Negative electrode active material for non-aqueous electrolyte secondary battery containing silicon oxide composite and method for producing same
A silicon oxide composite with internal pores and a carbon coating layer addresses the issue of volumetric expansion in negative electrode materials, improving battery life and capacity retention by stabilizing the mechanical structure and enhancing lithium ion diffusion.
Patent Information
- Application Number
- JP2020529539
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-03
- Filing Date
- 2018-12-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-12-03
AI Technical Summary
Existing negative electrode active materials in lithium secondary batteries, such as graphite, suffer from low capacity per unit mass, while alternative metals like Si, Sn, and Sb experience significant volumetric expansion and contraction leading to rapid deterioration of the battery's life characteristics due to alloying reactions with Li.
A silicon oxide composite with internal pores of 50 nm to 300 nm and a carbon coating layer is used, which buffers the volumetric expansion and contraction, improving mechanical stability and lithium ion diffusion.
The silicon oxide composite effectively prevents rapid deterioration of the battery life by managing expansion and contraction, enhancing capacity retention and initial efficiency.
Smart Images

Figure 0007593809000002 
Figure 0007593809000003 
Figure 0007593809000004
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery containing a silicon oxide composite, and a method for manufacturing the same.
Background Art
[0002] Lithium secondary batteries, which have recently been in the spotlight as power sources for portable small electronic devices, exhibit a high energy density with a discharge voltage more than twice as high as that of existing batteries using an alkaline aqueous solution by using an organic electrolyte solution.
[0003] As the positive electrode active material of a lithium secondary battery, oxides composed of transition metals having a structure capable of lithium intercalation, such as LiCoO2, LiMn2O4, LiNi 1-x Co x O2 (0 < x < 1), etc., are mainly used. As the negative electrode active material, various forms of carbon-based materials including artificial graphite, natural graphite, and hard carbon capable of lithium insertion and desorption have been applied.
[0004] Graphite is mainly used as the negative electrode material of a lithium secondary battery, but the capacity per unit mass of graphite is as small as 372 mAh / g, making it difficult to increase the capacity of a lithium secondary battery.
[0005] Metallic materials such as Si, Sn, Al, and Sb are being considered as new materials that can replace carbon-based anode active materials. These metallic materials are charged / discharged through alloying / dealloying reactions with Li, and are known to have higher capacity than graphite, a commercial anode active material. However, metals such as Si, Sn, Al, and Sb have problems in that they cause large volume expansion and contraction during the alloying / dealloying process with Li, which leads to pulverization, loss of conductive paths, and reduced life characteristics. In particular, Si is known to be an optimal material for a high-capacity anode material in terms of discharge capacity (4200mAh / g) and discharge voltage (0.4V), but the large volume expansion of up to about 400% induced when Li ions are inserted into the material (charging) causes the active material to degrade, resulting in a rapid decrease in life characteristics. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Publication No. 10-2014-0042146 (Publication date: 2014.04.07) Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above-mentioned problems of the prior art, the present invention aims to provide a new negative electrode active material for a non-aqueous electrolyte secondary battery, which contains a silicon oxide composite and can prevent a rapid deterioration of the life due to the volume expansion and contraction of lithium.
[0008] Another object of the present invention is to provide a method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery, which contains a silicon oxide composite.
[0009] Another object of the present invention is to provide a non-aqueous electrolyte lithium secondary battery containing a negative electrode active material for a non-aqueous electrolyte secondary battery, the negative electrode active material including the silicon oxide composite.
Means for Solving the Problem
[0010] The negative electrode active material for a non-aqueous electrolyte secondary battery according to an embodiment of the present invention contains silicon, silicon oxide (SiO x , 0 < x ≦ 2), and magnesium silicate, and contains a silicon oxide composite including pores having a size of 50 nm to 300 nm inside.
[0011] FIG. 1 is an image obtained by photographing the surface of a silicon oxide composite according to an embodiment of the present invention with a field emission scanning electron microscope (FE-SEM). Referring to FIG. 1, in the negative electrode active material for a non-aqueous electrolyte secondary battery according to an embodiment of the present invention, which contains a silicon oxide composite, the silicon oxide composite contains silicon, silicon oxide (SiO x , 0 < x ≦ 2), and magnesium silicate, and contains pores having a size of 50 nm to 300 nm disposed inside the silicon oxide composite.
[0012] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the internal pores can be represented by image processing.
