Electrochemical Cell

By using a second electrode with a metal oxide having oxygen non-stoichiometry in electrochemical cells, the issue of uneven reactions due to thermal expansion mismatches is addressed, ensuring stable and uniform reaction distribution and improved cell reliability.

JP7592986B2Active Publication Date: 2024-12-03DENSO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020105181
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-18
Publication Date
2024-12-03
Estimated Expiration
2040-06-18

AI Technical Summary

Technical Problem

Conventional electrochemical cells with different materials for the oxygen electrode and oxygen electrode power supply body experience thermal expansion mismatches leading to poor contact, resulting in uneven reactions and increased contact resistance.

Method used

Incorporating a second electrode with a metal oxide having oxygen non-stoichiometry and its decomposition product, which adjusts to varying oxygen concentrations, ensuring uniform reaction distribution by redistributing local overload reactions.

Benefits of technology

The configuration suppresses reaction unevenness within the cell surface, maintaining stable electrode activity and preventing microstructural deterioration, thus enhancing the reliability of the electrochemical cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592986000001
    Figure 0007592986000001
  • Figure 0007592986000002
    Figure 0007592986000002
  • Figure 0007592986000003
    Figure 0007592986000003
Patent Text Reader

Abstract

To provide an electrochemical cell capable of suppressing reaction unevenness in the cell surface.SOLUTION: An electrochemical cell 1 includes a solid electrolyte layer 2 having oxygen ion conductivity, a first electrode 3 that is arranged on one surface side of the solid electrolyte layer 2, and to which fuel F is supplied, a second electrode 4 arranged on the other surface side of the solid electrolyte layer 2 and paired with the first electrode 3. The second electrode 4 includes a metal oxide 41 having an oxygen indefinite ratio, and a decomposition product 42 of the metal oxide having an oxygen indefinite ratio. The metal oxide 41 having an oxygen indefinite ratio can include an oxygen-deficient metal oxide 411. The metal oxide 41 having an oxygen indefinite ratio can further include an oxygen-rich metal oxide 412.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to electrochemical cells. [Background technology]

[0002] Conventionally, electrochemical cells such as water electrolysis cells and fuel cells using a solid electrolyte layer having oxygen ion conductivity are known. For example, Patent Document 1 discloses a water electrolysis cell in which a part of an oxygen electrode power feeder that supplies a current is embedded inside an oxygen electrode. According to the document, such a configuration makes it possible to maintain the adhesion between the oxygen electrode and the oxygen electrode power feeder for a long period of time, to uniformly supply an electrolysis current to the oxygen electrode, and to suppress an increase in contact resistance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-045152 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the above-mentioned conventional technology, as long as the materials of the oxygen electrode and the oxygen electrode power feeder are different, poor contact due to differences in thermal expansion is unavoidable. In other words, in the conventional technology, contacting and non-contacting areas occur locally between the oxygen electrode and the oxygen electrode power feeder in the oxygen electrode. Therefore, in the conventional technology, a uniform reaction cannot be obtained within the cell surface, and reaction unevenness is likely to occur within the cell surface.

[0005] The present invention has been made in view of the above problems, and aims to provide an electrochemical cell capable of suppressing uneven reaction within the cell surface. [Means for solving the problem]

[0006] One aspect of the present invention is a fuel cell comprising: a solid electrolyte layer (2) having oxygen ion conductivity; a first electrode (3) disposed on one side of the solid electrolyte layer and supplied with fuels (F, F1, F2); and a second electrode (4) disposed on the other side of the solid electrolyte layer and paired with the first electrode; the second electrode includes an oxygen non-stoichiometric metal oxide (41) and a decomposition product (42) of the oxygen non-stoichiometric metal oxide; The metal oxide having oxygen non-stoichiometry is During steady-state cell operation, 10 -1 bar~10 -0.5 It does not decompose under oxygen partial pressure of less than bar and at the temperature of steady-state operation of the cell. Oxygen partial pressure is 10 -6 Bar or less or 10 -0.5 It is a material that decomposes at or above bar. In an electrochemical cell (1). Effect of the Invention

[0007] The electrochemical cell has the above-described configuration, and therefore, the electrochemical cell can suppress uneven reaction within the cell surface.

[0008] In addition, the symbols in parentheses described in the claims and the means for solving the problems indicate the correspondence with the specific means described in the embodiments described below, and do not limit the technical scope of the present invention. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is an explanatory diagram that illustrates a schematic microstructure of the electrochemical cell according to the first embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing how a part of the metal oxide having oxygen non-stoichiometry is converted into a decomposition product of the metal oxide having oxygen non-stoichiometry in a portion of the second electrode where current flows easily locally, and the reaction shifts to another reaction field. (a) shows the state before the decomposition of the metal oxide having oxygen non-stoichiometry, and (b) shows the state after the decomposition of the metal oxide having oxygen non-stoichiometry. [Diagram 3]FIG. 3 is an explanatory diagram for explaining a case where the electrochemical cell according to embodiment 1 is operated as a solid oxide electrolysis cell (SOEC mode). [Figure 4] FIG. 4 is an explanatory diagram for explaining a case where the electrochemical cell according to the first embodiment is operated as a solid oxide fuel cell (SOFC mode). [Diagram 5] FIG. 5 is an explanatory diagram that illustrates a schematic microstructure of the electrochemical cell according to the second embodiment. [Figure 6] FIG. 13 shows the results of XRD analysis of a second electrode of an electrochemical cell prepared in an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The electrochemical cell of the present embodiment includes a solid electrolyte layer having oxygen ion conductivity, a first electrode disposed on one side of the solid electrolyte layer and to which a fuel is supplied, and a second electrode disposed on the other side of the solid electrolyte layer and paired with the first electrode, The second electrode includes a metal oxide having oxygen non-stoichiometry and a decomposition product of the metal oxide having oxygen non-stoichiometry.

