Method for constructing a generative mold of a molded object by stereolithography

The method uses a doctor blade to form a smoothing layer with a uniform thickness greater than the predetermined thickness, addressing the inefficiencies of existing stereolithography methods by reducing cycle times and improving precision in ceramic dental restoration production.

JP7593799B2Active Publication Date: 2024-12-03IVOCLAR VIVADENT AG +1
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2020204095
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-08
Filing Date
2020-12-09
Publication Date
2024-12-03
Estimated Expiration
2040-12-09

AI Technical Summary

Technical Problem

Existing stereolithography methods for constructing ceramic dental restorations are time-consuming due to the need for moving build platforms between different vats and cleaning procedures, especially when using highly viscous materials, which affects precision and efficiency.

Method used

A method involving the use of a doctor blade to form a smoothing layer with a uniform layer thickness greater than the predetermined thickness, allowing for precise and rapid solidification of layers by minimizing the amount of build material displaced during layer thickness setting, and incorporating spatially selective coloring using inkjet printing.

Benefits of technology

This approach reduces cycle times, improves precision, minimizes cleaning complexity, and ensures accurate layer thicknesses, even with highly viscous materials, while allowing for aesthetically pleasing and precise dental restoration production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593799000001
    Figure 0007593799000001
  • Figure 0007593799000002
    Figure 0007593799000002
  • Figure 0007593799000003
    Figure 0007593799000003
Patent Text Reader

Abstract

To provide a method for constructing a molded body by the layered solidification of a photopolymerization construction material using stereolithography.SOLUTION: Regarding a method for constructing a molded body by the layered solidification of a photopolymerization construction material using stereolithography, in this method, a) a construction material is dispensed onto the planar transparent bottom of a vat 2, and b) the vat 2 is moved in a direction parallel to the flat face of a vat bottom 3 to a doctor blade 4, the doctor blade is suspended using adjustable positioning to the upper part of the vat bottom 3, thus the dispensed construction material is moved below the doctor blade 4 to form a smoothed layer 20 with a uniform layer thickness pre-determined by the positioning of the doctor blade 4 to the vat bottom.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for the generative building of shaped bodies by layer-by-layer solidification of a viscous photopolymerizable build material using stereolithography. [Background technology]

[0002] The build material can be an organic-based ceramic slurry, i.e., a flowable photopolymerized material filled with ceramic particles whose viscosity increases with increasing amount of ceramic particles, or it can consist of a highly viscous photocurable composite or photopolymer. When using a ceramic slurry as the build material, a green body is produced as a molded body, which is then further processed into a ceramic body by debinding and sintering. The present invention is particularly applicable in the field of dental restoration production.

[0003] To achieve aesthetically pleasing results for dental restorations, it is often desirable to use different build materials in a position-dependent manner and / or different colorants in a location-dependent manner. In conventional stereolithography processes for layer-by-layer accumulation of green bodies from ceramic slurries, it is known that the body being built is moved out of the build zone after the current layer solidifies, and a pigmented photopolymer is selectively applied to the last hardened layer using an inkjet printing method. Such a process is known, for example, from WO 2013 / 182547 A1, in which a drum-shaped carrier is used on which four build platforms are arranged around its circumference at 90° intervals relative to each other. Work stations are also distributed around the drum-shaped carrier at 90° intervals. Between the work stations are a vat with a transparent bottom under which an exposure unit is located, an inkjet printer for printing a pigment-filled photopolymer on the last cured layer, and a further exposure unit for solidifying the spatially selectively imprinted pigment-filled photopolymer. The drum-shaped carrier is mounted so that each of the build platforms is rotatable so that it is located within and processed in one of the work stations. After completion of a work step at each work station, the drum-shaped carrier is rotated 90° on the respective part of the build platform so that the next work step can be performed in the next work station. In this process, work steps can be performed in parallel on several parts of the build platform, but the process is very time-consuming, with much time being spent mechanically moving the build platform between the work stations.

[0004] Alternatively, different materials can be used to form the layers, which are kept ready in different vats. The build platform is then subsequently lowered into the different vats to successively solidify sub-areas of the layer to be cured with the different build materials in the different vats. Such a process is described in DE 10 2007 010 624 B4. To avoid cross-contamination (transfer of a quantity of build material into a vat with a different build material), after the build platform is raised with the part suspended thereon, it is necessary to clean the part before the part is lowered into another build material in the next vat. Therefore, after each change of build material, it is necessary to perform a cleaning procedure, which also makes the method time-consuming. In addition, the transport required to change between different vats is also time-consuming.

[0005] DE 10 2011 117 005 B4 relates to a method for producing ceramic dental restorations based on a productive manufacturing method in which a single slurry layer is successively deposited and solidified layer by layer. After depositing the slurry layer, the layer thickness of this layer is reduced by a doctor blade, which also results in a smoothing layer, after which spatially selective deposition of an ink liquid is carried out. In addition to the colorant, this ink also contains an initiator that induces a chemical reaction and causes the solidification of the slurry layer, so that coloring and solidification occur simultaneously.

[0006] US 5,975,323 B2 generally relates to generative 3D printing methods, and also describes generative methods in which a liquid in a vat is solidified in a spatially selective manner by a laser or another energy source. The described methods particularly emphasize that layers are selectively formed on top of each other, where the volume created by the layers on top of each other consists of multiple columns that exist adjacent to each other, each column consisting of multiple voxel elements or voxels (volume pixels) that exist one above the other, and in each column, the coloring / transparency of each of the voxel elements is created in a selected manner. Specific details regarding the individual coloring of single voxel elements and the application of individual colors to each voxel element are not described.

[0007] EP 2 337 667 B1 discloses a method according to the preamble of claim 1. In this method, a viscous photopolymerizable build material is dispensed onto the planar, transparent bottom of a vat. A doctor blade is suspended above the vat bottom with an adjustable positioning. The vat is moved relative to the doctor blade in a direction parallel to the plane of the vat bottom, so that the dispensed build material is forced under and over the doctor blade, thereby forming a smoothing layer having a uniform thickness predetermined by the positioning of the doctor blade relative to the vat bottom. This can be accomplished, for example, by rotating the vat about an axis of rotation perpendicular to the vat bottom so that the vat bottom is moved under a non-rotating doctor blade. The dispensed build material accumulates upstream of the doctor blade, and only a portion of the accumulated build material passes through the gap under the doctor blade, thereby forming the passed build material into a smoothing layer of a predetermined, uniform thickness. The smoothing layer is moved by relative movement of the vat to the area between the exposure unit located below the vat bottom and the build platform suspended above the vat in a height-adjustable manner. The build platform is then lowered relative to the vat bottom in a precisely controlled manner while displacing the build material from the smoothing layer, thereby setting the remaining layers in the clearance between the build platform and the vat bottom to a predetermined layer thickness determined by the distance of the lower surface of the build platform (or the lower surface of the last cured layer) to the vat bottom. In this manner, the predetermined layer thickness can be set with high precision. The layer with the predetermined layer thickness is then solidified by exposure in a spatially selective manner through controlled operation of the exposure unit to result in exposure within the desired contour of the current layer to be solidified. Finally, the build platform is raised, build material is dispensed onto the vat bottom, and the above-described steps are repeated until a molded body is formed by multiple layers selectively solidified on top of each other.

