Composite film, packaging material, lid material, packaging bag containing contents, and container with lid containing contents

JP7591921B2Active Publication Date: 2024-11-29KYODO PRINTING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020215568
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-11-29
Estimated Expiration
2040-12-24

AI Technical Summary

Benefits of technology

【0010】 本発明の複合フィルムによれば、ヒートシール層を容器本体や他のフィルム等の基材にヒートシールして包装体を形成し、当該包装体を開封したときに、基材にヒートシールされた部分の縁で、複合フィルムのヒートシール層のみが破断し、ヒートシール層が基材の側に残るようにして、開封することができる。これによれば、本発明の複合フィルムの粘着層によって、包装体を再封することが可能になる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591921000004
    Figure 0007591921000004
  • Figure 0007591921000005
    Figure 0007591921000005
  • Figure 0007591921000006
    Figure 0007591921000006
Patent Text Reader

Abstract

To provide a composite film for forming a package capable of repackaging by heat sealing where a repackaged face of a container main body does not become an adhesive layer when opening the package, a lid material formed from the composite film, and a container with a lid containing a content.SOLUTION: A composite film for forming a package capable of repackaging by heat sealing is a laminate of a specific laminate constitution using a specific material so that delamination occurs between an adhesive layer and a heat seal layer not to leave an adhesive layer on a container main body side when opening.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite film, a packaging material, a lid material, a packaging bag containing a content, and a lidded container containing a content. [Background technology]

[0002] Conventionally, various packages having a resealable function have been used as a means for packaging foods, medicines, etc. that cannot be consumed in one go. As such packages, a method of sealing using a multilayer film has been proposed that can impart a resealable function to the package itself without the need for an attachment such as a zipper.

[0003] As an example of a multilayer film that allows resealing, there has been disclosed a resealable film (I) having a multilayer resin layer in which a thermoplastic resin layer (A), a pressure-sensitive adhesive resin layer (B), and a heat-sealable resin layer (C) are laminated in the order of (A) / (B) / (C) (see Patent Document 1).

[0004] A package in which the multilayer film described in Patent Document 1 is heat-sealed to a container body or the like can be opened and resealed without any problems.

[0005] As shown in Patent Documents 2 to 4, it has been proposed to use a layer of an amorphous polyester having a glass transition temperature of 25° C. or lower as the easily peelable layer of an easily peelable laminate using a half cut. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-212846 A [Patent Document 2] JP 2017-144714 A [Patent Document 3] JP 2019-034753 A [Patent Document 4] JP 2019-156481 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above-mentioned background, and aims to provide a novel composite film that can be heat-sealed to form a resealable package, and which, when the package is opened, does not have an adhesive resin layer on the resealable surface of the container body, a packaging material made of the composite film, a lid material formed from the composite film, and a packaging bag containing contents, as well as a lidded container containing contents. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that by using a specific material for the adhesive layer of a composite film having a base layer, an adhesive layer, and a heat seal layer, the heat seal layer can be heat sealed and then resealed when opened, and have completed the present invention. That is, the present invention is as follows.

[0009] Aspect 1 The adhesive layer includes a base layer, an adhesive layer, and a heat seal layer in this order. the base layer and the heat seal layer are bonded to each other by the adhesive layer, and The adhesive layer contains an amorphous polyester. Composite film. Aspect 2 2. The composite film of claim 1, wherein the adhesive layer further comprises a rosin ester. Aspect 3 3. The composite film according to aspect 1 or 2, wherein the content of the amorphous polyester is 75 to 95% by mass based on the total mass of the adhesive layer. Aspect 4 The composite film according to any one of aspects 1 to 3, wherein the adhesive layer has a thickness of 5 μm or less. Aspect 5 The composite film according to any one of aspects 1 to 4, wherein the heat seal layer comprises a polyolefin resin. Aspect 6 A resealable packaging material comprising the composite film according to any one of the first to fifth aspects. Aspect 7 7. The packaging material according to claim 6, wherein when opened, the adhesive layer and the heat seal layer are delaminated to expose the adhesive layer in a resealable state with the heat seal layer. Aspect 8 A packaging material according to aspect 6 or 7, which has no half cut on the heat seal layer side. Aspect 9: A covering material formed from the composite film according to any one of the first to fifth aspects. Aspect 10 A packaging bag containing a content formed using the composite film according to any one of aspects 1 to 5, The contents contained in the packaging bag; The heat seal layers are heat sealed to each other to form a joint. Packaging bag with contents. Aspect 11 A container body having a storage portion and a flange portion; A content contained in the container body; A cover material formed from the composite film according to any one of aspects 1 to 5; Equipped with the heat seal layer is heat sealed to the flange portion to form a resealable joint; Lidded container with contents. Aspect 12 The container body is a paper cup, A lidded container containing a content according to claim 11, wherein the flange portion is coated with a polyethylene resin. Effect of the Invention

[0010] According to the composite film of the present invention, a package is formed by heat-sealing the heat-seal layer to a container body or other substrate such as another film, and when the package is opened, only the heat-seal layer of the composite film breaks at the edge of the portion heat-sealed to the substrate, and the heat-seal layer remains on the substrate side. This makes it possible to reseal the package by the adhesive layer of the composite film of the present invention.

[0011] In particular, the above-mentioned opening can be performed by causing delamination between the adhesive layer and the heat seal layer. In this way, when the package is a container, it is possible to prevent the adhesive layer from remaining on the container body, etc. For example, if the composite film of the present invention is applied as a lid material for a container such as a cup soup that is consumed by putting the container to the mouth, it is possible to prevent the adhesive layer from coming into contact with the lips and to avoid discomfort in the mouth, etc.

[0012] Furthermore, a package formed by heat-sealing the heat seal layer of the composite film of the present invention to a container body or the like can be opened by breaking the heat seal layer at one or both of the outer and inner edges of the heat-sealed joint, so there is no need to make a cut (half cut) for opening on the surface of the heat seal layer side of the composite film.

[0013] Therefore, there is no need to make half cuts along the area intended to be heat-sealed to the container, for example, the area to be heat-sealed to the flange portion of the container body, and no alignment operations are required when heat-sealing, which contributes to the productivity of composite films, packaging materials, lid materials, and packaging bodies and lidded containers. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view of a composite film according to one embodiment of the present invention. [Diagram 2] 1 is a schematic diagram of a packaging bag containing contents according to one embodiment of the present invention. [Diagram 3]1 is a diagram showing a peeling mechanism when a lidded container containing contents according to one embodiment of the present invention is opened. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Composite Film The composite film of the present invention is a composite film in which at least a base layer, an adhesive layer, and a heat seal layer are laminated in this order, and the base layer and the heat seal layer are bonded to each other by the adhesive layer.

[0016] The composite film of the present invention has a base layer, an adhesive layer, and a heat-sealing layer, and the adhesive layer is made of a specific material, so that the heat-sealing layer can be heat-sealed and then resealed when opened.

