Wet process for manufacturing panels or poles, products produced by said process and use of products produced by said process
A slurry-based method with inorganic and cellulose fibers addresses the mechanical weakness of airlaid boards by enhancing compressive and tensile strength, making them suitable for vacuum insulation panels and other applications with high mechanical demands.
Patent Information
- Application Number
- JP2021504500
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-10
- Filing Date
- 2019-08-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-08-02
AI Technical Summary
Existing mineral fiber boards produced by airlaid methods lack sufficient mechanical properties, particularly compressive and tensile strength, making them unsuitable for applications requiring high mechanical performance, such as vacuum insulation panels, filter materials, and battery separators, due to issues with binder decomposition and increased weight.
A method involving the production of a slurry with inorganic and cellulose fibers, pH 2-6, and a Schopper-Riegler index of 50 or more, forming a web, and drying it to create boards or mats with enhanced mechanical properties without binders, using mineral wool fibers and cellulose fibers like bleached kraft pulp.
The method results in boards or mats with improved compressive and tensile strength, suitable for vacuum insulation panels, filter materials, and battery separators, with reduced overall density and binder-free composition.
Smart Images

Figure 0007592005000009 
Figure 0007592005000001 
Figure 0007592005000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a board or mat by wet processing, to a product produced by this method, and to the use of this product. [Background technology]
[0002] The use of man-made mineral fibres to insulate buildings and industrial facilities has been state of the art for decades.
[0003] The manufacture of mineral fiber boards can be carried out by two methods well known to those skilled in the art. The conventional method, the so-called airlaid method, starts with the fiberization of a molten glass mass by a rotary method such as an internal or external centrifuge, also called the TEL or REX method, respectively, or by the nozzle blasting method. These methods are described, for example, in Ullmann's Encyclopedia of Industrial Chemistry, Vol. A11, Fibers, 5. Synthetic Inorganic.
[0004] These processes are defined by the primary formation of fibers entrained with a flow of air towards a moving foraminous element, optionally together with other compounds, such as binders, added to the fiber-containing gas stream, to form a felt, which is further processed, usually by a process including a drying or curing step, to form a mat or board.
[0005] A feature of these forming methods is the essentially lamellar orientation of the formed mat or board with fibers oriented primarily horizontally. Depending on the intended use of the product, this lamellar orientation can be beneficial for some properties, especially heat resistance, while being less desirable when the main property being targeted is mechanical performance such as compression resistance or tear strength.
[0006] To overcome this shortcoming of the products resulting from the airlaid process, various proposals have been made to increase the mechanical performance, for example by reorienting the fibers in the felt prior to drying or curing.
[0007] One area of application that is sensitive to mechanical properties is the use of mineral fiber boards or mat elements as core material in vacuum insulation panels. The core material must withstand atmospheric pressure during the entire service life of the vacuum insulation panel, since it is embedded in an airtight foil material that is vacuumed. The mechanical performance can be increased by increasing the overall density or by increasing the binder content, but the first option is avoided due to the high weight and material requirements, while the latter option has the disadvantage that the binder may decompose, thereby compromising the vacuum and thus increasing the internal pressure. As a result, the service life of the vacuum insulation panel can be significantly affected.
[0008] Alternatively, products with high demands on mechanical properties may be produced by a wet process, which differs from an airlaid formulation in that the fibers of the airlaid formulation are collected and suspended in a liquid that is further processed.
[0009] WO 00 / 70147 discloses a method for producing a board or mat, which comprises producing a slurry with a solid content comprising inorganic and cellulose fibers, and then producing a web from the slurry on at least one moving perforated element. Water is extracted from the web and the web is dried by passing hot air through the web. The aim of this method is to provide a method that allows the production of mineral fiber boards, in particular using recycled glass fibers, mineral fibers, rock wool or other inorganic fibers as input fibers, which have improved uniformity and compressive strength compared to boards produced by airlaid processes. Other fibers such as aramid, thermoplastic and cellulose fibers may be added to the mineral fibers. Products produced according to WO 00 / 70147 mostly contain a binder, but this method allows the production of binder-free products. Summary of the Invention [Problem to be solved by the invention]
[0010] However, there is still an interest in providing mineral fiber-based products with high mechanical properties, in particular compressive strength and / or tensile strength, for applications requiring such properties, in particular as core materials for vacuum insulation panels, filter materials, in particular filter papers, or battery separators. [Means for solving the problem]
[0011] This object is achieved by a method for producing a board or mat, comprising: - Producing a liquid slurry having a solid content comprising inorganic fibers and cellulosic fibers; - Producing a web from the slurry on at least one perforated element, preferably a moving perforated element; - Extracting water from the web, - Drying the web to make the product wherein said method is characterized in that: The pH of the slurry containing inorganic fibers and cellulose fibers is in the range of 2 to 6; and - The Schopper-Riegler index of cellulose fibers according to ISO 5267 is at least 50.
