Separator for lithium secondary battery, manufacturing method thereof, and lithium secondary battery including same
The use of a thermosetting phenolic resin in a porous coating layer on lithium secondary battery separators addresses thermal shrinkage and adhesive issues, enhancing thermal safety and adhesion, thus improving battery performance and safety.
Patent Information
- Application Number
- JP2022550012
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-03
- Filing Date
- 2021-03-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-03-31
AI Technical Summary
Existing lithium secondary battery separators exhibit severe thermal shrinkage and limited thermal safety due to the use of polyolefin-based porous polymer substrates, leading to potential short circuits and safety hazards, and the improvement of heat resistance and adhesive strength with electrodes is necessary.
A separator for lithium secondary batteries featuring a porous polymer base material with a porous coating layer containing inorganic particles and a thermosetting phenolic resin with hydroxyl groups and aromatic rings, which forms a network structure at high temperatures to enhance heat resistance and adhesion.
The thermosetting phenolic resin improves thermal safety by forming a network structure that maintains inorganic particles within the coating, enhancing adhesive strength and reducing the risk of short circuits, thereby improving the safety and performance of lithium secondary batteries.
Smart Images

Figure 0007592096000001 
Figure 0007592096000002 
Figure 0007592096000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator for a lithium secondary battery, a method for producing the same, and a lithium secondary battery including the same.
[0002] This application claims priority to Korean Patent Application No. 10-2020-0041002, filed on April 3, 2020, the entire contents of which are incorporated herein by reference in their entirety in the specification and drawings. [Background technology]
[0003] In recent years, interest in energy storage technology has been increasing. As the fields of application expand to include mobile phones, camcorders, and laptops, as well as the energy of electric vehicles, efforts in the research and development of electrochemical elements have been increasingly realized. Electrochemical elements are the field that has attracted the most attention from this perspective, and in particular, the development of rechargeable secondary batteries has attracted attention. In recent years, in the development of such batteries, research and development related to the design of new electrodes and batteries has been conducted in order to improve the capacity density and specific energy.
[0004] Among the secondary batteries currently in use, lithium secondary batteries, developed in the early 1990s, have been attracting attention due to their advantages of high operating voltage and significantly higher energy density compared to conventional batteries that use aqueous electrolytes, such as Ni-MH, Ni-Cd, and sulfuric acid-lead batteries.
[0005] Electrochemical devices such as lithium secondary batteries are produced by many manufacturers, but their safety characteristics vary from one another. It is very important to evaluate and ensure the safety of such electrochemical devices. The most important thing to consider is that the electrochemical device must not cause injury to users even if it malfunctions, and therefore safety standards strictly regulate fire and smoke generation in the electrochemical device. In terms of the safety characteristics of electrochemical devices, if the electrochemical device overheats and causes thermal runaway or the separator is penetrated, it may lead to an explosion.
[0006] The separator prevents short circuits between the cathode and anode and also provides a path for lithium ions to move. Therefore, the separator is an important factor that affects the safety and output characteristics of the battery. However, the polyolefin-based porous polymer substrate that is commonly used as a separator for electrochemical devices exhibits severe thermal shrinkage at temperatures above 130°C due to its material properties and manufacturing process characteristics, including stretching, which causes a short circuit between the cathode and anode.
[0007] In order to improve heat resistance, an attempt has been made to coat the porous polymer substrate with a porous coating layer containing inorganic particles and a thermoplastic binder polymer. When a porous coating layer is formed in this way, the heat resistance can be improved compared to the use of a porous polymer substrate alone. However, there is a limit to the improvement of thermal safety when exposed to a high temperature environment higher than the melting point of the binder polymer.
[0008] Meanwhile, good adhesion is required between the porous coating layer and the electrode. Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a separator for a lithium secondary battery having improved heat resistance and good adhesion to electrodes.
[0010] Another object of the present invention is to provide a method for producing a separator for a lithium secondary battery having the above-mentioned characteristics.
[0011] A further object of the present invention is to provide a lithium secondary battery including a separator having the above-mentioned characteristics. [Means for solving the problem]
[0012] An aspect of the present invention provides a separator for a lithium secondary battery according to the following embodiment.
[0013] The first embodiment is A porous polymer substrate having a large number of pores; a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a plurality of inorganic particles and a binder polymer; The present invention relates to a separator for a lithium secondary battery, wherein the binder polymer comprises a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring.
[0014] The second embodiment is the same as the first embodiment, The present invention relates to a separator for a lithium secondary battery, wherein the thermosetting phenolic resin includes at least one of a novolac-type phenolic resin represented by the following Chemical Formula 1 and a resole-type phenolic resin represented by the following Chemical Formula 2:
[0015] [ka] (In Chemical Formula 1, n is an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
[0016] [ka] (In Chemical Formula 2, n and m are each an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
[0017] The third embodiment is the first or second embodiment, The present invention relates to a separator for a lithium secondary battery, wherein the thermosetting phenolic resin is thermally cured at 120°C to 200°C.
