Titanium alloy member and method for manufacturing titanium alloy member

The titanium alloy member with controlled chemical compositions and manufacturing processes forms a martensitic structure through rapid cooling, overcoming the limitations of conventional Ti-Al-Fe alloys by achieving superior hardness and fatigue properties, suitable for structural applications.

JP7594199B2Active Publication Date: 2024-12-04NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022570813
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-22
Publication Date
2024-12-04
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Conventional α+β type Ti-Al-Fe alloys fail to achieve the high hardness and fatigue properties of Ti-6Al-4V alloys due to the rapid diffusion of elements like Fe, Cr, or Ni, which prevents the formation of a martensitic structure during rapid cooling, leading to inferior strength characteristics.

Method used

A titanium alloy member with specific chemical compositions and manufacturing processes, including three-dimensional additive manufacturing with controlled cooling rates and laser irradiation, forms a metal structure predominantly composed of needle-like acicular crystals, achieving a Vickers hardness of 350 HV or more and suppressing crack formation.

Benefits of technology

The titanium alloy member exhibits higher hardness and fatigue properties compared to conventional α+β type Ti-Al-Fe alloys, making it suitable for mechanical structural components and intermediate materials with enhanced strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594199000006
    Figure 0007594199000006
  • Figure 0007594199000007
    Figure 0007594199000007
  • Figure 0007594199000008
    Figure 0007594199000008
Patent Text Reader

Abstract

A titanium alloy member according to one embodiment of the present invention has a hard part which has a chemical composition that contains, in mass%, from 4.0% to 9.0% of Al, from 0.5% to 2.5% in total of one or more elements that are selected from the group consisting of Fe, Cr and Ni, from 0% to 0.100% of C, from 0% to 0.100% of N, from 0% to 0.100% of H and from 0% to 0.500% of O, with the balance being made up of Ti and impurities, and which has a Vickers hardness of 350 HV or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a titanium alloy part and a method for manufacturing a titanium alloy part. [Background technology]

[0002] Ti-6Al-4V alloys, which have an excellent balance between strength and ductility, account for approximately 70% of the practical use of structural titanium alloys. In order to further improve the strength of Ti-6Al-4V alloys, a method of generating a fine martensite structure by quenching from the β phase can be used (e.g., Patent Documents 1 and 2).

[0003] On the other hand, Ti-6Al-4V alloys, which are general-purpose alloys, contain expensive V as a constituent element. Therefore, the replacement of V with cheaper and more readily available general-purpose elements such as Fe, Cr, and Ni has been considered (for example, Patent Document 3).

[0004] However, when an α+β type titanium alloy, such as a Ti-Al-Fe alloy in which V is replaced with Fe, is heated to the β phase temperature range and then rapidly cooled, its strength (hardness and fatigue strength) tends to be inferior to that of a Ti-6Al-4V alloy. For example, in Figure 2 "Effect of cooling rates on Vickers hardness at room temperature in β heat treated Ti-5Al-1Fe" in Non-Patent Document 1, the room temperature hardness of a sample cooled at a constant cooling rate from the β range to room temperature is shown. Regarding Figure 2, Non-Patent Document 1 reports that "at a cooling rate of 0.5 to 1°C / s, the room temperature hardness of Ti-5Al-1Fe was approximately 300 HV, the minimum hardness value in this experimental range, and the room temperature hardness increased gradually with increasing cooling rate, reaching approximately 330 HV at 300°C / s, with a smaller cooling rate dependency than Ti-6Al-4V. This is a similar trend to Ti-5Al-2.5Sn, which contains only approximately 0.2 mass% Fe, a β-stabilizing element, and the rapid increase in hardness at cooling rates above a certain rate (10°C / s), as confirmed for Ti-6Al-4V, was not observed."

[0005] The reason why Ti-Al-Fe alloys that have been quenched from the β phase tend to have inferior strength to Ti-6Al-4V alloys is thought to be because it is not possible to produce a metal structure mainly composed of martensite. The reason why it is difficult to produce a martensite structure in Ti-Al-Fe alloys is because the diffusion rate of Fe in β-Ti is extremely fast. Even if α+β titanium alloys are quenched from the β phase using common methods, the diffusion of Fe will quickly produce an α+β two-phase structure.

[0006] For this reason, α+β type titanium alloys, such as Ti-Al-Fe alloys, have not been able to achieve the high hardness and high fatigue properties that are achieved by Ti-6Al-4V alloys (see Figure 2 in Non-Patent Document 1). The above problems that arise when part of V is replaced with Fe also arise when part of V is replaced with Cr or Ni. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent No. 4766408 [Patent Document 2] Japanese Patent No. 5419098 [Patent Document 3] Japanese Patent No. 3076697 [Non-patent literature]

[0008] [Non-Patent Document 1] Yoshitsugu Tatezawa et al., "Continuous Cooling Transformation Characteristics of Ti-5Al-1Fe", Iron and Steel, Japan, Iron and Steel Institute of Japan, 2016, Vol. 102, No. 5, p. 12 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in view of the above circumstances, and aims to provide a titanium alloy part having higher hardness than conventional α+β type Ti-Al-Fe alloys, and a method for producing the same. Another aim of the present invention is to provide a titanium alloy part having higher fatigue properties than conventional α+β type Ti-Al-Fe alloys. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention employs the following configuration.

[0011] (1) A titanium alloy part according to one embodiment of the present invention has a chemical composition, in mass%, of Al: 4.0-9.0%, one or more selected from the group consisting of Fe, Cr, and Ni: 0.5-2.5% in total, C: 0-0.100%, N: 0-0.100%, H: 0-0.100%, and O: 0-0.500%, with the balance being Ti and impurities, and has a hard part having a Vickers hardness of 350 HV or more. (2) In the titanium alloy structural member described in (1) above, the metal structure of the hard part may be composed of needle-like crystals, plate-like crystals, and a remaining structure, the total amount of the plate-like crystals and the remaining structure in a cross section of the hard part may be 10.0 area % or less, and the plate-like crystals in a cross section of the hard part may be 0 to 2.0 area %. (3) In the titanium alloy part according to the above (1) or (2), the hard portion may be disposed at a depth of 0.5 mm or more from the surface of the titanium alloy part. (4) The titanium alloy part according to any one of (1) to (3) above may have one or more parts selected from a mesh-shaped part, an extremely thin plate-shaped part, and a hollow-shaped part. (5) A method for producing a titanium alloy member according to another embodiment of the present invention is a method for producing a titanium alloy member according to any one of the above (1) to (4), comprising the steps of: applying a heat input of 30.0 J / mm to a raw material powder having chemical components containing, in mass%, Al: 4.0 to 9.0%, one or more selected from the group consisting of Fe, Cr, and Ni: 0.5 to 2.5% in total, C: 0 to 0.100%, N: 0 to 0.100%, H: 0 to 0.100%, and O: 0 to 0.500%, with the balance being Ti and impurities. 3 The method includes a step of melting the raw material powder by irradiating a laser under the following conditions, and a step of rapidly cooling the molten raw material powder. (6) The method for producing a titanium alloy part according to another embodiment of the present invention comprises the steps of: heating the titanium alloy part according to any one of the above (1) to (4) at an average heating rate of 50°C / sec or more to a final temperature within a temperature range of (β transformation temperature-200)°C or more to (β transformation temperature-100)°C or less; hot working the titanium alloy part within the temperature range at a strain rate of 0.10 to 10 / sec and a total strain of more than 0.50; and cooling the hot-worked titanium alloy part at an average cooling rate of 20°C / sec or more, and starting the hot working within 10 seconds from the time when the titanium alloy part is heated to the final temperature. Effect of the Invention