[0017] Specifically, the heat seal layer is heat sealed to a container body or a substrate such as another film to form a package, and when the package is opened, only the heat seal layer of the composite film breaks at the edge of the portion heat sealed to the substrate, and the heat seal layer remains on the substrate side, so that the package can be opened. In this way, the adhesive layer of the composite film of the present invention makes it possible to reseal the package.

[0018] In particular, the above-mentioned opening can be performed by causing delamination between the adhesive layer and the heat seal layer. This can prevent the adhesive layer from remaining on the container body, etc., when the package is a container, so that, for example, if the composite film of the present invention is applied as a lid material for a container such as a cup soup that is consumed by putting the container to the mouth, it can prevent the adhesive layer from coming into contact with the lips, and can avoid discomfort in the mouthfeel, etc.

[0019] In the present invention, the breaking of the heat seal layer at the edge of the portion heat-sealed to the container body or other substrate such as another film is sometimes referred to as "edge tearing." The composite film of the present invention utilizes such edge tearing at one or both of the outer and inner edges of the heat-sealed joint, making it unnecessary to provide a cut (half cut) for opening on the surface on the heat seal layer side.

[0020] <<Composition of the composite film>> The configuration of the composite film of the present invention will be described below with reference to the drawings. Fig. 1 shows a cross-sectional view of one embodiment of the composite film of the present invention.

[0021] 1 includes a base layer 1, an adhesive layer 2 laminated on the inner side of the base layer 1, and a heat seal layer 3 laminated on the inner side of the adhesive layer 2. That is, in the composite film 10 shown in FIG. 1, the base layer 1 and the heat seal layer 3 are bonded to each other by the adhesive layer 2.

[0022] The composite film of the present invention essentially comprises a base layer, an adhesive layer, and a heat seal layer, which are laminated in this order. The base layer and the heat seal layer are bonded to each other by the adhesive layer.

[0023] In the present invention, in addition to the base layer, the adhesive layer, and the heat seal layer, any layer may be provided. Examples of the optional layer include a layer that can become a surface layer of the composite film, a barrier layer for imparting barrier properties, a reinforcing layer for reinforcing strength, and an adhesive layer for bonding between layers.

[0024] The optional layer may be disposed on the outside of a laminate consisting of a base layer, an adhesive layer, and a heat seal layer, or the base layer may be a laminate and multiple layers may be present as the base layer.

[0025] The thickness and other properties of each layer constituting the composite film of the present invention can be appropriately determined depending on the application and other factors of the composite film.

[0026] <Base material layer> In the composite film of the present invention, the base layer, which is an essential constituent layer, is adjacent to the adhesive layer and is laminated to the heat seal layer via the adhesive layer.

[0027] The composite film of the present invention has a structure in which the base layer is laminated with the heat seal layer via an adhesive layer containing a specific material, and therefore the heat seal layer is heat sealed to a container body or other base material such as another film to form a package, and when the package is opened, only the heat seal layer breaks at the edge of the part heat sealed to the base material, and the heat seal layer remains on the base material side, so that the package can be opened. This makes it possible to reseal the package by the adhesive layer of the composite film of the present invention.

[0028] In the composite film of the present invention, when the base layer is the outermost layer, for example, when a structure such as a package is formed, the base layer becomes the outer layer of the structure. Therefore, the base layer can be a protective layer when a structure is formed by heat-sealing the heat seal layer that is the innermost layer. The base layer can also be a printing layer on which printing is performed to display the contents, etc.

[0029] The substrate layer may be a single layer or a laminate of multiple layers, or the composite film of the present invention may have two or more substrate layers, in which case one substrate layer is adjacent to the adhesive layer, and the substrate layer and the heat seal layer are bonded to each other by the adhesive layer.

[0030] When the substrate layer is a single layer, the material constituting the substrate layer may be a resin, particularly a resin that can be used as a protective layer and can be printed. Commonly used resins may be used, such as polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), and polycyclohexane terephthalate (PCT), polyolefin resins such as polyethylene (PE), polypropylene (PP), and polystyrene (PS), polyamide (PA) resins such as nylon-6 and nylon-66, and polycarbonate (PC) resins.

[0031] The above resins may be used alone or in a blend of two or more kinds, and additives for imparting functionality, etc. may be added as necessary.

[0032] Among these, from the viewpoints of imparting rigidity to the composite film, ease of availability, and ease of handling, the base layer may be a layer constituted of a polyester resin.

[0033] From the viewpoints of printability, imparting rigidity to the composite film, ease of availability, and ease of handling, the base layer may be made of a polyethylene resin.

[0034] In addition, when the base layer is a resin layer, it may be formed using a preformed film, or may be formed by melting and extruding the material for forming the base layer, and cooling and solidifying it. When a film is used as the base layer, it may be a film formed from the above-mentioned resin, etc., and may be unstretched or may be uniaxially or biaxially stretched. Among them, a biaxially stretched film is preferable.

[0035] The resin film serving as the base layer may have an inorganic vapor deposition film formed by vapor deposition of a metal such as aluminum, or an inorganic material such as silicon oxide or aluminum oxide. Alternatively, the resin film may have a barrier coat layer such as a vinylidene chloride coat layer or a polyvinylidene fluoride coat layer. Furthermore, the resin film serving as the base layer may be subjected to a roughening treatment or the like to roughen its surface.

[0036] When the composite film of the present invention has two or more substrate layers, it may have multiple layers made of the same resin as the layer in the case of a single layer described above, or it may have a separate layer made of a material other than resin.

[0037] Examples of layers made of materials other than resin include paper layers. Examples of paper layers include coated paper, art paper, etc. When the paper layer is the outermost layer as a base layer, it may be subjected to printing such as gravure printing or flexographic printing.

[0038] The thickness of the base layer in the composite film of the present invention is not particularly limited. For example, it may be 10 μm or more, 15 μm or more, 20 μm or more, or 50 μm or less, 40 μm or less. If it is 10 μm or more, it is preferable from the viewpoint of imparting rigidity to the package.

[0039] <Adhesive layer> The adhesive layer is an essential component of the composite film of the present invention, and is disposed between the base layer and the heat seal layer to bond them to each other. In the composite film of the present invention, the adhesive layer contains an amorphous polyester as an essential component.

[0040] In addition, as long as the adhesive layer contains the amorphous polyester as an essential component, it may contain other optional components. Examples of the optional components include resins other than the amorphous polyester and additives for imparting functionality.

[0041] In the composite film of the present invention, the adhesive layer contains the amorphous polyester as an essential component, so that a package is formed by heat-sealing the heat-seal layer to a substrate such as a container body or another film, and when the package is opened, only the heat-seal layer breaks at the edge of the portion heat-sealed to the substrate, and the heat-seal layer remains on the substrate side. This makes it possible to reseal the package by the exposed adhesive layer.

