Composite semipermeable membrane, composite semipermeable membrane element and filtration device
The composite semipermeable membrane with controlled pore diameters and amino group densities, and a hollow pleated structure, addresses the challenge of selective ion separation under acidic conditions, achieving high monovalent ion permeability and multivalent ion blocking.
Patent Information
- Application Number
- JP2023577798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-09-29
- Filing Date
- 2023-11-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-11-30
AI Technical Summary
Existing nanofiltration membranes face challenges in achieving effective monovalent ion/multivalent ion selective separation performance under acidic conditions, with issues such as low chemical resistance, poor selective separation, and pore size changes under varying pH conditions.
A composite semipermeable membrane with a porous support layer and a separation functional layer containing semi-aromatic crosslinked polyamide, irradiated with a positron beam, has controlled pore diameters and amino group densities, and a hollow pleated structure, ensuring uniform pore distribution and selective ion separation.
The membrane exhibits excellent monovalent ion/multivalent ion selective separation performance under acidic conditions, with high permeability and resistance to chemical changes, effectively blocking multivalent ions while allowing monovalent ions to pass through.
Smart Images

Figure 0007593512000007 
Figure 0007593512000008 
Figure 0007593512000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite semipermeable membrane, a composite semipermeable membrane element, and a filtration device. [Background technology]
[0002] Regarding the separation of mixtures, there are various technologies for removing substances (e.g., salts) dissolved in a solvent (e.g., water), but in recent years, the use of membrane separation methods has expanded as a process for saving energy and resources. Membranes used in membrane separation methods include microfiltration membranes, ultrafiltration membranes, nanofiltration membranes, and reverse osmosis membranes, and these membranes are used, for example, to produce drinking water from seawater, brackish water, and water containing harmful substances, to soften drinking water, for food applications, to produce ultrapure water for industrial use, to treat wastewater, and to recover valuable materials.
[0003] Most of the reverse osmosis and nanofiltration membranes currently on the market are composite semipermeable membranes, and there are two types: those with an active layer in which a gel layer and a polymer are crosslinked on a support membrane, and those with an active layer in which a monomer is polycondensed on a support membrane. Among them, composite semipermeable membranes obtained by coating a support membrane with a separation functional layer made of crosslinked polyamide obtained by the polycondensation reaction of a polyfunctional amine and a polyfunctional acid halide are widely used as separation membranes with high permeability and selective separation.
[0004] Conventionally, nanofiltration membranes have been widely used to separate specific substances from mixed solutions of monovalent ions, polyvalent ions, and organic matter, and a nanofiltration membrane equipped with a separation functional layer made of a cross-linked polyamide obtained by reacting an aliphatic amine with an acid halide has been proposed. For example, a nanofiltration membrane made of a polyamide obtained by reacting piperazine with a polyfunctional aromatic carboxylic acid chloride has been disclosed (Patent Document 1). On the other hand, one of the problems that occurs in membrane separation plants using nanofiltration membranes is fouling due to inorganic and organic substances. The water permeability of nanofiltration membranes is significantly reduced by fouling. As a method for improving this, a method of recovering water permeability by washing with an acid or chemical has been proposed, and a nanofiltration membrane with high chemical resistance (Patent Document 2) is also known. In addition, it is also known that a nanofiltration membrane with high chemical resistance can maintain excellent multivalent ion removal properties for a long period of time by forming a polyamide separation functional layer with a large specific surface area and a hydrophobic chemical composition (Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2007-277298 [Patent Document 2] Japan Special Publication No. 2003-534422 [Patent Document 3] International Publication No. 2021 / 085600 Summary of the Invention [Problem to be solved by the invention]
[0006] Thus, the performance required for a nanofiltration membrane includes not only water permeability and selective separation performance, but also chemical resistance, but the membrane described in Patent Document 1 has low chemical resistance. On the other hand, the membrane described in Patent Document 2 has high chemical resistance compared to the membrane described in Patent Document 1, but has a problem of low selective separation of monovalent ions and multivalent ions. In addition, the membrane described in Patent Document 3 suppresses hydrolysis due to contact with acid or alkali and maintains high multivalent ion removal performance under neutral conditions, but the pore size changes under acidic conditions, so there is room for improvement in the selective separation of monovalent ions and multivalent ions when the membrane is used under acidic conditions.
[0007] An object of the present invention is to provide a composite semipermeable membrane, a composite semipermeable membrane element, and a filtration device that exhibit excellent monovalent ion / polyvalent ion selective separation performance under acidic conditions.
Means for Solving the Problems
[0008] In order to achieve the above object, the present invention has the following configuration. [1] A composite semipermeable membrane comprising a porous support layer and a separation functional layer located on one surface side of the porous support layer, The separation functional layer contains a semi-aromatic crosslinked polyamide, Let the surface of the composite semipermeable membrane on the separation functional layer side be the first surface, and the surface opposite to the first surface be the second surface, The composite semipermeable membrane is irradiated with a positron beam from the first surface side, and the average pore diameters R1 and R2 of the separation functional layer derived from the positron annihilation lifetime measurement method are 0.30 nm or more and 2.00 nm or less, and 0.90 ≦ R1 / R2 ≦ 1.10 is satisfied. R1: Average pore diameter under the condition that the positron beam intensity is 0.1 keV R2: Average pore diameter under the condition that the positron beam intensity is 0.5 keV [2] The composite semipermeable membrane according to [1], wherein the average pore diameter R1 is 0.55 nm or more and 1.00 nm or less. [3] In the cross-section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane, the total number P1 of pores with a pore diameter of 0.30 nm or more and 1.20 nm or less, the total number P2 of pores with a pore diameter of 0.50 nm or more and less than 0.80 nm, the total number P3 of pores with a pore diameter of 0.80 nm or more and 1.20 nm or less, and the total number P4 of pores with a pore diameter exceeding 1.20 nm satisfy 0.20 < P2 / P1 < 0.40, P3 / P2 < 0.20, and P4 / P1 ≦ 0.01. The composite semipermeable membrane according to [1] or [2]. [4] The composite semipermeable membrane according to any one of [1] to [3] above, wherein in a cross section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane, the separation functional layer is divided into 5 equally spaced regions from the first surface side to the second surface side, and the regions are designated as regions a to e, and the amino group density Nb in region b and the amino group density Nd in region d satisfy Nb / Nd≦0.80. [5] The above Nb is 1.0×10 -23 mol / nm 2 The composite semipermeable membrane according to the above [4], which is as follows: [6] The composite semipermeable membrane according to any one of the above [1] to [5], wherein B / C is 10 or more, where B is the glucose permeability when a 1000 ppm aqueous glucose solution of pH 6.5 is permeated at an operating pressure of 0.5 MPa, 25°C, and C is the sucrose permeability when a 1000 ppm aqueous sucrose .... [7] The composite semipermeable membrane according to any one of the above [1] to [6], wherein the separating functional layer has a hollow pleated structure. [8] A composite semipermeable membrane element comprising the composite semipermeable membrane according to any one of the above [1] to [7]. [9] A filtration device comprising the composite semipermeable membrane element described in [8] above. Effect of the Invention
[0009] The composite semipermeable membrane of the present invention has a uniform pore size distribution in the thickness direction of the separation functional layer, and therefore the direction in which ions diffuse within the separation functional layer is uniform, and the permeation resistance of monovalent ions, which are large enough to move freely within the separation functional layer, can be sufficiently suppressed while effectively preventing the permeation of multivalent ions, thereby achieving excellent monovalent ion / multivalent ion selective separation performance under acidic conditions. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing a cross section of a composite semipermeable membrane according to one embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic diagram showing a composite semipermeable membrane element according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing a cross section of a separating functional layer in a composite semipermeable membrane according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram of a hollow pleated structure that the separating functional layer of the composite semipermeable membrane according to one embodiment of the present invention has. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following describes in detail the embodiments of the present invention; however, the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention.
[0012] 1.Composite semipermeable membrane The composite semipermeable membrane according to this embodiment includes a porous support layer and a separation functional layer provided on one side of the porous support layer. In the composite semipermeable membrane, the side on the separation functional layer side is called the first side, and the side opposite to the first side is called the second side. The composite semipermeable membrane according to this embodiment is a membrane in a region having fractionation characteristics positioned between a reverse osmosis membrane and an ultrafiltration membrane, and is generally defined as a nanofiltration membrane. Reverse osmosis membranes generally tend to remove most organic matter and ions, while ultrafiltration membranes generally do not remove most ionic species, but remove high molecular weight organic matter.
[0013] (1-1) Support membrane The composite semipermeable membrane according to the present embodiment may include a porous support layer and a separation functional layer, and the porous support layer is a layer constituting the support membrane. The support membrane may be composed of only the porous support layer, or may include a substrate 2 and a porous support layer 3 disposed on the substrate 2, as shown in FIG. 1. That is, as shown in FIG. 1, the composite semipermeable membrane 1 may include a porous support layer 3 and a separation functional layer 4, and the support membrane constituting the porous support layer 3 may be composed of only the porous support layer 3, or may include the substrate 2 and the porous support layer 3.
[0014] The supporting membrane is intended to provide strength to the composite semipermeable membrane by supporting the separating functional layer, and the supporting membrane itself does not substantially have a separating function for low-molecular-weight organic substances, ions, and the like.
[0015] The size and distribution of the pores in the support membrane are not particularly limited, but for example, uniform and fine pores, or pores that gradually become larger from the surface on which the separation functional layer is formed to the other surface, and the size of the fine pores on the surface on which the separation functional layer is formed is 0.1 nm or more and 100 nm or less, are preferred.
[0016] Examples of the material for the substrate include fabrics made of at least one material selected from polyester and aromatic polyamide. Among these, polyester is particularly preferred because of its high mechanical and thermal stability.
[0017] Examples of the fabric used for the substrate include long fiber nonwoven fabric, short fiber nonwoven fabric, etc. It is preferable to use a long fiber nonwoven fabric, since excellent film formability is required so that when a polymer solution is cast onto a substrate, the polymer solution does not strike through due to excessive penetration, the substrate and the porous support layer do not peel off, and defects such as non-uniformity of the film and pinholes do not occur due to fluffing of the substrate.
[0018] Examples of long-fiber nonwoven fabrics include long-fiber nonwoven fabrics composed of thermoplastic continuous filaments. By including a long-fiber nonwoven fabric in the substrate, it is possible to suppress non-uniformity during polymer solution casting and membrane defects caused by fluffing, which occur when only a short-fiber nonwoven fabric is used. In addition, in the process of continuously forming a composite semipermeable membrane, tension is applied to the substrate in the film formation direction, so that it is preferable to use a long-fiber nonwoven fabric, which has excellent dimensional stability, as the substrate.
