Photosensitive resin laminate for microchannel devices
The photosensitive resin laminate addresses fluid resistance and fluorescence interference issues in microchannel devices by ensuring high transmittance, adhesion, and composition ratios, enhancing detectability and precision.
Patent Information
- Application Number
- JP2023136088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-01
- Filing Date
- 2023-08-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-10-01
AI Technical Summary
Microchannel devices experience issues with fluid resistance, cracking, and fluorescence interference due to the properties of existing photosensitive resin laminates, which affect the accuracy and detectability of target substances.
A photosensitive resin laminate with specific transmittance, adhesion strength, and composition ratios, including a support film and a photosensitive resin composition layer, designed for direct exposure, ensuring high detectability and resistance to fluids and cracks.
The laminate provides excellent detectability of target substances by fluorescence emission with improved fluid resistance and crack resistance, maintaining dimensional accuracy and reducing interference, thus enhancing the precision of microchannel device operations.
Smart Images

Figure 0007593600000004 
Figure 0007593600000001 
Figure 0007593600000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin laminate for a microchannel device. [Background technology]
[0002] Microfluidic devices (also called microfluidic devices, microfluidic chips, μTAS (Micro Total Analysis Systems), LOC (Lab on a Chip), microreactors, etc.) are known as devices equipped with microcircuits formed using microfabrication technologies such as Micro Electro Mechanical Systems (MEMS) technology based on microfluidics, and are being used for various applications such as biotechnology research, drug discovery, diagnosis, testing, and chemical engineering. In particular, in recent years, there has been growing interest in the use of microfluidic devices in home healthcare, remote medical care, point-of-care testing (POCT), etc.
[0003] Conventionally, microchannel devices have been manufactured by injection molding, mold forming, and glass etching. However, instead of these, a method has been proposed in which a resin pattern for the channel is formed on a substrate by photolithography, and then a lid material (sealing material) is bonded (Patent Documents 1 to 3).
[0004] Patent Document 1 describes that a permanent photoresist composition comprising (A) a bisphenol A-novolac epoxy resin having a specific structure, (B) an epoxy resin having a specific structure, (C) one or more cationic photoinitiators (also known as photoacid generators or PAGs), and (D) one or more solvents, can be formed by ultraviolet lithography and is also useful for the manufacture of microfluidic components and the like.
[0005] Patent Document 2 describes a method for manufacturing a microfluidic chip package or assembly, in which a block containing a microfluidic structure is formed on a substrate, and a cover film is attached to cover the block, with a dry film resist being preferred as the cover film. Patent Document 3 describes that a method for producing a microfluidic device includes the steps of forming a resin layer from a photosensitive resin composition of a specific composition on a support, exposing a part of the resin layer to ultraviolet light and developing it, placing a lid material on the developed resin layer to obtain a laminate, and exposing the obtained laminate to ultraviolet light. The method describes that the patterned resin layer after lithography has sufficient strength and tack, making it possible to produce a microfluidic device having good flow paths, etc. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2007-522531 [Patent Document 2] Special Publication No. 2016-529116 [Patent Document 3] JP 2017-119340 A Summary of the Invention [Problem to be solved by the invention]
[0007] Microchannel devices are used for the analysis and chemical reactions of trace substances in various applications as described above, and fluids (liquids or gases) according to each application are introduced into the microchannels. If the members (e.g., partition materials and sealing materials) that come into contact with the fluid in the microchannel have poor resistance to the fluid (e.g., water resistance to aqueous fluids) and the members swell due to the fluid, or if the members have defects such as cracks, the intended flow of the fluid in the microchannel is not ensured, and in some cases the fluid leaks out of the microchannel, impairing the accuracy of the analysis, chemical reaction, etc. When a photosensitive resin laminate (also called a dry film resist or dry film photoresist) having a support film and a photosensitive resin composition layer is used, the properties of the members (water resistance, organic solvent resistance, mechanical properties, etc.) can be easily designed by changing the composition of the photosensitive resin composition, so that the resistance to the fluid and the crack resistance can be appropriately controlled according to the application, and the analysis, chemical reaction, etc. can be performed with high accuracy. Furthermore, since the photosensitive resin laminate can be pattern-exposed, it is possible to form a member with excellent dimensional accuracy without requiring a mold or the like (that is, with low equipment costs).
[0008] In analyses, chemical reactions, etc. using microfluidic devices, the presence of a target substance is often detected by irradiating light of a specific wavelength and detecting the emission signal from the target substance. For such fluorescence detection, for example, a fluorescein-based compound is often used to detect an excitation wavelength of about 490 nm and an emission wavelength of about 515 nm. In addition, a fluorescence microscope with an excitation wavelength of 510 to 560 nm and a detection wavelength of 590 nm or more may be used. Members formed using photosensitive resin laminates are excellent in terms of resistance to fluids, crack resistance, and dimensional accuracy, but have a problem in that they emit light when irradiated with light of a specific wavelength, preventing the desired fluorescence detection of the target substance.
[0009] Therefore, an object of the present invention is to provide a photosensitive resin laminate for a microchannel device, which has excellent detectability by fluorescence emission of a target substance. [Means for solving the problem]
[0010] The present disclosure encompasses the following aspects. [1] A photosensitive resin laminate for a microchannel device, comprising a support film and a photosensitive resin composition layer, the photosensitive resin laminate for microchannel devices has a transmittance of 80% or more at either or both of wavelengths of 515 nm and 600 nm after exposure, the adhesion strength between the support film and the photosensitive resin composition layer is 3 gf / inch or more and 100 gf / inch or less; Photosensitive resin laminate for microchannels. [2] The photosensitive resin laminate for a microchannel according to embodiment 1, which is for use in direct imaging exposure. [3] The photosensitive resin laminate for a microchannel according to the above-mentioned embodiment 1 or 2, wherein the photosensitive resin composition layer is composed of a photosensitive resin composition having a ratio (I / O) of an inorganic value (I) to an organic value (O) of 1.0 or less. [4] The photosensitive resin laminate for a microchannel according to any one of the above embodiments 1 to 3, wherein the photosensitive resin composition layer has an elastic modulus of 2 GPa or less and a breaking elongation of 30% or more after exposure. [5] The microchannel photosensitive resin laminate according to any one of the above aspects 1 to 4, wherein the photosensitive resin composition layer has a thickness of 100 μm or more. [6] In the thickness of the photosensitive resin composition layer, 30° C., 1% by mass Na 2 CO 3 6. The microchannel photosensitive resin laminate according to any one of the above embodiments 1 to 5, wherein the development time per 25 μm with an aqueous solution is 15 to 50 seconds / 25 μm. [7] The photosensitive resin composition layer contains (a) an alkali-soluble polymer having a carboxyl group, (b) an addition-polymerizable monomer, and (c) a photopolymerization initiator; (b) the addition polymerizable monomer is selected from the group consisting of the following (Formula I): C-((CH 2 )R 1 )((CH 2 )R 2 )((CH 2 )R 3 )((CH 2 )R 4 ) (Formula I) (In the formula, R 1 ~R 4 Each independently represents a monovalent organic group. and a molecular weight of 200 to 600 in an amount of 50 mass % or more in the (b) addition-polymerizable monomers. Effect of the Invention
[0011] According to the present invention, it is possible to provide a photosensitive resin laminate for a microchannel device, which provides a microchannel device having excellent detectability by fluorescence emission of a target substance. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing a flow path pattern formed in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, a detailed description will be given of an embodiment of the present invention (hereinafter, abbreviated as "embodiment"). Note that the present invention is not limited to the following embodiment, and can be modified in various ways within the scope of the present invention.
[0014] [Photosensitive resin laminate] This embodiment provides a photosensitive resin laminate for microchannel devices, which is composed of a support film and a photosensitive resin composition layer. The phrase "composed of a support film and a photosensitive resin composition layer" means that the laminate is substantially composed of a support film and a photosensitive resin composition layer, but does not exclude the possibility that other elements may be present within a range that does not impair the effects of the present invention. The photosensitive resin laminate for microchannel devices according to this embodiment (hereinafter, also simply referred to as "photosensitive resin laminate") has properties that are particularly suitable for forming microchannels by photolithography, and can be used, for example, as a partition material, a cover material, etc. for microchannels.