[0042] In particular, the above-mentioned opening can be performed by causing delamination between the adhesive layer and the heat seal layer. In this way, when the package is a container, it is possible to prevent the adhesive layer from remaining on the container body, etc. For example, if the composite film of the present invention is applied as a lid material for a container such as a cup soup that is consumed by putting the container to the mouth, it is possible to prevent the adhesive layer from coming into contact with the lips and to avoid discomfort in the mouth, etc.

[0043] The adhesive layer can be produced, for example, by preparing a composition containing an amorphous polyester and a solvent, and applying the composition to the surface of the layer to be laminated. Examples of the solvent capable of dissolving the amorphous polyester include ethyl acetate. Examples of the coating method include gravure printing, offset printing, flexographic printing, silk printing, and coating with a dry laminator.

[0044] The thickness of the adhesive layer is preferably 5 μm or less. When the heat seal layer is heat sealed to form a resealable package, the adhesive layer and the interlayer peeling between the adhesive layer and the heat seal layer can be more easily performed when the package is opened.

[0045] The thickness of the adhesive layer may be 4 μm or less, or 3 μm or less, and is preferably 1 μm or more, 1.5 μm or more, or 2 μm or more from the viewpoint of obtaining sufficient resealability.

[0046] The adhesive layer is 4.0 g / m 2The amount of the adhesive layer is preferably 3.8 g / m2 or less, from the viewpoints of achieving good delamination between the adhesive layer and the heat seal layer and good resealability. 2 Less than or equal to 3.5g / m 2 It may be less than 0.1 g / m 2 More than 0.3g / m 2 or more, or 0.5 g / m 2 It may be more than that.

[0047] (amorphous polyester) The amorphous polyester which is an essential component of the adhesive layer of the composite film of the present invention is an amorphous polyester.

[0048] Here, "amorphous" in the present invention means that there is no clear melting peak when the temperature is raised from -100°C to 300°C at a rate of 20°C / min using a differential scanning calorimeter (DSC).

[0049] The amorphous polyester constituting the adhesive layer of the composite film of the present invention is not particularly limited, and may have, for example, a glass transition temperature of 60° C. or lower. This glass transition temperature may be 60° C. or lower, 55° C. or lower, or 50° C. or lower, or may be −65° C. or higher, −50° C. or higher, −40° C. or higher, −30° C. or higher, or −20° C. or higher.

[0050] When the amorphous polyester has a glass transition temperature within the above range, it is possible to realize a composite film that can cause interlayer delamination between the adhesive layer and the heat seal layer without any practical problems and has good resealability.

[0051] Furthermore, from the viewpoint of preventing peeling accompanied by noise or snagging (pulse peeling) when opening, i.e., from the viewpoint of achieving smooth peeling, the glass transition temperature of the amorphous polyester is preferably 45° C. or lower. Furthermore, from the viewpoint of obtaining good easy peelability at room temperature, the glass transition temperature is preferably −65° C. or higher, −50° C. or higher, −20° C. or higher, −10° C. or higher, 0° C. or higher, 10° C. or higher, 20° C. or higher, or 25° C. or lower.

[0052] In this specification, the glass transition temperature (Tg) refers to the midpoint glass transition temperature (°C) determined by heat flux differential scanning calorimetry (heat flux DSC) at a heating rate of 10°C / min in accordance with JIS K7121 (1987), and the condition adjustment of the test piece is to be carried out in accordance with JIS K7121's "measurement of glass transition temperature after a certain heat treatment."

[0053] The number average molecular weight of the amorphous polyester is not particularly limited, but for example, if it is 100000 or less, 90000 or less, 80000 or less, 70000 or less, 60000 or less, or 50000 or less, the stickiness of the exposed adhesive layer after interlayer peeling between the adhesive layer and the heat seal layer can be suppressed. On the other hand, if it is 5000 or more, 6000 or more, 7000 or more, 8000 or more, 9000 or more, or 10000 or more, a moderate peel strength can be ensured.

[0054] In this specification, the number average molecular weight refers to a number average molecular weight measured by gel permeation chromatography using tetrahydrofuran as a solvent and polystyrene as a standard.

[0055] The amorphous polyester constituting the adhesive layer of the composite film of the present invention may be an amorphous polyester containing 50 mol % of a dicarboxylic acid component and 50 mol % of a diol component, and may be an amorphous polyester containing 30 mol % or more of terephthalic acid, 25 mol % or more of ethylene glycol, and 5 to 45 mol % of other dicarboxylic acid components and / or other diol components.

[0056] Examples of the other dicarboxylic acid components include aromatic dibasic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalic acid, 2,6-naphthalic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, and aliphatic or alicyclic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, and dimer acid.

[0057] Examples of other diol components include propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, cyclohexanedimethanol, neopentyl hydroxypivalic acid ester, 1,9-nonanediol, 2-methyloctanediol, 1,10-dodecanediol, 2-butyl-2-ethyl-1,3-propanediol, and tricyclodecane dimethanol.

[0058] The content of amorphous polyester in the adhesive layer may be 50% by mass or more, 60% by mass or more, 75% by mass or more, 80% by mass or more, 85% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass, and may be 99% by mass or less, 97% by mass or less, 95% by mass or less, 93% by mass or less, or 91% by mass or less, relative to the total mass of the adhesive layer.

[0059] In particular, if the content of amorphous polyester in the adhesive layer is 75 to 95 mass% relative to the total mass of the adhesive layer, when a package formed from the composite film is opened, the adhesive layer can be easily peeled off from the heat seal layer to expose the adhesive layer, making it possible to reseal the package.

[0060] The amorphous polyester constituting the adhesive layer of the composite film of the present invention may be used alone or in combination of two or more kinds of amorphous polyesters. When two or more kinds of amorphous polyesters are used in combination, they may be used as a mixture of amorphous polyesters having different physical properties such as different Tg.

[0061] (rosin ester) The adhesive layer of the composite film of the present invention preferably contains a rosin ester as an optional component. The rosin ester as an optional component is a compound obtained by esterifying rosin.

[0062] By incorporating a sufficient amount of rosin ester in the adhesive layer, the adhesive properties of the adhesive layer can be improved, and by ensuring that the amount of rosin ester is not excessive, the strength of the adhesive layer can be maintained.

[0063] The type of resin acid (various isomers) that is the main component of the rosin to be esterified is not particularly limited, and may be a conjugated resin acid having a conjugated double bond, a non-conjugated resin acid, or a mixture thereof.

[0064] Examples of conjugated resin acids include abietic acid, neoabietic acid, palustric acid, etc. Examples of non-conjugated resin acids include pimaric acid, isopimaric acid, dehydroabietic acid, etc.