[0008] It is an object of the present invention to provide a method of the type described above that can be carried out in such a manner that it can be carried out quickly and precisely even for highly viscous building materials. It would also be desirable if successive solidified layers of a shaped body could be colored in a spatially selective manner. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2013 / 182547 [Patent Document 2] German Patent No. 10 2007 010 624 [Patent Document 3] German Patent Invention No. 10 2011 117 005 [Patent Document 4] U.S. Patent No. 5,975,323 [Patent Document 5] European Patent No. 2 337 667 Summary of the Invention [Means for solving the problem]

[0010] This object is achieved by a method comprising the features of claim 1. Preferred embodiments are presented in the dependent claims. Therefore, a method for building a molded body by layer-by-layer solidification of a viscous photopolymerizable build material using stereolithography, comprising: a) build material is dispensed onto the flat, transparent bottom of the vat; b) the vat is moved in a direction parallel to the plane of the vat bottom relative to a doctor blade, the doctor blade being suspended with an adjustable positioning above the vat bottom, such that the dispensed build material is moved beneath the doctor blade, thereby forming a smoothed layer having a uniform layer thickness predetermined by the positioning of the doctor blade relative to the vat bottom; c) the smoothing layer is brought into the area between an exposure unit located below the bottom of the vat and a build platform, the height of which is adjustable and suspended above the vat, by relative movement of the vat; d) the build platform is lowered in a controlled manner relative to the vat bottom, thereby displacing the build material while allowing the remaining layer in the gap to build to a predetermined layer thickness; e) the layer is solidified in a spatially selective manner by controlled operation of the exposure unit within the contours desired for the current layer; f) the build platform is then raised, build material is dispensed onto the bottom of the vat, and steps b) to f) are repeated until the compact is built up by multiple layers solidified on top of each other; A method is provided.

[0011] According to the present invention, the positioning of the doctor blade relative to the vat bottom is adjusted so that the resulting predetermined uniform layer thickness is greater than the predetermined layer thickness to be set by lowering the build platform, but does not exceed the predetermined layer thickness by more than 50%. In other words, the build material dispensed onto the vat bottom, by its relative movement with respect to the doctor blade suspended above the vat bottom with adjusted positioning, is already formed into a layer having a predetermined uniform layer thickness that is greater than the predetermined layer thickness to be set by lowering the build platform, but is already close to the predetermined layer thickness (up to 50% higher than the predetermined layer thickness).

[0012] When the layer thickness, as determined by the positioning of the doctor blade relative to the vat bottom, exceeds the predetermined layer thickness as set by the build platform to some extent, this is advantageous because, in any case, even if deviations or tolerances in the definition of the layer thickness predetermined by the doctor blade (especially local shortfalls in the predetermined layer thickness) occur, sufficient build material is present everywhere within the area of ​​the layer to be defined, thereby ensuring that the predetermined layer thickness can still be set everywhere by lowering the build platform. In other words, when the gap to the vat bottom is set to the predetermined layer thickness, sufficient build material is present everywhere so that the lower surface of the build platform (or the lower surface of the last cured layer) over the entire area contacts the build material. For many build materials, especially those with low or medium viscosity values, a predetermined uniform layer thickness can be achieved over the entire area of ​​the layer without any problems. For build materials with higher viscosity values, some variation in the actual layer thickness may exist across the layer area, such that the actual layer thickness value as a function of position within the layer area is effectively a distribution of layer thickness values, with the distribution being very narrow and having a very small full width at half maximum around the average layer thickness. In such cases, the "predetermined uniform layer thickness" is considered to be the average layer thickness of the thickness distribution, and the term "uniform layer thickness" is justified and technically meaningful, since the standard deviation of the thickness distribution is small in any case compared to the average layer thickness. In such cases, it is desirable to set the predetermined uniform (average) layer thickness slightly higher than the desired layer thickness to be set by lowering the build platform, e.g., in practice, by three standard deviations higher than the distribution, so that the build platform will be in contact with the build material at all positions across the layer area when lowered to the desired layer thickness. Alternatively, the predetermined layer thickness may also be closer to the predetermined layer thickness, and compensation for potential variations in layer thickness across the area may be achieved by displacing the build material laterally as the build platform is lowered.

[0013] Due to the fact that the build material is formed by the doctor blade into a layer having a very low, predetermined layer thickness that exceeds the predetermined layer thickness by a maximum of 50%, it is ensured that the predetermined, uniform layer thickness formed by the doctor blade is already close to the predetermined layer thickness to be set by the build platform, and as a result, when the build platform is lowered toward the vat bottom, only a small amount of build material needs to be displaced from the gap. In this regard, when using a highly viscous build material, it must be taken into account that a high force is required to lower the build platform and displace the build material from the remaining gap from which the highly viscous build material needs to be displaced. If the maximum force that can be applied is limited by the vat material (e.g., to avoid breakage or other failure of the vat bottom), the build platform needs to be lowered slowly to limit that force. For this reason, lowering the build platform to set the predetermined layer thickness takes a long time for a highly viscous build material. Conversely, reducing the maximum amount of build material to be displaced shortens the time required for this. As a result of forming the build material dispensed by the doctor blade into a layer of uniform, predetermined thickness up to 150% of the desired layer thickness to be set by the build platform, the strict limitation of the maximum amount of build material to be displaced therefore makes it possible to rapidly set the layer thickness by lowering the build platform, thus allowing for shorter cycle times.

[0014] Setting a predetermined layer thickness with the build platform has the added advantage that a lower separation force is required to lift the build platform after the layer solidifies, compared to a situation in which a larger amount of build material is displaced to set the predetermined layer thickness. When lifting the build platform, the required separation force must overcome negative pressure because the volume created between the undersurface of the part being built and the vat bottom when the build platform is lifted must be filled with inflowing air. With a large amount of displaced build material, this displaced material forms a barrier around the build platform and the part being built, which impedes the flow of ambient air into the growing volume above the vat bottom as the build platform is raised. By minimizing the amount of displaced build material, the inflow of air into the growing volume above the vat bottom is improved, thereby reducing the separation force to lift the build platform.