[0018] The fourth embodiment is any one of the first to third embodiments, The present invention relates to a separator for a lithium secondary battery, wherein the thermosetting phenolic resin is a phenol-formaldehyde resin.
[0019] The fifth embodiment is any one of the first to fourth embodiments, The present invention relates to a separator for a lithium secondary battery, wherein the content of the thermosetting phenolic resin is 0.1% by weight to 20% by weight with respect to 100% by weight of the inorganic particles.
[0020] The sixth embodiment is any one of the first to fifth embodiments, The present invention relates to a separator for a lithium secondary battery, wherein the binder polymer further contains a non-phenolic resin in an amount of 0.1% by weight to 50% by weight based on 100% by weight of the inorganic particles.
[0021] The seventh embodiment is any one of the first to sixth embodiments, The thickness of the porous polymer substrate is 1 μm to 20 μm, The present invention relates to a separator for a lithium secondary battery, wherein the thickness of the porous coating layer is 0.5 to 20 μm based on one surface coating.
[0022] Another aspect of the present invention provides a method for manufacturing a separator according to the following embodiment.
[0023] The eighth embodiment is: (S1) preparing an inorganic particle dispersion liquid by dispersing inorganic particles in a first solvent and dissolving a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring; (S2) coating at least one surface of a porous polymer substrate with a slurry for forming a porous coating layer, the slurry including the inorganic particle dispersion, and drying the slurry to form a porous coating layer.
[0024] The ninth embodiment is the eighth embodiment, The method for producing a separator for a lithium secondary battery further comprises mixing a polymer solution in which a non-phenolic resin is dissolved in a second solvent with the inorganic particle dispersion liquid (S1).
[0025] The tenth embodiment is the ninth embodiment, The present invention relates to a method for producing a separator for a lithium secondary battery, wherein the first solvent and the second solvent each independently contain one compound or a mixture of two or more compounds selected from water, an alcohol having 2 to 5 carbon atoms, acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, and cyclohexane.
[0026] The eleventh embodiment is any one of the eighth to tenth embodiments, The present invention relates to a method for producing a separator for a lithium secondary battery, wherein the inorganic particle dispersion further contains a dispersant.
[0027] The twelfth embodiment is any one of the eighth to eleventh embodiments, The present invention relates to a method for producing a separator for a lithium secondary battery, wherein the thermosetting phenolic resin contains at least one of a novolac-type phenolic resin represented by the following chemical formula 1 and a resol-type phenolic resin represented by the following chemical formula 2.
[0028] [ka] (In Chemical Formula 1, n is an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
[0029] [ka] (In Chemical Formula 2, n and m are each an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
[0030] The thirteenth embodiment is any one of the eighth to twelfth embodiments, The present invention relates to a method for producing a separator for a lithium secondary battery, wherein the thermosetting phenolic resin is thermally cured at 120°C to 200°C.
[0031] The 14th embodiment is any one of the 8th to 13th embodiments, The present invention relates to a method for producing a separator for a lithium secondary battery, wherein the content of the thermosetting phenolic resin is 0.1% by weight to 20% by weight with respect to 100% by weight of the inorganic particles.
[0032] In yet another aspect of the present invention, there is provided a lithium secondary battery including a cathode, an anode, and a separator interposed between the cathode and the anode, the separator being any one of the above-described embodiments. Effect of the Invention
[0033] According to one aspect of the present invention, the binder polymer used in the porous coating layer including a plurality of inorganic particles and a binder polymer includes a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring. The thermosetting phenolic resin having such a structure functions as a dispersant in the slurry for forming the porous coating layer in addition to functioning as a binder polymer for fixing the inorganic particles. As a result, the inorganic particles and the binder polymer in the slurry are well mixed, so that the adhesive strength between the electrode and the porous coating layer is well maintained even if no dispersant is used or the content of the dispersant is reduced. In addition, the content of the dispersant can be reduced to increase the content of the binder polymer, thereby improving the adhesive strength with the electrode.
[0034] Meanwhile, when an electrochemical device including a separator is exposed to high temperatures due to ignition, the thermosetting phenolic resin is thermally cured to form a network structure, thereby enhancing the heat resistance of the separator and providing a separator with improved thermal safety. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Hereinafter, the embodiment of the present invention will be described in detail. Prior to this, the terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary and dictionary meanings, but should be interpreted as being in accordance with the meaning and concept of the technical idea of the present invention, in accordance with the principle that the inventor himself can appropriately define the concept of the term in order to best describe the invention. Therefore, it should be understood that the configurations shown in the embodiments described in this specification are merely the most preferable embodiment of the present invention, and do not represent the entire technical idea of the present invention, and therefore there may be various equivalents and modifications that can be substituted for them at the time of this application.