[0015] In one embodiment, the photosensitive resin laminate has a transmittance of 80% or more at either or both of wavelengths of 515 nm and 600 nm after exposure. The transmittance is a value measured by irradiating light having wavelengths of 515 nm and 600 nm from the photosensitive resin composition layer side after exposure. From the viewpoint of obtaining the desired detectability by the fluorescence emission of the target substance, particularly from the viewpoint of detecting the emission of a fluorescein-based compound, the transmittance is 80% or more, preferably 82% or more, more preferably 84% or more, and even more preferably 85% or more. The upper limit of the transmittance may be 100%, but from the viewpoint of ease of production of the photosensitive resin laminate, it may be preferably 99% or less. Means for adjusting the transmittance to 80% or more include, but are not limited to, ensuring that the photosensitive resin composition layer is substantially free of coloring substances (dyes, pigments, etc.) or dyes that develop color upon exposure to light (more specifically, ensuring that the content of coloring substances is 0% by mass or more and less than 0.001% by mass, based on the total solid content of the photosensitive resin composition layer), and ensuring that the haze of the support film is 5 or less.
[0016] In this disclosure, "after exposure" refers to 500 mJ / cm unless otherwise specified. 2 This refers to the state after 10 minutes of exposure to light of that amount.
[0017] In the present disclosure, the term "colored substance" refers to a substance that has absorption in the visible range before or after exposure (specifically, a molar absorption coefficient of 10,000 L / (mol cm) or more in the range of 420 to 800 nm when measured with a spectrophotometer).
[0018] Examples of coloring substances include color-developing dyes such as phthalocyanine green, crystal violet, methyl orange, Nile blue 2B, Victoria blue, malachite green, basic blue 20, diamond green, etc., or combinations of leuco dyes or fluoran dyes and halogen compounds. Leuco dyes include, for example, tris(4-dimethylamino-2-methylphenyl)methane [leuco crystal violet], tris(4-dimethylamino-2-methylphenyl)methane [leucomalachite green], and fluoran dyes.
[0019] In one embodiment, the photosensitive resin laminate is for use in a direct imaging exposure method. As a method for exposing a photosensitive resin, in addition to the direct imaging method, a method using a mask and the like are known, but the direct imaging exposure is desirable in that a microchannel having a complex shape can be formed with high dimensional accuracy. As a characteristic of a photosensitive resin composition layer suitable for direct imaging exposure, a photosensitive resin layer having high sensitivity is preferable. In general, in the direct imaging method, a large area is exposed by repeating or scanning exposure of a minute exposure area using a digital micromirror device or a polygon mirror. In this case, since the exposure time per unit area is shortened to shorten the exposure tact, it is preferable that the photosensitive resin layer has high sensitivity. As an example of a highly sensitive photosensitive resin composition, a radical negative type photosensitive resin layer containing an alkali-soluble polymer, an addition polymerizable monomer, and a photopolymerization initiator can be mentioned. Since the radical polymerization, i.e., the curing reaction, of such a negative type photosensitive resin layer is inhibited by oxygen in the air during exposure, it is preferable that the layer is covered with a plastic film having low oxygen permeability and high transparency. For these reasons, a photosensitive resin laminate is preferably used for direct imaging exposure.
[0020] In a preferred embodiment, the photosensitive resin composition layer is composed of a photosensitive resin composition having a ratio (I / O) of inorganic value (I) to organic value (O) of 1.0 or less. Includes.
[0021] The ratio (I / O) of inorganic value (I) to organic value (O), also called the I / O value or inorganic value / organic value, is a value that represents the polarity of a component or compound in terms of an organic concept, and is a type of functional group contribution method in which parameters are set for each functional group.
[0022] The ratio (I / O) is explained in detail in such documents as Organic Concept Diagram (Koda Yoshio, Sankyo Publishing (1984)); KUMAMOTO PHARMACEUTICAL BULLETIN, No. 1, pages 1-16 (1954); and Chemistry Area, Vol. 11, No. 10, pages 719-725 (1957). The ratio (I / O) is a measure that classifies the properties of a component or compound broadly into organic groups that exhibit covalent bonding and inorganic groups that exhibit ionic bonding, and indicates the positions of these groups on a rectangular coordinate system named the organic axis and inorganic axis.
[0023] The inorganic value (I) is a numerical value of the influence of various substituents or bonds on the boiling point of an organic compound, based on the hydroxyl group. Specifically, the distance between the boiling point curve of a straight-chain alcohol and that of a straight-chain paraffin is about 100°C when taken around the carbon number of 5, so the influence of one hydroxyl group is set to 100, and the value of the influence of various substituents or various bonds on the boiling point, which is quantified based on this value, is the inorganic value (I) of the substituents of the organic compound. For example, the inorganic value (I) of a -COOH group is 150, and the inorganic value (I) of a double bond is 2. Therefore, the inorganic value (I) of a certain organic compound means the sum of the inorganic values (I) of various substituents or bonds that the compound has.
[0024] The organic value (O) is determined based on the influence of the carbon atom representing the methylene group on the boiling point, using the methylene group in the molecule as a unit. In other words, the average increase in boiling point due to the addition of one carbon atom in linear saturated hydrocarbon compounds with carbon numbers of 5 to 10 is 20°C, so based on this, the organic value of one carbon atom is set to 20, and the influence of various substituents or bonds on the boiling point is quantified based on this to become the organic value (O). For example, a nitro group (-NO 2 ) has an organic value (O) of 70.
[0025] In general, the closer the ratio (I / O) is to 0, the more non-polar (more hydrophobic, more organic) the organic material is, while the larger the value, the more polar (more hydrophilic, more inorganic) the organic material is. The ratio (I / O) of the photosensitive resin composition layer is preferably 1.0 or less, more preferably 0.9 or less, even more preferably 0.8 or less, and particularly preferably 0.7 or less, from the viewpoint of the resistance (fluid resistance) of the photosensitive resin laminate to the fluid flowing through the microchannel. The ratio (I / O) is preferably 0.0 from the viewpoint of fluid resistance, but may be 0.1 or more, 0.2 or more, or 0.3 or more, from the viewpoint of the ease of manufacture and developability of the photosensitive resin laminate. The above ratio (I / O) is a value calculated based on the base resin and monomer of the photosensitive resin composition (i.e., excluding the photopolymerization initiator and additives).
[0026] In a preferred embodiment, the photosensitive resin composition layer has an elastic modulus of 2 GPa or less after exposure. From the viewpoint of obtaining good crack resistance, the elastic modulus is preferably 2 GPa or less, more preferably 1.5 GPa or less, and even more preferably 1.0 GPa or less, and from the viewpoint of obtaining good mechanical strength, the elastic modulus is preferably 0.1 GPa or more, more preferably 0.3 GPa or more, and even more preferably 0.5 GPa or more.
[0027] In a preferred embodiment, the photosensitive resin composition layer has a breaking elongation of 30% or more after exposure. From the viewpoint of obtaining good crack resistance, the breaking elongation is preferably 30% or more, more preferably 60% or more, and even more preferably 100% or more, and from the viewpoint of obtaining good mechanical strength, the breaking elongation is preferably 300% or less, more preferably 200% or less, and even more preferably 180% or less.
[0028] In a particularly preferred embodiment, the photosensitive resin composition layer has an elastic modulus of 2 GPa or less and a breaking elongation of 30% or more after exposure.
[0029] The components of the photosensitive resin laminate for a microchannel device according to this embodiment will be described below.
[0030] <Photosensitive resin composition layer> The photosensitive resin composition layer can be formed by applying the photosensitive resin composition to a support film, drying and laminating the composition. The photosensitive resin composition can contain any polymer and / or monomer as long as it can impart photosensitivity to the photosensitive resin laminate, and may further contain a photopolymerization initiator, other additives, and the like, as desired.
[0031] The photosensitive resin composition preferably contains (a) an alkali-soluble polymer containing a carboxyl group, (b) an addition-polymerizable monomer, and (c) a photopolymerization initiator, from the viewpoints of formability of a microchannel device member by photolithography, lamination property between the photosensitive resin laminate and the substrate of the microchannel device, etc. Furthermore, the photosensitive resin composition may contain an epoxy resin such as EPON (registered trademark) SU-8 type resin or bisphenol A novolac epoxy resin, so long as the photosensitive resin composition layer can be formed into a film using the photosensitive resin composition.