[0015] If lowering the build platform to set a predetermined layer thickness causes a large amount of build material displacement, this also adversely affects the dimensional accuracy of the part built by stereolithography, especially based on accuracy in the z-direction (the direction perpendicular to the plane of the vat bottom). In a "bottom-up" process, as in the present case, the layer to be solidified is sandwiched between the build platform (or the lower surface of the part being built, if one or more layers have already solidified) and the vat bottom surface. The height of this gap determines the predetermined layer thickness of the layer to be solidified. In this area, the maximum cure depth is determined by the gap height (predetermined layer thickness), even if the penetration depth of light depending on the build material at the selected exposure parameters (intensity and exposure time) causes a deeper cure depth. If the layer currently to be solidified protrudes laterally beyond the last previously solidified layer, the build material displaced during the setting of the layer thickness of the to-be-solidified layer also reaches the portion where the to-be-solidified layer protrudes beyond the last solidified layer, resulting in two large amounts of material and two high layer thicknesses in this laterally protruding portion of the to-be-solidified layer. Because the actual cure depth of the exposure is always greater than the predetermined layer thickness, in these portions, solidification of material occurs beyond the predetermined layer thickness in the z direction in deep regions of the last solidified layer, which can lead to an order of magnitude decrease in accuracy (oversizing) of some layer thicknesses in the z direction. Minimizing displaced build material, or in other words, optimal approximation of the predetermined layer thickness by the doctor blade to the predetermined layer thickness to be set by the build platform, also results in improved accuracy of the part to be built. In general, it is advantageous to keep the amount of displaced build material as small as possible by approximating the predetermined layer thickness, as determined by the doctor blade positioning, to the predetermined layer thickness to be set by the build platform.

[0016] At the end of the build process, there is always some displaced, excess, and uncured build material on the built part. Therefore, the need for a cleaning procedure exists, especially when the part will undergo thermal post-processing steps such as debinding and sintering. In the context of productive manufacturing processes, cleaning procedures are not trivial. For parts with complex geometries, tiny gaps or cavities are accessible to cleaning fluids only under considerable effort. Furthermore, solvents with good ability to remove monomer mixtures can damage the surface of the part under some circumstances, and in the case of suspensions (slurries), particulate filler material can remain on the surface. By keeping the amount of displaced build material during the build process as small as possible, the amount of excess build material that ultimately adheres to the part can also be kept as small as possible, which reduces the complexity of the cleaning procedure. These aspects are even more relevant when parts are built with different materials and the parts are changed between vats with different build materials during the build process, since in such cases a cleaning step would in principle need to be carried out for each material change before the part being built is transferred to the next vat with another build material. In the case of substantial minimization of the amount of build material displaced according to setting the layer thickness, cleaning according to the material change could then be omitted if slight contamination by small amounts of residue of adhesive build material on the part coming into contact with another build material in the next vat is acceptable.

[0017] Preferably, the positioning of the doctor blade relative to the vat bottom is adjusted so that the resulting predetermined uniform layer thickness is within 110-130% of the desired layer thickness to be set by lowering the build platform.

[0018] In a preferred embodiment, relative movement of the batt and doctor blade relative to one another is effected by rotating the batt about an axis of rotation centered on and perpendicular to the batt bottom while keeping the doctor blade suspended in a stationary state, or by rotating the doctor blade about an axis described with respect to the batt being held in a stationary state. In the case of a stationary doctor blade and a rotatable batt, the batt bottom can have the shape of a circular disk with the axis of rotation extending through the center of the disk. The stationary doctor blade has a directional component oriented radially relative to the axis of rotation, extending in a radially outward direction from the point radially closest to the axis of rotation.

[0019] In a preferred embodiment, the positioning of the doctor blade above the vat bottom is defined by a straight line coincident with the lower edge of the doctor blade. This straight line has a minimum distance to the vat bottom at the point where the lower edge of the doctor blade is closest radially to the axis of rotation. The positioning of the straight line is further defined between the straight line and a plane parallel to the vat bottom that is intersected by the straight line, and the slope angle is greater than 0° and less than 15°. A slope angle greater than 0° has the result that the vertical (perpendicular to the vat bottom) distance of the lower edge to the vat bottom increases from the minimum distance at the point where the lower edge is closest radially to the axis of rotation, and increases with increasing radial distance to the axis of rotation.

[0020] The doctor blade may comprise a planar doctor blade defining a plane oriented at an inclination angle relative to the vat bottom, the inclination angle being between 0° and 90°. Preferably, the planar doctor blade is inclined relative to the vat bottom, the inclination angle being preferably in the range of 30° to 75°, and defined relative to the direction of movement between the vat bottom and the doctor blade such that the lower edge of the doctor blade trails behind the upper edge of the doctor blade in the direction of relative movement.

[0021] As an alternative to the relative rotational movement of the vat and the doctor blade, the relative movement of the vat and the doctor blade can also be effected by a linear shift of the vat or a linear shift of the doctor blade. In such an embodiment, the positioning of the doctor blade above the bottom of the vat is desirably defined by a straight line coincident with the lower edge of the doctor blade, the straight line being spaced a fixed distance from the bottom of the vat and extending parallel to the bottom of the vat.

[0022] To ensure that the entire vat bottom is wetted with the build material without voids, and thus coats the vat bottom throughout, it may be useful to match the interfacial tension of the build material and the vat bottom surface. This can be achieved by setting the surface tension of the build material using additives such as antifoaming agents or surfactants and / or by modifying the surface of the vat bottom, for example, by silanization.

[0023] In a preferred embodiment, the surface of the smooth thin layer is colored by location-dependent application of a selected colorant in an intermediate step prior to lowering of the build platform and prior to location-dependent exposure. Preferably, the colorants for matching the color and translucency of the part will depend on the actual construction materials used, as follows: a) In the case of photopolymers as building materials, solutions containing dye molecules and / or suspensions containing pigments b) In the case of slurries containing glass ceramics as building materials, color pigments, in particular oxides, namely tin oxide or zirconium oxide, dispersed in an organic medium. c) In the case of ZrO2 slurries as building materials, solutions of nitrates (aqueous or based on another solvent) or acetylacetonates dissolved in ethanol.

[0024] In a preferred embodiment, the colorant is dissolved and / or dispersed in an ink and applied onto the smoothing layer by inkjet printing methods.

[0025] In a preferred embodiment, the colorant is photocurable or thermocurable and, after spatially selective application onto the smoothing layer, is fixed by electromagnetic radiation, the electromagnetic radiation used for fixing being outside the absorption spectrum of the photoinitiator of the build material.

[0026] In a preferred embodiment, a doctor blade made from polytetrafluoroethylene is used and for the circumferential sidewalls of the batt, sidewalls made from polytetrafluoroethylene are used.

