Coated Tools

A coated tool with Al-rich AlCr nitride or carbonitride, optimized via sputtering, addresses droplet defects and wear resistance issues in small-diameter tools, achieving superior durability and wear resistance.

JP7594220B2Active Publication Date: 2024-12-04MOLDINO TOOL ENG LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023542461
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-19
Filing Date
2022-08-19
Publication Date
2024-12-04
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

Small-diameter tools coated with Al-rich AlCr nitride using arc ion plating suffer from droplet defects, which degrade tool durability, and sputtering methods, while improving droplet reduction, compromise wear resistance.

Method used

A coated tool with a hard coating composed of Al-rich AlCr nitride or carbonitride, containing specific atomic percentages of Al, Cr, and controlled crystal orientation, applied via sputtering to enhance durability and wear resistance, with a face-centered cubic lattice structure and optimized X-ray intensity distribution.

Benefits of technology

The coated tool achieves improved durability and wear resistance comparable to arc ion plating methods, with reduced droplet defects and enhanced adhesion, suitable for small-diameter tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594220000004
    Figure 0007594220000004
  • Figure 0007594220000005
    Figure 0007594220000005
  • Figure 0007594220000006
    Figure 0007594220000006
Patent Text Reader

Abstract

A coated tool according to the present invention comprises a base material and a hard coating film on the base material. The hard coating film has a face-centered cubic lattice structure and is formed of a nitride or a carbonitride containing 65-90 at.% of Al, 10-35 at.% of Cr, and not more than 0.50 at.% of argon (Ar), with respect to the total amount of metal (including semi-metal) elements. The hard coating film exhibits, in an X-ray intensity distribution along the α-axis in a positive electrode dot diagram relating the (111) surface of the face-centered cubic lattice structure, a maximum intensity Ia in the α angle range of 80-90°, and the intensity Ia in the α angle range of 0-70° is not more than 35% of the maximum intensity Ia.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated tool applied to tools such as dies and cutting tools. This application claims priority based on Japanese Patent Application No. 2021-134034, filed on August 19, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] AlCr nitride is a film type with excellent wear resistance and heat resistance, and is widely used as a coated metal mold or a coated cutting tool. In recent years, coated tools coated with Al-rich AlCr nitride with an Al content of more than 70 atomic % by arc ion plating have been proposed (Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-032861 A [Patent Document 2] JP 2018-059146 A [Patent Document 3] JP 2020-040175 A Summary of the Invention [Problem to be solved by the invention]

[0004] In small-diameter tools with a tool diameter of 2 mm or less, the effect of droplets on tool performance tends to be large. The inventors confirmed that Al-rich AlCr nitride coated by the arc ion plating method tends to have a large number of droplets, and that there is room for improvement in the durability of the tool. The droplets can be reduced by using a sputtering method to form a hard coating. However, when a hard coating is formed simply by using a sputtering method, the hard coating may have inferior wear resistance to a hard coating formed by using an arc ion plating method. In view of the above circumstances, an object of the present invention is to provide a coated tool provided with an Al-rich AlCr nitride or carbonitride which reduces droplets by applying a sputtering method while achieving durability equal to or greater than that achieved by an arc ion plating method. [Means for solving the problem]

[0005] A coated tool according to one embodiment of the present invention is a coated tool having a substrate and a hard coating on the substrate, The hard coating is a nitride or carbonitride containing 65 atomic % or more and 90 atomic % or less of Al and 10 atomic % or more and 35 atomic % or less of Cr, both relative to the total amount of metal elements (including metalloid elements), and 0.50 atomic % or less of argon (Ar), both relative to the total amount of metal elements (including metalloid elements) and nonmetallic elements, and has a face-centered cubic lattice structure; The hard coating is a coated tool in which, in an X-ray intensity distribution of the α axis of a pole figure for a (111) plane of a face-centered cubic lattice structure, the maximum intensity Ia is exhibited in an α angle range of 80° to 90°, and the intensity in an α angle range of 0° to 70° is 35% or less of the Ia.