[0019] In particular, it is preferable that the orientation of the fibers on the surface of the substrate opposite to the surface in contact with the porous support layer is vertical to the film-forming direction, since this maintains the strength of the substrate and prevents film breakage. Here, "vertical orientation" means that the orientation direction of the fibers is parallel to the film-forming direction. Conversely, when the orientation direction of the fibers is perpendicular to the film-forming direction, it is called transverse orientation.
[0020] The fiber orientation degree of the fibers is preferably 0° or more and 25° or less. Here, the "fiber orientation degree" is an index showing the direction of the fibers in the nonwoven fabric, and means the average angle of the fibers constituting the nonwoven fabric when the film-forming direction during continuous film formation is set to 0° and the direction perpendicular to the film-forming direction, i.e., the width direction of the nonwoven fabric, is set to 90°. Therefore, the closer the fiber orientation degree is to 0°, the more vertically oriented it is, and the closer it is to 90°, the more horizontally oriented it is.
[0021] The manufacturing process of the composite semipermeable membrane and the manufacturing process of the element include a heating step, and the phenomenon of shrinkage of the support membrane or composite semipermeable membrane occurs due to heating. In particular, in continuous membrane production, since no tension is applied in the width direction, the membrane is prone to shrink in the width direction. Since the shrinkage of the support membrane or composite semipermeable membrane causes problems such as dimensional stability, it is desirable for the substrate to have a small thermal dimensional change rate.
[0022] In a substrate using a nonwoven fabric, it is preferable for the difference in fiber orientation between the surface opposite the surface in contact with the porous support layer and the surface facing the porous support layer to be 10° or more and 90° or less, since this can suppress dimensional changes in the width direction due to heat applied in a heating process, etc.
[0023] The air permeability of the base material is 0.5cc / cm 2 / s or more is preferable. When the air permeability is in this range, the water permeability of the composite semipermeable membrane is high. This is thought to be because, in the process of forming the support membrane, when a polymer is cast onto a substrate and immersed in a coagulation bath, the rate of non-solvent replacement from the substrate side increases, changing the internal structure of the porous support layer, which affects the amount of monomer retained and the diffusion rate in the subsequent process of forming the separation functional layer. The air permeability can be measured using a Frazier type testing machine based on JIS L1096 (2010). For example, a sample of 200 mm x 200 mm is cut out from the substrate. This sample is attached to the Frazier type testing machine, and the intake fan and air holes are adjusted so that the inclined barometer indicates a pressure of 125 Pa. The amount of air passing through the substrate, i.e., the air permeability, can be calculated from the pressure indicated by the vertical barometer at this time and the type of air hole used. For example, a Frazier type testing machine such as KES-F8-AP1 manufactured by Kato Tech Co., Ltd. can be used.
[0024] The thickness of the substrate is preferably 10 μm or more and 200 μm or less, and more preferably 30 μm or more and 120 μm or less.
[0025] Examples of materials for the porous support layer include polysulfone, polyethersulfone, cellulose acetate, polyvinyl chloride, and mixtures thereof. Among these, polysulfone and polyethersulfone, which have high chemical, mechanical, and thermal stability, are particularly preferred.
[0026] The thickness of the porous support layer affects the strength of the resulting composite semipermeable membrane and the packing density when it is made into an element. In order to obtain sufficient mechanical strength and packing density, the thickness of the porous support layer is preferably 50 μm or more and 300 μm or less, and more preferably 100 μm or more and 250 μm or less.
[0027] The morphology of the porous support layer can be observed by a scanning electron microscope, a transmission electron microscope, an atomic force microscope, or the like. For example, when observing by a scanning electron microscope, the porous support layer is peeled off from the substrate, and then cut in a direction perpendicular to the composite semipermeable membrane surface by freeze fracturing to obtain a sample for cross-sectional observation. This sample is thinly coated with platinum, platinum-palladium, or ruthenium tetrachloride, preferably ruthenium tetrachloride, and observed by a high-resolution field emission scanning electron microscope (hereinafter, "UHR-FE-SEM") at an accelerating voltage of 3 to 15 kV. For example, an S-900 type electron microscope manufactured by Hitachi, Ltd. can be used as the UHR-FE-SEM.
[0028] The support membrane may be selected from various commercially available materials such as "Millipore Filter VSWP" (product name) manufactured by Millipore Corporation and "Ultrafilter UK10" (product name) manufactured by Toyo Roshi Kaisha, Ltd., and may be manufactured according to the method described in "Office of Saline Water Research and Development Progress Report" No. 359 (1968).
[0029] The thickness of the substrate and the thickness of the composite semipermeable membrane can be measured by a digital thickness gauge. Since the thickness of the separation functional layer is very thin compared to the support membrane, the thickness of the composite semipermeable membrane can be regarded as the thickness of the support membrane. In other words, the thickness of the composite semipermeable membrane can be measured by a digital thickness gauge and regarded as the thickness of the support membrane. In addition, the thickness of the porous support layer can be calculated simply by subtracting the thickness of the substrate from the thickness of the composite semipermeable membrane. As the digital thickness gauge, for example, PEACOCK from Ozaki Seisakusho Co., Ltd. can be used. When using a digital thickness gauge, the thickness is measured at 20 different points and the average value is calculated. In addition, when it is difficult to measure the thickness of the substrate and the thickness of the composite semipermeable membrane using a thickness gauge, they may be measured using a scanning electron microscope. In this case, the thickness is measured from an electron microscope photograph of a cross section observed at any five points for one sample, and the thickness is calculated by averaging the measured thickness.
[0030] (1-2) Separation functional layer Among the components of the composite semipermeable membrane, the one that has substantial solute separation performance is the separation functional layer 4. As shown in FIG.
[0031] The separation functional layer contains a semi-aromatic crosslinked polyamide obtained by interfacial polycondensation of a polyfunctional aliphatic amine and a polyfunctional aromatic acid halide. The ratio of the semi-aromatic crosslinked polyamide to the components of the separation functional layer is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and is particularly preferably composed of only semi-aromatic crosslinked polyamide. When the separation functional layer contains 50% by mass or more of semi-aromatic crosslinked polyamide, excessive densification due to π-π interactions derived from aromatic rings in the polyamide is suppressed, and excellent monovalent ion permeability is easily obtained. Here, "crosslinked polyamide" means a compound having three or more amide bonds and a branched structure, with a molecular weight of 400 or more.
[0032] The polyfunctional aliphatic amine is preferably an alicyclic diamine, such as a bipiperidine derivative or a piperazine derivative.
[0033] The molecular weight of the alicyclic diamine is preferably 90 or more and 160 or less. The molecular weight of the alicyclic diamine is preferably 90 or more, more preferably 100 or more, and even more preferably 110 or more. When the molecular weight of the alicyclic diamine is 90 or more, the diffusion coefficient of the amine becomes small, and polyamide is gradually formed during interfacial polycondensation, so that pores that inhibit the permeation of polyvalent ions while suppressing the permeation resistance of monovalent ions can be formed. The molecular weight of the alicyclic diamine is preferably 160 or less, more preferably 150 or less. Usually, at the beginning of polycondensation, an excess of oligomers is generated on the first surface side in contact with the organic layer, and the pores on the first surface side are blocked, so that the pore size distribution in the film thickness direction is likely to become non-uniform. By making the molecular weight of the alicyclic diamine 160 or less, the molecular weight of the generated oligomers can be reduced, and the interaction with the semi-aromatic crosslinked polyamide can be reduced, so that the oligomers can be easily removed in the draining process and the post-treatment process immediately after the film is formed under high humidity conditions, which will be described later. By making the molecular weight of the oligomer small, the pore size in the film thickness direction is uniform, that is, the average pore size R1 and the average pore size R2 of the separation functional layer described later satisfy 0.90≦R1 / R2≦1.10, and a membrane with high monovalent ion permeability can be obtained.
[0034] Examples of alicyclic diamines having a molecular weight of 90 or more and 160 or less include substituted piperazines in which the piperazine ring is substituted with an alkyl group having 1 to 3 carbon atoms (e.g., 2-methylpiperazine, 2-ethylpiperazine, 2-normal propylpiperazine, 2,2-dimethylpiperazine, 2,2-diethylpiperazine, 2,3-dimethylpiperazine, 2,3-diethylpiperazine, 2,5-dimethylpiperazine, 2,5-diethylpiperazine, 2,6-dimethylpiperazine, 2,6-diethylpiperazine, 2,3,5,6-tetramethylpiperazine, etc.) and homopiperazine.
[0035] The term "polyfunctional aromatic acid halide" refers to an aromatic acid halide having two or more halogenated carbonyl groups in one molecule, and is not particularly limited as long as it gives a semi-aromatic crosslinked polyamide by reaction with the polyfunctional aliphatic amine. Examples of polyfunctional aromatic acid halides include halides of 1,3,5-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,3-benzenedicarboxylic acid, 1,4-benzenedicarboxylic acid, 1,3,5-benzenetrisulfonic acid, and 1,3,6-naphthalenetrisulfonic acid. Among polyfunctional aromatic acid halides, acid chlorides are preferred, and in particular, from the standpoints of economy, ease of availability, ease of handling, ease of reactivity, and the like, trimesoyl chloride (hereinafter, "TMC"), which is an acid halide of 1,3,5-benzenetricarboxylic acid, isophthaloyl chloride, which is an acid halide of 1,3-benzenedicarboxylic acid, terephthaloyl chloride, which is an acid halide of 1,4-benzenedicarboxylic acid, 1,3,5-benzenetrisulfonic acid chloride, which is an acid halide of 1,3,5-benzenetrisulfonic acid, and 1,3,6-naphthalenetrisulfonic acid chloride, which is an acid halide of 1,3,6-naphthalenetrisulfonic acid, are preferred. The polyfunctional aromatic acid halide may be used alone or in a mixture of two or more kinds, but by mixing the trifunctional TMC, 1,3,5-benzenetrisulfonic acid chloride, or 1,3,6-naphthalenetrisulfonic acid chloride with either one of the difunctional isophthalic acid chloride or terephthalic acid chloride, the molecular gap of the polyamide crosslinked structure is enlarged, and a membrane with a uniform pore size distribution can be controlled over a wide range. The molar ratio of the trifunctional acid chloride to the difunctional acid chloride is preferably 1:20 to 50:1, more preferably 1:1 to 20:1.