[0012] According to the present invention, it is possible to provide a titanium alloy part having higher hardness than conventional α+β type Ti-Al-Fe alloys and a manufacturing method thereof. Furthermore, according to the present invention, it is possible to provide a titanium alloy part having higher fatigue properties than conventional α+β type Ti-Al-Fe alloys. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is an electron microscope photograph of Test Example 3. [Diagram 2] FIG. 2 is an electron microscope photograph of Test Example 3, taken from a different field of view than that of FIG. [Diagram 3] FIG. 3 is a flowchart of a method for evaluating the structure of a hard portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] According to the conventional technology, it has not been possible to make the Vickers hardness of a part or all of a member made of a Ti-Al-Fe alloy 350HV or more. This is believed to be due to the extremely fast diffusion rate of Fe in β-Ti. Even if a Ti-Al-Fe alloy is heated to a β single-phase region (a temperature range in which the metal structure is entirely β phase) and then quenched, the metal structure quickly becomes an α+β two-phase structure due to the rapid diffusion of Fe. For this reason, it is believed that the hardness of a Ti-Al-Fe alloy quenched from a β single-phase region is inferior to that of a Ti-6Al-4V alloy, which can obtain a martensite structure by similarly quenching from a β single phase. This is also believed to apply to Ti alloys containing Ni and / or Cr in addition to or instead of Fe.

[0015] The present inventors have investigated a method for cooling an alloy at a rate faster than the diffusion rate of alloying elements such as Fe, and have focused on three-dimensional additive manufacturing technology. Three-dimensional additive manufacturing technology is a process that allows near-net forming without going through the usual melting, forging, and cutting processes. Thus, three-dimensional additive manufacturing technology does not use the usual melting process. Therefore, it was found that three-dimensional additive manufacturing is less likely to cause microsegregation of alloying elements such as Fe. And, in a Ti-Al-Fe alloy member manufactured using three-dimensional additive manufacturing technology and optimizing the manufacturing conditions, it was possible to achieve a Vickers hardness of 350HV or more, which was impossible to achieve by a normal manufacturing process. This is presumably because, after the member solidifies, cooling is completed faster than the diffusion of Fe in Ti, so that the β phase at high temperatures is cooled while containing a large amount of Fe, generating a hard martensite structure, and the amount of hard phase in the metal structure is increased. Similar results were also obtained in titanium alloy members containing Cr and / or Ni instead of Fe.

[0016] However, cracks were sometimes observed in components manufactured by applying 3D additive manufacturing technology to Ti-Al-Fe alloys. When using an electron beam 3D additive manufacturing method, which has a relatively slow cooling rate after solidification, it was possible to suppress cracks, but it was not possible to achieve the Vickers hardness of 350 HV or more that is the objective of this invention. On the other hand, when using a laser 3D additive manufacturing method, which has a fast cooling rate after solidification, cracks often occurred. Components with cracks are not only extremely poor in appearance and strength, but also cannot be used in practice because the cracks progress when subjected to external forces, leading to destruction. Even in titanium alloy parts containing Cr and / or Ni instead of Fe, cracking could not be suppressed. There have been no cases where cracking has been considered a problem in titanium alloy parts made by applying the casting method to Ti-Al-Fe alloys. Cracking was considered to be a problem specific to the application of three-dimensional additive manufacturing technology to Ti-Al-Fe alloys.

[0017] Therefore, the inventors of the present invention have further investigated a method for improving the hardness of a titanium alloy member without causing cracks. As a result, they have succeeded in preventing cracks by controlling the laser output in the three-dimensional additive manufacturing to an extremely small value.

[0018] Hereinafter, a titanium alloy part according to one embodiment of the present invention will be described. The titanium alloy member of this embodiment has a chemical composition, in mass%, of Al: 4.0-9.0%, one or more selected from the group consisting of Fe, Cr, and Ni: 0.5-2.5% in total, C: 0-0.100%, N: 0-0.100%, H: 0-0.100%, and O: 0-0.500%, with the balance being Ti and impurities, and has a hard part with a Vickers hardness of 350HV or more. In this embodiment, the "titanium alloy member" is understood to be a member that does not contain cracks that are problematic in the use of the member (for example, cracks that exceed 20% of the maximum thickness of the part including the hard part). This is because a member that contains cracks that are problematic in the use of the member cannot be used in practice, and therefore cannot be considered a member in the usual sense.

[0019] The chemical components of the titanium alloy member of this embodiment will be described below. Unless otherwise specified, "%" means "mass %".

[0020] Al: 4.0-9.0% In order to ensure the strength of the titanium alloy member, the lower limit of Al is set to 4.0% or more. If Al is less than 4.0%, the Vickers hardness decreases, making it difficult to obtain the desired strength characteristics. If Al exceeds 9.0%, the ductility of the titanium alloy member may be significantly reduced. Therefore, the Al content is preferably in the range of 4.0 to 9.0%. The Al content may be 4.2% or more, 4.5% or more, 4.8% or more, or 5.0% or more. The Al content may be 8.0% or less, 7.0% or less, 6.5% or less, or 6.0% or less.

[0021] One or more selected from the group consisting of Fe, Cr, and Ni: 0.5 to 2.5% in total The titanium alloy part contains one or more elements selected from the group consisting of Fe, Cr, and Ni. All of these elements are used in the titanium alloy part according to the present embodiment to ensure strength. Therefore, the total amount of these elements is specified in the titanium alloy part according to the present embodiment.

