obtained from the photoluminescent material I-2a or I-2b can be suppressed.
[0069] By using a cation with a small atomic weight (for example, a sodium ion) as the cation other than the silver ion, the density of the photoluminescent material II can be made lower than the density of the photoluminescent material I. A low-density photoluminescent material can maintain a good dispersion state in a mixture with a resin, rubber, solvent, etc., compared to a high-density photoluminescent material.
[0070] In addition, the operation of extracting silver atoms from the photoluminescent material I by using an extraction aqueous solution (hereinafter referred to as "extraction operation") may be performed only once, or may be performed two or more times. The extraction operation may be performed two or more times using one type of extraction aqueous solution (for example, an extraction aqueous solution containing sodium ions and ammonia). In addition, the extraction operation may be performed two or more times using two or more different types of extraction aqueous solutions. For example, the extraction operation may be performed using an extraction aqueous solution containing sodium ions and ammonia, and then the extraction operation may be performed using an extraction aqueous solution containing potassium ions and ammonia.
[0071] In order to efficiently extract silver atoms from the photoluminescent material I, the concentration of cations other than silver ions in the extraction aqueous solution (when two or more kinds of cations are used, the total concentration of those cations) is preferably 0.3% by weight to 20% by weight, more preferably 0.45% by weight to 20% by weight. For the same reason, the concentration of ammonia in the extraction aqueous solution is preferably 0.12% by weight to 30% by weight, more preferably 0.18% by weight to 30% by weight.
[0072] When only alkali metal ions are used as cations other than silver ions, the preferred range of the concentration of alkali metal ions in the aqueous extract is the same as the preferred range of the concentration of cations other than silver ions in the aqueous extract.When cations other than alkali metal ions and alkali metal ions are used in combination as cations other than silver ions, the concentration of alkali metal ions in the aqueous extract (when two or more kinds of alkali metal ions are used, the total concentration of them) is preferably 0.05% by weight or more and 10% by weight or less, more preferably 0.1% by weight or more and 5% by weight or less.
[0073] When only alkaline earth metal ions are used as cations other than silver ions, the preferred range of the concentration of alkaline earth metal ions in the aqueous extract is the same as the preferred range of the concentration of cations other than silver ions in the aqueous extract. When cations other than alkaline earth metal ions and alkaline earth metal ions are used in combination as cations other than silver ions, the concentration of alkaline earth metal ions in the aqueous extract (when two or more kinds of alkaline earth metal ions are used, the total concentration of them) is preferably 0.05% by weight or more and 10% by weight or less, more preferably 0.1% by weight or more and 5% by weight or less.
[0074] When only zinc ion is used as cation other than silver ion, the preferred range of zinc ion concentration in the extraction aqueous solution is the same as the preferred range of cation other than silver ion concentration in the extraction aqueous solution described above.When cation other than zinc ion and zinc ion are used in combination as cation other than silver ion, the concentration of zinc ion in the extraction aqueous solution is preferably 0.15% by weight or more and 0.30% by weight or less, more preferably 0.20% by weight or more and 0.26% by weight or less.
[0075] The aqueous extract may contain an organic solvent miscible with water. Examples of the organic solvent include alcohols such as methanol and ethanol, and ketones such as acetone. From the viewpoint of dissolving silver ions in the aqueous extract, the content of the organic solvent is preferably 50% by weight or less of the entire aqueous extract, more preferably 20% by weight or less. The content of the organic solvent is a value based on the entire aqueous extract. It is most preferable that the aqueous extract does not contain an organic solvent.
[0076] In order to efficiently extract silver atoms from the photoluminescent material I, the amount of the aqueous extraction solution used is preferably 5 to 500 mL, more preferably 7.5 to 300 mL, and even more preferably 10 to 100 mL per 1 g of the photoluminescent material I.
[0077] The temperature of the aqueous extraction solution in the extraction operation is preferably 0 to 30° C., more preferably 5 to 25° C., from the viewpoints of the solubility of cations and the volatility of ammonia. The time for the extraction operation is preferably 5 minutes to 24 hours, more preferably 10 minutes to 16 hours, from the viewpoints of the volatility of ammonia and the reaction time required for the formation of an ammine complex of silver.
[0078] When photoluminescent material I-1 is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.9% by weight or more and 18% by weight or less, and more preferably 1.2% by weight or more and 15% by weight or less.
[0079] When photoluminescent material I-2a is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.3% by weight or more and 18% by weight or less, more preferably 0.4% by weight or more and 16% by weight or less.