[0036] The thickness of the separation functional layer is preferably 15 nm or more and 50 nm or less, and more preferably 20 nm or more and 40 nm or less. When the thickness of the separation functional layer is 15 nm or more, a composite semipermeable membrane with sufficient water permeability can be easily obtained, and when the thickness of the separation functional layer is 20 nm or more, a composite semipermeable membrane with sufficient water permeability can be stably obtained without causing a decrease in removability due to the occurrence of defects. On the other hand, the thickness of the separation functional layer is preferably 50 nm or less, more preferably 40 nm or less. When the thickness of the separation functional layer is 50 nm or less, stable membrane performance can be obtained, and when the thickness of the separation functional layer is 40 nm or less, even more sufficient water permeability can be obtained. The thickness of the separation functional layer can be analyzed using observation techniques such as transmission electron microscopy, TEM tomography, and focused ion beam / scanning electron microscopy (FIB / SEM).
[0037] As a result of extensive investigations, the present inventors have found that a composite semipermeable membrane satisfying the following requirements exhibits excellent monovalent ion / multivalent ion selective separation performance under acidic conditions. A composite semipermeable membrane according to this embodiment, in which a positron beam is irradiated from the first surface side of the composite semipermeable membrane, and the average pore size R1 and the average pore size R2 of the separation functional layer derived by a positron annihilation lifetime measurement method are 0.30 nm or more and 2.00 nm or less, and satisfy 0.90≦R1 / R2≦1.10. Here, R1 and R2 are defined as follows: R1: Average hole diameter at positron beam intensity of 0.1 keV R2: Average hole diameter at positron beam intensity of 0.5 keV
[0038] The "positron annihilation lifetime measurement method" is a technique that measures the time (on the order of hundreds of picoseconds to tens of nanoseconds) between when a positron enters a sample and when it annihilates, and non-destructively evaluates information such as the size, number density, and size distribution of 0.1 to 10 nm voids based on the annihilation lifetime.
[0039] The measurement area in the depth direction from the sample surface can be adjusted by the energy amount of the positron beam incident on the sample. The higher the energy, the deeper the measurement area from the sample surface, but the depth depends on the density of the sample. For example, when measuring the separation functional layer of a composite semipermeable membrane, if a positron beam with an energy of about 0.1 keV is irradiated from the first surface side of the composite semipermeable membrane, a region with a depth of 0 to 5 nm from the sample surface is usually measured, and if a positron beam with an energy of about 0.5 keV is irradiated, a region with a depth of 0 to 50 nm from the sample surface is usually measured. In this embodiment, if another layer such as a protective layer is provided on the separation functional layer, the other layer such as the protective layer can be removed in advance to measure the average pore size R1 and the average pore size R2 of the separation functional layer.
[0040] As described above, a weaker positron beam intensity reflects the hole diameter on the first surface side, and a stronger positron beam intensity reflects the hole diameter on the second surface side, and the closer R1 / R2 is to 1, the more uniform the hole diameter is in the film thickness direction. In this embodiment, by satisfying 0.90≦R1 / R2≦1.10, excellent monovalent ion / multivalent ion selective separation performance can be realized. Although the details of the above mechanism are not fully understood, it is speculated that the uniformity of the pore size in the film thickness direction makes the direction of ion diffusion in the separation functional layer uniform, and suppresses the permeation resistance of monovalent ions, which are large enough to move freely in the separation functional layer. As a result, it is believed that excellent monovalent ion / multivalent ion selective separation performance is realized. Therefore, it is more preferable that the average pore sizes R1 and R2 of the separation functional layer satisfy 0.95≦R1 / R2≦1.05, and even more preferable that they satisfy 0.97≦R1 / R2≦1.03.
[0041] In the composite semipermeable membrane according to this embodiment, the average pore diameters R1 and R2 of the separation functional layer are 0.30 nm or more and 2.00 nm or less. When the average pore diameters R1 and R2 are within the above range, the function as a substantial nanofiltration membrane is exhibited. Preferably, R1 is 0.55 nm or more and 1.00 nm or less, more preferably 0.55 nm or more and 0.80 nm or less, still more preferably 0.55 nm or more and 0.70 nm or less, even more preferably 0.57 nm or more and 0.68 nm or less, and particularly preferably 0.60 nm or more and 0.65 nm or less. When R1 is within the above range, the effect of suppressing the permeation resistance of monovalent ions and inhibiting the permeation of polyvalent ions becomes remarkable. Also, from the viewpoint of exhibiting the function as a nanofiltration membrane, preferably, R2 is 0.50 nm or more and 1.10 nm or less, more preferably 0.50 nm or more and 0.80 nm or less, still more preferably 0.50 nm or more and 0.77 nm or less, even more preferably 0.55 nm or more and 0.70 nm or less, and particularly preferably 0.60 nm or more and 0.65 nm or less.
[0042] The average pore diameters R1 and R2 can be controlled, for example, by performing interfacial polycondensation under high humidity conditions, the molecular weight of the polyfunctional aliphatic amine used in the interfacial polycondensation, the temperature at which the organic solvent solution containing the polyfunctional aromatic acid halide is applied during the interfacial polycondensation, and the like. Specifically, when the polyfunctional aliphatic amine is an alicyclic diamine having a molecular weight of 90 or more and 160 or less, it becomes easy to remove oligomers in the liquid draining step and the post-treatment step immediately after film formation under high humidity conditions described later, and R1 / R2 can be controlled within a particularly preferable range.
[0043] In the cross-section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane according to this embodiment, the total number P1 of pores having a pore diameter of 0.30 nm or more and 1.20 nm or less, the total number P2 of pores having a pore diameter of 0.50 nm or more and less than 0.80 nm, the total number P3 of pores having a pore diameter of 0.80 nm or more and 1.20 nm or less, and the total number P4 of pores having a pore diameter exceeding 1.20 nm preferably satisfy 0.20 < P2 / P1 < 0.40, P3 / P2 < 0.20, and P4 / P1 ≤ 0.01.
[0044] Here, pores with a pore diameter of 0.30 nm or more and less than 0.50 nm are pores through which only water passes, pores with a pore diameter of 0.50 nm or more and 0.80 nm or less are effective pores through which only water and monovalent ions pass, pores with a pore diameter of 0.80 nm or more and 1.20 nm or less are large pores through which water, monovalent ions, and polyvalent ions pass, and pores with a pore diameter exceeding 1.20 nm are large pores through which polyvalent ions pass. That is, P2 / P1 means the ratio of effective pores through which only water and monovalent ions pass to the total number of pores with a pore diameter of 0.30 nm or more and 1.20 nm or less, P3 / P2 means the ratio of large pores through which polyvalent ions and water pass to the effective pores through which only water and monovalent ions pass, and P4 / P1 means the ratio of large pores through which polyvalent ions are more likely to permeate to the total number of pores with a pore diameter of 0.30 nm or more and 1.20 nm or less.
[0045] In the case of a composite semipermeable membrane that satisfies 0.20 < P2 / P1 < 0.40 and P3 / P2 < 0.20 in the cross-section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane, the abundance ratio of effective pores through which only water and monovalent ions pass with a pore diameter of 0.50 nm or more and 0.80 nm or less is high with respect to pores through which only water with a pore diameter of 0.30 nm or more and less than 0.50 nm passes and large pores through which polyvalent ions and water with a pore diameter of 0.80 nm or more and 1.20 nm or less pass. While suppressing the permeation resistance of monovalent ions, the effect of inhibiting the permeation of polyvalent ions becomes remarkable, and excellent monovalent ion / polyvalent ion selective separation performance can be obtained under acidic conditions. It is more preferable that P1 and P2 satisfy 0.26 ≦ P2 / P1 ≦ 0.35, and it is even more preferable that they satisfy 0.31 ≦ P2 / P1 ≦ 0.35. When P1 and P2 satisfy the above range, excellent permeability of monovalent ions is likely to be exhibited. Also, it is preferable that P2 and P3 satisfy P3 / P2 ≦ 0.12, more preferably P3 / P2 ≦ 0.09, and even more preferably P3 / P2 ≦ 0.05. When P2 and P3 satisfy the above range, the effect of inhibiting the permeation of polyvalent ions becomes more remarkable.
[0046] Furthermore, when P4 / P1≦0.01, better selective separation of monovalent ions / multivalent ions is achieved. When P4 / P1>0.01, a large number of coarse pores through which multivalent ions can easily pass are present, and the selective separation of monovalent ions / multivalent ions is reduced. Therefore, P4 / P1 is more preferably P4 / P1≦0.007, even more preferably P4 / P1≦0.005, and it is particularly preferable that P4 does not exist.
[0047] P1, P2, P3 and P4 can be controlled, for example, by the molecular weight of the polyfunctional aliphatic amine used in the interfacial polycondensation, the temperature at which the organic solvent solution containing the polyfunctional aromatic acid halide is applied during the interfacial polycondensation, hydrophilic solvent treatment, etc. More specifically, when the polyfunctional aliphatic amine is an alicyclic diamine having a molecular weight of 100 to 160, oligomers can be easily removed in the draining step and post-treatment step immediately after film formation under high humidity conditions described below, and P2 / P1 can be controlled within a particularly preferred range.
[0048] As shown in Figure 3, in a cross section perpendicular to the surface of the composite semipermeable membrane (cross section perpendicular to the first surface), when the separation functional layer is divided into five equally spaced regions a to e from the first surface side to the second surface side, it is preferable that the amino group density Nb in region b and the amino group density Nd in region d satisfy Nb / Nd ≦ 0.80.
[0049] The separation functional layer, which is mainly composed of semi-aromatic crosslinked polyamide formed by interfacial polycondensation, has amino and carboxyl groups as terminal functional groups. In particular, a separation functional layer with a high amino group density has a sparse structure under acidic conditions, and while the permeability of monovalent ions is increased, the blocking ability of large-sized polyvalent ions is decreased. In addition, a separation functional layer with a low amino group density has a dense structure under acidic conditions, and while the permeability of monovalent ions is decreased, the blocking ability of polyvalent ions is increased. Thus, there is a trade-off between the permeability of monovalent ions and the blocking ability of polyvalent ions, and by forming a separation functional layer in which the amino group density is uniformly distributed, a well-balanced performance of the permeability of monovalent ions and the blocking ability of polyvalent ions can be obtained.