[0022] The total amount of Fe, Cr, and Ni is 0.5% or more. If the total amount of Fe, Cr, and Ni is less than 0.5%, the Vickers hardness of the titanium alloy member is reduced, making it difficult to obtain the desired strength characteristics. If the total amount of Fe, Cr, and Ni exceeds 2.5%, the β phase is stabilized, making it difficult to obtain the desired strength characteristics. Furthermore, if the total amount of Fe, Cr, and Ni exceeds 2.5% and the amount of Fe is excessive, there is a risk that the equilibrium intermetallic compound phase (TiFe, TiFe2) is easily generated. If the intermetallic compound phase is contained in the titanium alloy member, there is a risk that the intermetallic compound will be brittle broken due to thermal expansion caused by temperature change, causing cracks, or that fatigue properties will be extremely deteriorated. In addition, when the total amount of Fe, Cr, and Ni exceeds 2.5% and the amount of Cr or Ni is excessive, the equilibrium intermetallic compound phase (Ti2Ni, TiCr2) is easily generated, which may cause brittle fracture and cracking due to thermal expansion caused by temperature changes, or may cause an extreme deterioration in fatigue properties. Therefore, the total amount of Fe, Cr, and Ni is set to a range of 0.5 to 2.5%. The total amount of Fe, Cr, and Ni may be set to 0.6% or more, 0.7% or more, 0.8% or more, or 1.0% or more. The total amount of Fe, Cr, and Ni may be set to 2.2% or less, 2.0% or less, 1.8% or less, 1.7% or less, or 1.5% or less.

[0023] As long as the above-mentioned total content is satisfied, the individual contents of Fe, Cr, and Ni are not particularly limited. For example, as long as the above-mentioned total content is satisfied, the content of one or two of the elements Fe, Cr, and Ni may be 0%.

[0024] The titanium alloy part may contain C as a chemical component. The titanium alloy part according to the present embodiment can solve the problem without containing C. Therefore, the C content may be 0%. On the other hand, in order to reduce refining costs and ensure strength, for example, about 0.100% C is permitted in the titanium alloy part. The C content may be 0.001% or more, 0.003% or more, or 0.005% or more. The C content may be 0.080% or less, 0.050% or less, or 0.010% or less.

[0025] The titanium alloy member may contain N as a chemical component. The titanium alloy member according to the present embodiment can solve the problem without containing N. Therefore, the N content may be 0%. On the other hand, in order to reduce refining costs and ensure strength, for example, about 0.100% N is permitted in the titanium alloy member. The N content may be 0.001% or more, 0.002% or more, or 0.003% or more. The N content may be 0.080% or less, 0.050% or less, or 0.010% or less.

[0026] The titanium alloy part may contain H as a chemical component. The titanium alloy part according to the present embodiment can solve the problem without containing H. Therefore, the content of H may be 0%. On the other hand, in order to reduce refining costs, for example, about 0.100% H is allowed in the titanium alloy part. The content of H may be 0.001% or more, 0.002% or more, or 0.003% or more. The content of H may be 0.080% or less, 0.050% or less, or 0.010% or less.

[0027] The titanium alloy member may contain O as a chemical component. The titanium alloy member according to the present embodiment can solve the problem without containing O. Therefore, the content of O may be 0%. On the other hand, in order to reduce refining costs and ensure strength, for example, about 0.500% of O is permitted in the titanium alloy member. The O content may be 0.010% or more, 0.050% or more, or 0.100% or more. The O content may be 0.300% or less, 0.250% or less, or 0.200% or less.

[0028] The balance of the chemical components of the titanium alloy structural member according to this embodiment includes Ti and impurities. The impurities refer to components that are mixed in due to various factors such as raw materials or manufacturing processes when industrially manufacturing a titanium alloy structural member, and are allowed within a range that does not adversely affect the titanium alloy structural member according to this embodiment. Examples of components that are mixed in due to various factors include Cl, Mn, Mg, Si, V, Cu, Sn, Mo, Nb, Ru, and Pd.

[0029] Next, the hard part of the titanium alloy part according to this embodiment will be described. The titanium alloy part according to this embodiment has a hard part with a Vickers hardness of 350HV or more. That is, the titanium alloy part according to this embodiment has a Vickers hardness of 350HV or more in part or in whole. Therefore, the titanium alloy part according to this embodiment has high strength and can be used as various mechanical structural parts. The hardness of the hard part may be 360HV or more, 380HV or more, or 400HV or more.

[0030] The size, shape, position, and range of the hard part in the member are not particularly limited, and can be selected according to the application of the titanium alloy member. The entire region of the titanium alloy member may be the hard part. On the other hand, the hard part may be provided only in the region of the titanium alloy member where strength is required, and the Vickers hardness in the other regions may be suppressed to less than 350HV. For example, when the titanium alloy member is manufactured by three-dimensional additive manufacturing technology, the size, shape, position, and range of the hard part in the member can be flexibly designed. For example, the hard part may be disposed at a depth of 0.5 mm or more, 0.8 mm or more, or 1.0 mm or more from the surface of the titanium alloy member. Here, "depth" refers to the shortest distance between the hard part and the surface of the titanium alloy member.

[0031] The Vickers hardness of a titanium alloy member is measured by cutting the member at an arbitrary location, polishing the cut surface, pressing a Vickers indenter into the cut surface to form an indentation, and measuring the size of the indentation. The load for pressing the Vickers indenter is, for example, 5 kgf. A titanium alloy member having one or more locations judged to have a Vickers hardness of 350 HV or more is a titanium alloy member having a hard part having a Vickers hardness of 350 HV or more. In addition, a titanium alloy member in which the center of the indentation at the location judged to have a Vickers hardness of 350 HV or more is 0.5 mm or more away from the outer edge of the cut surface of the titanium alloy member is a titanium alloy member in which a hard part having a Vickers hardness of 350 HV or more is located at a depth of 0.5 mm or more from the surface.

[0032] As long as the chemical composition is within the above-mentioned range and the hard part has a Vickers hardness of 350 HV or more, the other configurations of the titanium alloy part according to this embodiment are not particularly limited. However, the following is an example of a more suitable form of the titanium alloy part.

[0033] For example, in the titanium alloy member of this embodiment, the metal structure of the hard part may be composed of needle crystals, plate crystals, and a remaining structure, the total amount of the plate crystals and the remaining structure in a cross section of the hard part may be 10.0 area % or less, and the plate crystals in a cross section of the hard part may be 0 to 2.0 area %. Plate-like crystals are crystals that are determined to be α-phase by X-ray diffraction or EBSD. Crystals whose short side width, as measured by cross-sectional observation, is greater than 5 μm, and Crystals whose short side width measured by cross-sectional observation is 5 μm or less and which are judged to be in a layered aggregate form by cross-sectional observation This means both. The needle-like crystals refer to crystals other than plate-like crystals that are determined to be α-phase by X-ray diffraction or EBSD. The residual structure refers to a structure that is determined to be a phase other than the α phase by X-ray diffraction or EBSD.