[0011] In electrochemical cells using a solid electrolyte layer having oxygen ion conductivity, electrochemical reactions occurring at a three-phase interface in the first electrode to which fuel is supplied are often used, and if no measures are taken, reaction unevenness is likely to occur within the cell surface. In the above electrochemical cell, when a portion where electrolysis current or generation current is likely to flow locally occurs due to unevenness in the microstructure of the first electrode, a high oxygen concentration atmosphere or a low oxygen concentration atmosphere is locally generated in the second electrode paired with the first electrode due to a local overload electrolysis reaction or overload generation reaction (hereinafter, collectively referred to as an overload reaction). In the portion of the second electrode where such a high oxygen concentration atmosphere or low oxygen concentration atmosphere occurs, a metal compound having oxygen non-stoichiometry decomposes, generating decomposition products with reduced activity or inactive decomposition products. Therefore, the reaction moves to another reaction field, and the local overload reaction is suppressed. Therefore, according to the above electrochemical cell, reaction unevenness within the cell surface can be suppressed. Furthermore, by suppressing reaction unevenness within the cell surface, deterioration due to microstructural destruction in the first electrode is also suppressed, and a highly reliable electrochemical cell can be obtained.

[0012] Hereinafter, the electrochemical cell of the present embodiment will be described in detail with reference to the drawings. Note that the electrochemical cell of the present embodiment is not limited to the following examples.

[0013] (Embodiment 1) The electrochemical cell of the first embodiment will be described with reference to Figs. 1 to 4. As illustrated in Fig. 1, the electrochemical cell 1 of the present embodiment includes a solid electrolyte layer 2, a first electrode 3, and a second electrode 4. The first electrode 3 is disposed on one side of the solid electrolyte layer 2. The second electrode 4 is disposed on the other side of the solid electrolyte layer 2. Specifically, Fig. 1 shows an example in which the first electrode 3, the solid electrolyte layer 2, and the second electrode 4 are stacked in this order and joined to each other.

[0014] The electrochemical cell 1 may further include an intermediate layer (not shown) between the solid electrolyte layer 2 and the second electrode 4. The intermediate layer is a layer mainly for suppressing a reaction between the material of the solid electrolyte layer 2 and the material of the second electrode 4. In this case, the electrochemical cell 1 may specifically have a configuration in which the first electrode 3, the solid electrolyte layer 2, the intermediate layer, and the second electrode 4 are laminated in this order and joined together. The electrochemical cell 1 may have a flat cell structure. The electrochemical cell 1 may be configured so that the first electrode 3 also functions as a support, or the solid electrolyte layer 2 also functions as a support, or may be configured so that the cell is supported by another support (not shown) such as a metal member.

[0015] The solid electrolyte layer 2 has oxygen ion conductivity. Specifically, the solid electrolyte layer 2 can be formed in a layer shape from a solid electrolyte having oxygen ion conductivity. The solid electrolyte layer 2 is usually formed to be dense in order to ensure gas tightness. As the solid electrolyte constituting the solid electrolyte layer 2, for example, zirconium oxide-based oxides such as yttria-stabilized zirconia (YSZ) and scandia-stabilized zirconia (ScSZ) can be suitably used from the viewpoints of excellent strength and thermal stability. As the solid electrolyte constituting the solid electrolyte layer 2, yttria-stabilized zirconia and the like are suitable from the viewpoints of oxygen ion conductivity, mechanical stability, compatibility with other materials, and chemical stability from oxidizing atmosphere to reducing atmosphere.

[0016] When the solid electrolyte layer 2 does not function as a support, the thickness of the solid electrolyte layer 2 can be preferably 3 to 20 μm, more preferably 3.5 to 15 μm, and even more preferably 4 to 10 μm, from the viewpoints of electrical resistance, etc. When the solid electrolyte layer 2 functions as a support, the thickness of the solid electrolyte layer 2 can be preferably 30 to 300 μm, more preferably 50 to 200 μm, and even more preferably 100 to 150 μm, from the viewpoints of strength, electrical resistance, etc.

[0017] The first electrode 3 is a portion to which the fuel is supplied. The first electrode 3 can be formed to be porous. The first electrode 3 can be formed in a layered form, and may be composed of a single layer or multiple layers. FIG. 1 shows an example in which the first electrode 3 is composed of a single layer. When the first electrode 3 is composed of multiple layers, the first electrode 3 can be specifically configured to include, for example, an active layer (not shown) disposed on the solid electrolyte layer 2 side and a diffusion layer (not shown) disposed on the opposite side to the solid electrolyte layer 2 side. The active layer is a layer for enhancing the electrochemical reaction in the first electrode 3. The diffusion layer is a layer capable of diffusing the supplied fuel F in the in-plane direction of the first electrode 3.

[0018] Specifically, the first electrode 3 can be configured to include an electron conductive material 31 having electron conductivity and an oxygen ion conductive material 32 having oxygen ion conductivity, as exemplified in FIG. 1. Examples of the electron conductive material 31 include metal materials having catalytic activity, such as Ni and Ni alloys. These can be used alone or in combination of two or more. Examples of the oxygen ion conductive material used in the first electrode 3 include zirconium oxides such as yttria-stabilized zirconia and scandia-stabilized zirconia. These can be used alone or in combination of two or more. In this embodiment, the first electrode 3 can be specifically configured of a mixture of Ni and yttria-stabilized zirconia. In FIG. 1, the reference numeral 30 denotes a pore. In addition, both the electron conductive material 31 and the oxygen ion conductive material 32 in the first electrode 3 can be in the form of particles.

[0019] When the first electrode 3 is made to function as a support, the thickness of the first electrode 3 can be, for example, preferably 100 to 800 μm, more preferably 150 to 700 μm, and even more preferably 200 to 600 μm, from the viewpoints of strength, electrical resistance, gas diffusibility, etc. When the first electrode 3 is not made to function as a support, the thickness of the first electrode 3 can be, for example, preferably 10 to 40 μm, more preferably 15 to 35 μm, and even more preferably 20 to 30 μm, from the viewpoints of electrical resistance, gas diffusibility, etc.

