Hydrogen storage structural material composition, hydrogen storage structural material, and hydrogen storage single tube

A composite material with a micron-level honeycomb structure addresses safety and efficiency issues in hydrogen storage by using polyimide and metal compounds, achieving high-pressure stability and reduced volume with enhanced safety and cost-effectiveness.

JP7594823B2Active Publication Date: 2024-12-05SHANGHAI JIENENG TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023537449
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-28
Filing Date
2020-11-10
Publication Date
2024-12-05
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Current high-pressure hydrogen storage containers face issues with safety, stability, and efficiency due to reliance on carbon fiber materials, which are costly, have high risk of leakage, and occupy large volumes, while existing hollow internal structures fail to manage high pressure and temperature effectively.

Method used

Development of a hydrogen storage structure using a composite material composition comprising polyimide, polyvinyl acetate, metal chlorides, oxides, and carbides, forming a micron-level honeycomb structure with a high-pressure resistant, lightweight material that separates hydrogen into fine isolated storage spaces, enhancing safety and stability.

Benefits of technology

The new material achieves high-pressure hydrogen storage with safety factors twice that of carbon fiber containers, reduces volume by 50%, and ensures stability under dynamic conditions, with a continuous service life twice that of quartz capillaries, and production costs one-third of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594823000001
    Figure 0007594823000001
  • Figure 0007594823000002
    Figure 0007594823000002
  • Figure 0007594823000003
    Figure 0007594823000003
Patent Text Reader

Abstract

The present invention provides a hydrogen storage structural material, a single hydrogen storage tube, and a hydrogen storage structural material composition for producing the hydrogen storage structural material or the single hydrogen storage tube. [Solution] The single hydrogen storage tube of the present invention has a honeycomb high-pressure hydrogen storage structure with micron-level pore diameters, a low mass specific gravity, a pore diameter of 150 μm, a tube wall thickness of 35 μm, a hydrogen storage structure limit pressure of >200 MPa, a Rockwell hardness of 86-89, high-temperature resistance >1900°C, low-temperature resistance <-260°C, low thermal conductivity, high-temperature insulation, and resistance to strong acids and bases. The high-pressure hydrogen storage structure of the present invention is very stable even in high-density hydrogen operating atmospheres and complex dynamic environments.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of hydrogen storage technology, and in particular to a hydrogen storage structural material and a hydrogen storage single tube. [Background technology]

[0002] The year 2019 was the initial development stage for China to fully launch the hydrogen energy industrial chain. Hydrogen energy can be a clean alternative energy, and the important hydrogen storage technology directly affects social safety, as well as the macro-social benefits and efficiency of hydrogen storage, mobile transportation, and mobile applications. Therefore, under the premise of high safety and stability, 70MPa~110MPa high-pressure hydrogen storage technology is receiving more and more attention.

[0003] In terms of technology, most of China's 35MPa and 70MPa portable hydrogen storage containers use the internationally adopted hollow inner tube structure and also use Japan's Toray M40 or T1000 high-quality carbon fiber, which realizes the advantage of light weight, but also has comprehensive safety issues. In order to reliably achieve high-quality density ratio high pressure strength, high safety and stability, the present invention requires a technical breakthrough in the realization of a highly difficult micron-level pore size high-pressure hydrogen storage structure and high-pressure resistant lightweight material.

[0004] High safety and stability of hydrogen storage technology is the most important metric for the healthy development of hydrogen energy industry. The external pressure strength achieved by the thick carbon fiber coating layer of the container currently relies on determines that there will be unforeseen high risks during its application. Although safety performance inspections must be regularly conducted during the usage period, the dynamic high pressure energy and stress of hydrogen will cause the destruction and aging of the container pressure layer, and there is still a high potential risk.

[0005] The current 35MPa containers in Japan do not have sufficient hydrogen storage capacity for cruising, and many of them use multiple containers connected in parallel, which increases the risk of high risk many times in a small installation space. Even 70MPa containers have the same large and awkward cylindrical shape and occupy a very large volume space.

[0006] The hollow internal structure of 35MPa to 70MPa cannot avoid the critical high pressure generated under high temperature and dynamic environment, and the container must automatically release high pressure to reach a safe value, and the hydrogen loss will be very severe when the high pressure is released.

[0007] If China's current container hydrogen storage technology and future development continue to depend on imported carbon fiber, its high application costs will be detrimental to the rapid popularization and development of hydrogen energy, as well as to economic and social benefits, and the concerned supply chain tension issue will ultimately become a bottleneck. Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, there is a need in this field for a new type of high-pressure hydrogen storage technology that can solve the above-mentioned comprehensive problems existing in the hollow bile mobile high-pressure hydrogen storage technology, and has high pressure strength, high safety and stability. [Means for solving the problem]

[0009] Specifically, the present invention provides a hydrogen storage structure material composition, the raw materials of which include 20-24 parts by weight of polyimide, 12-13 parts by weight of polyvinyl acetate, 15-17 parts by weight of aluminum chloride, 3-5 parts by weight of magnesium chloride, 3-5 parts by weight of barium chloride, 10-12 parts by weight of alumina, 15-17 parts by weight of zirconia, 0.5-0.7 parts by weight of lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 32-35 parts by weight of silica, silicon carbide and / or beryllium oxide, 1.5-2.5 parts by weight of sodium hydroxide and / or potassium hydroxide, 1.5-3 parts by weight of yttrium oxide, 6-8 parts by weight of titania and / or titanium carbide, 0.3-0.5 parts by weight of hafnium oxide and / or hafnium carbide, 0.3-0.5 parts by weight of optional calcium chloride, and 10 parts by weight or less of optional zinc carbide.

[0010] In one or more embodiments, the hydrogen storage structural material composition feedstock further includes water and a polar solvent.

[0011] In one or more embodiments, the polar solvent is selected from the group consisting of dimethylacetamide, dimethylformamide, and N-methylpyrrolidone.

[0012] In one or more embodiments, the viscosity of the hydrogen storage structural material composition is 90,000±10,000 cP.

[0013] The present invention also provides a method for making a hydrogen storage structural material composition as described in any embodiment herein, the method comprising the steps of: (1) mixing aluminum chloride and magnesium chloride, dissolving them in water, adding sodium hydroxide and / or potassium hydroxide, reacting them to generate a white precipitate, taking out the white precipitate, adding barium chloride and optional calcium chloride, stirring uniformly, drying, subjecting them to high-temperature treatment at 700 to 900°C, and pulverizing them to obtain composition A; (2) mixing alumina, zirconia, yttrium oxide, titania and / or titanium carbide, hafnium oxide and / or hafnium carbide, and optionally zinc carbide to obtain composition B; (3) adding silica, silicon carbide and / or beryllium oxide to the polyimide solution, stirring uniformly, adding composition B, stirring uniformly, adding lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, stirring uniformly, and then obtaining composition C; and (4) adding composition A to the polyvinyl acetate solution, stirring uniformly, and then mixing the resulting mixture with composition C and stirring uniformly; Through these steps, the hydrogen storage structural material composition is obtained.

[0014] In one or more embodiments, the method has one or more of the following features. (1) In the step (1), the concentration of the mixed solution of aluminum chloride and magnesium chloride dissolved in water is 40 to 60 wt %, (2) In step (1), the high-temperature treatment time is 80 to 100 minutes; (3) In step (1), the mesh number of the pulverized composition A is 8000 mesh or more; (4) In the step (3), the polyimide solution is a solution in which a polyimide is dissolved in a polar solvent, the polar solvent is selected from dimethylacetamide, dimethylformamide, and N-methylpyrrolidone, and the viscosity of the polyimide solution is 90000 cP±2000 cP; (5) step (3) is carried out at 35 to 45°C and under a vacuum of -94 kPa to -101 kPa; (6) In step (4), the polyvinyl acetate solution is an aqueous solution of polyvinyl acetate and has a concentration of 70 to 80 wt %; (7) In step (4), the mixture of the polyvinyl acetate solution and composition A is mixed with composition C at 35 to 45° C. and at a vacuum of −94 kPa to −101 kPa; (8) In step (4), the mixture of the polyvinyl acetate solution and composition A is mixed with composition C, and then a polar solvent selected from dimethylacetamide, dimethylformamide, and N-methylpyrrolidone is added to adjust the viscosity of the mixture to 90,000±10,000 cP.

[0015] The present invention also provides a hydrogen storage structural material, which contains, based on the total mass of the hydrogen storage structural material, 33-39 wt% silica and / or beryllium oxide, 17-22 wt% alumina, 20-28 wt% zirconia, 6-10 wt% titania, 0.25-0.5 wt% hafnium oxide, 0.45-0.9 wt% lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 1-2.7 wt% yttrium oxide, 0.12-1 wt% potassium oxide and / or sodium oxide, 0.18-0.4 wt% magnesium oxide, 1-1.7 wt% barium oxide, 0-10 wt% zinc oxide, 0.07-0.7 wt% calcium oxide which is optionally present, and unavoidable impurities.

[0016] The present invention also provides a composite material for hydrogen storage structure, comprising a hydrogen storage structural material according to any of the embodiments herein and a reinforcing filler.

[0017] The present invention also provides a method for producing the hydrogen storage structural material or the composite material for hydrogen storage structure described herein, which comprises subjecting the hydrogen storage structural material composition described in any one of the embodiments herein, or a mixture of the hydrogen storage structural material composition and a reinforcing filler, to a curing treatment at 40-45°C for 200-250 min, followed by a heat treatment at 50-60°C for 50-70 min, followed by a heat treatment at 360-480°C for 50-70 min, followed by a sintering treatment at 850-900°C for 80-100 min, followed by a sintering treatment at 1400-1450°C for 250-350 min or a sintering treatment at 3000°C±100°C.

[0018] The present invention also provides a single hydrogen storage pipe, comprising a hydrogen storage unit made of a material for a hydrogen storage structure as described in any one of the embodiments herein, the hydrogen storage unit having a honeycomb micropore structure, the wall thickness of the micropores being preferably 35 to 40 μm, and the diameter of the micropores being preferably 140 to 150 μm.

[0019] In one or more embodiments, the single hydrogen storage tube further includes a shell, the material of which is a hydrogen storage structural material or a hydrogen storage structural composite material described in any of the embodiments herein.

[0020] The present invention also provides a method for producing the hydrogen storage single tube, comprising the steps of: (1) impregnating a polymer fiber bundle with a hydrogen storage structure material composition as described in any embodiment herein; (2) A process in which the polymer fiber bundle impregnated with the hydrogen storage structure material composition is subjected to a curing treatment at 40 to 45°C for 200 to 250 minutes, then a heat treatment at 50 to 60°C for 50 to 70 minutes, then a heat treatment at 360 to 480°C for 50 to 70 minutes, then a sintering treatment at 850 to 900°C for 80 to 100 minutes, then a sintering treatment at 1400 to 1450°C for 250 to 350 minutes or a sintering treatment at 3000°C ± 100°C; or The process includes the steps of filling a tubular mold with polymer fiber bundles impregnated with a storage structure material composition, curing the bundles at 40-45°C for 200-250 minutes, heat treating the bundles at 50-60°C for 50-70 minutes, heat treating the bundles at 360-480°C for 50-70 minutes, sintering the bundles at 850-900°C for 80-100 minutes, and sintering the bundles at 1400-1450°C for 250-350 minutes or sintering the bundles at 3000°C±100°C.

[0021] In one or more embodiments, the viscosity of the hydrogen storage structural material composition is adjusted to 200,000±10,000 cP prior to impregnation in step (1).

[0022] In one or more embodiments, the melting point of the polymer fibers is from 150°C to 380°C.

[0023] In one or more embodiments, the diameter of a single fiber in the polymer fiber bundle is 100 to 150 μm.

[0024] In one or more embodiments, in step (1), the impregnation causes the hydrogen storage structure material composition to coat the surface of each single fiber in the polymer fiber bundle to have an average thickness of 25 to 30 μm.