[0034] [Needle-shaped crystals] In this embodiment, the needle-like crystals are also called Widmanstätten-like structures. When the needle-like crystals are analyzed by X-ray diffraction or EBSD, they are identified as α-phase. However, compared with normal α-phase, the needle-like crystals have a very high Vickers hardness. Therefore, in the titanium alloy member according to this embodiment, it is presumed that the needle-like crystals are not α-phase, but α' martensite structures in which alloy elements such as Fe are solidified without being diffused. By making the metal structure of the hard portion of the titanium alloy part of this embodiment a structure mainly composed of needle-shaped crystals, the hard portion has a higher Vickers hardness than that of conventional α+β type titanium alloys. Needle crystals are distinguished from plate crystals, which will be described later, based on their shapes. Needle crystals are crystals whose short side width is smaller than that of plate crystals. However, it is not easy to accurately grasp the width of needle crystals and plate crystals. This is because when needle crystals and plate crystals are observed in the cross section of a titanium alloy component, the measured values ​​of the width of these crystals on the cross section change depending on the angle between the cross section and these crystals. The distinction between needle crystals and plate crystals is performed based on the flow chart shown in Figure 3, and the details will be described later.

[0035] [Plate crystals] The plate crystals are formed when the titanium alloy member of the present embodiment is quenched from the β single-phase temperature range, and as a result of the diffusion of some of the β stabilizing elements such as Fe, the parts lacking the β stabilizing elements are transformed into the α phase. When the plate crystals are analyzed by the X-ray diffraction method or the EBSD method, they are identified as the α phase. That is, when the plate crystals and the needle crystals are evaluated by the X-ray diffraction method or the EBSD method, both are evaluated as the α phase, so that the two cannot be distinguished by the X-ray diffraction method or the EBSD method. The plate crystals and the needle crystals are distinguished based on the apparent short side width and the state of assembly. Plate crystals have a lower Vickers hardness than needle crystals. Therefore, the area ratio of the plate crystals in the hard part is preferably 2.0 area% or less. The area ratio of the plate crystals in the hard part may be 1.8 area% or less, 1.5 area% or less, or 1.0 area% or less. From the viewpoint of further increasing the strength of the titanium alloy member, the fewer the plate crystals in the hard part, the better. Therefore, the lower limit of the area ratio of the plate crystals in the hard part may be 0 area%. On the other hand, the area ratio of the plate crystals in the hard part may be 0.1 area% or more, 0.2 area% or more, or 0.5 area% or more.

[0036] [Remaining tissue] The remaining structure of the hard part of the titanium alloy member of this embodiment is a β phase in part or in whole. Examples of the remaining structure other than the β phase include a portion where the phase could not be identified by EBSD due to residual strain or the like. The remaining structure other than the β phase is extremely small. Since the β phase is soft, from the viewpoint of further increasing the strength of the titanium alloy member, the smaller the remaining structure in the hard part, the better. In this embodiment, it is preferable that the total amount of the plate crystals and the remaining structure in the hard part is 10.0 area % or less. By setting the total amount of the plate crystals and the remaining structure in the hard part to 10.0 area % or less, the area ratio of the hard needle crystals is increased, and a higher Vickers hardness can be obtained. The area ratio of the remaining structure in the hard part may be 9.0 area % or less, 8.5 area % or less, or 8.0 area % or less. The smaller the remaining structure, the better, and the lower limit may be 0 area %. On the other hand, the area ratio of the remaining structure in the hard portion may be 2.5 area % or more, 3.0 area % or more, or 4.0 area % or more.

[0037] The crystalline structure in the hard part of the titanium alloy part of this embodiment is measured by a combination of cross-sectional metallographic observation and EBSD (Electron Backscatter Diffraction). As shown in Fig. 3, first, needle-like crystals and plate-like crystals, which are determined to be α-phase, are distinguished from the remaining structure, which is a structure other than the α-phase, by using EBSD. Next, the needle-like crystals and plate-like crystals are distinguished by cross-sectional metallographic observation. The evaluation method of the crystalline structure will be described in detail below. First, a test piece is taken with the cross section of the hard part as the observation surface. Note that the rough position of the hard part may be identified by hardness measurement using the above-mentioned means, and then the cross section of the hard part may be subjected to the following structural evaluation. On the other hand, the following structural evaluation may be performed on a portion estimated to be the hard part, and then the hardness of that portion may be measured using the above-mentioned means to determine whether or not that portion is the hard part.

[0038] Next, a rectangular area of ​​3 mm length and 3 mm width at the measurement point of the observation surface of the test piece is taken as the field of view, and measurements are made using EBSD with a measurement interval of 1.0 μm and an acceleration voltage of 15 kV. EBSD pixels are 1.0 μm square. Pixels with a CI value (Confidence interval) of 0.1 or less are considered noise and removed.

[0039] From the obtained measurement results, a PQ (pattern quality) map and a phase map are created by Kikuchi pattern analysis, and the α and β phases are extracted separately. Note that the Kikuchi pattern analysis is performed only on the α and β phases.

[0040] From the obtained phase map, the area ratios of the α phase and β phase, as well as the area ratios of the parts not classified as either the α phase or the β phase, are determined as the area ratios of the remaining structure.

[0041] Next, for the crystal grains identified as α phase from the phase map of the EBSD measurement, in order to distinguish whether these are plate-like structures made of α phase or needle-like structures made of α' martensite phase, the cross section of the hard part is etched to reveal the crystal structure. The cross section to be observed is an arbitrary cross section parallel to the thickness direction, and the etching is performed, for example, by applying an aqueous solution at room temperature containing 2.0 mass% hydrofluoric acid and 6.0 mass% nitric acid to the cross section of the hard part and reacting for about 2 to 10 seconds. Then, crystal grains with a short side width of more than 5 μm are extracted, and the area of ​​the crystal grains with a short side width of more than 5 μm is obtained. In the cross section, crystals with an apparent short side width of more than 5 μm are determined to be plate-like crystals. Note that the thickness direction of the titanium alloy component according to this embodiment is the direction in which stacking proceeds in three-dimensional additive manufacturing, and refers to the direction perpendicular to the powder bed. In the direction perpendicular to the thickness direction (i.e., the direction parallel to the powder bed in 3D additive manufacturing), all directions are considered to be equivalent, so the cross section for microstructural observation can be any cross section parallel to the thickness direction.