[0027] As vat bottom, preferably a disk made of glass or polymethylmethacrylate (PMMA) is used, onto which an ethylene tetrafluoroethylene film is bonded on its surface facing the vat bottom. For example, the present invention provides the following items. (Item 1) 1. A method for building a molded body by layer-by-layer solidification of a viscous photopolymerized build material using stereolithography, comprising: a) the build material is dispensed onto the flat, transparent bottom of the vat (2); b) the vat (2) is moved in a direction parallel to the plane of the vat bottom (3) relative to a doctor blade (4), the doctor blade being suspended above the vat bottom (3) with an adjustable positioning, so that the dispensed build material is moved under the doctor blade (4), thereby forming a smoothing layer (20) having a uniform layer thickness predetermined by the positioning of the doctor blade (4) relative to the vat bottom (3); c) the smoothing layer (20) is brought into the area between an exposure unit (6) located below the vat bottom (3) and a height-adjustable build platform (8) suspended above the vat by relative movement of the vat (4); d) the build platform (8) is lowered in a controlled manner relative to the vat bottom, thereby displacing the build material while allowing the remaining layer in the gap to be formed to a predetermined layer thickness; e) the layer is solidified in a spatially selective manner by controlled movement of the exposure unit (6) within the contour desired for the current layer; f) the build platform (8) is then raised, build material is dispensed onto the bottom of the vat, and steps b) to f) are repeated until the body is built up by several layers solidified on top of each other; the positioning of the doctor blade (4) relative to the vat bottom (3) is adjusted in such a way that the resulting predetermined uniform layer thickness is higher than the predetermined layer thickness to be set by lowering the build platform (8), but does not exceed the predetermined layer thickness by more than 50%. (Item 2) The method according to the preceding item, characterized in that the position of the doctor blade (4) relative to the vat bottom (3) is adjusted in such a manner that the resulting predetermined uniform layer thickness is within the range of 110% to 130% of the desired layer thickness. (Item 3) 10. The method according to claim 9, wherein the relative movement of the vat (2) and the doctor blade (4) is effected by rotating the vat (2) about a central axis perpendicular to the vat bottom (3) with the doctor blade (4) suspended in a stationary manner, or by rotating the doctor blade (4) about the axis described with respect to the vat (2) in a stationary state. (Item 4) 10. The method according to claim 9, wherein the position of the doctor blade (4) above the vat bottom (3) is defined by a slope angle (α) between a straight line coincident with the lower edge of the doctor blade, the slope angle being defined by the minimum distance to the vat bottom (3) at the point of the linear lower edge of the doctor blade closest to the axis of rotation, and the straight line of the lower edge and a plane parallel to the vat bottom (3) intersected by the straight line, the slope angle being greater than 0° and less than 15° such that the distance of the lower edge to the vat bottom (3) increases from the minimum distance with increasing radial distance to the axis of rotation. (Item 5) 10. The method according to claim 9, wherein the doctor blade (4) comprises a planar blade and is inclined at an inclination angle (κ) relative to the vat bottom (3), the inclination angle (κ) being greater than 0° and less than 90°, preferably in the range of 30° to 75°, and the inclination angle is defined in relation to the direction of relative movement between the vat bottom (3) and the doctor blade (4) in such a way that the lower edge of the doctor blade (4) in the direction of relative movement of the doctor blade (4) relative to the vat bottom follows behind the upper edge of the doctor blade (4). (Item 6) 10. The method according to claim 9, wherein the relative movement of the vat (2) and the doctor blade (4) is effected by linearly shifting the vat (2) or linearly shifting the doctor blade (4). (Item 7) 10. The method according to claim 9, wherein the position of the doctor blade (4) above the vat bottom is defined by the extension of a straight line coinciding with the lower edge of the doctor blade (4), said straight line extending at a constant distance from and parallel to the vat bottom (3). (Item 8) 10. The method according to any one of the preceding items, characterized in that the surface of the smooth thin layer is colored by applying a selected colorant in a spatially selective manner in an intermediate step before the lowering of the build platform (8) and before the spatially selective exposure. (Item 9) The colorant for setting color and translucency is a) in the case of photopolymers as building materials, solutions containing dye molecules and / or suspensions containing pigments; b) in the case of slurries containing glass ceramics as building materials, color pigments, in particular oxides, tin oxide or zirconium oxide, dispersed in an organic medium; c) For ZrO2 slurries as building materials, solutions of nitrates (aqueous or based on another solvent) or acetylacetonates dissolved in ethanol 10. The method according to claim 1, wherein the materials are selected from the group consisting of: (Item 10) Item 10. The method according to any one of the preceding items, characterized in that the colorant is dissolved and / or dispersed in ink and applied in a spatially selective manner onto the smoothing layer by an inkjet printer. (Item 11) The method according to any one of the preceding items, characterized in that the colorant is photocurable or thermocurable and, after spatially selective application onto the smoothing layer, is fixed by electromagnetic radiation, the electromagnetic radiation used for fixing being outside the absorption spectrum of the photoinitiator of the build material. (Item 12) 10. The method according to claim 9, wherein the doctor blade is made of polytetrafluoroethylene and the circumferential side wall of the vat (2) is made of polytetrafluoroethylene. (Item 13) 10. The method according to claim 9, wherein a glass or polymethylmethacrylate plate is used as the bottom of the vat (3), and an ethylene tetrafluoroethylene film is bonded to the surface of the plate facing the bottom of the vat. (Summary) The present invention relates to a method for building a molded body by layer-by-layer solidification of a photopolymerized building material using stereolithography, the method comprising: a) the build material is dispensed onto the flat, transparent bottom of the vat (2); b) the vat (2) is moved in a direction parallel to the plane of the vat bottom (3) relative to a doctor blade (4), the doctor blade being suspended above the vat bottom (3) with an adjustable positioning, so that the dispensed build material is moved under the doctor blade (4) to form a smoothing layer (20) having a uniform layer thickness predetermined by the positioning of the doctor blade (4) relative to the vat bottom; c) the smoothing layer (20) is brought into the area between the exposure unit (6) located below the vat bottom (3) and the build platform (8) whose height is adjustable and suspended above the vat by the relative movement of the vat (4); d) the build platform (8) is lowered in a controlled manner against the bottom of the vat, thereby displacing the build material while allowing the remaining layers in the gap to be built to a predetermined layer thickness; e) the layer is solidified in a spatially selective manner by controlled operation of the exposure unit (6) within the contours desired for the current layer; f) the build platform (8) is raised, the build material is dispensed onto the bottom of the vat, and steps b) to f) are repeated until the body is built up by several layers solidified on top of each other; The positioning of the doctor blade (4) relative to the vat bottom (3) is characterized in that it is adjusted in such a way that the resulting predetermined uniform layer thickness is higher than the predetermined layer thickness to be set by lowering the build platform (8), but does not exceed the predetermined layer thickness by more than 50%. [Brief explanation of the drawings]

[0028] The present invention will now be described with reference to embodiments in the drawings. [Figure 1] FIG. 1 shows a schematic perspective view of the components of an apparatus for carrying out the method according to the invention. [Figure 2] FIG. 2 shows a schematic top view of an apparatus for carrying out the method according to the invention, as well as a sequence of four subsequent steps during the implementation of the method according to the invention. [Figure 3] FIG. 3 shows the corresponding top view as a sequence of four subsequent steps during the implementation of the method according to the invention. [Figure 4] FIG. 4 shows a detailed view in cross section through the vat bottom and doctor blade of an apparatus for carrying out the method according to the invention. [Figure 5] FIG. 5 is a plan view in partial section from plane AA of FIG. 4 of the vat bottom and doctor blade, as well as a top view of these components from above, on the right hand side. [Figure 6] FIG. 6 shows a corresponding view as in FIG. 5 for an alternative embodiment for providing relative movement between the doctor blade and the batt. [Figure 7] FIG. 7 shows a cross-sectional view of a portion of a vat bottom with a smoothed layer of build material thereon. [Figure 8] FIG. 8 shows a cross-sectional view corresponding to FIG. 7, with a portion of the vat bottom moved to a position below the inkjet printer. [Figure 9] Figure 9 shows a cross-sectional view corresponding to Figure 7, with part of the vat bottom already leaving the inkjet printer area and moving towards the build area, with a build platform located above the vat and an exposure unit located below the vat bottom. [Figure 10] FIG. 10 is a cross-sectional view corresponding to FIG. 7, where a portion of the vat bottom has been moved into the build area below the build platform. [Figure 11]FIG. 11 is a cross-sectional view corresponding to FIG. 10 after lowering the build platform and during exposure of a defined layer of build material with applied colorant. [Figure 12] FIG. 12 is a cross-sectional view corresponding to FIGS. 10 and 11 after completion of exposure and elevation of the build platform. DETAILED DESCRIPTION OF THE INVENTION