[0080] When photoluminescent material I-2b is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.3% by weight or more and 25% by weight or less, more preferably 0.4% by weight or more and 22% by weight or less.
[0081] When photoluminescent material I-2c is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.3 wt % or more and 31 wt % or less, more preferably 0.4 wt % or more and 28 wt % or less.
[0082] When photoluminescent material I-3a is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.1 wt % or more and 7.2 wt % or less, more preferably 0.2 wt % or more and 6.4 wt % or less.
[0083] When photoluminescent material I-3b is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.39% by weight or more and 15% by weight or less, more preferably 0.52% by weight or more and 14% by weight or less.
[0084] When photoluminescent material I-3c is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 0.66% by weight or more and 27% by weight or less, more preferably 0.88% by weight or more and 25% by weight or less.
[0085] When photoluminescent material I-3d is used as photoluminescent material I, the silver atom content of photoluminescent material II obtained by the above-mentioned extraction operation is preferably 1.05% by weight or more and 44% by weight or less, more preferably 1.4% by weight or more and 39% by weight or less.
[0086] The ratio of the silver atom content of the photoluminescent material II obtained by the method of the present invention to the silver atom content of the photoluminescent material I (silver atom content of the photoluminescent material II / silver atom content of the photoluminescent material I) is preferably 3 / 100 to 9 / 10, more preferably 1 / 25 to 3 / 4, and even more preferably 1 / 20 to 1 / 2. Here, the unit of the content used in the ratio is "% by weight".
[0087] The present invention provides a photoluminescent material (i.e., photoluminescent material II with a reduced content of silver atoms) produced by the above-mentioned method. The photoluminescent material II may be used alone or in combination of two or more. The photoluminescent material II may also be used in combination with other photoluminescent materials. The photoluminescent material II can be used in, for example, lighting devices, luminescent paints, luminescent fibers, resin molded products, rubber molded products, light-emitting elements, sensors, etc. EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above-mentioned intent, and all of these modifications are included in the technical scope of the present invention.
[0089] The raw materials (eg, A-type zeolite) used in the following Examples and Comparative Examples were the same products obtained from the same manufacturer (eg, Union Showa Co., Ltd.) unless otherwise specified.
[0090] The properties of the resulting photoluminescent material were evaluated as follows. The composition of the photoluminescent material was measured using a scanning X-ray fluorescence analyzer ZSX Primus III+ manufactured by Rigaku Corporation, and the mass (A) per mole of the photoluminescent material was calculated based on the results. Next, the lattice constant of the photoluminescent material was measured using a fully automated multipurpose X-ray diffraction instrument SmartLab manufactured by Rigaku Corporation, and the volume (B, unit: cm) per molecule of the photoluminescent material was calculated by cubed. 3 From these values, the density of the photoluminescent material (unit: g / cm) was calculated using the following formula: 3 ) was calculated. Density (g / cm 3 ) = A(g) / Avogadro's constant (6.02×10 -23 ) / B(cm 3 ) Furthermore, the emission intensity of this photoluminescent material was measured using a FluoroMax-4 fluorescence spectrophotometer manufactured by Horiba, Ltd.
[0091] Example 1 (1) Preparation of photoluminescent material I (A-type zeolite containing silver atoms) 5.00 g of A-type zeolite (manufactured by Union Showa Co., Ltd., average particle size 5 μm, containing 11 wt% sodium ions as exchangeable cations), 0.93 g of silver nitrate (manufactured by Inshou Kikinzoku Co., Ltd., purity 99.8 wt%), 2.85 g of zinc nitrate hexahydrate (manufactured by Kishida Chemical Co., Ltd., purity 99 wt%), and 30 mL of ion-exchanged water were mixed, and the resulting mixture was stirred and held at room temperature for 1 hour. After that, the stirring was stopped, and the solid was collected by suction filtration. The collected solid was dried at 105°C for 16 hours and then calcined at 230°C for 16 hours, to obtain 5.95 g of photoluminescent material (A-type zeolite containing silver atoms).
[0092] (2) Preparation of photoluminescent material II with reduced content of silver atoms 0.28 g of sodium nitrate (Nacalai Tesque, purity 99% by weight), 0.33 g of zinc nitrate hexahydrate, 1.5 mL of aqueous ammonia (Kishida Chemical, ammonia concentration 28.7% by weight) and 30 mL of ion-exchanged water were mixed to obtain an aqueous extract (sodium ion concentration in the aqueous extract: 0.24% by weight, zinc ion concentration: 0.23% by weight, ammonia concentration: 1.20% by weight).