[0042] For crystal grains with an apparent short side width of 5 μm or less in a cross section, it is not possible to determine whether they are needle-like or plate-like crystals based on the short side width alone. This is because when the observation surface is formed perpendicular to the plate surface of the plate crystal, the short side width of the plate crystal appears to be 5 μm or less. On the other hand, needle-like crystals and plate-like crystals can be distinguished by evaluating the crystal assembly form. As shown in Figures 1 and 2, needle-like crystals extend in various directions. Plate-like crystals have an assembly form in which flat crystal grains are stacked. Therefore, when the observation surface is formed perpendicular to the plate surface of the plate crystal, the plate crystals appear to be regularly arranged on the observation surface. For example, in Figure 3(d) of the non-patent document, the judgment symbol "α L In the region marked with "," the plate crystals are regularly arranged in an observation plane formed perpendicular to the plate surface of the plate crystal. Therefore, it can be assumed that the regularly arranged crystal grains are plate crystals. In this way, it can be assumed that the crystal grains are needle crystals or plate crystals based on whether the crystal grains are in a stacked aggregate form or in some other aggregate form.

[0043] Next, the shape of the titanium alloy member of this embodiment will be described. The titanium alloy member of this embodiment is manufactured using a three-dimensional additive manufacturing technique as described later, so the shape is not particularly limited. For example, the titanium alloy member may be a simple shape such as a plate, a rod, or a tube. On the other hand, the titanium alloy member may be a complex part shape having one or more selected from a mesh shape part, an extremely thin plate shape part, and a hollow shape part. The titanium alloy member of this embodiment has high strength and can be flexibly designed, so that it can be suitably used as a structural member. The size of the titanium alloy member is not particularly limited, but it may have a part with a thickness of 1 mm or more, and a hard part may be provided at this part.

[0044] Next, an example of a method for manufacturing a titanium alloy part will be described. Although the method for manufacturing the titanium alloy part is not particularly limited, it is preferable to manufacture the titanium alloy part using, for example, a laser-type three-dimensional additive manufacturing technique. The titanium alloy part of this embodiment is manufactured as follows. First, a raw material powder having the above-mentioned chemical components as an average composition is deposited to form a raw material powder layer. Next, a part of the raw material powder layer is melted by a laser beam and then solidified to form a solidified layer. Next, a new raw material powder layer is laminated on the raw material powder layer after melting and solidifying, and the new raw material powder layer is melted and solidified by a laser beam. In this way, after laminating the raw material powder layer and melting and solidifying by the laser beam are repeated several times, the raw material powder in the unsolidified state is removed. In this way, a titanium alloy part is manufactured in which solidified layers melted and solidified by the laser beam are laminated. By adjusting the irradiation range of the laser beam, the titanium alloy part can be formed into a desired shape.

[0045] When a laser beam is irradiated onto a layer of raw powder, the raw powder melts and becomes liquid metal. The laser beam then moves to another location, lowering the temperature of the molten liquid metal, which becomes a solidified layer made of the β phase. The temperature of the solidified layer continues to drop after that, and reaches the α+β phase region. If the solidified layer is rapidly cooled, it will not become an α+β two-phase state, but will form a martensite structure. By cooling the solidified layer at a high rate, for example at 1000 K / s or more, the diffusion of Fe is suppressed and a hard part with a Vickers hardness of 350 HV or more is formed. However, when the above-mentioned manufacturing method is applied to raw material powder having the components of the titanium alloy part according to this embodiment, cracks occur in the titanium alloy part. This is presumably because, under normal conditions for implementing three-dimensional additive manufacturing, the temperature of the molten liquid metal becomes too high, causing a large temperature difference between the molten part and its surrounding area, and the difference in the amount of thermal contraction inside the titanium alloy part due to cooling after solidification becomes large. In order to suppress cracks, a heat input of 30.0 J / mm 3 It is necessary to melt the raw material powder by irradiating the laser under the following conditions. This heat input is a lower value than usual, which is disadvantageous in terms of manufacturing efficiency, but in the manufacturing method of the titanium alloy part according to this embodiment, it is extremely desirable to adopt the above conditions from the viewpoint of suppressing cracks.

[0046] The raw powder has an average particle size of 10 to 50 μm and a standard deviation of the particle size of about 5 to 15 μm. Such raw powder is produced by a method such as gas atomization. The raw powder may be a titanium alloy powder having the above chemical composition, or may be a mixed powder prepared by mixing titanium metal powder, aluminum metal powder, iron powder, chromium metal powder, nickel metal powder, and alloy powder containing a part of each of them to have the above chemical composition.

[0047] The raw powder is deposited on a substrate to form a raw powder layer. The substrate on which the first raw powder layer is deposited may be the bed of a three-dimensional additive manufacturing device, and the substrate on which the second and subsequent raw powder layers are deposited may be the previously formed raw powder layer. The thickness of each raw powder layer may be, for example, 10 to 50 μm.

[0048] Next, a laser beam is irradiated from above the raw material powder layer at a predetermined scanning speed. The irradiation conditions of the laser beam are important in controlling the cooling rate after solidification. In this embodiment, the laser beam irradiation speed is set to P / (V d t) × 10 6 Heat input (J / mm 3 ) to 30.0 (J / mm 3 ) or less. The heat input is limited to 30.0 (J / mm 3 ), the amount of thermal contraction caused by cooling after solidification of the raw material powder layer becomes large, and cracks occur due to the difference in strain between the solidified part and its surrounding area. Here, V is the scanning speed of the laser beam (mm / s), P is the output of the laser beam (W), d is the pitch (μm) of the laser beam trajectory when scanning with the laser beam, and t is the average penetration depth (μm) of the raw material powder layer.

[0049] The scanning speed V is preferably in the range of 400 to 900 mm / s. The laser beam output P may be in the range of 70 to 150 W, or may be in the range of 80 to 120 W. The laser beam pitch d is preferably in the range of 50 to 150 μm. The average penetration depth t is preferably in the range of 50 to 150 μm.

[0050] The beam diameter of the laser beam is preferably in the range of 30 to 70 μm, may be 40 to 60 μm, or may be 45 to 55 μm.

[0051] In addition, the atmosphere during irradiation with the laser beam is preferably an inert gas atmosphere such as argon in order to prevent oxidation of the titanium alloy.

[0052] By going through the above steps, a titanium alloy part having a hard portion with a Vickers hardness of 350 HV or more can be manufactured.