[0029] 1 shows a schematic, highly simplified perspective view of the essential components of an apparatus for carrying out the method according to the invention. The apparatus comprises a rotatable vat 2, which for reasons of simplicity is shown as a vat bottom 3 in the form of a circular disk without the side walls that actually surround the circular disk. Vat bottom 3 is transparent, at least in the area where an exposure unit 6 can expose the build area. Opposite exposure unit 6, a vertically movable build platform 8 is arranged above vat bottom 2. A part 10 under construction is suspended above build platform 10.

[0030] A doctor blade 4 is suspended above the vat bottom 3 in an adjustable position. The vat 2 is rotatable about a vertically extending axis of rotation extending from the center of the circular disk of the horizontal vat bottom 3. A rotary drive (not shown) is provided that rotates the vat 2 under the control of a control unit (not shown) and stops the vat at a position determined by the control unit. A dispensing device (not shown in FIG. 1 ) for the viscous build material is arranged upstream of the doctor blade 4 in the direction opposite to the rotation of the vat 2, indicated by the arrow, and dispenses the viscous build material. This may be, for example, a cartridge, and a driven piston may deliver the build material from the cartridge through an output outlet. Due to the rotation of the vat 2, the build material accumulates in front of the doctor blade 4. Due to the rotation of the vat 2, a portion of the dispensed build material is moved below and past the doctor blade 4, thereby forming a smoothing layer 20 with a predetermined, uniform layer thickness determined by the positioning of the doctor blade 4 relative to the vat bottom 3.

[0031] An inkjet printer 12 is movably supported above the vat 2, displaced approximately 90° circumferentially relative to the doctor blade 4. The inkjet printer 12 is used after stopping the rotation of the vat 2 to apply colorant in a spatially selective manner to predetermined areas of the smoothing layer 20 in order to obtain the desired location-dependent coloration for the layer to be subsequently solidified.

[0032] After the printing process by the inkjet printer 12 is completed, the vat 2 is rotated another 90° so that the area of ​​the smoothing layer 20, to which the colorant has been applied by the inkjet printer, is moved to the region between the exposure unit 6 and the build platform 8. The build platform 8 is then lowered, under the control of the control unit, relative to the surface of the vat bottom 3 to such an extent that the lower surface of the build platform (in the case of the first layer to be solidified on the build platform), or the lower surface of the last cured layer of the part 10 being built, is at a distance to the vat bottom equal to the predetermined layer thickness, thereby displacing the build material from the gap and creating the remaining layer having the predetermined layer thickness. According to the present invention, the positioning of the doctor blade 4 above the vat bottom 3 is set in such a way that the smoothing layer 20 is already close to, and optionally only slightly exceeding, the predetermined layer thickness. To this end, the positioning of the doctor blade relative to the vat bottom is adjusted so that after passing through the doctor blade, the resulting predetermined uniform layer thickness is within 100% to 150% of the desired layer thickness to be set by lowering the build platform. As explained above, there are several advantages if the amount of build material to be displaced while setting the layer thickness by lowering the build platform is small, ideally negligibly small.

[0033] After setting a predetermined layer thickness by controlled lowering of the build platform relative to the vat bottom, the layer of build material imprinted with colorant defined in the gap is exposed in a spatially selective manner by exposure unit 6 through the vat bottom and thereby solidified. The build platform, with part 10 being built suspended thereon, is then raised so that the now solidified layer disengages from vat bottom 3 and is lifted upward.

[0034] The operation of the inkjet printer 12 and the operation of the exposure unit 6 are controlled by a control unit (not shown), in which three-dimensional shape data of the molded body to be accumulated is stored, in particular data on the contour shapes of the individual layers to be solidified successively, as well as data on the distribution of colorants within the area of ​​each layer to be solidified.

[0035] 2 shows a sequence of method steps in a schematic top view from above for an apparatus such as that shown in FIG. 1 , illustrating a series of four work steps during the implementation of the method according to the present invention. In the first step, illustrated on the left edge of FIG. 2 , the vat is rotated counterclockwise about a vertical rotation axis perpendicular to the vat bottom 3. Simultaneously, build material, e.g., a photopolymerizable material filled with particulate ceramic material, is dispensed from a cartridge in the direction of rotation upstream of the doctor blade 4 on the vat bottom, so that a subsequent portion of the build material 18 is developed at the doctor blade 4. Due to the rotation of the vat bottom 3, the build material is moved under and past the doctor blade 4, which is suspended above the vat bottom in an adjustable position so that a smoothing layer 20 having a predetermined uniform layer thickness determined by the positioning of the doctor blade 4 relative to the vat bottom 3 is formed by the lower edge of the doctor blade. The smoothing layer 20 is moved by the rotation of the vat to the area below the inkjet printer 12, which is shifted 90° counterclockwise relative to the doctor blade 4. As soon as the area of ​​the smoothing layer 20 that will later become the build area for solidifying additional layers reaches the area below the inkjet printer 12, the vat is stopped. In this phase, the layer of build material is imprinted with colorant in a spatially selective manner. The result of the application of colorant is shown diagrammatically in the second drawing from the left in FIG. 2, where the printed letters DLP are intended to represent the applied colorant imprinted in a spatially selective manner (of course, in methods for producing dental products, discrete color structures such as letters are generally not applied, but rather continuously varying colorings are applied). The movable suspension of the inkjet printer 12 is indicated by the crossed arrow, and the inkjet printer is moved in a controlled manner controlled by a control unit (not shown) to achieve the spatially selective application of colorant in the build area.

[0036] The vat is then rotated again counterclockwise by 90° and then stopped again, as shown in the second-from-the-right image in FIG. 2. Due to the rotation, the area where the colorant represented by the DLP was applied in the previous step reaches the exposure unit 6 opposite the doctor blade 4, where it is solidified in a spatially selective manner by exposure after the build platform is lowered to set a predetermined layer thickness. This is shown in FIG. 2 by the grid opposite the doctor blade 4, which represents the picture elements (pixels) of the exposure unit. (The build platform is omitted in FIG. 2 so that the build area below the build platform remains visible.) Simultaneously with the exposure, the build area of ​​the subsequent wet build material layer at the 6 o'clock position is imprinted with the colorant represented in reverse by the DLP. During the rotation phase, the doctor blade 4 continues to form the smoothing layer 20 with a predetermined, uniform layer thickness. Again, note that in the view of FIG. 2, for illustration reasons, the build platform that is actually positioned over the exposure unit above the vat bottom has been omitted so that the exposure area of ​​the exposure unit is visible.