[0012] The product produced by this method also achieves this objective.In terms of use, this objective is achieved by using said product as a core material for vacuum insulation panels, or as a filter material, in particular as filter paper, or as a battery separator.
[0013] The present invention relates in particular to a method for producing a board or mat, comprising the steps of: - Producing a slurry having a solid content comprising inorganic fibers and cellulosic fibers; - Producing a web from the slurry on at least one perforated element, preferably a moving perforated element; - Extracting water from the web, - Drying the web to make the product Here, the pH of the slurry containing inorganic fibers and cellulose fibers is in the pH range of 2 to 6, and The cellulose fibers have a Schopper-Riegler index according to ISO 5267 of 50 or greater. [Brief description of the drawings]
[0014] (Not stated in the original text) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The web can have any thickness, and can be as thin as paper, and in order to produce a product of the desired thickness, it may be necessary to foresee a process of laminating multiple web layers on top of each other by known methods such as folding, stacking, etc.
[0016] The Schopper-Riegler index, determined according to ISO 5267, is a measure for determining the beating index (freeness). Beating allows, among other things, the defibration of the fibre walls by the liberation of macrofibrils, which gives rise to more inter-fibre connections in the final product. The occurrence of such inter-fibre connections increases the mechanical properties of the final product.
[0017] The inventors have recognised that when the method is carried out on a particular range of cellulose fibres, the compressive and / or tensile strength is substantially increased, this increase being due to the formation of hydrogen bonds between the cellulose fibres.
[0018] The beaten cellulose fibers preferably have a Schopper-Riegler index according to ISO 5267 of 60 or more and / or a Schopper-Riegler index according to ISO 5267 of 100 or more.
[0019] The pH value is preferably in the range of 3 to 5, especially 3 to 4. Excessively acidic conditions have been shown to reduce compressive strength, but the beneficial effect decreases as the pH value approaches neutrality.
[0020] Preferably, the pH value is adjusted by a strong acid with an acid dissociation constant pKa of less than or equal to 3, such as sulfuric acid or hydrochloric acid.
[0021] In a preferred embodiment of the invention, the inorganic fibers are selected from mineral wool fibers, i.e. glass wool fibers, stone wool fibers or slag wool fibers, preferably produced by the rotary or nozzle blasting process, which are available in large quantities at low cost.
[0022] The micronaire of the inorganic fibers is preferably 20 liters / minute or less, more preferably 12 liters / minute or less, and particularly preferably 8 liters / minute or less.
[0023] Thereby, the micronaire is measured according to known techniques described in WO 2003 / 098209. This patent application in fact relates to an apparatus for determining the fineness index of fibers, comprising a device for measuring the fineness index. Said device for measuring the fineness index has, on the one hand, at least one first orifice connected to a measurement cell designed to receive a sample composed of a plurality of fibers, and on the other hand, second orifices located on both sides of said sample, connected to a device for measuring the differential pressure. Said device for measuring the differential pressure is designed to be connected to a fluid flow generating device, characterised in that the device for measuring the fineness index comprises at least one volumetric flowmeter for the fluid passing through said cell. This device provides a correspondence between the "micronaire" value and liters per minute (liters per minute).
[0024] A low fiber index, i.e., a low micronaire value, means a large number of relatively thin and fine fibers. The use of fine fibers is beneficial for providing products with high mechanical compressive strength and improved lambda performance.
[0025] Preferably, the cellulose fibers are pulp fibers, in particular wood pulp from softwoods such as spruce, pine, fir, larch and hemlock, and hardwoods such as eucalyptus, aspen and birch. The pulping process applied to produce the pulp can be a standard pulping process such as mechanical pulp, thermomechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), chemical pulp (kraft, sulfite and organosolv), recycled pulp, etc. It is particularly preferred to use kraft pulp, in particular chemically bleached kraft wood pulp from softwoods such as spruce, pine, fir, larch and hemlock, and hardwoods such as eucalyptus, aspen and birch. The different pulps can be used alone or in various mixtures.