[0050] In the separation functional layer in the composite semipermeable membrane according to this embodiment, when the amino group density Nb in region b and the amino group density Nd in region d satisfy Nb / Nd≦0.80, that is, when the separation functional layer contains a semi-aromatic crosslinked polyamide having the above-mentioned density difference in the amino group density in the thickness direction of the separation functional layer, a composite semipermeable membrane having better monovalent ion permeability and polyvalent ion blocking performance can be obtained. From the viewpoint of achieving both monovalent ion permeability and polyvalent ion blocking performance, it is more preferable that the amino group density Nb and the amino group density Nd satisfy Nb / Nd≦0.70, more preferably that they satisfy Nb / Nd≦0.65, and particularly preferably that they satisfy Nb / Nd≦0.60. In addition, from the viewpoint of suppressing the change in polyamide structure due to excessive density difference of amino groups and the significant performance fluctuations associated therewith, it is preferable that the amino group density Nb and the amino group density Nd satisfy Nb / Nd≧0.10. In order to control the amino group distribution within the above range, the atmospheric humidity must be controlled to 80% or more, more preferably 90% or more, and even more preferably 95% or more. This is because the evaporation of water from the polyamide formed can be suppressed, and the insolubilization of excess oligomers with many amino groups due to intermolecular hydrogen bonds can be suppressed, allowing the oligomers to be efficiently removed in the draining step and solvent treatment step. In addition, the terminal amino group density on the first surface side can be reduced compared to the amino group density on the second surface side by a method of forming a separation functional layer by applying an aqueous solution containing a polyfunctional aliphatic amine to the surface of a porous support layer.
[0051] In addition, in the separation functional layer of the composite semipermeable membrane according to this embodiment, the amino group density Nb in the region b is 1.0 × 10 -23 mol / nm 2 It is preferable that Nb is 1.0×10 or less. -23 mol / nm 2 By keeping the content below 0.9×10, excellent monovalent ion permeability can be achieved. -23 mol / nm 2 More preferably, it is 0.8×10 or less. -23 mol / nm 2From the viewpoint of suppressing the decrease in water permeability due to the hydrophobization of the polyamide forming the separation functional layer, Nb is more preferably 0.1×10 -23 mol / nm 2 It is preferable that the amino group density Nb is equal to or higher than the above. The amino group density Nb can be controlled to be low by increasing the concentration of the polyfunctional acid halide during the interfacial polymerization. However, if the monomer balance during the interfacial polymerization is disturbed by increasing the concentration of the polyfunctional acid halide, the degree of polymerization does not increase, so that many coarse holes are easily formed, and the removal of multivalent ions is reduced. In addition, although the amino group density Nb can be reduced by reacting the amino group on the first surface side of the separation functional layer with an acid anhydride after the interfacial polymerization, this is not preferable because it leads to a decrease in the permeability and water permeability of monovalent ions. Therefore, in order to control the amino group distribution Nb within the above range, as described above, the atmospheric humidity needs to be controlled to 80% or more, more preferably 90% or more, and even more preferably 95% or more. In addition, the amino group distribution Nb can be further reduced by simultaneously carrying out a treatment process with a hydrophilic solvent described later.
[0052] The separation functional layer is divided into five equal-spaced regions a to e, which are determined by the following method. The composite semipermeable membrane is immersed in a tungstic acid aqueous solution multiple times. A cross section of the separation functional layer perpendicular to the thickness direction of the separation functional layer in this composite semipermeable membrane is photographed at a magnification of 100,000 using a field emission scanning transmission electron microscope (hereinafter referred to as "STEM"). In the obtained image, as shown in Figure 3, a reference point P is set at an arbitrary position on the outer surface of the separation functional layer (the surface opposite to the surface on the porous support layer side), and straight lines Y1 and Y2 parallel to the normal line are drawn at an arbitrary interval of 3 to 10 nm on both sides of the direction perpendicular to the normal line Y0, centered on the normal line Y0 passing through the reference point P. Also, draw a tangent line X1 to the outer surface of the separation functional layer that passes through reference point P, and a tangent line X2 to the inner surface (the surface on the porous support layer side) of the separation functional layer that is parallel to the tangent line X1. Draw four straight lines that divide the area between X1 and X2 into five equal parts. The areas surrounded by Y1 and Y2, and also surrounded by X1, X2 and the four straight lines between them, are designated as areas a to e, in order from the outer surface of the separation functional layer. If the separation functional layer forms multiple pleated structures, a cross-sectional image is taken using the same method as above, and among the pleated structures in the obtained image, the pleat with the highest pleat height is used as a reference, and Y1 and Y2 are drawn using the same procedure in any area that is within 50 to 100% of the height from the surface on the second side of the separation functional layer (the surface of the support film) to the apex of the convex portion. Next, regions a to e are determined using the same procedure as above. The area of each of regions a to e is 5 nm 2 More than 30nm 2 The following applies.
[0053] The amino group density in each of the regions a to e obtained by dividing the separation functional layer into five equal intervals is determined by the following method. The brightness is measured by STEM for each of the regions enclosed by the above-mentioned X1, X2 or the four straight lines between them, and Y1 and Y2 (each region consisting of regions a to e). The minimum brightness Lmin and maximum brightness Lmax are obtained for each region. The area of the parts showing a brightness of {Lmin+(Lmax-Lmin) / 3} or more for the obtained minimum brightness Lmin and maximum brightness Lmax is integrated for each region. This integral value is the area (nm 2 The integral obtained corresponds to the area per amino group molecule (0.04 nm 2 ), Avogadro's constant (6.0×10 23 The amino group density (mol / nm 2 The average of the amino group densities obtained for five randomly selected regions of the pleated structure is taken as the amino group density of each region.
[0054] In the composite semipermeable membrane according to the present embodiment, the monovalent ion removal rate is preferably 75% or less, more preferably 60% or less, and even more preferably 50% or less. When the monovalent ion removal rate is within the above range, the monovalent ion concentration in the permeate is increased, and the monovalent ion concentration step in the monovalent ion purification process can be made more efficient or omitted, contributing to shortening the purification time and reducing the purification cost. The multivalent ion removal rate is preferably 99.4% or more, more preferably 99.6% or more, and even more preferably 99.8% or more. When the multivalent ion removal rate is within the above range, the multivalent ion concentration in the permeate is reduced, and the monovalent ion purification step can be made more efficient or omitted. In addition, the multivalent ion concentration in the non-permeate is increased, so that the multivalent ions can be efficiently purified.
[0055] The "selectivity of monovalent ions / multivalent ions" below means a value calculated by the following formula from the monovalent ion removal rate and multivalent ion removal rate calculated based on the ion concentrations contained in the permeate obtained when an aqueous solution containing monovalent ions and multivalent ions is used as feed water and a membrane filtration process is performed with a separation membrane. In this specification, the ions used in the calculation of the selectivity of monovalent ions / multivalent ions mean cations. Selectivity for monovalent ions / multivalent ions = (100-monovalent ion removal rate) / (100-multivalent ion removal rate)
[0056] The selectivity of monovalent ions / polyvalent ions is preferably at least 70, more preferably at least 80, and even more preferably at least 100. When the selectivity of monovalent ions / polyvalent ions is within the above range, the purification efficiency of both monovalent and polyvalent ions is improved, which contributes to shortening the purification time and reducing the purification cost.
[0057] The separation functional layer of the composite semipermeable membrane according to this embodiment preferably has a hollow pleated structure. When the separation functional layer of the composite semipermeable membrane has a hollow pleated structure, the number of apparent holes per unit membrane area increases. As a result, the pressure required for treating a solution with the composite semipermeable membrane can be reduced, and the exhaust heat and electricity of the operating device can be reduced.
[0058] The pleated structure of the separation functional layer is determined by measuring the pleat height 201 and the separation functional layer thickness 202 for the separation functional layer 4 on the porous support layer 3 shown in Figure 4 in an image obtained by observing a cross section of the separation functional layer perpendicular to the composite semipermeable membrane surface with a transmission electron microscope (TEM), and determining the ratio of the pleat height to the separation functional layer thickness (pleat height / separation functional layer thickness). If the pleat height of the separation functional layer / the separation functional layer thickness is 1.2 or more, the separation functional layer is deemed to have a pleated structure, and if it is less than 1.2, the separation functional layer is deemed to have no pleats.
[0059] "Thickness of the separation functional layer" refers to the length of the shortest line segment connecting two points on the supply water side and the permeate water side of the separation functional layer in the cross-sectional image of the separation functional layer, and corresponds to the length shown as thickness 202 of the separation functional layer in Figure 4. The measurement point on the supply water side is determined by dividing the cross-sectional image of the separation functional layer into 10 sections, and the measurement point is determined to be the point in each section that is the furthest from the support membrane. When the separation functional layer forms a pleated structure and the pleated structure is formed across the above sections, the measurement point is determined to be the section that is the furthest from the support membrane.
[0060] "Pleated height" is the length of a line segment connecting two points where a perpendicular line drawn from a point on the feed water side to the support membrane surface when the thickness of the separation functional layer is measured and the perpendicular line intersects with the support membrane surface, and corresponds to the length shown as pleated height 201 in Figure 4. The pleated height is determined by measuring 100 randomly selected pleats in an image of a cross section of the separation functional layer perpendicular to the composite semipermeable membrane surface observed with a transmission electron microscope (TEM), and calculating the average value.
[0061] From the viewpoint of water permeability, the pleat height is preferably 20 nm to 500 nm, more preferably 50 nm to 300 nm. By making it 20 nm or more, the specific surface area of the separation functional layer can be sufficiently increased, and high water permeability can be obtained at low pressure. In addition, by making it 500 nm or less, clogging of the water flow path due to overlapping of adjacent pleats and concentration polarization on the membrane surface can be suppressed, so that high water permeability can be obtained at low pressure. The height of the pleats can be controlled by the fat solubility and molecular weight of the polyfunctional amine and the temperature during interfacial polymerization.
[0062] In order to form a separation functional layer having a hollow pleated structure, the logP of the polyfunctional aliphatic amine used in the interfacial polycondensation is preferably −0.5 or more and 2.0 or less, and more preferably −0.5 or more and 1.5 or less.
[0063] The term "logP" refers to a value calculated based on the octanol-water partition coefficient of a compound from the octanol-water partition coefficients of each functional group contained in the compound, based on Non-Patent Document 1, and in the present specification, the value is calculated using ChemDraw, which is a structural formula drawing software.
[0064] It has long been known that the interfacial polymerization of polyamide proceeds by the distribution and diffusion of amines into an organic phase and reaction with polyfunctional acid halides in the organic phase (Non-Patent Document 2). When logP is between -0.5 and 2.0, the distribution and diffusion of polyfunctional aliphatic amines into an organic solvent during interfacial polycondensation is optimized, making it easier to form a separation functional layer having a hollow pleated structure.