[0032] (a) Alkali-soluble polymers containing carboxyl groups (a) The alkali-soluble polymer containing a carboxyl group has an α,β-unsaturated carboxyl group-containing monomer as a polymerization component, and the acid equivalent of the alkali-soluble polymer is preferably 100 to 600 and the weight average molecular weight is preferably 5,000 to 500,000. The carboxyl group in the alkali-soluble polymer containing a carboxyl group is necessary for the photosensitive resin composition to have developability or strippability with respect to a developer or stripper consisting of an alkaline aqueous solution. The acid equivalent refers to the mass of the alkali-soluble polymer having one equivalent of a carboxyl group therein. The more preferred lower limit of the acid equivalent is 250, and the more preferred upper limit is 450. The acid equivalent of (a) the alkali-soluble polymer containing a carboxyl group is preferably 100 or more from the viewpoints of improving development resistance, improving resolution and adhesion between the cured product of the photosensitive resin composition layer (also referred to as "cured resist film" in this disclosure) and other members, and further ensuring compatibility with the solvent or other components in the photosensitive resin composition, particularly the (b) addition polymerizable monomer described below, and is preferably 600 or less from the viewpoint of improving developability and peelability. The acid equivalent is measured by potentiometric titration using 0.1 mol / L sodium hydroxide using a Hiranuma automatic titrator (COM-555) manufactured by Hiranuma Sangyo Co., Ltd.
[0033] The weight average molecular weight of the (a) alkali-soluble polymer containing a carboxyl group is preferably 5,000 to 500,000. The weight average molecular weight is preferably 5,000 or more from the viewpoint of improving the fluid resistance of the photosensitive resin laminate, suppressing air from entering the microchannel during lamination, and obtaining resistance to the developer by making the thickness of the photosensitive resin laminate uniform, and is preferably 500,000 or less from the viewpoint of maintaining developability. In order to achieve both fluid resistance and developability, the lower limit of the weight average molecular weight of the (a) alkali-soluble polymer containing a carboxyl group is more preferably 20,000 or more or 40,000 or more, and the upper limit is more preferably 250,000 or less, 200,000 or less, 150,000 or less, or 100,000 or less.
[0034] The weight average molecular weight in this specification means a weight average molecular weight measured by gel permeation chromatography (GPC) using a calibration curve of polystyrene (Shodex STANDARD SM-105 manufactured by Showa Denko K.K.). (a) The weight average molecular weight of an alkali-soluble polymer containing a carboxyl group can be measured using a gel permeation chromatography manufactured by JASCO Corporation under the following conditions: Differential Refractometer: RI-1530 Pump: PU-1580 Degasser: DG-980-50 Column oven: CO-1560 Columns: KF-8025, KF-806M x 2, KF-807 Eluent: THF.
[0035] The (a) alkali-soluble polymer containing a carboxyl group is preferably a (co)polymer containing, as a component, one or more monomers selected from the first and second monomers described below.
[0036] The first monomer is a carboxylic acid or an acid anhydride having one polymerizable unsaturated group in the molecule. Examples include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, maleic anhydride, and maleic acid half ester. Among them, (meth)acrylic acid is preferred from the viewpoint of alkaline developability.
[0037] The second monomer is a monomer that is non-acidic and has at least one polymerizable unsaturated group in the molecule. Examples of the second monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, esters of vinyl alcohol such as vinyl acetate, (meth)acrylonitrile, styrene, and polymerizable styrene derivatives. Among these, from the viewpoint of resolution of the microchannel pattern, at least one selected from the group consisting of methyl (meth)acrylate, n-butyl (meth)acrylate, styrene, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and benzyl (meth)acrylate is preferred, and styrene is more preferred.
[0038] In this specification, "(meth)acrylic" means "acrylic" and the corresponding "methacrylic", "(meth)acrylate" means "acrylate" and the corresponding "methacrylate", and "(meth)acryloyl" means "acryloyl" and the corresponding "methacryloyl".
[0039] (a) The alkali-soluble polymer containing a carboxyl group can be synthesized by mixing the above-mentioned monomers, diluting the solution with a solvent such as acetone, methyl ethyl ketone, or isopropanol, adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile, and heating and stirring. In some cases, the synthesis is performed while dropping a part of the mixture into the reaction solution. After the reaction is completed, further solvent is added to the reaction product to adjust the concentration to the desired level. As a synthesis method, bulk polymerization, suspension polymerization, or emulsion polymerization may be used in addition to solution polymerization.
[0040] In the (a) alkali-soluble polymer containing a carboxyl group, the copolymerization ratio of the first monomer and the second monomer is preferably 10 to 60 mass % of the first monomer and 40 to 90 mass % of the second monomer, and more preferably 15 to 35 mass % of the first monomer and 65 to 85 mass % of the second monomer.
[0041] More specific examples of the (a) alkali-soluble polymer containing a carboxyl group include a polymer containing methyl methacrylate, methacrylic acid, and styrene as copolymerization components, a polymer containing methyl methacrylate, methacrylic acid, and n-butyl methacrylate as copolymerization components, a polymer containing methacrylic acid, benzyl methacrylate, and styrene as copolymerization components, a polymer containing methacrylic acid and benzyl methacrylate as copolymerization components, and a polymer containing methacrylic acid, 2-ethylhexyl acrylate, 2-hydroxyethyl methacrylate, and styrene as copolymerization components.
[0042] The content of (a) the alkali-soluble polymer containing a carboxyl group in the photosensitive resin composition is preferably 20 to 90 mass %, more preferably 40 to 60 mass %, based on the total solid content of the photosensitive resin composition. The content of (a) the alkali-soluble polymer containing a carboxyl group is preferably 20 mass % or more from the viewpoint of maintaining the resistance of the photosensitive resin composition in photolithography, and is preferably 90 mass % or less from the viewpoint of the flexibility of the photosensitive resin composition before curing and the resist pattern after curing.
[0043] (b) Addition-polymerizable monomer (b) The addition-polymerizable monomer is a compound having at least one polymerizable ethylenically unsaturated bond in the molecule. The ethylenically unsaturated bond is preferably a terminal ethylenically unsaturated group. From the viewpoint of development speed, the addition polymerizable monomer (b) contains a monomer having a structure represented by formula I and having a molecular weight of 200 to 600 in an amount of preferably 50% by mass or more, more preferably 60% by mass, even more preferably 70% by mass or more, and particularly preferably 100% by mass, in the addition polymerizable monomer (b). C-((CH 2 )R 1 )((CH 2 )R 2 )((CH 2 )R 3 )((CH 2 )R 4 ) (Formula I) Here, R 1 ~R 4 refers to a monovalent organic group.
[0044] The monovalent organic group is a -C, -N, -O, -S, or -P bond, and is the -CH 2 - is a group bonded to the -CH group in (Formula I) at the -C, -N, -O, -S, or -P bond of the monovalent organic group. 2 The portion not bonded to the - group may include a saturated aliphatic hydrocarbon group, an unsaturated aliphatic hydrocarbon group, an aromatic group, a heterocyclic group, an ether group, an ester group, an amide group, an imide group, an amino group, a urethane group, a sulfone group, a halogen, an alkylene oxide group, a (meth)acryloyl group, a carboxyl group, a hydroxyl group, etc. In particular, an ethylene oxide group, a propylene oxide group, a butylene oxide group, and a -CH group in (Formula I) bonded to the -CH group through any of these groups. 2 A structure in which a (meth)acryloyl group, a carboxyl group, a hydroxyl group, or the like is bonded to the - group is preferred. The monovalent organic group may have a polyalkylene oxide chain. Examples of the alkylene oxide constituting the polyalkylene oxide chain include polyethylene oxide and polypropylene oxide.
[0045] Furthermore, the monomer having the structure of formula I preferably has a molecular weight of 200 or more from the viewpoint of the tail after development, and 600 or less from the viewpoint of the development speed. Examples include trimethylolpropane triacrylate (molecular weight 296), trimethylolpropane EO-modified triacrylate (e.g., EO 3-mol modified, molecular weight 428), trimethylolpropane trimethacrylate (molecular weight 338), pentaerythritol tetraacrylate (molecular weight 352), pentaerythritol triacrylate (molecular weight 284), pentaerythritol tetramethacrylate (molecular weight 408), pentaerythritol EO-modified tetramethacrylate (e.g., EO 4-mol modified, molecular weight 584), pentaerythritol EO-modified tetraacrylate (e.g., EO 4-mol modified, molecular weight 528), and the like.