[0036] Throughout this specification, when a part "comprises" another component, it means that the part may further include the other component, not excluding the other component, unless otherwise specified.
[0037] In lithium secondary batteries, a porous polymer substrate is usually used as the separator. Examples of the porous polymer substrate include a nonwoven fabric substrate made of polymer fibers and a film substrate made of a film obtained by melt-extruding a polymer, but these polymer substrates, especially the film substrates, have a problem of exhibiting thermal shrinkage behavior. Therefore, in order to improve the heat resistance of the separator, a porous coating layer containing a large number of inorganic particles and a binder polymer has been introduced on at least one surface of the porous polymer substrate. When the porous coating layer is formed in this way, the heat resistance of the separator can be improved compared to when the porous polymer substrate is used alone.
[0038] As the binder polymer, a fluorine-based binder polymer having thermoplasticity has been mainly used, but there is a limit to the improvement of thermal safety when exposed to a high temperature environment higher than the melting point of the binder polymer. Also, good adhesion is required between the porous coating layer and the electrode so that the performance of the lithium secondary battery can be fully expressed.
[0039] The present inventors have focused on these problems and have attempted to provide a separator in which the heat resistance of a porous coating layer is improved and the adhesive strength with an electrode is also good when an electrochemical device including the separator is exposed to high temperatures due to ignition or the like.
[0040] In order to solve the above problems, The separator for a lithium secondary battery according to one aspect of the present invention comprises: A porous polymer substrate having a large number of pores; a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a plurality of inorganic particles and a binder polymer; The binder polymer comprises a thermosetting phenolic resin having at least one hydroxy group and an aromatic ring.
[0041] In the separator according to one aspect of the present invention, when the separator is exposed to a high temperature, which is an abnormal environment, the thermosetting phenolic resin present in the porous coating layer is thermally cured to form a network structure. Here, the network structure means a structure formed by a thermal curing reaction of the thermosetting phenolic resin, and the network structure may be a three-dimensional network structure.
[0042] In this way, if the thermosetting phenolic resin in the porous coating layer undergoes a thermosetting reaction in an abnormal high temperature environment to form a network structure, the heat resistance and numerical stability can be improved compared to when a thermoplastic polymer is used. In other words, if a network structure is formed by a thermosetting reaction, the inorganic particles can be firmly maintained within the network structure up to a fairly high temperature.
[0043] [Thermosetting phenolic resin] The thermosetting phenolic resin has at least one hydroxy group and an aromatic ring.
[0044] The thermosetting phenolic resin forms a network structure by undergoing a curing reaction at high temperatures, specifically, for example, at a high temperature of 120°C or higher, more specifically, at a high temperature of 120 to 200°C.
[0045] Meanwhile, the thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring can function as a dispersant in the slurry for forming the porous coating layer, which makes it easier to disperse inorganic particles in the slurry for forming the porous coating layer, and therefore, other dispersants may not be used or may be used in reduced amounts.
[0046] The thermosetting phenolic resin includes at least one of a novolac type phenolic resin represented by the following formula 1 and a resole type phenolic resin represented by the following formula 2, and may also include a modified phenolic resin. Specifically, any thermosetting phenolic resin obtained by condensation reaction of phenol and its derivatives with aldehyde may be used.
[0047] In this case, Chemical Formula 1 can be represented as follows: [ka]
[0048] In Chemical Formula 1, n is an integer of 1 or more, and R can be any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent, in which case the number of carbon atoms may be 1 to 100 or less, 1 to 50 or less, 1 to 30 or less, or 1 to 10 or less.
[0049] In the present invention, the "novolac type phenolic resin" is obtained by reacting a phenolic compound with an aldehyde compound in the presence of an acid catalyst. The novolac type phenolic resin has a phenolic hydroxyl group and is therefore soluble in alkali, but the solubility decreases as the molecular weight increases.
[0050] The novolac resin has almost no methylol groups that act on the curing reaction, so when a curing agent such as hexamethylenetetramine ((CH2)6N4) is added and heated, a cured product with a three-dimensional structure can be formed.
[0051] The novolac phenolic resin may be present in ortho- or para-bonds. In a specific embodiment of the present invention, the novolac phenolic resin may have an ortho-bond / para-bond ratio of less than 0.2, more particularly less than 0.1.
