Compound

A novel merocyanine skeleton compound addresses the durability and absorption issues of existing ultraviolet absorbers by providing efficient 380 to 400 nm absorption with improved weather resistance and minimal coloration.

JP7591870B2Active Publication Date: 2024-11-29SUMITOMO CHEM CO LTD

Patent Information

Application Number
JP2020025265
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-08
Filing Date
2020-02-18
Publication Date
2024-11-29
Estimated Expiration
2040-02-18

AI Technical Summary

Technical Problem

Existing organic ultraviolet absorbers with a merocyanine skeleton suffer from low durability, particularly weather resistance, making them unsuitable for applications requiring severe weather resistance, and struggle to efficiently absorb light in the 380 to 400 nm wavelength range without causing coloration.

Method used

A novel compound with a merocyanine skeleton, represented by formula (I), featuring specific electron-withdrawing groups and ring formations, exhibits high absorption selectivity for visible light in the 380 to 400 nm range and improved weather resistance.

Benefits of technology

The compound efficiently absorbs ultraviolet to near ultraviolet light with high selectivity and minimal side absorption, maintaining color stability and durability even under harsh weather conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591870000001
    Figure 0007591870000001
  • Figure 0007591870000002
    Figure 0007591870000002
  • Figure 0007591870000003
    Figure 0007591870000003
Patent Text Reader

Abstract

To provide a novel compound with a merocyanine skeleton having high absorption selectivity for short-wavelength visible light having a wavelength of 380-400 nm.SOLUTION: The compound is represented by formula (I). [In formula (I), R3, R4 and R5 each independently represent an electron-attracting group; R1, R2, R6 and R7 each independently represent a hydrogen atom, a heterocyclic group, a halogen atom, a nitro group, a cyano group, a hydroxy group, a thiol group, a carboxy group, -SCF3, -SF5, -SF3, -SO3H, -SO2H, an optionally substituted aliphatic hydrocarbon group having 1-25 carbon atoms, or an optionally substituted aromatic hydrocarbon group having 6-18 carbon atoms; and R1 and R2, R1 and R6, R6 and R7, or R4 and R5 may be bonded to each other to form a ring.]SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a compound. [Background technology]

[0002] Conventionally, ultraviolet absorbers have been used in various applications and products to protect the human body and resin materials from deterioration due to ultraviolet rays. UV absorbers are roughly divided into inorganic UV absorbers and organic UV absorbers. Inorganic UV absorbers have good durability such as light resistance and heat resistance, but tend to be inferior in control of absorption wavelength and compatibility with organic materials. On the other hand, organic UV absorbers are inferior in durability to inorganic UV absorbers, but due to the freedom of molecular structure in organic UV absorbers, it is possible to control absorption wavelength and compatibility with organic materials, and they are used in a wide range of fields such as sunscreens, paints, optical materials, building materials, and automotive materials.

[0003] As organic ultraviolet absorbents, compounds having a triazole skeleton, a benzophenone skeleton, a triazine skeleton, and a cyanoacrylate skeleton can generally be mentioned. However, most organic ultraviolet absorbents having the above skeleton have a maximum absorption wavelength (λmax) of 360 nm or less, so they cannot efficiently absorb the ultraviolet to near ultraviolet region of 380 to 400 nm, and it was necessary to use a very large amount in order to fully absorb light in this region. In addition, many compounds having the above skeleton have a broad absorption spectrum, and when they are made to fully absorb light of 380 to 400 nm, they absorb not only the wavelength region of 380 to 400 nm but also light of 420 nm or more, which causes a problem that the composition containing the ultraviolet absorbent becomes colored.

[0004] As a means for solving the above problems, for example, Patent Document 1 proposes a compound having a merocyanine skeleton as represented by the following formula as an organic ultraviolet absorber. Patent Document 1 also describes that a film containing a compound having a merocyanine skeleton as represented by the following formula has low light transmittance at a wavelength of around 390 nm. [ka] [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-111823 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, compounds having a merocyanine skeleton have low durability (particularly weather resistance), and are therefore difficult to apply to applications requiring severe weather resistance. An object of the present invention is to provide a novel compound having a merocyanine skeleton that can be used as an ultraviolet to near ultraviolet absorbent that efficiently absorbs light with a wavelength of 380 to 400 nm and has good weather resistance. [Means for solving the problem]

[0007] The present invention includes the following inventions. [1] A compound represented by formula (I). [ka] [In formula (I), R 3 , R 4 and R 5 each independently represents an electron-withdrawing group. R 1 , R 2 , R 6 and R 7each independently represents a hydrogen atom, a heterocyclic group, a halogen atom, a nitro group, a cyano group, a hydroxy group, a thiol group, a carboxy group, -SCF3, -SF5, -SF3, -SO3H, -SO2H, an aliphatic hydrocarbon group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent, and -CH2- or -CH= contained in the aliphatic hydrocarbon group or the aromatic hydrocarbon group is -NR 1A -, -SO2-, -CO-, -O-, -COO-, -OCO-, -CONR 2A -, -NR 3A It may be substituted by -CO-, -S-, -SO-, -CF2- or -CHF-. R 1A , R 2A and R 3A each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. R 1 and R 2 may be linked to each other to form a ring. R 1 and R 6 may be linked to each other to form a ring. R 6 and R 7 may be linked to each other to form a ring. R 4 and R 5 may be linked to each other to form a ring. [2] R 3 However, nitro group, cyano group, -F, -OCF3, -SCF3, -SF5, -SF3, -SO2-R 222 (R 222 represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent), a fluoroalkyl group, or a fluoroaryl group. [3] R 3 is a cyano group. [4]R 4 and R 5 At least one selected from the group consisting of a cyano group, a nitro group, -OCF3, -SCF3, -SF5, -CO-OR222 , -SO2-R 222 (R 222 represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent), a fluoroalkyl group, or a fluoroaryl group. [5]R 4 and R 5 At least one selected from the group consisting of: is a cyano group. [6]R 4 and R 5 and wherein both are cyano groups. [7]R 1 and R 2 and each independently represents an optionally substituted aliphatic hydrocarbon group. [8]R 1 and R 2 are linked to each other to form a ring. [9]R 1 and R 2 The compound according to [8], wherein the ring formed by linking together has no unsaturated bond.

[10] The compound according to any one of [1] to [9], wherein the compound represented by formula (I) is a compound represented by formula (II): [ka] [In the formula, R 1 , R 2 , R 3 , R 4 and R 5 has the same meaning as above. Ring W 1 represents a ring structure having at least one double bond as a ring component and not having aromaticity.

[11] Tamaki W 1 is a 5- to 7-membered ring structure.

[12] Tamaki W 1is a 6-membered ring structure.

[13] The compound according to any one of [1] to

[12] , wherein λmax is 370 nm or more. (λmax represents the maximum absorption wavelength [nm] of the compound represented by formula (I).)

[14] The compound according to any one of [1] to

[13] , which satisfies formula (B). ε(λmax) / ε(λmax+30nm)≧5 (B) (In the formula, ε(λmax) represents the gram absorption coefficient at the maximum absorption wavelength [nm] of the compound represented by formula (I), and ε(λmax+30nm) represents the gram absorption coefficient at the wavelength [nm] of (maximum absorption wavelength [nm]+30nm) of the compound represented by formula (I).)

[15] A composition comprising the compound according to any one of [1] to

[14] . Effect of the Invention

[0008] The present invention provides a novel compound having a merocyanine skeleton that has high absorption selectivity for short-wavelength visible light of 380 to 400 nm. The compound of the present invention also has good weather resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The compound of the present invention is a compound having a structure represented by formula (I) (hereinafter, sometimes referred to as compound (I)).

[0010] <Compound (I)> [ka] [In formula (I), R 3 , R 4 and R 5 each independently represents an electron-withdrawing group. R 1 , R 2 , R 6 and R 7each independently represents a hydrogen atom, a heterocyclic group, a halogen atom, a nitro group, a cyano group, a hydroxy group, a thiol group, a carboxy group, -SCF3, -SF5, -SF3, -SO3H, -SO2H, an aliphatic hydrocarbon group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent, and -CH2- or -CH= contained in the aliphatic hydrocarbon group or the aromatic hydrocarbon group is -NR 1A -, -SO2-, -CO-, -O-, -COO-, -OCO-, -CONR 2A -, -R 3A It may be substituted by -CO-, -S-, -SO-, -SO2-, -CF2- or -CHF-. R 1A , R 2A and R 3A each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. R 1 and R 2 may be linked to each other to form a ring. R 1 and R 6 may be linked to each other to form a ring. R 6 and R 7 may be linked to each other to form a ring. R 4 and R 5 may be linked to each other to form a ring.

[0011] In this specification, the number of carbon atoms does not include the number of carbon atoms of substituents, and when -CH2- or -CH= is substituted, for example, as described above, it refers to the number of carbon atoms before substitution.

[0012] R 3 , R 4 and R 5 Examples of the electron-withdrawing group represented by the formula (X-1) include a halogen atom, a nitro group, a cyano group, a carboxy group, a halogenated alkyl group, a halogenated aryl group, -OCF3, -SCF3, -SF5, -SF3, -SO3H, -SO2H, and a group represented by the formula (X-1). [ka] [In formula (X-1), X 1 are -CO-, -COO-, -OCO-, -CS-, -CSS-, -COS-, -CSO-, -SO2-, -NR 223 CO- or -CONR 224 - represents. R 222 represents a hydrogen atom, an optionally substituted alkyl group having 1 to 25 carbon atoms, or an optionally substituted aromatic hydrocarbon group having 6 to 18 carbon atoms. R 223 and R 224 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group. * represents a bond.]

[0013] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the halogenated alkyl group include fluoroalkyl groups such as trifluoromethyl group, perfluoroethyl group, perfluoropropyl group, perfluoroisopropyl group, perfluorobutyl group, perfluorosec-butyl group, perfluorotert-butyl group, perfluoropentyl group, and perfluorohexyl group, and the like, and the perfluoroalkyl group is preferable. The number of carbon atoms of the halogenated alkyl group is usually 1 to 25, and preferably 1 to 12. The halogenated alkyl group may be linear or branched. Examples of the halogenated aryl group include a fluorophenyl group, a chlorophenyl group, and a bromophenyl group, and are preferably a fluoroaryl group, and more preferably a perfluoroaryl group. The number of carbon atoms in the halogenated aryl group is usually 6 to 18, and preferably 6 to 12.

[0014] X 1 is preferably -COO- or -SO2-. R 222Examples of the alkyl group having 1 to 25 carbon atoms represented by the formula (I) include linear or branched alkyl groups having 1 to 25 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, an n-hexyl group, a 1-methylbutyl group, a 3-methylbutyl group, an n-octyl group, an n-decyl group, and a 2-hexyl-octyl group. 222 is preferably an alkyl group having 1 to 12 carbon atoms. R 222 Examples of the substituent that the alkyl group having 1 to 25 carbon atoms represented by the following formula may have include a halogen atom and a hydroxy group. R 222 Examples of the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the formula (I) include aryl groups having 6 to 18 carbon atoms, such as a phenyl group, a naphthyl group, an anthracenyl group, and a biphenyl group; and aralkyl groups having 7 to 18 carbon atoms, such as a benzyl group, a phenylethyl group, and a naphthylmethyl group. R 222 Examples of the substituent that the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the following formula may have include a halogen atom and a hydroxy group. R 223 and R 224 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, an n-hexyl group, a 1-methylbutyl group, and a 3-methylbutyl group.

[0015] R 3 is a nitro group, a cyano group, -F, -OCF3, -SCF3, -SF5, -SF3, -SO2-R 222 (R 222represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent.), preferably a fluoroalkyl group (preferably a fluoroalkyl group having 1 to 25 carbon atoms) or a fluoroaryl group (preferably a fluoroaryl group having 6 to 18 carbon atoms), more preferably a cyano group, -F, -OCF3, -SCF3 or a fluoroalkyl group (preferably a fluoroalkyl group having 1 to 25 carbon atoms), and even more preferably a cyano group.

[0016] R 4 and R 5 At least one selected from the group consisting of a cyano group, a nitro group, -OCF3, -SCF3, -SF5, -CO-OR 222 , -SO2-R 222 (R 222 represents a hydrogen atom, an alkyl group having 1 to 25 carbon atoms which may have a substituent, or an aromatic hydrocarbon group having 6 to 18 carbon atoms which may have a substituent.), a fluoroalkyl group (preferably a fluoroalkyl group having 1 to 25 carbon atoms) or a fluoroaryl group (preferably a fluoroaryl group having 6 to 18 carbon atoms) is preferable. A cyano group, a nitro group, -CO-OR 222 or -SO2-R 222 and more preferably a cyano group. R 4 and R 5 are preferably of the same structure.

[0017] R 4 and R 5 may be bonded to each other to form a ring. 4 and R 5 The ring formed by bonding with each other may be a monocyclic ring or a condensed ring, but is preferably a monocyclic ring. 4 and R 5 The ring formed by bonding with each other may contain a heteroatom (nitrogen atom, oxygen atom, sulfur atom) or the like as a ring component. R 4 and R 5The ring formed by bonding with each other is usually a 3- to 10-membered ring, preferably a 5- to 7-membered ring, and more preferably a 5- or 6-membered ring. R 4 and R 5 Examples of the ring formed by bonding to each other include the structures shown below. [ka] [In the formula, * represents a bond to a carbon atom. 1E ~R 16E each independently represents a hydrogen atom or a substituent.