[0053] According to the titanium alloy part of this embodiment, the metal structure is mainly composed of needle-shaped crystals, and these needle-shaped crystals have a higher Vickers hardness than the α phase of titanium, so that the titanium alloy part of this embodiment can exhibit high strength characteristics. The needle-shaped crystals in the titanium alloy part of this embodiment are presumed to be α' martensite structures. In addition, the titanium alloy part of the present embodiment does not contain V, but contains at least one of Fe, Cr, and Ni, Al, with the balance being Ti and impurities. Although it does not contain V, it has needle-like crystals that are presumed to be α' martensite structures, and a titanium alloy part having higher strength than conventional α+β type Ti-Al-Fe alloys can be realized.

[0054] As described above, the titanium alloy part according to this embodiment is extremely useful as a mechanical structural part. On the other hand, it is also extremely useful to use the titanium alloy part according to this embodiment as an intermediate material to manufacture a titanium alloy part having different properties. Specifically, it has been found that a titanium alloy part having random crystal orientation and fine equiaxed crystal grains can be obtained by rapidly heating the titanium alloy part according to this embodiment, hot working it, and then rapidly cooling it. The obtained titanium alloy part has high strength and excellent fatigue strength.

[0055] Based on the above findings, a method for producing a titanium alloy part according to another embodiment of the present invention will be described. The method for producing a titanium alloy part according to another embodiment of the present invention includes the steps of heating the titanium alloy part according to the present embodiment described above to a temperature in the range of (β transformation temperature -200) ℃ or more and (β transformation temperature -100) ℃ or less at an average heating rate of 50 ℃ / sec or more, hot working the titanium alloy part in this temperature range under the conditions of a strain rate of 0.10 to 10 / sec and a total strain of more than 0.50, and cooling the hot-worked titanium alloy part at an average cooling rate of 20 ℃ / sec or more. Hereinafter, for convenience, the titanium alloy part used as an intermediate material in this manufacturing method will be referred to as a "first titanium alloy part", and the titanium alloy part obtained by this manufacturing method will be referred to as a "second titanium alloy part".

[0056] First, the first titanium alloy member, which is an intermediate material, is heated to a target temperature within the temperature range of (β transformation temperature -200) ° C. or more and (β transformation temperature -100) ° C. or less at an average heating rate of 50 ° C. / sec or more. By rapidly heating the intermediate material at an average heating rate of 50 ° C. / sec or more, the intermediate material can be heated to a high temperature range suitable for hot working before alloying elements such as Fe diffuse from the α' martensite structure, and a fine α + β structure can be formed directly from the α' martensite structure. If the average heating rate when heating the intermediate material is low, alloying elements such as Fe diffuse from the α' martensite structure during heating, transforming to the α phase, and coarse α crystal grains grow. This reduces the fatigue strength of the second titanium alloy member. The faster the average heating rate, the more preferable, and more preferably 60 ° C. / sec or more, and even more preferably 80 ° C. / sec or more. The average heating rate here refers to the average heating rate at which the surface temperature of the intermediate material reaches the target temperature from 700 ° C. In other words, the average heating rate is calculated by subtracting 700°C from the target temperature and dividing the result by the time it takes for the surface temperature of the intermediate material to reach the target temperature from 700°C.

[0057] The temperature (maximum heating temperature) reached after rapid heating is preferably in the range of (β transformation temperature -200) ° C. or more and (β transformation temperature -100) ° C. or less. If the temperature reached is less than (β transformation temperature -200) ° C., the load required for processing in the subsequent hot working increases and the deformability of the material decreases. As a result, voids and cracks are generated inside the material, and the fatigue properties of the second titanium alloy member decrease. Also, if the temperature reached exceeds (β transformation temperature -100) ° C., the strength and fatigue properties decrease. This is presumably because a part of the α' martensite structure transforms into an α + β structure during processing of the first titanium alloy member and grows, and it is not possible to form a fine α + β structure directly from the α' martensite structure, and the α phase grows excessively, resulting in an increase in the average circle equivalent diameter of the equiaxed crystal grains. A more preferable temperature reached is in the range of (β transformation temperature -150) ° C. or more and (β transformation temperature -100) ° C. or less. The reached temperature is the surface temperature of the intermediate material.

[0058] The heated first titanium alloy member is then hot worked. The number of times of hot working may be one or more. In addition, it is preferable to start hot working immediately after the intermediate material reaches the target temperature, for example, it is preferable to start hot working within 10 seconds from the time when the intermediate material reaches the target temperature. If the time from the time when the target temperature is reached to the start of hot working is long, it is considered that alloy elements such as Fe will diffuse from the α' martensite structure and transform into α+β phase, making it impossible to obtain a preferable metal structure. More preferably, it is preferable to start hot working within 5 seconds from the time when the target temperature is reached.

[0059] The strain rate during hot working is preferably in the range of 0.10 to 10 / sec. If the strain rate is less than 0.10 / sec, the strength and fatigue properties of the second titanium alloy member are reduced. This is presumably because a part of the α' martensite structure is transformed into an α+β structure during hot working of the first titanium alloy member, causing the α phase to grow excessively, and the average equivalent circle diameter of the equiaxed crystal grains becomes large. The higher the strain rate, the more preferable it is. However, if the strain rate exceeds 10 / sec, the effect of improving the strength and fatigue properties is saturated. Therefore, the upper limit of the strain rate during hot rolling is set to 10 / sec or less.

[0060] In addition, the total strain amount when hot working is performed once or twice or more is preferably more than 0.50. If the total strain amount is less than 0.50, the fatigue properties of the titanium alloy member are deteriorated. This is presumably because sufficient nucleation is not obtained to directly form a fine α+β structure from the α' martensite structure, and a part of it remains unrecrystallized.

[0061] The first titanium alloy member is cooled immediately after hot working. This freezes the structure. The cooling method is preferably water cooling. The average cooling rate during cooling is preferably 20°C / sec or more. If the average cooling rate is less than 20°C / sec, the fatigue properties of the titanium alloy member are reduced. This is presumably because the average circle equivalent diameter of the equiaxed crystal grains increases during cooling. The average cooling rate is the average cooling rate from the start of cooling to 700°C. In other words, the average cooling rate is the value obtained by dividing the temperature difference between the surface temperature of the intermediate material at the start of cooling and 700°C by the time required for the surface temperature of the intermediate material to decrease to 700°C from the start of cooling of the intermediate material. The cooling end temperature is not particularly limited, but is preferably 700°C or less, for example.