[0052] In a specific embodiment of the present invention, the novolac phenolic resin may include two or more types of novolac phenolic resins having different ortho-bond / para-bond ratios. In this case, when a high-para novolac phenolic resin having more para bonds than ortho bonds is used, curing occurs more quickly at high temperatures, which can further improve the safety of the separator.
[0053] The novolac phenolic resin preferably has a weight average molecular weight (Mw) of 1,000 to 4,000 and a dispersity (Mw / Mn, Mn is number average molecular weight) of 2.0 or less. If the weight average molecular weight of the novolac phenolic resin is in the above range, it is advantageous to ensure heat resistance and fluidity during slurry production, and is also advantageous for forming a thin porous coating layer. On the other hand, if the dispersity is 2.0 or less, it is more advantageous for improving the dispersibility of inorganic particles. The novolac phenolic resin may have a hydroxyl equivalent of 100 to 200 g / eq.
[0054] The above-mentioned formula 2 may have the following structure:
[0055] [ka]
[0056] In Chemical Formula 2, n and m are each an integer of 1 or more, and R can be any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.
[0057] In the present invention, the "resole type phenolic resin" is obtained by reacting a phenolic compound with an aldehyde compound in the presence of a metal catalyst. The resol type phenolic resin has a hydroxyl group and can react with the novolac type phenolic resin to form a crosslinked structure.
[0058] In this case, the metal catalyst may include manganese, magnesium, zinc, etc. Specifically, the metal catalyst may be a metal acetate. For example, the metal catalyst may include manganese acetate, magnesium acetate, zinc acetate, etc. These may be used alone or in combination.
[0059] The resol type phenolic resin preferably has a weight average molecular weight (Mw) of 420 to 1,500 and a dispersity (Mw / Mn, Mn is number average molecular weight) of 2.0 or less. If the weight average molecular weight of the resol type phenolic resin is in the above numerical range, it is advantageous to ensure heat resistance and fluidity during slurry production, and is also advantageous for forming a thin porous coating layer. On the other hand, if the dispersity is 2.0 or less, it is further advantageous for improving the dispersibility of inorganic particles. The resol type phenolic resin may have a hydroxyl equivalent of 100 to 200 g / eq.
[0060] In this case, the weight average molecular weight can be measured using gel permeation chromatography (GPC, PLGPC220, manufactured by Agilent Technologies).
[0061] Specifically, the measurement can be performed under the following analytical conditions. -Column: PL MiniMixed Bx2 -Solvent: THF or DMF -Flow rate: 0.3ml / min -Sample concentration: 2.0mg / ml -Injection volume: 10μl -Column temperature: 40℃ -Detector: Agilent RI detector -Standard: Polystyrene (corrected by a cubic function) -Data processing: ChemStation
[0062] In a specific embodiment of the present invention, the thermosetting phenolic resin is selected from the group consisting of 2,3,4-trihydroxybenzophenone, 2,4,6-trihydroxybenzophenone, 2,2'-tetrahydroxybenzophenone, 4,4'-tetrahydroxybenzophenone, 2,3,4,3'-tetrahydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, 2,3,4,2'-tetrahydroxy4'-methylbenzophenone, 2,3,4,4'-tetrahydroxy3'-methoxybenzophenone, 2,3,4,2'-pentahydroxybenzophenone, 2,3,4,6'-pentahydroxybenzophenone, 2,4,6,3'-hexahydroxybenzophenone, 2,4,6,4'-hexahydroxybenzophenone, 2,4,6,5'-hexahydroxybenzophenone, and 3,4,5,3'-hexahydroxybenzophenone. The thermosetting phenolic resin may be a resin such as phenone, 3,4,5,4'-hexahydroxybenzophenone, 3,4,5,5'-hexahydroxybenzophenone, bis(2,4-dihydroxyphenyl)methane, bis(p-hydroxyphenyl)methane, tri(p-hydroxyphenyl)methane, 1,1,1-tri(p-hydroxyphenyl)ethane, bis(2,3,4-trihydroxyphenyl)methane, 2,2-bis(2,3,4-trihydroxyphenyl)propane, 1,1,3-tris(2,5-dimethyl4-hydroxyphenyl)-3-phenylpropane, 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol, or bis(2,5-dimethyl4-hydroxyphenyl)-2-hydroxyphenylmethane, and these compounds may be used alone or in combination to produce a resin. For example, the thermosetting phenolic resin may be a phenol-formaldehyde resin.
[0063] In a specific embodiment of the present invention, the thermosetting phenolic resin may form a network structure having the following structure when thermally cured in an abnormally high temperature environment.
[0064] For example, the network structure may be represented by the following Chemical Formula 3.