[0046] From the viewpoints of high resolution of the microchannel pattern and the shape of the partition walls, it is preferable to use, as the (b) addition-polymerizable monomer, at least one selected from the group consisting of bisphenol A-based (meth)acrylate compounds, polyfunctional monomers, monomers having a repeating unit of alkylene oxide, cyclic monomers, and aromatic monomers.
[0047] In this specification, a bisphenol A-based (meth)acrylate compound is a compound having a (meth)acryloyl group or a carbon-carbon unsaturated double bond derived from a (meth)acryloyl group and a -C derived from bisphenol A. 6 H 4 -C(CH 3 ) 2 -C 6 H 4- group. Specific examples include dimethacrylate of polyethylene glycol having an average of 2 mole units of ethylene oxide added to both ends of bisphenol A (NK Ester BPE-200 manufactured by Shin-Nakamura Chemical Co., Ltd.), dimethacrylate of polyethylene glycol having an average of 5 mole units of ethylene oxide added to both ends of bisphenol A (NK Ester BPE-500 manufactured by Shin-Nakamura Chemical Co., Ltd.), dimethacrylate of polyalkylene glycol having an average of 6 mole units of ethylene oxide and an average of 2 mole units of propylene oxide added to both ends of bisphenol A, and dimethacrylate of polyalkylene glycol having an average of 15 mole units of ethylene oxide and an average of 2 mole units of propylene oxide added to both ends of bisphenol A.
[0048] Examples of the (b) addition polymerizable monomer other than bisphenol A-based (meth)acrylate compounds include 4-nonylphenylheptaethylene glycol dipropylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, phenoxyhexaethylene glycol acrylate, a reaction product of a half-ester compound of phthalic anhydride and 2-hydroxypropyl acrylate with propylene oxide (manufactured by Nippon Shokubai Kagaku, product name OE-A200), dimethacrylate of glycol in which an average of 3 moles of ethylene oxide are further added to both ends of polypropylene glycol to which an average of 12 moles of propylene oxide have been added, and dimethacrylate of polybutylene glycol to which an average of 28 moles of butylene oxide have been added; polyoxyalkylene glycol di(meth)acrylates such as 4-n-octylphenoxypentapropylene glycol acrylate, 1,6-hexanediol (meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate, 2-di(p-hydroxyphenyl)propane di(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri-, tetra-, or penta(meth)acrylate, and trimethylolpropane triglycidyl ether tri(meth)acrylate; 2,2-bis(4-(meth)acryloxypentaethoxyphenyl)propane, 2,2-bis(4-((meth)acryloxypentaethoxy)cyclohexyl)propane; Examples of such polyfunctional (meth)acrylates include those containing a urethane group, such as a urethane compound of hexamethylene diisocyanate and nonapropylene glycol monomethacrylate, dimethacrylates of polyurethane diols synthesized from polybutylene glycol to which an average of 28 moles of butylene oxide has been added and hexamethylene diamine, and polyfunctional (meth)acrylates of isocyanuric acid ester compounds. These may be used alone or in combination of two or more kinds, and may also be used in combination with a bisphenol A-based (meth)acrylate compound.
[0049] The content of the (b) addition polymerizable monomer in the photosensitive resin composition is preferably 5 to 75 mass %, more preferably 15 to 70 mass %, and even more preferably 20 to 55 mass %, based on the total solid content of the photosensitive resin composition. The content of the (b) addition polymerizable monomer is preferably 5 mass % or more from the viewpoints of resolution and adhesion between the cured resist film and other members, and is preferably 75 mass % or less from the viewpoint of flexibility of the cured resist film.
[0050] (c) Photopolymerization initiator (c) As the photopolymerization initiator, any of those commonly used as photopolymerization initiators for photosensitive resins can be used as appropriate, for example, hexaarylbisimidazole (hereinafter also referred to as triarylimidazolyl dimer).
[0051] Examples of triaryl imidazolyl dimers include 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer (hereinafter also referred to as "2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,1'-bisimidazole"), 2,2',5-tris-(o-chlorophenyl)-4-(3,4-dimethoxyphenyl)-4',5'-diphenylimidazolyl dimer, and 2,4-bis-(o-chlorophenyl)-5-(3,4-dimethoxyphenyl)-diphenylimidazolyl dimer; 2,4,5-tris-(o-chlorophenyl)-diphenylimidazolyl dimer, 2-(o-chlorophenyl)-bis-4,5-(3,4-dimethoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2-fluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3-difluoromethylphenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; 2,2'-bis-(2,5-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,6-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,4-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; 2,2'-bis-(2,3,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,4,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer; Examples include 2,2'-bis-(2,3,4,5-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, 2,2'-bis-(2,3,4,6-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer, and 2,2'-bis-(2,3,4,5,6-pentafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-imidazolyl dimer.
[0052] Among them, 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer is preferred because it has a high effect on the resolution and strength of the cured resist film. These may be used alone or in combination of two or more kinds, and may also be used in combination with an acridine compound, a pyrazoline compound, etc. described below.
[0053] (c) As the photopolymerization initiator, an acridine compound or a pyrazoline compound can also be used. Examples of the acridine compound include acridine, 9-phenylacridine, 9-(4-tolyl)acridine, 9-(4-methoxyphenyl)acridine, 9-(4-hydroxyphenyl)acridine, 9-ethylacridine, 9-chloroethylacridine, 9-methoxyacridine, and 9-ethoxyacridine; 9-(4-methylphenyl)acridine, 9-(4-ethylphenyl)acridine, 9-(4-n-propylphenyl)acridine, 9-(4-n-butylphenyl)acridine, 9-(4-tert-butylphenyl)acridine, 9-(4-ethoxyphenyl)acridine, 9-(4-acetylphenyl)acridine, 9-(4-dimethylaminophenyl)acridine, 9-(4-chlorophenyl)acridine; Examples of such acridine include 9-(4-bromophenyl)acridine, 9-(3-methylphenyl)acridine, 9-(3-tert-butylphenyl)acridine, 9-(3-acetylphenyl)acridine, 9-(3-dimethylaminophenyl)acridine, 9-(3-diethylaminophenyl)acridine, 9-(3-chlorophenyl)acridine, 9-(3-bromophenyl)acridine, 9-(2-pyridyl)acridine, 9-(3-pyridyl)acridine, and 9-(4-pyridyl)acridine. Of these, 9-phenylacridine is preferred. The acridine compound is preferably used in combination with a halogen compound in terms of the curing property after exposure of the photosensitive resin layer. Examples of the halogen compound include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzal bromide, methylene bromide, tribromomethylphenylsulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, hexachloroethane, and chlorinated triazine compounds. Among them, tribromomethylphenylsulfone is preferable in terms of the curing property.
[0054] As the pyrazoline compound, 1-phenyl-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-(4-(benzoxazol-2-yl)phenyl)-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-octyl-phenyl)-pyrazoline are preferred.
[0055] Other photopolymerization initiators include, for example, quinones such as 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, 2,3-dimethylanthraquinone, and 3-chloro-2-methylanthraquinone; aromatic ketones such as benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], and 4,4'-bis(diethylamino)benzophenone; benzoin ethers such as benzoin, benzoin ethyl ether, benzoin phenyl ether, methylbenzoin, and ethylbenzoin; Examples of the oxime esters include benzil dimethyl ketal, benzil diethyl ketal, combinations of thioxanthones and alkylaminobenzoic acids, and oxime esters such as 1-phenyl-1,2-propanedione-2-O-benzoin oxime and 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime. In cases where colorless transparency of the microchannel is required or from the viewpoint of suppressing fluorescence emission and facilitating detection of the luminescence signal of the microchannel device, an oxime compound is preferred. Examples thereof include Irgacure OXE01 and Irgacure OXE02 manufactured by BASF Japan Ltd. and ADEKA Arcles NCI-831 manufactured by ADEKA Corporation.
[0056] In addition, the combination of the above-mentioned thioxanthones and alkylaminobenzoic acids includes, for example, a combination of ethylthioxanthones and ethyl dimethylaminobenzoate, a combination of 2-chlorothioxanthones and ethyl dimethylaminobenzoate, and a combination of isopropylthioxanthones and ethyl dimethylaminobenzoate. In addition, N-arylamino acids may be used. Examples of N-arylamino acids include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine. Among them, N-phenylglycine is particularly preferred.