[0006] The intensity in the α angle range of 0° to 70° is preferably 30% or less of the intensity Ia. In the hard coating, the (111) plane of the face-centered cubic lattice structure preferably exhibits maximum intensity in the intensity profile of an X-ray diffraction or selected area diffraction pattern obtained by a transmission electron microscope. Effect of the Invention

[0007] According to the present invention, it is possible to obtain a coated tool having excellent durability and provided with a sputtered coating of Al-rich AlCr nitride or carbonitride. [Brief description of the drawings]

[0008] [Figure 1] 2 is an example of an X-ray intensity distribution of the α axis of a pole figure for a (111) plane in the AlCr nitride of this Example 1. [Diagram 2]2 is an example of an X-ray intensity distribution of the α axis of a pole figure for a (200) plane in the AlCr nitride of this Example 1. [Diagram 3] 2 is an example of an X-ray intensity distribution of the α axis of a pole figure for a (111) plane in the AlCr nitride of Comparative Example 1. [Figure 4] 2 is an example of an X-ray intensity distribution of the α axis of a pole figure for a (200) plane in the AlCr nitride of Comparative Example 1. [Diagram 5] 1 is an example of an XRD measurement result of this Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present inventors have found that the durability of Al-rich AlCr nitride or carbonitride produced by sputtering tends to improve by controlling the orientation of the crystals with a face-centered cubic lattice structure. Hereinafter, the details of the embodiment of the present invention will be described. The coated tool of this embodiment is a coated tool having an Al-rich nitride or carbonitride mainly composed of Al and Cr on the surface of a substrate. The coated tool of this embodiment can be applied to dies and cutting tools. In particular, it is preferably applied to small-diameter end mills having a tool diameter of 5 mm or less, and more preferably 3 mm or less.

[0010] In this embodiment, the substrate is not particularly limited. Cold work tool steel, hot work tool steel, high speed steel, cemented carbide, etc. may be appropriately applied depending on the application. The substrate may be previously subjected to nitriding treatment, bombardment treatment, etc.

[0011] The hard coating according to the present embodiment is a nitride or carbonitride, and contains 65 atomic % to 90 atomic % of Al and 10 atomic % to 35 atomic % of Cr relative to the total amount of metal elements (including metalloids; the same applies below). Nitrides or carbonitrides mainly containing Al and Cr are a type of film that is excellent in balance between wear resistance and heat resistance, and also has excellent adhesion to the substrate, and the heat resistance of the hard coating is further improved by increasing the Al content ratio in particular. The hard coating according to the present embodiment is preferably a nitride that has excellent heat resistance. In addition, by increasing the Al content ratio, an oxidation protective coating is easily formed on the tool surface, and the coating structure becomes fine, making it easier to suppress wear of the hard coating due to welding.

[0012] In order to fully exert the above-mentioned effect of adding Al, the hard coating according to this embodiment has an Al content of 65 atomic % or more when the total metal elements are taken as 100 atomic %. More preferably, the Al content is 70 atomic % or more. More preferably, the Al content is 75 atomic % or more. On the other hand, if the Al content is too high, the crystal structure of the hard coating changes and becomes brittle. Therefore, the hard coating according to this embodiment has an Al content of 90 atomic % or less when the total metal elements are taken as 100 atomic %. More preferably, the Al content is 85 atomic % or less. More preferably, the Al content is 78 atomic % or less.

[0013] In the hard coating according to the present embodiment, the Cr content is set to 10 atomic % or more when the total metal elements are taken as 100 atomic %. This makes it easier to form a uniform and dense oxidation protective coating on the tool surface during machining, and makes it easier to suppress tool damage. Furthermore, it is preferable that the Cr content is set to 15 atomic % or more. On the other hand, if the Cr content in the hard coating is too high, it is difficult to obtain the above-mentioned effect of increasing the Al content. Therefore, in the hard coating according to the present embodiment, the Cr content is set to 35 atomic % or less when the total metal elements are taken as 100 atomic %. Furthermore, it is preferable that the Cr content is 30 atomic % or less. Furthermore, it is preferable that the Cr content is 25 atomic % or less. Furthermore, it is preferable that the Cr content is 20 atomic % or more.

[0014] In the hard coating according to this embodiment, the total content of Al and Cr is preferably 90 atomic % or more when the total metal elements are taken as 100 atomic %. The hard coating according to this embodiment may be a nitride or carbonitride of Al and Cr. The content ratio of the metal element in the hard coating according to the present embodiment can be measured by using an electron probe microanalyzer (EPMA) for the mirror-finished hard coating. In this case, for example, after mirror-finishing the hard coating surface, the content ratio can be determined from the average of five analysis points with a diameter of about 1 μm.