[0065] [ka]
[0066] In a specific embodiment of the present invention, when the thermosetting phenolic resin is thermally cured to form a network structure, the inorganic particles of the porous coating layer may be located within the network structure.
[0067] In this case, the content of the thermosetting phenolic resin may be, for example, 0.1 to 20% by weight, more specifically, 0.5 to 15% by weight, based on 100% by weight of the inorganic particles. Within this content range, the interfacial resistance between the porous polymer substrate and the porous coating layer is not significantly increased, and the effect of improving heat resistance can be sufficiently exhibited.
[0068] [Inorganic particles] In the present invention, the inorganic particles are not particularly limited as long as they are electrochemically stable. In other words, the inorganic particles usable in the present invention are those that are within the operating voltage range (e.g., Li / Li + There are no particular limitations as long as the oxidation and / or reduction reaction does not occur at a voltage of 0 to 5 V relative to the reference voltage. In particular, when inorganic particles having a high dielectric constant are used as the inorganic particles, the degree of dissociation of an electrolyte salt, for example, a lithium salt, in the liquid electrolyte can be increased, thereby improving the ionic conductivity of the electrolyte.
[0069] For the reasons mentioned above, the inorganic particles may be inorganic particles having a dielectric constant of 5 or more, inorganic particles having lithium ion transport ability, or a mixture thereof.
[0070] The inorganic particles having a dielectric constant of 5 or more are Al2O3, SiO2, ZrO2, AlO(OH), TiO2, BaTiO3, Pb(Zr x Ti 1-x )O3(PZT, where 0 <x<1)、Pb 1-x La x Zr 1-y Ti yO3 (PLZT, where 0 < x < 1, 0 < y < 1), (1 - x)Pb(Mg 1 / 3 Nb 2 / 3 )O3 - xPbTiO3 (PMN - PT, where 0 < x < 1), and can be one or more mixtures selected from the group consisting of hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, and SiC.
[0071] The inorganic particles having lithium ion transport ability are lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y - based glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2), SiS2 - based glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) and P2S5 - based glass (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) and can be one or more mixtures selected from the group consisting of these.
[0072] The average particle size of the inorganic particles is not particularly limited, but is preferably in the range of 0.001 to 10 μm in order to form a porous coating layer of uniform thickness and appropriate porosity, and specifically, may be 100 nm or more, 150 nm or more, 200 nm or more, or 1000 nm or less, 900 nm or less, 800 nm or less, or 700 nm or less.
[0073] [Non-phenolic resin] In a specific embodiment of the present invention, the porous coating layer may further include a non-phenolic resin in addition to the thermosetting phenolic resin described above as the binder polymer.
[0074] As the non-phenolic resin, a binder polymer that is commonly used in the art for forming a porous coating layer may be used. In particular, the non-phenolic resin may have a glass transition temperature (T g ) may be used because it can improve mechanical properties such as flexibility and elasticity of the finally formed porous coating layer. Such non-phenolic resins effectively play the role of a binder that connects and stably fixes inorganic particles to each other, thereby contributing to preventing deterioration of the mechanical properties of the separator having the porous coating layer introduced therein.
[0075] In addition, the non-phenolic resin does not necessarily have to have ion-conducting ability, but when a polymer having ion-conducting ability is used, the performance of the electrochemical element can be further improved. Therefore, the non-phenolic resin may have as high a dielectric constant as possible. In fact, since the degree of dissociation of salt in the electrolyte depends on the dielectric constant of the electrolyte solvent, the higher the dielectric constant of the non-phenolic resin, the more the degree of dissociation of salt in the electrolyte can be improved. The dielectric constant of such non-phenolic resins can be in the range of 1.0 to 100 (measurement frequency = 1 kHz), and can be particularly 10 or more.
[0076] In addition to the above-mentioned functions, the non-phenolic resin may have a feature of exhibiting a high degree of swelling in the electrolyte by gelling when impregnated with the liquid electrolyte. Therefore, the solubility index, i.e., Hildebrand solubility parameter, of the non-phenolic resin is 15 to 45 MPa. 1 / 2 , 15~25MPa 1 / 2 Or 30 to 45 MPa 1 / 2 Therefore, it is more preferable to use a hydrophilic polymer having many polar groups than a hydrophobic polymer such as polyolefins. 1 / 2 Less than or 45MPa 1 / 2 If the content is excessive, it may be difficult for the material to swell with a typical liquid electrolyte for batteries.
[0077] Non-limiting examples of such non-phenolic resins include polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polyvinylidene fluoride-trifluoroethylene, polyvinylidene fluoride-chlorotrifluoroethylene, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose.
[0078] The separator according to an embodiment of the present invention may further include other additives such as a dispersant in addition to the inorganic particles and binder polymer described above as components of the porous coating layer.