[0093] 1.00 g of the photoluminescent material (A-type zeolite containing silver atoms) obtained in (1) above was added to the obtained aqueous extract solution, and the resulting mixture was stirred at room temperature for 1 hour. Then, the solid was collected by suction filtration and dried at 105°C for 16 hours to obtain 0.98 g of a photoluminescent material with a reduced content of silver atoms.
[0094] Comparative Example 1: Photoluminescent material (A-type zeolite containing silver atoms) The photoluminescent material (A-type zeolite containing silver atoms) produced in Example 1(1) was used as Comparative Example 1.
[0095] Comparative Example 2: Production of photoluminescent material (A-type zeolite containing silver atoms) 5.00g of A-type zeolite, 0.093g of silver nitrate, 2.85g of zinc nitrate hexahydrate, and 30mL of ion-exchanged water were mixed, and the resulting mixture was stirred and held at room temperature for 1 hour. After that, the stirring was stopped, and the solid was collected by suction filtration. The collected solid was dried at 105°C for 16 hours, and then calcined at 230°C for 16 hours to obtain 5.60g of photoluminescent material (A-type zeolite containing silver atoms).
[0096] The compositions and densities of the photoluminescent materials obtained in Example 1(2) and Comparative Examples 1 and 2 are shown in Table 1. In addition, the relative luminescent intensities of the photoluminescent materials obtained in Example 1(2) and Comparative Examples 1 and 2, calculated with the luminescent intensity of the photoluminescent material obtained in Comparative Example 1 set to 1, are shown in Table 1.
[0097] [Table 1]
[0098] The photoluminescent material obtained in Example 1(2) had a reduced silver atom content compared to that obtained in Comparative Example 1, but the luminescence intensity of the photoluminescent material obtained in Example 1(2) was higher than that of the photoluminescent material obtained in Comparative Example 1.
[0099] The silver atom contents of the photoluminescent materials obtained in Example 1(2) and Comparative Example 2 were equivalent, but the luminescence intensity of the photoluminescent material obtained in Example 1(2) was higher than that of the photoluminescent material obtained in Comparative Example 2, which did not include a step of reducing silver atoms.
[0100] Example 2 (1) Preparation of photoluminescent material I (sodalite containing silver atoms) 10.00 g of A-type zeolite, 25.60 g of sodium hydroxide (manufactured by Nacalai Tesque, purity 97% by weight) and 38.40 g of ion-exchanged water were mixed, and the resulting mixture was allowed to stand at 95° C. for 16 hours. Thereafter, the solid was collected by suction filtration and dried at 105° C. for 16 hours to obtain 10.00 g of sodalite (average particle size 3 μm, containing 12% by weight of sodium ions as exchangeable cations).
[0101] 5.00 g of the obtained sodalite, 0.070 g of silver nitrate, 1.85 g of zinc nitrate hexahydrate, 2.51 g of potassium nitrate (Nacalai Tesque, purity 99 wt%), and 30 mL of ion-exchanged water were mixed, and the mixture was stirred at room temperature for 1 hour. Then, the solid was collected by suction filtration, dried at 105°C for 16 hours, and then baked at 230°C for 16 hours to obtain 5.57 g of photoluminescent material (sodalite containing silver atoms).
[0102] (2) Preparation of photoluminescent material II with reduced content of silver atoms 0.28 g of sodium nitrate, 0.25 g of potassium nitrate, 0.4 mL of aqueous ammonia, and 30 mL of ion-exchanged water were mixed to obtain an aqueous extract solution (sodium ion concentration: 0.25 wt %, potassium ion concentration: 0.31 wt %, ammonia concentration: 0.33 wt %).
[0103] 1.00 g of the photoluminescent material (sodalite containing silver atoms) obtained in (1) above was added to the obtained aqueous solution of the extracted material, and the mixture was stirred at room temperature for 1 hour. Then, the solid was collected by suction filtration and dried at 105°C for 16 hours to obtain 0.99 g of a photoluminescent material with a reduced content of silver atoms.
[0104] Comparative Example 3: Photoluminescent material (sodalite containing silver atoms) The photoluminescent material (sodalite containing silver atoms) produced in Example 2(1) was used as Comparative Example 3.