[0018] R 4 and R 5 The ring formed by bonding with each other is a substituent (R 1E ~R 16E ) may be included. R 1E ~R 16EExamples of the substituent represented by the formula (I) include halogen atoms such as fluorine atom, chlorine atom, bromine atom, and iodine atom; alkyl groups having 1 to 12 carbon atoms such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and nonyl groups; halogenated alkyl groups having 1 to 12 carbon atoms such as fluoromethyl, difluoromethyl, trifluoromethyl, 2-fluoroethyl, 2,2-difluoroethyl, 2,2,2-trifluoroethyl, 1,1,2,2-tetrafluoroethyl, and 1,1,2,2,2-pentafluoroethyl groups; alkoxy groups having 1 to 12 carbon atoms such as methoxy, ethoxy, propoxy, butoxy, pentyloxy, and hexyloxy groups; methylthio, ethylthio, propylthio, butylthio, pentylthio, hexylthio, and the like. fluorinated alkoxy groups having 1 to 12 carbon atoms, such as a monofluoromethoxy group, a difluoromethoxy group, a trifluoromethoxy group, a 2-fluoroethoxy group, or a 1,1,2,2,2-pentafluoroethoxy group; amino groups which may be substituted with an alkyl group having 1 to 6 carbon atoms, such as an amino group, a methylamino group, an ethylamino group, a dimethylamino group, a diethylamino group, or a methylethyl group; alkylcarbonyloxy groups having 2 to 12 carbon atoms, such as a methylcarbonyloxy group or an ethylcarbonyloxy group; alkylsulfonyl groups having 1 to 12 carbon atoms, such as a methylsulfonyl group or an ethylsulfonyl group; arylsulfonyl groups having 6 to 12 carbon atoms, such as a phenylsulfonyl group; a cyano group; a nitro group; a hydroxyl group; a thiol group; a carboxy group; -SF3; and -SF5. R 1E ~R 16E are each independently preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and further preferably a methyl group.

[0019] R 1 , R 2 , R 6 and R 7Examples of the aliphatic hydrocarbon group having 1 to 25 carbon atoms represented by the formula (I) include linear or branched alkyl groups having 1 to 25 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, an isopentyl group, an n-hexyl group, an isohexyl group, an n-octyl group, an isooctyl group, an n-nonyl group, an isononyl group, an n-decyl group, an isodecyl group, an n-dodecyl group, an isododecyl group, an undecyl group, a lauryl group, a myristyl group, a cetyl group, or a stearyl group; cycloalkyl groups having 3 to 25 carbon atoms, such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, or a cyclohexyl group; and cycloalkylalkyl groups having 4 to 25 carbon atoms, such as a cyclohexylmethyl group. R 1 , R 2 , R 6 and R 7 Each of the aliphatic hydrocarbon groups having 1 to 25 carbon atoms represented by the following formula is preferably an alkyl group having 1 to 15 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. R 1 , R 2 , R 6 and R 7 Examples of the substituent that the aliphatic hydrocarbon group having 1 to 25 carbon atoms represented by the following formula may have include a halogen atom, a hydroxyl group, a nitro group, a cyano group, -SO3H, a thiol group, and an amino group.

[0020] R 1 , R 2 , R 6 and R 7 -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms represented by the formula: 1A -, -SO2-, -CO-, -O-, -COO-, -OCO-, -CONR 2A -, -NR 3A It may be substituted by -CO-, -S-, -SO-, -CF2- or -CHF-. When -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms is substituted, it is preferable that it is substituted with -O-, -S-, -COO- or -SO2-. When -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms is replaced with -O-, the aliphatic hydrocarbon group is represented by -OR 111 (R 111 is preferably an alkoxy group represented by an alkyl group having 1 to 24 carbon atoms which may have a halogen atom. Alternatively, it may be a polyalkyleneoxy group such as a polyethyleneoxy group or a polypropyleneoxy group. When -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms is replaced by -S-, the aliphatic hydrocarbon group is represented by -SR 111 (R 111 is preferably an alkylthio group represented by an alkyl group having 1 to 24 carbon atoms which may have a halogen atom). When -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms is replaced with -COO-, the aliphatic hydrocarbon group is represented by -COO-R 111 (R 111 is preferably a group represented by an alkyl group having 1 to 24 carbon atoms which may have a halogen atom). When -CH2- or -CH= contained in the aliphatic hydrocarbon group having 1 to 25 carbon atoms is replaced with -SO2-, the aliphatic hydrocarbon group is represented by -SO2-R 111 (R 111 is preferably a group represented by an alkyl group having 1 to 24 carbon atoms which may have a halogen atom), and may be -SO2CHF2, -SO2CH2F, or the like.

[0021] R 1 , R 2 , R 6 and R 7Examples of the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the formula (I) include aryl groups having 6 to 18 carbon atoms, such as a phenyl group, a naphthyl group, an anthracenyl group, a tetracenyl group, a pentacenyl group, a phenanthryl group, a chrysenyl group, a triphenylenyl group, a tetraphenyl group, a pyrenyl group, a perylenyl group, a coronenyl group, and a biphenyl group; and aralkyl groups having 7 to 18 carbon atoms, such as a benzyl group, a phenylethyl group, and a naphthylmethyl group. An aryl group having 6 to 18 carbon atoms is preferable, and a phenyl group or a benzyl group is more preferable. R 1 , R 2 , R 6 and R 7 Examples of the substituent that the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the following formula may have include a halogen atom, a hydroxyl group, a thiol group, an amino group, a nitro group, a cyano group, and a -SO3H group.

[0022] R 1 , R 2 , R 6 and R 7 -CH2- or -CH= contained in the aromatic hydrocarbon group having 6 to 18 carbon atoms represented by the formula: 1A -, -SO2-, -CO-, -O-, -COO-, -OCO-, -CONR 2A -, -NR 3A It may be substituted by -CO-, -S-, -SO-, -CF2- or -CHF-. When -CH2- or -CH= contained in the aromatic hydrocarbon group having 6 to 18 carbon atoms is substituted, it is preferable that it is substituted with -O- or -SO2-. When -CH2- or -CH= contained in the aromatic hydrocarbon group having 6 to 18 carbon atoms is replaced with -O-, the aromatic hydrocarbon group is preferably an aryloxy group having 6 to 17 carbon atoms, such as a phenoxy group; or an arylalkoxy group such as a phenoxyethyl group, a phenoxydiethylene glycol group, or a phenoxypolyalkylene glycol group. When -CH2- or -CH= contained in the aromatic hydrocarbon group having 6 to 17 carbon atoms is replaced with -SO2-, the aromatic hydrocarbon group is represented by -SO2-R 112 (R 112represents an aryl group having 6 to 17 carbon atoms or an aralkyl group having 7 to 17 carbon atoms.

[0023] R 1A , R 2A and R 3A As the alkyl group having 1 to 6 carbon atoms represented by the formula: 223 Examples of the alkyl group include the alkyl group having 1 to 6 carbon atoms represented by the following formula:

[0024] R 1 , R 2 , R 6 and R 7 Examples of the halogen atom represented by the formula (I) include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0025] R 1 , R 2 , R 6 and R 7 Examples of the heterocyclic group represented by the formula (I) include a pyridyl group, a pyrrolidyl group, a tetrahydrofurfuryl group, a tetrahydrothiophene group, a pyrrole group, a furyl group, a thiopheno group, a piperidine group, a tetrahydropyranyl group, a tetrahydrothiopyranyl group, a thiapyranyl group, an imidazolino group, a pyrazole group, an oxazole group, a thiazolyl group, a dioxanyl group, a morpholino group, a thiazinyl group, a triazole group, a tetrazole group, a dioxolanyl group, a pyridazinyl group, a pyrimidinyl group, a pyrazinyl group, an indolyl group, an isoindolyl group, a benzimidazolyl group, a proline group, a phenyl ... Examples of the heterocyclic groups include aliphatic heterocyclic groups having 3 to 16 carbon atoms and aromatic heterocyclic groups having 3 to 16 carbon atoms, such as a quinolinyl group, a benzotriazolyl group, a quinolinyl group, an isoquinolinyl group, a quinazolinyl group, a quinoxalinyl group, a cinnolinyl group, a pteridinyl group, a benzopyranyl group, an anthryl group, an acridinyl group, a xanthenyl group, a carbazolyl group, a tetracenyl group, a porphinyl group, a chlorinyl group, a cholinyl group, an adenyl group, a guanyl group, a cytosyl group, a thyminyl group, a uracil group, a quinolyl group, a thiophenyl group, an imidazolyl group, an oxazolyl group, and a thiazolyl group. 1 , R 2 , R 6 and R 7Each of the heterocyclic groups represented by the following formula (I) is preferably independently a pyrrolidyl group, a piperidyl group, a tetrahydrofurfuryl group, a tetrahydropyranyl group, a tetrahydrothiopheno group, a tetrahydrothiopyranyl group, or a pyridyl group.

[0026] R 1 and R 2 The ring formed by combining these contains one nitrogen atom as a ring member. 1 and R 2 The ring formed by bonding with each other may be a monocyclic ring or a condensed ring, but is preferably a monocyclic ring. 1 and R 2 The ring formed by bonding with each other may further contain a heteroatom (oxygen atom, sulfur atom, nitrogen atom, etc.) as a ring component. 1 and R 2 The ring formed by bonding with each other preferably has no unsaturated bond. R 1 and R 2 The ring formed by bonding with each other is usually a 3- to 10-membered ring, preferably a 5- to 7-membered ring, and more preferably a 5- or 6-membered ring. R 1 and R 2 The ring formed by bonding together may have a substituent. 1E The substituents include the same ones as those represented by the following formula: R 1 and R 2 Examples of the ring formed by bonding to each other include the rings shown below. [ka] [In the formula, * represents a bond.]

[0027] R 1 and R 6 may be linked to each other to form a ring. 1 and R 6 The ring formed by combining and contains one nitrogen atom as a ring component. R 1 and R 6 The ring formed by bonding with each other may be a monocyclic ring or a condensed ring, but is preferably a monocyclic ring. 1 and R 6 The ring formed by bonding with each other may further contain a heteroatom (such as an oxygen atom, a sulfur atom, or a nitrogen atom) as a ring component. R 1 and R 6 The ring formed by bonding with each other is usually a 3- to 10-membered ring, preferably a 5- to 7-membered ring, and more preferably a 5- or 6-membered ring. R 1 and R 6 Examples of the ring formed by linking together include the rings described below. [ka]

[0028] R 6 and R 7 may be linked together to form a ring. 6 and R 7 The ring formed by bonding with each other has at least one double bond as a ring component. 6 and R 7 The number of double bonds contained in the ring formed by linking together is usually 1 to 4, preferably 1 to 3, more preferably 1 or 2, and even more preferably 1. R 6 and R 7 It is preferable that the ring formed by linking R to each other does not have aromaticity. 6 and R 7 The ring formed by linking together may be a heterocycle containing a heteroatom (for example, an oxygen atom, a sulfur atom, a nitrogen atom, etc.) as a ring component. R 6 and R 7 The ring formed by linking together is a ring having 5 to 18 carbon atoms, preferably a 5- to 7-membered ring structure, and more preferably a 6-membered ring structure. R 6 and R7 The ring formed by linking together may be a monocyclic ring or a condensed ring, but is preferably a monocyclic ring. R 6 and R 7 The ring formed by linking together may have a substituent, and the substituent may be R 1E The substituents include the same ones as those represented by the following formula:

[0029] R 6 and R 7 Examples of the ring formed by linking together include the rings described below. [ka] [ka] [ka] [In the formula, *1 represents a bond to a nitrogen atom, and *2 represents a bond to a carbon atom.]

[0030] R 1 and R 2 are each independently preferably an alkyl group having 1 to 25 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably a linear alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group, an ethyl group, an n-propyl group, or an n-butyl group. R 6 and R 7 are each independently preferably an alkyl group having 1 to 25 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably a branched alkyl group having 1 to 6 carbon atoms, and particularly preferably an isopropyl group, an isobutyl group, or a t-butyl group. R 6 and R 7 are preferably linked to each other to form a ring.

[0031] Compound (I) is preferably a compound represented by formula (II). [ka] [In the formula, R 1 , R 2 , R 3 , R 4 and R 5 has the same meaning as above. Ring W 1 represents a ring structure having at least one double bond as a ring component and not having aromaticity. Ring W 1 As for R 6 and R 7 are the same as those formed by linking together.

[0032] Ring W 1 is preferably, for example, the ring shown below. [ka] [In the formula, *1 represents a bond to a nitrogen atom, and *2 represents a bond to a carbon atom. R x1 and R x2 each independently represents a hydrogen atom or a substituent. R x1 and R x2 The substituent represented by the formula: 1E The substituents include the same ones as those represented by the following formula:

[0033] The maximum absorption wavelength λmax of compound (I) is preferably 370 nm or more and 420 nm or less. When the maximum absorption wavelength λmax of compound (I) is 370 nm or more and 420 nm or less, it can efficiently absorb ultraviolet to near ultraviolet light in the wavelength range of 380 nm or more and 400 nm or less. λmax may be a wavelength of more than 370 nm and 420 nm or less, preferably a wavelength of 375 nm or more and 415 nm or less, more preferably a wavelength of 375 nm or more and 410 nm or less, and even more preferably a wavelength of 380 nm or more and 400 nm or less.

[0034] The compound (I) preferably has a gram absorption coefficient ε at λmax of 0.5 or more, more preferably 0.75 or more, and particularly preferably 1.0 or more. There is no particular upper limit, but it is generally 10 or less. Here, λmax represents the maximum absorption wavelength [nm] of the compound (I). When the gram absorption coefficient ε at λmax of compound (I) is 0.5 or more, even a small amount added can efficiently absorb ultraviolet to near ultraviolet light in the wavelength range of 370 nm or more and 420 nm or less. Compound (I) preferably has ε(λmax) / ε(λmax+30nm) of 5 or more, more preferably 10 or more, and particularly preferably 20 or more. There is no particular upper limit, but it is generally 1000 or less. ε(λmax) represents the gram absorption coefficient at the maximum absorption wavelength [nm] of compound (I), and ε(λmax+30nm) represents the gram absorption coefficient at the wavelength [nm] of (maximum absorption wavelength [nm]+30nm) of compound (I). When ε(λmax) / ε(λmax+30 nm) is 5 or more, side absorption at wavelengths of 420 nm or more can be minimized, making it difficult for coloring to occur. The unit of gram absorptivity is L / (g cm).

[0035] Examples of compound (I) include the compounds shown below. Compound (I) is preferably a compound represented by formulas (1-1) to (1-4), (1-7), (1-8), (1-10), (1-12), (1-20) to (1-25), (1-55) to (1-57), (1-59), (1-63), (1-64), (1-67), (1-69) to (1-76), (1-123), (1-126), (1-127), (1-129), (1-161), (1-166), or (1-337) to (1-404); More preferably, it is a compound represented by formula (1-4), formula (1-7), formula (1-20), formula (1-55), formula (1-56), formula (1-59), formula (1-63), formula (1-64), formula (1-123), formula (1-126), formula (1-127), formula (1-129), formula (1-141), formula (1-147), formula (1-153), formula (1-337) to formula (1-404), More preferred are the compounds represented by formula (1-55), formula (1-59), formula (1-63), formula (1-64), formula (1-123), formula (1-141), formula (1-147), formula (1-153), and formulas (1-337) to (1-404).