[0065] The form of the rosin ester is not particularly limited, and may be, for example, an ester of rosin or polymerized rosin with a polyhydric alcohol, an ester of hydrogenated rosin, or a maleic acid-modified rosin ester obtained by adding maleic acid to an ester.

[0066] The rosin ester may be a commercially available rosin ester, such as the Haritac series manufactured by Harima Chemical Industries, Ltd., the Ester Gum series and the Pencel (registered trademark) series manufactured by Arakawa Chemical Industries, Ltd.

[0067] The rosin ester content in the adhesive layer may be 1 mass% or more, 3 mass% or more, 5 mass% or more, 7 mass% or more, or 9 mass% or more, and may be 50 mass% or less, 40 mass% or less, 25 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, or 5 mass% or less, relative to the total mass of the adhesive layer.

[0068] The rosin ester constituting the adhesive layer of the composite film of the present invention may be used alone or in combination of two or more kinds of rosin esters.

[0069] <Heat seal layer> The heat seal layer is an essential constituent layer of the composite film of the present invention. The heat seal layer is a layer used for heat sealing when forming a package or the like using the composite film of the present invention. For this reason, the heat seal layer is disposed so as to be the innermost layer of the composite film.

[0070] The material constituting the heat seal layer is not particularly limited as long as it is heat-adhesive and can impart sufficient seal strength to the molded structure. Known materials can be used, such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), polypropylene (EAA), ethylene-methacrylic acid copolymer (EMAA), ionomer resin, ethylene-vinyl acetate copolymer (EVA), etc.

[0071] Among them, the heat seal layer of the composite film of the present invention preferably contains a polyolefin resin, which is capable of thermal adhesion and imparts sufficient seal strength to the formed structure, and when the heat seal layer is heat sealed to form a package and the package is opened, interlayer peeling occurs between the above-mentioned adhesive layer and the heat seal layer to expose the adhesive layer, thereby exhibiting good resealability.

[0072] Furthermore, the heat seal layer also serves as a layer that forms a space for filling the contents when a structure such as a packaging bag is formed. Therefore, when it is desired to impart resistance to contents to a structure such as a packaging bag, it is preferable to form the heat seal layer using, for example, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), or the like.

[0073] The heat seal layer may be formed using a preformed film, or may be formed by melting and extruding a material for forming the heat seal layer onto the surface of the target laminate, and then cooling and solidifying it.

[0074] The material constituting the heat seal layer may be one type or a blend of two or more types. In addition, the heat seal layer may contain additives for imparting functionality, etc., as necessary.

[0075] Furthermore, the heat seal layer may be a single layer or a multi-layered layer.

[0076] The heat seal layer constituting the composite film of the present invention has a density of 0.920 to 0.958 g / cm 3 According to this constitution, sufficient film-forming property and heat sealability are provided, and edge cutting can be made easier.

[0077] In the present invention, the density may be a value measured in accordance with JIS K7112-1999.

[0078] The density of the heat seal layer is 0.923 g / cm 3 More than 0.925g / cm 3 More than 0.927g / cm 3 More than 0.930g / cm 3 More than 0.933g / cm 3 or more than 0.935g / cm 3 or more, and 3 Below, 0.950g / cm 3 or less than 0.948g / cm3 It may be the following:

[0079] In the composite film of the present invention, the heat seal layer may contain high density polyethylene and low density polyethylene. If the heat seal layer is a mixed resin layer containing high density polyethylene and low density polyethylene, the film formability of the heat seal layer can be improved.

[0080] Whether the heat seal layer is a layer made of a mixed resin containing high density polyethylene and low density polyethylene can be confirmed, for example, by using a differential scanning calorimeter (DSC) to compare a curve measured for the heat seal layer with a curve measured for each polyethylene constituting the mixed resin layer.

[0081] In addition, when the polyethylene resin layer contained in the heat seal layer is a mixed resin layer containing high density polyethylene and low density polyethylene, the above density may be a weighted average in which the density of each component is weighted by the content of each component.

[0082] The thickness of the heat seal layer is not particularly limited and may be, for example, 1 μm or more, 2 μm or more, or 3 μm or more. From the viewpoint of easier edge cutting, the thickness is preferably less than 10 μm, 7 μm or less, 6 μm or less, or 5 μm or less.

[0083] (High density polyethylene) In the present specification, high density polyethylene refers to polyethylene having a density of 0.942 g / cm3, which contains 80 mol% or more, 90 mol% or more, 95 mol% or more, or 98 mol% or more of repeating units of methylene groups, including the branching difference if the branched chain is present, or in which substantially all of the repeating units are methylene groups. 3 This refers to the above polyethylene.

[0084] In particular, 0.942 g / cm 3 More than 0.945g / cm 3 More than 0.948g / cm 3 More than 0.950g / cm 3More than 0.952g / cm 3 or more than 0.955g / cm 3 The polyolefin resin has a density of or above 100%, is substantially free of a long-chain branched structure, and is obtained by radical polymerization of ethylene by a low-pressure method.

[0085] The density of high density polyethylene is 0.970 g / cm 3 Below, 0.967g / cm 3 Below, 0.965g / cm 3 Below, 0.962g / cm 3 or less than 0.960g / cm 3 It may be the following:

[0086] The thermal properties of the preferred high-density polyethylene are not particularly limited, but for example, when measured under conditions of a temperature of 190° C. and a load of 21.18 N in accordance with JIS K6922-1 and -2, and JIS K7210-1, the melt mass flow rate is preferably 0.1 g / 10 min or more, 0.5 g / 10 min or more, 1.0 g or more, 3.0 g / 10 min or more, or 5.0 g / 10 min or more, and 100 g / 10 min or less, 50 g / 10 min or less, 30 g / 10 min or less, or 20 g / 10 min or less.

[0087] When the heat seal layer is a mixed resin layer containing high density polyethylene and low density polyethylene, the content of high density polyethylene in the heat seal layer is preferably 50 to 90 mass % based on the total mass of the heat seal layer.

[0088] Furthermore, the content of high-density polyethylene may be 55 mass% or more, 60 mass% or more, or 65 mass% or more, and may be 85 mass% or less, 80 mass% or less, or 75 mass% or less, based on the total mass of the heat seal layer.

[0089] (Low Density Polyethylene) In this specification, low density polyethylene (LDPE) refers to polyethylene having a density of 0.930 g / cm3 or less, which contains 80 mol% or more, 90 mol% or more, 95 mol% or more, or 98 mol% or more of repeating units of methylene groups, including branched chains, or in which substantially all repeating units are methylene groups. 3 This refers to polyethylene less than 100 mm.

[0090] The density of low density polyethylene is 0.925 g / cm 3 or less than 0.923 g / cm 3 or less, 0.870 g / cm 3 More than 0.875g / cm 3 More than 0.880g / cm 3 More than 0.900g / cm 3 More than 0.910g / cm 3 or more than 0.915g / cm 3 It may be more than that.