[0037] In the state transition shown on the right edge of Figure 2, a further 90° rotation of the vat bottom 3 occurs, and the doctor blade 4 continues to form the smoothing layer 20 having a predetermined uniform layer thickness. After the 90° rotation of the vat bottom and the step of stopping the rotation, the inkjet printer 12 again applies colorant in the next build zone, while the build zone previously imprinted with colorant in the second-to-right view of Figure 2 is now in the area of ​​the exposure unit at the 3 o'clock position in the view at the right edge of Figure 2 and is exposed after the build platform (not shown) is lowered. In this example, it is assumed that the zone corresponding to the letter DLP is exposed and solidified.

[0038] The area DLP exposed in the second-to-the-right figure has been rotated to the 12 o'clock position in a subsequent method step shown on the right edge of Figure 2, and is shown there as an area with a character sequence DLP where the bottom of the vat is visible, because after solidification of this area, the build platform is raised again, whereby a negative image of the remainder of the solidified layer in layer 20 remains, i.e., after raising the build platform with the previously solidified layer in the shape of the character sequence DLP, this area remains as a negative image or void in layer 20, since the build platform is not shown in Figure 2.

[0039] FIG. 3 shows the sequence of method steps corresponding to FIG. 2 during the implementation of the method according to the present invention. The apparatus for carrying out this method differs from the apparatus shown in FIG. 2 in the following respects. In FIG. 3, a build material dispensing device 30, not shown in FIG. 2, is shown. This build material dispensing device comprises two cartridges with different build materials. The cartridges are connected to a common mixing device that prepares a selected mixture of the build materials and dispenses the mixture. The doctor blade 4 in this case is configured as a double or twin doctor blade, i.e., it comprises two parallel doctor blades, between which a cavity that is open at the bottom is formed. The build material is delivered directly into the cavity between the two doctor blades by the mixing device. The positioning of the doctor blade downstream in the direction of rotation is set so that a smoothing layer 20 is formed with a predetermined uniform layer thickness, again determined by the positioning of the doctor blade 4 relative to the bottom of the vat.

[0040] At the 12 o'clock position, a vacuum doctor blade 34 is mounted, which is also configured as a double or twin doctor blade with a cavity between them that is open at the bottom. The cavity of the vacuum doctor blade 34 is kept under negative pressure so that any remaining build material left behind after the exposure step at the 3 o'clock position and the lift-off step of the build platform is sucked away.

[0041] 4 and 5, an embodiment of an adjustable doctor blade for forming smoothing layer 20 is described, with layer 20 having a predetermined, uniform thickness determined by the positioning of doctor blade 4 relative to the vat bottom. In the right-hand view of FIG. 5, a schematic plan view of vat bottom 3 from above is shown. The longitudinal direction of doctor blade 4 here extends radially outward from a starting point near the axis of rotation of circular vat bottom 3 to an end point near the outer periphery of circular vat bottom 3. In FIG. 4, a cross-sectional view of a portion of vat bottom 3 and a portion of doctor blade 4 is shown, with the cross-sectional plane perpendicular to the radial and longitudinal extension of doctor blade 4 visible in FIG. 5. As can be seen in the view of FIG. 4, the blade of doctor blade 4 is not oriented perpendicular to vat bottom 3, but is tilted relative to vat bottom 3, forming an inclination angle κ with respect to the vat bottom. The tilt angle is an acute angle, preferably within an angle range of 30° to 75°, and the doctor blade 4 is tilted at this tilt angle κ so that the doctor blade 4 is positioned relative to the direction of relative movement of the doctor blade 4 relative to the vat bottom such that the lower edge of the doctor blade 4, which is in the direction of relative movement of the doctor blade 4 relative to the vat bottom, trails behind the upper edge of the doctor blade 4. Referring to FIG. 4, this means that the direction of relative movement of the doctor blade 4 relative to the vat bottom 3 is oriented to the right-hand side, and then the lower edge of the doctor blade 4 trails behind the upper edge during its relative movement relative to the vat bottom. In front of the doctor blade 4, in the direction of movement of the doctor blade 4 relative to the vat bottom 3, the build material dispensed onto the vat bottom accumulates. The positioning of the doctor blade relative to the vat bottom is such that the portion of the build material passing through the gap between the vat bottom and the lower edge of the doctor blade is deposited in a predetermined uniform layer thickness D, which is determined by the positioning of the doctor blade relative to the vat bottom 3. NThe tilt angle described creates a funnel effect, i.e., the build material is forced toward the gap between the lower edge of the doctor blade and the bottom of the vat by the relative movement of the tilted doctor blade.

[0042] For the embodiment of the apparatus described herein having a rotatable vat 2 and a non-rotating doctor blade 4, it is advantageous to adjust a further angle, which will now be described in connection with FIG. 5. FIG. 5 shows a plan view taken from plane AA of FIG. 4, i.e., the viewing direction is in the x-direction and directed toward the side of the doctor blade 4. The positioning of the doctor blade 4 relative to the vat bottom is defined by the path of a straight line coincident with the lower edge of the doctor blade 4. The line coincident with the lower edge of the doctor blade 4 essentially extends radially relative to the rotatable vat 2, but is not parallel to the surface of the vat bottom 3. Instead, it is inclined relative to the surface of the vat bottom at an inclination angle α, which is greater than 0° and less than 15°, such that the distance of the lower edge of the doctor blade 4 to the vat bottom 3 starts from a minimum distance and increases with increasing radial distance from the axis of rotation. Such adjustment of the slope angle α is necessary for a rotating vat because, with increasing radial distance from the axis of rotation, an increasing amount of build material is required because the area across which the build material must be dispersed increases with increasing radial distance. In other words, the relative speed of the lower edge of the doctor blade relative to the bottom of the vat is a linearly growing function of the radial distance to the axis of rotation, such that at larger radial distances, correspondingly more build material is required, which in turn results in a larger area being dispersed due to the relatively higher speed of the bottom of the vat relative to the doctor blade. It has been observed that upstream of the doctor blade material accumulates at the doctor blade along the entire length of the build material dispensed within the radial range. Furthermore, in this embodiment with a rotating vat, and at larger radial distances from the axis of rotation, it was found that the layer thickness is determined by the distance of the lower edge of the doctor blade to the bottom of the vat, but the gap width, which depends on the radial distance to the axis of rotation, is not equal to the resulting layer thickness in the radially outer region of the doctor blade, which is lower than the gap width.Rather, material properties such as the viscoelasticity of the build material, coupled with its surface tension and adhesive behavior on the vat bottom, have the effect of further separating the build material into a thinner layer in areas at greater radial distances than that determined by the gap width between the lower edge of the doctor blade and the vat bottom. This requires that when changing to a different build material that differs in viscosity, surface tension, and adhesive properties, the doctor blade's position relative to the vat bottom must be adapted so that the desired, predetermined, uniform layer thickness is achieved over the entire area of ​​the dispensed build material. In this regard, it has been found that the optimal positioning of the doctor blade relative to the vat bottom can be found somewhat quickly using an adjustable suspension of the doctor blade, which allows the actuator drive to continuously adjust the height and bevel angle of the lower edge of the doctor blade and vary the doctor blade's positioning, thereby enabling rapid adaptation of the doctor blade's positioning by varying its positioning until the desired layer is formed.