[0025] The present invention also provides applications of the hydrogen storage structure material composition, hydrogen storage structure material, hydrogen storage structure composite material, hydrogen storage structure, and hydrogen storage tube described herein in high-pressure hydrogen storage and / or liquid hydrogen storage. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 shows a schematic diagram of the micron honeycomb hydrogen storage structure inside a single tube of the present invention. [Diagram 2] FIG. 2 shows a photograph of a single circular tube of the present invention. [Diagram 3] FIG. 3 shows a mechanical schematic diagram of the honeycomb structure module made of the hexagonal hydrogen storage single tubes of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In order to facilitate understanding of the features and advantages of the present invention to those skilled in the art, the following provides general explanations and definitions for the terms and terms used in the specification and claims. Unless otherwise specified, all technical and scientific terms used herein shall have the ordinary meaning that those skilled in the art would understand to the present invention, and in the event of conflict, the definitions in this specification shall govern. The theories or mechanisms explained or disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any manner, i.e., the subject matter of the present invention can be practiced without being limited to any particular theory or mechanism.

[0028] In this document, all characteristics, e.g., amounts, contents, concentrations, defined in numerical or percentage ranges, are merely for brevity and convenience, and thus the description of a numerical or percentage range should be considered to cover and specifically disclose all possible subranges and individual numerical values ​​(including integers and fractions) within the range. In this text, unless otherwise specified, ratios refer to mass ratios and percentages refer to mass percentages.

[0029] In order to simplify the description, the present specification does not describe all possible combinations of each technical feature in each embodiment or example. Therefore, as long as there is no contradiction in the combination of these technical features, each technical feature in each embodiment or example can be arbitrarily combined, and all possible combinations are considered to be within the scope described in this specification.

[0030] The most important link in the popularization and development of hydrogen energy is high-pressure hydrogen storage with high safety. Internationally, most of the current high-pressure hydrogen storage containers adopt high-quality carbon fiber / epoxy resin composite material (CFRP) with hollow inner tube and multi-layer coating on the outer surface, which realizes high pressure and strength by applying high pressure to the surface layer and has the advantage of quality-density ratio, and now our country also adopts this technology. However, in a complex dynamic environment, the dynamic high pressure of hydrogen, temperature rise, and the risk of collapse and leakage due to internal stress cannot be solved by thickening the carbon fiber coating layer, and many accidents of leakage explosion and injury have already occurred in our country in 70MPa natural gas transfer tool. In addition, the use of a large amount of imported carbon fiber not only has high cost and limited resources, but also has many problems such as sustainable development and economic feasibility. In response to the various problems of safety and stability of the current hollow inner tube high-pressure hydrogen storage container, the present invention proposes a new type of composite material for high-pressure hydrogen storage structure and high-pressure hydrogen storage structure. The basic design concept of the present invention includes: 1. Instead of relying on imported carbon fiber, high-performance materials with light mass density are used; 2. Instead of hollow galli, research and development of micron-level micro-pore honeycomb structure is used. In the present invention, the large-capacity hydrogen is separated into fine isolated storage spaces like hair threads, which can very effectively limit the activation energy of high-pressure hydrogen; the concentrated micro-pore honeycomb structure can thoroughly eliminate the high-risk problems existing in high-pressure hydrogen storage in hollow galli, the safety pressure can reach 70MPa-110MPa, and the safety factor is several times, eliminating the thick and huge coating layer outside the hollow galli, improving hydrogen storage efficiency, greatly reducing the volume, and effectively increasing the economic benefits of hydrogen storage.

[0031] The present invention provides a composite material composition (also referred to as a material composition for hydrogen storage structures) used for manufacturing a hydrogen storage structure, the composite material composition being a solid-liquid mixture having a certain viscosity at room temperature. The material for hydrogen storage structures of the present invention is obtained by curing and sintering the material composition for hydrogen storage structures of the present invention. The hydrogen storage structure of the present invention is obtained by impregnating polymer fibers with the composite material composition of the present invention, followed by curing and sintering. The hydrogen storage structure of the present invention is also referred to as a high-pressure hydrogen storage structure, since it is applied to high-pressure hydrogen storage.

[0032] The raw material of the composite material composition of the present invention includes polyimide (PI). The composite material of the present invention has an inorganic metal phase structure. Therefore, in this document, the composite material of the present invention is abbreviated as PMTS material (abbreviation for organic polymer PI + inorganic metal phase structure), the composite material composition of the present invention is also abbreviated as PMTS material composition, and the high-pressure hydrogen storage structure of the present invention is also abbreviated as PMTS material high-pressure hydrogen storage structure. The composite material of the present invention is suitable as a material for hydrogen storage structures, and is therefore also called material for hydrogen storage structures.

[0033] The raw materials for the PMTS material composition of the present invention include 10-40 parts by weight of polyimide, 8-18 parts by weight of polyvinyl acetate, 15-40 parts by weight of metal chloride, 10-70 parts by weight of metal oxide and / or metal carbide, 10-40 parts by weight of silica and / or silicon carbide, 0.5-5 parts by weight of rare earth metal oxide, and 1-5 parts by weight of alkali metal hydroxide. In some embodiments, the raw materials for the PMTS material composition further include an appropriate amount of water and a polar solvent. In some embodiments, the raw materials for the PMTS material composition include a metal chloride that includes one or more selected from the group consisting of aluminum chloride, magnesium chloride, barium chloride, and calcium chloride, and preferably includes aluminum chloride, magnesium chloride, and barium chloride, and optionally further includes calcium chloride. When contained in the raw materials of the PMTS material composition, the amount of aluminum chloride used is preferably 10 to 20 parts by weight, the amount of magnesium chloride used is preferably 1 to 10 parts by weight, the amount of barium chloride used is preferably 1 to 10 parts by weight, and the amount of calcium chloride used is preferably 0.1 to 1 part by weight. In the present specification, the metal oxide does not include a rare earth metal oxide. In some embodiments, the raw materials of the PMTS material composition include one or more metal oxides selected from alumina, zirconia, titania, hafnium oxide, and beryllium oxide. When contained in the raw materials of the PMTS material composition, the amount of alumina used is preferably 5 to 15 parts by weight, the amount of zirconia used is preferably 10 to 20 parts by weight, the amount of titania used is preferably 5 to 10 parts by weight, the amount of hafnium oxide used is preferably 0.1 to 1 part by weight, and the amount of beryllium oxide used is preferably 30 to 40 parts by weight. In some embodiments, the raw material for the PMTS material composition includes at least one metal carbide selected from silicon carbide, titanium carbide, hafnium carbide, and zinc carbide. When contained in the raw materials for the PMTS material composition, the amount of silicon carbide used is preferably 10 to 40 parts by weight, the amount of titanium carbide used is preferably 5 to 10 parts by weight, and the amount of hafnium carbide used is preferably 0.1 to 1 part by weight.In some embodiments, the raw material for the PMTS material composition includes rare earth metal oxides selected from lanthanum oxide, cerium oxide, lanthanum cerium oxide, and yttrium oxide, and preferably includes yttrium oxide and at least one selected from lanthanum oxide, cerium oxide, and lanthanum cerium oxide. When included in the raw material for the PMTS material composition, the total amount of lanthanum oxide, cerium oxide, and lanthanum cerium oxide used is preferably 0.2 to 1 part by weight, and the amount of yttrium oxide used is preferably 1 to 5 parts by weight. In some embodiments, the raw material for the PMTS material composition includes alkali metal hydroxides selected from one or both of sodium hydroxide and potassium hydroxide.

[0034] In a preferred embodiment, the raw materials of the PMTS material composition are 20-24 parts by weight of polyimide (PI), 12-13 parts by weight of polyvinyl acetate (PVAc), 15-17 parts by weight of aluminum chloride (AlCl3), 3-5 parts by weight of magnesium chloride (MgCl2), 3-5 parts by weight of barium chloride (BaCl2), 10-12 parts by weight of alumina (Al2O3), 15-17 parts by weight of zirconia (ZrO2), 0.5-0.7 parts by weight of lanthanum oxide (La2O3), cerium oxide and / or lanthanum cerium oxide. , 32-35 parts by weight of silica (SiO2), silicon carbide and / or beryllium oxide, 1.5-2.5 parts by weight of sodium hydroxide (NaOH) and / or potassium hydroxide (KOH), 1.5-3 parts by weight of yttrium oxide (Y2O3), 6-8 parts by weight of titania (TiO2) and / or titanium carbide, 0.3-0.5 parts by weight of hafnium oxide (HfO2) and / or hafnium carbide, 0.3-0.5 parts by weight of optional calcium chloride (CaCl2), and optionally up to 10 parts by weight of zinc carbide. In some embodiments, the 32-35 parts by weight of silica, silicon carbide and / or beryllium oxide is 32-35 parts by weight of silica and / or silicon carbide, or 32-35 parts by weight of silica and / or silicon carbide and beryllium oxide, and the amount of beryllium oxide used is preferably 5-15 parts by weight. In some embodiments, the ingredients of the PMTS material composition include 20-24 parts by weight PI, 12-13 parts by weight polyvinyl acetate, 15-17 parts by weight aluminum chloride, 3-5 parts by weight magnesium chloride, 3-5 parts by weight barium chloride, 10-12 parts by weight alumina, 15-17 parts by weight zirconia, 0.5-0.7 parts by weight lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 32-35 parts by weight silica and / or beryllium oxide, 1.5-2.5 parts by weight sodium hydroxide and / or potassium hydroxide, 1.5-3 parts by weight yttrium oxide, 6-8 parts by weight titania (TiO2), 0.3-0.5 parts by weight hafnium oxide (HfO2), and optionally 0.3-0.5 parts by weight calcium chloride (CaCl2). In some embodiments, the silica and / or beryllium oxide is 32 to 35 parts by weight of silica, or 32 to 35 parts by weight of silica and beryllium oxide, with the amount of beryllium oxide being preferably 5 to 15 parts by weight.In the present invention, the optional 5-15 parts by weight of beryllium oxide replaces a portion of the silica or silicon carbide to provide better mass density and hardness.

[0035] The raw material of the PMTS material composition further contains an appropriate amount of water and a polar solvent. The raw material of the PMTS material composition preferably contains 3 to 5.5 parts by weight of water, more preferably 3.5 to 5 parts by weight of water, per 12 to 13 parts by weight of PVAc. In some embodiments, the raw material of the PMTS material composition contains or consists of the above weight parts of PI, PVAc, aluminum chloride, magnesium chloride, barium chloride, alumina, zirconia, lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, silica, silicon carbide and / or beryllium, sodium hydroxide and / or potassium hydroxide, yttrium oxide, titania and / or titanium carbide, hafnium oxide and / or hafnium carbide, water, optional calcium chloride, optional zinc carbide, and an appropriate amount of polar solvent. In the present invention, the amount of polar solvent used as the raw material of the PMTS material composition is preferably an amount that allows the viscosity of the PMTS material composition to be 90000±10000 cP.

[0036] In the present invention, the water is preferably distilled water or deionized water. In the present invention, the polar solvent is preferably one or more selected from dimethylacetamide (DMAc), dimethylformamide (DMF) and N-methylpyrrolidone (NMP).

[0037] In this specification, parts by weight represent the blending ratio of parts by weight between each raw material / ingredient, and it can be understood that the sum of the parts by weight of each raw material is not required to be 100 parts by weight.

[0038] In the present invention, the metal oxide and metal carbide raw materials other than zirconia, hafnium oxide, hafnium carbide, lanthanum oxide, cerium oxide, and lanthanum cerium oxide are preferably ultrafine powders of nano-level, preferably with a fineness of 10,000 or more, and preferably with an average particle size of 300 nm to 2 μm. In order to ensure the high quality of the PMTS material and to avoid oxidation and decay of harmful impurities during the high-temperature sintering process, it is preferable to use high-purity raw materials in the present invention, for example raw materials with a purity of 4N, 5N, or 6N. The raw materials used in the present invention may be commercially available products, or may be obtained by ultrafine processing by a method such as high-pressure airflow pulverization suspension fine powder collection method.

[0039] The PMTS material composition is obtained by a process comprising the steps of: (1) mixing aluminum chloride and magnesium chloride, dissolving them in an appropriate amount of water, adding sodium hydroxide and / or potassium hydroxide, reacting them to generate a white precipitate, taking out the white precipitate, adding barium chloride and optional calcium chloride, stirring uniformly, drying, subjecting them to high-temperature treatment at 700 to 900°C, and pulverizing them to obtain composition A; (2) mixing alumina, zirconia, yttrium oxide, titania and / or titanium carbide, hafnium oxide and / or hafnium carbide, and optionally zinc carbide to obtain composition B; (3) adding silica, silicon carbide and / or beryllium oxide to the polyimide solution, stirring uniformly, adding composition B, stirring uniformly, adding lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, stirring uniformly, and then obtaining composition C; and (4) adding composition A to the polyvinyl acetate solution and stirring uniformly, and then mixing the resulting mixture with composition C and stirring uniformly; These steps result in a PMTS material composition.