[0091] The low-density polyethylene may be a so-called linear low-density polyethylene (LLDPE) or may have a long-chain or short-chain branched structure. The short-chain branched structure may be a branched structure derived from an α-olefin having 4 to 18, 4 to 10, or 4 to 8 carbon atoms, such as 1-butene, 1-hexene, 4-methylpentene-1, or 1-octene.

[0092] The thermal properties of the preferred low-density polyethylene are not particularly limited, but for example, when measured under conditions of a temperature of 190°C and a load of 21.18 N in accordance with JIS K6922-1 and -2, and JIS K7210-1, the melt mass flow rate is preferably 0.1 g / 10 min or more, 0.5 g / 10 min or more, 1.0 g or more, 3.0 g / 10 min or more, or 5.0 g / 10 min or more, and 100 g / 10 min or less, 50 g / 10 min or less, 30 g / 10 min or less, or 20 g / 10 min or less.

[0093] The content of low-density polyethylene in the heat seal layer is not particularly limited, and may be, for example, 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more, and 50% by mass or less, 45% by mass or less, 40% by mass or less, or 35% by mass or less, relative to the total mass of the heat seal layer.

[0094] <Other layers> The composite film of the present invention includes a base layer, an adhesive layer, and a heat seal layer in this order, and may include layers other than these, so long as the base layer and the heat seal layer are bonded to each other by the adhesive layer.

[0095] The other layers are not particularly limited, and examples thereof include a layer that can be a surface layer of the composite film, a barrier layer for imparting barrier properties, a reinforcing layer for reinforcing strength, and an adhesive layer for bonding between layers.

[0096] The optional layer may be disposed outside the laminate consisting of the substrate layer, the adhesive layer, and the heat seal layer, or the substrate layer may be a laminate in which multiple layers are present as the substrate layer, or may have a second substrate layer that is not adjacent to the adhesive layer.

[0097] (Barrier layer) In the composite film of the present invention, the barrier layer, which is an optional constituent layer, is a layer for imparting barrier properties to the composite film.

[0098] Examples of the barrier layer include layers made of ethylene-vinyl alcohol copolymer (EVOH), nylon (NY), polyvinylidene chloride (PVDC), or polyacrylonitrile (PAN), which exhibit a function of blocking gases such as oxygen and water vapor.

[0099] The above resins may be used alone or in a blend of two or more kinds, and additives for imparting functionality, etc. may be added as necessary.

[0100] Alternatively, as described above, an inorganic vapor deposition layer or an organic coating layer may be formed on the base layer to impart barrier properties.

[0101] A metal foil may be present as a barrier layer. Examples of the metal foil that can serve as a barrier layer include metal foils such as aluminum foil, copper foil, and titanium foil, and alloy foils such as aluminum alloy foil and stainless steel foil.

[0102] When an inorganic vapor deposition film or an organic coating layer is present as the barrier layer, the thickness of the barrier layer is preferably 100 nm or more, 200 nm or more, 300 nm or more, 500 nm or more, 700 nm or more, or 1 μm or more, from the viewpoint of ensuring strength and barrier properties, and is preferably 5 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less, from the viewpoint of improving handleability when the composite film is used as a packaging material, etc.

[0103] When a metal foil is present as the barrier layer, the thickness of the barrier layer is preferably 3 μm or more, 5 μm or more, 7 μm or more, 10 μm or more, or 15 μm or more from the viewpoint of ensuring strength and barrier properties, and is preferably 100 μm or less, 80 μm or less, 60 μm or less, 55 μm or less, 50 μm or less, 45 μm or less, 40 μm or less, or 35 μm or less from the viewpoint of improving handleability when the composite film is used as a packaging material or the like.

[0104] (Reinforcement layer) In the composite film of the present invention, the reinforcing layer for reinforcing the strength may be any layer. Examples of the material for the reinforcing layer include paper, synthetic paper, and nonwoven fabric.

[0105] (adhesive layer) In the composite film of the present invention, the adhesive layer for bonding between layers may be any layer. Examples of the adhesive layer include a layer made of ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA), and an ionomer.

[0106] The adhesive layer may be a layer made of an adhesive used when dry laminating or hot melt laminating the layers constituting the laminate that becomes the composite film of the present invention, for example, a dry lamination adhesive, a hot melt adhesive, a water-soluble adhesive, an emulsion adhesive, a non-solvent lamination adhesive, a thermoplastic resin for extrusion lamination, etc.

[0107] <<Method for manufacturing composite film>> The method for producing the composite film of the present invention is not particularly limited, and any method capable of forming a laminated composite film may be used. Known methods may be used, such as dry lamination, hot melt lamination, extrusion lamination, and sandwich lamination.

[0108] <<Applications of composite film>> The uses of the composite film of the present invention are not particularly limited, but include, for example, the following uses.

[0109] <Packaging material> The composite film of the present invention can be used as a packaging material. The packaging material formed from the composite film can be sealed to itself or to a substrate such as another film using a heat seal layer to form a package such as a packaging bag or a container with a lid.

[0110] The packaging material formed from the composite film of the present invention can be heat-sealed to a container body or other substrate such as another film to form a package, and then when the package is opened, the adhesive layer of the packaging material and the heat-seal layer are delaminated to expose the adhesive layer, thereby making it possible to reseal the package by the adhesive layer of the packaging material.

[0111] In addition, since the heat seal layer is broken at one or both of the outer and inner edges of the joint that is heat sealed to the base material, etc., to open the package, there is no need to make a cut (half cut) on the surface of the heat seal layer side of the packaging material to be used for opening the package.

[0112] <Packaging bag with contents> The composite film of the present invention may be used to form a packaging bag containing a content. For example, the heat seal layers of the composite film may be heat sealed to each other to form a three-side sealed bag, a four-side sealed bag, a gusseted packaging bag, a pillow packaging bag, or the like, which is filled with a content.

[0113] Fig. 2 shows a schematic diagram of a packaging bag containing contents according to one embodiment of the present invention. Fig. 2 shows a packaging bag containing contents 20 formed using the composite film of the present invention as a packaging material. Fig. 2(a) is a front view of the formed packaging bag containing contents 20, and Fig. 2(b) is a back view.

[0114] The content-containing packaging bag 20 shown in Fig. 2 is formed from a packaging material 30 made of a composite film. As shown in Fig. 2(a) and Fig. 2(b), at the upper and lower ends of the packaging material 30, the heat seal layers are heat sealed to each other to form joints 31 of 10 mm each.

[0115] In addition, as shown in FIG. 2(b), a joint 31 is formed in the vertical direction of the packaging bag 20 by heat-sealing the ends of the packaging material 30 so as to connect the joint 31 at the upper end and the joint 31 at the lower end.