[0015] The hard coating according to the present embodiment may contain metal elements other than Al and Cr. For example, the hard coating according to the present embodiment may contain one or more elements selected from the elements of Groups 4a, 5a, and 6a of the periodic table and Si, B, Y, Yb, and Cu for the purpose of improving wear resistance and heat resistance. These elements are generally contained in order to improve the coating properties of the coated tool, and can be added within a range that does not significantly reduce the durability of the coated tool. However, if the content ratio of metal elements other than Al and Cr is too high, the durability of the coated tool may be reduced. Therefore, when the hard coating according to the present embodiment contains metal elements other than Al and Cr, the total content ratio is preferably 10 atomic % or less when the total metal elements are 100 atomic %. More preferably, it is 5 atomic % or less.

[0016] The hard coating according to the present embodiment contains argon (Ar) at 0.50 atomic % or less with respect to the total amount of metallic elements and nonmetallic elements. The hard coating according to the present embodiment is a sputtered coating, i.e., a sputtered hard coating. The occurrence frequency of droplets, which become defects in the hard coating, can be reduced by applying a sputtering method. On the other hand, in the sputtering method, the target components are sputtered using argon ions, so the hard coating coated by the sputtering method contains a fair amount of argon. In particular, argon tends to concentrate at the grain boundaries, and the argon content tends to increase when the grain size becomes fine. However, when the argon content increases, the bonding force between particles at the grain boundaries decreases. In a hard coating having a high Al content, such as the hard coating according to the present embodiment, excessive argon can become a defect, so it is effective to keep the content below a certain level. Specifically, the hard coating according to this embodiment contains argon in an amount of 0.50 atomic % or less, and more preferably 0.40 atomic % or less, based on the total amount of metallic elements and non-metallic elements. The hard coating according to this embodiment may contain a rare gas other than argon if sputtering is performed using a mixed gas containing a rare gas other than argon.

[0017] In the sputtering method, if the content ratio of argon in the hard coating is made as close as possible to 0 atomic %, the flow rate of argon becomes too small, and sputtering becomes unstable. Even if the content ratio of argon approaches 0 atomic %, the basic properties of the hard coating applied to cutting tools, such as toughness, heat resistance, and wear resistance, may be impaired. Although the lower limit of the content ratio of argon in the hard coating according to this embodiment is not particularly limited, in order to stabilize the sputtering method and ensure the basic film properties of the hard coating applied to coated tools, it is preferable that argon is contained at 0.02 atomic % or more with respect to the total amount of metal elements and nonmetal elements. Furthermore, it is preferable that the content ratio of argon is 0.05 atomic % or more. It is further preferable that argon is 0.10 atomic % or more.

[0018] The nitrogen and argon content ratios of the hard coating according to this embodiment can be measured by using an electron probe microanalyzer (EPMA) for the mirror-finished hard coating in the same manner as in the measurement of the content ratios of the metal elements described above. As in the measurement of the content ratios of the metal elements described above, the nitrogen and argon content ratios can be determined by averaging five analysis points in an analysis range of about 1 μm in diameter after mirror finishing. The hard coating according to this embodiment may contain trace amounts of argon, oxygen, and carbon as non-metallic elements in addition to nitrogen.

[0019] <Crystal structure> The hard coating according to the present embodiment has a face-centered cubic lattice structure, and in the X-ray intensity distribution of the α axis of the pole figure for the (111) plane of the face-centered cubic lattice structure, the maximum intensity Ia is shown in the range of α angles of 80° to 90°, and the intensity in the range of α angles of 0° to 70° is 35% or less of the maximum intensity Ia. As a result, the intensity in the range of α angles of 0° to 70° is relatively low compared to the maximum intensity at α angles of 80° to 90°, and most of the (111) planes are present at α angles of 80° to 90°, which are almost perpendicular to the substrate plane direction. It is believed that the orientation of the (111) planes in a direction almost perpendicular to the substrate plane direction makes the entire hard coating denser, improving durability. It is preferable that the maximum intensity Ia is shown in the range of α angles of 85° to 90°. It is preferable that the intensity of the (111) plane in the range of α angles of 0° to 70° is 30% or less, more preferably 25% or less, of the maximum intensity Ia. In the hard coating according to the present embodiment, the (111) plane of the face-centered cubic lattice structure preferably exhibits the maximum intensity in the intensity profile of an X-ray diffraction or electron beam diffraction pattern. It is believed that the wear resistance of the hard coating is enhanced and the durability of the coated tool is improved by orienting the (111) planes of the face-centered cubic lattice structure exhibiting the maximum intensity in approximately the same direction. In X-ray diffraction, the peak intensity of the (111) plane is preferably four times or more than the peak intensity of the (200) plane. With these configurations, the wear resistance of the hard coating is further improved, and the durability of the coated tool is further improved. The upper limit of the peak intensity ratio of the (111) plane to the (200) plane is preferably 8 or less.