[0020] The second electrode 4 is an electrode that forms a pair with the first electrode 3. Specifically, as shown in FIG. 1, the second electrode 4 can be disposed so as to face the first electrode 3 with the solid electrolyte layer 2 interposed therebetween. The outer shape of the second electrode 4 may be formed to be the same size as the outer shape of the first electrode 3, or may be formed to be smaller than the outer shape of the first electrode 3. The second electrode 4 can be formed to be porous. The second electrode 4 can be formed in a layered shape, and may be composed of a single layer or may be composed of multiple layers. FIG. 1 shows an example in which the second electrode 4 is composed of a single layer.

[0021] Here, the second electrode 4 contains a metal oxide 41 having oxygen non-stoichiometry and a decomposition product 42 of the metal oxide having oxygen non-stoichiometry. The metal oxide 41 having oxygen non-stoichiometry is a composite metal oxide, and is a material that can have point defects at oxygen positions by containing metal elements having different valences. The decomposition product 42 of the metal oxide having oxygen non-stoichiometry is a substance generated by decomposition of the metal oxide 41 having oxygen non-stoichiometry. The metal oxide 41 having oxygen non-stoichiometry may be contained in the second electrode 4 in one or two or more kinds. In addition, the decomposition product 42 of the metal oxide having oxygen non-stoichiometry may be contained in the second electrode 4 in one or two or more kinds.

[0022] The metal oxide 41 having oxygen non-stoichiometry can be configured to include an oxygen-deficient metal oxide 411. The oxygen-deficient metal oxide 411 is a metal oxide with oxygen vacancies, and the above-mentioned point defect positions are vacant. The oxygen-deficient metal oxide 411 becomes unstable when excessive oxygen enters, and tends to change into a more stable oxide or the like. Therefore, the configuration in which the metal oxide 41 having oxygen non-stoichiometry includes the oxygen-deficient metal oxide 411 has the following advantages. That is, the oxygen-deficient metal oxide 411 increases sensitivity to a high oxygen concentration atmosphere, and as shown in FIG. 2(a), in a portion where a high oxygen concentration atmosphere occurs, the oxygen-deficient metal oxide 411 is decomposed by the excessive oxygen that has entered, and a decomposition product with reduced activity or an inactive decomposition product is generated. That is, as shown in FIG. 2(b), a decomposition product 421 of the oxygen-deficient metal oxide is generated. Since the decomposition product 421 of the oxygen-deficient metal oxide has poor electrode activity, the reaction moves to another reaction field 44 as shown in Figures 2(a) and (b), and local overload reactions (local overload water electrolysis reactions in the SOEC mode described later, and local overload power generation reactions in the SOFC mode described later) are suppressed, thereby suppressing reaction unevenness within the cell surface.

[0023] The metal oxide 41 having oxygen non-stoichiometry can have a perovskite structure or a double perovskite structure. According to this structure, metal elements with different valences are fixed, so that in a steady operating environment of a solid oxide electrochemical cell (hereinafter, sometimes referred to as SOEC) such as a water electrolysis cell (including a steam electrolysis cell, omitted below) or a solid oxide fuel cell (hereinafter, sometimes referred to as SOFC), the structure having oxygen non-stoichiometry can be changed in response to oxygen concentration fluctuations to form a stable compound. Therefore, according to this structure, even if the second electrode 4 is placed in an environment with a different oxygen concentration during steady operation of the electrochemical cell 1, it is easy to ensure electrode activity. The metal oxide 41 having oxygen non-stoichiometry can preferably have a perovskite structure. According to this structure, the metal at the A site or the B site can form a stable compound due to oxygen concentration fluctuations. Therefore, this configuration is advantageous in realizing a uniform electrolytic reaction while maintaining power generation performance.

[0024] The oxygen-deficient metal oxide 411 is, for example, (La,Sr)CoO 3-δ , (La,Sr)(Co,Fe)O 3-δ , (La,Sr)(Mn,Fe)O 3-δ , (La,Sr)FeO 3-δ , (Sm,Sr)CoO 3-δ , (La,Ca)CrO 3-δ , (Ba,La)CoO 3-δ These may be used alone or in combination of two or more. Here, δ indicates the oxygen non-stoichiometric amount. The above (A, B) means that at least one of the A element and the B element is included, and that the A element and the B element are partially substitutable for each other so that the total chemical composition of the A element and the B element is 1 (the same applies below). Of the above-mentioned oxygen-deficient metal oxides 411, from the viewpoints of electrical resistivity, low toxicity to other functional layers, raw material cost, etc., it is preferable to use (La,Sr)CoO 3-δ, (La,Sr)(Co,Fe)O 3-δ , (Sm,Sr)CoO 3-δ etc., more preferably (La,Sr)CoO 3-δ It is.

[0025] (La,Sr)CoO 3-δ Specifically, La 1-x Sr x Chief of Staff 3-δ (0≦x≦1, preferably 0.1≦x≦0.5), (La,Sr)(Co,Fe)O 3-δ Specifically, La 1-x Sr x Co 1-y Fe y O 3-δ (0≦x≦1, 0≦y≦1, preferably 0.1≦x≦0.5, 0.5≦y≦0.9), (La,Sr)(Mn,Fe)O 3-δ Specifically, La 1-x Sr x Mn 1-y Fe y O 3-δ (0≦x≦1, 0≦y≦1, preferably 0.1≦x≦0.5, 0.5≦y≦0.9), (La,Sr)FeO 3-δ Specifically, La 1-x Sr x FeO 3-δ (0≦x≦1, preferably 0.1≦x≦0.5), (Sm,Sr)CoO 3-δ Specifically, Sm 1-x Sr x Chief of Staff 3-δ (0≦x≦1, preferably 0.4≦x≦0.6), (La,Ca)CrO 3-δ Specifically, La 1-x Ca x Chief of Staff 3-δ (0≦x≦1, preferably 0.1≦x≦0.5), (Ba,La)CoO 3-δ Specifically, Ba 1-x La x Chief of Staff 3-δ(0≦x≦1, preferably 0.1≦x≦0.5) can be exemplified. These can be used alone or in combination of two or more. These metal oxides have a perovskite structure.