[0057] The content of the (c) photopolymerization initiator in the photosensitive resin composition is preferably within the range of 0.01 to 30 mass% based on the total solid content of the photosensitive resin composition, with a more preferred lower limit of 0.05 mass% or more, an even more preferred lower limit of 0.1 mass% or more, and a more preferred upper limit of 15 mass% or less, and an even more preferred upper limit of 10 mass% or less. The content of the (c) photopolymerization initiator is preferably 0.01 mass% or more from the viewpoint of obtaining sufficient sensitivity during photopolymerization by exposure, and is preferably 30 mass% or less from the viewpoint of sufficiently transmitting light to the bottom surface of the photosensitive resin composition (i.e., the part far from the light source) during photopolymerization, obtaining good resolution and good adhesion between the cured resist film and other members.
[0058] (d) Other additives The photosensitive resin composition may contain various additives in addition to the above components (a) to (c).
[0059] For example, in order to improve the thermal stability and storage stability of the photosensitive resin composition, it is preferable to incorporate at least one compound selected from the group consisting of radical polymerization inhibitors, benzotriazoles, carboxybenzotriazoles, and hindered phenol-based antioxidants in the photosensitive resin composition.
[0060] Examples of the radical polymerization inhibitor include p-methoxyphenol, hydroquinone, pyrogallol, naphthylamine, tert-butylcatechol, cuprous chloride, 2,6-di-tert-butyl-p-cresol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), nitrosophenylhydroxyamine aluminum salt, and diphenylnitrosamine.
[0061] Examples of benzotriazoles include 1,2,3-benzotriazole, 1-chloro-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-tolyltriazole, and bis(N-2-hydroxyethyl)aminomethylene-1,2,3-benzotriazole.
[0062] Examples of carboxybenzotriazoles include 4-carboxy-1,2,3-benzotriazole, 5-carboxy-1,2,3-benzotriazole, (N,N-dibutylamino)carboxybenzotriazole, N-(N,N-di-2-ethylhexyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-hydroxyethyl)aminomethylenecarboxybenzotriazole, and N-(N,N-di-2-ethylhexyl)aminoethylenecarboxybenzotriazole.
[0063] Examples of the hindered phenol-based antioxidant include the IRGANOX series from BASF Japan and the Adeka STAB (AO) series from ADEKA.
[0064] The total amount of radical polymerization inhibitor, benzotriazoles, carboxybenzotriazoles and / or hindered phenol antioxidant is preferably 0.001 to 3 mass% based on the total solid content of the photosensitive resin composition, with a more preferred lower limit of 0.05 mass% or more and a more preferred upper limit of 1 mass% or less. From the viewpoint of imparting storage stability to the photosensitive resin composition, this total amount is preferably 0.001 mass% or more, and from the viewpoint of maintaining sensitivity, preferably 3 mass% or less.
[0065] The photosensitive resin composition may contain a plasticizer as necessary. Examples of the plasticizer include compounds obtained by modifying bisphenol A with polyalkylene oxide. Other examples of the plasticizer include sorbitan derivatives such as polyoxyethylene sorbitan laurate and polyoxyethylene sorbitan oleate, polyalkylene glycols such as polyethylene glycol and polypropylene glycol, phthalic acid esters such as diethyl phthalate, o-toluenesulfonic acid amide, p-toluenesulfonic acid amide, tributyl citrate, triethyl citrate, triethyl acetyl citrate, tri-n-propyl acetyl citrate, and tri-n-butyl acetyl citrate. In particular, it is preferable to use sorbitan derivatives and polyalkylene glycols.
[0066] The content of the plasticizer in the photosensitive resin composition is preferably 1 to 50 mass% based on the total solid content of the photosensitive resin composition, more preferably 3 mass% as the lower limit and 30 mass% as the upper limit. From the viewpoint of suppressing delay in development time and imparting flexibility to the cured film, the content is preferably 1 mass% or more, and from the viewpoint of suppressing insufficient curing, the content is preferably 50 mass% or less.
[0067] In one embodiment, the thickness of the photosensitive resin composition layer is preferably 100 μm or more, more preferably 120 μm or more, and even more preferably 240 μm or more, and may be preferably 720 μm or less, and more preferably 480 μm or less.
[0068] Photosensitive resin composition layer thickness at 30° C., 1% by mass Na 2 CO 3 The development time per 25 μm thickness using the aqueous solution is preferably 15 to 50 seconds / 25 μm, more preferably 20 to 40 seconds / 25 μm, and even more preferably 25 to 35 seconds / 25 μm. The above-mentioned development time is as shown below. First, a photosensitive resin laminate having a photosensitive resin layer thickness of 25 μm is prepared by the method described in the Example of this specification <Preparation of photosensitive resin laminate 2>. Next, a copper-clad laminate having a plate thickness of 1.2 mm, copper foil of 35 μm, length of 150 mm, and width of 250 mm is laminated by a normal pressure laminator (VA-400III manufactured by Taisei Laminator Co., Ltd.) at a speed of 0.2 m / min, a cylinder pressure of 0.2 MPa, and a roll temperature of 70° C. After peeling off the support film, development is performed using a 1% by mass aqueous sodium carbonate solution at 30° C. using a conveyor-type spray developer, and the minimum time required for removing the photosensitive resin composition layer is defined as the development time.
[0069] <Support film> The support film supports the photosensitive resin composition layer in the form of a film. The support film is preferably one that transmits light with wavelengths of 510 nm and 600 nm and light emitted from an exposure light source. Examples of such support films include polyethylene terephthalate film, polyvinyl alcohol film, polyvinyl chloride film, vinyl chloride copolymer film, polyvinylidene chloride film, vinylidene chloride copolymer film, polymethyl methacrylate copolymer film, polystyrene film, polyacrylonitrile film, styrene copolymer film, polyamide film, and cellulose derivative film. These films may be stretched as necessary. From the viewpoint of resolution, a film with a haze value of 5 or less is preferred. A haze value of 3 or less is more preferred, a haze value of 2.5 or less is even more preferred, and a haze value of 1 or less is even more preferred. The thinner the support film, the more advantageous it is in terms of image forming properties and economic efficiency, but from the viewpoint of the film thickness of the photosensitive resin laminate or the viewpoint of reducing the influence of heat shrinkage during coating of the photosensitive resin composition layer, a film with a haze value of 10 to 30 μm is preferably used. For example, GR-19 and GR-16 manufactured by Teijin Films Limited, R310-16 and R340G16 manufactured by Mitsubishi Plastics, Inc., FB40 (16 μm film thickness) and FB60 (16 μm film thickness) manufactured by Toray Polyester Film Co., Ltd. can be mentioned.
[0070] In one embodiment, the adhesion strength between the support film and the photosensitive resin composition layer is 3 gf / inch or more from the viewpoint of easy handling without peeling when the photosensitive resin laminate is slit and laminated on a substrate. In addition, from the viewpoint of suppressing the occurrence of peeling lines when peeling the support film after exposure, it is 100 gf / inch or less, preferably 80 gf / inch or less, more preferably 50 gf / inch or less, and even more preferably 30 gf / inch or less. For example, the adhesion strength can be designed to be small by increasing the ratio of the alkali-soluble polymer in the photosensitive resin composition, increasing the weight average molecular weight of the alkali-soluble polymer, increasing the constituent ratio of the first monomer in the alkali-soluble resin, reducing the proportion of the addition polymerizable monomer with a relatively low viscosity in the photosensitive resin composition, etc. The peeling line is a minute step on the surface of the photosensitive resin composition layer after peeling off the support film, which occurs when the adhesion between the support film and the photosensitive resin composition layer is excessively high. Usually, the peeling line occurs in a direction approximately perpendicular to the peeling direction. Since the peeling line can cause non-uniformity in the film thickness of the photosensitive resin composition layer and lead to non-uniformity in the volume of the fluid held in the microchannel, it is desirable to suppress the occurrence of the peeling line. The above adhesion strength is a value measured under the conditions described in the [Example] section of this disclosure (i.e., the value at a peel angle of 180 degrees).
[0071] In one embodiment, the photosensitive resin laminate of the present embodiment is preferably combined with a protective film. In one embodiment, the protective film may be disposed on the photosensitive resin composition layer. The protective film may be any film as long as the protective film has a smaller adhesion to the photosensitive resin composition layer than the support film and is peelable. For example, a polyethylene film, a polypropylene film, an oriented polypropylene film, or the like can be used as the protective film. In addition, a film having excellent peelability, such as that disclosed in JP-A-59-202457, can be used. The protective film is preferably a polypropylene film or a plastic film that has been subjected to a release treatment, from the viewpoint of good peelability, from the viewpoint of being peeled off from the photosensitive resin laminate when forming a microchannel device.