[0013] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the pores disposed inside the silicon oxide composite play a role of buffering the expansion during the charging process to solve the problem of swelling, and can play a role of preventing a rapid deterioration in life due to expansion and contraction. The negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention concentrates the volume expansion and the stress caused thereby during charging and discharging of a lithium secondary battery on the internal pores to efficiently control the volume expansion, and thereby can improve the life characteristics of the lithium secondary battery.
[0014] In the negative electrode active material for a non-aqueous electrolyte secondary battery including the silicon oxide composite according to the present invention, the pores may be closed pores disposed inside the silicon oxide composite, and some of the pores may include open pores that are open to the outside.
[0015] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the pores may preferably be closed pores disposed inside the silicon oxide composite.
[0016] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the average diameter of the pores may be 50 to 300 nm.
[0017] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite according to the present invention, if the average diameter of the pores is less than 50 nm, the size of the pores may be too small to accommodate the volume expansion of Si during charging and discharging of a lithium secondary battery, and if the average diameter of the pores is more than 300 nm, the energy density may decrease due to the large number of pores remaining after accommodating the volume expansion of Si, and the mechanical strength of the negative electrode active material comprising a large number of pores may decrease. In addition, if the mechanical strength of the negative electrode active material decreases, the negative electrode active material may be damaged during the manufacturing process of the battery, such as mixing the slurry and rolling after coating.
[0018] In the negative electrode active material for a non-aqueous electrolyte secondary battery comprising the silicon oxide composite according to the present invention, the non-aqueous electrolyte is impregnated into the pores, and lithium ions can be introduced into the interior of the silicon oxide composite, thereby making the diffusion of lithium ions more efficient and improving the charge and discharge efficiency of the lithium secondary battery.
[0019] In the negative electrode active material for a non-aqueous electrolyte secondary battery including the silicon oxide composite according to the present invention, the ratio of the area of the pores to the total area of the cross section may be 3 to 40%.
[0020] When the ratio of the area of the pore portion is less than 3%, the volume expansion of the negative electrode active material cannot be suppressed during charging and discharging of the lithium secondary battery. When it exceeds 40%, due to the large number of pores present in the negative electrode active material, the mechanical strength decreases, and the negative electrode active material may be destroyed during the battery manufacturing process (such as slurry mixing, rolling after coating, etc.).
[0021] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the silicon may be crystalline or amorphous. When it is amorphous, the expansion and contraction during charging and discharging are reduced, and when used as the negative electrode active material of a secondary battery, the performance of the battery can be improved.
[0022] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the silicon oxide can be silicon dioxide.
[0023] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, when the silicon oxide (SiO X , 0 < x ≤ 2) is in an amorphous form during discharge, it can undergo an irreversible reaction with lithium ions to form Li-Si-O and Si + Li2O. Therefore, the higher the content of silicon oxide, the more the initial irreversible reaction increases, and the initial efficiency may decrease. In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the silicon oxide is preferably contained in an amount of 5 to 45 mol% based on the total number of moles of the silicon oxide composite.
[0024] When using the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, when the content of the silicon oxide is less than 5 mol%, the volume expansion and life characteristics may decrease. When it exceeds 45 mol%, the initial irreversible reaction increases, and the life of the secondary battery may decrease.
[0025] The negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, during the X-ray diffraction analysis of the silicon oxide composite, Si( 111The diffraction peak due to the diffraction method may be expressed at 2θ=27.5° to 29.5°, and the size of the silicon crystallites calculated from the full width at half maximum (FWHM) of the diffraction peak may be 1 nm to 20 nm.
[0026] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon oxide may have a ratio of silicon atoms to oxygen atoms (Si / O) of 0.5 to 2.
[0027] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the silicon can be dispersed in magnesium silicate, which further suppresses the expansion and contraction of silicon and further improves the battery performance when used as a negative electrode active material for a secondary battery.
[0028] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, which contains the silicon oxide composite, the magnesium silicate may contain at least one of MgSiO3 and Mg2SiO4. The magnesium silicate may contain MgSiO3 as a main component. In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, which contains the silicon oxide composite, the magnesium silicate may be represented by the general formula Mg x SiO y (0.5≦x≦2, 2.5≦y≦4).
[0029] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, magnesium may be contained in an amount of 2 wt % to 40 wt %, preferably 4 wt % to 30 wt %, and more preferably 4 wt % to 20 wt %, based on the total weight of the silicon oxide composite.