[0065] Examples of polyfunctional aliphatic amines having a logP of -0.5 or more and 2.0 or less include substituted piperazines in which the piperazine ring is substituted with an alkyl group having a total of 1 to 4 carbon atoms (e.g., 2-methylpiperazine, 2-ethylpiperazine, 2-normal propylpiperazine, 2,2-dimethylpiperazine, 2,2-diethylpiperazine, 2,3-dimethylpiperazine, 2,3-diethylpiperazine, 2,5-dimethylpiperazine, 2,5-diethylpiperazine, 2,6-dimethylpiperazine, 2, 6-diethylpiperazine, 2-ethyl-3-methylpiperazine, 2-ethyl-5-methylpiperazine, 2-ethyl-6-methylpiperazine, 2-methyl-3-propylpiperazine, 2-methyl-5-propylpiperazine, 2-methyl-6-propylpiperazine, 2,5-diethylpiperazine, 2,3,5,6-tetramethylpiperazine, etc.), bipiperidine derivatives (e.g., 2,2'-bipiperidine, 3,3'-bipiperidine, 4,4'-bipiperidine, etc.), etc.
[0066] The composite semipermeable membrane according to the present embodiment is suitable for separating nonionic solutes in addition to ionic solutes such as lithium, and is characterized by the ratio of permeability of each solute. For example, examples of nonionic solutes include glucose and sucrose. When the glucose permeability when a 1000 ppm glucose aqueous solution at 25°C and pH 6.5 is permeated at an operating pressure of 0.5 MPa is B, and the sucrose permeability when a 1000 ppm sucrose aqueous solution at 25°C and pH 6.5 is permeated at an operating pressure of 0.5 MPa is C, B / C is preferably 10 or more, more preferably 30 or more, and even more preferably 50 or more. The upper limit of B / C is not particularly limited, but is, for example, 1000 or less. Here, the permeability of each solute is expressed as 100 x (solute concentration in permeated water / solute concentration in feed water). A high B / C contributes to, for example, shortening the separation and purification time of monosaccharides and polysaccharides in sugar purification, and reducing the cost of purification.
[0067] 2. Manufacturing method of composite semipermeable membrane Next, a method for producing the composite semipermeable membrane will be described. The method for producing the composite semipermeable membrane includes a step of forming a support membrane and a step of forming a separation functional layer.
[0068] (2-1) Support membrane formation process The step of forming a support membrane can also be referred to as a step of forming a porous support layer. This step includes, for example, a step of applying a polymer solution to a substrate and a step of immersing the substrate to which the polymer solution has been applied in a coagulation bath to coagulate the polymer.
[0069] In the step of applying the polymer solution to the substrate, the polymer solution is prepared, for example, by dissolving a polymer, which is a component of the porous support layer, in a good solvent for the polymer. When polysulfone is used as the polymer, the temperature of the polymer solution during application is preferably 10°C or higher and 60°C or lower. If the temperature of the polymer solution is within this range, the polymer does not precipitate, and the polymer solution is sufficiently impregnated into the spaces between the fibers of the substrate and then solidified. As a result, a porous support layer that is firmly bonded to the substrate due to the anchor effect can be obtained. The preferred temperature range of the polymer solution can be appropriately adjusted depending on the type of polymer used, the desired solution viscosity, etc.
[0070] As a solvent for the polymer solution, N,N-dimethylformamide (hereinafter, "DMF") is preferable. After the polymer solution is applied onto the substrate, the time until the substrate is immersed in the coagulation bath is preferably 0.1 seconds or more and 5 seconds or less. If the time until the substrate is immersed in the coagulation bath is within this range, the polymer solution is sufficiently impregnated into the spaces between the fibers of the substrate and then solidified. The preferred range of the time until the substrate is immersed in the coagulation bath can be appropriately adjusted depending on the type of polymer solution used, the desired solution viscosity, and the like.
[0071] Water is usually used as the coagulation bath, but any solution that does not dissolve the polymer that is a component of the porous support layer is sufficient. The temperature of the coagulation bath is preferably -20°C or higher and 100°C or lower, and more preferably 10°C or higher and 50°C or lower. If the temperature of the coagulation bath is 100°C or lower, the vibration of the coagulation bath surface due to thermal motion can be suppressed, and the smoothness of the membrane surface after membrane formation can be maintained. Furthermore, if the temperature is -20°C or higher, the coagulation speed can be maintained, improving membrane formability.
[0072] Next, the support membrane thus obtained may be washed with hot water to remove the solvent remaining in the membrane. The temperature of the hot water at this time is preferably 40°C or more and 100°C or less, more preferably 60°C or more and 95°C or less. If the washing temperature is 100°C or less, the shrinkage of the support membrane does not become too large, and the decrease in water permeability can be suppressed. Also, if the washing temperature is 40°C or more, a high washing effect can be obtained.
[0073] (2-2) Formation process of separation functional layer Next, an example of a process for forming a separation functional layer constituting a composite semipermeable membrane will be described. In the process for forming a separation functional layer, an aqueous solution containing a polyfunctional aliphatic amine compound and an organic solvent solution containing a polyfunctional aromatic acid halide are used to form a semi-aromatic crosslinked polyamide on the surface of a support membrane by interfacial polycondensation. Specifically, the step of forming the separation functional layer includes: (a) coating the surface of the porous support layer with an aqueous solution of a polyfunctional aliphatic amine; (b) After the step (a), the method further includes a step of contacting the polyfunctional aromatic acid halide-containing solution at a temperature of 10° C. or higher and 38° C. or lower.
[0074] In the aqueous solution containing the polyfunctional aliphatic amine compound, the concentration of the polyfunctional aliphatic amine is preferably 0.1% by mass or more and 10% by mass or less.
[0075] The aqueous solution containing the polyfunctional aliphatic amine may contain alcohols. Examples of the alcohols include ethanol, 1-propanol, 2-propanol, butanol, etc. By containing alcohols in the aqueous solution containing the polyfunctional aliphatic amine, the same effect as that of the above-mentioned surfactant can be obtained.
[0076] The aqueous solution containing the polyfunctional aliphatic amine may contain an alkaline compound. Examples of the alkaline compound include sodium hydroxide, trisodium phosphate, and triethylamine. By containing the alkaline compound, hydrogen halide generated in the interfacial polycondensation reaction is removed, and the reactivity of the polyfunctional aliphatic amine is prevented from decreasing, so that the polyamidation reaction is promoted, and the selective separation property and durability against acid and alkali are improved.
[0077] The solvent in the polyfunctional aromatic acid halide-containing solution is an organic solvent. The organic solvent is immiscible with water, does not destroy the support film, does not inhibit the reaction for producing the semi-aromatic crosslinked polyamide, and has a solubility parameter (hereinafter, "SP value") of 15.2 (MPa). 1 / 2 It is preferable to use an organic solvent having a logP of 3.2 or more and an SP value of 15.2 (MPa). 1 / 2 With this and logP being 3.2 or more, the distribution and diffusion of the polyfunctional aliphatic amine during interfacial polycondensation are optimized, and the amount of functional groups can be increased.
[0078] SP value is 15.2 (MPa) 1 / 2 As organic solvents having a pH of 10 or more and a logP of 3.2 or more, for example, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, heptadecane, hexadecane, cyclooctane, ethylcyclohexane, 1-octene, 1-decene, etc., alone or in mixtures thereof, are preferably used.
[0079] The aqueous solution containing the polyfunctional aliphatic amine compound may contain a surfactant. Examples of the surfactant include sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, sodium dodecyldiphenyletherdisulfonate, styrenebis(sodiumnaphthalenesulfonate), sodium polyoxyethylene alkylethersulfate, etc. By containing a surfactant, the surface of the porous support layer can be uniformly coated with the aqueous solution, so that the separation functional layer is formed uniformly, and the effect of stabilizing the membrane performance and the effect of increasing the adhesion between the separation functional layer and the porous support layer can be obtained.
[0080] The aqueous solution containing a polyfunctional aliphatic amine compound and the organic solvent solution containing a polyfunctional aromatic acid halide may each contain compounds such as an acylation catalyst, a polar solvent, an acid scavenger, and an antioxidant, as necessary.
[0081] In order to carry out the interfacial polycondensation of the polyfunctional aliphatic amine and the polyfunctional aromatic acid halide on the porous support layer, the surface of the porous support layer is first coated with an aqueous solution containing the polyfunctional aliphatic amine to form a coating layer. The method of coating the surface of the porous support layer with the aqueous solution containing the polyfunctional aliphatic amine may be any method that allows the surface of the porous support layer to be uniformly and continuously coated with the aqueous solution, and may include, for example, a method of applying the aqueous solution to the surface of the porous support layer, a method of immersing the support film in the aqueous solution, etc. Among them, the method of applying the aqueous solution to the surface of the porous support layer is preferred. By applying an aqueous solution containing a polyfunctional aliphatic amine to the surface of the porous support layer, the amount of water contained in the porous support layer is reduced compared to the immersion method, i.e., the amount of amine contained in the support membrane is reduced. As a result, excessive supply of amine to the reaction site can be suppressed in the early stages of interfacial polycondensation after application of the polyfunctional aromatic acid halide, which contributes to the formation of pores that inhibit the permeation of polyvalent ions while suppressing the permeation resistance of monovalent ions, and at the same time, the density of terminal amino groups on the first surface side of the formed separation functional layer can be reduced compared to the density of amino groups on the second surface side.
[0082] Next, it is preferable to remove the excess aqueous solution applied by a draining process. For example, the method of draining the aqueous solution may be a method of holding the membrane surface vertically and allowing the aqueous solution to flow down naturally. After draining the aqueous solution, the membrane surface may be dried to remove all or part of the water in the aqueous solution on the membrane surface.
[0083] Thereafter, the organic solvent solution containing the polyfunctional aromatic acid halide is applied to the porous support layer containing the aqueous solution containing the polyfunctional aliphatic amine. The application temperature is preferably 10°C or higher and 38°C or lower, more preferably 20°C or higher and 35°C or lower. When the application temperature is 10°C or higher, the diffusion speed of the amine into the organic solvent is sufficient, and it is easy to form a polyamide with a pore size required for selective removal of multivalent ions. In addition, when the temperature during application is 38°C or lower, the inhibition of diffusion due to the improvement of the reaction rate is suppressed, so that the pore structure becomes uniform and the selective separation property is improved.
[0084] When trimesoyl chloride is contained as the polyfunctional aromatic acid halide, the concentration of trimesoyl chloride in the organic solvent solution is preferably 0.05% by mass or more and 0.7% by mass or less, more preferably 0.08% by mass or more and 0.3% by mass or less. If the concentration of trimesoyl chloride is within this range, sufficient water permeability, selective separation performance, and durability against acid can be obtained. When other trifunctional acid chlorides or difunctional acid chlorides are used, the molar concentration of the acid chloride is adjusted to be approximately the same as that of the above-mentioned trimesoyl chloride in terms of the molecular weight ratio.