[0043] The predetermined layer thickness, set by lowering the build platform and causing a displacement of the build material, is typically in the range of 20 μm to 100 μm in a typical build process; for example, the predetermined layer thickness can be 50 μm. To generate a predetermined, uniform layer thickness with the doctor blade that is higher than the predetermined layer thickness but not more than 50% higher than the predetermined layer thickness, it is necessary to adjust the minimum distance of the lower edge of the doctor blade 4 relative to the vat bottom 3 and to implement an adjustable suspension of the doctor blade that allows the two angles described above in connection with FIGS. 4 and 5 to be adjusted precisely and reproducibly without the risk of the adjusted positioning changing during operation. This can be accomplished, for example, using two positioning tables configured to adjust the table positions with high precision and forming a combined suspension for the doctor blade. The positioning tables are coupled to each other. One of the positioning tables serves to adjust the minimum distance of the lower edge of the doctor blade relative to the vat bottom, while the other adjusts the slope angle α (see Figure 4) of the lower edge of the doctor blade relative to the vat bottom via a goniometer.

[0044] FIG. 6 illustrates an alternative embodiment for achieving relative movement of the doctor blade 4 and vat bottom 3. In this case, a rectangular vat bottom 3 is used, as shown on the right-hand side of FIG. 6 as a plan view from above (view in the z-direction). In this case, the vat is linearly movable in the x-direction, as indicated by the arrow in the right-hand view of FIG. 6. On the left-hand side of FIG. 6, a plan view of the doctor blade and vat bottom from the side (view direction = x-direction) is shown. In this case, the doctor blade 4 is suspended so that its lower edge extends parallel to the surface of the vat bottom 3 and the distance of the lower edge of the doctor blade 4 to the vat bottom 3 is adjustable. In this case, the distance from the lower edge of the doctor blade to the vat bottom is the same everywhere, since the relative speed of the lower edge of the doctor blade with respect to the vat bottom is the same everywhere. The distance of the lower edge of the doctor blade to the vat bottom is equal to the predetermined uniform layer thickness to be formed by the doctor blade 4.

[0045] As can be seen on the right-hand side of Figure 6, a subsequent portion 18 of the dispensed build material is formed in the direction of travel of the vat in front of the doctor blade 4, while a flat layer 20 with a predetermined uniform layer thickness is formed in the direction of travel behind the doctor blade 4. It has been observed that for many types of build material, the actual generated layer thickness of the smoothed build behind the doctor blade is not strictly equal to the gap width between the lower edge of the doctor blade and the vat bottom, although the layer thickness is often slightly smaller. In this regard, it has also been found that by varying the positioning of the lower edge of the doctor blade, for example, using an actuation drive controlled by the control unit, the correct positioning of the doctor blade relative to the vat bottom can be quickly found, which correct positioning of the doctor blade results in the desired predetermined uniform layer thickness.

[0046] 7-12 show another representation of the sequence of method steps during the implementation of the method of the present invention. FIG. 7 shows a schematic plan view of a portion of a vat bottom 3, on which a doctor blade 4 has already formed a smoothing layer 20 with a predetermined uniform layer thickness. This smoothing layer is then moved by the rotation of the vat to the area below the inkjet printer 12, where the rotation of the vat is stopped. This stage is shown in the plan view of FIG. 8, which illustrates the movement and operation of the inkjet printer 12, which applies colorant 22 in a spatially selective manner. After the inkjet printer operation is completed, the vat is further rotated, and FIG. 9 shows a plan view of the vat during this rotation stage, showing the area of ​​layer 20 previously provided with colorant. The rotation of the vat continues until the imprinted layer area reaches the build area between the build platform 8 and the exposure unit. This state is illustrated in FIG. 10. In this step of the method, the build platform 8 is lowered by drives controlled by the control unit until the distance between the lower surface of the last cured layer of the currently built part 10 and the surface of the vat bottom is equal to the predetermined layer thickness. This step is completed in Figure 11, from which the currently defined layer above the vat bottom 3 is solidified in a spatially selective manner by controlled operation of the exposure unit. The layer thus cured by exposure becomes firmly attached to the previously last cured layer by ongoing polymerization, which leads to a firm adhesion of the two layers, which ultimately leads to a molded body of layers firmly connected to each other.

[0047] After the exposure step is completed, the build platform 8 is raised again in Fig. 12 so that the part 10 hanging thereon, with the last layer previously cured in Fig. 11, is lifted away from the vat bottom. Empty areas or holes remain on the vat bottom in the areas of the last cured layer, as can be seen in Fig. 12. These areas are again completely filled when the vat is rotated and the empty areas reach the build material dispensing zone in front of the doctor blade.

[0048] When selecting materials for the doctor blade, vat bottom, and vat sidewalls, the following must be considered: PTFE (polytetrafluoroethylene) is the most suitable material for the doctor blade and vat sidewalls. Due to its low surface energy, PTFE is advantageous for all components that come into direct contact with the build material to be treated. In this case, the build material to be treated does not adhere to the doctor blade or vat sidewalls. On the other hand, when using doctor blades made of other plastic materials, such as polycarbonate or polyamide, empty zones in the coating have been observed.

[0049] The excellent sliding properties of PTFE ensure that the rotation mechanism of the vat is generally not blocked if the doctor blade comes into direct contact with the side wall of the vat. PTFE is chemically inert to solvents, reactive components, and colorants in the suspension. The rigidity of PTFE and its abrasion resistance to the abrasive ceramic suspension are sufficient that no tearing or abrasion effects were observed in experiments.

[0050] When selecting a material for the vat bottom, two aspects must be considered. First, the vat bottom must have sufficient rigidity. Second, the surface must be very smooth and planar. Third, the vat bottom surface must be wettable by the suspension of the build material. For this aspect, the contact angle and viscosity of the build material are important. These requirements were best met by a combination of PMMA (polymethyl methacrylate, 3 mm thick) with an ETFE (ethylene tetrafluoroethylene, 80 μm thick) film on top. Instead of PMMA, glass or a similar material can also be considered for the vat bottom. Limitations on the material selection for the vat bottom result from additional requirements regarding transparency for exposure and pull-out force during the stereolithography build process. The ETFE film used in connection with this invention has a self-adhesive side that allows for bubble-free, planar bonding of the ETFE film onto the PMMA support disk. The highly planar bottom of the vat thus formed is one of the prerequisites for forming thin build material layers with high precision using a doctor blade. Like PTFE, ETFE is also inert to the chemicals used that come into contact with the ETFE film. In combination with the build material formulations used in connection with the present invention that use ETFE, a smaller contact angle and therefore better wettability can be obtained compared to FEP (fluoroethylene propylene).