[0026] Particularly preferred is the use of bleached kraft pulp of eucalyptus fibers, as this material is available on the international market in large quantities at low cost.
[0027] The cellulose fibers preferably have an arithmetic mean length of 0.2 mm to 5 mm and an arithmetic mean diameter of 10 μm to 70 μm.
[0028] The morphological parameters length and diameter are measured using the MorFi instrument (Techpap, Grenoble, France) as measuring device, according to a measurement method that defines as fibers elements with a length in the range of 200 μm to 10 mm and a diameter of 5 μm to 75 μm. The fine part consists of elements with a length less than 200 μm and / or a width less than 5 μm.
[0029] The measurement principle involves taking an image of the fiber suspension in a fluid using a CCD camera and processing the image with specific software to determine the morphology of the object. According to this, measurements are made on the suspended fibers, i.e. on the pulped material. The average is calculated from a sample of at least 5000 fibers analyzed.
[0030] Beaten cellulose fibers are characterized by the presence of macrofibrils visible on the outer surface of the fiber wall. The measure of macrofibril content is defined as follows:
[0031]
number
[0032] It is particularly preferred that the macrofibril content is between 0.1% and 1.5% (based on evaluation of at least 300 fibres according to the above definition).
[0033] The fine fiber content is more preferably 5 to 80%. According to this, the fine fiber content is defined by the following formula:
[0034]
number
[0035] Preferably, the proportion of inorganic fibers is 90% or more, and the proportion of cellulose fibers is more than 0% and 10% or less. In a particularly preferred embodiment, the proportion of inorganic fibers is 92-98%, and the proportion of cellulose fibers is 2-8%. In particular, it is preferred that the proportion of inorganic fibers is 94-98%, and the proportion of cellulose fibers is 2-6%. These percentages refer to the weight of solids in the slurry.
[0036] Preferably, the proportion of other compounds contributing to the formation of the solid material of the slurry is less than 3% by weight of the solids content. Such other non-binder compounds may be, for example, opacifiers, fillers, dyes, etc.
[0037] It is further preferred that the slurry does not contain any additional binder. The synergistic interaction between the inorganic and cellulose fibers provides sufficient mechanical properties, which makes it possible to avoid the use of binders to obtain improved mechanical properties. Furthermore, binder-free products are interesting for various specific applications, such as use as non-outgassing / non-degrading core materials for vacuum insulation panels.
[0038] In case of specific requirements for mechanical properties, the slurry may contain a binder, which may in particular be added in a mass relationship of up to 4 parts by weight of binder solid material per 100 parts by weight of the solid content of the slurry not including the binder solid material.
[0039] Special protection is also required for products manufactured according to the above-mentioned manufacturing processes.
[0040] In a preferred embodiment, the raw material density of the product subjected to 1 bar compression is 250 kg / m 3 Less than 200 kg / m 3 Less than 180 kg / m, most preferably 3 The following is the result.
[0041] Preferably, the increase in overall density of the product subjected to a compression of 1 bar is less than 150%, in particular less than 100%, of the overall density of the product subjected to a compression of 250 Pa. As a result, the mechanical compressive strength of the product when subjected to the standard conditions of this particular application makes it suitable for use as a core material in vacuum insulation panels.
[0042] As a result, the product's compressive mechanical strength when exposed to standard conditions for this particular application makes it suitable for use as a core material in vacuum insulation panels.
[0043] Compressibility measurements are carried out on a rigid platen testing machine with a 5 kN measuring cell, for example a Buchel-Van Der Korput press. The speed of the platens during the test is 1.4 cm / min and the selected measurement range is 0-5000 N. The thickness at 250 Pa (ISO 29466:2008) is measured with a separate device. The surface subjected to pressure is 10 x 10 cm 2 This measurement corresponds to the reference thickness used to calculate the compression ratio. Once the thickness at 250 Pa has been measured, a disk of 10 cm radius is placed on the bottom board which rises to compress the mat. A sensor placed above the device measures the force detected on the top plate. During this experiment, the compression is stopped when the force reaches a value corresponding to a pressure of 1 bar (3140 N for a specimen with a diameter of 20 cm) and the thickness is measured immediately. The pressure is maintained for 30 seconds. The bottom board is then lowered and the mat is released for 5 minutes, after which the compression procedure is repeated. Several specimens of 10 cm radius are stacked together to obtain a sufficient thickness (approximately 10 mm) to carry out the compression test.