[0079] The thickness of the porous coating layer is not particularly limited, but may be 0.5 to 20 μm, more particularly 1.5 to 10 μm, based on one side coating. The porosity of the porous coating layer is not particularly limited, but is preferably 35 to 85%.
[0080] [Porous polymer base material] In the separator according to one embodiment of the present invention, the porous polymer substrate may be, specifically, a porous polymer film substrate or a porous polymer nonwoven fabric substrate.
[0081] The porous polymer film substrate may be a porous polymer film made of a polyolefin such as polyethylene or polypropylene, and such a polyolefin porous polymer film substrate exhibits a shutdown function at a temperature of, for example, 80 to 150°C.
[0082] In this case, the polyolefin porous polymer film may be formed from a polyolefin polymer such as polyethylene (such as high density polyethylene, linear low density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination of two or more of these.
[0083] In addition, the porous polymer film substrate may be manufactured by forming various polymers such as polyester in addition to polyolefin into a film shape. In addition, the porous polymer film substrate may be formed in a structure in which two or more film layers are laminated, and each film layer may be formed from the above-mentioned polymers such as polyolefin and polyester alone or a mixture of two or more of them.
[0084] In addition, the porous polymer film substrate and the porous nonwoven fabric substrate may be formed from a polymer such as polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalate, etc., either alone or in combination, in addition to the above-mentioned polyolefin-based polymers.
[0085] The thickness of the porous polymer substrate is not particularly limited, but is preferably 1 to 20 μm, more preferably 5 to 15 μm. The size and porosity of the pores present in the porous polymer substrate are not particularly limited, but are preferably 0.01 to 50 μm and 20 to 75%, respectively.
[0086] A method for producing a separator according to an embodiment of the present invention is as follows, but is not limited thereto.
[0087] Specifically, inorganic particles are dispersed in a first solvent to prepare an inorganic particle dispersion liquid in which a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring is dissolved (S1).
[0088] At this time, the method may further include a step of mixing a polymer solution in which a non-phenolic resin is dissolved in a second solvent with the inorganic particle dispersion liquid of (S1). Also, the inorganic particle dispersion liquid may further include a dispersant.
[0089] In this case, the first solvent and the second solvent may be the same or different.
[0090] In this case, the first and second solvents preferably have a solubility index similar to that of the thermosetting phenolic resin and non-phenolic resin, respectively, which are the binder polymers, and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include one compound or a mixture of two or more compounds selected from water, alcohols having 2 to 5 carbon atoms, acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, and cyclohexane.
[0091] Next, the slurry for forming a porous coating layer containing the inorganic particle dispersion is coated on at least one surface of the porous polymer substrate and dried to form a porous coating layer (S2).
[0092] The method of coating the porous polymer substrate with the slurry for forming the porous coating layer is not particularly limited, but it is preferable to use a slot coating or dip coating method. In the slot coating method, a composition supplied through a slot die is applied to the entire surface of the substrate, and the thickness of the coating layer can be controlled by the flow rate supplied from a metering pump. In addition, in the dip coating method, a substrate is immersed in a tank filled with the composition to coat it, and the thickness of the coating layer can be controlled by the concentration of the composition and the speed at which the substrate is pulled up from the composition tank. In order to control the coating thickness more accurately, the substrate may be post-weighed using a Mayer bar after immersion.
[0093] The porous polymer substrate coated with the porous coating layer forming slurry is dried using a dryer such as an oven to form a porous coating layer on at least one surface of the porous polymer substrate.
[0094] In the porous coating layer, inorganic particles may be dispersed in a matrix of the binder polymer, which may be a thermosetting phenolic resin and / or a non-phenolic resin.
[0095] In addition, the inorganic particles are bound to each other by the binder polymer in a packed and contacting state, whereby an interstitial volume is formed between the inorganic particles, and the interstitial volume between the inorganic particles becomes an empty space to form a pore. That is, the binder polymer attaches the inorganic particles to each other so that they can maintain their bonded state, for example, the binder polymer can connect and fix the inorganic particles. In addition, the pores of the porous coating layer are pores formed when the interstitial volume between the inorganic particles becomes an empty space, and this can be a space limited by inorganic particles that are substantially in contact with each other in a packed structure (closely packed or densely packed) of inorganic particles.
[0096] The inorganic particles, the thermosetting phenolic resin, the non-phenolic resin and the porous polymer substrate have been described above, and therefore further description will be omitted.
[0097] A lithium secondary battery according to an embodiment of the present invention includes a cathode, an anode, and a separator interposed between the cathode and the anode, the separator being the separator according to the embodiment of the present invention described above.
[0098] Examples of the lithium secondary battery include a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, and a lithium ion polymer secondary battery.