[0116] When opening, the heat seal layer is broken at one or both of the outer and inner edges of the heat-sealed joint 31, exposing the adhesive layer. This makes it possible to reseal the packaging bag by the exposed adhesive layer. In addition, since the heat seal layer is broken to open the bag, there is no need to make a cut (half cut) for opening on the surface of the packaging material on the side of the heat seal layer.

[0117] The packaging bag containing the contents shown in FIG. 2 is very useful as a package filled with snack foods or the like, for example.

[0118] <Lid material> The composite film of the present invention may be used to form a lid. The lid formed from the composite film of the present invention can be, for example, a lid for sealing the upper end opening of a container body. Since the lid formed from the composite film of the present invention is a resealable lid, a resealable lidded packaging container can be formed.

[0119] The lid material formed from the composite film of the present invention is, for example, heat-sealed to the upper opening of the container body to form a lidded packaging container, and when the packaging container is opened, the adhesive layer is exposed in a resealable state with the heat seal layer due to edge cuts and interlayer peeling between the adhesive layer and the heat seal layer constituting the lid material, and when the packaging container is resealed, it is resealed between the adhesive layer and the heat seal layer.

[0120] <Container with lid containing contents> A lid material formed using the composite film of the present invention may be used to form a lidded container containing a content.

[0121] Specifically, a lidded container containing contents can be formed, which comprises a container body having a storage section and a flange section, contents contained in the container body, and a lid material formed from the composite film of the present invention, wherein the heat seal layer of the lid material is heat sealed to the flange section of the container body to form a resealable joint.

[0122] In a lidded container containing a content, which is formed using a lid material formed from the composite film of the present invention, the joint where the lid material is heat sealed is resealable.

[0123] Specifically, when a content-containing lidded container formed using a lid material formed from the composite film of the present invention is opened, edge cuts and delamination occurs between the adhesive layer and the heat seal layer. After opening, only the delaminated heat seal layer is exposed at the joint formed by heat sealing on the container body side, and the adhesive layer remains on the lid material side.

[0124] As a result, when a lid material formed from the composite film of the present invention is applied to a food container or the like, the adhesive layer will not come into contact with the human body, and discomfort in the mouth, etc. can be avoided.

[0125] When resealing, the container can be resealed between the adhesive layer remaining on the lid side and the heat seal layer exposed on the container body side.

[0126] [Function of a lidded container with contents] The function of a lidded container containing a content and formed using the composite film of the present invention will be described below with reference to the drawings.

[0127] FIG. 3 is a diagram showing a peeling mechanism when a lidded container containing a content according to one embodiment of the present invention is opened.

[0128] A lidded container containing contents formed using the composite film of the present invention can be produced by heat-sealing the innermost layer, the heat seal layer, of the composite film of the present invention to the flange portion of a container body having a flange.

[0129] The lidded container 300 containing contents according to one embodiment of the present invention shown in Figure 3 is produced by heat-sealing a lid material 100 formed from the composite film of the present invention to a flange portion 202 of a container body 200 having a flange portion 202 in which contents 250 are stored, thereby forming a joint portion 202a.

[0130] The covering material 100 formed from the composite film of the present invention shown in Fig. 3 includes a base material layer 101, an adhesive layer 102 laminated on the inner side of the base material layer 101, and a heat seal layer 103 laminated on the inner side of the adhesive layer 102. That is, in the covering material 100 shown in Fig. 3, the base material layer 101 and the heat seal layer 103 are bonded to each other by the adhesive layer 102.

[0131] When opening a lidded container 300 containing contents formed using the lid material 100 of one embodiment of the present invention having the above-mentioned features, as shown in Figure 3(a), by pinching the tab 110 protruding from the flange portion 202 and pulling up the lid material 100, only the heat seal layer 103 breaks (the outer edge is cut) at a position corresponding to the outer periphery of the joint 202a, exposing the first break portion 120a corresponding to this position.

[0132] Furthermore, when the lid material 100 is pulled up, as shown in Fig. 3(b), the lid material 100 undergoes delamination at the interface between the adhesive layer 102 and the heat seal layer 103. Thereafter, when the delamination reaches a position corresponding to the inner circumference of the joint portion 202a, the heat seal layer 103 breaks (the inner edge breaks) as shown in Fig. 3(c), exposing the second break portion 120b corresponding to this position, and forming a reseal portion 106 in the flange portion 202 of the container body 200.

[0133] In other words, the resealing portion 106 is the heat seal layer 103 that is cut away from the lid material 100 by outer edge cuts, interlayer peeling, and inner edge cuts in the area of ​​the joint 202a formed in the flange portion 202, and the heat seal layer 103 is exposed on the surface.

[0134] When resealing the opened lidded container 300 containing the contents, the lid material 100 is pressed against the resealing portion 106, causing the adhesive layer 102 and the heat seal layer 103 to come into close contact with each other and reseal the container.

[0135] [Configuration of container with lid containing contents] The lidded container containing the contents comprises a container body, the contents, and a lid material formed from the composite film of the present invention. (Container body) A container body for forming a lidded container containing a content has a storage portion and a flange portion.

[0136] The material of the container body is not particularly limited as long as the heat seal layer of the lid material formed from the composite film of the present invention can be heat sealed with the material. For example, a paper container with a resin-coated surface or a resin container can be used.

[0137] {Storage section} The storage section is a section in which the contents are stored. The shape of this section is not particularly limited, and may be, for example, a substantially circular truncated cone, a polygonal truncated pyramid, a rectangular parallelepiped, a cube, or the like.

[0138] {Flange part} The flange portion is a peripheral portion of the upper end opening of the storage portion of the container body. The shape of the flange portion is not particularly limited, and may be, for example, a brim-like shape. The outer peripheral shape of the flange portion can be appropriately selected depending on the shape of the lid material.

[0139] Among these, it is preferable that at least the flange portion of the container is coated with a polyethylene-based resin.Furthermore, it is preferable that the container body is a paper cup and the flange portion is coated with a polyethylene-based resin.

[0140] If the container body is a paper cup having a flange portion coated with polyethylene resin, it is possible to obtain a certain seal strength between the heat seal layer of the lid material formed from the composite film of the present invention, while smoothly peeling off the layers at the interface between the adhesive layer and the aluminum layer.

[0141] (Contents) The contents are contained in the storage unit. The contents are not particularly limited, but examples thereof include heated foods such as soup, instant noodles, chilled foods, and frozen foods, and non-heated foods such as snacks and gummy candies. EXAMPLES

[0142] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to these.