[0026] Specific examples of the decomposition product 421 of the oxygen-deficient metal oxide include inactive oxides containing one or more of the metal elements constituting the oxygen-deficient metal oxide 411 described above. (La,Sr)CoO 3-δ Examples of decomposition products include Sr3Co2O 6.6 Examples include oxides containing Sr and Co, such as Sr2Co2O5. (La,Sr)(Co,Fe)O 3-δ Examples of decomposition products include Sr3Co2O 6.6 Examples of the oxides include oxides containing Sr and Co and / or Fe, such as Sr2Co2O5 and SrFeO2. (Sm,Sr)CoO 3-δ Examples of decomposition products include Sr3Co2O 6.6 , and oxides containing Sr and Co such as Sr2Co2O5.

[0027] FIG. 1 shows an example in which the metal oxide 41 having oxygen non-stoichiometry is composed of an oxygen-deficient metal oxide 411. Therefore, in this embodiment, as exemplified in FIG. 1, the second electrode 4 contains the oxygen-deficient metal oxide 411 and a decomposition product 421 of the oxygen-deficient metal oxide. The decomposition product 421 of the oxygen-deficient metal oxide is a substance generated by decomposition of a part of the oxygen-deficient metal oxide 411 contained in the second electrode 4. Note that the above-mentioned metal oxide 41 having oxygen non-stoichiometry, the decomposition product 42 of the metal oxide having oxygen non-stoichiometry, the oxygen-deficient metal oxide 411, and the decomposition product 421 of the oxygen-deficient metal oxide can all be in the form of particles.

[0028] The metal oxide 41 having oxygen non-stoichiometry is During steady-state cell operation, 10 -1 bar~10 -0.5 It does not decompose under oxygen partial pressure of less than bar and at the temperature of steady-state operation of the cell. Oxygen partial pressure is 10 -6 Bar or less or 10-0.5 Normally, during steady-state operation of SOECs and SOFCs, the oxygen electrode of the SOEC and the air electrode (oxidizer electrode) of the SOFC are exposed to an oxygen concentration of 10 -1 bar~10 -0.5 The pressure is less than bar. Therefore, according to the above configuration, when the electrochemical cell 1 is operated in a steady state as at least one of an SOEC and an SOFC, the metal oxide 41 having oxygen non-stoichiometry is unlikely to decompose in the oxygen concentration atmosphere to which the second electrode 4 is exposed. Therefore, according to the above configuration, an electrochemical cell 1 that can easily ensure a stable output during steady state operation can be obtained.

[0029] For example, the above-mentioned (La,Sr)CoO 3-δ , (La,Sr)(Co,Fe)O 3-δ As can be understood from the literature "K. Kendall, M. Kendall, "Chapter 6-Cathodes" High-temperature Solid Oxide Fuel Cells for the 21st Century, p166, Figure 6.4 (2015)", -8 Decomposition occurs at an oxygen concentration of 1 bar. In addition, (La,Sr)MnO 3+δ As can be understood from the literature "T. Ishihara "Perovskite Oxide for Cathode of SOFCs" Perovskite Oxide for Solid Oxide Fuel Cells, p160, Fig7.9 (2009)", -7 Decomposition occurs at an oxygen concentration of 1 bar.

[0030] As illustrated in FIG. 1, the second electrode 4 may further include an oxygen ion conductive material 43 having oxygen ion conductivity. Examples of the oxygen ion conductive material 43 used in the second electrode 4 include ceria (CeO2), ceria doped with one or more elements selected from Gd, Y, Sm, La, Nd, Yb, Ca, and Ho, zirconia doped with one or more elements selected from Y, Ca, and Sc, (La,Sr)(Ga,Mg)O3, (La,Sr)(Sc,Mg)O3, and (La,Sr)(Al,Mg)O3. These may be used alone or in combination. Specific examples of (La,Sr)(Ga,Mg)O3 include La, 1-x Sr x Ga 1-y Mg y O3 (0≦x≦1, 0≦y≦1, preferably 0.1≦x≦0.3, 0.1≦y≦0.3), (La,Sr)(Sc,Mg)O3 is specifically, 1-x Sr x Sc 1-y Mg y O3 (0≦x≦1, 0≦y≦1, preferably 0.1≦x≦0.5, 0.1≦y≦0.3), (La,Sr)(Al,Mg)O3 is La 1-x Sr x Al 1-y Mg y O3 (0≦x≦1, 0≦y≦1, preferably 0.1≦x≦0.5, 0.1≦y≦0.5) can be exemplified.

[0031] Of the above-mentioned oxygen ion conductive materials 43 used in the second electrode 4, Gd-doped ceria is preferable from the viewpoints of small temperature dependence of oxygen ion conductivity, electronic conductivity, and suppression of reaction with other functional layers. In Fig. 1, reference numeral 40 denotes pores. The oxygen ion conductive material 43 used in the second electrode 4 may be in the form of particles.

[0032] In the second electrode 4, the amount of the oxygen-unstable metal oxide 41 in the total of the oxygen-unstable metal oxide 41 and the decomposition product 42 of the oxygen-unstable metal oxide is preferably 95% by volume or more in order to ensure a sufficient number of reaction sites for electrolysis and power generation reactions. The volume percentage can be calculated using the results of 3D element mapping using FIB-SEM-EDS (energy dispersive X-ray spectroscopy using a focused ion beam scanning electron microscope) or the like.

[0033] The thickness of the second electrode 4 can be 5 μm or more. In the electrochemical cell 1, in addition to the metal oxide 41 having oxygen non-stoichiometry, the second electrode 4 contains a decomposition product 42 of the metal oxide having oxygen non-stoichiometry. In other words, the second electrode 4 loses a part of its electrode activity due to the decomposition of a part of the metal oxide 41 having oxygen non-stoichiometry, compared to an electrode that contains the metal oxide 41 having oxygen non-stoichiometry and does not contain the decomposition product 42 of the metal oxide having oxygen non-stoichiometry. Therefore, if the thickness of the second electrode 4 is within the above range, it becomes easier to secure reaction points where sufficient reaction can be obtained by ensuring the electrode thickness, and it becomes easier to suppress the performance deterioration of the second electrode 4.