[0040] The numbers of the above steps are used only to distinguish each step and do not limit the order of operation of each step. It is understood that it is sufficient to prepare the necessary raw materials and / or ingredients before performing a certain step, for example, to first perform steps (2) and (3), then perform step (1), and finally perform step (4).

[0041] In the present invention, the aluminum chloride is preferably analytically pure anhydrous aluminum chloride, the magnesium chloride is preferably analytically pure magnesium chloride, and the sodium hydroxide and potassium hydroxide are preferably analytically pure. In step (1), the amount of aluminum chloride used is 15 to 17 parts by weight, and the amount of magnesium chloride used is 3 to 5 parts by weight. In step (1), the amount of water used is preferably such that the concentration of the solution in which aluminum chloride and magnesium chloride are dissolved is 40 wt% to 60 wt%, for example, 40 wt% to 50 wt%. In step (1), the total amount of sodium hydroxide and / or potassium hydroxide used is 1.5 to 2.5 parts by weight, and the amount of each of sodium hydroxide and potassium hydroxide used is not particularly limited in general, and for example, only sodium hydroxide or only potassium hydroxide may be used. When sodium hydroxide and / or potassium hydroxide are added in step (1), it is preferable to add them stepwise. In a preferred embodiment, in step (1), 1.2 to 2 parts by weight of sodium hydroxide and 0.3 to 0.5 parts by weight of potassium hydroxide are added. After the sodium hydroxide and / or potassium hydroxide are added, the reaction generates heat. It is preferable that a white precipitate is generated before the reaction is cooled, and the white precipitate is removed and barium chloride and optional calcium chloride are added. In step (1), the amount of barium chloride used is 3 to 5 parts by weight. Calcium chloride may or may not be added, and when added, the amount of calcium chloride used is 0.3 to 0.5 parts by weight. In some embodiments, in step (1), barium chloride and optional calcium chloride are added, stirred, and then allowed to stand and dried, and the standing time is preferably 30 minutes or more. In step (1), the drying temperature is preferably 90 to 110°C. In step (1), the temperature of high-temperature treatment is preferably 700 to 900°C, and the time is preferably 80 to 100 minutes. In some embodiments, in step (1), after the high-temperature treatment, the mixture is cooled and pulverized to 8,000 mesh or more in a ball mill to obtain composition A.

[0042] In the present invention, the alumina is nano alumina, the zirconia is ultrafine zirconia, preferably micron-class zirconia (for example, particle size 1-5 μm); the yttrium oxide is nano yttrium oxide, the titania is nano titania, preferably rutile titania, the hafnium oxide is ultrafine hafnium oxide (for example, particle size 800 nm-2 μm); the hafnium carbide is ultrafine hafnium carbide (for example, particle size 800 nm-2 μm); the titanium carbide is nano titanium carbide; the zinc carbide is nano zinc carbide. In step (2), the amount of alumina used is 10-12 parts by weight, the amount of zirconia used is 15-17 parts by weight, the amount of yttrium oxide used is 1.5-3 parts by weight, the total amount of titania and titanium carbide used is 6-8 parts by weight, and the total amount of hafnium oxide and hafnium carbide used is 0.3-0.5 parts by weight; if added, the amount of zinc carbide used is less than 10 parts by weight.

[0043] The PI suitable for the present invention is preferably an electrical engineering level or higher level PI, and may be a thermosetting PI, such as SP-1 by DuPont, USA, or a thermoplastic PI, such as JNF3020 by Mitsui Chemicals, Japan. The characteristic viscosity of the PI suitable for the present invention is preferably 0.52 to 0.81 dL / g. In the present invention, the PI solution is a solution in which the PI is diluted with a polar solvent. In step (3), the amount of PI used is 20 to 24 parts by weight, that is, the weight parts of PI contained in the PI solution used are 20 to 24 parts by weight. The viscosity of the PI solution used in step (3) is 90000 cP±2000 cP. In the present invention, the viscosity is a viscosity measured at room temperature and normal pressure (25° C., 1 atm). The method for producing the PI solution used in step (3) is not particularly limited, and for example, a solid PI raw material can be used, and the solid PI can be dissolved in an appropriate amount of polar solvent to obtain a PI solution with a viscosity of 90000 cP ± 2000 cP; a PI solution with a high viscosity (e.g., a PI solution with a concentration of 28 to 32 wt%) that has been dissolved in a polar solvent in advance can be used as a raw material, and diluted with a polar solvent to obtain a PI solution with a viscosity of 90000 cP ± 2000 cP. In some embodiments, a polar solvent is added to solid PI or a PI solution with a concentration of 28 to 32 wt% under a vacuum of 35 to 45°C and -94 kPa to -101 kPa, and the mixture is stirred to obtain a PI solution with a viscosity of 90000 cP ± 2000 cP; the stirring speed is preferably 8 to 12 r / min, and the stirring time is preferably 15 to 25 min. In step (3), it is preferable to mix the PI solution with silica, silicon carbide and / or beryllium oxide at 35 to 45°C and under a vacuum of -94 kPa to -101 kPa, further mix with composition B, and further mix with lanthanum oxide, cerium oxide and / or lanthanum cerium oxide. In step (3), it is preferable to have a stirring speed of 8 to 12 r / min. When mixing the PI solution with silica, silicon carbide and / or beryllium oxide in step (3), it is preferable to stir for 10 to 15 minutes, and after adding composition B, it is preferable to stir for 15 to 20 minutes. It is preferable to stir for 15 to 20 minutes after adding lanthanum oxide, cerium oxide and / or lanthanum cerium oxide. In the present invention, it is preferable that the silica is nanosilica and has a particle size of 100 nm to 500 nm.The silicon carbide is preferably nano silicon carbide, and has a particle size of 100 nm to 500 nm. The beryllium oxide is preferably 99.95% or more pure, and since this substance is highly toxic, production safety management must be strengthened. In step (3), the total amount of silica, silicon carbide, and beryllium oxide used is 32 to 35 parts by weight, and when used, the amount of beryllium oxide used is preferably 5 to 15 parts by weight. When silica is added in step (3), it is preferably added stepwise. In step (3), the amount of composition B used is the total amount of composition B obtained in step (2). In the present invention, lanthanum oxide, cerium oxide, and lanthanum cerium oxide are ultrafine lanthanum oxide, ultrafine cerium oxide, and ultrafine lanthanum cerium oxide (preferably with a particle size of 1 μm to 5 μm). In the step (3), one or more selected from lanthanum oxide, cerium oxide, and lanthanum cerium oxide may be used, and the total amount of lanthanum oxide, cerium oxide, and lanthanum cerium oxide used is 0.5 to 0.7 parts by weight.

[0044] PI has ideal precision plasticity such as high insulation, antistatic, and high resistance to high pressure, but its shortcoming is the high temperature limit determined by the polymer polymerization characteristics. The present invention obtains the plasticity of PI micron-level precision processing and the high strength of inorganic materials that can withstand high and low temperatures, and does not shrink or deform under high-temperature sintering. In order to achieve this, the composition is continuously adjusted through the ion chelate and metal phase structure in the compounding, and the mass specific gravity is lightened during the correlation with temperature during the hardening process, achieving high strength and high temperature resistance.

[0045] The PVAc suitable for the present invention is PVAc of industrial level or higher. The purity of PVAc is preferably 99.9% or more. The characteristic viscosity of PVAc suitable for the present invention is preferably 0.7 to 0.9 dL / g. In the present invention, the PVAc solution is an aqueous solution of PVAc. In step (4), the amount of PVAc used is 12 to 13 parts by weight, that is, the weight parts of PVAc contained in the PVAc solution used is 12 to 13 parts by weight. In step (4), the solid content of the PVAc solution used is 70 to 80 wt%, for example, about 73 to 77 wt%. In step (4), the amount of composition A used is the total amount of composition A obtained in step (1). In step (4), after adding composition A, stirring is preferably performed for 15 to 25 minutes. In step (4), the amount of composition C used is the total amount of composition C obtained in step (3). In step (4), the mixture of composition A and the PVAc solution is preferably mixed with composition C at 35 to 45°C and under a vacuum of -94 kPa to -101 kPa. In some embodiments, the mixture of composition A and the PVAc solution is added to composition C obtained in step (3) at 35 to 45°C and under a vacuum of -94 kPa to -101 kPa. The stirring speed when the mixture of composition A and the PVAc solution is mixed with composition C is preferably 8 to 12 r / min. In some embodiments, when the mixture of composition A and the PVAc solution is mixed with composition C, a polar solvent is added to adjust the viscosity of the PMTS material composition to 90000±10000 cP. In a preferred embodiment, when the mixture of composition A and the PVAc solution is mixed with composition C, a polar solvent is added, the mixture is heated to 45 to 52°C, and stirred at a rotation speed of 8 to 12 r / min to adjust the viscosity of the PMTS material composition to 90000±10000 cP. The PMTS material composition of the present invention is a white, bubble-free solid-liquid mixture with a certain viscosity, preferably 90,000±10,000 cP. The PMTS material composition of the present invention can be stably stored at a viscosity of 90,000±10,000 cP.

[0046] The present invention is based on the improved properties of organic-inorganic composites, and by adjusting the organic and inorganic phase components, obtains a PMTS material composition through a chelating affinity reaction between organic and inorganic ions. The PMTS material composition has the horizontal ductility of PI, and can obtain a film with a thickness of several tens of microns. Through desolvation treatment at 50℃~60℃, it can achieve three different property applications: 1. Application of PI bendable properties from liquid to plastic solid phase; 2. Application of PI plastic properties with precision micron-level structure that can be processed after dumping; 3. Lightweight high hardness precision application from dumping to high temperature sintering.

[0047] By curing the PMTS material composition at room temperature and pressure, the following products / materials can be produced as needed: 1. performance films having a thickness of tens to hundreds of microns, 2. various precision parts obtained by injection molding or high-temperature sintering, 3. various mold materials for precision machining after high-temperature sintering, and 4. the high-pressure hydrogen storage structure of the present invention obtained by precision machining and high-temperature sintering molding.

[0048] A solid semi-finished product can be obtained from the PMTS material composition by curing at 40-45°C, heat treatment at 50-60°C, and high-temperature treatment at 360-480°C. Therefore, the present invention also includes solid semi-finished products obtained by subjecting the PMTS material composition to three-stage treatment at 40-45°C, 50-60°C, and 360-480°C. In the present invention, the time for curing at 40-45°C is preferably 200-250 min, and the environmental humidity during curing at 40-45°C is preferably 8-12%. In the present invention, the time for heat treatment at 50-60°C is preferably 50-70 min, and the time for heat treatment at 360-480°C is preferably 50-70 min. In some embodiments, the PMTS material composition is cured at 40-45°C for 200-250 min, then processed at 50-60°C for 50-70 min, and then dumped (dumping means that the polymeric material decomposes into gas phase under high temperature) at 360-480°C for 50-70 min to obtain a solid semi-finished product.

[0049] The PMTS material composition can be cured at 40-45°C, heat-treated at 50-60°C, treated at high temperature at 360-480°C, and sintered at high temperature at 850-900°C to obtain a semi-finished product having a metal phase structure. Therefore, the present invention also includes a semi-finished product having a metal phase structure obtained by treating the PMTS material composition in four stages at 40-45°C, 50-60°C, 360-480°C, and 850-900°C. In the present invention, the time for the heat treatment at 850-900°C is preferably 80-100 minutes. In some embodiments, the PMTS material composition is cured at 40-45°C for 200-250 minutes, then treated at 50-60°C for 50-70 minutes, then treated at 360-480°C for 50-70 minutes, and then sintered at 850-900°C for 80-100 minutes to obtain a semi-finished product having a metal phase structure.