[0044] Actual experiments show that the thickness after 5 minutes of pressure release remains substantially constant over time. For practical reasons, the thickness data has been converted to bulk density for the tested embodiments.
[0045] In a preferred embodiment the tensile strength index of the product is at least 1.5 Nm / g, preferably at least 2.0 Nm / g, most preferably at least 2.5 Nm / g, whereby in the case of a dynamic production process using a moving perforated belt the tensile strength index is measured in the running direction.
[0046] For static manufacturing processes, the tensile strength index does not show a large effect of orientation: in this case, the tensile strength index is the lower of the tensile strength index in both directions.
[0047] As a result, the product is suitable for use as a filter material, particularly filter paper, or as a battery separator, either of which applications require increased tensile strength properties.
[0048] The Tensile Strength Index (TSI) is determined as follows:
[0049] Tensile specimens (150 mm x 20 mm) are cut using a cutter (to limit edge effects) in the machine direction as well as in the cross direction of the mat or sheet produced. The machine direction represents the direction of manufacture of the device and in most cases represents the preferential orientation of the fibers. The cross direction is located perpendicular to the machine direction.
[0050] These samples are then tested at a constant speed of 10 mm / min using standard tensile measuring equipment, e.g., an INSTRON device connected to Bluehill acquisition software. The normal force cell for tensile strength testing of sensors in the 2 kN range is replaced with a force cell with a maximum capacity of 10 N to match the typical breaking force of the samples tested at a magnitude of approximately 1 N.
[0051] The tensile strength index is calculated by multiplying the tensile strength value (expressed in N) at break of a test specimen for direct comparison with the width (20 mm), i.e. the elongation perpendicular to the tear force of the test specimen, and the basis weight (g / m2) using the following formula: 2 ) and calculate:
[0052]
number
[0053] The invention will be understood in more detail from the description of the preferred embodiments. EXAMPLES
[0054] Preparation of Samples According to the Invention and Comparative Samples Eucalyptus-based bleached kraft pulp marketed by Cenibra, Brazil, is used as the raw material for the cellulosic fiber compound.
[0055] In a first step, the bleached kraft pulp is further pretreated and beaten in a beating machine PFI according to ISO 5264. The beating index, i.e. the Schopper-Riegler index, is determined for both the raw pulp and the beaten pulp. This index is normalized according to ISO 5267. Beating of the bleached kraft pulp aims to obtain a Schopper-Riegler index of 40+ / -5 for the first beaten pulp and 70+ / -5 for the second beaten pulp.
[0056] Table 1 shows the morphological parameters of the raw bleached kraft pulp and the bleached kraft pulp after the beating process.
[0057] [Table 1]
[0058] To evaluate the effect of the Schopper-Riegler index on the tensile strength index, two further beaten pulps 3 and 4 were similarly prepared, having Schopper-Riegler indices of 83 and 85, respectively.
[0059] Two different glass fibers were provided, fiber 1 and fiber 2, having micronaires of 18 liters / min and 4 liters / min, respectively.
[0060] A liquid slurry containing fibre 1 and fibre 2, respectively, and beaten eucalyptus pulp is prepared, adjusted to a pH value of 3 by titration, and processed into a mat using dynamic processing. No additional binder is added. The suspension is sprayed into a water wall formed on a rotating web, reproducing the orientation effect, which is an important feature of papermaking machines or dip-formers. Dynamic forming has the effect of creating an anisotropic network in which the fibres are oriented in the direction of the drum rotation, i.e. in the running direction. This orientation of the fibres results in a difference in mechanical strength between the direction of the sheet and its perpendicular cross direction. The mat thus produced is dried in an oven at a temperature of 130°C until a constant mass is obtained. This method results in a VIP core element with a basis weight of 400 g / m2 after drying. 3 The objective was to produce a sample having a grammage of 300 g / m2 after drying, while the target basis weight of the battery separator paper was 300 g / m2 after drying. 3 It was decided.