[0034] From the viewpoint of ensuring sufficient reaction sites, the thickness of the second electrode 4 is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, and even more preferably 25 μm or more. From the viewpoint of gas diffusibility, electrical resistance, and the like, the thickness of the second electrode 4 is preferably 100 μm or less, more preferably 60 μm or less, and even more preferably 50 μm or less.

[0035] When the electrochemical cell 1 has an intermediate layer, the intermediate layer can be specifically formed in a layer shape from a solid electrolyte having oxygen ion conductivity. Examples of the solid electrolyte used in the intermediate layer include ceria (CeO2) and ceria doped with one or more elements selected from Gd, Sm, Y, La, Nd, Yb, Ca, and Ho. These can be used alone or in combination. Gd-doped ceria is preferable as the solid electrolyte used in the intermediate layer.

[0036] The thickness of the intermediate layer can be set to preferably 1 to 20 μm, and more preferably 2 to 10 μm, from the viewpoints of reducing ohmic resistance, suppressing element diffusion from the second electrode, and the like.

[0037] The thickness of each portion of the electrochemical cell 1 described above is the arithmetic mean value of thickness measurements at 10 points in each portion measured by observing a cross section perpendicular to the cell surface of the electrochemical cell 1 with a scanning electron microscope (SEM).

[0038] The electrochemical cell 1 can be produced, for example, as follows.

[0039] A cell (not shown) is fabricated, which includes a solid electrolyte layer 2 having oxygen ion conductivity, a first electrode 3 disposed on one side of the solid electrolyte layer 2, and a second electrode precursor (not shown) disposed on the other side of the solid electrolyte layer 2, which includes a metal oxide 41 having oxygen non-stoichiometry but does not include a decomposition product 42 of the metal oxide having oxygen non-stoichiometry. In this embodiment, specifically, for example, a second electrode precursor containing an oxygen-deficient metal oxide 411 but not a decomposition product 421 of the oxygen-deficient metal oxide can be used. Next, a leveling process is performed on this cell, which is operated at a current density higher than the current density during steady operation of the electrochemical cell 1, that is, in a current density region in which non-uniform reactions become more evident. As a result, in a portion in the second electrode precursor where current is likely to flow locally, the metal oxide 41 having oxygen non-stoichiometry decomposes, generating a decomposition product 42 of the metal oxide having oxygen non-stoichiometry. On the other hand, in a portion in the second electrode precursor where local current does not flow, decomposition of the metal oxide 41 having oxygen non-stoichiometry hardly progresses. The leveling process converts the second electrode precursor into the second electrode 4 containing the metal oxide 41 having oxygen non-stoichiometry and the decomposition product 421 of the metal oxide having oxygen non-stoichiometry, and the electrochemical cell 1 described above is obtained. That is, in the manufacturing method of the electrochemical cell 1, the leveling process is performed on the cell, and a part of the metal oxide 41 having oxygen non-stoichiometry is intentionally decomposed in the state of the cell, thereby mitigating the reaction distribution in the cell surface of the electrochemical cell 1 obtained. That is, the reaction in the cell surface of the electrochemical cell 1 is leveled. Note that, as the leveling process, for example, a process of supplying a mixed gas of H2 and H2O to the first electrode 3, supplying air to the second electrode precursor, and operating at a leveling temperature of 650°C to 850°C in a current density region higher than the current density during steady operation can be exemplified. As the current density region higher than the current density during steady operation, for example, a current density range of 2 to 4 times the current density (described later) when the electrochemical cell 1 is operated for steady power generation can be exemplified. The treatment time for the power generation operation can be, for example, 2 to 10 hours. The above treatment can be carried out once, or can be carried out multiple times under the same conditions or different conditions.The electrochemical cell 1 thus obtained is preferably operated in a steady state at a current density equal to or lower than the current density during the above-mentioned leveling treatment.

[0040] The electrochemical cell 1 can be used as at least one of an SOEC and an SOFC. That is, the electrochemical cell 1 may be operated as an SOEC, or may be operated as an SOFC, or may be configured to be switchable between an SOEC mode in which the electrochemical cell 1 is operated as an SOEC and an SOFC mode in which the electrochemical cell 1 is operated as an SOFC, and may be operated as an SOEC and an SOFC. An example of the operation of the electrochemical cell 1 will be described below.

[0041] First, an example of operating the electrochemical cell 1 as an SOEC will be described with reference to FIG. 3. In this case, the first electrode 3 is used as a hydrogen electrode, and the second electrode 4 is used as an oxygen electrode. The first electrode 3 can be supplied with a water (H2O)-containing gas F1, such as water vapor gas, as a fuel F. The second electrode 4 can be supplied with a gas A1, such as air, or no gas A1. FIG. 3 shows an example of supplying the gas A1 to the second electrode 4. A first electrode side gas flow passage 5 can be arranged in contact with the first electrode 3 on the first electrode 3 side. A second electrode side gas flow passage 6 can be arranged in contact with the second electrode 4 on the second electrode 4 side. As illustrated in FIG. 3, a power source 7 is connected between the first electrode 3 and the second electrode 4. In the SOEC mode, the fuel F supplied from the supply port 51 of the first electrode side gas flow passage 5 passes through the first electrode side gas flow passage 5 and reaches the first electrode 3. At the first electrode 3, H2O+2e - →H2+O 2- The remaining fuel F is discharged from the exhaust port 52 together with the generated hydrogen gas (H2) through the first electrode side gas flow passage 5. On the other hand, at the second electrode 4, O 2- →1 / 2O2+2e -The electrode reaction of the following occurs. The generated oxygen gas (O2) is discharged from the outlet 62. When the gas A1 is not supplied to the second electrode 4, the generated oxygen gas is discharged from the outlet 62 due to the difference in oxygen concentration with the outside. When the gas A1 is supplied to the second electrode 4, there is an advantage that the generated oxygen gas is diluted by the gas A1 and discharged to the outside. In the solid electrolyte layer 2, oxygen ions (O 2- ) moves. In this way, the electrochemical cell 1 can be operated as an SOEC. Note that, in the first electrode 3, a conditioning gas (reducing gas) (not shown) such as hydrogen gas can be mixed with the water-containing gas F1 as the fuel F. In this case, oxidation of the metal material that may be contained in the first electrode 3 during the SOEC operation can be suppressed.