[0036] [ka]

[0037] [ka]

[0038] [ka]

[0039] [ka]

[0040] [ka]

[0041] [ka]

[0042] [ka]

[0043] [ka]

[0044] [ka]

[0045] [ka]

[0046] [ka]

[0047] [ka]

[0048] [ka]

[0049] <Method for producing compound (I)> Compound (I) can be obtained, for example, by reacting a compound represented by formula (I-1) (hereinafter, sometimes referred to as compound (I-1)) with a compound represented by formula (I-2) (hereinafter, sometimes referred to as compound (I-2)). [ka] [In the formula, R 1 ~R 7 has the same meaning as above.]

[0050] The reaction of compound (I-1) with compound (I-2) is usually carried out by mixing compound (I-1) with compound (I-2), and it is preferable to add compound (I-2) to compound (I-1). In addition, the reaction of compound (I-1) with compound (I-2) is preferably carried out by mixing compound (I-1) with compound (I-2) in the presence of a base and a methylating agent, It is preferable to mix compound (1-1), compound (I-2), a base and a methylating agent, It is more preferable to mix compound (I-2) and a base with a mixture of compound (1-1) and a methylating agent, It is more preferable to add a mixture of compound (I-2) and a base to a mixture of compound (1-1) and a methylating agent.

[0051] Examples of the base include metal hydroxides (preferably alkali metal hydroxides) such as sodium hydroxide, lithium hydroxide, potassium hydroxide, cesium hydroxide, rubidium hydroxide, calcium hydroxide, barium hydroxide, and magnesium hydroxide; metal alkoxides (preferably alkali metal alkoxides) such as sodium methoxide, potassium methoxide, lithium methoxide, sodium ethoxide, sodium isopropoxide, sodium t-butoxide, and potassium t-butoxide; metal hydrides such as lithium hydride, sodium hydride, potassium hydride, lithium aluminum hydride, sodium borohydride, aluminum hydride, and sodium aluminum hydride; metal oxides such as calcium oxide and magnesium oxide; metal carbonates (preferably alkaline earth metal carbonates) such as sodium bicarbonate, sodium carbonate, and potassium carbonate; organic alkyl metal compounds such as trimethyllithium, tertiary butyllithium, methyllithium, and Grignard reagents; amine compounds such as ammonia, triethylamine, diisopropylethylamine, ethanolamine, pyrrolidine, piperidine, diazabicycloundecene, diazabicyclononene, guanidine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, pyridine, aniline, dimethoxyaniline, ammonium acetate, and β-alanine (preferably tertiary amines such as triethylamine and diisopropylethylamine); metal amide compounds such as lithium diisopropylamide, sodium amide, and potassium hexamethyldisilazide (preferably alkali metal amides); sulfonium compounds such as trimethylsulfonium hydroxide; iodonium compounds such as diphenyliodonium hydroxide; and phosphazene bases. The amount of the base used is usually 0.1 to 5 mol, and preferably 0.5 to 2 mol, per 1 mol of compound (I-1).

[0052] Examples of the methylating agent include iodomethane, dimethyl sulfate, methyl methanesulfonate, methyl fluorosulfonate, methyl paratoluenesulfonate, methyl trifluoromethanesulfonate, and trimethyloxonium tetrafluoroborate. The amount of the methylating agent used is usually 0.1 to 5.0 mol, and preferably 0.5 to 2.0 mol, per 1 mol of compound (I-1).

[0053] The reaction between compound (I-1) and compound (I-2) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tert-butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are acetonitrile, tetrahydrofuran, chloroform, dichloromethane, and diethyl ether, more preferred are acetonitrile, tetrahydrofuran, and chloroform, and even more preferred is acetonitrile. The solvent is preferably a dehydrated solvent.

[0054] The reaction time of compound (I-1) and compound (I-2) is usually 0.1 to 10 hours, preferably 0.2 to 3 hours. The reaction temperature of the compound (I-1) and the compound (I-2) is usually from -50 to 150°C, and preferably from -20 to 100°C. The amount of compound (I-2) used is usually 0.1 to 10 mol, and preferably 0.5 to 5 mol, per 1 mol of compound (I-1).

[0055] Examples of the compound (I-1) include the compounds shown below. [ka]

[0056] As the compound (I-2), a commercially available product may be used, and examples thereof include the compounds described below. [ka]

[0057] Compound (I-1) can be obtained, for example, by reacting a compound represented by formula (I-3) (hereinafter, sometimes referred to as compound (I-3)) with a compound represented by formula (I-4) (hereinafter, sometimes referred to as compound (I-4)). [ka] [In the formula, R 1 , R 2 , R 3 , R 6 and R 7 has the same meaning as above. E1 represents a leaving group.]

[0058] Examples of the leaving group represented by E1 include a halogen atom, a p-toluenesulfonyl group, and a trifluoromethylsulfonyl group.

[0059] The reaction of compound (I-3) with compound (I-4) is carried out by mixing compound (I-3) with compound (I-4). The amount of compound (I-4) used is usually 0.1 to 5 mol, preferably 0.5 to 2 mol, per 1 mol of compound (I-3). The reaction between compound (I-3) and compound (I-4) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tert-butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are acetonitrile, tetrahydrofuran, chloroform, dichloromethane, and diethyl ether, more preferred are acetonitrile, tetrahydrofuran, and chloroform, and even more preferred are methanol, ethanol, isopropanol, and acetonitrile. The reaction time of compound (I-3) and compound (I-4) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-3) and the compound (I-4) is usually -50 to 150°C.

[0060] Examples of the compound (I-3) include the compounds shown below. [ka]

[0061] Compound (I-4) may be a commercially available product. For example, chlorocyanide, bromocyanide, paratoluenesulfonyl cyanide, trifluoromethanesulfonyl cyanide, 1-chloromethyl-4-fluoro-1,4-diazoniabicyclo[2.2.2]octane bis(tetrafluoroborate (also called Select Fluoro (registered trademark of Air Products and Chemicals)), benzoyl(phenyliodonio)(trifluoromethanesulfonyl)methanide, 2,8-difluoro-5-(trifluoromethyl)-5H-dibenzo[b,d]thiophene-5-ium trifluoromethanesulfonate, N-bromosuccinimide, N-chlorosuccinimide, N-iodosuccinimide, etc. may be mentioned.

[0062] Compound (I-3) can be obtained by reacting a compound represented by formula (I-5) (hereinafter, sometimes referred to as compound (I-5)) with a compound represented by formula (I-6) (hereinafter, sometimes referred to as compound (I-6)). [ka] [In the formula, R 1 , R 2 , R 6 and R 7 has the same meaning as above.] In formula (I-5), R 6 and R 7 may be linked to each other to form a ring, and in this case, the ring may or may not contain a double bond as a component of the ring.

[0063] The reaction of compound (I-5) with compound (I-6) is carried out by mixing compound (I-5) with compound (I-6). The amount of compound (I-6) used is usually 0.1 to 5 mol, and preferably 0.5 to 2 mol, per 1 mol of compound (I-5). The reaction between compound (I-5) and compound (I-6) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tertiary butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are benzene, toluene, ethanol, and acetonitrile. The reaction time of compound (I-5) and compound (I-6) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-5) and the compound (I-6) is usually -50 to 150°C.

[0064] Examples of compound (I-5) include the compounds shown below. [ka]

[0065] Examples of the compound (I-6) include primary amines such as methylamine, ethylamine, ethanolamine, and 4-hydroxybutylamine; and secondary amines such as dimethylamine, diethylamine, dibutylamine, pyrrolidine, piperidine, 3-hydroxypyrrolidine, and 4-hydroxypiperidine.

[0066] Compound (I-1) can also be obtained by reacting a compound represented by formula (I-5-1) (hereinafter sometimes referred to as compound (I-5-1)) with compound (I-6). [ka] [In formula (I-5-1), R3 , R 6 and R 7 has the same meaning as above.] In formula (I-5-1), R 6 and R 7 may be linked to each other to form a ring, and in this case, the ring may or may not contain a double bond as a component of the ring.

[0067] The reaction of compound (I-5-1) with compound (I-6) is carried out by mixing compound (I-5-1) with compound (I-6). The amount of compound (I-6) used is usually 0.1 to 5 mol, and preferably 0.5 to 2 mol, per 1 mol of compound (I-5-1). The reaction between compound (I-5-1) and compound (I-6) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tertiary butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are benzene, toluene, ethanol, and acetonitrile. The reaction time of compound (I-5-1) and compound (I-6) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-5-1) and the compound (I-6) is usually -50 to 150°C.

[0068] Examples of the compound represented by formula (I-5-1) include the compounds shown below. [ka]

[0069] Compound (I) can also be obtained by reacting a compound represented by formula (I-7) (hereinafter sometimes referred to as compound (I-7)) with compound (I-6). [ka] [In formula (I-7), R 3 ~R 7 has the same meaning as above.] In formula (I-7), R 6 and R 7 may be linked to each other to form a ring, and in this case, the ring may or may not contain a double bond as a component of the ring.

[0070] The reaction of compound (I-7) with compound (I-6) is usually carried out by mixing compound (I-7) with compound (I-6), and it is preferable to add compound (I-6) to compound (I-7). The reaction of compound (I-7) with compound (I-6) is preferably carried out by mixing compound (I-7) with compound (I-6) in the presence of a base and a methylating agent, It is more preferable to mix compound (I-7), compound (I-6), a base and a methylating agent, It is more preferable to mix compound (I-6) with a mixture of compound (I-7), a methylating agent and a base.

[0071] The base may be the same as that used in the reaction of compound (I-1) with compound (I-2). The amount of the base used is usually 0.1 to 5.0 mol, and preferably 0.5 to 2.0 mol, per 1 mol of compound (I-7). The methylating agent may be the same as the methylating agent used in the reaction of compound (I-1) with compound (I-2). The amount of the methylating agent used is usually 0.1 to 5.0 mol, and preferably 0.5 to 2.0 mol, per 1 mol of compound (I-7). The amount of compound (I-6) used is usually 0.1 to 10 mol, and preferably 0.5 to 5 mol, per 1 mol of compound (I-7).

[0072] The reaction of compound (I-7) with compound (I-6) may be carried out in the presence of a solvent. Examples of the solvent include the same solvents as those used in the reaction of compound (I-1) with compound (I-2). Preferred are methanol, ethanol, isopropanol, toluene, and acetonitrile.

[0073] The reaction time of compound (I-7) and compound (I-6) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-7) and the compound (I-6) is usually -50 to 150°C.

[0074] Examples of compound (I-7) include the compounds shown below. [ka]

[0075] Compound (I-7) can be obtained by reacting a compound represented by formula (I-8) with compound (I-4). [ka] [In formula (I-8), R 4 ~R 7 has the same meaning as above.] In formula (I-8), R 6 and R 7 may be linked to each other to form a ring, and in this case, the ring may or may not contain a double bond as a component of the ring.

[0076] The reaction of compound (I-8) with compound (I-4) can be carried out by mixing compound (I-8) with compound (I-4). The reaction between compound (I-8) and compound (I-4) is preferably carried out in the presence of a base. Examples of the base include the same bases as those used in the reaction between compound (I-1) and compound (I-2). Preferred are metal hydroxides, metal alkoxides, amine compounds, and metal amide compounds. The amount of the base used is usually 0.1 to 10 mol, and preferably 0.5 to 2.0 mol, per 1 mol of compound (I-8). The reaction of compound (I-8) with compound (I-4) may be carried out in the presence of a solvent. Examples of the solvent include the same solvents as those used in the reaction of compound (I-1) with compound (I-2). Preferred are toluene, acetonitrile, methanol, ethanol, and isopropanol. The reaction time of compound (I-8) and compound (I-4) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-8) and the compound (I-4) is usually -50 to 150°C.

[0077] Examples of compound (I-8) include the compounds shown below. [ka]

[0078] Compound (I-8) can also be obtained by reacting compound (I-5) with compound (I-2). The reaction of compound (I-5) with compound (I-2) can be carried out by mixing compound (I-5) with compound (I-2). The reaction between compound (I-5) and compound (I-2) is preferably carried out in the presence of a base. Examples of the base include the same bases as those used in the reaction between compound (I-1) and compound (I-2). The amount of the base used is usually 0.1 to 5 moles, preferably 0.5 to 2 moles, per mole of compound (I-5). The reaction of compound (I-5) with compound (I-2) may be carried out in the presence of a solvent. The solvent may be the same as that used in the reaction of compound (I-1) with compound (I-2). Preferred are methanol, ethanol, isopropanol, toluene, and acetonitrile. The reaction time of compound (I-5) and compound (I-2) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-5) and the compound (I-2) is usually -50 to 150°C. The amount of compound (I-2) used is usually 0.1 to 10 mol, preferably 0.5 to 2 mol, per 1 mol of compound (I-5).

[0079] Compound (I) can also be obtained by reacting a compound represented by formula (1-9) (hereinafter sometimes referred to as compound (I-9)) with compound (I-4). [ka] [In formula (I-9), R 1 , R 2 , R 4 ~R 7 has the same meaning as above.]

[0080] The reaction of compound (I-9) with compound (I-4) is carried out by mixing compound (I-9) with compound (I-4). The amount of compound (I-4) used is usually 0.1 to 5 mol, and preferably 0.5 to 2 mol, per 1 mol of compound (I-9). The reaction between compound (I-9) and compound (I-4) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tert-butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are acetonitrile, tetrahydrofuran, chloroform, dichloromethane, and diethyl ether, more preferred are acetonitrile, tetrahydrofuran, and chloroform, and even more preferred are methanol, ethanol, isopropanol, and acetonitrile. The reaction time of compound (I-9) and compound (I-4) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-9) and the compound (I-4) is usually -50 to 150°C.

[0081] Examples of the compound represented by formula (I-9) include the compounds shown below. [ka]

[0082] The compound represented by formula (I-9) can be obtained by reacting a compound represented by formula (I-10) with a compound (I-2). [ka] [In formula (I-10), R 1 , R 2 , R 6 , R 7 has the same meaning as above.]