[0030] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, if the magnesium content is less than 2 wt %, the initial charge and discharge efficiency may decrease, and if it exceeds 40 wt %, the capacity retention rate and handling stability may decrease.
[0031] In the negative electrode active material for a non-aqueous electrolyte secondary battery including the silicon oxide composite according to the present invention, the magnesium silicate does not easily react with Li ions. Therefore, when used as a negative electrode active material, the magnesium silicate can suppress an initial irreversible reaction in a lithium secondary battery and can improve the life characteristics by reducing the amount of expansion and contraction of the electrode when Li ions rapidly increase.
[0032] In the negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the silicon oxide composite has a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of 1 m 2 / g~40m 2 / g. If the specific gravity of the silicon oxide composite is less than 1.8, the mechanical stability may be reduced, and if the specific gravity is more than 3.2, the charge and discharge capacity may be reduced when used as a negative electrode active material of a secondary battery. If the average particle size of the silicon oxide composite is less than 0.5 μm, the volume density may be small, and the charge and discharge capacity per unit volume may be reduced, and when used as a negative electrode active material, it may be difficult to disperse the slurry, and a phenomenon of aggregation may occur.
[0033] If the average particle size of the silicon oxide complex exceeds 20 μm, it may be difficult to prepare an electrode film, the negative electrode active material containing the silicon oxide complex may peel off from the current collector, and it may be difficult to uniformly react the inside of the negative electrode active material with lithium, which may result in a decrease in the life of the secondary battery.
[0034] The negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention may contain magnesium in an amount of 2 wt % to 40 wt % based on the total weight of the silicon oxide composite.
[0035] The negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention may contain oxygen in an amount of 25 wt % to 40 wt % based on the total weight of the silicon oxide composite.
[0036] The present invention may further include a carbon-containing coating layer on the surface of the silicon oxide composite-containing negative electrode active material for non-aqueous electrolyte secondary batteries. In the silicon oxide composite-containing negative electrode active material for non-aqueous electrolyte secondary batteries according to the present invention, the coating layer may be present in an amount of 2 wt% to 20 wt%, more preferably 2 wt% to 10 wt%, based on the total weight of the silicon oxide composite. If the carbon-containing coating layer has a content of less than 2 wt%, sufficient improvement in electrical conductivity cannot be expected, and the electrode life of the lithium secondary battery may be shortened. If the carbon-containing coating layer has a content of more than 20 wt%, the discharge capacity may be reduced, and the charge and discharge capacity per unit volume may be reduced.
[0037] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the carbon-containing coating layer may contain at least one selected from the group consisting of amorphous carbon, carbon nanofibers, graphene, and graphene oxide.
[0038] In the negative electrode active material for non-aqueous electrolyte secondary batteries containing the silicon oxide composite according to the present invention, the coating layer can provide excellent electrical conductivity between particles of the silicon oxide composite, thereby further improving the performance of the lithium secondary battery. In the negative electrode active material for non-aqueous electrolyte secondary batteries containing the silicon oxide composite according to the present invention, the coating layer containing carbon can suppress side reactions with the electrolyte and improve the performance of the lithium secondary battery.
[0039] In the negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite according to the present invention, the average thickness of the carbon-containing coating layer disposed on the surface of the silicon oxide composite may be 1 nm to 5 μm, preferably 5 nm to 2 μm, and more preferably 10 nm to 1 μm.
[0040] When the average thickness of the coating layer is 1 nm or more, the conductivity can be improved, and when the average thickness is 5 μm or less, the decrease in battery capacity can be suppressed when used as an anode active material of a lithium ion battery. When the average thickness of the coating layer is less than 1 nm, the effect of increasing the electrical conductivity due to the carbon coating is negligible, and when applied to an anode active material, the initial efficiency can be reduced due to high reactivity with the electrolyte. When the average thickness of the coating layer is more than 5 μm, the mobility of lithium ions can be hindered, and a problem of increased resistance can occur.
[0041] The negative electrode active material for a non-aqueous electrolyte secondary battery according to the present invention includes a silicon oxide composite having a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of 1 m 2 / g~40m 2 / g.
[0042] The silicon oxide composite including the coating layer according to the present invention may contain 1.5 wt % to 30 wt % of magnesium based on the total weight.
[0043] The silicon oxide composite according to the present invention may contain 15 wt % to 33 wt % of oxygen based on the total weight of the silicon oxide composite including the coating layer.