[0042] Next, an example of operating the electrochemical cell 1 as an SOFC will be described with reference to FIG. 4. In this case, the first electrode 3 is used as a fuel electrode, and the second electrode 4 is used as an air electrode (oxidizer electrode). The first electrode 3 can be supplied with a hydrogen-containing gas F2 such as hydrogen gas as a fuel F. The second electrode 4 can be supplied with an oxygen-containing gas A2 such as air or oxygen gas as an oxidizer. A first electrode side gas flow passage 5 can be arranged in contact with the first electrode 3 on the first electrode 3 side. A second electrode side gas flow passage 6 can be arranged in contact with the second electrode 4 on the second electrode 4 side. As illustrated in FIG. 4, a load 8 is connected between the first electrode 3 and the second electrode 4. In the SOFC mode, the fuel F supplied from the supply port 51 of the first electrode side gas flow passage 5 passes through the first electrode side gas flow passage 5 and reaches the first electrode 3. At the first electrode 3, H2+O 2- →H2O+2e - The electrode reaction of 1 / 2O2+2e occurs. The remaining fuel F passes through the first electrode gas flow passage 5 together with the generated water vapor (H2O) and is discharged from the outlet 52. On the other hand, the oxygen-containing gas A2 supplied from the supply port 61 of the second electrode gas flow passage 6 passes through the second electrode gas flow passage 6 and reaches the second electrode 4. At the second electrode 4, the reaction is expressed as 1 / 2O2+2e - →O 2-The remaining oxygen-containing gas A2 passes through the second electrode side gas flow passage 6 and is discharged from the outlet 62. In the solid electrolyte layer 2, oxygen ions (O 2- ) moves. In this way, the electrochemical cell 1 can be operated as a SOFC. Note that, at the first electrode 3, the hydrogen-containing gas F2 as the fuel F can also be mixed with water vapor or the like (not shown).

[0043] Next, an example of operating the electrochemical cell 1 as both an SOEC and an SOFC (operating the electrochemical cell 1 reversibly) will be described. In this case, the electrochemical cell 1 may be configured to be operable as both an SOEC and an SOFC as described above. With this configuration, it is possible to obtain an electrolysis / power generation device that uses electricity from surplus power, renewable energy, etc. to operate the electrochemical cell 1 as an SOEC, stores the generated hydrogen gas separately, and uses the stored hydrogen gas as fuel to operate the electrochemical cell 1 as an SOFC to generate power.

[0044] The steady-state operating temperature of the electrochemical cell 1 can be, for example, 400° C. or higher and 800° C. or lower when functioning as an SOEC, and 400° C. or higher and 800° C. or lower when functioning as an SOFC, similar to the SOEC. The current density during steady-state operation of the electrochemical cell 1 can be, for example, 0.4 A / cm when functioning as an SOEC. 2 More than 2.0A / cm 2 When functioning as a SOFC, the current is 0.2A / cm 2 More than 1.0A / cm 2 It can be as follows:

[0045] (Embodiment 2) The electrochemical cell of the second embodiment will be described with reference to Fig. 5. Of the symbols used in the second and subsequent embodiments, the same symbols as those used in the previous embodiments represent the same components, etc. as those in the previous embodiments, unless otherwise specified.

[0046] 5, the electrochemical cell 1 of this embodiment is different from the electrochemical cell 1 of embodiment 1 in the configuration of the second electrode 4. Specifically, in this embodiment, the metal oxide 41 having oxygen non-stoichiometry in the second electrode 4 can further include an oxygen-excess metal oxide 412.

[0047] The oxygen-excess metal oxide 412 is a metal oxide with interstitial oxygen, and the above-mentioned point defect positions are excessively filled. When the interstitial oxygen is removed, the oxygen-excess metal oxide 412 becomes unstable and tends to change into a more stable oxide. Therefore, the following advantages are obtained when the metal oxide 41 having oxygen non-stoichiometry includes not only the oxygen-deficient metal oxide 411 but also the oxygen-excess metal oxide 412. That is, when a high oxygen concentration atmosphere is locally generated in the second electrode 4, even if the oxygen-deficient metal oxide 411 contained in the second electrode 4 decomposes excessively, the oxygen-excess metal oxide 412 does not decompose. Conversely, when a low oxygen concentration atmosphere is locally generated in the second electrode 4, even if the oxygen-excess metal oxide 412 contained in the second electrode 4 decomposes excessively, the oxygen-deficient metal oxide 411 does not decompose. Therefore, according to the above-mentioned configuration, it is possible to prevent the amount of catalytically active material in the second electrode 4 from becoming excessively small, and to prevent a decrease in the electrode activity of the second electrode 4. In other words, according to the above configuration, even if a high oxygen concentration atmosphere or a low oxygen concentration atmosphere is locally generated within the second electrode 4, excessive decomposition of the metal oxide 41 having oxygen instability that exhibits catalytic activity can be suppressed.

[0048] The oxygen-excess metal oxide 412 is, for example, (La,Sr)MnO 3+δ , PrBaCoO 5+δ , PrBaFeO 5+δ These can be used alone or in combination of two or more. Here, δ indicates the non-stoichiometric amount of oxygen. Among the above-mentioned oxygen-excess metal oxides 412, (La,Sr)MnO is preferable from the viewpoint of electrical resistivity, cost required for material purification, and the like. 3+δ , PrBaCoO 5+δand the like, and more preferably (La,Sr)MnO 3+δ It is.