[0083] The reaction of compound (I-10) with compound (I-2) is carried out by mixing compound (I-10) with compound (I-2). The amount of compound (I-2) used is usually 0.1 to 5 mol, and preferably 0.5 to 2 mol, per mol of compound (I-10). The reaction between compound (I-10) and compound (I-2) may be carried out in the presence of a solvent. Examples of the solvent include acetonitrile, benzene, toluene, acetone, ethyl acetate, chloroform, dichloroethane, monochlorobenzene, methanol, ethanol, isopropanol, tertiary butanol, 2-butanone, tetrahydrofuran, diethyl ether, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, and water. Preferred are benzene, toluene, ethanol, and acetonitrile. The reaction time of compound (I-10) and compound (I-2) is usually 0.1 to 10 hours. The reaction temperature of the compound (I-10) and the compound (I-2) is usually -50 to 150°C.

[0084] Examples of the compound represented by formula (I-10) include the compounds shown below, which are available commercially as malonaldehyde dianilide hydrochloride. [ka]

[0085] <Composition containing compound (I)> The present invention also includes compositions containing compound (I). The composition containing compound (I) of the present invention is preferably a resin composition containing compound (I) and a resin. The composition is particularly suitable for use in applications where it may be exposed to sunlight or light including ultraviolet light.Specific examples include glass substitutes and surface coating materials thereof; coating materials for window glass, daylighting glass, and light source protection glass for residences, facilities, transport equipment, etc.; window films for residences, facilities, transport equipment, etc.; interior and exterior materials and interior and exterior paints for residences, facilities, transport equipment, etc., and coating films formed by the paints; alkyd resin lacquer paints and coating films formed by the paints; acrylic lacquer paints and coating films formed by the paints; light source members that emit ultraviolet light such as fluorescent lamps and mercury lamps; precision machinery, electronic and electrical equipment members, and shielding materials for electromagnetic waves generated from various displays; containers or packaging materials for food, chemicals, medicines, etc.; bottles, boxes, blisters, cups, special packaging, compact disc coatings, agricultural and industrial sheets or films; anti-fading agents for printed matter, dyed matter, dye pigments, etc.; polymer supports ( Examples of suitable applications include protective films for plastic parts such as machinery and automotive parts; overcoats for printed matter; inkjet media coatings; matte laminations; optical light films; safety glass / windshield interlayers; electrochromic / photochromic applications; overlaminate films; solar heat control films; cosmetics such as sunscreen creams, shampoos, conditioners, hair products, etc.; apparel textiles and fibers such as sportswear, stockings, hats, etc.; household interior items such as curtains, carpets, wallpaper, etc.; medical devices such as plastic lenses, contact lenses, artificial eyes, etc.; optical products such as optical filters, backlit display films, prisms, mirrors, photographic materials, etc.; stationery such as mold films, transfer stickers, anti-graffiti films, tapes, inks, etc.; sign boards, markers, etc. and their surface coating materials, etc.

[0086] The shape of the polymer molded product formed from the above resin composition may be any of a flat film, powder, spherical particles, crushed particles, a continuous mass, fibers, tubes, hollow fibers, granules, plates, porous shapes, and the like.

[0087] Examples of the resin used in the resin composition include thermoplastic resins and thermosetting resins that have been conventionally used for producing various known molded articles, sheets, films, and the like. Examples of thermoplastic resins include olefin-based resins such as polyethylene resins, polypropylene resins, and polycycloolefin resins, poly(meth)acrylic acid ester-based resins, polystyrene-based resins, styrene-acrylonitrile-based resins, acrylonitrile-butadiene-styrene-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polyvinyl acetate-based resins, polyvinyl butyral-based resins, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol-based resins, polyethylene terephthalate resins, polybutylene terephthalate resins, and polyester-based resins such as liquid crystal polyester resins, polyacetal resins, polyamide resins, polycarbonate resins, polyurethane resins, and polyphenylene sulfide resins. These resins may be used as a polymer blend or polymer alloy of one or more kinds.

[0088] Examples of the thermosetting resin include epoxy resin, melamine resin, unsaturated polyester resin, phenol resin, urea resin, alkyd resin, and thermosetting polyimide resin.

[0089] When the resin composition is used as an ultraviolet absorbing filter or an ultraviolet absorbing film, the resin is preferably a transparent resin.

[0090] The resin composition can be obtained by mixing the compound (I) with a resin. The compound (I) may be contained in an amount necessary to impart the desired performance, for example, 0.01 to 20 parts by mass per 100 parts by mass of the resin. The composition of the present invention may contain other additives, such as a solvent, a crosslinking catalyst, a tackifier, a plasticizer, a softener, a dye, a pigment, and an inorganic filler, as necessary.

[0091] The composition and the resin composition may be a composition for eyeglass lenses. An eyeglass lens can be formed by molding or the like using the composition for eyeglass lenses. The molding method of the composition for eyeglass lenses may be injection molding or cast polymerization. Note that cast polymerization is a method in which a composition for eyeglass lenses, mainly consisting of a monomer or oligomer resin, is injected into a lens mold, and the composition for eyeglass lenses is cured by heat or light to be molded into a lens. The composition for eyeglass lenses may have a suitable composition according to the molding method. For example, when the eyeglass lenses are formed by injection molding, the composition may be a resin composition for eyeglass lenses containing a resin and compound (I). When the eyeglass lenses are formed by cast polymerization, the composition may be a composition for eyeglass lenses containing a curable monomer that is cured by heat or light and compound (I).

[0092] The resin contained in the composition for eyeglass lenses includes the above-mentioned resins, and is preferably a transparent resin. The resin contained in the composition for eyeglass lenses is preferably used as a polymer blend or polymer alloy of one or more of poly(meth)acrylic acid ester resins, polycarbonate resins, polyamide resins, polyurethane resins, and polythiourethane resins. In addition, the composition may contain not only polymers but also monomer components.

[0093] The spectacle lens composition may be a composition containing a curable monomer and a compound (I). The curable monomer may contain two or more kinds. Specifically, the composition may be a mixture of a polyol compound and an isocyanate compound, or a mixture of a thiol compound and an isocyanate compound, preferably a mixture of a thiol compound and an isocyanate, and more preferably a mixture of a multifunctional thiol compound and a multifunctional isocyanate compound.

[0094] The thiol compound is not particularly limited as long as it is a compound having at least one thiol group in the molecule. It may be chain-like or cyclic. In addition, it may have a sulfide bond, a polysulfide bond, or other functional groups in the molecule. Specific examples of the thiol compound include thiol group-containing organic compounds having one or more thiol groups in one molecule, such as aliphatic polythiol compounds, aromatic polythiol compounds, thiol group-containing cyclic compounds, and thiol group-containing sulfide compounds, as described in JP-A-2004-315556. Among these, from the viewpoint of improving the refractive index and glass transition temperature of the optical material, a polyfunctional thiol compound having two or more thiol groups is preferred, an aliphatic polythiol compound having two or more thiol groups, a sulfide compound containing two or more thiol groups is more preferred, and bis(mercaptomethyl)sulfide, 1,2-bis[(2-mercaptoethyl)thio]-3-mercaptopropane, pentaerythritol tetrakisthiopropionate, and 4,8-dimercaptomethyl-1,11-mercapto-3,6,9-trithiaundecane are even more preferred. The thiol compounds may be used alone or in combination of two or more.

[0095] The isocyanate compound is preferably a polyfunctional isocyanate compound having at least two isocyanato groups (-NCO) in the molecule, and examples thereof include aliphatic isocyanate compounds (e.g., hexamethylene diisocyanate, etc.), alicyclic isocyanate compounds (e.g., isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate), aromatic isocyanate compounds (e.g., tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, etc.), and the like. Further, the isocyanate compound may be an adduct of a polyhydric alcohol compound (e.g., an adduct of glycerol, trimethylolpropane, or the like), an isocyanurate, a biuret type compound, or a derivative of a urethane prepolymer type isocyanate compound obtained by addition reaction with a polyether polyol, a polyester polyol, an acrylic polyol, a polybutadiene polyol, a polyisoprene polyol, or the like.

[0096] When the spectacle lens composition contains a curable monomer, it may contain a curing catalyst to improve the curing property. Examples of the curing catalyst include tin compounds such as dibutyltin chloride, amines described in JP-A-2004-315556, phosphines, quaternary ammonium salts, quaternary phosphonium salts, tertiary sulfonium salts, secondary iodonium salts, mineral acids, Lewis acids, organic acids, silicic acids, tetrafluoroboric acids, peroxides, azo compounds, condensates of aldehydes and ammonia compounds, guanidines, thioureas, thiazoles, sulfenamides, thiurams, dithiocarbamates, xanthogenates, acidic phosphates, etc. These curing catalysts may be used alone or in combination of two or more.

[0097] The content of compound (I) in the spectacle lens composition, when the spectacle lens composition is a resin composition, may be, for example, 0.01 to 20 parts by mass relative to 100 parts by mass of the resin. When the spectacle lens composition is a curable composition, the content of compound (I) may be, for example, 0.00001 to 20 parts by mass relative to 100 parts by mass of the curable component. The content of compound (I) is preferably 0.0001 to 15 parts by mass, more preferably 0.001 to 10 parts by mass, still more preferably 0.01 to 5 parts by mass, and particularly preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the resin or curable component. The amount of the curing catalyst added is preferably 0.0001 to 10.0% by mass, and more preferably 0.001 to 5.0% by mass, relative to 100% by mass of the spectacle lens composition. The composition for spectacle lenses may contain the additives described above. EXAMPLES

[0098] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the examples, % and parts representing the content or amount used are based on mass unless otherwise specified.

[0099] (Example 1) Synthesis of compound represented by formula (UVA-6) [ka] A 500 mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with 20 parts of dimedone, 11.2 parts of pyrrolidine, and 200 parts of toluene in a nitrogen atmosphere, and the mixture was refluxed and stirred for 5 hours. The solvent was distilled off from the mixture obtained, and the mixture was purified to obtain 27.4 parts of the compound represented by formula (M-3).

[0100] [ka] Under a nitrogen atmosphere, 1.0 part of the compound represented by formula (M-3), 2.8 parts of paratoluenesulfonyl cyanide, and 10 parts of acetonitrile were mixed. The mixture was stirred at 0 to 5° C. for 5 hours. The solvent was distilled off from the mixture, and the mixture was purified to obtain 0.6 part of the compound represented by formula (M-4).

[0101] [ka] Under a nitrogen atmosphere, 4.8 parts of the compound represented by formula (M-4), 4.6 parts of methyl triflate, and 24 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 1.9 parts of malononitrile, 3 parts of triethylamine, and 24 parts of acetonitrile were added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 2.9 parts of the compound represented by formula (UVA-6).

[0102] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-6) was produced. 1 H-NMR(CDCl3)δ:0.99(s, 6H), 1.90-1.96(m, 4H), 2.48-2.51(m, 4H), 3.70-3.88(dt, 4H) LC-MS; [M+H] + =284.5

[0103] <Measurement of maximum absorption wavelength and gram absorption coefficient ε> The obtained 2-butanone solution (0.006 g / L) of the compound represented by formula (UVA-6) was placed in a 1 cm quartz cell, and the quartz cell was set in a spectrophotometer UV-2450 (Shimadzu Corporation), and the absorbance was measured in 1 nm steps in the wavelength range of 300 to 800 nm by the double beam method. The gram extinction coefficient for each wavelength was calculated from the obtained absorbance value, the concentration of the compound represented by formula (UVA-6) in the solution, and the optical path length of the quartz cell. ε(λ)=A(λ) / CL [In the formula, ε(λ) represents the gram absorption coefficient (L / (g cm)) of the compound represented by formula (UVA-6) at a wavelength of λ nm, A(λ) represents the absorbance at a wavelength of λ nm, C represents the concentration (g / L), and L represents the optical path length (cm) of the quartz cell.] The maximum absorption wavelength of the compound represented by formula (UVA-6) was 380 nm. The ε(λmax) of the compound represented by formula (UVA-6) was 1.75 L / (g cm), ε(λmax+30 nm) was 0.032 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 54.53.

[0104] (Example 2) Synthesis of compound represented by formula (UVA-7) [ka] Under a nitrogen atmosphere, 1 part of the compound represented by formula (M-4), 0.6 parts of methyl triflate, and 10 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 5.2 parts of ethyl cyanoacetate, 4.6 parts of triethylamine, and 10 parts of acetonitrile were added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 0.5 parts of the compound represented by formula (UVA-7).

[0105] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-7) was produced. 1 H-NMR (heavy DMSO) δ: 0.960-0.994 (d, 6H), 1.20-1.26 (m, 3H), 1.93 (m, 4H), 2.53-2.91 (m, 4H), 3.77-3.81 (m, 4H), 4.10-4.19 (m, 2H) LC-MS; [M+H] + =314.5(+H)

[0106] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-7) was 382.7 nm. The ε(λmax) of the compound represented by the formula (UVA-7) was 1.08 L / (g cm), ε(λmax+30 nm) was 0.153 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 7.04.

[0107] (Example 3) Synthesis of compound represented by formula (UVA-8) [ka] Under a nitrogen atmosphere, 0.5 parts of the compound represented by formula (M-4), 0.5 parts of dimethyl sulfate, and 5 parts of acetonitrile were mixed and reacted with stirring at 20 to 30° C. for 3 hours. Furthermore, 0.4 parts of pivaloylacetonitrile, 0.5 parts of triethylamine, and 5.0 parts of acetonitrile were added and reacted with stirring at 20 to 30° C. for 3 hours. After the reaction was completed, the solvent was distilled off and purification was performed to obtain 0.07 parts of the compound represented by formula (UVA-8).

[0108] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-8) was produced. 1 H-NMR (heavy DMSO) δ: 0.92 (s, 6H), 1.26 (s, 9H), 1.90 (s, 4H), 2.55 (m, 4H), 3.64-3.71 (m, 4H) LC-MS; [M+H] + =326.5

[0109] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-8) was 377.4 nm. The ε(λmax) of the compound represented by the formula (UVA-8) was 0.66 L / (g cm), ε(λmax+30 nm) was 0.395 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 1.68.

[0110] (Example 4) Synthesis of compound represented by formula (UVA-9) [ka] A 300mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with 70.0 parts of dimedone, 10.4 parts of malononitrile, 40.6 parts of diisopropylethylamine, and 100.0 parts of ethanol, and the mixture was heated and refluxed for 3 hours. After the reaction was completed, the solvent was distilled off and purification was performed to obtain 15.1 parts of the compound represented by formula (M-5).