[0020] <Middle film, upper layer> In order to further improve the adhesion of the hard coating to the coated tool of this embodiment, an intermediate coating may be provided between the substrate of the tool and the hard coating, if necessary. For example, a layer made of a metal, nitride, carbonitride, or carbide may be provided between the substrate of the tool and the hard coating. Moreover, a hard coating having a different component ratio or composition from that of the hard coating of the present embodiment may be formed separately on the hard coating of the present embodiment.Furthermore, the hard coating of the present embodiment and another hard coating having a different component ratio or composition from that of the hard coating of the present embodiment may be laminated together.

[0021] <Droplet> In the hard coating according to this embodiment, droplets with a circle equivalent diameter of 1 μm or more are 100 μm in cross-section observation. 2 It is preferable that the number of droplets is 5 or less per unit area. In the arc ion plating method, the "droplet" refers to a deposit on the hard coating caused by molten particles of about 1 to several tens of μm flying out from the cathode. In the sputtering method, the "droplet" refers to a deposit on the hard coating caused by metal particles of about 1 to several tens of μm flying out suddenly from the target.

[0022] In hard coatings coated by physical vapor deposition, droplets can be the main physical defect. In particular, coarse droplets with a circle equivalent diameter of 1 μm or more can be the starting point of fracture inside the hard coating, so the toughness of the hard coating can be increased by reducing the frequency of their occurrence. In this embodiment, droplets with a circle equivalent diameter of 1 μm or more were measured in a cross-sectional observation of the hard coating, and the droplets were measured in a cross-sectional observation of 100 μm. 2 It is preferable to set the number of particles per 100 μm or less. 2 More preferably, the number of particles is 3 or less per 100 μm. 2 It is further preferred that the droplets do not contain droplets with an equivalent circle diameter of 5 μm or more. In addition, on the surface of the hard coating, droplets with a circle equivalent diameter of 1 μm or more were observed to be 100 μm in diameter. 2 More preferably, the droplets on the surface of the hard coating are 100 μm or less. 2 More preferably, the droplets on the surface of the hard coating are 100 μm or less. 2 There is less than one per prize.

[0023] To evaluate droplets in cross-sectional observation of a hard coating, the hard coating is mirror-finished, processed by a focused ion beam method, and the mirror-finished surface is observed in multiple fields of view at 5,000 to 10,000 times magnification using a transmission electron microscope. The number of droplets on the surface of the hard coating can be determined by observing the surface of the hard coating using a scanning electron microscope (SEM) or the like.

[0024] <Manufacturing method> In the coating of the hard film according to the present embodiment, it is preferable to use a sputtering method in which three or more AlCr-based alloy targets are used, power is applied to the targets in sequence, and when the target to which power is applied is switched, a time is provided in which power is applied simultaneously to both the target to which power application ends and the target to which power application starts. In such a sputtering method, the ionization rate of the target is maintained high during coating, and a hard film that is dense at the micro level is obtained, and the amount of argon and oxygen that is inevitably contained tends to be small. In addition, it is preferable that the temperature inside the furnace of the sputtering device is 350°C to 500°C, the negative pressure bias voltage applied to the substrate is -200V to -70V, and the furnace pressure is 0.1Pa to 0.4Pa by introducing Ar gas and N2 gas. In addition, when coating with carbonitride, a small amount of carbon may be added to the target, or a part of the reaction gas may be replaced with methane gas.