[0044] A non-aqueous electrolyte lithium secondary battery according to an embodiment of the present invention includes the negative electrode active material for non-aqueous electrolyte secondary batteries.
[0045] A method for manufacturing a non-aqueous electrolyte lithium secondary battery according to an embodiment of the present invention may include a first step of placing a mixture of silicon particles having an average particle size of 0.1 μm to 20 μm and silicon dioxide particles having an average particle size of 10 nm to 100 nm and magnesium having an average particle size of 1 mm to 100 mm into a reactor; a second step of adjusting the pressure of the reactor to 0.001 torr to 1 torr; a third step of heating the mixture and the magnesium at 600° C. to 1600° C. to prepare a silicon oxide composite; a fourth step of cooling the silicon oxide composite and depositing it on a metal plate; and a fifth step of pulverizing the silicon oxide composite cooled and deposited on the metal plate to an average particle size of 0.5 μm to 15 μm.
[0046] In the method for manufacturing a non-aqueous electrolyte lithium secondary battery according to the embodiment of the present invention, when the deposition temperature is 1200°C or higher, the vapor state particles of the silicon oxide complex are densely deposited on the metal plate and pores are hardly formed inside the particles, and when the deposition temperature is 500°C or lower, the vapor state particles of the silicon oxide complex are not deposited on the metal plate. Also, when the deposition temperature is in the range of 700 to 1000°C, the vapor state particles of the silicon oxide complex may easily form pores on the metal plate. The deposited mass is pulverized and powdered using a coarse pulverizer and a jet mill to adjust the particle size, thereby producing a silicon oxide complex powder having nanopores.
[0047] The method for producing a non-aqueous electrolyte lithium secondary battery according to the embodiment of the present invention may further include a sixth step of mixing the silicon oxide complex of the fifth step with at least one carbon source selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene, and heat-treating the mixture at 600° C. to 1200° C. to form a carbon-containing coating layer on the surface.
[0048] The carbon-containing coating layer disposed on the silicon oxide composite can be formed by mixing a carbon source containing one selected from carbon dioxide gas, argon, methane, ethane, propane, butane, water vapor or a mixed gas of hydrogen, hydrogen, acetylene, benzene, and toluene, or a gas mixture of combinations thereof, and reacting the carbon source with the silicon oxide composite at 600°C to 1200°C.
[0049] The carbon source gas may be methane, a mixture containing methane and an inert gas, or a mixture containing methane and an oxygen-containing gas.
[0050] The gas mixture may further include a plurality of inert gases selected from the group consisting of nitrogen, helium, and argon in addition to the carbon source gas.
[0051] In one embodiment, the carbon source gas is a mixture of CH4:CO2, which may have a molar ratio of about 1:0.20-0.50, preferably about 1:0.25-0.45, and more preferably about 1:0.30-0.40.
[0052] In one embodiment, the carbon source can be a mixture of CH4:CO2:H2O. The mixture of CH4:CO2:H2O can have a molar ratio of about 1:0.20-0.50:0.01-1.45, preferably about 1:0.25-0.45:0.10-1.35, and more preferably about 1:0.30-0.40:0.50-1.0.
[0053] In one embodiment, the carbon source can be carbon monoxide (CO) or carbon dioxide (CO2).
[0054] In one embodiment, the carbon source may be a mixture of CH4 and N2.
[0055] The CH4:N2 gas mixture may have a molar ratio of about 1:0.20-0.50, preferably about 1:0.25-0.45, and more preferably about 1:0.30-0.40.
[0056] The silicon oxide composite having the coating layer disposed on its surface may exhibit high conductivity due to the coating layer when the gas mixture contains water vapor. The content of water vapor in the gas mixture is not limited, and the preferred content of water vapor may be 0.01 to 10% by volume based on 100% by volume of the total carbon source gas.
[0057] A non-aqueous electrolyte lithium secondary battery according to an embodiment of the present invention includes the negative electrode active material for non-aqueous electrolyte secondary batteries.
[0058] A non-aqueous electrolyte secondary battery using the silicon oxide composite in the negative electrode is excellent in capacity retention rate and initial efficiency.