[0099] The cathode and anode electrodes to be applied with the separator of the present invention are not particularly limited, and may be prepared by a conventional method known in the art in the form of an electrode active material used in a lithium secondary battery bound to an electrode current collector. Among the electrode active materials, non-limiting examples of the cathode active material include conventional cathode active materials used in the cathode of a conventional lithium secondary battery, and in particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide combining these. Non-limiting examples of the anode active material include conventional anode active materials used in the anode of a conventional lithium secondary battery, and in particular, lithium adsorbent materials such as lithium metal or lithium alloy, carbon, petroleum coke, activated carbon, graphite, or other carbons are preferred. Non-limiting examples of the cathode current collector include foils made of aluminum, nickel, or a combination thereof, and non-limiting examples of the anode current collector include foils made of copper, gold, nickel, or copper alloy, or a combination thereof.
[0100] The electrolyte used in the lithium secondary battery of the present invention is A + B - A salt with the structure: + Li + , Na + , K + or a combination thereof, such as B - PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 -or a combination thereof, dissolved or dissociated in an organic solvent such as, but not limited to, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, or a mixture thereof.
[0101] The electrolyte may be injected at an appropriate stage in the battery manufacturing process depending on the manufacturing process and desired physical properties of the final product, i.e., before battery assembly or at the final stage of battery assembly.
[0102] The present invention will be described in detail below with reference to specific examples. However, the examples according to the present invention can be modified into many other forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those skilled in the art.
[0103] Example 1 First, aluminum hydroxide (Al(OH)3) (particle size: 800 nm) was added as inorganic particles to acetone as the first solvent so that the solid content ratio was 30%. Here, the solid content ratio means the content of the powder after drying the solvent with respect to the total content of the solvent and raw material composition. Isopropyl trioleyl titanate as a dispersant and resol-based phenolic resin (thermosetting temperature: about 150°C, acetone-soluble type, solid content 50%, viscosity 250 mPas at 25°C) manufactured by Kangnam Chemical as a thermosetting phenolic resin were added thereto as shown in Table 1, and then stirred for 2 hours. As a result, the inorganic particles were dispersed in the first solvent, and an inorganic particle dispersion liquid in which the thermosetting phenolic resin was dissolved was produced.
[0104] Next, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) as a non-phenolic resin was added to acetone as the second solvent as shown in Table 1, and dissolved at 50° C. for about 4 hours to prepare a polymer solution.
[0105] The inorganic particle dispersion liquid and the polymer solution prepared as above were mixed so that the weight ratio of the inorganic particles to the binder polymer was 75:25, and then the inorganic particles were crushed and dispersed using a ball mill method for 3 hours to prepare a slurry for forming a porous coating layer having a solid content of 18%.
[0106] Then, the slurry for forming the porous coating layer was applied in a coating manner at 23° C. and 45% relative humidity with a total slurry loading of 9.5 g / m 2 A separator having a porous coating layer was manufactured by coating and drying both sides of a 9 μm thick polyethylene porous film (porosity: 43%, ventilation time: 110 sec / 100 ml, resistance: 0.45 ohms) so as to obtain a separator having a porous coating layer.
[0107] Examples 2 to 7 A separator was manufactured in the same manner as in Example 1, except that the types and contents of the materials contained in the slurry were controlled as shown in Table 1.
[0108] Comparative Example 1 to Comparative Example 4 A separator was manufactured in the same manner as in Example 1, except that the types and contents of the materials contained in the slurry were controlled as shown in Table 1.
[0109] [Table 1]
[0110] [Evaluation method] 1) Thickness measurement The thickness of the separator was measured using a thickness measuring device (Mitutoyo Corporation, VL-50S-B).
[0111] 2) Measurement of the heat curing temperature of thermosetting phenolic resin For the thermosetting phenolic resin, the heat generation peak temperature measured using a differential scanning calorimeter (DSC) was determined as the heat curing temperature.
[0112] 3) Measurement of air permeability The measurements were taken using a Girlie air permeability meter according to JIS P-8117. The diameter was 28.6 mm and the area was 645 mm. 2 The time it took for 100 ml of air to pass through was measured.