[0111] [ka] Under a nitrogen atmosphere, 5 parts of the compound represented by formula (M-5), 5.8 parts of paratoluenesulfonyl cyanide, 3 parts of potassium tert-butoxide, and 50 parts of ethanol were mixed. The resulting mixture was stirred at 0 to 5°C for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 3.3 parts of the compound represented by formula (M-6).

[0112] [ka] Under a nitrogen atmosphere, 1 part of the compound represented by formula (M-6), 1 part of methyl triflate, 0.8 parts of diisopropylethylamine, and 20 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 1.4 parts of piperidine and 20 parts of acetonitrile were added, and the mixture was stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 0.5 parts of the compound represented by formula (UVA-9).

[0113] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-9) was produced. 1 H-NMR (heavy DMSO) δ: 0.99 (s, 6H), 1.60 (m, 6H), 2.71 (s, 2H), 3.80 (m, 4H) LC-MS; [M+H] + =281.5

[0114] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-9) was 385.6 nm. The ε(λmax) of the compound represented by the formula (UVA-9) was 1.65 L / (g cm), ε(λmax+30 nm) was 0.088 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 18. It was .8.

[0115] (Synthesis Example 1) Synthesis of compound represented by formula (UVA-A1) [ka] A 200mL-four-neck flask equipped with a Dimroth condenser and a thermometer was filled with nitrogen, and 10 parts of a compound represented by formula (M-7) synthesized with reference to JP-A-2014-194508, 3.6 parts of acetic anhydride, 6.9 parts of (2-butyloctyl) cyanoacetate, and 60 parts of acetonitrile were charged and stirred at 20 to 30°C. 4.5 parts of diisopropylethylamine were added dropwise to the resulting mixture over 1 hour, and the mixture was stirred for 2 hours. The solvent was distilled off from the resulting mixture and purified to obtain 4.6 parts of a compound represented by formula (UVA-A1).

[0116] (Synthesis Example 2) Synthesis of compound represented by formula (UVA-A2) [ka] A 100mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with nitrogen, and 6 parts of the compound represented by formula (M-8), 14.2 parts of dibutylamine, and 31.3 parts of isopropanol were mixed and heated under reflux, followed by stirring for 3 hours. The solvent was removed from the mixture obtained, and the mixture was purified to obtain 4.6 parts of the compound represented by formula (UVA-A2).

[0117] (Synthesis Example 3) Synthesis of compound represented by formula (UVA-A3) [ka] A 300 mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with nitrogen and charged with 30 parts of malonaldehyde dianilide hydrochloride, 18.4 parts of Meldrum's acid, 12.9 parts of triethylamine, and 90 parts of methanol, and the mixture was stirred and reacted for 3 hours at 20 to 30° C. After completion of the reaction, the solvent was distilled off and purification was performed to obtain 24.4 parts of the compound represented by formula (M-8).

[0118] [ka] 6 parts of the compound represented by formula (M-8), 21.7 parts of dibenzylamine, and 31.3 parts of isopropanol were mixed, heated under reflux, and then reacted with stirring for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 3.5 parts of the compound represented by formula (UVA-A3).

[0119] (Synthesis Example 4) Synthesis of compound represented by formula (UVA-A4) [ka] A 100mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with nitrogen, and 5 parts of 2-phenyl-1-methylindole-3-carboxaldehyde, 1.8 parts of piperidine, 1.5 parts of malononitrile, and 20 parts of ethanol were mixed and heated to reflux, followed by stirring for 18 hours. The resulting mixture was heated to 80°C and kept at 80°C for 18 hours. The solvent was distilled off from the resulting mixture, and purification was performed to obtain 4.9 parts of a compound represented by the formula (UVA-A4).

[0120] (Example 5) Preparation of light selective absorbing composition (1) The components were mixed in the following ratio to prepare a photoselective absorption composition (active energy ray-curable resin composition) (1). Multifunctional acrylate ("A-DPH-12E": manufactured by Shin-Nakamura Chemical Co., Ltd.) 70 parts Urethane acrylate (UV-7650B: Nippon Chemical Industry Co., Ltd.) 30 parts Polymerization initiator ("NCI-730": manufactured by ADEKA Corporation) 3 parts Compound represented by formula (UVA-6) synthesized in Example 1 Part 2 Methyl ethyl ketone 34 parts

[0121] (Example 6) Preparation of light selective absorbing composition (2) A light selective absorbing composition (2) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-7).

[0122] (Example 7) Preparation of photoselective absorption composition (3) A light selective absorbing composition (3) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-8).

[0123] (Example 8) Preparation of photoselective absorption composition (4) A light selective absorbing composition (4) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-9).

[0124] (Preparation Example 1) Preparation of light selective absorption composition (A1) A light selective absorbing composition (A1) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-A1).

[0125] (Preparation Example 2) Preparation of light selective absorption composition (A2) A light selective absorbing composition (A2) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-A2).

[0126] (Preparation Example 3) Preparation of light selective absorption composition (A3) A light selective absorbing composition (A3) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-A4).

[0127] (Example 9) Preparation of film (1) with cured layer A 23 μm-thick resin film made of a cyclic polyolefin resin (trade name "ZEONOR", manufactured by Zeon Corporation) was subjected to a corona discharge treatment on its surface, and the light selective absorbing composition (1) was applied to the corona discharge treated surface using a bar coater. The coated film was placed in a drying oven and dried at 100°C for 2 minutes. The dried coated film was placed in a nitrogen replacement box, and nitrogen was sealed in the box for 1 minute. The coated surface was then irradiated with ultraviolet light to obtain a film (1) with a cured layer. The thickness of the cured layer was approximately 6.0 μm. The ultraviolet irradiation device used was a belt conveyor equipped ultraviolet irradiation device (using an "H bulb" lamp manufactured by Fusion UV Systems) with an accumulated light output of 400 mJ / cm 2 The specimen was exposed to ultraviolet light (UVB).

[0128] (Comparative Example 1) Preparation of film (A1) with cured layer A film with a cured layer (A1) was obtained in the same manner as in Example 9, except that the light selective absorbing composition (1) was replaced with the light selective absorbing composition (A1).

[0129] (Comparative Example 2) Preparation of film (A2) with cured layer A film with a cured layer (A2) was obtained in the same manner as in Example 9, except that the light selective absorbing composition (1) was replaced with the light selective absorbing composition (A2).

[0130] (Comparative Example 3) Preparation of film (A3) with cured layer A film with a cured layer (A3) was obtained in the same manner as in Example 9, except that the light selective absorbing composition (1) was replaced with the light selective absorbing composition (A3).

[0131] <Absorbance measurement of film with cured layer> The film (1) with the cured layer obtained in Example 9 was cut to a size of 30 mm x 30 mm to obtain sample (1). The obtained sample (1) and non-alkali glass (trade name "EAGLE XG" manufactured by Corning Incorporated) were bonded via an acrylic adhesive to obtain sample (2). The absorbance of the prepared sample (2) in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The measured absorbance at wavelengths of 395 nm and 430 nm was taken as the absorbance of the film (1) with the cured layer at wavelengths of 395 nm and 430 nm. The results are shown in Table 1. In addition, the absorbance of alkali-free glass at wavelengths of 395 nm and 430 nm is approximately 0, the absorbance of a resin film made of a cyclic polyolefin resin at wavelengths of 395 nm and 430 nm is approximately 0, and the absorbance of an acrylic adhesive at wavelengths of 395 nm and 430 nm is approximately 0.

[0132] <Measurement of absorbance retention of film with cured layer> After the absorbance measurement, sample (2) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 48 hours under conditions of a temperature of 63°C and a relative humidity of 50% RH, and a weather resistance test was performed. The absorbance of sample (2) after the weather resistance test was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of sample (2) at a wavelength of 395 nm was calculated based on the following formula. The results are shown in Table 1. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. A(395) indicates the absorbance at a wavelength of 395 nm. Absorbance retention rate (%) = (A(395) after durability test / A(395) before durability test) x 100

[0133] Instead of the film with a cured layer (1), the film with a cured layer (A1), the film with a cured layer (A2), and the film with a cured layer (A3) were used, and evaluations were carried out in the same manner as for the film with a cured layer (1). The results are shown in Table 1.

[0134] [Table 1]

[0135] (Example 10) Preparation of Optical Film (1) A resin solution (solid concentration: 25% by mass) consisting of 70 parts of polymethyl methacrylate resin (Sumitomo Chemical Co., Ltd.: Sumipex MH), 30 parts of rubber particles having a particle diameter of 250 nm and consisting of a core-shell structure of polymethyl methacrylate resin (PMMA) / polybutyl acrylate resin (PBA), 2 parts of a compound represented by formula (UVA-6), and 2-butanone was placed in a mixing tank and stirred to dissolve each component. The obtained solution was uniformly cast onto a glass support using an applicator, dried in an oven at 40° C. for 10 minutes, and then further dried in an oven at 80° C. for 10 minutes. After drying, the optical film (1) was peeled off from the glass support to obtain an optical film (1) having selective light absorption ability. The film thickness of the optical film (1) after drying was 30 μm.

[0136] (Example 11) Preparation of Optical Film (2) A resin solution (solid content concentration: 7% by mass) consisting of 100 parts of cellulose triacetate (acetyl substitution degree: 2.87), 2 parts of the compound represented by formula (UVA-6), and a mixed solution of chloroform and ethanol (mass ratio, chloroform:ethanol=90:10) was placed in a mixing tank and stirred to dissolve each component. The obtained solution was uniformly cast onto a glass support using an applicator, dried in an oven at 40° C. for 10 minutes, and then further dried in an oven at 80° C. for 10 minutes. After drying, the optical film (2) was peeled off from the glass support to obtain an optical film (2) having light selective absorption ability. The film thickness of the optical film (2) after drying was 30 μm.

[0137] (Example 12) Preparation of Optical Film (3) A resin solution (solid content concentration: 20% by mass) consisting of 100 parts of a cycloolefin polymer resin (ARTON F4520 manufactured by JSR), 2 parts of the compound represented by the formula (UVA-6), and a mixed solution of dichloromethane and toluene (mass ratio, dichloromethane:toluene=50:50) was placed in a mixing tank and stirred to dissolve each component. The obtained solution was uniformly cast onto a glass support using an applicator, dried in an oven at 40°C for 10 minutes, and then further dried in an oven at 80°C for 10 minutes. After drying, the optical film (3) was peeled off from the glass support to obtain an optical film (3) having light selective absorption ability. The film thickness of the optical film (3) after drying was 30 μm.

[0138] (Comparative Example 4) Preparation of Optical Film (4) An optical film (4) was produced in the same manner as in Example 10, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A1).

[0139] (Comparative Example 5) Preparation of Optical Film (5) An optical film (5) was produced in the same manner as in Example 11, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A1).

[0140] (Comparative Example 6) Preparation of Optical Film (6) An optical film (6) was produced in the same manner as in Example 10, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A4).

[0141] (Comparative Example 7) Preparation of Optical Film (7) An optical film (7) was produced in the same manner as in Example 11, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A4).

[0142] <Absorbance measurement of optical films> After corona discharge treatment was performed on one side of the optical film (1) obtained in Example 10, an acrylic adhesive was laminated using a laminator, and the film was aged for 7 days under conditions of a temperature of 23°C and a relative humidity of 65%RH to obtain an optical film (1) with adhesive. Next, the optical film (1) with adhesive was cut into a size of 30 mm x 30 mm and laminated to an alkali-free glass (trade name "EAGLE XG" manufactured by Corning Incorporated) to prepare a sample (3). The absorbance of the prepared sample (3) in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The measured absorbance at wavelengths of 395 nm and 430 nm was taken as the absorbance of the optical film (1) at wavelengths of 395 nm and 430 nm. The results are shown in Table 2. The absorbance of the alkali-free glass at wavelengths of 395 nm and 430 nm is nearly zero, and the absorbance of the acrylic adhesive at wavelengths of 395 nm and 430 nm is nearly zero.

[0143] After the absorbance measurement, sample (3) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) under conditions of a temperature of 63°C and a relative humidity of 50% RH, and a weather resistance test was carried out for 200 hours. The absorbance of sample (3) after the weather resistance test was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of sample (3) at a wavelength of 395 nm was calculated based on the following formula. The results are shown in Table 2. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. Absorbance retention rate (%) = (A(395) after durability test / A(395) before durability test) x 100

[0144] Instead of the optical film (1), the optical films (2) to (7) were each used and evaluated in the same manner as the optical film (1). The results are shown in Table 2.

[0145] [Table 2]

[0146] (Example 13) Preparation of adhesive composition (1) <Preparation of acrylic resin (A)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 70.4 parts of butyl acrylate, 20.0 parts of methyl acrylate, and 8.0 parts of 2-phenoxyethyl acrylate, 1.0 parts of 2-hydroxyethyl acrylate, and 0.6 parts of acrylic acid as a monomer, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 1.42 million as determined by GPC in terms of polystyrene, and an Mw / Mn ratio of 5.2. This is designated as acrylic resin (A).

[0147] <Preparation of Pressure-Sensitive Adhesive Composition (1)> 100 parts of the solid content of the ethyl acetate solution (1) (resin concentration: 20%) of the acrylic resin (A) synthesized above was mixed with 0.5 parts of a crosslinker (ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate (solid content concentration 75%), manufactured by Tosoh Corporation, product name "Coronate L"), 0.5 parts of a silane compound (3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM403"), and 2.0 parts of a compound represented by the formula (UVA-6), and ethyl acetate was further added to the mixture so that the solid content concentration became 14%, to obtain a pressure-sensitive adhesive composition (1). The amount of the crosslinker is the number of parts by mass as an active ingredient.

[0148] (Example 14) Preparation of adhesive composition (2) A pressure-sensitive adhesive composition (2) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-7).

[0149] (Example 15) Preparation of adhesive composition (3) A pressure-sensitive adhesive composition (3) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-8).

[0150] (Example 16) Preparation of adhesive composition (4) A pressure-sensitive adhesive composition (4) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-9).

[0151] (Comparative Example 8) Preparation of Pressure Sensitive Adhesive Composition (5) A pressure-sensitive adhesive composition (5) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A1).

[0152] (Example 17) Preparation of pressure-sensitive adhesive layer (1) and pressure-sensitive adhesive sheet (1) The obtained pressure-sensitive adhesive composition (1) was applied to the release-treated surface of a release-treated polyethylene terephthalate separate film (trade name "PLR-382190" available from Lintec Corporation) using an applicator, and dried at 100°C for 1 minute to prepare a pressure-sensitive adhesive layer (1). The thickness of the obtained pressure-sensitive adhesive layer was 15 µm.