[0050] The PMTS material can be obtained from the PMTS material composition by curing at 40-45°C, heat treatment at 50-60°C, high temperature treatment at 360-480°C, high temperature sintering at 850-900°C, and high temperature sintering at 1400-1450°C. Thus, the PMTS material of the present invention can be obtained by subjecting the PMTS material composition to five treatment steps at 40-45°C, 50-60°C, 360-480°C, 850-900°C, and 1400-1450°C. In the present invention, the time for the heat treatment at 1400-1450°C is preferably 250-350 minutes. In some embodiments, the PMTS material composition is cured at 40-45°C for 200-250 min, then treated at 50-60°C for 50-70 min, then treated at 360-480°C for 50-70 min, then sintered at 850-900°C for 80-100 min, and then sintered at 1400-1450°C for 250-350 min to obtain the PMTS material. The PMTS material composition used in producing the PMTS material using the 1400-1450°C sintering method as the fifth step may be a PMTS material composition containing the raw materials described herein, such as polyimide, polyvinyl acetate, aluminum chloride, magnesium chloride, barium chloride, alumina, zirconia, lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, silica, sodium hydroxide and / or potassium hydroxide, yttrium oxide, titania, hafnium oxide, and optionally calcium chloride, or may be a PMTS material composition obtained by replacing some or all of the silica in the raw materials with silicon carbide, replacing some or all of the titania with titanium carbide, replacing some or all of the hafnium oxide with hafnium carbide, and / or further including zinc carbide. When some or all of the silica in the raw material is replaced with silicon carbide, some or all of the titania in the raw material is replaced with titanium carbide, some or all of the hafnium oxide in the raw material is replaced with hafnium carbide, and / or the raw material further contains zinc carbide, it is preferred that the total amount of carbides used does not exceed 45% of the total amount of carbides and oxides used in the raw material, and more preferably does not exceed 30%.

[0051] In this document, the terms hardening, hardening treatment, heating, heat treatment, high temperature treatment, high temperature sintering, sintering, sintering treatment, and similar terms are all used to express the meaning of heat treating a material at a certain temperature, and usually, the material is left in an environment of a certain temperature for a while. In the present invention, "50-60°C for 50-70 min, then 360-480°C for 50-70 min" means that the material is left in an environment of 50-60°C for 50-70 min, and then moved to an environment of 360-480°C for 50-70 min, and is inferred as follows. In the present invention, the device for the heating / high temperature / sintering treatment is not particularly limited. In some embodiments, the heating / high temperature / sintering treatment of the present invention is performed in a tunnel kiln, and in the tunnel kiln, the kiln body temperature of each stage is set in advance, and sintering is performed for each stage. For example, when producing PMTS material, a tunnel kiln may include four stages set at 50-60°C, 360-480°C, 850-900°C, and 1400-1450°C, respectively.

[0052] The PMTS material composition can also be obtained by 40-45°C curing, 50-60°C heat treatment, 360-480°C high-temperature treatment, 850-900°C high-temperature sintering, and 3000°C±100°C sintering. Thus, the PMTS material of the present invention can be obtained by subjecting the PMTS material composition to five-stage treatment at 40-45°C, 50-60°C, 360-480°C, 850-900°C, and 3000°C±100°C. In the present invention, the method of 3000°C±100°C sintering is not particularly limited as long as the temperature reaches 3000°C±100°C. For example, 3000°C±100°C sintering may be performed by a spark plasma sintering (abbreviated as SPS) process. The SPS suitable for the present invention may be any of various known SPS techniques, such as direct current sintering (abbreviated as DCS). In the present invention, when sintering at 3000°C±100°C is performed by SPS, the sintering time is usually 1-10s, preferably 3-6s. When sintering at 3000°C±100°C is performed by other sintering methods, the sintering time may be determined based on the actual situation. In some embodiments, the PMTS material composition is cured at 40-45°C for 200-250min, then treated at 50-60°C for 50-70min, then treated at 360-480°C for 50-70min, then sintered at 850-900°C for 80-100min, and then sintered at 3000°C±100°C to obtain the PMTS material. The PMTS material composition used in producing the PMTS material by the 3000°C±100°C sintering method in the fifth step may be a PMTS material composition containing the raw materials described herein, such as polyimide, polyvinyl acetate, aluminum chloride, magnesium chloride, barium chloride, alumina, zirconia, lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, silica, sodium hydroxide and / or potassium hydroxide, yttrium oxide, titania, hafnium oxide and optionally calcium chloride, and is preferably a PMTS material composition in which some or all of the silica in the above raw materials has been replaced with silicon carbide, some or all of the titania has been replaced with titanium carbide, some or all of the hafnium oxide has been replaced with hafnium carbide, and / or more preferably, further contains zinc carbide.In the present invention, when oxides are replaced by corresponding carbides in the raw materials of the PMTS material composition (e.g., silica is replaced by silicon carbide, titania is replaced by titanium carbide, hafnium oxide is replaced by hafnium carbide), and zinc carbide is introduced into the raw materials of the PMTS material composition, these carbides can be made into microelectrodes during sintering, which is advantageous for the progress of sintering at 3000°C±100°C, especially for the progress of SPS sintering at 3000°C±100°C. When some or all of the raw materials are replaced by silicon carbide, some or all of the titania in the raw materials is replaced by titanium carbide, some or all of the hafnium oxide in the raw materials is replaced by hafnium carbide, and / or the raw materials further contain zinc carbide, it is preferable that the total amount of carbides used does not exceed 45% of the total amount of carbides and oxides used in the raw materials, and more preferably does not exceed 30%.

[0053] When the PMTS material composition is used to produce the solid semi-finished products, semi-finished products having a metal phase structure, and PMTS materials described herein, the viscosity of the PMTS material composition may be adjusted as necessary before the above-mentioned 40-45°C curing and subsequent processing. For example, it will be understood that the viscosity of the PMTS material composition may be adjusted to 20,000 cP±10,000 cP by heating, and then the above-mentioned 40-45°C curing and subsequent processing may be performed.

[0054] The PMTS material composition, the solid semi-finished product of the present invention, the semi-finished product with metal phase structure of the present invention and the PMTS material are applied to the manufacture of precision micron-level microporous materials and special structures with resist / precision press / 3D printing, high temperature resistance, strong acid and alkali resistance, high pressure resistance, flame retardant heat insulation, strong tensile strength, antistatic, high insulation, high hardness and / or plasticity. The PMTS material of the present invention is also characterized by not chemically reacting with hydrogen.

[0055] The material of the high-pressure hydrogen storage structure of the present invention is a PMTS material, and is obtained by impregnating a polymer fiber with a PMTS material composition, curing it, and sintering it, so it is also called a PMTS material hydrogen storage structure. Specifically, the high-pressure hydrogen storage structure may be obtained by impregnating a polymer fiber with a PMTS material composition, curing it at 40 to 45°C for 200 to 250 minutes, treating it at 50 to 60°C for 50 to 70 minutes, treating it at 360 to 480°C for 50 to 70 minutes, sintering it at 850 to 900°C for 80 to 100 minutes, and sintering it at 1400 to 1450°C for 250 to 350 minutes or sintering it at 3000°C ± 100°C.

[0056] The high pressure hydrogen storage structure of the present invention has a honeycomb structure (as shown in FIG. 1). When the polymer fiber is impregnated with the PMTS material composition, the polymer fiber is impregnated in the form of a fiber bundle. After impregnation, the surface of each single fiber in the fiber bundle is covered with a certain thickness of the PMTS material composition, and each adjacent single fiber is bonded to each other, so that each single fiber is arranged in a honeycomb shape in the cross section of the fiber bundle; after the fiber bundle impregnated with the PMTS material composition is sintered, the polymer fiber is decomposed into a gas phase, leaving a honeycomb structure of micropores (also called single-hole tubes), and the PMTS material composition on the surface of the fiber forms a PMTS material to form the pore walls of the honeycomb structure. In this specification, the honeycomb structure has the usual meaning, and when viewed from the cross section, six adjacent micropores are closely arranged around each micropore. In this specification, it can be understood that the micropore is a single-hole tube with a long diameter ratio, and the diameter of the micropore (i.e., the inner diameter of the single-hole tube) is usually 100 to 200 μm. The above-mentioned honeycomb structure and microporous structure of the hydrogen storage structure of the present invention are also referred to as honeycomb microporous structure. In this specification, the walls of adjacent single-hole tubes are fused together, and the wall thickness of the microporous tubes refers to the fused wall thickness between two adjacent single-hole tubes.

[0057] The hydrogen storage structure of the PMTS material of the present invention has the following outstanding advantages: the mass density is light, the plasticity precision error is ±2μm, the pore size is 150μm, and the wall thickness is 35μm. The micro-porous honeycomb structure has a limit pressure of >200MPa, a Rockwell hardness of 86-89, high temperature resistance of >1900℃, and low temperature resistance of <-260℃. It has low thermal conductivity, high temperature insulation, and resistance to strong acids and alkalis. The hydrogen storage structure of the PMTS material is very stable even in a high-density hydrogen working atmosphere or a complex dynamic environment.

[0058] At present, in the field of materials, the materials that can realize the focused honeycomb structure and have a certain pressure strength include quartz glass capillary, four kinds of fiber, metal-based materials that do not react with hydrogen, organic polymer-based capillary, inorganic ceramic millimeter-level honeycomb structure and other finished materials. After studying the above-mentioned materials, the present invention found that although each of these materials has its own advantages, their defects in hydrogen atmosphere and high pressure strength are determined by their materials and processes, and there are several major problems such as many uncertainties such as easy hydrogenation and aging, sensitive temperature rise reaction with hydrogen, high mass density specific gravity, defects in the finished product, high defect removal costs, high material costs and high reprocessing costs. Based on the desired optimal material properties and the controllable quality of the micron-level micropore honeycomb structure, the present invention constructs the high-pressure hydrogen storage structure of the present invention.

[0059] In the present invention, a highly reliable, high hydrogen density, high safety and high stability storage structure is constructed based on the compression relationship between the micro volume and mass density ratio, and the PMTS material properties realized by the organic-inorganic optimization are the key determinants. In response to the high risk of high pressure operation of hydrogen storage containers, a research was conducted on the processing technology for a highly safe and stable honeycomb structure that can be realized by combining the developed PMTS material with micron-level pores: if the PMTS material is processed into a honeycomb structure consisting of about 14,000 micropores, with a pore diameter of about 150 μm, a pore wall thickness of about 35 μm, and a depth of about 600 mm, on a mold material with a Rockwell hardness of 86-89 and a diameter of about 25 mm, it is difficult to realize it with the conventional precision processing technology of various micron-level pores. The solution realized by the present invention is as follows: by utilizing the dense liquid phase adhesiveness of the PMTS material composition, the high precision achieved by high temperature melting and sintering of the dense metal phase structure, and the high strength of the wall thickness of several tens of microns, the spatial volume occupied by the micron-diameter polymeric fiber itself is used as the skeleton to form micron spaces through high temperature pyrolysis, and the hardened micron-scale coating layer of PMTS is sintered at high temperature to form an isolation tube wall in which the micron spaces are closely interconnected, thereby realizing a micron-scale pore honeycomb structure.

[0060] The hydrogen storage structure of the PMTS material of the present invention is obtained by a method comprising the following steps. (1) impregnating a polymer fiber bundle with a PMTS material composition; (2) A process of curing the polymer fiber bundle impregnated with the PMTS material composition at 40-45°C, then treating at 50-60°C, then treating at 360-480°C, then sintering at 850-900°C, then sintering at 1400-1450°C or sintering at 3000°C±100°C. These steps result in a hydrogen storage structure of PMTS material.

[0061] In step (2), preferred process conditions (e.g., time) for curing at 40-45°C, treatment at 50-60°C, treatment at 360-480°C, sintering at 850-900°C, sintering at 1400-1450°C, and sintering at 3000°C±100°C are as described in any of the above embodiments.

[0062] Among the many processing problems that the present invention faces and aims to overcome, high-temperature sintering shrinkage deformation and high residual rate are the main difficulties to be overcome, and the following requirements must be realized: it must have relatively high stability in the high-temperature sintering process, the metal phase must achieve a relatively light mass density, the high temperature resistance must be greater than 1900°C, the low temperature resistance must be less than -260°C, the compression limit of the hydrogen storage structure with pore size 100-150μm / wall thickness 35μm must be greater than 200MPa, the formed honeycomb mechanical structure must have strong tensile strength, a Rockwell hardness of about 86, and a relatively high insulation coefficient. In the present invention, the above requirements are realized by optimizing the process parameters of step (2).