[0072] The thickness of the protective film is preferably 10 to 100 μm, more preferably 10 to 50 μm, from the viewpoint of the thickness and dimensional stability of the laminate of the photosensitive resin laminate and the protective film. Specific examples of the protective film include release-treated PET film 25X (thickness 25 μm) manufactured by Lintec Corporation, and GF-18, GF-818, and GF-858 manufactured by Tamapoly Co., Ltd.
[0073] <Method for producing photosensitive resin laminate> A known method can be used as a method for producing the photosensitive resin laminate. For example, the photosensitive resin composition constituting the photosensitive resin composition layer is mixed with a solvent to prepare a photosensitive resin composition preparation liquid, which is then applied to a support film using a bar coater or roll coater and dried, and a photosensitive resin composition layer made of the photosensitive resin composition is laminated on the support film to obtain the photosensitive resin laminate. If desired, a protective film may be further laminated on the photosensitive resin composition layer.
[0074] The photosensitive resin composition preparation is preferably prepared by adding a solvent so that the viscosity of the preparation is 500 to 4000 mPa·sec at 25° C. The solvent may be methyl ethyl ketone, acetone, ethanol, methanol, propanol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, toluene, or the like, and may be appropriately selected from the viewpoints of the viscosity, drying property, amount of remaining solvent, coatability, or foamability of the photosensitive resin composition preparation.
[0075] The photosensitive resin laminate can be used in a roll state by being wound around a core, optionally laminated with a protective film. The photosensitive resin laminate can be covered with a light-shielding sheet such as a polyethylene film from the viewpoint of suppressing adhesion of foreign matter and light exposure during storage or transportation.
[0076] [Microfluidic device and its manufacturing method] The photosensitive resin laminate for microchannel devices of the present embodiment can be used as a component of various microchannel devices such as a POCT (Point of Care Testing) kit, an ELISA (Enzyme-Linked ImmunoSorbent Assay) device, and a microreactor. In one aspect, the microchannel device includes a substrate having a microchannel formed on its surface through which a fluid (liquid or gas) passes, a cover material arranged to cover the microchannel, an inlet for introducing the fluid into the microchannel, and an outlet for discharging the fluid from the microchannel. The substrate may be made of an inorganic material (e.g., silicon, glass, carbon material, etc.) or an organic material (e.g., various polymers). In one aspect, the fluid may be delivered to a desired position in the device by a pump, centrifugal force, or the like. In one aspect, the microchannel is formed by a partition material arranged on the substrate (e.g., a partition material that is a cured resist film formed on the substrate by photolithography). In one aspect, the microchannel is formed by cutting a groove-shaped portion of the substrate surface.
[0077] In a typical embodiment, the photosensitive resin laminate of the present embodiment is included in the microchannel device as a permanent film after exposure. In one embodiment, after exposure of the photosensitive resin composition layer, the support film is removed and only the cured resist film is included in the microchannel device. In another embodiment, after exposure of the photosensitive resin composition layer, the support film is not removed and the support film and the cured resist film are included in the microchannel device.
[0078] The size of the microchannel is selected depending on the purpose, and may be, for example, a width of 1 to 1000 μm, or 1 to 100 μm, or 10 to 70 μm, and a depth of 1 to 50 μm, or 5 to 30 μm. In one embodiment, the bottom and side surfaces of the microchannel are both flat and may form an approximately right angle, but the shape of the microchannel is not limited thereto and may be designed depending on the purpose.
[0079] According to the photosensitive resin laminate of this embodiment, a member having a complex shape can be formed with excellent dimensional accuracy and good fluid resistance and crack resistance. Therefore, the photosensitive resin laminate of this embodiment is particularly useful as a partition material for a microchannel. In particular, in a device configured to deliver a fluid to a desired position using centrifugal force (see, for example, the above-mentioned Patent Document 1 (JP Patent Publication No. 2017-122618)), the shape of the microchannel tends to be complex, so the photosensitive resin laminate of this embodiment can be particularly suitably applied to the partition material of the microchannel in such a device. In addition, the photosensitive resin laminate of this embodiment can be advantageously applied to the cover material of the microchannel due to its good fluid resistance and crack resistance. In any application, the good detectability during fluorescence detection obtained by the photosensitive resin laminate of this embodiment is advantageous for highly accurate detection of a target substance.
[0080] The method for producing the microchannel device is not particularly limited, and the microchannel device can be produced, for example, by a method including a step of forming a microchannel on a substrate and a step of laminating a cover material on the microchannel to seal the microchannel. For example, when the photosensitive resin laminate of the present embodiment is used as a partition wall material and a cover material, the microchannel device can be produced, for example, by a microchannel forming step of laminating a photosensitive resin laminate on a substrate, and forming a cured resist film as a partition material for the microchannel by pattern exposure and development of the photosensitive resin composition layer; a microchannel sealing step of laminating a photosensitive resin laminate on at least the partition material so as to cover the microchannel, and forming a cured resist film as a cover material for the microchannel by exposure to light over the entire surface; The method can be produced by a method comprising the steps of:
[0081] In the microchannel forming step, the photosensitive resin laminate is laminated onto a substrate with the photosensitive resin composition layer side facing the substrate, and exposed to light (preferably by direct exposure) in a pattern corresponding to the desired shape of the partition material. The support film is then removed and developed to form a plurality of partition materials each composed of a cured resist film and defining a microchannel.
[0082] Next, in the microchannel sealing step, the photosensitive resin laminate is laminated at least on the partition material so as to cover the microchannel, with the photosensitive resin composition layer side facing the partition material, and exposed to light over the entire surface, typically without removing the support film, to form a lid material composed of the support film and the cured resist film.
[0083] The lamination of the photosensitive resin laminate is preferably carried out under reduced pressure, more preferably at a vacuum degree of 30 to 70 Pa, and even more preferably at a vacuum degree of 40 to 60 Pa, from the viewpoint of forming a cured resist film with good dimensional accuracy.
[0084] When forming a cured resist film having a multi-layer structure, lamination of a single photosensitive resin composition layer, exposure and development may be repeated several times, or multiple photosensitive resin composition layers may be laminated in advance and then exposed at once. The batch exposure is preferred in that a cured resist film having excellent dimensional accuracy (i.e., little misalignment between layers) can be formed.
[0085] The photosensitive resin laminate according to this embodiment is particularly suitable for use as a partition material and / or a cover material for a compact disc (CD) type microfluidic device for ELISA. An example of the configuration of a CD type ELISA device will be described below.
[0086] In the CD-type ELISA device according to the exemplary embodiment, a liquid tank for storing a liquid, an analysis section for detecting, reacting, adsorbing, desorbing or decomposing the liquid, and a microchannel for connecting the liquid tank and the analysis section and flowing the liquid between them are formed on a disk-shaped substrate (as a base material), and the microchannel is sealed with a lid. In the exemplary embodiment, the diameter of the substrate is about 10 cm, the minimum flow width of the microchannel is about 45 μm, and the depth of the microchannel is about 30 μm. The number of analysis sections on the substrate is, for example, 4 to 20, or 14 to 16. The liquid is sent from the center to the outside in the radial direction by utilizing the centrifugal force caused by the rotation of the substrate, and is supplied to each analysis section from the liquid tank through the microchannel.
[0087] The substrate may be made of either a light-transmitting material or a light-non-transmitting material, and is preferably made of a light-transmitting material such as resin or glass, and more preferably made of resin. Note that the term "light-transmitting" is broadly interpreted as meaning that light can pass through it, regardless of whether it is colored or colorless and regardless of the degree of light transmittance.
[0088] Examples of resins constituting the substrate include acrylic resin, polypropylene, polycarbonate resin, cycloolefin resin, polystyrene resin, polyester resin, urethane resin, vinyl chloride resin, silicone resin, and fluorine-based resin, from the viewpoint of suitability for forming a microchannel.
[0089] In an exemplary embodiment, the method for producing a CD-type ELISA device comprises the following steps: (1) forming a plurality of partitions on a substrate to form a microchannel; (2) providing a through hole in the substrate; (3) fitting an analysis unit through the through-hole from the rear side of the substrate; (4) a step of laminating a lid material from the front side of the substrate; (5) If desired, a step of partially cutting the substrate on which the microchannel is formed to adjust the outer shape; and (6) optionally, washing the septum; The order of each step can be freely changed depending on the efficiency of the manufacturing process.