[0025] The maximum power density of the power pulse is 0.1kW / cm 2 It is preferable that the density is 0.3 kW / cm or more. 2 It is preferable that the energy of the film-forming ions in this composition system is too high, otherwise the hcp structure will be easily formed. Therefore, the maximum power density of the power pulse is 0.7 kW / cm 2 It is preferable to set it to 0.6 kW / cm or less. 2The duration of the power pulse applied to each target is preferably 30 milliseconds or less. The duration of the power pulse applied to each target is preferably 30 milliseconds or less. In addition, the duration of the power application to both the alloy target to which the power application is terminated and the alloy target to which the power application is initiated is preferably 20 microseconds or more and 100 microseconds or less. EXAMPLES

[0026] <Base material> As the substrate, a two-blade ball end mill made of cemented carbide with the composition WC (bal.)-Co (8.0 mass%)-VC (0.3 mass%)-Cr3C2 (0.5 mass%) and hardness of 94.0 HRA (Rockwell hardness, value measured in accordance with JIS G 0202) was prepared.

[0027] A sputtering device capable of mounting six sputter evaporation sources was used in this Example 1 and Comparative Example 3. Among these evaporation sources, six Al75Cr25 alloy targets (numerical values ​​are atomic ratios, the same applies below) were installed in the device as evaporation sources to coat the hard coating. A sputtering device capable of mounting six sputter evaporation sources was used in Comparative Example 2. Among these evaporation sources, six Al80Cr20 alloy targets were installed in the device as evaporation sources for coating a hard film. The tool, which is the substrate, was fixed to the sample holder in the sputtering device, and a bias power supply was connected to the tool. The bias power supply was designed to apply a negative bias voltage to the tool independently of the target. The tool rotated at two revolutions per minute and revolved around the fixture and sample holder. The distance between the tool and the target surface was 100 mm. The gases used were Ar and N2, and were introduced from a gas supply port provided in the sputtering device.

[0028] <Bombardment Processing> First, before coating the tool with a hard coating, the tool was bombarded in the following manner. The furnace temperature was raised to 400°C by the heater in the sputtering device, and the tool was heated for 30 minutes. After that, the sputtering device was evacuated to a vacuum, and the pressure in the furnace was reduced to 5.0×10 -3 Pa or less. Then, Ar gas was introduced into the furnace of the sputtering device, and the pressure inside the furnace was adjusted to 0.8 Pa. Then, a DC bias voltage of -170 V was applied to the tool, and cleaning (bombardment treatment) of the tool with Ar ions was performed for 20 minutes or more.

[0029] <Hard coating> In the coating of this Example 1, the temperature inside the furnace was set to 400°C, and Ar gas (0.2 Pa) and N2 gas (0.1 Pa) were introduced into the furnace of the sputtering device to set the pressure inside the furnace to 0.3 Pa. A DC bias voltage was applied to the substrate, and the overlap time of the power applied to the targets was set to 50 microseconds, and the discharge time per cycle of the power applied to each target was set to 1 millisecond. The negative pressure bias voltage applied to the substrate was set to -120 V, and the maximum power was set to 0.4 kW / cm. 2 As a result, electric power was continuously applied to six Al75Cr25 alloy targets to coat the surface of the substrate with a hard coating of approximately 3.0 μm. In the coating of Comparative Example 2, the temperature inside the furnace was set to 400°C, and Ar gas (0.2 Pa) and N2 gas (0.1 Pa) were introduced into the furnace of the sputtering device to set the pressure inside the furnace to 0.3 Pa. A DC bias voltage was applied to the substrate, and the overlap time of the power applied to the targets was set to 50 microseconds, and the discharge time per cycle of the power applied to each target was set to 1 millisecond. The negative pressure bias voltage applied to the substrate was set to -120 V, and the maximum power was set to 0.8 kW / cm. 2 As a result, electric power was continuously applied to six Al80Cr20 alloy targets to coat the surface of the substrate with a hard coating of approximately 3.0 μm. In the coating of Comparative Example 3, the temperature inside the furnace was set to 400°C, and Ar gas (0.2 Pa) and N2 gas (0.1 Pa) were introduced into the furnace of the sputtering device to set the pressure inside the furnace to 0.3 Pa. A DC bias voltage was applied to the substrate, and the overlap time of the power applied to the targets was set to 50 microseconds, and the discharge time per cycle of the power applied to each target was set to 1 millisecond. The negative pressure bias voltage applied to the substrate was set to -120 V, and the maximum power was set to 0.8 kW / cm. 2 As a result, electric power was continuously applied to six Al75Cr25 alloy targets to coat the surface of the substrate with a hard coating of approximately 3.0 μm.