[0059] The silicon oxide composite may be used as a negative electrode active material for a non-aqueous electrolyte secondary battery, a positive electrode active material, a binder, and a conductive material. The negative electrode active material is capable of absorbing and releasing lithium ions. Effect of the Invention
[0060] The negative electrode active material for a non-aqueous electrolyte secondary battery containing the silicon oxide composite of the present invention contains a silicon oxide composite and has pores having a size of 50 nm to 300 nm therein, and a secondary battery containing the negative electrode active material of the present invention exhibits the effect of preventing a rapid deterioration of the battery life due to the volume expansion and contraction of Si, while improving the capacity characteristics. [Brief description of the drawings]
[0061] [Figure 1] 1 is an image of the surface of a silicon oxide composite according to Example 1 taken with a scanning electron microscope (FE-SEM) at 30,000 times magnification. [Diagram 2]1 is an image of the surface of a silicon oxide composite according to Example 1 taken with a scanning electron microscope (FE-SEM) at 100,000 times magnification. [Diagram 3] 1 is an image of the surface of a silicon oxide composite according to Example 2 taken with a scanning electron microscope (FE-SEM) at 20,000 times magnification. [Figure 4] 1 is an image of the surface of a silicon oxide composite according to Example 2 taken with a scanning electron microscope (FE-SEM) at 100,000 times magnification. [Diagram 5] 1 is an image of the surface of a silicon oxide composite according to Example 3 taken with a scanning electron microscope (FE-SEM) at 20,000 times magnification. [Figure 6] 1 is an image of the surface of a silicon oxide composite according to Example 3 taken with a scanning electron microscope (FE-SEM) at 100,000 times magnification. [Figure 7] 1 is an image of the surface of a silicon oxide composite according to Comparative Example 1 taken with a scanning electron microscope (FE-SEM) at 30,000 times magnification. [Figure 8] 1 is an image of the surface of a silicon oxide composite according to Comparative Example 1 taken with a scanning electron microscope (FE-SEM) at 100,000 times magnification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0062] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples.
[0063] <Example 1> Preparation of magnesium-containing silicon oxide composite
[0064] 15 kg of powder, which is a homogeneous mixture of silicon powder and silicon dioxide (SiO2) powder in a 1:1 molar ratio, and 1.5 kg of magnesium are heat-treated at 1,400°C in a reduced pressure atmosphere of 0.01 torr to 1 torr, and silicon oxide vapor and magnesium vapor are generated simultaneously from the mixed powder of silicon and silicon dioxide (SiO2) to react in the gas phase, and then cooled to 700°C to precipitate. The mixture is then pulverized in a jet mill to obtain a powder with an average particle size (D 50 A magnesium-containing silicon oxide composite powder having a particle size of 6.3 μm was recovered.
[0065] To form a carbon-containing coating layer, the recovered magnesium-containing silicon oxide composite powder was subjected to CVD treatment in a tubular electric furnace under a mixed gas of argon (Ar) and methane (CH4) at 1,000℃ for 2 hours to produce a silicon oxide composite (sample 1) containing 9 wt% magnesium and having a carbon coating layer with a carbon content of 5 wt%.
[0066] The magnesium-containing silicon oxide composite (sample 1) had a BET specific surface area of 5.5 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 6.3 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.
[0067] <Example 2> Preparation of magnesium-containing silicon oxide composite
[0068] A silicon oxide composite (sample 2) containing 9 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 800°C to precipitate, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 5 wt% was prepared.
[0069] The magnesium-containing silicon oxide composite (sample 2) had a BET specific surface area of 6.2 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D50 ) was 6.5 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.
[0070] <Example 3> Preparation of magnesium-containing silicon oxide composite
[0071] A silicon oxide composite (sample 3) containing 4 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 900°C to precipitate, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 10 wt% was prepared.
[0072] The magnesium-containing silicon oxide composite (sample 3) had a BET specific surface area of 6.3 m 2 / g, specific gravity 2.4g / cm 3 , average particle size (D 50 ) was 6.2 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 11 nm.
[0073] <Example 4> Preparation of magnesium-containing silicon oxide composite
[0074] A silicon oxide composite (sample 4) containing 12 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 1000°C to precipitate, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 7 wt% was prepared.
[0075] The magnesium-containing silicon oxide composite (sample 4) had a BET specific surface area of 5.8 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 6.8 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 13 nm.
[0076] <Example 5> Preparation of magnesium-containing silicon oxide composite
[0077] A silicon oxide composite (sample 5) containing 16 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 1100°C to precipitate, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 4 wt% was prepared.