[0049] (La,Sr)MnO 3+δ Specifically, La 1-x Sr x MnO 3+δ (0≦x≦1, preferably 0.1≦x≦0.4) can be exemplified. These can be used alone or in combination of two or more. These metal oxides have a perovskite structure or a double perovskite structure.

[0050] Specific examples of the decomposition product 422 of the oxygen-excess metal oxide include inactive oxides containing one or more metal elements constituting the oxygen-excess metal oxide 412 described above. (La,Sr)MnO 3+δ Examples of the decomposition products include oxides containing Sr and Mn, such as Sr2Mn2O5 and Sr2MnO4.

[0051] In this embodiment, the second electrode 4 may contain an oxygen-deficient metal oxide 411, a decomposition product 421 of the oxygen-deficient metal oxide, and an oxygen-excess metal oxide 412, or may contain an oxygen-deficient metal oxide 411, a decomposition product 421 of the oxygen-deficient metal oxide, an oxygen-excess metal oxide 412, and a decomposition product 422 of the oxygen-excess metal oxide. The decomposition product 422 of the oxygen-excess metal oxide is a substance generated by decomposition of a part of the oxygen-excess metal oxide 412 contained in the second electrode 4. The metal oxide 41 having oxygen non-stoichiometry, the decomposition product 42 of the metal oxide having oxygen non-stoichiometry, the oxygen-deficient metal oxide 411, the decomposition product 421 of the oxygen-deficient metal oxide, the oxygen-excess metal oxide 412, and the decomposition product 422 of the oxygen-excess metal oxide may all be in the form of particles. The electrochemical cell 1 having the second electrode 4 in this embodiment may be manufactured, for example, as follows. Specifically, the second electrode precursor described above in the first embodiment includes an oxygen-deficient metal oxide 411 and an oxygen-excess metal oxide 412, but does not include a decomposition product 421 of the oxygen-deficient metal oxide and a decomposition product 422 of the oxygen-excess metal oxide. As described above in the first embodiment, the electrochemical cell 1 is operated at a current density in the range of 2 to 4 times the current density during steady-state power generation, and then the electrochemical cell 1 is further operated at a current density in the range of 2 to 4 times the current density during steady-state electrolysis. The treatment time for the electrolysis operation can be, for example, 2 to 10 hours.

[0052] The second electrode 4 may further include an oxygen ion conductive material 43 having oxygen ion conductivity as described above in the embodiment 1. In Fig. 5, an example is shown in which the second electrode 4 includes an oxygen-deficient metal oxide 411, a decomposition product 421 of the oxygen-deficient metal oxide, an oxygen-excess metal oxide 412, a decomposition product 422 of the oxygen-excess metal oxide, and the oxygen ion conductive material 43.

[0053] The other configurations and effects are the same as those of the first embodiment.

[0054] (Experimental Example) <Material preparation> NiO powder (average particle size: 1.0 μm), yttria-stabilized zirconia (hereinafter, YSZ) powder (average particle size: 0.5 μm) containing 8 mol% Y2O3, carbon (pore former), polyvinyl butyral, isoamyl acetate, and 1-butanol were mixed in a ball mill to prepare a slurry. The mass ratio of NiO powder to YSZ powder was 65:35. The above slurry was applied in layers on a resin sheet using a doctor blade method, dried, and then the resin sheet was peeled off to prepare a sheet for forming a first electrode. The above average particle size is the particle size (diameter) d50 when the cumulative frequency distribution on a volume basis measured by a laser diffraction / scattering method shows 50% (hereinafter the same).

[0055] A slurry was prepared by mixing YSZ powder (average particle size: 0.5 μm), polyvinyl butyral, isoamyl acetate, and 1-butanol in a ball mill. Thereafter, a sheet for forming a solid electrolyte layer was prepared in the same manner as in the preparation of the sheet for forming the first electrode.

[0056] A slurry was prepared by mixing Gd-doped CeO2 (hereinafter, GDC) powder (average particle size: 0.3 μm), polyvinyl butyral, isoamyl acetate, 2-butanol, and ethanol in a ball mill. In this experimental example, CeO2 doped with 10 mol% Gd was used as GDC. Thereafter, an intermediate layer forming sheet was prepared in the same manner as in the preparation of the first electrode forming sheet.

[0057] (La,Sr)CoO as an oxygen-deficient metal oxide 3-δ Powder (average particle size: 1.5 μm) as an oxygen ion conductive material and GDC powder (average particle size: 2.0 μm) were mixed, and the mixture was dispersed in terpineol as a solvent together with a dispersant. Ethyl cellulose as a binder was added to the obtained dispersion and mixed to prepare a paste for forming a second electrode. Note that the above (La,Sr)CoO 3-δ Specifically, the powder contains La 0.6 Sr0.4 Chief of Staff 3-δ Powder was used. (La,Sr)CoO 3-δ The mass ratio of the powder to the GDC powder was 50:50.

[0058] <Preparation of electrochemical cell> A plurality of sheets for forming the first electrode, a sheet for forming the solid electrolyte layer, and a sheet for forming the intermediate layer were laminated in this order and pressed together using a hydrostatic press (WIP) molding method. The WIP molding conditions were a temperature of 85°C, a pressure of 50 MPa, and a pressing time of 10 minutes. The obtained molded body was degreased.

[0059] The obtained molded body was then sintered in an air atmosphere at 1350° C. for 2 hours, thereby obtaining a sintered body in which a layered first electrode (thickness 400 μm), a solid electrolyte layer (3.5 μm), and an intermediate layer (3 μm) were laminated in this order.

[0060] Next, a paste for forming a second electrode was applied to the surface of the intermediate layer of the fired body by screen printing, and fired (baked) in an air atmosphere at 950°C for 2 hours to form a layered second electrode precursor (thickness 50 μm). The outer shape of the second electrode precursor was formed smaller than that of the first electrode. This formed a flat cell. The formed cell is usually assembled to a metal stack member and can operate as a system. In this experimental example, in order to eliminate various environmental factors such as poisonous substances scattered from metal members and temperature distribution due to large size, a small cell was formed, and only this cell was used to perform the following processing and evaluation using an element evaluation bench.