[0061] <Product sample with improved compressive strength properties> Therefore, in a first test, examples were produced using the three eucalyptus pulps of Table 1 with different Schopper-Riegler indices, with fiber 1 at 6% by weight of the solids of the beaten eucalyptus pulp.
[0062] Compressibility measurements were performed using a Buchel-Van Der Korput press equipped with a 5 kN measuring cell as described above.
[0063] Table 2 lists the slurry parameters and the overall density of mats produced from the slurries, calculated from the compressibility measurements of the mats. Overall density is given for the reference values at a load of 250 Pa and a load of 1 bar.
[0064] Table 2: Slurry parameters and overall density of mats produced from the slurries.
[0065] [Table 2]
[0066] The table shows that the Schopper-Riegler index has a significant effect on the mechanical properties of the product. When using beaten pulp with an SR index of about 40, the overall density is about 280 kg / m at a load of 1 bar. 3 For untreated unbeaten raw materials, this raw material density increases to about 480 kg / m 3 even up to 280 kg / m2 which can occur for VIP (vacuum insulation panel) elements used at atmospheric pressure. 3 The overall density of is unacceptably very high, which would make the VIP element heavier and potentially increase the risk of damage to the seam welds and / or the gas-tight coating layer. The raw material density achieved with untreated pulp is significantly too high for use as a core material for VIP elements.
[0067] The examples and comparative examples were carried out in the same manner as described, without pH adjustment or without adding beaten eucalyptus pulp 2, which has the highest Schopper-Riegler index of 67. The pH value of the liquid slurry without adjustment is about 9, which is mainly determined by the pH of the glass fibers used, and the eucalyptus fibers added to the slurry have little effect on the pH value.
[0068] As with the first test series, compressibility measurements were performed using a Buchel-Van Der Korput press equipped with a 5 kN measurement cell as described above. Table 3 lists the slurry parameters and the overall density calculated from the compressibility measurements for mats made from the slurries using the first fibers. As with Table 2, both reference values for a load of 250 Pa and values at a load of 1 bar are listed.
[0069] Table 4 lists the same parameters for the second fiber.
[0070] Table 3: Slurry parameters and overall density of mats produced from slurries using first fiber
[0071] [Table 3]
[0072] Table 4: Slurry parameters and overall density of mats produced from slurries with secondary fibers.
[0073] [Table 4]
[0074] In the case of comparative examples 3 and 4, the raw material density could not be measured due to the coarse structure of fiber 1 in the absence of binder. The finer fiber distribution of fiber 2, which gives a certain mechanical resistance to pressure loads, allowed the measurement of the overall density.
[0075] The presented overall density data demonstrate that the overall density under load depends on the Schopper-Riegler index of the pulp used, the pH value of the slurry during mat preparation, and the amount of cellulose fibers / pulp. Of particular interest is the SR index (see Table 2 and results analysis). An increase in pH from pH 3 to pH 9 leads to an increase in overall density under load for the same other parameters (glass fiber type and glass fiber content, beaten pulp content; e.g., Example 1 to Comparative Example 7). This increase in overall density is at least 70 kg / m 3 which is a huge mass excess compared to the examples.
[0076] In addition to other benefits such as material cost, the reduction in the overall density of the core material in the VIP process allows for faster operation, primarily due to a significant reduction in the time for core evacuation, and in principle allows for improved thermal properties of the VIP core elements due to the reduced thermal conductivity of the core material.
[0077] In direct comparison, the impact of changing the pH value of the slurry during mat preparation improves the overall density by less than 1 bar for both Fiber 1 and Fiber 2: -Comparison between Comparative Example 5 and Example 1: 282 kg / m 3 from 221 kg / m 3, or about 21%. -Comparison between Comparative Example 6 and Example 2: 578 kg / m 3 from 296 kg / m 3 , or about 49%. -Comparison between Comparative Example 9 and Example 3: 263 kg / m 3 from 160kg / m 3 , or about 39%. -Comparison between Comparative Example 10 and Example 4: 454 kg / m 3 from 277 kg / m 3 , or about 39%.
[0078] Vacuum insulation panels Core Material For use as such, it should be borne in mind that the data on the overall density of different fibres should not be compared on their own. The different fibre morphologies of fibre 1 and fibre 2 result in differences in the thermal properties of the VIP element and the corresponding core material.