[0090] When step (1) is carried out by photolithography, a protective film (if present) is peeled off from the photosensitive resin laminate (when the photosensitive resin laminate of the present embodiment is used for a partition wall material, this photosensitive resin laminate), and the support film is maintained while being laminated onto a substrate, followed by exposure and development, and then the support film is removed, thereby forming a plurality of partition wall materials that define microchannels.
[0091] Furthermore, when step (4) is performed by photolithography, the photosensitive resin laminate (when the photosensitive resin laminate of the present embodiment is used for a lid material, this photosensitive resin laminate) can be laminated onto a substrate and cured by exposure to form a permanent film consisting of a support film and a cured resist film. Specifically, the protective film (if present) is peeled off from the photosensitive resin laminate, and the support film is maintained, and lamination can be performed at about 0.18 m / min by a biaxial roll in the stacking order of the support film, the photosensitive resin composition layer, the CD-type ELISA device substrate, the CD-type ELISA device analysis part, and a jig that aligns the surface irregularities of the ELISA substrate on a single plane as necessary. The aforementioned jig is preferably made of a material that has low adhesion to the resist even during lamination, such as Teflon (registered trademark). EXAMPLES
[0092] Hereinafter, examples of the embodiments of the present invention will be described in detail. First, the method for preparing the evaluation samples of the examples and comparative examples is described, and then the evaluation method and the evaluation results for the obtained samples are shown. Tables 1 to 3 show the names of the material components in the photosensitive resin composition preparation, the blending amounts in the resin composition preparation (parts by mass based on the solid content), and some of the evaluation results.
[0093] [Preparation of evaluation samples] The evaluation samples in the examples and comparative examples were prepared as follows. <Preparation of photosensitive resin laminate 1> The photosensitive resin composition having the composition shown in Example 1 and Example 6 in Table 1 below (where the number of each component indicates the amount (parts by mass) of solid content) and ethanol as a solvent were added and thoroughly stirred and mixed to obtain a photosensitive resin composition preparation liquid, which was uniformly applied to the surface of a 16 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., FB40) as a support using a bar coater and dried to form a photosensitive resin composition layer, thereby obtaining a photosensitive resin laminate. The thickness of the photosensitive resin composition layer was 240 μm. The solvent remaining in the photosensitive resin composition layer was 1.5 mass %. Next, GF-18 manufactured by Tamapoly Co., Ltd. was attached as a protective film to the surface of the photosensitive resin composition layer on which the polyethylene terephthalate film was not laminated.
[0094] <Preparation of photosensitive resin laminate 2> A photosensitive resin composition having the composition shown in Examples 2 to 5 and Comparative Examples 1 and 2 in Table 1 below (where the number for each component indicates the amount (parts by mass) of solid content) and ethanol as a solvent were added and thoroughly stirred and mixed to prepare a photosensitive resin composition preparation liquid, which was uniformly applied to the surface of a 16 μm-thick polyethylene terephthalate film (Toray Industries, Inc., FB40) as a support using a bar coater and dried at 95° C. for 5 minutes to form a photosensitive resin composition layer, thereby obtaining a photosensitive resin laminate. The thickness of the photosensitive resin composition layer was 25 μm. Next, GF-818 manufactured by Tamapoly Co., Ltd. was attached as a protective film to the surface of the photosensitive resin composition layer on which the polyethylene terephthalate film was not laminated.
[0095] <Preparation of photosensitive resin laminate 3> The photosensitive resin composition having the composition shown in Examples 1 to 5 and Comparative Examples 1 and 2 in Table 1 below (wherein the number of each component indicates the amount of solid content (parts by mass)) and ethanol as a solvent were added and thoroughly stirred and mixed to obtain a photosensitive resin composition preparation liquid, which was uniformly applied to the surface of a 16 μm thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., FB40) as a support using a bar coater and dried at 95° C. for 5 minutes to form a photosensitive resin composition layer, thereby obtaining a photosensitive resin laminate. The thickness of the photosensitive resin composition layer was 5 μm. Next, GF-18 manufactured by Tamapoly Co., Ltd. was attached as a protective film to the surface of the photosensitive resin composition layer on which the polyethylene terephthalate film was not laminated.
[0096] [evaluation] 1. Calculating the ratio (I / O) Based on the composition shown in Table 1, the ratio (I / O) of the photosensitive resin composition for each example was calculated from the inorganic value (I) and organic value (O) of the base resin (B) and monomer (M) as follows. First, for each base resin (B), calculate the inorganic value (I) based on the organic conceptual diagram, and multiply it by the blending amount (mass) shown in Table 1 to obtain B (I×配合量) The organic value (O) is calculated and multiplied by the amount of the compound to obtain B (O×配合量) Calculate the value. Similarly, for each monomer (M), calculate the inorganic value (I) based on the organic conceptual diagram, and multiply it by the blending amount shown in Table 1 to obtain M (I×配合量) The organic value (O) is calculated and multiplied by the amount of the compound to obtain M (O×配合量) Calculate the value. All base resins (B) (I×配合量) The sum of the values and the M of all monomers (M) (I×配合量) Add the sum of the values and get the sum I (B+M) get. All base resins (B) (O×配合量) The sum of the values and the M of all monomers (M) (O×配合量) Add the sum of the values and get the total value O (B+M) get. I (B+M) O (B+M) Divide by I (B+M) / O (B+M) Calculate the ratio (I / O).
[0097] 2. Transmittance Measurement The photosensitive resin laminate obtained in the above <Preparation of photosensitive resin laminate 3> was exposed to 500 mJ / cm 2 using an exposure machine HMW-201KB manufactured by Oak Manufacturing Co., Ltd. while the protective film was laminated thereon. 2 After 10 minutes of exposure, the protective film was peeled off, and the transmittance was measured using a spectrophotometer U-3010 manufactured by Hitachi High-Tech Science Corp. The analysis was performed in a state in which the support film and the photosensitive resin composition layer were laminated, and the measurement was performed in a state in which the analysis light was incident from the photosensitive resin composition layer side.
[0098] 3. Elastic Modulus Measurement The photosensitive resin laminate obtained in the above <Preparation of photosensitive resin laminate 2> was exposed to 500 mJ / cm 2 using an exposure machine HMW-201KB manufactured by Oak Manufacturing Co., Ltd. while the protective film was laminated thereon. 2After exposure and peeling off the protective film, the film was developed for twice the minimum development time to prepare a test piece measuring 5 cm in length and 5 mm in width. The test piece was stored for one day in an environment of 23°C and 50% relative humidity while peeled off from the support film. A tensile test was performed on the test piece at a pulling speed of 100 mm / min using a tensile tester Tensilon RTM-500 manufactured by A&D Co., Ltd. The elastic modulus of the cured product of the photosensitive resin composition layer was calculated from the initial gradient of the obtained stress-strain curve. The elongation at which the test piece broke was calculated as the elongation of the test piece.
[0099] 4. Microchannel Luminescence Detectability Evaluation The protective film was peeled off from the photosensitive resin laminate obtained in <Preparation of photosensitive resin laminate 3> above. An acrylic resin microchannel was produced by injection molding, with one side of the channel having a width of 70 μm, a depth of 30 μm and a length of 2.5 mm connected to a circular through-hole with a diameter of 5 mm. Nine channels were arranged in one set, and 15 sets were radially arranged on a circular substrate. Using a vacuum laminator manufactured by Takatori Co., Ltd., the photosensitive resin laminate shown in Table 1 was attached to the microchannel at a vacuum degree of 50 Pa and 70°C. After attachment, the laminate was exposed to light at 500 mJ / cm using an exposure machine HMW-201KB manufactured by Oak Seisakusho Co., Ltd. 2 The light was then exposed to light and the seal was completed. TM Luminescence experiments were carried out using West Femto. Microchannel luminescence detectability was ranked as follows: ◎: Luminescence detection is possible without any problems. ○: The emission contrast is affected and the detection sensitivity is reduced. △: The emission contrast is significantly affected, resulting in reduced detection sensitivity. ×: No luminescence was detected.
[0100] 5. Water Resistance Evaluation of Microchannels The microchannel was sealed in the same manner as in "4. Evaluation of Microchannel Luminescence Detectability" above, to prepare a microchannel. Ion-exchanged water was introduced into the microchannel, and the state of the cured product of the photosensitive resin composition layer was observed after 1 hour. The water resistance was ranked as follows: : No wrinkles are visible. ○: Wrinkles are observed around the circular through-hole. △: Wrinkles are observed in some parts of the flow path. ×: Wrinkles are observed throughout the entire flow channel.