[0063] In some embodiments, the viscosity of the PMTS material composition is first adjusted to 200,000 cP±10,000 cP by heating to provide suitable adhesion and flowability, and then the polymer fiber bundle is impregnated. Preferably, the PMTS material composition is treated at 40-45° C. to adjust its viscosity to 200,000 cP±10,000 cP. In some embodiments, the initial viscosity of the PMTS material composition is 90,000±10,000 cP. The amount of the PMTS material composition used is usually sufficient to completely impregnate the polymer fibers. In some embodiments, after the polymer fibers are completely impregnated with the PMTS material composition, the liquid level of the PMTS material composition is about 10 mm higher than the fibers.

[0064] The material of the polymer fiber suitable for the present invention is not particularly limited as long as it has a melting point of 150°C to 380°C. The polymer fiber includes, but is not limited to, continuous fibers and filaments of polymers such as polyvinyl chloride (PVC), polystyrene (PS), ABS plastic, polyethylene (PE), polypropylene (PP), polycarbonate (PC), polyurethane (PU), polyamide (PA, nylon, nylon), etc. The diameter of the polymer fiber may be in the range of microns to millimeters, for example, 70 μm to 5000 μm. A polymer fiber with an appropriate diameter may be selected depending on the desired pore size. In some embodiments, the diameter of the polymer fiber is 100 to 150 μm, for example, 140 to 150 μm. It is preferable that the length of the polymer fiber is 10 mm or more. The upper limit of the length of the polymer fiber is not particularly limited as long as the polymer fiber bundle impregnated with the PMTS material composition does not deform under high-temperature sintering. Preferably, in the present invention, polymer fibers with small diameter error, no impurities, and consistent flexibility are used.

[0065] The number of fibers in the fiber bundle is not particularly limited, and may be, for example, 10,000 to 200,000. The relationship between the bundle volume before impregnation and the bundle volume after impregnation is the bundle volume after impregnation = bundle volume before impregnation + bundle impregnation coating layer volume. The method of impregnating the polymer fiber assembly with the PMTS material composition is not particularly limited, as long as the surface of each individual fiber in the fiber assembly after impregnation is coated with a PMTS material composition having a certain thickness, and adjacent individual fibers are bonded to each other. In some embodiments, both ends of the fiber bundle are locked (e.g., locked with a suspension vice), both ends of the fiber assembly are not impregnated with a fiber assembly of a predetermined length (e.g., about 50 mm), the fiber assembly is impregnated with the PMTS material composition, and both ends are driven to the middle to relax the fiber assembly, and the process is repeated many times until the surface of each single fiber is coated with a certain thickness of the PMTS material composition; the bundled fiber is taken out, both ends are tensioned, sheared at half the length, one end is hung vertically, and the bundle is automatically bonded by the droplet process of the balance tension and gravity of the PMTS material composition. In the present invention, the average thickness of the coating layer of each single fiber in the fiber bundle impregnated with the PMTS material composition is preferably 25 to 30 μm.

[0066] In some embodiments, in step (2), the fiber bundle impregnated with the PMTS material composition is filled into a tubular mold, and then cured at 40 to 45°C, then treated at 50 to 60°C, then treated at 360 to 480°C, then treated at 850 to 900°C, and then sintered at 1400 to 450°C or sintered at 3000°C ± 100°C, thereby producing a single tube having a hydrogen storage structure (also abbreviated as hydrogen storage single tube). Since the PMTS material can be cured at room temperature and normal pressure, it can be understood that it is necessary to fill the fiber bundle impregnated with the PMTS material composition into the tubular mold when it is not basically cured. In the present invention, the material of the tubular mold is preferably the PMTS material or PMTS composite material of the present invention. The PMTS composite material of the present invention includes the PMTS material of the present invention and a reinforcing filler, or is composed of the PMTS material of the present invention and a reinforcing filler, and is obtained by adding the reinforcing filler to the PMTS material composition of the present invention and subjecting it to five treatment steps at 40 to 45°C, 50 to 60°C, 360 to 480°C, 850 to 900°C, and 1400 to 1450°C as described herein. The reinforcing filler suitable for the PMTS composite material of the present invention may be any of various known lightweight and high-strength reinforcing fillers in order to reduce the specific gravity of the PMTS material and / or improve its strength. The reinforcing filler may be, for example, carbon fiber. The amount of reinforcing filler added may be determined as necessary. The shape of the tubular mold suitable for the present invention is not particularly limited as long as it can load and fix the shape of the fiber bundle impregnated with the PMTS material composition, but for example, the tubular mold may include an inner tube and a sleeve. The cross-sectional shape of the tubular mold is not particularly limited, and may be, for example, a hexagon, a circle, a rectangle, a square, a triangle, a concave-convex wedge shape, a parallel polygon, etc. In order to facilitate loading, the inner tube may be divided into two halves; the two inner tubes are respectively filled with bundled fibers, flattened, and then the two inner tubes are glued together to complete loading. The inner tube wall thickness may be 150 μm to 300 μm. The cross-sectional area of ​​the inner space of the inner tube is 69 mm 2 ~1940mm 2It is preferable that the inner tube has a diameter of 10 mm to 50 mm, for example, a circular cross section. It is understood that the length of the tubular mold is the same as the length of the polymer fiber, and is slightly smaller than the length of the polymer fiber normally filled. Both ends of the sleeve are open. The cross-sectional shape, size, and length of the sleeve are the same as the cross-sectional shape of the inner tube, and it is understood that the cross-sectional shape of the sleeve is usually the same as the cross-sectional shape of the inner tube, the inner diameter of the sleeve is usually slightly larger than the outer diameter of the inner tube, and the length of the sleeve is the same as the length of the inner tube. It is preferable that the wall thickness of the sleeve is 1.0 mm to 2.5 mm, for example, about 1.5 mm. In some embodiments, after the inner tube is placed in the sleeve, it is sealed with a PMTS material composition (for example, a PMTS block liquid with a viscosity of 1,000,000 ± 20,000 cP, obtained by adjusting the viscosity by removing the solvent from the PMTS material composition), covered with a plastic sealing film, cured at 40 to 45 ° C, and then processed. It can be understood that in step (2), prior to the treatment at 50 to 60° C., the non-impregnated portion of the bundled fibers may be removed as necessary.

[0067] The bundle of polymer fibers impregnated with the PMTS material composition is then subjected to step (2) to obtain the high pressure hydrogen storage structure of the present invention, or when loaded into a tubular mold, is subjected to step (2) to obtain a mono-tube having the honeycomb hydrogen storage structure of the present invention (abbreviated as mono-tube). Thus, the mono-tube of the present invention includes the high pressure hydrogen storage structure of the present invention and the mono-tube wall (also called shell, from the tubular mold used in manufacturing the mono-tube). After sintering, the high pressure hydrogen storage structure is integrated with the tubular mold (e.g., inner tube and sleeve).

[0068] The high pressure hydrogen storage structure of the present invention preferably has a wall thickness of 35-40 μm and a diameter of 140-150 μm. The single tube of the present invention can be manufactured in a variety of tube shapes, including but not limited to hexagonal, circular, rectangular, quadrangular, triangular, concave-convex wedge, parallel polygonal, etc., and can be applied to special designs and equipment. The tube length of the single tube is preferably within 800 mm. The cross-sectional area of ​​the single tube high pressure hydrogen storage structure is not particularly limited, and for example, when the single tube has a circular cross section and is used in a mobile hydrogen storage transportation means, the diameter of the single tube high pressure hydrogen storage structure may be optimally selected between 10 mm and 50 mm; for example, when applied to a hydrogen storage mobile transportation and mobile hydrogenation station, including a large hydrogen storage station and a large mobile tool such as a ship or a high speed train, the diameter may be enlarged to 200 mm. Depending on the size of the high pressure hydrogen storage structure in the single tube, the wall thickness of the single tube may be 1-15 mm, for example, 1-5 mm. In some embodiments, as shown in FIG. 2, the single tube of the present invention is a circular tube with an outer diameter of 25 mm, an inner diameter (diameter of the high-pressure hydrogen storage structure) of 22 mm, a length of 600 mm, a micropore diameter of 150 μm, a wall thickness of 35 μm, and a single-hole (also called a single-hole tube) volume of 10.5975 mm. 3 The number of single-hole tubes is about 14,000, and the total hydrogen storage capacity of the single tubes is 148,365 mm 3 It is.

[0069] The hydrogen storage structure of the PMTS material of the present invention can meet the hydrogen storage demand of 70 MPa, and is particularly suitable for storing high-pressure gaseous hydrogen. In addition, the PMTS material of the present invention has excellent low-temperature resistance, and can be used for storing liquid hydrogen at ultra-low temperatures by fabricating the PMTS material into a double-layer vacuum structure like a hot water bottle and supplementing it with a high-insulation material. Therefore, the present invention also includes the use of the PMTS material of the present invention in high-pressure hydrogen storage and liquid hydrogen storage.

[0070] After the above single tube is fabricated, N single tubes are put into a PMTS matching tube to be made into one focusing tube based on the shape and diameter of the single tube bundle to be set, and N focusing tubes are arranged in a honeycomb structure module box to obtain a module with excellent overall performance; N multi-modules can be very flexibly combined to the desired capacity and various shapes. Many N modules can be connected in parallel to form the desired large capacity. By using a monomer hydrogen storage tube with a micron-level micropore honeycomb structure with small capacity, high pressure strength, high safety and stability, and combining it into a module (hereinafter referred to as a module) by N tube bundle, it can be combined to any desired capacity. This is a high-pressure hydrogen storage method that achieves high safety and high stability through material and structural performance. Any hydrogen storage capacity can be achieved by combining N single tubes into a focusing tube and combining N focusing tubes into a module. The safe hydrogen storage pressure strength of the module is 70MPa to 110MPa, the pressure strength limit is greater than 200MPa, and the hydrogen storage safety factor at 100MPa is 2.3 times.

[0071] The PMTS material of the present invention generally contains, based on the total mass of the PMTS material, 15-50 wt% silica, 0.5-5 wt% transition metal oxide, 45-85 wt% metal oxide, and unavoidable impurities. The transition metal oxide may contain at least one selected from lanthanum oxide, cerium oxide, lanthanum cerium oxide, and yttrium oxide, and preferably contains at least one selected from lanthanum oxide, cerium oxide, and lanthanum cerium oxide, and yttrium oxide. In some cases, the total content of lanthanum oxide, cerium oxide, and lanthanum cerium oxide in the PMTS material is preferably 0.2-1 wt%, and the content of yttrium oxide is preferably 0.5-5 wt%. The metal oxide may include one or more selected from alumina, zirconia, titania, hafnium oxide, potassium oxide, sodium oxide, magnesium oxide, calcium oxide, zinc oxide and beryllium oxide, and preferably includes alumina, zirconia, titania, hafnium oxide, potassium oxide and / or sodium oxide, magnesium oxide, optional zinc oxide, optional calcium oxide, and optional beryllium oxide. When contained in the PMTS material, it is preferable that the alumina content is 15 to 30 wt%, the zirconia content is 15 to 35 wt%, the titania content is 5 to 15 wt%, the hafnium oxide content is 0.1 to 10 wt%, the combined content of potassium oxide and sodium oxide is 0.1 to 1 wt%, the magnesium oxide content is 0.1 to 0.5 wt%, the barium oxide content is 1 to 2 wt%, the calcium oxide content is 0.05 to 1 wt%, the zinc oxide content is 0 to 10 wt%, and the beryllium oxide content is 1 to 20 wt%.

[0072] Preferably, the PMTS material comprises or consists of, based on the total mass of the PMTS material, 33-39 wt% silica and / or beryllium oxide, 17-22 wt% alumina, 20-28 wt% zirconia, 6-10 wt% titania, 0.25-0.5 wt% hafnium oxide, 0.45-0.9 wt% lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 1-2.7 wt% yttrium oxide, 0.12-1 wt% potassium oxide and / or sodium oxide (e.g., 0.1-0.2 wt% potassium oxide and 0.5-0.9 wt% sodium oxide), 0.18-0.4 wt% magnesium oxide, 1-1.7 wt% barium oxide, 0-10 wt% zinc oxide, and optionally 0.07-0.7 wt% calcium oxide, and unavoidable impurities. In the present invention, the unavoidable impurities usually include one or more selected from carbon, chromium oxide, and iron trioxide, and may also include elements such as mercury, arsenic, phosphorus, manganese, copper, and zinc. When contained, the carbon content is usually 0.013 to 0.015 wt% based on the total mass of the PMTS material. When contained, the chromium oxide content is usually 0.01 to 0.02 wt% based on the total mass of the PMTS material. When contained, the iron trioxide content is usually 0.01 to 0.015 wt% based on the total mass of the PMTS material. It can be understood that the iron trioxide and chromium oxide are due to trace components contained in the raw material, and the carbon is left behind after the polymer or carbide is sintered. In some embodiments, the PMTS material contains 0.013-0.015 wt% carbon, 0.01-0.015 wt% iron trioxide, and 0.01-0.02 wt% chromium oxide, based on the total mass of the PMTS material. In the present invention, the total content of impurities other than carbon, chromium oxide, and iron trioxide in the unavoidable impurities does not usually exceed 0.01 wt% of the total mass of the PMTS material, but such impurities may include elements such as mercury, arsenic, phosphorus, manganese, copper, and zinc. In some embodiments, the silica and / or beryllium oxide contained in the PMTS material may be 33-39 wt% silica, or 33-39 wt% silica and beryllium oxide, and the content of beryllium oxide is preferably 3-15 wt% of the total mass of the PMTS material, such as 3-13 wt%, 5-15 wt%.