[0085] In this way, the polyfunctional aliphatic amine and the polyfunctional aromatic acid halide are brought into contact with each other to cause interfacial polycondensation. The interfacial polycondensation is preferably carried out under a temperature condition of 10° C. or higher, more preferably under a temperature condition of 80° C. or higher, and even more preferably above the melting point of the polyfunctional aliphatic amine. The interfacial polycondensation is preferably carried out under a temperature condition of 120° C. or lower. By carrying out the interfacial polycondensation at 10° C. or higher, the decrease in the mobility of the oligomer can be suppressed in the interfacial polycondensation reaction, the polyfunctional aliphatic amine can maintain high mobility in the reaction system, an efficient crosslinking reaction can proceed, and excellent selective removal of polyvalent ions can be achieved. In addition, by carrying out the interfacial polycondensation at 120° C. or lower, the porous support layer can be prevented from being overdried, and practical water permeability can be ensured.
[0086] As a result of intensive research, the present inventors have found that the composite semipermeable membrane according to the present embodiment is easily obtained by controlling the atmospheric humidity (relative humidity) during the interfacial polycondensation to 80% or more. By setting the atmospheric humidity during the interfacial polycondensation to 80% or more, the evaporation of water from the polyamide formed can be suppressed, and the insolubilization of oligomers with many amino groups generated in excess due to intermolecular hydrogen bonds can be suppressed. As a result, the oligomers can be efficiently removed in the draining step and solvent treatment step described below, so that the pore size expansion associated with the swelling of the semi-aromatic crosslinked polyamide during membrane operation under acidic conditions can be suppressed, the amino group density on the first surface side of the separation functional layer is reduced, and the gradient of the amino group density in the membrane thickness direction becomes large, and the swelling of the polyamide on the first surface side that comes into contact with a high concentration of acid during membrane operation under acidic conditions and the associated excessive pore size expansion can be suppressed, and it is considered that excellent monovalent ion permeability and excellent polyvalent ion removal properties can be achieved at the same time. Therefore, it is preferable that the atmospheric humidity during the interfacial polycondensation is 80% or more, more preferably 90% or more, and even more preferably 95% or more. The atmospheric humidity can be adjusted by using a precision air conditioner.
[0087] The time for carrying out the interfacial polycondensation is preferably from 0.1 seconds to 3 minutes, and more preferably from 1 second to 1 minute.
[0088] Next, it is preferable to remove the organic solvent solution after the reaction by a draining step. For example, the organic solvent can be removed by a method of holding the membrane vertically and removing the excess organic solvent by gravity flow, a method of drying the organic solvent by blowing air with a blower, or a method of removing the excess organic solvent with a mixed fluid of water and air. Among them, the method of removing the organic solvent with a mixed fluid of water and air is particularly preferable. When a mixture of water and air is used, the water contained in the separation functional layer causes it to swell and increase its water permeability. In the case of gravity flow, the vertical holding time is preferably between 1 minute and 5 minutes, and more preferably between 1 minute and 3 minutes. Holding for 1 minute or more makes it easier to obtain a separation functional layer having the desired function, while holding for 5 minutes or less can prevent defects caused by over-drying of the organic solvent, thereby preventing performance degradation.
[0089] The composite semipermeable membrane obtained by the above-mentioned method can be further treated with a hydrophilic solvent at 25°C to 90°C for 1 minute or more to promote the removal of amide oligomers with many excess amino groups on the first surface side and to homogenize the pore size distribution in the thickness direction of the separation functional layer, thereby further improving the monovalent ion / multivalent ion selective separation property of the composite semipermeable membrane. Here, the "hydrophilic solvent" refers to a solvent that dissolves in water at 10% by mass or more, and may be used as an aqueous solution of 10% by mass or more. The solubility of the hydrophilic solvent in water is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable to use the hydrophilic solvent in bulk.
[0090] As the hydrophilic solvent, a solvent that does not damage the support membrane is suitable, and alcohols are particularly preferred. Examples of alcohols include monohydric alcohols such as methanol, ethanol, or 2-propanol, glycols such as ethylene glycol, 1,3-butylene glycol (1,3-butanediol), diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, or polybutylene glycol, glycerin, diglycerin derivatives, and glycerin fatty acid esters. Among them, from the viewpoint of being easily removed by washing with water and having a high effect of improving the selective separation of monovalent ions / polyvalent ions, it is preferable to use at least one alcohol selected from the group consisting of alcohols, glycols, and glycerin having a molecular weight of 500 or less as the hydrophilic solvent. In particular, from the viewpoint of removing excess oligomers and from the viewpoint of the effect of uniforming the pore size by reconstructing the polyamide structure, glycols having a molecular weight of 200 or less that have high permeability to polyamide are particularly preferred as the hydrophilic solvent.
[0091] 3. Composite semipermeable membrane element The composite semipermeable membrane element according to this embodiment is characterized by comprising the composite semipermeable membrane according to this embodiment. The composite semipermeable membrane element according to this embodiment exhibits excellent monovalent ion / polyvalent ion selective separation performance because it comprises the composite semipermeable membrane according to this embodiment. One embodiment of the configuration of the composite semipermeable membrane element according to this embodiment will be described with reference to FIG. 2.
[0092] In one embodiment of the composite semipermeable membrane element according to the present embodiment, as shown in Fig. 2, a composite semipermeable membrane element 100 includes a composite semipermeable membrane 1, a feed-side flow path material 11, a permeate-side flow path material 12, a water collection pipe 6, a first end plate 7, and a second end plate 8. The composite semipermeable membrane 1 is bonded together to form an envelope-shaped membrane 20. The envelope-shaped membrane 20 is spirally wound around the water collection pipe 6 to form a wound body 26. Other members such as a film and a filament may be wound around the outer periphery of the wound body 26 to protect the wound body 26.
[0093] The supply-side flow passage material 11 is disposed so as to face the supply side of the composite semipermeable membrane 1, and is wound around the water collection pipe 6 together with the composite semipermeable membrane 1. For example, a net is preferably used as the supply-side flow passage material 11. The permeate-side flow passage material 12 is disposed so as to face the permeate side of the composite semipermeable membrane 1, and is wound around the water collection pipe 6 together with the composite semipermeable membrane 1. For example, tricot or a protrusion-fixed sheet can be used as the permeate-side flow passage material 12. In addition, when protrusions (corresponding to the permeate-side flow passage material) are directly fixed to the surface of the composite semipermeable membrane on the substrate side, the permeate-side flow passage material 12 can be omitted. The water collection pipe 6 is a hollow cylindrical member and has a plurality of holes on the side. The first end plate 7 is a disk-shaped member having a plurality of supply ports. The first end plate 7 is disposed at the first end of the wound body 26. The second end plate 8 is a disk-shaped member having an outlet for concentrated water and an outlet for permeated water. The second end plate 8 is disposed at a second end of the wrap 26 .
[0094] Fluid separation by the composite semipermeable membrane element 100 will be described. Feed water 101 is supplied to the wound body 26 from a plurality of feed ports in the first end plate 7. The feed water 101 moves in the feed-side flow path formed by the feed-side flow path material 11 on the feed side of the composite semipermeable membrane 1. The fluid that has permeated the composite semipermeable membrane 1 (shown as permeated water 102 in FIG. 2) moves in the permeate-side flow path formed by the permeate-side flow path material 12. The permeated water 102 that has reached the water collection pipe 6 passes through the holes in the water collection pipe 6 and enters the inside of the water collection pipe 6. The permeated water 102 that has flowed in the water collection pipe 6 is discharged to the outside from the second end plate 8. On the other hand, the fluid that has not permeated the composite semipermeable membrane 1 (shown as concentrated water 103 in FIG. 2) moves in the feed-side flow path and is discharged to the outside from the second end plate 8. In this way, the feed water 101 is separated into the permeated water 102 and the concentrated water 103.
[0095] 4. Manufacturing method of composite semipermeable membrane element As a method for producing a composite semipermeable membrane element, the methods disclosed in Japanese Patent Publication No. 44-14216, Japanese Patent Publication No. 4-11928, Japanese Patent Laid-Open No. 11-226366, and the like can be used.
[0096] 5. Use of composite semipermeable membranes and composite semipermeable membrane elements The composite semipermeable membrane and composite semipermeable membrane element according to the present embodiment can be suitably used as a nanofiltration membrane and nanofiltration membrane element for separating monovalent ions and polyvalent ions. The composite semipermeable membrane and composite semipermeable membrane element according to the present embodiment can be used, for example, for removing salt and adjusting minerals from brackish water or seawater, removing salt and adjusting minerals in the food industry, recovering acids from industrial applications such as plating and refining, and recovering metals from acid solutions.
[0097] The composite semipermeable membrane elements according to this embodiment can also be connected in series or in parallel and housed in a pressure vessel to form a composite semipermeable membrane module.
[0098] Furthermore, the above-mentioned composite semipermeable membrane, composite semipermeable membrane element, and composite semipermeable membrane module can be combined with a pump that supplies raw water to them, a device that pretreats the raw water, etc. to form a fluid separation device. By using this separation device, raw water can be separated into permeated water such as drinking water and concentrated water that did not permeate the membrane, thereby obtaining water suitable for the purpose.
[0099] 6. Filtration equipment The filtration system according to this embodiment includes a separation device and a flow control facility. The separation device includes the composite semipermeable membrane element, and the flow control facility controls the flow rates of the permeate and concentrated water from the separation device.
[0100] The separation device preferably has a pressure container (vessel) filled with a composite semipermeable membrane element, and has a structure in which a solution can be supplied to the vessel by a high-pressure pump.
[0101] The permeate and concentrate flow rate control equipment preferably has an instrument (flow meter) capable of measuring the flow rates of the permeate and concentrate from the composite semipermeable membrane element in order to control the flow rates of the permeate and concentrate from the composite semipermeable membrane element. In controlling the permeate flow rate, the high-pressure pump preferably has a mechanism for receiving data from the permeate flow meter at any time and controlling the output of the high-pressure pump so as to maintain a constant permeate flow rate. In controlling the concentrate flow rate, it is preferable to have an electromagnetic valve near the concentrate flow meter, and the electromagnetic valve preferably has a mechanism for receiving data from the concentrate flow meter at any time and controlling the concentrate flow rate to a constant value.