[0105] Comparative Example 4: Production of photoluminescent material (sodalite containing silver atoms) 5.00g of sodalite, 0.018g of silver nitrate, 1.85g of zinc nitrate hexahydrate, 2.51g of potassium nitrate, and 30mL of ion-exchanged water were mixed, and the mixture was stirred at room temperature for 1 hour. The solid was then collected by suction filtration, dried at 105°C for 16 hours, and then calcined at 230°C for 16 hours to obtain 5.58g of photoluminescent material (sodalite containing silver atoms).
[0106] The compositions and densities of the photoluminescent materials obtained in Example 2(2) and Comparative Examples 3 and 4 are shown in Table 2. The relative luminescent intensities of the photoluminescent materials obtained in Example 2(2) and Comparative Examples 3 and 4, calculated based on the luminescent intensity of the photoluminescent material obtained in Comparative Example 3 being 1, are also shown in Table 2.
[0107] [Table 2]
[0108] The photoluminescent material obtained in Example 2(2) had a reduced silver atom content compared to that obtained in Comparative Example 3, but the luminescence intensity of the photoluminescent material obtained in Example 2(2) was higher than that of the photoluminescent material obtained in Comparative Example 3.
[0109] The silver atom contents of the photoluminescent materials obtained in Example 2(2) and Comparative Example 4 were equivalent, but the luminescence intensity of the photoluminescent material obtained in Example 2(2) was higher than that of the photoluminescent material obtained in Comparative Example 4, which did not include a step of reducing silver atoms.
[0110] Example 3 (1) Preparation of photoluminescent material I (X-type zeolite containing silver atoms) 0.60 g of silver nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in ion-exchanged water to prepare 100 mL of an aqueous solution. 3.00 g of X-type zeolite (manufactured by Tosoh Corporation, average particle size 5 μm, containing 8 wt% sodium ions as exchangeable cations) was added to the resulting aqueous solution, and the resulting mixture was stirred at 25°C for 2 hours. The solid was then collected by suction filtration and dried at 70°C for 24 hours to obtain 4.05 g of a photoluminescent material (X-type zeolite containing silver atoms).
[0111] (2) Fabrication of photoluminescent materials with reduced silver atom content 2.19 g of sodium nitrate and 3.6 mL of aqueous ammonia were mixed with ion-exchanged water to obtain 100 mL of an aqueous extract solution (the concentration of sodium ions in the aqueous extract solution was 0.56% by weight, and the concentration of ammonia was 0.88% by weight).
[0112] 3.00 g of the photoluminescent material (X-type zeolite containing silver atoms) obtained in (1) above was added to the obtained aqueous extract solution, and the resulting mixture was stirred at room temperature for 2 hours. Then, the solid was collected by suction filtration and dried at 70°C for 24 hours to obtain 2.36 g of a photoluminescent material with a reduced content of silver atoms.
[0113] Comparative Example 5: Photoluminescent material (X-type zeolite containing silver atoms) The photoluminescent material (X-type zeolite containing silver atoms) produced in Example 3(1) was used as Comparative Example 5.
[0114] Comparative Example 6: Production of photoluminescent material (X-type zeolite containing silver atoms) 0.033 g of silver nitrate was dissolved in ion-exchanged water to prepare 100 mL of aqueous solution. 0.95 g of X-type zeolite was added to the obtained aqueous solution, and the obtained mixture was stirred at 25°C for 2 hours. Then, the solid was collected by suction filtration and dried at 70°C for 24 hours to obtain 1.00 g of photoluminescent material (X-type zeolite containing silver atoms).
[0115] The compositions and densities of the photoluminescent materials obtained in Example 3(2) and Comparative Examples 5 and 6 are shown in Table 3. The relative luminescent intensities of the photoluminescent materials obtained in Example 3(2) and Comparative Examples 5 and 6, calculated with the luminescent intensity of the photoluminescent material obtained in Comparative Example 5 set to 1, are also shown in Table 3.
[0116] [Table 3]
[0117] The photoluminescent material obtained in Example 3(2) had a reduced silver atom content compared to that obtained in Comparative Example 5, but the luminescence intensity of the photoluminescent material obtained in Example 3(2) was equivalent to that of the photoluminescent material obtained in Comparative Example 5.
[0118] Although the silver atom contents of the photoluminescent materials obtained in Example 3(2) and Comparative Example 6 were equivalent, the luminescence intensity of the photoluminescent material obtained in Example 3(2) was higher than that of the photoluminescent material obtained in Comparative Example 6, which did not include a step of reducing silver atoms.