[0073] In some embodiments, the PMTS material is prepared from a zinc carbide-free PMTS material composition, such PMTS material comprising, or consisting of, by weight of the total PMTS material, 37-39 wt.% silica and / or beryllium oxide, 19-22 wt.% alumina, 23-28 wt.% zirconia, 7-10 wt.% titania, 0.3-0.5 wt.% hafnium oxide, 0.5-0.9 wt.% lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 1.2-2.7 wt.% yttrium oxide, 0.12-1 wt.% potassium oxide and / or sodium oxide (e.g., 0.1-0.2 wt.% potassium oxide and 0.5-0.9 wt.% sodium oxide), 0.2-0.4 wt.% magnesium oxide, 1.2-1.7 wt.% barium oxide, and optionally 0.08-0.7 wt.% calcium oxide, and unavoidable impurities. In these embodiments, the 37-39 wt% silica and / or beryllium oxide contained in the PMTS material may be 37-39 wt% silica, or 37-39 wt% silica and beryllium oxide, with the beryllium oxide content being preferably 5-18 wt%, for example 7-18 wt%, 5-15 wt%, of the total mass of the PMTS material.

[0074] Similar implementation scheme to the present invention: Micron-class glass capillary is generally used in non-pressure applications, and can also be used as a concentrated hydrogen storage material with a certain pressure in terms of high-pressure hydrogen storage. Its advantages: it can meet the hydrogen storage demand of 70MPa, with a pressure limit of 140MPa and a safety factor of 2. Disadvantages: 1. The upper limit of strength is determined by the material, and there is no development potential; 2. It is difficult to resolve defects such as impurities / bubbles / cracks caused by raw materials and processes, and the defect rate is very high, which is difficult to detect with the naked eye; The collapse of a defect on a single capillary under high pressure will lead to leakage throughout the entire public hydrogen storage system, and for hydrogen storage containers with hundreds of thousands of capillaries, it is difficult to control the quality and there is a high risk of danger; 3. The high cost of applying glass capillaries with micron-level pore size to hydrogen storage containers = (1) application cost per capillary tube x hundreds of thousands of capillaries + (2) cost of addressing capillary defects + (3) high-temperature sealing cost per capillary tube and cost of addressing sealing defects + (4) cost of gluing and bundling N capillaries + (5) time cost.

[0075] Compared with the micron-grade glass capillary solution, the present invention has the following outstanding advantages:

[0076] 1. The single tube honeycomb hydrogen storage structure is made of PMTS material with directional design for new high-pressure hydrogen storage structure and micron pores made by special process. Through intelligent high-temperature sintering, it has low specific gravity, high purity, high precision and high hardness, and is widely used. The process quality has relatively good consistency;

[0077] 2. The performance of PMTS micron pore honeycomb structure in all respects exceeds the limit index of quartz capillary by more than two times, and the pressure strength of the microtube with 150μm pore diameter and 35μm wall thickness of the honeycomb structure is >200MPa;

[0078] 3.Production cost comparison: A single tube with a diameter of 25 mm and a micro-hole honeycomb structure has 14,000 micro-holes with a pore diameter of 150 μm and a length of 600 mm. The production cost in the mass production pipeline is one-third of the cost of a single quartz capillary tube with a pore diameter of 150 μm and a length of 1,000 mm;

[0079] 4. Analysis of metallographic structure and aging test of PMTS material: The hydrogen storage container with PMTS microporous honeycomb structure has a continuous service life of more than 20,000 hours, which is more than twice as long as the continuous service life of quartz capillary tube (8,000 hours).

[0080] The present invention has the following advantages:

[0081] 1. The present invention provides a hydrogen storage container material PMTS (hereinafter referred to as PMTS, which is an organic polymer PI + inorganic metal phase structure) that is lightweight, resistant to high pressure, high temperature, strong acid-base resistance, and has high safety and stability, and can achieve higher hydrogen storage mass density instead of imported high-quality carbon fiber.

[0082] 2. Invented a honeycomb high-pressure hydrogen storage structure integrated with micron-sized micropores on PMTS, limiting the chain reaction of degradation caused by dynamic and active collision of hydrogen through the micron-sized micro-pores of the hydrogen storage space, realizing a high-pressure hydrogen storage capacity of 70MPa to 110MPa with high safety and high stability under complex dynamic working environment, and having a safety factor of more than twice as much, the volume is reduced by 50% compared with carbon fiber containers of the same pressure and capacity, overturning the current situation where the CFRP coating layer of the container is large and clumsy. The honeycomb high-pressure hydrogen storage structure of the micron-sized micropores of the present invention can be very conveniently formed into various shapes, has very strong convenience and flexibility of use, and can be applied according to the national conditions of our country, and can be a reference technology with broad development prospects.

[0083] 3. Outstanding advantages of PMTS material and micron pore honeycomb structure: (1) Mass specific gravity: 5.2g / cm 3 degree can be reached; (2) Fast gas filling: With the same volume, gas filling takes just a few seconds, which is significantly lower than the 5kg / 3min gas filling standard. (3) Small volume and can be miniaturized: The micron-level microporous honeycomb structure has super strong high-pressure hydrogen storage capacity, and omits the thick and clumsy carbon fiber coating layer. The hydrogen storage module is half the volume of a carbon fiber container with the same pressure capacity. The hydrogen storage tube has flexible placement and can be scientifically designed to be reasonably placed on the wings, cabin panels, bottom panels and any plate walls of an aircraft, making the hydrogen storage container almost invisible. The microporous honeycomb high-pressure hydrogen storage structure can be miniaturized and combined with a micro hydrogen fuel cell (the combined volume is the size of a cigarette case) to form a wearable micro mobile power supply device. (4) Hardness: Rocks 86-89, (5) High pressure resistance: Due to the superiority of PMTS material and the mechanical structure of the micro-pore honeycomb net, it can easily achieve hydrogen storage pressures of 70MPa to 110MPa, with a safety factor of 2.3 times. In a comparative test of high-pressure hydrogen storage with a quartz capillary tube with a higher mass density, the quartz capillary tube burst at 140MPa, but the PMTS micro-pore honeycomb structure single tube had a tolerance of up to 200MPa. (6) Large hydrogen storage capacity: It can withstand high pressure in a small volume and store hydrogen at a high density. The module formed by parallel bundling of single tubes can be connected in parallel with any number of modules to realize hydrogen transfer tools of any capacity, high-density hydrogen transportation, mobile hydrogen addition stations, and large-scale hydrogen storage stations; (7) Strong stability: the module tensile strength is 3200MPa, high temperature resistance >1900℃, acid-base resistance pH 3-14, and good safety stability even in unforeseen force majeure; (8) High safety: The PMTS microporous honeycomb structure breaks up the fluid turbulence under the impact of the high-pressure hydrogen injection gas flow through its dense microporosity, so that no high-pressure temperature rise occurs. The microporous honeycomb structure effectively limits the dynamic activation energy of hydrogen under any dynamic conditions, and even if the internal stress caused by the unexpected ultra-high pressure is instantly broken down in the honeycomb structure, it can effectively avoid the harm caused by the internal stress caused by the high-pressure high-velocity temperature rise, thereby ensuring the quality stability and high safety of the container; (9) Service life: The continuous service life is more than 20,000 hours, which is about three times that of a quartz capillary tube; (10) Strong economical efficiency: the structure is sturdy, the defect rate is extremely low, the service life is long, and the cost is only 30-40% of that of carbon fiber containers.

[0084] 4. The focused hydrogen storage module formed from PMTS and microporous honeycomb structure of the present invention realizes a lightweight, small-volume, high-safety, high-stability high-pressure hydrogen storage technology exceeding 100 MPa, overturning the technical line of hollow hydrogen storage quality density dependent on CFRP. In contrast to the application limit of CFRP technology in 70 MPa high-pressure hydrogen storage, PMTS and microporous honeycomb structure have great potential for quality improvement in high-pressure hydrogen storage capacity and more hydrogen energy application fields. The microporous single-tube focused module of the present invention is not subject to any capacity or external shape restrictions. The application effect and economy of the highly safe / highly stable hydrogen storage method of the present invention can greatly promote the widespread application of hydrogen energy. The present invention can be adapted to various complex working environments in special fields, and has broader application potential in the field of mobile power generation of micro-sized hydrogen fuel cells. EXAMPLES

[0085] The present invention will be described below as specific embodiments, with the purpose of providing a better understanding of the contents of the present invention. It should be understood that these embodiments are merely illustrative and not limiting. The raw materials and reagents used in the examples are commonly purchased on the market unless otherwise specified. The experimental methods, manufacturing methods and measurement methods used in the examples are all common methods or methods recommended by the manufacturers unless otherwise specified. The equipment used in the examples are all common equipment in the art unless otherwise specified. In the examples, percentages refer to mass percentages unless otherwise specified.

[0086] In the following examples, except for high purity ultrafine hafnium oxide and ultrafine lanthanum oxide, the other high purity oxides (purity 4N, 5N, 6N grade) are all ultrafine powders of 10,000 grade or higher obtained by high pressure air current pulverization suspension fine powder collection method; the metal oxide particles used are all nano-sized high purity raw materials. Here, the following material / product properties / performance detection devices / methods and experimental equipment / conditions were adopted:

[0087] 1.Raw material quality inspection: Thermo Scientific NITON(Niton)XL5 handheld alloy analyzer.

[0088] 2. Elemental testing of process products and final products: Thermo Fisher ARL Perform'X 4200 XRF wavelength-dispersive sequential scanning X-ray fluorescence spectrometer; Maximum output power of X-ray generator: ≧4.2kW; Rated voltage: ≧70kW; Rated current: ≧140kW; X-ray light tube: Rh target; Ceramic end window X-ray tube: ≧4.2kW; Beryllium window thickness: ≦50μm; Sample excitation distance: ≦16mm; Irradiation method: bottom irradiation method, that is, the sample is above the X-ray tube; Solid-state high-frequency generator: external voltage fluctuation 1%, output voltage stability ±0.00005%, ensuring high accuracy of testing; Scanning method: continuous scanning; Detector: fluid positive ratio counter, scintillation counter, two counters arranged in parallel, all in the spectrum chamber; Detection type: sequential detection, automatic recording; It was required that the sample was free of contamination.

[0089] 3. Viscosity test: NDJ-8S rotational speed viscometer.

[0090] 4. Metallography: Carl Zeiss research-grade upright metallography microscope Axio Lab A1 Pol.

[0091] 5. Acid-alkali resistance test: pH3 test: Dimension 30mm from PMTS template 3Several cubes were laser cut, without the need for precise polishing, and prepared for microscopic examination; In the laboratory at 25°C, they were placed in a glass beaker containing pure ethanol for 30 minutes, then removed with a bamboo clip and placed on a dry filter paper plate for 20 minutes. Three pieces were taken out and placed in a glass beaker containing a pH=3 hydrochloric acid solution in a control box, sealed and left for 24 hours, then removed, rinsed with clean water, and dried with dry paper. pH14 test: The glass beaker containing a pH=3 hydrochloric acid solution in the control box was replaced with a glass beaker containing a pH=14 sodium hydroxide solution, and the other steps were tested at pH3; pH microstructural examination and evaluation criteria: Microcorrosion metals and alloys regulations ASTM E 407-07 (Reapproved 2015) el 7.1-7.15 inspection criteria.

[0092] 6. High temperature resistance test: Using a thermal conductivity tester, the temperature inside the car was set to 60°C to simulate the heat of summer.