[0030] In Comparative Example 1, an arc ion plating device was used. An Al60Cr40 alloy target was placed in the device as a deposition source. First, cleaning of the tool was performed using Ar ions (bombardment treatment). Next, the pressure inside the arc ion plating device was increased to 5.0×10 -3 The furnace was evacuated to a vacuum of 500 Pa or less, the temperature inside the furnace was set to 500°C, and N2 gas was introduced so that the pressure inside the furnace was 3.2 Pa. Next, a DC bias voltage of -100 V was applied to the tool, and a current of 150 A was supplied to the Al60Cr40 alloy target, so that a hard film of about 3.0 μm was coated on the surface of the tool. Comparative Example 1 is a composition that is commonly used on the market.

[0031] The composition of the hard coating was measured using a wavelength dispersive electron probe microanalysis (WDS-EPMA) attached to an electron probe microanalyzer (JXA-8500F, manufactured by JEOL Ltd.). A ball end mill for evaluating physical properties was mirror-finished, and the accelerating voltage was 10 kV and the probe current was 5 × 10 -8 A, the acquisition time was 10 seconds, and measurements were taken at five points in the analysis area of ​​a diameter of 1 μm. The metal content of the hard coating and the Ar content in the total of the metal and non-metallic components were calculated from the average values.

[0032] The crystal structure was confirmed using an X-ray diffraction apparatus (EMPYREA manufactured by PaNalytical Co., Ltd.) under measurement conditions of a tube voltage of 45 kV, a tube current of 40 mA, an X-ray source of Cukα (λ=0.15405 nm), and 2θ of 20 to 80 degrees.

[0033] The hardness and elastic modulus of the hard coating were analyzed using a nanoindentation tester (ENT-2100 manufactured by Elionix Co., Ltd.). For the analysis, the cross section of the coating was mirror-polished by tilting a test piece 5 degrees from the outermost surface of the coating, and an area was selected within the polished surface of the coating where the maximum indentation depth was approximately 1 / 10 of the thickness of the coating. Measurements were taken at 15 points under the measurement condition of an indentation load of 9.807 mN, and the hardness and elastic modulus were calculated from the average value of the 5 points excluding the 5 points with the larger value and the 5 points with the smaller value. The coating composition and the results of the physical property evaluation are shown in Table 1.

[0034] [Table 1]

[0035] As a result of X-ray diffraction, Example 1 and Comparative Example 1 had a face-centered cubic lattice structure (fcc structure), whereas Comparative Examples 2 and 3 had a hexagonal close-packed structure (hcp structure).

[0036] The X-ray intensity distribution was evaluated by pole figure for this Example 1 and Comparative Example 1, which had an fcc structure. The measurement conditions for the X-ray intensity distribution by pole figure were as follows. When the normal to the sample surface is on a plane determined by the incident ray and the diffracted ray, the α angle is set to 90°. When the α angle is 90°, it is the center point on the pole figure. Bulb: CuKα ray Output: 45kV, 200mA Beam: Parallel method Optical system: In-plane Detector: D / teX Ultra250 Solar slit opening angle: 0.5deg Entrance slit width: 1.0 mm Receiving slit width: 1.0 mm Scanning method: concentric circles β Scan Range: 0°~360° / 3.0° step Fixed 2θ angle: The diffraction angle of the (111) plane is the angle at which the diffraction intensity is highest between 36.0° and 39.0°. The diffraction angle of the (200) plane is the angle at which the diffraction intensity is highest between 42.0° and 45.0°. The crystal plane was specified based on CrN. α Scan Range: 0~90° / 3.0° step

[0037] [Table 2]