[0119] Example 4 (1) Preparation of photoluminescent material I (A-type zeolite containing silver atoms) 5.00g of A-type zeolite, 0.47g of silver nitrate, 2.49g of zinc nitrate hexahydrate, 1.97g of ammonium nitrate (Kanto Chemical Co., Ltd., purity 99% by weight), 2.67g of cesium nitrate (Mitsuwa Chemical Co., Ltd., purity 99% by weight) and 30mL of ion-exchanged water were mixed, and the resulting mixture was stirred at room temperature for 1 hour. The solid was then collected by suction filtration, dried at 105°C for 16 hours, and then calcined at 150°C for 16 hours to obtain 6.30g of photoluminescent material (A-type zeolite containing silver atoms).
[0120] (2) Preparation of photoluminescent material II with reduced content of silver atoms 0.58 g of strontium nitrate (Kishida Chemical Co., Ltd., purity 98% by weight), 0.4 mL of ammonia water, and 30 mL of ion-exchanged water were mixed to obtain an aqueous extract (strontium ion concentration in the aqueous extract: 0.76% by weight, ammonia concentration: 0.33% by weight).
[0121] 1.00 g of the photoluminescent material (A-type zeolite containing silver atoms) obtained in (1) above was added to the obtained aqueous extract solution, and the resulting mixture was stirred at room temperature for 1 hour. Then, the solid was collected by suction filtration and dried at 105°C for 16 hours to obtain 0.82 g of a photoluminescent material with a reduced content of silver atoms.
[0122] Comparative Example 7: Photoluminescent material (A-type zeolite containing silver atoms) The photoluminescent material I-2b (A-type zeolite containing silver atoms) produced in Example 4(1) was used as Comparative Example 7.
[0123] Comparative Example 8: Production of photoluminescent material (A-type zeolite containing silver atoms) 5.00g of A-type zeolite, 0.33g of silver nitrate, 2.85g of zinc nitrate hexahydrate, 1.97g of ammonium nitrate, 0.53g of cesium nitrate, 2.90g of strontium nitrate and 30mL of ion-exchanged water were mixed, and the mixture was stirred at room temperature for 1 hour. The solid was then collected by suction filtration, dried at 105°C for 16 hours, and then calcined at 150°C for 16 hours to obtain 5.98g of photoluminescent material (A-type zeolite containing silver atoms).
[0124] The compositions and densities of the photoluminescent materials obtained in Example 4(2) and Comparative Examples 7 and 8 are shown in Table 4. In addition, the relative luminescent intensities of the photoluminescent materials obtained in Example 4(2) and Comparative Examples 7 and 8, calculated based on the luminescent intensity of the photoluminescent material obtained in Comparative Example 7 being 1, are shown in Table 4.
[0125] [Table 4]
[0126] The photoluminescent material obtained in Example 4(2) had a reduced silver atom content compared to that obtained in Comparative Example 7, but the luminescence intensity of the photoluminescent material obtained in Example 4(2) was equivalent to that of the photoluminescent material obtained in Comparative Example 7.
[0127] The silver atom contents of the photoluminescent materials obtained in Example 4(2) and Comparative Example 8 were equivalent, but the luminescence intensity of the photoluminescent material obtained in Example 4(2) was higher than that of the photoluminescent material obtained in Comparative Example 8, which did not include a step of reducing silver atoms.
[0128] Example 5 (1) Preparation of photoluminescent material I (sodalite containing silver atoms) 5.00 g of sodalite produced in the same manner as in Example 2(1), 0.070 g of silver nitrate, 2.46 g of zinc nitrate hexahydrate, and 30 mL of ion-exchanged water were mixed, and the resulting mixture was stirred for 3 hours at 80° C. Then, the solid was collected by suction filtration, dried at 105° C. for 16 hours, and then calcined at 230° C. for 16 hours to obtain 5.81 g of a photoluminescent material (sodalite containing silver atoms).
[0129] (2) Preparation of photoluminescent material II with reduced content of silver atoms 0.75 g of sodium nitrate, 0.4 mL of aqueous ammonia, 24 mL of ion-exchanged water, and 6 mL of methanol (Kanto Chemical Co., Ltd., purity 99.8% by weight) were mixed to obtain an aqueous extract (sodium ion concentration in the aqueous extract: 0.68% by weight, ammonia concentration: 0.44% by weight, methanol concentration: 15.9% by weight).