[0143] Examples 1 to 10 <Material> The following materials were prepared to form the layers:

[0144] (1) Base material layer NY: Biaxially oriented nylon film (Bonyl (registered trademark) ON25, Kohjin Film & Chemicals Co., Ltd., thickness: 15 μm) OPP: Biaxially oriented polypropylene film (Filmax, thickness 30 μm) (2)Adhesive layer Amorphous Polyester Elitel (registered trademark) XP-1541 [Tg: -12℃] Unitika Ltd.) Elitel (registered trademark) XP-1586 [Tg: -63℃] (Unitika Ltd.) Elitel (registered trademark) XP-1648 [Tg: unknown] (Unitika Ltd.) Rosin Ester Haritac(TM) 8LJA (Harima Chemical Group Co., Ltd., softening point: 89°C) (3) Heat seal layer CPP#20: Non-oriented PP film (Pylen (registered trademark) P1128, Toyobo Co., Ltd., thickness: 20 μm)

[0145] <Preparation of composite film> Using the materials shown in Table 1, a composite film having a laminated structure of (base layer / adhesive layer / heat seal layer) was produced by the method described below.

[0146] A laminate was prepared by bonding a film to be a base layer and a film to be a heat seal layer with an adhesive layer. The solution containing the amorphous polyester to be the adhesive layer was prepared using ethyl acetate as a solvent, and had a dry weight of 3 g / m2. 2 When a mixture of amorphous polyester and rosin ester was used as the material for the adhesive layer, the ratio was as shown in Table 1.

[0147] <Making packaging bags> The resulting composite film was used as a packaging material to produce a packaging bag as shown in Figure 2. A rectangular packaging material measuring 148 mm in length and 200 mm in width was cut out from the composite film. Next, as shown in Figure 2(b), 10 mm of the long end of the packaging material was heat-sealed to form a cylindrical object, and finally, 10 mm of each of the upper and lower ends was heat-sealed to produce a packaging bag measuring 148 mm in length and 95 mm in width.

[0148] Heat sealing was performed using a Fuji Impulse FA-300-10W under conditions of a sealing temperature of 200° C., a sealing time of 1.0 second, and a cooling time of 2.0 seconds.

[0149] "evaluation" (Initial interlaminar strength at room temperature) The composite films obtained in Examples 1 to 5 were cut into rectangles measuring 15 mm wide x 120 mm long, which were used as evaluation samples.

[0150] The evaluation sample was placed at a temperature of 150°C and a pressure of 3 kgf / cm 2 The heat-sealed sample was then heat-sealed to a polyethylene film under conditions of 1.5 seconds, 100 mm width, and 1.5 cm width, and the heat-sealed sample was then heat-sealed to a polyethylene film under conditions of 1.5 seconds, 100 mm width, and 1.5 cm width. Next, the heat-sealed sample was subjected to interlayer peeling by the following method, and the initial interlayer strength of the peeled surface was measured.

[0151] The measurements were performed using a Strograph AGS-X (Shimadzu Corporation) as a measuring device, and the average peel strength was calculated for a peel length of 10 to 30 mm when peeling at 180° under conditions of 200 mm / min and a peel length of 35 mm. The measurements were performed in a room temperature environment. The results are shown in Table 1.

[0152] (Reseal strength at room temperature) After measuring the initial interlaminar strength, the peeled portion was pressed with a finger to re-adhere. Thereafter, the interlaminar strength was measured in the same manner as above. The results are shown in Table 1.

[0153] (Check resealability) The packaging bags produced in Examples 1 to 10 were opened, and the opening was closed by finger pressure. The same area was then opened again, and the resistance when reopening was evaluated according to the following evaluation criteria. The results are shown in Table 1. Good: You feel resistance under your fingers when re-opening the package. ×: No resistance is felt with the fingers when re-opening.

[0154] [Table 1]

[0155] Examples 11 to 16, Comparative Examples 1 to 2 <Material> The following materials were prepared to form the layers:

[0156] (1) Second base layer Paper (NM Art, Nippon Paper Industries Co., Ltd., basis weight: 79.1 g / m 2 )

[0157] (2) Aluminum layer Aluminum foil (1N30, manufactured by UACJ Corporation, thickness: 7 μm)

[0158] (3) Base material layer ·PET film (PETB, Unitika Ltd., thickness: 12μm)

[0159] (4) Adhesive layer Amorphous Polyester Elitel (registered trademark) XP-1541 [Tg: -12℃] (Unitika Ltd.) Elitel (registered trademark) UE-3520 [Tg: -39℃] (Unitika Ltd.) Rosin Ester Haritac(TM) 28JA (Harima Chemical Group Co., Ltd., softening point: 130~140℃) Haritac(TM) 8LJA (Harima Chemical Group Co., Ltd., softening point: 89°C) SBBS (N515, Asahi Kasei Corporation) Polyterpene (Sylvares® TRB115, Kraton)

[0160] (5) Heat seal layer LDPE (Suntec® LD L2340, Asahi Kasei Corporation, density: 0.923 g / cm 3 ) HDPE (Novatec® HD HJ490, Japan Polyethylene Co., Ltd., density: 0.958 g / cm 3 ) MDPE (Petrothene® LW04-1, Tosoh Corporation, density: 0.940 g / cm 3 )

[0161] <Preparation of composite film> Using the materials shown in Table 2, a composite film with a laminated structure of (base layer / / aluminum layer / / polyester resin layer / adhesive layer / heat seal layer) was produced by the method shown below. The parts bonded by dry lamination are indicated with " / / ". The composition of the adhesive layer (mass%) indicates the solid content of each component relative to the entire adhesive layer.

[0162] 1. An aluminum foil serving as the aluminum layer and a polyester film serving as the base layer were laminated by dry lamination to produce a laminate of (aluminum layer / PET film). An organic solvent-based adhesive (LX500 / KW-75, DIC Corporation) was used as the adhesive for dry lamination.

[0163] 2. A paper layer, which was to be the second base layer, was attached to the aluminum layer side by dry lamination to produce a laminate of (paper / aluminum layer / PET film). An organic solvent-based adhesive (LX500 / KW-75, DIC Corporation) was used as the adhesive for dry lamination.

[0164] 3. On the PET film side, which is the base layer, a mixed resin of amorphous polyester and rosin ester, or amorphous polyester, which will become the adhesive layer, is applied at a dry weight of 3 g / m. 2 A laminate of (paper / aluminum layer / PET film / adhesive layer) was produced by coating to a thickness of 3 μm. The mixing ratio of the amorphous polyester and the rosin ester in the adhesive layer is as shown in Table 2. Ethyl acetate was used as the solvent for coating.

[0165] 4. A resin or resin composition that will become the heat seal layer was extrusion laminated onto the adhesive layer to a thickness of 5 μm to obtain a composite film with the structure (paper / aluminum layer / PET film / adhesive layer / heat seal layer). The type of resin used in the heat seal layer and the ratio of the resin in the heat seal layer are as shown in Table 2.

[0166] <Creating the lid> The obtained composite film was cut into a size of φ101 mm with a tab to prepare a lid material.