[0102] In addition to the above, the filtration device of this embodiment can be arbitrarily combined with pumps, piping, valves, tanks, vessels, temperature control devices, and instruments (pH meters, conductivity meters, flow meters, pressure gauges, etc.). EXAMPLES
[0103] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0104] <Positron annihilation lifetime measurement using positron beam method> The positron annihilation lifetime measurement of the separation functional layer was carried out using a positron beam method as follows. The composite semipermeable membrane was washed with pure water at 70°C for 1 hour, and then left to stand in pure water at 25°C for 30 minutes. The composite semipermeable membrane was then freeze-dried under reduced pressure at -30°C and cut into 1.5cm x 1.5cm squares to prepare test samples. The separation functional layer side of the test sample was measured with a barium difluoride scintillation counter using a photomultiplier tube at a total count of 5 million at room temperature under vacuum using a thin-film positron annihilation lifetime measurement device equipped with a positron beam generator (this device is described in detail in, for example, Radiation Physics and Chemistry, 58,603, Pergamon (2000)). From the mean lifetime τ of the third component obtained by analysis, the mean hole diameter was calculated as R1 when the beam intensity was 0.1 keV, and as R2 when the beam intensity was 0.5 keV.
[0105] <Number and diameter of holes in cross section of separation functional layer> The number of holes and the hole diameter of the cross section of the separation functional layer were measured using a field emission transmission microscope (hereinafter, "STEM") as follows. The composite semipermeable membrane was freeze-dried under reduced pressure at -30°C and cut into 1.5 cm x 1.5 cm squares to prepare observation samples. Using a STEM (Hitachi HF5000) using GMS3 (Gatana) as software and DeConv.HAADF (HREM) as a plug-in, images of the cross section of the separation functional layer in this composite semipermeable membrane were taken under the conditions of a pressurizing power of 200 kV, a spherical aberration (Cs) of 1 μm, an aperture of 22 mrad, and an observation magnification of 100,000. The obtained images were used to calculate the circle equivalent diameter by converting the hole area into a perfect circle using ImageJ (Fiji), and the value rounded off to the third decimal place was used as the hole diameter. Based on the obtained pore diameters, the total number of pores with diameters of 0.30 nm to 1.20 nm (P1), the total number of pores with diameters of 0.50 nm to less than 0.80 nm (P2), the total number of pores with diameters of 0.80 nm to 1.20 nm (P3), and the total number of pores with diameters of more than 1.20 nm (P4) were counted. Three images were analyzed for each of three different cross sections randomly selected, and the average values obtained were calculated.
[0106] <Measurement of amino group density> After treating a 5 cm × 5 cm composite semipermeable membrane obtained by physically peeling a substrate by the cryo-ultramicrotomy method, placing it on a grid, immersing it in pure water for 4 hours, then immersing it in a 10 mass% aqueous 2-propanol solution for 1 hour, washing it, and using it as a sample. The obtained sample was immersed in a 1.0×10 -3 mol / L aqueous solution of Na2WO4·2H2O adjusted to pH 3.8 and 25 °C for 10 minutes three times in succession, and then the sample was immersed in a 1.0×10 -7 mol / L aqueous solution of Na2WO4·2H2O adjusted to pH 3.8 and 25 °C for 7 minutes four times in succession. Then, after removing the moisture of the sample with filter paper, it was freeze-dried at -30 °C to obtain a sample for measuring the amino group density. A cross-sectional image of the obtained sample for measuring the amino group density was taken using STEM (HF5000 manufactured by Hitachi High-Tech) under the condition of an acceleration voltage of 200 kV to obtain a STEM image at a magnification of 100,000. The obtained image was analyzed with image processing software. By the above method, in the cross-section perpendicular to the surface of the composite semipermeable membrane (the cross-section perpendicular to the first surface), from the first surface side to the second surface side, each region obtained by equally dividing the above separation functional layer into 5 parts at equal intervals was defined as region a~e, and the amino group density was calculated for each region a~e from the luminance value. Let the amino group density in region b be Nb and the amino group density in region d be Nd, and Nb / Nd was calculated.
[0107] <Mg removal rate, Li removal rate> An aqueous solution adjusted to a temperature of 25 °C, pH 1, sulfuric acid concentration of 100 mmol / L, lithium sulfate concentration of 45 mmol / L, and magnesium sulfate concentration of 115 mmol / L was supplied to the composite semipermeable membrane at a flow rate of 3.5 L / min, and the pressure was adjusted so that the membrane permeation flux, which is the value converted to the water permeation amount (cubic meters) per square meter of the membrane surface per day, was 0.4 m 3 / m 2 / day, and membrane filtration treatment was performed. The magnesium ion (hereinafter, "Mg 2+ ") concentration and lithium ion (hereinafter, "Li +The " concentration was measured using a Hitachi P-4010 ICP (inductively coupled plasma atomic emission spectrometry) device, and the Mg removal rate and Li removal rate were calculated based on the following formula. Mg removal rate (%) = {1-(Mg in permeate 2+ concentration) / (Mg in the supply water 2+ concentration)}×100 Li removal rate (%) = {1-(Li in the permeate + concentration) / (Li in the supply water + concentration)}×100
[0108] <Monovalent ion / divalent ion selectivity> The monovalent ion / divalent ion selectivity was calculated based on the values of the Mg removal rate and Li removal rate calculated from the above-mentioned "Mg removal rate, Li removal rate" measurements and according to the following formula. Monovalent ion / divalent ion selectivity = (100-Li removal rate) / (100-Mg removal rate) The above evaluation is for Mg 2+ The evaluation was carried out using the removal rate of Mg 2+ If the permeation of Mg can be inhibited, it can be assumed that the permeation of other multivalent ions can also be inhibited. 2+ is a typical divalent ion, and generally, multivalent ions with a valence of three or more have a larger ion size than divalent ions.
[0109] <Glucose permeability, sucrose permeability> The glucose permeability B when a 1000 ppm glucose aqueous solution at 25°C and pH 6.5 was permeated through the composite semipermeable membrane at an operating pressure of 0.5 MPa and the sucrose permeability C when a 1000 ppm sucrose aqueous solution at 25°C and pH 6.5 was permeated through the composite semipermeable membrane were calculated using the following formulas, and the glucose permeability relative to the sucrose permeability (B / C) was calculated. The glucose and sucrose concentrations were measured using a refractometer (Shimadzu Corporation, RID-6A). Glucose permeability B = (glucose concentration in permeate water / glucose concentration in feed water) x 100 Sucrose permeability C = (sucrose concentration in permeate water / sucrose concentration in feed water) × 100
[0110] <Preparation of the support film> Nonwoven fabric made of polyester fibers produced by papermaking method (breathability 1.0cc / cm 2 A 18% by mass solution of polysulfone in dimethylformamide (DMF) was cast onto a substrate (1000 x 1000 / s, thickness 42 μm) at room temperature (25°C) to a coating thickness of 180 μm, and then the substrate was immediately immersed in pure water for 5 minutes to form a porous support layer on the substrate, thereby producing a support membrane.
[0111] <Preparation of composite semipermeable membrane> Example 1 The support membrane obtained above was immersed in a 30°C aqueous solution containing 2.0% by mass of homopiperazine (logP: -0.65), 250 ppm of sodium dodecyl diphenyl ether disulfonate, and 1.0% by mass of trisodium phosphate for 15 seconds, and then nitrogen was blown from an air nozzle to remove excess aqueous solution, forming a coating layer of an amine aqueous solution on the support membrane. The membrane was then immersed in a 38°C n-decane solution containing 0.2% by mass of TMC, and then left to stand for 1 minute at an atmospheric humidity (relative humidity) of 80% at 25°C, and two fluids (pure water and air) were blown onto the membrane surface to remove the solution on the surface. The membrane was then washed with 80°C pure water to obtain a composite semipermeable membrane.
[0112] Example 2 After carrying out the same operation as in Example 1, the membrane was further immersed in glycerin at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0113] Example 3 After carrying out the same operation as in Example 1, the membrane was further immersed in triethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0114] Example 4 A composite semipermeable membrane was prepared in the same manner as in Example 1, except that an aqueous amine solution was applied onto the support membrane and allowed to stand for 15 seconds to form a coating layer.
[0115] Example 5 A composite semipermeable membrane was prepared in the same manner as in Example 3, except that an amine aqueous solution was applied onto the support membrane and allowed to stand for 15 seconds to form a coating layer.
[0116] Example 6 A composite semipermeable membrane was prepared in the same manner as in Example 4, except that the polyfunctional aliphatic amine was changed to 2-methylpiperazine (logP: -0.44).
[0117] Example 7 A composite semipermeable membrane was prepared in the same manner as in Example 6, except that the atmospheric humidity was changed to 90%.
[0118] Example 8 A composite semipermeable membrane was prepared in the same manner as in Example 6, except that the atmospheric humidity was changed to 95%.
[0119] Example 9 After carrying out the same operation as in Example 8, the membrane was further immersed in 1,3-butanediol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0120] Example 10 A composite semipermeable membrane was prepared in the same manner as in Example 1, except that the polyfunctional aliphatic amine was changed to 2,5-dimethylpiperazine (logP: -0.12).
[0121] Example 11 A composite semipermeable membrane was prepared in the same manner as in Example 10, except that the atmospheric humidity was changed to 90%.
[0122] Example 12 A composite semipermeable membrane was prepared in the same manner as in Example 11, except that a coating layer was formed by applying an aqueous amine solution onto the support membrane and leaving it to stand for 15 seconds.
[0123] (Example 13) After carrying out the same operation as in Example 12, the membrane was further immersed in diethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0124] Example 14 A composite semipermeable membrane was prepared in the same manner as in Example 1, except that the polyfunctional aliphatic amine was changed to 2,5-diethylpiperazine (logP: 0.85).
[0125] Example 15 A composite semipermeable membrane was prepared in the same manner as in Example 13, except that the polyfunctional aliphatic amine was changed to 2,5-diethylpiperazine and diethylene glycol was changed to ethylene glycol.
[0126] Example 16 A composite semipermeable membrane was prepared in the same manner as in Example 8, except that the polyfunctional aliphatic amine was changed to 2,5-diethylpiperazine.
[0127] (Example 17) After carrying out the same operation as in Example 16, the membrane was further immersed in ethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0128] Comparative Example 1 A composite semipermeable membrane was prepared in the same manner as in Example 1, except that the polyfunctional aliphatic amine was changed to piperazine and the atmospheric humidity was changed to 75%.
[0129] Comparative Example 2 After carrying out the same operation as in Example 1, the membrane was further immersed in glycerin at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0130] Comparative Example 3 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 1, except that an amine aqueous solution was applied onto the support membrane and allowed to stand for 15 seconds to form a coating layer.