[0101] 6. Fabrication of Microchannel Patterns <Fabrication of microchannel pattern 1> The protective film was peeled off from the photosensitive resin laminate obtained in the above <Preparation of Photosensitive Resin Laminate 1>, and the laminate was laminated twice on a 6-inch silicon wafer using a normal pressure laminator (VA-400III manufactured by Taisei Laminator Co., Ltd.) at a speed of 0.2 m / min, a cylinder pressure of 0.2 MPa, and a roll temperature of 70°C, to laminate a 480 μm-thick photosensitive resin composition layer and a support film on the 6-inch silicon wafer.
[0102] Next, using Nuvogo fine 10 manufactured by Orbotech Japan, 1 J / cm 2 The photosensitive resin composition layer was exposed to light with a ratio of 0-100% ih light to expose a flow path pattern, and then the support film was peeled off, and the layer was developed at 30°C using a 1% by mass aqueous sodium carbonate solution for 1.5 times the minimum development time using a conveyor-type spray developer, washed with water, and dried to obtain a flow path pattern. FIG. 1 is a diagram showing a flow path pattern formed in the example, where the area inside the frame of the pattern is an unexposed area, and the area outside the frame is an exposed area. A plurality of flow path patterns 1 are arranged in a circular arc shape in the silicon wafer, with an inlet 11 in the center direction of the silicon wafer, a waste liquid section 12 in the circumferential direction, and a weighing section 13 between the inlet 11 and the waste liquid section 12. The weighing section 13 is composed of a plurality of weighing microflow paths having a flow path long side (a), a flow path short side (b), a flow path width (c), and a partition width (d) as shown in FIG. 1.
[0103] <Fabrication of microchannel pattern 2> Furthermore, a photosensitive resin laminate was prepared by a method conforming to <Preparation of photosensitive resin laminate 1> with the composition and film thickness shown in Examples 7 to 12 in Table 3, and a trapezoidal weighing microchannel was prepared by a method conforming to the above <Preparation of microchannel pattern 1> with the channel depth, channel long side (a), channel short side (b) and channel width (c) shown in Examples 7 to 12 in Table 3. However, a circular acrylic plate was used as the base material. When the film thickness of the photosensitive resin layer of the photosensitive resin laminate was small, an acrylic plate with a large diameter was required to arrange 96 channels. In addition, when the development time per 25 μm was long, long development time was required, and productivity tended to be low.
[0104] Next, 10 μL of pure water was injected from the injection port, and the pure water was dispensed from the injection port to the weighing parts arranged in a circular shape by rotating with a spin coater. When the film thickness exceeds 100 μm, the development time is 15 to 50 seconds / 25 μm, and the photosensitive resin layer has a composition as in Example 1, it is possible to obtain a microchannel substrate with good liquid delivery control, a small substrate area, and high productivity.
[0105] 7.Mandrel Evaluation <Preparation of photosensitive resin laminate 2> The protective film was peeled off from the photosensitive resin laminate prepared using the photosensitive resin composition of Examples 2 to 5, and the laminate was laminated onto a copper-clad laminate for flexible printed wiring boards (NIKAFLEX F-30VC1 25RC11(H) manufactured by Nikkan Industries Co., Ltd.), and exposed to 500 mJ / cm 2 using an exposure machine HMW-201KB manufactured by Oak Manufacturing Co., Ltd. 2 The film was exposed to light and developed for twice the minimum development time to produce a test piece 42 mm wide and 20 cm long. This was then conditioned for one day at 23°C and 50% relative humidity, and a bending test was carried out using a cylindrical mandrel testing machine. The minimum mandrel value for which no cracks occurred was taken as the mandrel evaluation value. The results were ranked as follows. The better this value, the more flexible the microchannels that can be produced. ◎:3mmφ or less 〇: More than 3mmφ and less than 6mmφ △: More than 6mmφ and less than 10mmφ ×: Exceeds 10mmφ.
[0106] 8. Support film adhesion strength evaluation <Preparation of photosensitive resin laminate 3> The protective film was peeled off from the photosensitive resin laminate 20cm x 20cm prepared with the photosensitive resin composition composition of Examples 1 to 6 and Comparative Examples 1 and 2, and laminated to a jet scrubbed copper clad laminate 20cm x 10cm so that a film of 20cm x 10cm was left over. Then, the photosensitive resin laminate was cut into a 1-inch-wide strip with a cutter so as to straddle the part laminated to the copper clad laminate and the remaining part of the film. In this way, a strip-shaped sample of 1 inch width was obtained, with only half of it laminated on the copper clad laminate. Then, the sample was conditioned for one day in an environment of 23°C and 50% relative humidity, and the unlaminated part of the strip-shaped sample was held and subjected to a tensile test to evaluate the adhesion strength between the support film and the photosensitive resin composition layer. The tensile test was performed using a Tensilon RTM-500 tensile tester manufactured by A&D Co., Ltd., with a peel angle of 180 degrees and a pulling speed of 100 m / min. The maximum value of the adhesion strength was taken as the adhesion strength value.
[0107] 9. Support film adhesion evaluation In "8. Evaluation of adhesion strength of support film", while preparing the tensile test sample, it was observed whether unnecessary peeling occurred between the support film and the photosensitive resin composition layer. In addition, the surface of the photosensitive resin composition layer after the tensile test was observed to observe the presence or absence of peeling lines. The observation results were ranked as follows. ⊚: Neither unnecessary peeling nor peeling lines were observed. ◯: Either unnecessary peeling or peeling lines were observed. ×: Unnecessary peeling was observed over half or more of the area of the sample, or a peeling line with obvious irregularities was observed.
[0108] [Table 1]
[0109] [Table 2]
[0110] [Table 3] [Explanation of symbols]
[0111] 1 Flow path pattern 11 Inlet 12 Waste liquid section 13 Weighing section (a) Long side of channel (b) Short side of channel (c) Channel width (d) Bulkhead width
Claims
1. A photosensitive resin laminate for a microchannel device, comprising a support film and a photosensitive resin composition layer, the photosensitive resin composition layer is composed of a photosensitive resin composition having a ratio (I / O) of an inorganic value (I) to an organic value (O) of 0.57 or more and 1.0 or less; The thickness of the photosensitive resin composition layer is 120 μm or more and 720 μm or less, In the film thickness of the photosensitive resin composition layer, 30° C., 1% by mass Na 2 CO 3 The development time per 25 μm using an aqueous solution is 16 to 50 seconds / 25 μm. Photosensitive resin laminate for microchannels.
2. 2. The photosensitive resin laminate for a microchannel according to claim 1, which is for direct imaging exposure.
3. 3. The photosensitive resin laminate for a microchannel according to claim 1, wherein the photosensitive resin composition layer has an elastic modulus of 2 GPa or less and a breaking elongation of 30% or more after exposure.
4. The photosensitive resin composition layer is (a) an alkali-soluble polymer having a carboxyl group; (b) an addition polymerizable monomer, and (c) a photopolymerization initiator, Including, The photosensitive resin composition layer is a radical negative type. The photosensitive resin laminate for a microchannel according to any one of claims 1 to 3.
5. The (b) addition polymerizable monomer is represented by the following formula (I): C-((CH 2 )R 1 )((CH 2 )R 2 )((CH 2 )R 3 )((CH 2 )R 4 ) ... (Formula I) (In the formula, R 1 ~R 4 each independently represents a monovalent organic group.
5. The photosensitive resin laminate for a microchannel according to claim 4, wherein the addition polymerizable monomer (b) contains 50% by mass or more of a monomer having a structure represented by the following formula (1) and a molecular weight of 200 to 600.
6. A photosensitive resin laminate for a microchannel described in any one of claims 1 to 5, wherein the film thickness of the photosensitive resin composition layer is 240 μm or more.
Citation Information
Patent Citations
Photosensitive resin composition, photosensitive film, method for manufacturing micro chemical chip using same, and micro chemical chip
JP2007086723A
Permanent resist compositions, cured products thereof, and uses thereof
JP2007522531A
Pattern forming material and pattern forming method
JP2008058636A
Colored curable composition, color filter, method of manufacturing color filter, and liquid crystal display
JP2009288313A
Manufacture of a microfluidic chip package or assembly having separable chips
JP2016529116A