[0051] A low contact angle (considered to be indicative of wettability) correlates well with a thin build material layer thickness. If the wettability is not good enough, the build material will shrink or atrophy locally, leading to "dissolution" and "island formation" of the build material layer. Pores will form in the coating, and potentially droplets will form. These effects can be greatly reduced or delayed by increasing the viscosity of the build material suspension. Experiments have shown that a viscosity of 10-50 Pa·s is suitable for a contact angle of 50°-60° for typical build materials used.

[0052] In the method according to the invention, the layer of build material, while still wet, may be imprinted in a spatially selective manner with colorants before the build platform is lowered onto the layer and the layer is exposed and solidified by the exposure unit. The colorants must be selected according to the type of build material, and the following allocation is desirable:

[0053] For unfilled and filled photopolymers as building materials, solutions containing dye molecules and / or suspensions containing pigments can be used.

[0054] In the case of the use of glass-ceramic slurries as building materials as colorants, preferably color pigments dispersed in an organic medium are used, in particular oxides, tin oxide or zirconium oxide.

[0055] In the case of ZrO2 slurries as building materials, preferably solutions of nitrates (aqueous or based on another solvent) or acetylacetonates dissolved in ethanol are used.

Claims

1. 1. A method for building a molded body by layer-by-layer solidification of a build material, the build material being a flowable photopolymerized material filled with ceramic particles, using stereolithography, comprising: a) a build material is dispensed onto the planar transparent bottom of a vat (2); b) the vat (2) is moved in a direction parallel to the plane of the vat bottom (3) relative to a doctor blade (4), the doctor blade being suspended with an adjustable positioning above the vat bottom (3), such that the dispensed build material is moved under the doctor blade (4), thereby forming a smoothing layer (20) having a uniform layer thickness, which is predetermined by the positioning of the doctor blade (4) relative to the vat bottom (3); c) the smoothing layer (20) is brought into the area between an exposure unit (6) located below the vat bottom (3) and a height-adjustable build platform (8) suspended above the vat by relative movement of the vat (2); d) the build platform (8) is lowered in a controlled manner relative to the vat bottom, thereby displacing the build material while allowing the remaining layer in the gap to be built to a predetermined layer thickness; e) the layer is solidified in a spatially selective manner by controlled movement of the exposure unit (6) within the contour desired for the current layer; f) the build platform (8) is then raised and build material is dispensed onto the bottom of the vat and steps b) to f) are repeated until the body is built up by several layers solidified on top of each other; a method comprising: adjusting the positioning of the doctor blade (4) relative to the vat bottom (3) in such a manner that the resulting predetermined uniform layer thickness is higher than the predetermined layer thickness to be set by lowering the build platform (8), but does not exceed the predetermined layer thickness by more than 50%; and wherein the surface of the smoothing layer is colored by applying a selected colorant in a spatially selective manner in an intermediate step before lowering the build platform (8) and before spatially selective exposure.

2. 2. The method of claim 1, characterized in that the position of the doctor blade (4) relative to the vat bottom (3) is adjusted in such a manner that the resulting predetermined uniform layer thickness is within the range of 110% to 130% of the desired layer thickness.

3. 3. The method according to claim 1 or 2, characterized in that the relative movement of the vat (2) and the doctor blade (4) is brought about by rotating the vat (2) about a central axis perpendicular to the vat bottom (3) with respect to the doctor blade (4) suspended in a stationary manner, or by rotating the doctor blade (4) about said central axis stated with respect to the vat (2) in a stationary state.

4. 4. The method according to claim 3, characterized in that the position of the doctor blade (4) above the bat bottom (3) is defined by a straight line coincident with the lower edge of the doctor blade defined by the minimum distance to the bat bottom (3) at the point of the linear lower edge of the doctor blade closest to the central axis, and by a slope angle (α) defined by the lower edge straight line and a plane parallel to the bat bottom (3) intersected by the straight line, said slope angle being greater than 0° and less than 15° such that the distance of the lower edge to the bat bottom (3) increases from the minimum distance with increasing radial distance to the central axis.

5. 5. The method according to claim 4, characterized in that the doctor blade (4) comprises a planar blade and that the doctor blade is inclined at an inclination angle (κ) to the vat bottom (3), the inclination angle (κ) being greater than 0° and less than 90°, the inclination angle being defined in relation to the direction of relative movement between the vat bottom (3) and the doctor blade (4) in such a way that the lower edge of the doctor blade (4) in the direction of relative movement of the doctor blade (4) to the vat bottom follows behind the upper edge of the doctor blade (4).

6. The method according to claim 5, wherein the tilt angle (κ) is in the range of 30° to 75°.

7. 3. The method according to any one of claims 1 to 2, characterized in that the relative movement of the bat (2) and the doctor blade (4) is brought about by a linear shifting of the bat (2) or by a linear shifting of the doctor blade (4).

8. 8. The method according to claim 7, characterized in that the position of the doctor blade (4) above the vat bottom is defined by the extension of a straight line coinciding with the lower edge of the doctor blade (4), said straight line extending at a constant distance relative to the vat bottom (3) and parallel to the vat bottom (3).

9. The coloring agent for setting color and translucency is a) in the case of a photopolymer as the building material, a solution containing dye molecules and / or a suspension containing a pigment, b) in the case of slurries containing glass-ceramics as the building material, color pigments dispersed in an organic medium; c) ZrO as a construction material 2 For slurries, solutions of nitrates (either aqueous or based on another solvent) or acetylacetonates dissolved in ethanol 9. The method according to claim 1, characterized in that the materials are selected from the group consisting of fluorine, arsenic, fluorine, fluorine-containing ...

10. 10. The method of claim 9, wherein the color pigment is an oxide, tin oxide, or zirconium oxide.

11. 10. The method according to claim 1, wherein the colorant is dissolved and / or dispersed in an ink and applied in a spatially selective manner onto the smoothing layer by means of an inkjet printer.

12. 12. The method according to any one of claims 1 to 11, characterized in that the doctor blade is made of polytetrafluoroethylene and that the circumferential side wall of the batt (2) is made of polytetrafluoroethylene.

13. 13. The method according to any one of claims 1 to 12, characterized in that as vat bottom (3) a plate of glass or polymethylmethacrylate is used, on which an ethylenetetrafluoroethylene film is bonded on its surface facing the vat bottom.

Citation Information

Patent Citations

  • Photocuring three-dimensional printing equipment and printing method

    CN108081611A

  • Powder spreading device for metal powder additive manufacturing

    CN209363616U

  • Layered molding device for generative stereolithographic production layer by layer of three-dimensional parts of a mold, e.g. as a tooth replacement, uses radiation to compact composite substances

    DE102007010624A1

  • Producing ceramic molded article in form of denture, by providing suspension e.g. from powder composition by position-layer deposition of individual slurry layer and solidifying individual slurry layer area to construct the molded body

    DE102011117005A1

  • Device and method for processing light-polymerizable material for the layered assembly of molds