[0167] <Making a container with a lid> The obtained lid material was heat-sealed to a PE-coated paper cup (flange width: 3 mm, opening inner diameter: 90 mm) using a heated heat seal bar under conditions of a heat seal width of 3 mm, pressure of 65 MPa, and time of 0.7 seconds to produce a lidded container.

[0168] Comparative Example 1 <Preparation of composite film> A container with a lid was prepared using a commercially available composite film in the same manner as in Example 1. The prepared composite film was a laminate having a structure of a base layer (A) / adhesive resin layer (B) / heat seal layer (C), and the materials were as follows. In the base layer (A), the polyethylene layer (a4) shown below was disposed so as to be adjacent to the adhesive resin layer.

[0169] Base layer (A): A laminate consisting of the following (a1) / (a2) / (a3) / (a4) (a1) PET layer (a2) Ethylene-vinyl alcohol copolymer (EVOH) layer (a3) Nylon layer (a4) Polyethylene layer Adhesive resin layer (B): Polystyrene resin Heat seal layer (C): Polyethylene resin

[0170] Comparative Example 2 As shown in Table 2, a mixed resin of styrene-butadiene-butylene-styrene copolymer (SBBS) and polyterpene was used as the material for forming the adhesive layer, and the dry weight was 6 g / m. 2 A composite film was produced in the same manner as in Example 11, except that the composition of the polyethylene resin constituting the heat seal layer was changed, and a lidded container was produced using the obtained composite film.

[0171] [Table 2]

[0172] "evaluation" (Initial interlaminar strength at room temperature) The composite films obtained in Examples 11 to 16 and Comparative Examples 1 and 2 were cut into rectangles measuring 15 mm wide x 120 mm long, which were used as evaluation samples.

[0173] The evaluation sample was placed at a temperature of 150°C and a pressure of 3 kgf / cm 2The heat-sealed sample was then heat-sealed to a polyethylene film under conditions of 1.5 seconds, 100 mm width, and 1.5 cm width, and the heat-sealed sample was then heat-sealed to a polyethylene film under conditions of 1.5 seconds, 100 mm width, and 1.5 cm width. Next, the heat-sealed sample was subjected to interlayer peeling by the following method, and the initial interlayer strength of the peeled surface was measured.

[0174] The measurements were performed using a Strograph AGS-X (Shimadzu Corporation) as a measuring device, and the average peel strength was calculated for a peel length of 10 to 30 mm when peeling at 180° under conditions of 200 mm / min and a peel length of 35 mm. The measurements were performed in a room temperature environment. The results are shown in Table 3. An initial interlaminar strength of 2.0 (N / 15 mm) or more was considered to be acceptable.

[0175] (Interlaminar strength under high temperature conditions) For the measurement of interlayer strength under high temperature conditions, samples that had been subjected to interlayer peeling in the above-mentioned measurement of initial interlayer strength at room temperature were used, and after the measurement of the initial interlayer strength, the samples were re-adhered (resealed) with finger pressure to return them to a composite film state, and interlayer peeling was performed in a 50°C environment using the same equipment and operations as in the above-mentioned measurement of initial interlayer strength at room temperature, and the average peel strength was calculated. The results are shown in Table 2. An interlayer strength in the range of 1.5 to 3.0 (N / 15 mm) was considered to be acceptable.

[0176] (Check for delamination) The lidded containers produced in Examples 11 to 16 and Comparative Examples 1 and 2 were initially opened to check for the location of delamination. The locations of delamination are shown in Table 3.

[0177] It was confirmed that the lidded containers produced in Comparative Examples 1 and 2 had delamination between the base layer and the adhesive layer, whereas the lidded containers produced from the composite films of Examples 11 to 16 had delamination between the adhesive layer and the heat seal layer.

[0178] (Sealing test after supplying hot water) The containers with lids produced in Examples 11 to 16 and Comparative Examples 1 and 2 were opened by about 1 / 3, and then 90°C hot water was poured into them and they were resealed by finger pressure. After resealing, it was evaluated for 5 minutes whether the lids were tightly sealed. The results are shown in Table 3. 〇: Sealed for 5 minutes ×: The lid was opened within 5 minutes

[0179] (Evaluation of adhesive residue on flange) The containers with lids produced in Examples 11 to 16 and Comparative Examples 1 and 2 were opened by about 1 / 3, and then 90°C hot water was poured into them and resealed with finger pressure. After resealing, the containers were sealed for 5 minutes, and when they were opened again, it was evaluated whether any adhesive remained on the flange. In the evaluation, the flange was touched with a finger to confirm the presence or absence of tack. The results are shown in Table 3. 〇: No tack ×: There was a tack

[0180] [Table 3] [Explanation of symbols]

[0181] 1 Base material layer 2 Adhesive layer 3 Heat seal layer 10 Composite Film 20 Packaging bag with contents 30 Packaging materials 31 Joint 100 Lid material 101 Base material layer 102 Adhesive layer 103 Heat seal layer 106 Re-sealing section 110 Tabs 120a first break 120b Second break 200 Container body 202 Flange part 202a Joint 250 Contents 300 Lidded container with contents

Claims

1. The adhesive layer includes a base layer, an adhesive layer, and a heat seal layer in this order. The base layer and the heat seal layer are bonded to each other by the adhesive layer, and The adhesive layer contains an amorphous polyester and a rosin ester. Composite film.

2. The composite film according to claim 1, wherein the content of the amorphous polyester is 75 to 95% by mass based on the total mass of the adhesive layer.

3. The composite film according to claim 1 or 2, wherein the adhesive layer has a thickness of 5 μm or less.

4. The composite film according to any one of claims 1 to 3, wherein the heat seal layer comprises a polyolefin resin.

5. A resealable packaging material comprising the composite film according to any one of claims 1 to 4.

6. The packaging material according to claim 5 , wherein when opened, the adhesive layer and the heat seal layer are delaminated to expose the adhesive layer in a resealable state with the heat seal layer.

7. The packaging material according to claim 5 or 6, which has no half cut on the heat seal layer side.

8. A covering material formed from the composite film according to any one of claims 1 to 4.

9. A packaging bag containing a content formed using the composite film according to any one of claims 1 to 4, The contents contained in the packaging bag; The heat seal layers are heat sealed to each other to form a joint. Packaging bag with contents.

10. A container body having a storage portion and a flange portion; A content contained in the container body; A cover material formed from the composite film according to any one of claims 1 to 4; Equipped with the heat seal layer is heat sealed to the flange portion to form a resealable joint; Lidded container with contents.

11. The container body is a paper cup, The lidded container containing the contents according to claim 10, wherein the flange portion is coated with a polyethylene resin.

Citation Information

Patent Citations

  • Heat-shrinkable, heat-sealable polymer film for packaging

    JP2003520740A

  • Resealable bag

    JP2005212846A

  • Laminate

    JP2006315385A

  • Easily peelable laminate

    JP2017144714A

  • Resealable sealant film