[0038] Fig. 1 shows an example of the X-ray intensity distribution of the α axis of a pole figure for the (111) plane of this Example 1. Fig. 2 shows an example of the X-ray intensity distribution of the α axis of a pole figure for the (200) plane of this Example 1. Fig. 3 shows an example of the X-ray intensity distribution of the α axis of a pole figure for the (111) plane of Comparative Example 1. Fig. 4 shows an example of the X-ray intensity distribution of the α axis of a pole figure for the (200) plane of Comparative Example 1. From FIG. 1, it can be seen that the (111) plane of this Example 1 has a maximum peak intensity at an α angle of 90°, a low peak intensity in the range of α angles from 0° to 70°, and is strongly oriented in the narrow range of α angles from 80° to 90°. Table 2 shows the peak intensity values ​​read from the figure. The (111) plane of this Example 1 exhibits a maximum intensity Ia (=1276) at an α angle of 90°, and a maximum intensity in the range of α angles from 0° to 70° is 287. The intensity of the (111) plane of this Example 1 in the range of α angles from 0° to 70° is 22% of the maximum intensity Ia, and it was confirmed that the (111) plane is strongly oriented in the range of α angles from 80° to 90°. That is, the intensity of the (111) plane of this Example 1 in the range of α angles from 0° to 70° is 35% or less and 30% or less of the maximum intensity Ia.

[0039] FIG. 5 shows an example of the XRD measurement result of the AlCrN of this Example 1. It was confirmed that the peak intensity of (111) of the face-centered cubic lattice structure of the AlCrN of this Example 1 shows the maximum intensity. Furthermore, the peak intensity of AlN of the hcp structure of the AlCrN of this Example 1 was not confirmed by XRD. In FIG. 5, the three peaks showing the crystal planes (111), (200), and (220) are diffraction peaks caused by the AlCrN of the face-centered cubic structure. The other four peaks not showing the crystal planes are all diffraction peaks caused by the WC of the substrate.

[0040] As shown in Table 1, the coated tool of this Example 1 has a hard coating with a face-centered cubic lattice structure in which the (111) plane is strongly oriented with an α angle of 80° to 90°, and it was confirmed that, despite its Al-rich composition, the coating hardness and elastic modulus are higher than those of Comparative Example 1. Furthermore, with the coated tool of this Example 1, droplets are reduced by application of the sputtering method, so that coating damage caused by droplets can be suppressed compared to the coated tool of Comparative Example 1.

[0041] (Condition) Dry processing Tool: 2-blade carbide ball end mill Model number: EPDBE2010-6, ball radius 0.5mm Cutting method: bottom cutting Work material: STAVAX (52HRC) (manufactured by BOHER-Uddeholm Co., Ltd.) Cut: Axial, 0.03mm, Radial, 0.03mm Cutting speed: 67.8m / min Feed per blade: 0.0135mm / blade Cutting distance: 15m Evaluation method: After cutting, the material was observed at a magnification of 1000x using a scanning electron microscope, and the width of the abrasion between the tool and the workpiece on the tool flank was measured. The part with the largest abrasion width was recorded as the maximum wear width on the flank.

[0042] [Table 3]

[0043] It was confirmed that the maximum flank wear width of this Example 1 was small, and that it was more durable than AlCrN used in the conventional arc ion plating method.

Claims

1. A coated tool having a substrate and a hard coating on the substrate, the hard coating is a nitride or carbonitride containing 65 atomic % or more and 90 atomic % or less of Al and 10 atomic % or more and 35 atomic % or less of Cr, both relative to the total amount of metal elements (including metalloid elements), and 0.50 atomic % or less of argon (Ar), both relative to the total amount of metal elements (including metalloid elements) and nonmetallic elements, and has a face-centered cubic lattice structure; The hard coating exhibits a maximum intensity Ia in an α-axis range of 80° to 90° in an X-ray intensity distribution of a pole figure for a (111) plane of a face-centered cubic lattice structure, and an intensity in an α-angle range of 0° to 70° is 35% or less of the maximum intensity Ia.

2. 2. The coated tool according to claim 1, wherein the strength in the α angle range of 0° to 70° is 30% or less of the maximum strength Ia.

3. 3. The coated tool according to claim 1, wherein the hard coating has a face-centered cubic lattice structure in which a (111) plane shows maximum intensity in an intensity profile of an X-ray diffraction or a selected area diffraction pattern obtained by a transmission electron microscope.

Citation Information

Patent Citations

  • Surface-coated cutting tool with hard coating layer exercising superior chipping resistance

    JP2009061514A

  • Coating member

    JP2009203485A

  • Surface-coated cutting tool provided with hard coated layer demonstrating superior chipping resistance

    JP2010094761A

  • Surface-coated cutting tool provided with hard coated layer demonstrating superior chipping resistance and wear resistance

    JP2010094764A

  • Coated tool

    JP2016032861A