[0093] 7. High and low temperature Charpy impact test: A single tube loaded with 70MPa air pressure was placed in a high temperature environment of 50℃, held there for 15 minutes, then transferred to a low temperature environment of -15℃ for 20 seconds and held there for 15 minutes. This was repeated 17 times (9 high temperature and 8 low temperature), and the holding time between high and low temperature for each test was 15 minutes, and the switching time between high and low temperature was always 20 seconds. It was observed whether the single tube burst.

[0094] 8. Tensile strength test: A general-purpose material performance tester was used, and the force value accuracy was ±0.5%; the sample was 30 mm thick, 1000 mm long, and 500 mm wide, and there were three PMTS molding templates for testing.

[0095] 9.Density test: Electronic hydrometer.

[0096] 10. Sintering analysis, temperature monitoring: automatic far-infrared temperature detector.

[0097] 11. Electro-hydraulic servo fatigue test: MTS electro-hydraulic servo fatigue tester; Inspection standard: Engine blade and material vibration fatigue test method HB 5287-96 7; Sustained durability and continuous use life simulation.

[0098] 12. Limit pressure test: Computer type 200MPa test stand, Schmidt, model number: SUPC_XT_200.

[0099] 13. Gas filling speed test: SUPC_XT_200 test stand, Schmidt, 0.1Pa~70MPa water pressure speed test: based on the sample pressure, the booster pump outputs the set high pressure; test pressure: 0~200MPa; booster flow rate: 1.2L / min; pressure control accuracy: upper limit +2%, lower limit -1%; test medium: liquid water; pressure control: computer / manual; operation method: computer / manual; structure: circulation system, pressure control system; workpiece: installation device, manual control; note: the content and method of this test were the test method designed by the inventor himself, since there was no corresponding inspection mechanism or inspection standard; installation of the facility, test process: (1) The inflation valve of a 70 MPa, 5 kg capacity air tank (A tank) for testing was attached to the high-pressure output connector of the pressure pump on the test stand, and the water intake of the pressure pump was connected to a filtered purified water source dedicated for testing; (2) Open the air intake valve of the PMTS hydrogen storage module (B tank) with a hydrogen storage capacity of 2 kg, and connect the expansion valve to the interface of the air intake solenoid valve of the A tank via a chrome molybdenum connecting tube from the high-pressure flow meter → pressure gauge → computer-controlled pressure solenoid valve, open the air intake valve and expansion valve of the A tank, then connect a vacuum pump to the air intake valve of the B tank. After inspection, start the vacuum pump to create a vacuum in the connected A and B tanks, and close the air intake valves of the A and B tanks. (3) set the output pressure value on the test bench computer to 70 MPa; (4) The air valve of tank A was opened; (5) The test stand was computer-activated or manually activated; (6) When the test stand was boosted and the set pressure value of 70 MPa was reached in Tank A, the pressure was maintained for 2 minutes, and then the air supply solenoid valve of Tank A was opened to supply air to Tank B. Within a few seconds, the pressure in Tank B reached 70 MPa, the gas-filled solenoid valve of Tank B was closed, and the test was completed.

[0100] 14. Intermittent and constant temperature control: intelligent high temperature regulation console.

[0101] 15. Vacuum reaction kettle / vacuum pump / temperature / intelligent control: The vacuum reaction kettle's preliminary operating state was 35℃, and its operating state was 40℃~42℃, and the vacuum degree had to be constantly maintained in the range of -96kPa~-101kPa.

[0102] 16. Operating condition / operational stability test: Operating condition / operational stability at temperatures of -18℃~65℃ under 70MPa pressure with Tenney (TJR-T2) environmental test box / pressure gauge, PMTS material and hydrogen storage tube.

[0103] 17. Rockwell hardness test: The test accuracy standard is based on the GB / T230 and ISO6508 standards. A 120-degree diamond cone indenter is used to indent the surface of the sample in two steps. After the main test force is removed, the residual indentation depth is measured under the first test force. The residual indentation depth indicates the hardness.

[0104] 18. Liquid nitrogen cryogenic test: PMTS precision structure was placed in liquid nitrogen for 10 minutes and then taken out.

[0105] Example 1 In this example, a PMTS material composition of the present invention was prepared by the following process:

[0106] (1) Preparation of composition A: 17 parts by weight of analytical pure anhydrous aluminum chloride and 5 parts by weight of analytical pure magnesium chloride are added to a transparent reaction vessel, mixed, 22 parts by weight of distilled water are added, and stirred to obtain a mixed solution of aluminum chloride and magnesium chloride with a concentration of 50 wt%, 1.2 parts by weight of analytical pure sodium hydroxide and 0.5 parts by weight of analytical pure potassium hydroxide are added stepwise, reacted and cooled to produce a white precipitate, a transparent liquid is extracted, 3 parts by weight of analytical pure barium chloride are added to the white precipitate, stirred and left to stand for 30 minutes, dried at 100°C, treated at a high temperature of 870°C for 90 minutes, cooled, and pulverized to 8000 mesh or more by a ball mill to prepare composition A;

[0107] (2) Preparation of composition B: Composition B was prepared by stirring 12 parts by weight of nano alumina (model number: MG-AI032, purity 99.99%), 16 parts by weight of zirconia (model number: VK-R60, particle size 1-5 μm, purity 99.9%), nano yttrium oxide (purity 99.99%), 8 parts by weight of nano titania (model number: DT-O-007-2, rutile type, purity >99.9%), and 0.5 parts by weight of ultrafine hafnium oxide (model number: H301462, purity 99.99%).

[0108] (3) Preparation of composition C: 24 parts by weight of PI (US DuPont SP-1) was dissolved in dimethylformamide to obtain a PI solution with a concentration of 30 wt%, which was then added to a vacuum reaction vessel. The temperature inside the vessel was maintained at 40°C, the degree of vacuum was maintained at -94 kPa, dimethylformamide was gradually added to adjust the viscosity to 90,000 cP, and the mixture was stirred for 25 minutes at a rotation speed of 10 r / min. Then, 33 parts by weight of nanosilica (purity 99.999%, 5N grade) was gradually added, and the mixture was stirred for 15 minutes. The entire composition B prepared in step (2) was then added, and the mixture was mixed for 20 minutes. Then, 0.5 parts by weight of ultrafine lanthanum oxide (purity 99.99%) was added, and the mixture was stirred for 15 minutes to prepare composition C.

[0109] (4) Preparation of PMTS material composition: 12 parts by weight of PVAc (Shandong Jinan Pulihua Chemical Co., Ltd., industrial grade, purity 99.9%, characteristic viscosity 0.80 dL / g) was diluted with distilled water to a concentration of 75 wt%, stirred for 10 minutes, the entire composition A prepared in step (1) was added and stirred for 20 minutes, the resulting mixture was added to the vacuum reaction kettle containing the entire composition C prepared in step (3), an appropriate amount of dimethylformamide was added, the mixture was heated to 45°C, and stirred at a rotation speed of 10 r / min to adjust the viscosity to 90000 cP, and a white bubble-free product, i.e., PMTS material composition, was prepared.

[0110] The PMTS material composition obtained in this embodiment can be stably stored and can be used to manufacture a single-tube high-pressure hydrogen storage structure made of PMTS material. For details, see Example 2.

[0111] Example 2 In this example, a single tube of a high-pressure hydrogen storage structure made of the PMTS material of the present invention was manufactured using the PMTS material composition manufactured in Example 1 by the following process:

[0112] First step: The PMTS material composition with a viscosity of 90,000 cP prepared in Example 1 was placed in a stainless steel U-shaped flat-bottom tank (length 1,500 mm, width 500 mm, height 200 mm), heated to 42°C to adjust the viscosity to 20,000 cP, and a PMTS concentrate was prepared. The final amount of PMTS concentrate added to the flat-bottom tank was such that after the polymer fibers were placed in, the liquid level of the PMTS concentrate was 10 mm higher than the completely impregnated fibers.

[0113] Step 2: Prepare a fiber bundle consisting of approximately 16,800 polypropylene continuous fibers with a diameter of 150 μm and a length of 1,340 mm in advance, lock both ends of the fiber bundle in a suspension vice, and leave both ends of the fiber bundle unimpregnated for a length of 50 mm each. The fiber bundle is impregnated with the PMTS concentrated solution prepared in step 1, and the ends are pushed toward the middle to relax the fiber bundle. This process is repeated many times until the surface of each single fiber is covered with a PMTS concentrated solution with a thickness of approximately 25 μm to 30 μm; the bundle is removed from the liquid tank, both ends are tensioned, sheared at half the length, and one end is hung vertically, and the bundle is automatically adhered by the balanced tension of the PMTS concentrated solution and the droplet process of gravity. Before curing, the bonded bundled fibers were inserted into an inner tube with a regular hexagonal cross section, parallel opposite side outer diameter (distance between parallel opposite sides including wall thickness) of 24.5 mm, wall thickness of 150 μm, length of 620 mm, and the inner tube was divided into two halves, and the bundled fibers were laid out in the two halves of the inner tube and flattened, and then the other half of the inner tube was bonded; the inner tube was inserted into a sleeve with a regular hexagonal cross section, parallel opposite side inner diameter (excluding the distance between parallel opposite sides including wall thickness) of 25 mm, wall thickness of 1.5 mm, length of 620 mm, and one end was sealed with a PMTS blocking liquid with a viscosity of 1,000,000 cP (the viscosity was adjusted by removing the solvent from the PMTS material composition of Example 1 at 45 ° C). Then, the plastic sealing film was covered, and the tube was continued to be hung and cured in a sealed environment with a constant room temperature of 42 ° C and air humidity of 10% for 240 minutes.

[0114] The material of the tubular mold (including the inner tube and sleeve) used in this embodiment is PMTS material. The PMTS material composition prepared in Example 1 was cured in a sealed environment at 42°C and 10% humidity for 240 minutes, then cured at 50°C for 60 minutes, and then sintered at 480°C for 60 minutes to obtain a hardened semi-finished product, which was then sintered at 880°C for 90 minutes to obtain a metal phase structure semi-finished product, which was then sintered at 1430°C for 300 minutes.

[0115] Step 3: Remove the unimpregnated part of the fiber bundle, put it into the tunnel kiln, set the kiln body temperature of each stage of the tunnel kiln in advance, harden at 50°C for 60 minutes, then sinter at 480°C for 60 minutes to obtain a hardened semi-finished product, then sinter at 880°C for 90 minutes to obtain a metal phase structure semi-finished product, then sinter at 1430°C for 300 minutes to complete the sintering, and obtain a single high pressure hydrogen storage structure tube made of PMTS material.

[0116] As measured by an X-ray fluorescence spectrometer (Thermo Fisher ARL Perform'X 4200 XRF), the PMTS material produced in this example consists of 38.74 wt% silica, 19.71 wt% alumina, 26.32 wt% zirconia, 8.65 wt% titania, 0.46 wt% hafnium oxide, 0.71 wt% lanthanum oxide, 2.43 wt% yttrium oxide, 0.12 wt% potassium oxide, 0.84 wt% sodium oxide, 0.36 wt% magnesium oxide, 0.015 wt% carbon, 1.61 wt% barium oxide, 0.013 wt% iron trioxide, 0.014 wt% chromium oxide, and 0.008 wt% impurities, based on the total mass of the PMTS material.

[0117] The high pressure hydrogen storage structure single tube made of PMTS material manufactured in this example has a micron micropore honeycomb structure, the length of the single tube is 620 mm, the cross section is a regular hexagon, the parallel opposite side outer diameter of the sleeve is 28 mm, the parallel opposite side inner diameter is 25 mm, the microscopic dimension of the wall thickness of each micropore is 35 μm to 40 μm, and the microscopic diameter of each micropore is 140 μm to 150 μm. One single tube has about 16,800 micron single hole tubes, and the hydrogen storage volume of each micron single hole tube is about 10.6 mm. 3Therefore, a single tube with a micro-porous honeycomb structure has a hydrogen storage capacity of about 178080 mm3. 3 , i.e. 0.000178m 3 The high-pressure hydrogen storage structure single tube made of PMTS material can be applied to complex dynamic environments and can realize highly safe and highly stable hydrogen storage. The volume of the high-pressure hydrogen storage structure single tube made of PMTS material was reduced by 50% compared to a hollow carbon fiber container of the same capacity of 70 MPa. The desired hydrogen storage capacity or scale can be realized by a focusing tube obtained by connecting N single tubes in parallel, a module combining N focusing tubes, and / or a combination of N modules. A mechanical schematic diagram of the honeycomb structure module made of single tubes of this embodiment is shown in Figure 3.