[0131] Comparative Example 4 After carrying out the same operation as in Comparative Example 3, the membrane was immersed in ethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0132] Comparative Example 5 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 3, except that the concentration of the polyfunctional acid chloride was changed to 0.4% by mass.
[0133] Comparative Example 6 A composite semipermeable membrane was produced in the same manner as in Comparative Example 3, except that the temperature during the interfacial polycondensation was changed to 80°C.
[0134] Comparative Example 7 After carrying out the same operation as in Comparative Example 3, the membrane was further immersed in a 1.0 mass % aqueous solution of propionic anhydride at 25° C. for 10 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0135] Comparative Example 8 A composite semipermeable membrane was prepared in the same manner as in Example 1, except that the polyfunctional aliphatic amine was changed to 4,4'-bipiperidine (logP: -0.17).
[0136] Comparative Example 9 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 8, except that an amine aqueous solution was applied onto the support membrane and allowed to stand for 15 seconds to form a coating layer.
[0137] Comparative Example 10 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 9, except that the atmospheric humidity was changed to 90%.
[0138] Comparative Example 11 A composite semipermeable membrane was produced in the same manner as in Example 4, except that the atmospheric humidity was changed to 75%.
[0139] Comparative Example 12 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 11, except that the concentration of the polyfunctional acid chloride was changed to 0.4% by mass.
[0140] Comparative Example 13 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 11, except that the temperature during the interfacial polycondensation was changed to 80°C.
[0141] Comparative Example 14 After carrying out the same operation as in Comparative Example 11, the membrane was further immersed in triethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0142] Comparative Example 15 After carrying out the same operation as in Comparative Example 11, the membrane was further immersed in a 1.0% by mass aqueous solution of acetic anhydride at 25° C. for 10 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0143] Comparative Example 16 A composite semipermeable membrane was prepared in the same manner as in Example 6, except that the atmospheric humidity was changed to 75%.
[0144] Comparative Example 17 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 16, except that the concentration of the polyfunctional acid chloride was changed to 0.4% by mass.
[0145] (Comparative Example 18) A composite semipermeable membrane was produced in the same manner as in Comparative Example 16, except that the temperature during the interfacial polycondensation was changed to 80°C.
[0146] Comparative Example 19 After carrying out the same operation as in Comparative Example 16, the membrane was further immersed in 1,3-butanediol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0147] Comparative Example 20 After carrying out the same operation as in Comparative Example 16, the membrane was further immersed in a 1.0 mass% aqueous solution of propionic anhydride at 25°C for 10 minutes, and then in pure water at 25°C for 24 hours to prepare a composite semipermeable membrane.
[0148] Comparative Example 21 A composite semipermeable membrane was prepared in the same manner as in Example 12, except that the atmospheric humidity was changed to 75%.
[0149] Comparative Example 22 A composite semipermeable membrane was prepared in the same manner as in Comparative Example 21, except that the concentration of the polyfunctional acid chloride was changed to 0.4% by mass.
[0150] (Comparative Example 23) A composite semipermeable membrane was produced in the same manner as in Comparative Example 21, except that the temperature during the interfacial polycondensation was changed to 80°C.
[0151] Comparative Example 24 After carrying out the same operation as in Comparative Example 21, the membrane was further immersed in diethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0152] Comparative Example 25 After carrying out the same operation as in Comparative Example 21, the membrane was further immersed in a 1.0% by mass aqueous solution of acetic anhydride at 25° C. for 10 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0153] Comparative Example 26 A composite semipermeable membrane was prepared in the same manner as in Example 16, except that the atmospheric humidity was changed to 75%.
[0154] (Comparative Example 27) A composite semipermeable membrane was prepared in the same manner as in Comparative Example 26, except that the concentration of the polyfunctional acid chloride was changed to 0.4% by mass.
[0155] (Comparative Example 28) A composite semipermeable membrane was produced in the same manner as in Comparative Example 26, except that the temperature during the interfacial polycondensation was changed to 80°C.
[0156] Comparative Example 29 After carrying out the same operation as in Comparative Example 26, the membrane was further immersed in ethylene glycol at 80° C. for 2 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0157] (Comparative Example 30) After carrying out the same operation as in Comparative Example 26, the membrane was further immersed in a 1.0% by mass aqueous solution of acetic anhydride at 25° C. for 10 minutes, and then in pure water at 25° C. for 24 hours to prepare a composite semipermeable membrane.
[0158] (Comparative Example 31) A composite semipermeable membrane was prepared in the same manner as in Comparative Example 1, except that the polyfunctional aliphatic amine was changed to 2,5-diisopropylpiperazine (logP: 1.65).
[0159] (Comparative Example 32) A composite semipermeable membrane was produced in the same manner as in Comparative Example 31, except that the atmospheric humidity was changed to 95%, an amine aqueous solution was applied onto the support membrane and left to stand for 15 seconds to form a coating layer, and then the membrane was immersed in ethylene glycol at 80°C for 2 minutes and then in pure water at 25°C for 24 hours.
[0160] (Comparative Example 33) A composite semipermeable membrane was prepared in the same manner as in Comparative Example 32, except that the polyfunctional aliphatic amine was changed to metaphenylenediamine (logP: 0.43).
[0161] [Table 1]
[0162] [Table 2]
[0163] [Table 3]
[0164] [Table 4]
[0165] [Table 5]
[0166] [Table 6]
[0167] As shown in Tables 1 to 6, the composite semipermeable membranes of Examples 1 to 17 in which R1 and R2 were 0.30 nm or more and 2.00 nm or less and satisfied 0.90≦R1 / R2≦1.10 showed higher monovalent ion / divalent ion selectivity under acidic conditions than the composite semipermeable membranes of Comparative Examples 1 to 33.
[0168] A comparison between Examples 4 and 5 and Examples 11 and 12 shows that a composite semipermeable membrane satisfying 0.31≦P2 / P1≦0.35, P3 / P2≦0.09, and P4 / P1≦0.005 exhibits superior monovalent ion / divalent ion selectivity. Comparing Example 1 and Example 3, it is clear that the monovalent ion / multivalent ion selectivity is improved by satisfying Nb / Nd≦0.80. In addition, by comparing Example 8 and Example 9, it was found that Nb was 1.0 × 10 -23 mol / nm 2 It can be seen that the monovalent ion / multivalent ion selectivity is improved by setting the concentration to the following: It can be seen that in Examples 6 to 17 in which the separation functional layer has a pleated structure, operation can be performed at a lower pressure than in Examples 1 to 5 in which the separation functional layer does not have a pleated structure.
[0169] Although the present invention has been described in detail with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2022-192377) filed on November 30, 2022, a Japanese patent application (Patent Application No. 2022-192378) filed on November 30, 2022, and a Japanese patent application (Patent Application No. 2023-169359) filed on September 29, 2023, which are incorporated by reference in their entirety. In addition, all references cited herein are incorporated in their entirety. [Explanation of symbols]
[0170] 1 Composite semipermeable membrane 2 Base material 3 Porous support layer 4 Separation functional layer 6 Water collection pipe 7 First end plate 8 Second end plate 11 Supply side channel material 12 Permeate side channel material 20 Envelope membrane 26 Rolled body 100 Composite semipermeable membrane element 101 Supply water 102 Permeated water 103 Concentrated water 201 Pleats height 202 Thickness of separation functional layer P reference point X1 Tangent to the outer surface of the thin film passing through reference point P X2 Tangent to the inner surface of the thin film parallel to tangent X1 Y0 Normal line passing through reference point P Y1, Y2 Straight line parallel to normal Y0 a, b, c, d, e Each of the five regions of the separation functional layer
Claims
1. A composite semipermeable membrane comprising a porous support layer and a separation functional layer located on one side of the porous support layer, The separation functional layer contains a semi-aromatic crosslinked polyamide, A surface of the composite semipermeable membrane on the separating functional layer side is designated as a first surface, and a surface opposite to the first surface is designated as a second surface, The composite semipermeable membrane is irradiated with a positron beam from the first surface side, and the average pore size R1 and the average pore size R2 of the separation functional layer derived by a positron annihilation lifetime measurement method are 0.30 nm or more and 2.00 nm or less and satisfy 0.90≦R1 / R2≦1.
10. R1: Average pore diameter at a positron beam intensity of 0.1 keV R2: Average pore diameter at a positron beam intensity of 0.5 keV
2. The composite semipermeable membrane according to claim 1, wherein the average pore size R1 is 0.55 nm or more and 1.00 nm or less.
3. 3. The composite semipermeable membrane according to claim 1 or 2, wherein in a cross section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane, the total number P1 of pores having a pore diameter of 0.30 nm or more and 1.20 nm or less, the total number P2 of pores having a pore diameter of 0.50 nm or more and less than 0.80 nm, the total number P3 of pores having a pore diameter of 0.80 nm or more and 1.20 nm or less, and the total number P4 of pores having a pore diameter of more than 1.20 nm satisfy 0.20 < P2 / P1 < 0.40, P3 / P2 < 0.20, and P4 / P1 ≦ 0.
01.
4. 3. The composite semipermeable membrane according to claim 1, wherein in a cross section of the separation functional layer perpendicular to the surface of the composite semipermeable membrane, the separation functional layer is divided into five equally spaced regions a to e from the first surface side toward the second surface side, and the amino group density Nb in region b and the amino group density Nd in region d satisfy Nb / Nd≦0.
80.
5. The Nb is 1.0×10 -23 mol / nm 2 The composite semipermeable membrane according to claim 4, wherein:
6. 3. The composite semipermeable membrane according to claim 1 or 2, wherein B / C is 10 or more, where B is the glucose permeability when a 1000 ppm glucose aqueous solution having a pH of 6.5 and an operating pressure of 0.5 MPa is permeated at 25° C. and C is the sucrose permeability when a 1000 ppm sucrose aqueous solution having a pH of 6.5 and an operating pressure of 0.5 MPa is permeated at 25° C.
7. 3. The composite semipermeable membrane according to claim 1, wherein the separating functional layer has a hollow pleated structure.
8. A composite semipermeable membrane element comprising the composite semipermeable membrane according to claim 1 or 2.
9. A filtration device comprising the composite semipermeable membrane element according to claim 8.
Citation Information
Patent Citations
Filter membrane and its production
JP1998225629A
modified sulfonamide polymer
JP2003534422A
Conjugate nano-filtering membrane
JP2007277298A
Electrode for secondary battery, and its utilization
JP2008181751A
Composite semipermeable membrane
JP2014233652A