[0130] 1.00 g of the photoluminescent material (sodalite containing silver atoms) obtained in (1) above was added to the obtained aqueous solution of the extracted material, and the mixture was stirred at room temperature for 1 hour. Then, the solid was collected by suction filtration and dried at 105°C for 16 hours to obtain 0.99 g of a photoluminescent material with a reduced content of silver atoms.
[0131] Comparative Example 9: Photoluminescent material (sodalite containing silver atoms) The photoluminescent material (sodalite containing silver atoms) produced in Example 5(1) was used as Comparative Example 9.
[0132] The compositions and densities of the photoluminescent materials obtained in Example 5(2) and Comparative Example 9 are shown in Table 5. In addition, the relative luminescence intensities of the photoluminescent materials obtained in Example 5(2) and Comparative Example 9, calculated based on the luminescence intensity of the photoluminescent material obtained in Comparative Example 9 being 1, are shown in Table 5.
[0133] [Table 5]
[0134] The photoluminescent material obtained in Example 5(2) had a reduced silver atom content compared to that obtained in Comparative Example 9, but the luminescence intensity of the photoluminescent material obtained in Example 5(2) was equivalent to that of the photoluminescent material obtained in Comparative Example 9.
[0135] Experimental example: Measurement of the luminescence intensity of a cured material containing a photoluminescent material 0.75 g of A liquid and 0.75 g of B liquid of two-component type silicone rubber for LED ("SCR-1012" manufactured by Shin-Etsu Chemical Co., Ltd.) and 0.05 g of the photoluminescent material obtained in Example 1(2) or the photoluminescent material of Comparative Example 1 (i.e., the photoluminescent material obtained in Example 1(1)) were mixed. The luminescence intensity of the obtained mixture immediately after preparation was measured using a FluoroMax-4 fluorescence spectrophotometer manufactured by Horiba, Ltd. Thereafter, the mixture was left to stand in a 105°C air dryer for 1 hour to prepare a cured product, and the luminescence intensity of the obtained cured product was measured in the same manner as above. The relative luminescence intensity of the cured product, calculated by assuming the luminescence intensity of the mixture immediately after preparation to be 1, is shown in Table 6.
[0136] [Table 6]
[0137] The cured product obtained using the photoluminescent material of Comparative Example 1 was visually discolored, and its luminescence intensity was significantly lower than that of the mixture immediately after preparation. On the other hand, the cured product obtained using the photoluminescent material obtained in Example 1(2) did not discolor, and its luminescence intensity was almost unchanged compared to that of the mixture immediately after preparation. [Industrial Applicability]
[0138] The photoluminescent material obtained by the production method of the present invention can be used for, for example, lighting devices, luminescent paints, luminescent fibers, resin molded products, rubber molded products, light-emitting devices, sensors, and the like.
Claims
1. A method for producing a photoluminescent material that emits visible light when irradiated with light, comprising the steps of: The method includes obtaining a photoluminescent material II having a reduced content of silver atoms by extracting silver atoms from a photoluminescent material I containing silver atoms in an aqueous solution containing alkali metal ions and / or alkaline earth metal ions, ammonia, and zinc ions; and The method wherein the photoluminescent material I is a zeolite containing silver atoms.
2. 2. The method according to claim 1, wherein the photoluminescent material I is at least one selected from the group consisting of faujasite-type zeolite containing silver atoms, A-type zeolite containing silver atoms, and sodalite containing silver atoms.
3. 3. The method according to claim 2, wherein the faujasite-type zeolite containing silver atoms is a faujasite-type zeolite containing 5% by weight or more and 30% by weight or less of silver ions.
4. 4. The method according to claim 2 or 3, wherein the A-type zeolite containing silver atoms is an A-type zeolite containing 2.5% by weight or more and 40% by weight or less of silver ions.
5. 5. The method according to claim 2, wherein the sodalite containing silver atoms is a sodalite containing 0.25% by weight or more and 51% by weight or less of silver atoms.
6. The method according to any one of claims 1 to 5, wherein the ratio of the silver atom content of the photoluminescent material II to the silver atom content of the photoluminescent material I (silver atom content of the photoluminescent material II / silver atom content of the photoluminescent material I) is 3 / 100 to 9 / 10.
7. A photoluminescent material produced by the method of any one of claims 1 to 6.
Citation Information
Patent Citations
Antibacterial polymer composition and preparation thereof
JP1991081369A
Zeolite shaped article
JP2006219359A
Photoluminescent material containing silver ion
JP2012052102A
Photoluminescent material
JP2014037492A
Photoluminescent material
JP2018197296A