[0078] The magnesium-containing silicon oxide composite (sample 5) had a BET specific surface area of 6.7 m 2 / g, specific gravity 2.4g / cm 3 , average particle size (D 50 ) was 6.7 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 14 nm.
[0079] <Example 6> Preparation of magnesium-containing silicon oxide composite
[0080] A silicon oxide composite (sample 6) containing 15 wt% magnesium was prepared in the same manner as in Example 1, except for cooling at 800°C to precipitate, and a silicon oxide composite powder having a carbon coating layer with a carbon content of 5 wt% was prepared.
[0081] The magnesium-containing silicon oxide composite (sample 6) had a BET specific surface area of 5.2 m 2 / g, specific gravity 2.3g / cm 3 , average particle size (D 50 ) was 6.6 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 14 nm.
[0082] <Example 7> Preparation of magnesium-containing silicon oxide composite
[0083] A silicon oxide composite containing 15 wt% magnesium and having a carbon coating layer with a carbon content of 15 wt% was prepared in the same manner as in Example 1, except for rapid cooling and precipitation.
[0084] The magnesium-containing silicon oxide composite (sample 7) had a BET specific surface area of 7.2 m 2 / g, specific gravity 2.0g / cm 3 , average particle size (D 50 ) was 6.5 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 12 nm.
[0085] <Comparative Example 1> Preparation of magnesium-containing silicon oxide composite
[0086] A silicon oxide composite containing 1 wt% magnesium and having a carbon coating layer with a carbon content of 5 wt% was prepared in the same manner as in Example 1, except that the precipitation was performed by natural cooling.
[0087] For the magnesium-containing silicon oxide composite (sample 8), the BET specific surface area was 5 m 2 / g, specific gravity 2.2g / cm 3 , average particle size (D 50 ) was 6.5 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 8 nm.
[0088] <Comparative Example 2> Preparation of magnesium-free silicon oxide composite
[0089] A silicon oxide composite (sample 9) having a carbon coating layer with a carbon content of 5 wt % was prepared in the same manner as in Example 1, except that the heat treatment was performed without adding magnesium.
[0090] The silicon oxide composite (sample 9) had a BET specific surface area of 6.5 m 2 / g, specific gravity 2.0g / cm 3 , average particle size (D 50 ) was 6.0 μm, and the size of the silicon crystallites measured by X-ray diffraction analysis (CuKα) was confirmed to be 5 nm.
[0091] <Experimental Example 1>
[0092] The pore size, pore area ratio (area ratio of pores to the total area in the image-processed cross section) of the silicon oxide composites prepared in Examples 1 to 7 and Comparative Examples 1 and 2, and the D of the silicon composite particles 50 The specific gravity and specific surface area of the silicon composite, the size of the Si crystallites, the initial discharge capacity efficiency, and the capacity retention rate were measured and are shown in Table 1.
[0093] In Table 1 below, it can be seen that no pores are generated inside the particles when magnesium is not included (Comparative Example 2) or when magnesium is included but is produced by natural cooling (Comparative Example 1).
[0094] [Table 1]
[0095] <Production Example>
[0096] A negative electrode for a lithium secondary battery and a battery (coin cell) containing the silicon oxide composite powder prepared according to the above examples and comparative examples as an electrode active material were fabricated.
[0097] The active material, SUPER-P as a conductive material, and polyacrylic acid were mixed with water in a weight ratio of 80:10:10 to prepare a negative electrode slurry.
[0098] The composition was applied to a copper foil having a thickness of 18 μm and dried to prepare an electrode having a thickness of 70 μm. The copper foil to which the electrode was applied was punched into a circle having a diameter of 14 mm to prepare a negative electrode for a coin cell, and a metallic lithium foil having a thickness of 0.3 mm was used as the counter electrode.
[0099] A 0.1 mm thick porous polyethylene sheet was used as the separator, and a 1:1 volumetric solution of ethylene carbonate (EC) and diethylene carbonate (DEC) dissolved in 1M LiPF6 was used as the electrolyte. Using the above components, a coin cell (battery) with a thickness of 2 mm and a diameter of 32 mm (the so-called 2032 type) was fabricated.
[0100] <Experimental Example>
[0101] The coin cell manufactured in the above manufacturing example was charged at a constant current of 0.1 C until the voltage reached 0.005 V, and discharged at a constant current of 0.1 C until the voltage reached 2.0 V. The charge capacity (mAh / g), discharge capacity (mAh / g), and initial charge / discharge efficiency (%) were determined, and the results are shown in Table 1.