[0153] The obtained pressure-sensitive adhesive layer (1) was attached to a 23 μm cycloolefin film using a laminator, and then cured for 7 days under conditions of a temperature of 23° C. and a relative humidity of 65% RH to obtain a pressure-sensitive adhesive sheet (1).

[0154] (Example 18) Preparation of adhesive layer (2) and adhesive sheet (2) An adhesive layer (2) and an adhesive sheet (2) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (2).

[0155] (Comparative Example 9) Preparation of Pressure-Sensitive Adhesive Layer (3) and Pressure-Sensitive Adhesive Sheet (3) An adhesive layer (3) and an adhesive sheet (3) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (5).

[0156] <Measurement of absorbance of adhesive sheet> The obtained adhesive sheet (1) was cut into a size of 30 mm x 30 mm, the separate film was peeled off, and the adhesive layer (1) and non-alkali glass (trade name "EAGLE XG" manufactured by Corning Incorporated) were attached to each other to obtain sample (4). The absorbance of the prepared sample (4) in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The measured absorbance at wavelengths of 395 nm and 430 nm was taken as the absorbance of the adhesive sheet (1) at wavelengths of 395 nm and 430 nm. The results are shown in Table 3. The absorbance at a wavelength of 390 nm was 0 for both the cycloolefin film alone and the non-alkali glass alone.

[0157] <Measurement of absorbance retention of adhesive sheet> After the absorbance measurement, sample (4) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 200 hours under conditions of a temperature of 63°C and a relative humidity of 50% RH, and a weather resistance test was performed. The absorbance of the removed sample (4) was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of sample (4) at 395 nm was calculated based on the following formula. The results are shown in Table 3. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. Absorbance retention rate (%) = (A(395) after durability test / A(395) before durability test) x 100

[0158] Instead of the pressure-sensitive adhesive sheet (1), the pressure-sensitive adhesive sheet (2) and the pressure-sensitive adhesive sheet (3) were used, and the evaluation was carried out in the same manner as for the pressure-sensitive adhesive sheet (1). The results are shown in Table 3.

[0159] [Table 3]

[0160] (Example 19) Synthesis of compound represented by formula (UVA-10) [ka] Under a nitrogen atmosphere, 2.5 parts of the compound represented by formula (M-9), 15.1 parts of benzoyl(phenyliodonio)(trifluoromethanesulfonyl)methanide, 0.4 parts of copper(I) chloride, and 100 parts of dioxane were mixed. The resulting mixture was stirred at 30° C. for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 1.7 parts of the compound represented by formula (M-10).

[0161] [ka] Under a nitrogen atmosphere, 1.5 parts of the compound represented by formula (M-10), 1.4 parts of methyl triflate, and 10 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 1.3 parts of diisopropylethylamine and 0.7 parts of malononitrile were added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 1.0 part of the compound represented by formula (UVA-10).

[0162] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-10) was produced. 1 H-NMR (heavy DMSO) δ: 1.00 (s, 3H), 1.15 (s, 3H), 1.86 (m, 2H), 2.18 (m, 2H), 2.32~2.91 (m, 4H), 3.50~4.20 (m, 4H) LC-MS; [M+H] + =343.5

[0163] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-10) was 384.2 nm. The ε(λmax) of the compound represented by the formula (UVA-10) was 1.29 L / (g cm), ε(λmax+30 nm) was 0.075 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 17.2.

[0164] (Example 20) Synthesis of compound represented by formula (UVA-11) [ka] Under a nitrogen atmosphere, 5 parts of the compound represented by formula (M-6), 4.9 parts of methyl triflate, 3.8 parts of diisopropylethylamine, and 10 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 5 parts of dimethylamine was added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 3.1 parts of the compound represented by formula (UVA-11).

[0165] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-11) was produced. 1 H-NMR (heavy DMSO) δ: 1.08 (s, 6H), 2.42 (s, 2H), 2.55 (s, 2H), 3.40 (m, 6H) LC-MS; [M+H] + =241.5

[0166] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by formula (UVA-11) was 379.4 nm. The ε(λmax) of the compound represented by formula (UVA-11) was 1.93 L / (g cm), ε(λmax+30 nm) was 0.063 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 30.6.

[0167] (Example 21) Synthesis of compound represented by formula (UVA-12) [ka] Under a nitrogen atmosphere, 5 parts of the compound represented by formula (M-6), 4.9 parts of methyl triflate, 3.8 parts of diisopropylethylamine, and 10 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 8.4 parts of diethylamine was added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 2.9 parts of the compound represented by formula (UVA-12).

[0168] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-12) was produced. 1 H-NMR (heavy DMSO) δ: 1.08 (s, 6H), 1.39 (t, 6H), 2.44 (s, 2H), 2.58 (s, 2H), 3.74 (m, 4H) LC-MS; [M+H] + =269.5

[0169] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by formula (UVA-12) was 380.5 nm. The ε(λmax) of the compound represented by formula (UVA-12) was 1.75 L / (g cm), ε(λmax+30 nm) was 0.098 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 17.6.

[0170] (Example 22) Synthesis of compound represented by formula (UVA-13) [ka] Under a nitrogen atmosphere, 5 parts of the compound represented by formula (M-6), 4.9 parts of methyl triflate, 3.8 parts of diisopropylethylamine, and 10 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 14.8 parts of dibutylamine was added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 2.5 parts of the compound represented by formula (UVA-13).

[0171] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-13) was produced. 1 H-NMR (heavy DMSO) δ: 0.99 (t, 6H), 1.07 (s, 6H), 1.32~1.46 (m, 4H), 1.70 (m, 4H), 2.40 (s, 2H), 2.57 (s, 2H), 3.32~3.85 (m, 4H). LC-MS; [M+H] + =325.5

[0172] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by formula (UVA-13) was 382.8 nm. The ε(λmax) of the compound represented by formula (UVA-13) was 1.42 L / (g cm), ε(λmax+30 nm) was 0.095 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 0.095 L / (g cm). The figure was 14.9.

[0173] (Example 23) Synthesis of compound represented by formula (UVA-14) [ka] Under a nitrogen atmosphere, 5 parts of the compound represented by formula (M-6), 3.6 parts of potassium carbonate, 7.7 parts of methyl triflate, and 40 parts of methyl ethyl ketone were mixed and stirred at 0 to 5° C. for 4 hours. 2 parts of azetidine was added to the resulting mixture and stirred at 0 to 5° C. for 10 minutes. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 2.6 parts of the compound represented by formula (UVA-14).

[0174] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-14) was produced. 1 H-NMR (heavy DMSO) δ: 1.05 (s, 6H), 2.14 (s, 2H), 2.45~2.53 (m, 4H), 4.36 (t, 2H), 4.91 (t, 2H) LC-MS; [M+H] + =253.3

[0175] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-14) was 377.2 nm. The ε(λmax) of the compound represented by the formula (UVA-14) was 1.93 L / (g cm), ε(λmax+30 nm) was 0.028 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 68.9.

[0176] (Example 24) Synthesis of compound represented by formula (UVA-15) [ka] Under a nitrogen atmosphere, 4.0 parts of the compound represented by formula (M-6), 3.7 parts of methyl triflate, and 40 parts of acetonitrile were mixed and stirred at 20 to 30° C. for 3 hours. 2.9 parts of diisopropylethylamine and 40 parts of a solution of methylamine dissolved in tetrahydrofuran (methylamine concentration: 7% by mass) were added to the resulting mixture and stirred at 20 to 30° C. for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 1.9 parts of the compound represented by formula (UVA-15).

[0177] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-15) was produced. 1 H-NMR (heavy DMSO) δ: 0.98 (s, 6H), 2.48~2.58 (m, 4H), 3.03 (s, 3H), 9.15 (s, 1H) LC-MS; [M+H]+ =226.5

[0178] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-15) was 364.8 nm. The ε(λmax) of the compound represented by the formula (UVA-15) was 1.86 L / (g cm), ε(λmax+30 nm) was 0.066 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 28.2.

[0179] (Example 25) Synthesis of compound represented by formula (UVA-16) [ka] Under a nitrogen atmosphere, 4.0 parts of the compound represented by formula (M-6), 3.7 parts of methyl triflate, and 40 parts of acetonitrile were mixed and stirred at 20 to 30° C. for 3 hours. 2.9 parts of diisopropylethylamine and 40 parts of a solution in which ethylamine was dissolved in tetrahydrofuran (ethylamine concentration: 10% by mass) were added to the resulting mixture and stirred at 20 to 30° C. for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 1.5 parts of the compound represented by formula (UVA-16).

[0180] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-16) was produced. 1 H-NMR (heavy DMSO) δ: 0.98 (s, 6H), 2.48~2.58 (m, 4H), 3.03 (t, 3H), 4.21 (m, 2H), 9.15 (s, 1H) LC-MS; [M+H] + =240.5

[0181] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by formula (UVA-16) was 364.8 nm. The ε(λmax) of the compound represented by formula (UVA-16) was 1.80 L / (g cm), ε(λmax+30 nm) was 0.074 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 24.4.

[0182] (Example 26) Synthesis of compound represented by formula (UVA-17) [ka] Under a nitrogen atmosphere, 1.7 parts of the compound represented by formula (M-6), 1.6 parts of methyl triflate, and 17 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 1.2 parts of diisopropylethylamine and 100 parts of a solution of ammonia dissolved in tetrahydrofuran (ammonia molar concentration: 0.4 mol%) were added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 0.7 parts of the compound represented by formula (UVA-17).

[0183] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-17) was produced. 1 H-NMR (heavy DMSO) δ: 0.98 (s, 6H), 2.48~2.58 (m, 4H), 9.15 (m, 2H) LC-MS; [M+H] + =213.5

[0184] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by formula (UVA-17) was 352.6 nm. The ε(λmax) of the compound represented by formula (UVA-17) was 1.75 L / (g cm), ε(λmax+30 nm) was 0.11 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 15.9.

[0185] (Example 27) Preparation of photoselective absorption composition (5) A light selective absorbing composition (5) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-10).

[0186] (Example 28) Preparation of photoselective absorption composition (6) A light selective absorbing composition (6) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-11).

[0187] (Example 29) Preparation of photoselective absorption composition (7) A light selective absorbing composition (7) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-12).

[0188] (Example 30) Preparation of photoselective absorption composition (8) A light selective absorbing composition (7) was prepared in the same manner as in Example 5, except that the compound represented by formula (UVA-6) was replaced with a compound represented by formula (UVA-13).

[0189] (Example 31) Preparation of film (2) with cured layer A film (2) with a cured layer was obtained in the same manner as in Example 9, except that the light selective absorbing composition (1) was replaced with the light selective absorbing composition (6).

[0190] (Example 32) Preparation of film (3) with cured layer A film (3) with a cured layer was obtained in the same manner as in Example 9, except that the light selective absorbing composition (1) was replaced with the light selective absorbing composition (7).

[0191] <Measurement of absorbance and absorbance retention rate of film with cured layer> The absorbance was measured in the same manner as in <Measurement of absorbance of film with cured layer> described above, except that film with cured layer (2) and film with cured layer (3) were used instead of film with cured layer (1). In addition, the absorbance retention of the film with cured layer (1) obtained in Example 9 and the film with cured layer (A3) obtained in Comparative Example 3 were measured in the same manner as in <Measurement of absorbance retention of film with cured layer> described above, except that the time of insertion into the sunshine weather meter was 75 hours. Furthermore, the absorbance retention was measured in the same manner as in <Measurement of absorbance retention of film with cured layer> above, except that film with cured layer (2) and film with cured layer (3) were used instead of film with cured layer (1) and the time of insertion into the sunshine weather meter was changed to 75 hours. These results are shown in Table 4. Table 4 also shows the absorbance values ​​of the film with a cured layer (1) obtained in Example 9 and the film with a cured layer (A3) obtained in Comparative Example 3.

[0192] [Table 4]

[0193] (Example 33) Preparation of adhesive composition (6) A pressure-sensitive adhesive composition (6) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to a compound represented by formula (UVA-10).

[0194] (Example 34) Preparation of adhesive composition (7) A pressure-sensitive adhesive composition (7) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to a compound represented by formula (UVA-11).

[0195] (Example 35) Preparation of adhesive composition (8) A pressure-sensitive adhesive composition (8) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-12).

[0196] (Example 36) Preparation of adhesive composition (9) A pressure-sensitive adhesive composition (9) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to a compound represented by formula (UVA-13).

[0197] (Example 37) Preparation of adhesive layer (4) and adhesive sheet (4) An adhesive layer (4) and an adhesive sheet (4) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (4).

[0198] (Example 38) Preparation of pressure-sensitive adhesive layer (5) and pressure-sensitive adhesive sheet (5) An adhesive layer (5) and an adhesive sheet (5) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (6).

[0199] (Example 39) Preparation of adhesive layer (6) and adhesive sheet (6) An adhesive layer (6) and an adhesive sheet (6) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (7).

[0200] (Example 40) Preparation of adhesive layer (7) and adhesive sheet (7) An adhesive layer (7) and an adhesive sheet (7) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (8).

[0201] (Example 41) Preparation of adhesive layer (8) and adhesive sheet (8) An adhesive layer (8) and an adhesive sheet (8) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (9).

[0202] <Measurement of absorbance and absorbance retention rate of pressure sensitive adhesive sheet> Except for using the pressure-sensitive adhesive sheets (4) to (8) instead of the pressure-sensitive adhesive sheet (1), the absorbance and absorbance retention were measured in the same manner as in <Measurement of absorbance of pressure-sensitive adhesive sheets> and <Measurement of absorbance retention of pressure-sensitive adhesive sheets> described above. The results are shown in Table 5.

[0203] [Table 5]

[0204] (Example 42) Synthesis of compound represented by formula (UVA-20) [ka] Under a nitrogen atmosphere, 17 parts of the compound represented by formula (M-3), 12.2 parts of potassium carbonate, 15.9 parts of 1-chloromethyl-4-fluoro-1,4-diazoniabicyclo[2.2.2.]octane bis(tetrafluoroborate) (Select Fluoro, a registered trademark of Air Products and Chemicals) and 85 parts of methyl ethyl ketone were mixed and stirred in an ice bath for 3 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 3.7 parts of the compound represented by formula (M-11).