[0061] Next, sealing glass was applied to the end face of the obtained cell. The cell was heated to 850°C in an air atmosphere, and the first electrode and the fuel pipe were sealed with glass to form a gas seal structure. Next, the first electrode was subjected to a reduction treatment. The reduction treatment conditions were as follows: reduction temperature: 800°C, reduction treatment gas: hydrogen gas, reduction time: 3 hours.

[0062] Next, after the reduction treatment, the temperature was lowered slightly to the power generation temperature, and the cell was supplied with a current density twice that during steady-state power generation (specifically, 1.5 A / cm 2 ) for 4 hours of power generation. At this time, a mixed gas of H2 and H2O (H2:H2O=6:4 in volume ratio) was supplied to the first electrode, and air was supplied to the second electrode precursor. The power generation temperature was set to 700°C. In this experimental example, the cell that had been power-generated was further subjected to an electrolysis operation for 4 hours at the same current density as above. At this time, a mixed gas of H2 and H2O (H2:H2O=6:4 in volume ratio) was supplied to the first electrode, and air was supplied to the second electrode precursor. The water electrolysis temperature was set to 700°C. Thereafter, the temperature was lowered while maintaining the atmosphere of the first electrode. In this way, an electrochemical cell according to this experimental example was produced. In this experimental example, both the power generation operation and the electrolysis operation were performed as the leveling process. This is because the reaction distribution caused by factors such as unevenness in the voids within the cell surface creates areas that are difficult to react in power generation operation due to a rate-limiting part for the supply of hydrogen, whereas during electrolysis operation, creates areas that are difficult to react in due to a rate-limiting part for the supply of water vapor. This ensures that a uniform reaction is obtained in both modes.

[0063] <XRD analysis of the second electrode> The electrochemical cell was removed from the element evaluation bench and the structure of the second electrode was analyzed using an X-ray diffraction device (RIGAKU Corporation, fully automated multipurpose X-ray diffraction device "SmartLab"). In this experimental example, in order to eliminate various environmental factors during the production of the electrochemical cell, the leveling process was performed using only a small cell. Therefore, the substances that can be contained in the second electrode were basically the (La,Sr)CoO 3-δ These can be broadly divided into GDCs (including impurities in the raw materials) and other substances, i.e., compounds formed during production.

[0064] The XRD analysis results of the second electrode are shown in FIG. 6. According to FIG. 6, the second electrode of the electrochemical cell is composed of (La,Sr)CoO 3-δIn addition to the peaks of La2O3 and GDC, the peaks of La2O3 and Sr2Co2O5 were detected. The peaks of La2O3 and Sr2Co2O5 were detected because of the oxygen nonstoichiometric metal oxide (La,Sr)CoO 3-δ However, the leveling treatment decomposed the precursor to produce La2O3 and Sr2Co2O5. For comparison, the second electrode precursor in a cell that had not been subjected to the leveling treatment was subjected to similar XRD analysis, and no peaks for La2O3 or Sr2Co2O5 were detected in the second electrode precursor.

[0065] The electrochemical cell and the cell that had not been subjected to the leveling treatment were used as an SOFC, and the cells were charged at 700°C and a current density of 0.5 A / cm 2 The electrochemical cell was operated at a steady state at 100°C. As a result, the electrochemical cell had a reduced reaction temperature distribution within the cell surface compared to a cell that had not been subjected to the above-mentioned leveling process. The electrochemical cell was operated as an SOFC to confirm the reaction temperature distribution within the cell surface because, since a power generation reaction occurs in an SOFC, it is easier to confirm the reaction temperature distribution within the cell surface compared to an SOEC. From these results, it was confirmed that the electrochemical cell can suppress reaction unevenness within the cell surface.

[0066] The present invention is not limited to the above-described embodiments and experimental examples, and various modifications are possible without departing from the spirit and scope of the present invention. Furthermore, the configurations shown in the embodiments and experimental examples can be combined in any manner. [Explanation of symbols]

[0067] 1. Electrochemical cell 2 Solid electrolyte layer 3 1st electrode 4 Second electrode F fuel F1 Water-containing gas F2 Hydrogen-containing gas

Claims

1. a solid electrolyte layer (2) having oxygen ion conductivity, a first electrode (3) disposed on one side of the solid electrolyte layer and supplied with fuels (F, F1, F2), and a second electrode (4) disposed on the other side of the solid electrolyte layer and paired with the first electrode; The second electrode includes a metal oxide having oxygen non-stoichiometry (41) and a decomposition product of the metal oxide having oxygen non-stoichiometry (42), The metal oxide having oxygen non-stoichiometry does not decompose under an oxygen partial pressure of 10 −1 bar to less than 10 −0.5 bar during steady-state cell operation, and does not decompose under a temperature during steady-state cell operation and an oxygen partial pressure of 10 -6 Bar or less, or 10 -0.5 It is a material that decomposes at or above bar. Electrochemical cell (1).

2. The metal oxide having oxygen non-stoichiometry includes an oxygen-deficient metal oxide (411), 10. The electrochemical cell of claim 1.

3. The metal oxide having oxygen non-stoichiometry further includes an oxygen-excess metal oxide (412), 3. The electrochemical cell of claim 2.

4. The metal oxide having oxygen non-stoichiometry has a perovskite structure.

4. An electrochemical cell according to any one of claims 1 to 3.

5. The thickness of the second electrode is 5 μm or more.

5. An electrochemical cell according to any one of claims 1 to 4.

6. Used as at least one of a solid oxide electrolysis cell and a solid oxide fuel cell, 6. An electrochemical cell according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Manufacturing method of material for solid oxide fuel cell

    JP2007200693A

  • High temperature water vapor electrolyzer, method therefor and cell for fuel cell

    JP2008045152A

  • Air electrode material and solid oxide fuel cell

    JP2011228270A

  • Positive electrode material for fuel cell, positive electrode for fuel cell including the same, and solid oxide fuel cell

    JP2012227142A

  • A fuel cell system configured to capture chromium

    JP2016512388A