[0102] In addition, in the above manufacturing examples, the coin cells prepared for each sample were charged and discharged once, and then from the second charge and discharge, they were charged at a constant current of 0.5 C until the voltage reached 0.005 V, and discharged at a constant current of 0.5 C until the voltage reached 2.0 V. The cycle characteristics (capacity retention rate after 50 cycles) were determined, and the results are shown in Table 1 above.
[0103] It can be seen from Table 1 that when pores are formed inside the particles, the capacity retention rate for 50 cycles is significantly improved.
Claims
1. Silicon, silicon oxide (SiO x , 0<x≦2), and magnesium silicate, the silicon oxide composite having pores with a diameter of 50 nm to 300 nm therein, The magnesium silicate is MgSiO 3 Including, The silicon oxide composite contains magnesium in an amount of 2 wt % to 40 wt % based on the total weight of the silicon oxide composite, The silicon oxide composite contains 25 wt % to 40 wt % of oxygen based on the total weight of the silicon oxide composite, In the X-ray diffraction analysis, the silicon oxide composite has a diffraction peak due to Si(111) at 2θ=27.5° to 29.5°; The size of the silicon crystallites calculated from the full width at half maximum (FWHM) of the diffraction peak is 1 nm to 20 nm; The ratio of the area of the pores to the total area of the cross section of the silicon oxide composite is 3 to 40%. Negative electrode active material for non-aqueous electrolyte secondary batteries.
2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the silicon oxide has a ratio of silicon atoms to oxygen atoms (Si / O) of 0.5 to 2.
3. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the silicon oxide complex has a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of 1 m 2 / g to 40 m 2 / g.
4. The silicon oxide composite further comprises a coating layer containing carbon on a surface thereof, 2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the coating layer is 2 wt % to 20 wt % of the total weight of the silicon oxide composite.
5. The negative electrode active material for a non-aqueous electrolyte secondary battery as described in claim 4, wherein the carbon-containing coating layer contains at least one selected from the group consisting of amorphous carbon, carbon nanofibers, graphene, and graphene oxide.
6. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 4, wherein the silicon oxide complex has a specific gravity of 1.8 to 3.2, an average particle size of 0.5 μm to 20 μm, and a specific surface area of 1 m 2 / g to 40 m 2 / g.
7. A negative electrode comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or any one of claims 3 to 6.
8. A non-aqueous electrolyte lithium secondary battery comprising the negative electrode according to claim 7.
9. A first step of introducing a mixture of silicon particles having an average particle size of 0.1 μm to 20 μm and silicon dioxide particles having an average particle size of 10 nm to 100 nm and magnesium particles having an average particle size of 1 mm to 100 mm into a reactor; a second step of adjusting the pressure of the reactor to 0.001 torr to 1 torr; a third step of heating the mixture and the magnesium metal particles at 600° C. to 1600° C. to produce a silicon oxide composite; a fourth step of cooling the silicon oxide composite at a temperature in the range of from greater than 500° C. to less than 1100° C. and depositing the cooled silicon oxide composite on a metal plate; and a fifth step of pulverizing and classifying the silicon oxide composite cooled and deposited on the metal plate to an average particle size of 0.5 μm to 15 μm. The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1.
10. A method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery as described in claim 9, further comprising a sixth step of mixing the silicon oxide complex of the fifth step and a carbon source and heat-treating the mixture at 600°C to 1200°C to form a carbon-containing coating layer on the surface of the silicon oxide complex.
11. The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery described in claim 10, wherein the carbon source is at least one selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene.
12. The method for producing a negative electrode active material for a non-aqueous electrolyte secondary battery described in claim 11, wherein the silicon oxide complex and the carbon source are mixed further containing at least one selected from the group consisting of nitrogen, helium, argon, carbon dioxide gas, and water vapor.
Citation Information
Patent Citations
Negative electrode material for secondary battery, and its manufacturing method
JP2010170943A
Negative electrode active material for lithium ion secondary battery, negative electrode mixture for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2013030428A
Method and material for lithium ion battery anodes
WO2016085953A1
Anode material for non-aqueous electrolyte secondary battery, preparation method therefor, and non-aqueous electrolyte secondary battery including same
WO2016204366A1
Anode active material for lithium secondary battery and method for producing same
WO2017052281A1