[0205] [ka] Under a nitrogen atmosphere, 18 parts of the compound represented by formula (M-11), 28 parts of methyl triflate, and 90 parts of methyl ethyl ketone were mixed and stirred for 3 hours at 20 to 30° C. To the resulting mixture, 13.0 parts of potassium carbonate and 8.4 parts of malononitrile were added and stirred for 3 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 5.8 parts of the compound represented by formula (UVA-20).

[0206] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-20) was produced. 1 H-NMR (heavy DMSO) δ: 1.08 (s, 6H), 1.97 (m, 4H), 2.40 (d, 2H), 2.50 (d, 2H), 3.53 (m, 2H), 3.86 (m, 2H) LC-MS; [M+H] + =260.5

[0207] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-20) was 407.5 nm. The ε(λmax) of the compound represented by the formula (UVA-20) was 2.30 L / (g cm), ε(λmax+30 nm) was 0.041 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 56.0.

[0208] (Example 43) Synthesis of compound represented by formula (UVA-21) [ka] Under a nitrogen atmosphere, 5 parts of 3-hydroxypiperidine, 13.6 parts of tertiary butyldiphenylsilyl chloride, 6.7 parts of imidazole, and 40 parts of dichloromethane were mixed and stirred for 4 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 10.5 parts of a compound represented by formula (M-12).

[0209] [ka] Under a nitrogen atmosphere, 4.0 parts of the compound represented by formula (M-6), 3.2 parts of diisopropylethylamine, 4.0 parts of methyl triflate, and 80 parts of acetonitrile were mixed and stirred at 20 to 30° C. for 4 hours. 8.3 parts of the compound represented by formula (M-12) was added to the obtained mixture and stirred at 20 to 30° C. for 3 hours. The solvent was distilled off from the obtained mixture, and the mixture was purified to obtain 6.5 parts of the compound represented by formula (UVA-21).

[0210] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-21) was produced. 1H-NMR (heavy DMSO) δ::0.97(s, 6H), 1.04(s, 9H), 1.70(m, 2H), 1.85(m, 2H), 2.48(s, 2H), 2. 65(s, 2H), 3.72(m, 2H), 3.94(m, 2H), 4.13(m, 1H), 7.42~7.52(m, 6H), 7.61~7.64(m, 4H) LC-MS; [M+H] + =535.9

[0211] (Example 44) Synthesis of compound represented by formula (UVA-22) [ka] Under a nitrogen atmosphere, 4.2 parts of the compound represented by formula (UVA-21) and 50 parts of a 1M solution of tetrabutylammonium fluoride / tetrahydrofuran were mixed and stirred for 40 hours at 20 to 30° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 1.8 parts of the compound represented by formula (UVA-22).

[0212] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-22) was produced. 1 H-NMR (heavy DMSO) δ: 0.98 (s, 6H), 1.59 (m, 2H), 1.92 (m, 2H), 2.67 (s, 2H), 3.68~3.95 (m, 4H), 4.97 (m, 1H) LC-MS; [M+H] + =297.5

[0213] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-22) was 384.6 nm. The ε(λmax) of the compound represented by the formula (UVA-22) was 1.43 L / (g cm), ε(λmax+30 nm) was 0.085 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 16.8.

[0214] (Example 45) Synthesis of compound represented by formula (UVA-23) [ka] Under a nitrogen atmosphere, 5.0 parts of the compound represented by formula (M-6), 3.6 parts of potassium carbonate, 7.7 parts of methyl triflate, and 40 parts of acetonitrile were mixed and stirred at 20 to 30° C. for 4 hours. 2.0 parts of azetidine was added to the obtained mixture and stirred at 20 to 30° C. for 4 hours. The solvent was distilled off from the obtained mixture, and the mixture was purified to obtain 2.3 parts of the compound represented by formula (UVA-23).

[0215] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-23) was produced. 1 H-NMR (heavy DMSO) δ: 1.05 (s, 6H), 2.14 (s, 2H), 2.44~2.53 (m, 4H), 4.36 (t, 2H), 4.91 (t, 2H) LC-MS; [M+H] + =253.5

[0216] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-23) was 377.2 nm. The ε(λmax) of the compound represented by the formula (UVA-23) was 1.93 L / (g cm), ε(λmax+30 nm) was 0.028 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 68.9.

[0217] (Example 46) Synthesis of compound represented by formula (UVA-26) [ka] A 500 mL four-neck flask equipped with a Dimroth condenser and a thermometer was filled with 40 parts of malonaldehyde dianilide hydrochloride, 22 parts of diisopropylamine, 200 parts of acetonitrile, and 11 parts of malononitrile, and the mixture was stirred in an ice bath for 5 hours. The solvent was distilled off from the mixture obtained, and the mixture was purified to obtain 29 parts of the compound represented by formula (M-15).

[0218] [ka] Under a nitrogen atmosphere, 7 parts of the compound represented by formula (M-15), 5 parts of diisopropylethylamine, 56 parts of acetonitrile, and 7 parts of paratoluenesulfonyl cyanide were mixed and refluxed and stirred for 3 hours at 80° C. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 0.1 part of the compound represented by formula (UVA-26).

[0219] LC-MS measurement confirmed that the compound represented by formula (UVA-26) was produced. LC-MS; [M+H] + =221.5

[0220] (Synthesis Example 5) Synthesis of compound represented by formula (UVA-A5) [ka] Under a nitrogen atmosphere, 40 parts of malonaldehyde dianilide hydrochloride, 10.7 parts of malononitrile, and 200 parts of acetonitrile were mixed, and 22 parts of diisopropylethylamine were added dropwise while stirring in an ice bath, and the mixture was stirred for 4 hours. The solvent was distilled off from the resulting mixture, and the mixture was purified to obtain 28 parts of the compound represented by the formula (M-90).

[0221] [ka] Under a nitrogen atmosphere, 5.0 parts of the compound represented by formula (M-90), 2.9 parts of acetic anhydride, 6.6 parts of diisopropylethylamine, and 40 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. 2.7 parts of pyrrolidine was added to the obtained mixture and stirred for another 1 hour, and the solvent was distilled off from the obtained mixture and purified to obtain 2.6 parts of the compound represented by formula (UVA-A5).

[0222] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-A5) was produced. 1 H-NMR (heavy DMSO) δ: 1.83~2.00 (m, 4H), 3.37~3.40 (m, 2H), 3.61~3.65 (t, 2H), 5.39~5.45 (t, 1H), 7.55~7.58 (d, 1H), 7.84~7.87 (d, 1H) LC-MS; [M+H] + =174.5

[0223] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-A5) was 379.3 nm. The ε(λmax) of the compound represented by the formula (UVA-A5) was 3.41 L / (g cm), ε(λmax+30 nm) was 0.10 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 33.5.

[0224] (Synthesis Example 6) Synthesis of compound represented by formula (UVA-A6) [ka] Under a nitrogen atmosphere, 5.0 parts of the compound represented by formula (M-90), 2.9 parts of acetic anhydride, 6.6 parts of diisopropylethylamine, and 40 parts of acetonitrile were mixed and stirred for 3 hours at 20 to 30° C. 3.0 parts of piperidine was added to the resulting mixture and stirred for another 1 hour, and the solvent was distilled off from the resulting mixture, followed by purification to obtain 2.7 parts of the compound represented by formula (UVA-A6).

[0225] LC-MS measurement and 1 H-NMR analysis confirmed that the compound represented by formula (UVA-A6) was produced. 1 H-NMR (heavy DMSO) δ: 1.72 (m, 6H), 3.40~3.44 (m, 4H), 5.44~5.70 (m, 1H) 6.98~7.00 (d, 1H), 7.19~7.25 (m, 1H) LC-MS; [M+H] + =188.5

[0226] The maximum absorption wavelength and gram absorption coefficient were measured in the same manner as above. The maximum absorption wavelength of the compound represented by the formula (UVA-A6) was 374.7 nm. The ε(λmax) of the compound represented by the formula (UVA-A6) was 2.89 L / (g cm), ε(λmax+30 nm) was 0.14 L / (g cm), and ε(λmax) / ε(λmax+30 nm) was 20.6.

[0227] (Example 47) Preparation of adhesive composition (10) A pressure-sensitive adhesive composition (10) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to a compound represented by formula (UVA-23) and its content was 0.5 parts per 100 parts of the acrylic resin (A).

[0228] (Comparative Example 10) Preparation of adhesive composition (11) A pressure-sensitive adhesive composition (11) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to the compound represented by formula (UVA-A5) and its content was 1.5 parts per 100 parts of the acrylic resin (A).

[0229] (Comparative Example 11) Preparation of adhesive composition (12) A pressure-sensitive adhesive composition (12) was obtained in the same manner as in Example 13, except that the compound represented by formula (UVA-6) was changed to a compound represented by formula (UVA-A6) and its content was 1.5 parts per 100 parts of the acrylic resin (A).

[0230] (Example 48) Preparation of adhesive layer (9) and adhesive sheet (9) An adhesive layer (9) and an adhesive sheet (9) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (10).

[0231] (Comparative Example 12) Preparation of pressure-sensitive adhesive layer (10) and pressure-sensitive adhesive sheet (10) An adhesive layer (10) and an adhesive sheet (10) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (11).

[0232] (Comparative Example 13) Preparation of pressure-sensitive adhesive layer (11) and pressure-sensitive adhesive sheet (11) An adhesive layer (11) and an adhesive sheet (11) were produced in the same manner as in Example 17, except that the adhesive composition (1) was changed to the adhesive composition (12).

[0233] <Measurement of absorbance and absorbance retention rate of pressure sensitive adhesive sheet> Except for using adhesive sheets (9) to (11) instead of adhesive sheet (1), the absorbance and absorbance retention were measured in the same manner as in <Measurement of absorbance of adhesive sheets> and <Measurement of absorbance retention of adhesive sheets> described above. The results are shown in Table 6.

[0234] [Table 6]

[0235] (Example 49) Preparation of adhesive composition (13) <Preparation of acrylic resin (A-2)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 96 parts of butyl acrylate as a monomer, 3 parts of 2-hydroxyethyl acrylate and 1 part of acrylic acid, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while the internal temperature was raised to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and when the concentration of the acrylic resin reached 35%, the addition of ethyl acetate was stopped, and the temperature was kept at this temperature until 12 hours had passed from the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The weight average molecular weight Mw of the obtained acrylic resin in terms of polystyrene by GPC was 1.4 million. The Mw / Mn was 4.8. This is designated as acrylic resin (A-2).

[0236] <Preparation of Pressure-Sensitive Adhesive Composition (13)> 100 parts of the solid content of the ethyl acetate solution (resin concentration: 20%) of the acrylic resin (A-2) synthesized above was mixed with 0.5 parts of a crosslinker (ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate (solid content concentration 75%), manufactured by Tosoh Corporation, product name "Coronate L"), 0.3 parts of a silane compound (1,6-bis(trimethoxysilyl)hexane, manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM3066"), and 3 parts of a compound represented by the formula (UVA-6), and ethyl acetate was added to the mixture so that the solid content concentration became 14%, to obtain a pressure-sensitive adhesive composition (13). The amount of the crosslinker is the mass part as an active ingredient.

[0237] (Example 50) Preparation of adhesive composition (14) <Preparation of acrylic resin (A-3)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 60 parts of methyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 20 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The weight average molecular weight Mw of the obtained acrylic resin was 920,000 as calculated based on polystyrene by GPC. Mw / Mn was 7.8. This is designated as acrylic resin (A-3).

[0238] <Preparation of Pressure-Sensitive Adhesive Composition (14)> A pressure-sensitive adhesive composition (14) was obtained in the same manner as in Example 49, except that the acrylic resin (A-3) synthesized above was used instead of the acrylic resin (A-2).

[0239] (Example 51) Preparation of adhesive composition (15) <Preparation of acrylic resin (A-4)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 10 parts of butyl acrylate, 60 parts of methyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 10 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The weight average molecular weight Mw of the obtained acrylic resin was 940,000 as calculated based on polystyrene by GPC. Mw / Mn was 8.5. This is designated as acrylic resin (A-4).

[0240] <Preparation of Pressure-Sensitive Adhesive Composition (15)> A pressure-sensitive adhesive composition (15) was obtained in the same manner as in Example 49, except that the acrylic resin (A-4) synthesized above was used instead of the acrylic resin (A-2).

[0241] (Example 52) Preparation of adhesive composition (16) <Preparation of acrylic resin (A-5)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 20 parts of butyl acrylate, 50 parts of methyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 10 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 910,000 as calculated based on polystyrene by GPC, and is designated as acrylic resin (A-5).

[0242] <Preparation of Pressure-Sensitive Adhesive Composition (16)> A pressure-sensitive adhesive composition (16) was obtained in the same manner as in Example 49, except that the acrylic resin (A-5) synthesized above was used instead of the acrylic resin (A-2).

[0243] (Example 53) Preparation of adhesive composition (17) <Preparation of acrylic resin (A-6)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 50 parts of butyl acrylate, 10 parts of methyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 20 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 1.2 million as determined by GPC in terms of polystyrene standards, and is designated as acrylic resin (A-6).

[0244] <Preparation of Pressure-Sensitive Adhesive Composition (17)> A pressure-sensitive adhesive composition (17) was obtained in the same manner as in Example 49, except that the acrylic resin (A-6) synthesized above was used instead of the acrylic resin (A-2).

[0245] (Example 54) Preparation of adhesive composition (18) <Preparation of acrylic resin (A-7)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 60 parts of butyl acrylate, 10 parts of methyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 10 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, a solution of 0.14 parts of azobisisobutyronitrile (polymerization initiator) dissolved in 10 parts of ethyl acetate was added in its entirety. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 1,180,000 as determined by GPC in terms of polystyrene standards, and is designated as acrylic resin (A-7).

[0246] <Preparation of Pressure-Sensitive Adhesive Composition (18)> A pressure-sensitive adhesive composition (18) was obtained in the same manner as in Example 49, except that the acrylic resin (A-7) synthesized above was used instead of the acrylic resin (A-2).