[0062] It is preferable that the time required from the end of hot working to the start of cooling is as short as possible, for example, within 5 seconds, and more preferably within 3 seconds. If the time required from the end of hot working to the start of cooling is long, the fatigue properties of the second titanium alloy component are deteriorated. This is presumably because the average equivalent circle diameter of the equiaxed crystal grains increases. Note that "the start of cooling" refers to the time when accelerated cooling is started on the first titanium alloy component after hot working is completed. When the accelerated cooling method is water cooling, the time when accelerated cooling is started refers to the time when cooling water is started to be poured on the first titanium alloy component after hot working is completed.

[0063] By sequentially carrying out the above steps, the second titanium alloy part is obtained. EXAMPLES

[0064] The present invention will be described in more detail below with reference to examples. The present invention is of course not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, all of which are included in the technical scope of the present invention.

[0065] (Example 1: First titanium alloy member) Titanium alloy powder having the chemical composition shown in Table 1 was prepared as the raw material powder. The average particle size of the raw material powder was as shown in Table 1. The standard deviation of the particle size of the raw material powder was within the range of 5 to 15 μm. In Table 1 and other tables described later, values ​​outside the range of the invention are underlined.

[0066] The first titanium alloy member was manufactured by three-dimensional additive manufacturing using the prepared raw material powder. Specifically, the raw material powder was first deposited to form a raw material powder layer with a thickness of 30 μm, and then a part of the raw material powder layer was melted by a laser beam and then solidified to form a solidified layer. Next, a new raw material powder layer was laminated with a thickness of 30 μm on the raw material powder layer after melting and solidifying, and the new raw material powder layer was melted and solidified by a laser beam. In this way, the lamination of the raw material powder layer and the melting and solidifying by the laser beam were repeated several times, and then the raw material powder in the unsolidified state was removed. As a result, a first titanium alloy member was manufactured in which solidified layers melted and solidified by the laser beam were laminated. Hereinafter, in this experiment, the first titanium alloy member is simply referred to as a titanium alloy member.

[0067] The shape of the titanium alloy part was a rod-shaped evaluation part with a length of 32 mm, a width of 6.25 mm, and a thickness of 4.0 mm, and a grip part with a maximum width of 15 mm and a length of 19 mm provided on both ends of the longitudinal direction of the evaluation part. Here, the thickness direction is the direction in which deposition proceeds in three-dimensional additive manufacturing, and refers to the direction perpendicular to the powder bed.

[0068] The conditions for irradiating the laser beam were as shown in Table 2. The diameter of the laser beam was 50 μm, and the atmosphere during irradiation of the laser beam was an argon gas atmosphere.

[0069] The crystal structure of the obtained titanium alloy part was measured. First, a test piece was taken from the 3.13 mm wide evaluation part of the titanium alloy component, with a cross section parallel to the thickness direction as the observation surface. The measurement point on the observation surface was at a depth of t / 4 in the direction of the thickness t of the evaluation part. Next, a rectangular area of ​​3 mm length and 3 mm width at the measurement point on the observation surface of the test piece was set as the field of view, and measurements were performed using EBSD at a measurement interval of 2.0 μm and an acceleration voltage of 15 kV. From the obtained measurement results, a PQ (pattern quality) map and a phase map were created by Kikuchi pattern analysis, and the β phase was extracted to determine the area ratio of β crystal grains in the metal structure. The area ratio of β crystal grains was taken as the area ratio of the remaining structure. Note that no remaining structure other than β crystal grains was confirmed in any of the samples. In this embodiment, since all directions perpendicular to the thickness direction are considered to be equivalent, any cross section parallel to the thickness direction may be used as the observation surface. In this example, a test piece was prepared from the center position of the width of the evaluation portion of the titanium alloy component.

[0070] In order to distinguish whether the crystal grains identified as α phase from the phase map of the EBSD measurement are plate-like structures made of α phase or needle-like structures made of α' martensite phase, the observation surface of the sample was etched to reveal the crystal structure. The cross section to be observed was a cross section parallel to the thickness direction, as in the EBSD measurement. An aqueous solution at room temperature containing 2.0 mass% hydrofluoric acid and 6.0 mass% nitric acid was applied to the cross section of the hard part and reacted for about 2 to 10 seconds, thereby etching the observation surface of the test piece to reveal the crystal structure of the hard part. Then, needle-like crystals and plate-like crystals were distinguished based on the procedure described in Figure 3.

[0071] The Vickers hardness of each titanium alloy member was also measured. The load for pressing the Vickers indenter was set to 5 kgf. The results are shown in Table 3.

[0072] [Table 1]

[0073] [Table 2]

[0074] [Table 3]

[0075] As shown in Table 3, the titanium alloy members of Test Examples 2 to 4, 6 to 16, and 18 to 24 had chemical compositions that satisfied the ranges of the present invention, and the heat input was 30.0 J / mm 3 As a result, a hard portion having a Vickers hardness of 350 HV or more was formed.

[0076] Figures 1 and 2 show electron microscope photographs of Test Example 3. Figures 1 and 2 are photographs taken from different fields of view. As shown in Figures 1 and 2, it can be seen that the metal structure of Test Example 3 mainly contains needle-shaped crystals.

[0077] On the other hand, in Test Example 1, the heat input during manufacturing was 30.0 J / mm 3 However, since the amount of one or more elements selected from the group consisting of Fe, Cr, and Ni was less than the range of the present invention, there was no hard portion with a Vickers hardness of 350 HV or more.

[0078] In addition, in Test Example 5, the heat input during manufacturing was 30.0 J / mm 3 However, since the amount of one or more elements selected from the group consisting of Fe, Cr, and Ni was more than the range of the present invention, there was no hard portion with a Vickers hardness of 350 HV or more.

[0079] In Test Example 17, the chemical composition was within the range of the present invention, but the heat input was 30.0 J / mm 3 Therefore, there was no hard portion with a Vickers hardness of 350 HV or more.

[0080] In addition, in Test Example 25, a titanium alloy having the chemical composition shown in Table 2 was heated to the β-phase temperature range and then rapidly cooled at a cooling rate of 300°C / sec. Therefore, the additive manufacturing conditions for Test Example 25 are indicated as "-". Test Example 25 had chemical compositions that met the ranges of the present invention, but did not have a hard part with a Vickers hardness of 350HV or more. This is presumably due to an insufficient cooling rate.