[0079] Besides the primary goal of improved compressive strength, the test samples according to the invention also showed an increase in the tensile strength index, however, due to the optimization of the compressive strength, the increase was less significant compared to the tensile strength optimized products described below.
[0080] Product sample with improved tensile strength index
[0081] 300g / m 3 To achieve a target basis weight of 1000 g, test embodiments were made in both the machine and cross directions using the dynamic method described above with glass fiber 1 (Micronaire 18 liters / min) and beaten eucalyptus pulp 2, 3, and 4. As comparative examples, embodiments were made with glass fiber 1 and glass fiber 2 without the addition of beaten fibers.
[0082] In light of findings regarding the effect of pH, all embodiments, including the comparative examples, were prepared at an improved pH of 3.
[0083] For all tested embodiments, the basis weight, overall density at 250 Pa load, and tensile strength index (TSI) were measured according to the methods described above. The values for the embodiments in the machine direction are summarized in the table below:
[0084] Table 5: Slurry parameters, overall density and tensile strength index of mats produced from the slurries
[0085] [Table 5]
[0086] The tensile strength index as a function of beaten eucalyptus pulp type and consistency is also shown in Figure 1. For clarity, Comparative Example 2 is not shown in Figure 1.
[0087] While the tensile strength index for both comparative examples is very low, Examples 5-15 demonstrate a steady increase in tensile strength index depending on both pulp consistency and Schopper-Riegler index.
[0088] A preferred tensile strength index of at least 1.5 Nm / g is achieved by combining the pulp content and Schopper-Riegler index for each pulp according to the graphical representation in FIG.
[0089] Example 7 (7% pulp 2, SR69), Example 10 (7% pulp 3, SR83) and Example 13 (5% pulp 4, SR85) show measurements that exceed the preferred TSI.
[0090] Besides the main goal of improved tensile strength index, the test samples according to the invention also showed increased compressive strength, however, due to the optimization of tensile strength, especially for the application as VIP core, the increase was not so significant compared to that of the compressive strength optimized products mentioned above. Some of the embodiments of the present invention are described in items 1 to 16 below. <Item 1> A method for manufacturing a board or mat, comprising: - Producing a liquid slurry having a solid content comprising inorganic fibers and cellulosic fibers; - creating a web from said slurry on at least one perforated element, preferably on a moving perforated element; - extracting water from the web; and drying said web to form a product wherein said method is characterized in that: - the pH of the slurry containing the inorganic fibers and the cellulose fibers is in the range of 2 to 6; and The cellulose fibres have a Schopper-Riegler index according to ISO 5267 of at least 50. <Item 2> The method according to Item 1, characterized in that the cellulose fiber has a Schopper-Riegler index according to ISO 5267 of 60 or more and / or a Schopper-Riegler index according to ISO 5267 of 100 or less. <Item 3> The method according to item 1 or 2, wherein the pH value is in the range of 3 to 5, particularly 3 to 4. <Item 4> The method according to any one of Items 1 to 3, wherein the pH value is adjusted with a strong acid having an acid dissociation constant pKa of 3 or less. <Item 5> The method according to any one of Items 1 to 4, characterized in that the inorganic fibers are mineral wool fibers, i.e., glass wool, stone wool or slag wool fibers, and preferably mineral wool fibers produced by a rotary method or a nozzle blasting method. <Item 6> The method according to any one of Items 1 to 5, characterized in that the cellulose fibers are pulp fibers, in particular wood pulp from conifers such as spruce, pine, fir, larch, and hemlock, and hardwoods such as eucalyptus, aspen, and birch, in particular chemically bleached kraft wood pulp from conifers such as spruce, pine, fir, larch, and hemlock, and hardwoods such as eucalyptus, aspen, and birch. <Item 7> The method according to any one of Items 1 to 6, characterized in that the micronaire of the inorganic fibers is 20 liters / minute or less, preferably 12 liters / minute or less, particularly 8 liters / minute or less. <Item 8> The method according to any one of Items 1 to 7, characterized in that the inorganic fibers account for 90% by weight or more, preferably 92 to 98% by weight, and most preferably 94 to 98% by weight of the solid content, and the cellulose fibers account for more than 0% by weight and less than 10% by weight, preferably 2 to 8% by weight, and most preferably 2 to 6% by weight of the solid content. <Item 9> The method according to any one of Items 1 to 8, wherein the slurry does not contain any additional binder. <Item 10> The method according to any one of Items 1 to 8, wherein the slurry contains a binder, preferably in a mass relationship of 4 parts by weight or less of the binder solid material per 100 parts by weight of the solid content of the slurry not including the binder solid material. <Item 11> A product manufactured by the method according to any one of items 1 to 10. Item 12: The product described in Item 11, characterized in that the increase in overall density of the product exposed to a compression of 1 bar is less than 150%, preferably less than 100%, of the overall density of the product exposed to a compression of 250 Pa. <Item 13> The overall density of the product subjected to 1 bar compression is 250 kg / m 3 Less than 200 kg / m 3 Less than 180 kg / m, most preferably 3 13. Product according to item 11 or 12, characterized in that: <Item 14> The product according to item 11, characterized in that the tensile strength index is at least 1.5 Nm / g, preferably at least 2.0 m / g, and most preferably at least 2.5 Nm / g. <Item 15> Use of the product according to any one of items 11 to 13 as a core material for a vacuum insulation panel. <Item 16> Use of the product according to items 11 or 14 as a filter material, in particular as a filter paper, or as a battery separator.