[0113] 4) Measurement of adhesion strength (laminar strength) between electrode and separator The separators manufactured in the examples and comparative examples were cut to a size of 25 mm x 100 mm and prepared. The prepared separator and anode were stacked, sandwiched between 100 μm PET films, and bonded using a flat press. At this time, the flat press was performed by heating and pressing at 70 ° C and a pressure of 600 kgf for 1 second. The bonded separator and anode (artificial graphite: carbon black: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) = 96: 1: 2: 2 (weight ratio)) were attached to a slide glass using double-sided tape. The end of the separator adhesive surface (10 mm or less from the end of the adhesive surface) was pulled away, and the separator was attached to a 25 mm x 100 mm PET film and a cross-sectional adhesive tape so that the longitudinal direction was connected. Then, the slide glass was attached to the lower holder of a UTM device (LFPlus manufactured by LLOYD Instruments), and the separator and the attached PET film were attached to the upper holder of the UTM device. A force was applied at a measurement speed of 300 mm / min and 180° to measure the force required to peel the anode from the porous coating layer facing the anode.
[0114] 5) Measurement of heat shrinkage rate The heat shrinkage rate was calculated by (initial length-length after heat shrinkage treatment at 150°C for 30 minutes) / (initial length)×100.
Claims
1. The present invention relates to a fuel cell comprising: a cathode; an anode; and a separator interposed between the cathode and the anode, the separator comprising: A porous polymer substrate having a large number of pores; a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a plurality of inorganic particles and a binder polymer; The binder polymer comprises a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring; The thermosetting phenolic resin includes at least one of a novolac-type phenolic resin represented by the following Chemical Formula 1 and a resol-type phenolic resin represented by the following Chemical Formula 2: The content of the thermosetting phenolic resin is 0.1 to 20% by weight based on 100% by weight of the inorganic particles. [Formula 1] (In Chemical Formula 1, n is an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group having 1 to 100 carbon atoms, which may have a substituent, an alkoxy group, and an alkenyl group.) [chemical 2] (In Chemical Formula 2, n and m are each an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
2. 2. The lithium secondary battery according to claim 1, wherein the thermosetting phenolic resin is thermally cured at a temperature of 120° C. to 200° C.
3. 3. The lithium secondary battery according to claim 1, wherein the thermosetting phenolic resin is a phenol-formaldehyde resin.
4. 4. The lithium secondary battery according to claim 1, wherein the binder polymer further comprises a non-phenolic resin in an amount of 0.1% by weight to 50% by weight based on 100% by weight of the inorganic particles.
5. The thickness of the porous polymer substrate is 1 μm to 20 μm; 5. The lithium secondary battery according to claim 1, wherein the thickness of the porous coating layer is 0.5 to 20 μm based on one side coating.
6. A method for manufacturing a lithium secondary battery including a cathode, an anode, and a separator interposed between the cathode and the anode, comprising: (S1) preparing an inorganic particle dispersion liquid by dispersing inorganic particles in a first solvent and dissolving a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring; (S2) coating at least one surface of a porous polymer substrate with a slurry for forming a porous coating layer, the slurry including the inorganic particle dispersion, and drying the porous coating layer to form a porous coating layer.
7. The method of claim 6, further comprising mixing the inorganic particle dispersion liquid (S1) with a polymer solution in which a non-phenolic resin is dissolved in a second solvent.
8. 8. The method for producing a lithium secondary battery according to claim 7, wherein the first solvent and the second solvent each independently comprise one compound or a mixture of two or more selected from the group consisting of water, an alcohol having 2 to 5 carbon atoms, acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, and cyclohexane.
9. The method for producing a lithium secondary battery according to claim 6 , wherein the inorganic particle dispersion further contains a dispersant.
10. The method for producing a lithium secondary battery according to any one of claims 6 to 9, wherein the thermosetting phenolic resin includes at least one of a novolac-type phenolic resin represented by the following Chemical Formula 1 and a resol-type phenolic resin represented by the following Chemical Formula 2. [C3] (In Chemical Formula 1, n is an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group having 1 to 100 carbon atoms, which may have a substituent, an alkoxy group, and an alkenyl group.) [C4] (In Chemical Formula 2, n and m are each an integer of 1 or more, and R is any one of a hydrogen atom, an alkyl group, an alkoxy group, and an alkenyl group having 1 to 100 carbon atoms which may have a substituent.)
11. The method for producing a lithium secondary battery according to any one of claims 6 to 10, wherein the thermosetting phenolic resin is thermally cured at 120°C to 200°C.
12. The method for manufacturing a lithium secondary battery according to any one of claims 6 to 11, wherein the content of the thermosetting phenolic resin is 0.1 wt% to 20 wt% based on 100 wt% of the inorganic particles.
Citation Information
Patent Citations
Storage battery separator
JP1998031991A
Separator for non-aqueous electrolytic solution secondary battery and non-aqueous electrolytic solution secondary battery using it
JP2005038793A
Separator for lithium secondary battery, method for manufacturing the same, and lithium secondary battery
JP2013235810A
Separator for lithium secondary batteries with adhesive layer
JP2019536242A
Separator for rechargeable battery and rechargeable battery including the same
US20170133654A1