[0081] (Example 2: Second titanium alloy member) A first titanium alloy member having a length of 80 mm, a width of 25 mm, and a thickness of 25 mm was prepared by the same procedure as in the above-mentioned test examples 1 to 25, and this was used as an intermediate material, and hot working was performed under the conditions shown in Table 4 to manufacture a second titanium alloy member. Specifically, the intermediate material was rapidly heated to reach the final temperature, and then hot working was performed once or more, and was immediately quenched after the hot working was completed. The time required from the point at which the surface temperature of the intermediate material reached the final temperature to the start of hot working was within 5 seconds, and the time required from the end of hot working to the start of cooling was also within 5 seconds. In this way, the second titanium alloy members of test examples 1 to 25 were manufactured. Hereinafter, in this experiment, the second titanium alloy member is simply referred to as a titanium alloy member.

[0082] The fatigue strength of the titanium alloy members of Test Examples 1 to 25 was also measured. The fatigue strength was measured on round bar test pieces with circular cross sections taken from these titanium alloy members. The longitudinal direction of the parallel portion of the round bar test pieces was aligned with the longitudinal direction of the titanium alloy members. The parallel portion of the round bar test pieces was polished to a surface roughness of at least #600 abrasive paper. A rotating bending fatigue test was performed in air at 25°C, at 360 rpm, and with a stress ratio R of -1.0, using an Ono-type rotating bending tester. 1×10 7 The maximum stress at which fatigue failure did not occur even when stress loading was repeated up to 1000 times was defined as the fatigue strength. The results are shown in Table 5. Titanium alloy parts with a fatigue strength of 625 MPa or more were considered to have passed the fatigue strength test. Values ​​that did not meet the pass / fail criteria are underlined.

[0083] Furthermore, the tensile strength of the titanium alloy members of Test Examples 1 to 25 was measured. The tensile strength was measured using ASTM half-size tensile test pieces (parallel part width 6.25 mm, parallel part length 32 mm, gauge length 25 mm) taken from the titanium alloy members. The longitudinal direction of the parallel part of the tensile test piece was aligned with the longitudinal direction of the titanium alloy member. In the atmosphere at 25°C, the strain rate was 0.5% / min up to a strain of 1.5%, and then 30% / min until fracture. The tensile strength at this time was measured. The results are shown in Table 5. Titanium alloy members with a tensile strength of 1100 MPa or more were deemed to have passed the tensile strength test. Values ​​that did not meet the pass / fail criteria were underlined.

[0084] As shown in Table 5, the titanium alloy members of Test Examples 2 to 4, 6 to 16, and 18 to 20 had chemical compositions that satisfied the ranges of the present invention, and the manufacturing conditions that satisfied the ranges of the present invention, and therefore exhibited high fatigue strength and tensile strength.

[0085] On the other hand, in Test Example 1, the amount of one or more elements selected from the group consisting of Fe, Cr, and Ni was small, and the intermediate material did not have a hard portion. As a result, the fatigue strength and tensile strength of the titanium alloy part of Test Example 1 were insufficient. In Test Example 5, the amount of one or more elements selected from the group consisting of Fe, Cr, and Ni was excessive, and the intermediate material did not have a hard portion. As a result, the fatigue strength and tensile strength of the titanium alloy part of Test Example 5 were insufficient. In Test Example 17, the heat input during production of the intermediate material was 30.0 J / mm 3 As a result, the fatigue strength and tensile strength of the titanium alloy part of Test Example 17 were insufficient.

[0086] In Test Example 21, the average heating rate before hot working of the intermediate material was low, so the fatigue strength and tensile strength were insufficient. In Test Example 22, the strain rate during hot working of the intermediate material was low, so the fatigue strength and tensile strength were insufficient. In Test Example 23, the total strain amount during hot working of the intermediate material was small, so the fatigue strength and tensile strength were insufficient. In Test Example 24, the average cooling rate after hot working was low and cooling took a long time, so the fatigue strength and tensile strength were insufficient.

[0087] In the test example 25, the intermediate material was not manufactured by the laser-type three-dimensional additive manufacturing method, but was a cast product of a titanium alloy. Therefore, the fatigue strength and tensile strength of the test example 25 were insufficient.

[0088] [Table 4]

[0089] [Table 5]

Claims

1. Chemical composition, by mass%, Al: 4.0-9.0%, One or more selected from the group consisting of Fe, Cr, and Ni: 0.5 to 2.5% in total, C: 0-0.100%, N: 0-0.100%, H: 0 to 0.100%, and O: 0-0.500% with the remainder being Ti and impurities, The hard portion has a Vickers hardness of 350 HV or more. The metal structure in a cross section of the hard portion is composed of plate-like crystals having a short side width of 5 μm or more and made of an α phase in a laminated aggregate form, needle-like crystals made of an α phase other than the plate-like crystals, and a remaining structure other than the α phase, The total amount of the plate crystals and the remaining structure in a cross section of the hard portion is 10.0 area% or less, The titanium alloy member has a cross section of the hard portion in which the plate-like crystals account for 0 to 2.0% by area.

2. 2. The titanium alloy part according to claim 1, wherein the hard portion is disposed at a depth of 0.5 mm or more from the surface of the titanium alloy part.

3. 3. The titanium alloy part according to claim 1, further comprising at least one selected from the group consisting of a mesh-shaped part, an extremely thin plate-shaped part, and a hollow-shaped part.

4. Chemical composition, by mass%, Al: 4.0-9.0%, One or more selected from the group consisting of Fe, Cr, and Ni: 0.5 to 2.5% in total, C: 0-0.100%, N: 0-0.100%, H: 0 to 0.100%, and O: 0-0.500% The raw material powder contained 30.0 J / mm 3 A step of melting the raw material powder by irradiating a laser under the following conditions: a step of quenching the molten raw material powder; The method for producing a titanium alloy part according to any one of claims 1 to 3, comprising:

5. A process of heating the titanium alloy part according to any one of claims 1 to 3 as an intermediate material at an average heating rate of 50 ° C. / sec or more to an ultimate temperature within a temperature range of (β transformation temperature - 200) ° C. or more and (β transformation temperature - 100) ° C. or less; hot working the titanium alloy component in the temperature range at a strain rate of 0.10 to 10 / sec and a total strain of more than 0.50; and cooling the hot worked titanium alloy component at an average cooling rate of 20° C. / sec or more; The method for producing a titanium alloy part, wherein the hot working is started within 10 seconds after the titanium alloy part is heated to the ultimate temperature.

Citation Information

Patent Citations

  • Manufacturing method of fuel pin

    JP1979019098A

  • Α+β type titanium alloy extruded shape

    JP2018154922A

  • α+β type titanium alloy

    JP3076697B2

  • Nanocrystalline titanium alloy and method for manufacturing the same

    JP4766408B2

  • Heat treatment method for improving mechanical property of metal product manufactured by 3D printing

    KR1020170019558A