Claims
1. A method for producing a vacuum insulation panel, comprising: - Producing a liquid slurry having a solid content comprising inorganic and cellulose fibers; - creating a web from said slurry on at least one perforated element; - extracting water from the web; - drying the web to form a product; and - using said product as a core material for said vacuum insulation panels; wherein said method is characterized in that: - the pH of the slurry containing the inorganic fibers and the cellulose fibers is in the range of 2 to 6; and the cellulose fibres have a Schopper-Riegler index according to ISO 5267 of 50 or more;
2. 2. The method according to claim 1, characterized in that the cellulose fibers have a Schopper-Riegler index according to ISO 5267 of 60 or more and / or a Schopper-Riegler index according to ISO 5267 of 100 or less.
3. 3. The method according to claim 1, wherein the pH value is in the range from 3 to 5.
4. 4. The method according to claim 1, wherein the pH value is adjusted with a strong acid having an acid dissociation constant pKa of 3 or less.
5. The method according to any one of claims 1 to 4, characterized in that the inorganic fibres are mineral wool fibres, i.e. glass wool, stone wool or slag wool fibres.
6. The method according to any one of claims 1 to 5, characterized in that the cellulose fibres are pulp fibres.
7. The method according to any one of claims 1 to 6, characterized in that the micronaire of the inorganic fibers is 20 liters / min or less.
8. The method according to any one of claims 1 to 7, characterized in that the inorganic fibers are 90% by weight or more of the solid content, and the cellulose fibers are more than 0% by weight and less than 10% by weight of the solid content.
9. The method according to any one of claims 1 to 8, characterized in that the slurry does not contain any binder.
10. The method according to any one of claims 1 to 8, characterized in that the slurry comprises a binder.
11. A vacuum insulation panel obtainable by the method according to any one of claims 1 to 10.
12. 12. The vacuum insulation panel of claim 11, characterized in that the increase in overall density of the product subjected to a compression of 1 bar is less than 150% of the overall density of the product subjected to a compression of 250 Pa.
13. The overall density of the product subjected to 1 bar compression is 250 kg / m 3 13. The vacuum insulation panel according to claim 11 or 12, characterized in that:
14. 12. The vacuum insulation panel of claim 11, characterized in that it has a tensile strength index of at least 1.5 Nm / g.
15. Use of a product obtained by a process comprising the steps of: - Producing a liquid slurry having a solid content comprising inorganic fibers and cellulose fibers, wherein the pH of the slurry comprising said inorganic fibers and said cellulose fibers is in the range of 2 to 6, and the Schopper-Riegler index according to ISO 5267 of said cellulose fibers is 50 or more; - creating a web from said slurry on at least one perforated element; - extracting water from the web; and - Drying the web to form a product.
Citation Information
Patent Citations
Preparation method of glass fiber reinforcement paper
CN105040513A
Water-felted mineral wool building insulation product
GB1107413A
Fire retardant fiberboard for building
JP1987111053A
Method for making inorganic paper and inorganic paper by the method
JP1992011091A
Enhancement of a cellulose-based paper product with glass fibers
US20040231814A1