[0247] (Example 55) Preparation of adhesive composition (19) <Preparation of acrylic resin (A-8)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with a mixed solution of 81.8 parts of ethyl acetate as a solvent, 70 parts of butyl acrylate, 10 parts of 2-hydroxyethyl acrylate, 10 parts of acrylic acid and 10 parts of 2-phenoxyethyl acrylate as monomers, and the air in the reaction vessel was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55°C. Then, the entire amount of a solution in which 0.14 parts of azobisisobutyronitrile (polymerization initiator) was dissolved in 10 parts of ethyl acetate was added. After adding the initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C, and the addition of ethyl acetate was stopped when the concentration of the acrylic resin reached 35%, and the temperature was kept at this temperature until 12 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the acrylic resin to 20%, and an ethyl acetate solution of the acrylic resin was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 1.1 million as calculated based on polystyrene by GPC, and was designated acrylic resin (A-8).

[0248] <Preparation of Pressure-Sensitive Adhesive Composition (19)> A pressure-sensitive adhesive composition (19) was obtained in the same manner as in Example 49, except that the acrylic resin (A-8) synthesized above was used instead of the acrylic resin (A-2).

[0249] <Evaluation of crystal precipitation (bleed resistance) of adhesive layer> The adhesive composition (13) was applied to the release-treated surface of a release-treated polyethylene terephthalate film (trade name "PLR-382190" obtained from Lintec Corporation) using an applicator, and dried at 100°C for 1 minute to prepare an adhesive layer. A separate film was further laminated on the other side of this adhesive layer to obtain an adhesive layer with double-sided separate films. The thickness of the obtained adhesive layer was 15 μm.

[0250] The resulting pressure-sensitive adhesive layer with double-sided separate films was aged for 7 days under conditions of a temperature of 23°C and a relative humidity of 65%. After aging, the pressure-sensitive adhesive layer with double-sided separate films was examined using a microscope to check for the presence or absence of crystal precipitation of the compound within the surface. Cases where there was no crystal precipitation were evaluated as a, and cases where there was crystal precipitation were evaluated as b. The evaluation results are shown in the "After aging" column of Table 7. The resulting pressure-sensitive adhesive layer with double-sided separate films was stored for one month under air at a temperature of 40°C. After storage, the pressure-sensitive adhesive layer with double-sided separate films was examined using a microscope to check for the presence or absence of crystal precipitation of the compound within the surface. Cases where no crystal precipitation was observed were evaluated as a, and cases where crystal precipitation was observed were evaluated as b. The evaluation results are shown in the "40°C 1M" column in Table 7.

[0251] The presence or absence of crystal precipitation was confirmed in the same manner, except that the pressure-sensitive adhesive composition (13) was replaced with the pressure-sensitive adhesive composition (14) to (19). The results are shown in Table 7.

[0252] [Table 7] (Example 56) Preparation of adhesive layer (12) and adhesive sheet (12) The obtained pressure-sensitive adhesive composition (13) was applied to the release-treated surface of a release-treated polyethylene terephthalate separate film (trade name "PLR-382190" available from Lintec Corporation) using an applicator, and dried at 100°C for 1 minute to produce a pressure-sensitive adhesive layer (12). The thickness of the obtained pressure-sensitive adhesive layer was 15 µm.

[0253] The obtained adhesive layer (12) was laminated to a 23 μm cycloolefin film not containing an ultraviolet absorber using a laminator, and then cured for 7 days under conditions of a temperature of 23° C. and a relative humidity of 65% to obtain an adhesive sheet (12).

[0254] (Example 57) Preparation of adhesive layer (13) and adhesive sheet (13) An adhesive layer (13) and an adhesive sheet (13) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (14).

[0255] (Example 58) Preparation of adhesive layer (14) and adhesive sheet (14) An adhesive layer (14) and an adhesive sheet (14) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (15).

[0256] (Example 59) Preparation of adhesive layer (15) and adhesive sheet (15) An adhesive layer (15) and an adhesive sheet (15) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (16).

[0257] (Example 60) Preparation of adhesive layer (16) and adhesive sheet (16) An adhesive layer (16) and an adhesive sheet (16) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (17).

[0258] (Example 61) Preparation of adhesive layer (17) and adhesive sheet (17) An adhesive layer (17) and an adhesive sheet (17) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (18).

[0259] (Example 62) Preparation of adhesive layer (18) and adhesive sheet (18) An adhesive layer (18) and an adhesive sheet (18) were produced in the same manner as in Example 56, except that the adhesive composition (13) was changed to the adhesive composition (19).

[0260] <Measurement of absorbance retention of adhesive sheet> The obtained adhesive sheet (12) was cut into a size of 30 mm x 30 mm, the separate film was peeled off, and the adhesive layer (12) and non-alkali glass [trade name "EAGLE XG" manufactured by Corning Incorporated] were attached to each other to obtain sample (5). The absorbance of the prepared sample (5) in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The measured absorbance at a wavelength of 400 nm was taken as the absorbance of the adhesive sheet (12) at a wavelength of 400 nm. The results are shown in Table 8. The absorbance at a wavelength of 400 nm was 0 for both the cycloolefin film alone and the non-alkali glass alone.

[0261] After the absorbance measurement, sample (5) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 150 hours under conditions of a temperature of 63°C and a relative humidity of 50% RH, and a weather resistance test was performed. The absorbance of the removed sample (5) was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of the sample at a wavelength of 400 nm was calculated based on the following formula. The results are shown in Table 8. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. In addition, the absorbance retention rate was also determined when sample (5) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 225 hours under conditions of a temperature of 63° C. and a relative humidity of 50% RH. Absorbance retention rate (%) = (A(400) after durability test / A(400) before durability test) x 100

[0262] The absorbance retention was measured in the same manner, except that the pressure-sensitive adhesive sheet (12) was replaced with the pressure-sensitive adhesive sheets (13) to (18). The results are shown in Table 8.

[0263] [Table 8]

[0264] (Example 63) Preparation of adhesive sheet (19) A pressure-sensitive adhesive sheet (19) was produced in the same manner as in Example 56, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0265] (Example 64) Preparation of adhesive sheet (20) A pressure-sensitive adhesive sheet (20) was produced in the same manner as in Example 57, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0266] (Example 65) Preparation of adhesive sheet (21) A pressure-sensitive adhesive sheet (21) was produced in the same manner as in Example 58, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0267] (Example 66) Preparation of adhesive sheet (22) A pressure-sensitive adhesive sheet (22) was produced in the same manner as in Example 59, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0268] (Example 67) Preparation of adhesive sheet (23) A pressure-sensitive adhesive sheet (23) was produced in the same manner as in Example 60, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0269] (Example 68) Preparation of adhesive sheet (24) A pressure-sensitive adhesive sheet (24) was produced in the same manner as in Example 61, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0270] (Example 69) Preparation of adhesive sheet (25) A pressure-sensitive adhesive sheet (25) was produced in the same manner as in Example 62, except that the 23 μm cycloolefin film not containing an ultraviolet absorbent was changed to a 23 μm cycloolefin film containing an ultraviolet absorbent.

[0271] <Measurement of absorbance retention of adhesive sheet> The obtained adhesive sheet (19) was cut into a size of 30 mm x 30 mm, the separate film was peeled off, and the adhesive layer (19) and non-alkali glass [trade name "EAGLE XG" manufactured by Corning Incorporated] were attached to each other to obtain sample (6). The absorbance of the prepared sample (5) in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). The measured absorbance at a wavelength of 405 nm was taken as the absorbance of the adhesive sheet (19) at a wavelength of 405 nm. The results are shown in Table 9. The absorbance of the non-alkali glass alone at a wavelength of 405 nm was 0.

[0272] After the absorbance measurement, sample (6) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 150 hours under conditions of a temperature of 63°C and a relative humidity of 50% RH, and a weather resistance test was performed. The absorbance of the removed sample (5) was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of the sample at a wavelength of 405 nm was calculated based on the following formula. The results are shown in Table 9. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. In addition, the absorbance retention rate was also determined when sample (6) was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 225 hours under conditions of a temperature of 63° C. and a relative humidity of 50% RH. Absorbance retention rate (%) = (A(405) after durability test / A(405) before durability test) x 100

[0273] The absorbance retention was measured in the same manner, except that the pressure-sensitive adhesive sheet (19) was replaced with the pressure-sensitive adhesive sheets (20) to (25). The results are shown in Table 9.

[0274] [Table 9] (Example 70) <Preparation of Resin Composition for Eyeglass Lenses> 40 parts of xylylene diisocyanate, 60 parts of trimethylolpropane tris(thioglycolate), 1.6 parts of the compound represented by formula (UVA-6), 0.2 parts of a release agent (trade name: ZELEC-UN, obtained from Sigma-Aldrich), and 0.03 parts of dibutyldichlorotin were mixed and stirred. The mixture obtained was left to stand in a vacuum dryer for 1 hour and degassed. The mixture obtained was poured into a glass mold and heated at 120°C for 1 hour. Only the resin plate was peeled off to prepare a resin plate of 2 mm thickness and 3 cm x 3 cm.

[0275] <Measurement of absorbance retention of resin plate> The absorbance of the resin plate obtained above in the wavelength range of 300 to 800 nm was measured in 1 nm steps using a spectrophotometer (UV-2450: manufactured by Shimadzu Corporation). After the measurement, the resin plate was placed in a Sunshine Weather Meter (manufactured by Suga Test Instruments Co., Ltd.) for 75 hours under conditions of a temperature of 63°C and a relative humidity of 50% RH to conduct a weather resistance test. The absorbance of the removed resin plate was measured in the same manner as above. From the measured absorbance, the absorbance retention rate of the sample at a wavelength of 420 nm was calculated based on the following formula. The results are shown in Table 10. The closer the absorbance retention rate is to 100, the less deterioration of the light selective absorption function and the better the weather resistance. In addition, eyeglass lenses are required to have a good absorbance retention rate at a wavelength of 420 nm in order to efficiently block blue light, which is likely to have adverse effects on health. Also, the higher the A(420) / A(480) value, the less coloring is needed to block blue light. Absorbance retention rate (%) = (A(420) after durability test / A(420) before durability test) x 100

[0276] [Table 10]

[0277] The compound of the present invention has high absorption selectivity for visible light with a short wavelength of 380 to 400 nm, and has high absorbance retention even after a weather resistance test, and has good weather resistance.

Claims

1. A compound represented by formula (II): 【Chemistry 1】 [In formula (II), R 3 , R 4 and R 5 each independently represents an electron-withdrawing group, and the electron-withdrawing group is a halogen atom, a cyano group, -SCF 3 or a group represented by formula (X-1). 【Chemistry 2】 (In formula (X-1), X 1 represents -CO- or -COO-; R 222 represents an alkyl group having 1 to 25 carbon atoms, and * represents a bond. R 1 and R 2 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 25 carbon atoms. Ring W1 represents a 6-membered ring structure having at least one double bond as a ring component, not having aromaticity, and not containing a heteroatom as a ring component.

2. A compound represented by formula (II): 【Chemistry 3】 [In formula (II), R 3 , R 4 and R 5 each independently represents an electron-withdrawing group, and the electron-withdrawing group is a halogen atom, a cyano group, -SCF 3 or a group represented by formula (X-1). 【Chemistry 4】 (In formula (X-1), X 1 represents -CO- or -COO-; R 222 represents an alkyl group having 1 to 25 carbon atoms, and * represents a bond. R 1 and R 2 are linked to each other to form a ring, and the ring is a 3- to 10-membered ring that contains only one nitrogen atom as a ring component and does not contain any heteroatoms other than the nitrogen atom, and may have a hydroxyl group or a tert-butyldiphenylsilyl group as a substituent. Ring W1 represents a 6-membered ring structure having at least one double bond as a ring component, not having aromaticity, and not containing a heteroatom as a ring component.

3. R 1 and R 2 The compound according to claim 2 , wherein the ring formed by linking together has no unsaturated bond.

4. R 1 and R 2 The compound according to claim 2 or 3, wherein the ring formed by linking together has no substituent.

5. R 3 is a cyano group, -F, -SCF 3 or a group represented by formula (X-1).

6. R 3 The compound according to any one of claims 1 to 5, wherein is a cyano group.

7. R 4 and R 5 At least one selected from the group consisting of a cyano group, -SCF 3 or -CO-O-R 222 (R 222 has the same meaning as above.

8. R 4 and R 5 8. The compound according to claim 1, wherein at least one selected from the group consisting of: is a cyano group.

9. R 4 and R 5 The compound according to any one of claims 1 to 8, wherein both of are cyano groups.

10. R 3 , R 4 and R 5 is the following [i] or [ii]: [i] R 3 is a cyano group, and R 4 and R 5 one of which is a cyano group, and the other is a halogen atom, a cyano group, or -SCF 3 or a group represented by formula (X-1): [ii] R 3 is a halogen atom, -SCF 3 or a group represented by formula (X-1), 4 and R 5 are both cyano groups; The compound according to any one of claims 1 to 4,

11. The compound according to any one of claims 1 to 10, wherein ring W1 is a ring represented by the following formula: 【Chemistry 5】 [In the above formula, *1 represents a bond to a nitrogen atom, and *2 represents a bond to a carbon atom. R x1 and R x2 each independently represents a hydrogen atom or a substituent, and the substituent is a halogen atom, an alkyl group having 1 to 12 carbon atoms, a halogenated alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, a fluorinated alkoxy group having 1 to 12 carbon atoms, an amino group which may be substituted with an alkyl group having 1 to 6 carbon atoms, an alkylcarbonyloxy group having 2 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, an arylsulfonyl group having 6 to 12 carbon atoms, a cyano group, a nitro group, a hydroxyl group, a thiol group, a carboxy group, -SF 3 , or -SF 5 .]

12. R x1 and R x2 The compound according to claim 11, wherein each of the substituents represented by the following formula (I) is independently an alkyl group having 1 to 12 carbon atoms.

13. The compound according to any one of claims 1 to 12, wherein λmax is 370 nm or more. (λmax represents the maximum absorption wavelength [nm] of the compound represented by formula (II).)

14. The compound according to any one of claims 1 to 13, which satisfies formula (B). ε(λmax) / ε(λmax+30nm)≧5 (B) (In the formula, ε(λmax) represents the gram absorption coefficient at the maximum absorption wavelength [nm] of the compound represented by formula (II), and ε(λmax+30 nm) represents the gram absorption coefficient at the wavelength [nm] of (maximum absorption wavelength [nm]+30 nm) of the compound represented by formula (II).)

15. A composition comprising a compound according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Ultraviolet light-absorbing composition, cosmetic and pharmaceutical preparation each using the same, and method for blocking ultraviolet light radiation

    JP2010111823A

Cited By

  • compound

    JP2021006516A