[0118] Test example 1: Performance test of single tube high pressure hydrogen storage structure made of PMTS material The single tube manufactured in Example 2 was subjected to high and low temperature Charpy impact tests, and the results showed that the single tube had no burst leakage, indicating that the single tube of the present invention can meet the hydrogen storage requirement of 70 MPa.

[0119] The single pipe manufactured in Example 2 was subjected to an electric-hydraulic servo fatigue test, and the continuous service life simulation measurement of the single pipe was >20,000 hours, indicating that the single pipe of the present invention has a long service life.

[0120] The limit pressure of the single tube manufactured in Example 2 was measured on a 200 MPa test bench, and the pressure that the single tube could withstand exceeded the detection limit (detection limit is 200 MPa), indicating that the single tube of the present invention has a high limit pressure. The safe hydrogen storage pressure was set based on the limit pressure as follows: safe hydrogen storage pressure = hydrogen storage limit pressure / safety factor (usually 2); for special applications, it is necessary to set a relatively small safe hydrogen storage pressure with a larger safety factor. The micron-level microporous honeycomb hydrogen storage structure of the present invention suppresses the pressure rise of high-pressure hydrogen activation energy in any environment, so that the microporous honeycomb hydrogen storage structure of the present invention can have particularly high safety and high stability in any complex environment with a safety factor of 2 times.

[0121] A gas filling speed test was conducted on the single tube manufactured in Example 2, and the simulated gas filling speed of 70 MPa was 2 kg / 3 s, demonstrating that the hydrogen storage structure of the present invention has a fast gas filling speed, and showing that the PMTS material and the micro-porous honeycomb hydrogen storage structure eliminate the influence of turbulence caused by the high-speed gas filling flow of the hollow bile hydrogen storage structure on the gas filling speed. At present, the gas filling speed standard of 70 MPa hollow bile hydrogen storage containers at home and abroad is 5 kg / 3 min.

[0122] A liquid nitrogen ultra-low temperature test was conducted on the single tube manufactured in Example 2. The single tube was immersed in liquid nitrogen for 10 minutes and then removed, and there was no burst deformation. This demonstrates that the single tube of the present invention has excellent low temperature resistance.

[0123] As a result of the operating condition / operating stability test of the single tube manufactured in Example 2, the single tube was maintained at a low temperature (-18°C) and a high temperature (65°C) for 15 minutes each, and the compression change was within the range of ±5% at 70 MPa, indicating that the single tube of the present invention has good operating stability.

[0124] Test example 2: Performance test of PMTS material The PMTS material composition of Example 1 was cast into a thin plate, cured in a sealed environment at 42°C and 10% humidity for 240 min, then cured at 50°C for 60 min, then sintered at 480°C for 60 min to obtain a hardened semi-finished product, then sintered at 880°C for 90 min to obtain a metallographic semi-finished product, and then sintered at 1430°C for 300 min to obtain PMTS samples with thicknesses of 5 mm and 30 mm.

[0125] The PMTS template with a thickness of 5 mm made from the PMTS material composition of Example 1 has a specific gravity of 5.2 g / cm 3 , the Rockwell hardness was 87, indicating that the PMTS material of the present invention has high hardness.

[0126] The acid-base resistance test was conducted on the 5 mm thick PMTS template, and the PMTS template showed no corrosion damage at pH=3 and pH=14 (ASTM E407-07 (Reapproved 2015) el 7.1-7.15 measurement standard). The PMTS samples that underwent the acid-base resistance pH3 test and pH14 test were subjected to Rockwell hardness measurement, and the hardness was all 87, demonstrating that the PMTS material of the present invention has excellent acid-base resistance.

[0127] A high temperature resistance test was conducted on a PMTS template with a thickness of 5 mm at a vehicle interior temperature of 60°C to simulate exposure to a hot summer day. As a result, the thermal conductivity of the PMTS template manufactured from the PMTS material composition of Example 1 was 2.67 W / (m K), demonstrating that the PMTS material of the present invention has excellent high temperature resistance.

[0128] A tensile strength test was carried out on a PMTS template having a thickness of 30 mm, and the results showed that the tensile strength of the PMTS template made from the PMTS material composition of Example 1 was >3000 MPa, indicating that the PMTS material of the present invention has high tensile strength.

Claims

1. The raw materials of the hydrogen storage structure material composition include 20 to 24 parts by weight of polyimide, 12 to 13 parts by weight of polyvinyl acetate, 15 to 17 parts by weight of aluminum chloride, 3 to 5 parts by weight of magnesium chloride, 3 to 5 parts by weight of barium chloride, 10 to 12 parts by weight of alumina, 15 to 17 parts by weight of zirconia, 0.5 to 0.7 parts by weight of lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 32 to 35 parts by weight of silica, silicon carbide and / or beryllium oxide, 1.5 to 2.5 parts by weight of sodium hydroxide and / or potassium hydroxide, 1.5 to 3 parts by weight of yttrium oxide, 6 to 8 parts by weight of titania and / or titanium carbide, and 0.3 to 0.5 parts by weight of hafnium oxide and / or hafnium carbide; The raw material of the hydrogen storage structure material composition further contains water and a polar solvent selected from the group consisting of dimethylacetamide, dimethylformamide, and N-methylpyrrolidone; The viscosity of the hydrogen storage structure material composition is 90,000±10,000 cP; The hydrogen storage structural material composition is prepared by a method comprising the steps of: (1) A process for obtaining composition A by mixing aluminum chloride and magnesium chloride, dissolving them in water, adding sodium hydroxide and / or potassium hydroxide, reacting them to produce a white precipitate, collecting the white precipitate, adding barium chloride, stirring uniformly, drying, subjecting the mixture to a high-temperature treatment at 700 to 900°C, and pulverizing the mixture to obtain composition A, wherein the concentration of the mixed solution of aluminum chloride and magnesium chloride obtained by adding water is 40 to 60 wt%, the time of the high-temperature treatment is 80 to 100 min, and the mesh number of composition A after pulverization is 8000 mesh or more, (2) mixing alumina, zirconia, yttrium oxide, titania and / or titanium carbide, and hafnium oxide and / or hafnium carbide to obtain composition B; (3) adding silica, silicon carbide and / or beryllium oxide to a polyimide solution, stirring uniformly, adding composition B, stirring uniformly, adding lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, stirring uniformly, and then obtaining composition C; wherein the polyimide solution is a solution in which polyimide is dissolved in a polar solvent, the polar solvent being selected from dimethylacetamide, dimethylformamide and N-methylpyrrolidone, the viscosity of the polyimide solution is 90000 cP±2000 cP, and step (3) is carried out at 35 to 45° C. and under a vacuum of −94 kPa to −101 kPa; (4) adding composition A to the polyvinyl acetate solution, stirring uniformly, and then mixing the resulting mixture with composition C and stirring uniformly, wherein the polyvinyl acetate solution is an aqueous solution of polyvinyl acetate and has a concentration of 70-80 wt %, mixing the mixture of the polyvinyl acetate solution and composition A with composition C at 35-45° C. and under a vacuum of −94 kPa to −101 kPa, mixing the mixture of the polyvinyl acetate solution and composition A with composition C, and then adding a polar solvent selected from dimethylacetamide, dimethylformamide, and N-methylpyrrolidone to adjust the viscosity of the mixture to 90,000±10,000 cP, Through these steps, the hydrogen storage structural material composition is obtained. Structural hydrogen storage material compositions.

2. A hydrogen storage structural material comprising, by total mass, 33-39 wt% silica and / or beryllium oxide, 17-22 wt% alumina, 20-28 wt% zirconia, 6-10 wt% titania, 0.25-0.5 wt% hafnium oxide, 0.45-0.9 wt% lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 1-2.7 wt% yttrium oxide, 0.12-1 wt% potassium oxide and / or sodium oxide, 0.18-0.4 wt% magnesium oxide, 1-1.7 wt% barium oxide, and unavoidable impurities; The hydrogen storage structure material is manufactured by a method including the steps of: subjecting the hydrogen storage structure material composition according to claim 1 to a hardening treatment at 40-45°C for 200-250 min, followed by a heat treatment at 50-60°C for 50-70 min, followed by a heat treatment at 360-480°C for 50-70 min, followed by a sintering treatment at 850-900°C for 80-100 min, followed by a sintering treatment at 1400-1450°C for 250-350 min or a sintering treatment at 3000°C±100°C. Structural materials for hydrogen storage.

3. A composite material for hydrogen storage structure comprising a material for hydrogen storage structure and a reinforcing filler, The hydrogen storage structural material contains, based on the total mass of the hydrogen storage structural material, 33 to 39 wt % of silica and / or beryllium oxide, 17 to 22 wt % of alumina, 20 to 28 wt % of zirconia, 6 to 10 wt % of titania, 0.25 to 0.5 wt % of hafnium oxide, 0.45 to 0.9 wt % of lanthanum oxide, cerium oxide and / or lanthanum cerium oxide, 1 to 2.7 wt % of yttrium oxide, 0.12 to 1 wt % of potassium oxide and / or sodium oxide, 0.18 to 0.4 wt % of magnesium oxide, 1 to 1.7 wt % of barium oxide, and inevitable impurities; The hydrogen storage structural composite material is produced by a method including: subjecting a mixture of the hydrogen storage structural material composition and a reinforcing filler according to claim 1 to a curing treatment at 40-45°C for 200-250 min, followed by a heat treatment at 50-60°C for 50-70 min, followed by a heat treatment at 360-480°C for 50-70 min, followed by a sintering treatment at 850-900°C for 80-100 min, followed by a sintering treatment at 1400-1450°C for 250-350 min or a sintering treatment at 3000°C±100°C; Structural composite materials for hydrogen storage.

4. 3. A single hydrogen storage tube comprising a hydrogen storage unit, the hydrogen storage unit being made of the hydrogen storage structural material according to claim 2, the hydrogen storage unit having a honeycomb microporous structure.

5. A hydrogen storage tube as described in claim 4, wherein the wall thickness of the micropores is 35 to 40 μm.

6. A hydrogen storage tube as described in claim 4, wherein the pore diameter is 140 to 150 μm.

7. 5. The hydrogen storage single tube according to claim 4, further comprising a shell, the material of which is the hydrogen storage structural material according to claim 2 or the hydrogen storage structural composite material according to claim 3.

8. 5. A method for manufacturing a hydrogen storage single tube according to claim 4, said method comprising the steps of: (1) impregnating a polymer fiber bundle with the hydrogen storage structural material composition of claim 1; (2) A process of subjecting the polymer fiber bundle impregnated with the hydrogen storage structure material composition to a curing treatment at 40 to 45°C for 200 to 250 minutes, followed by a heat treatment at 50 to 60°C for 50 to 70 minutes, followed by a heat treatment at 360 to 480°C for 50 to 70 minutes, followed by a sintering treatment at 850 to 900°C for 80 to 100 minutes, followed by a sintering treatment at 1400 to 1450°C for 250 to 350 minutes or a sintering treatment at 3000°C ± 100°C; or The polymer fiber bundles impregnated with the storage structure material composition are filled into a tubular mold, followed by a curing treatment at 40-45°C for 200-250 min, followed by a heat treatment at 50-60°C for 50-70 min, followed by a heat treatment at 360-480°C for 50-70 min, followed by a sintering treatment at 850-900°C for 80-100 min, followed by a sintering treatment at 1400-1450°C for 250-350 min or a sintering treatment at 3000°C±100°C, A method for manufacturing a single hydrogen storage tube, wherein the material of the tubular mold is the material for a hydrogen storage structure according to claim 2 or the composite material for a hydrogen storage structure according to claim 3.

9. A method for manufacturing a single hydrogen storage tube as described in claim 8, wherein the viscosity of the hydrogen storage structural material composition is adjusted to 200,000 ± 10,000 cP before impregnation in step (1).

10. A method for manufacturing a single hydrogen storage tube as described in claim 8, wherein the melting point of the polymer fiber is 150°C to 380°C.

11. A method for manufacturing a single hydrogen storage tube as described in claim 8, wherein the diameter of a single fiber in the polymer fiber bundle is 100 to 150 μm.

12. A method for manufacturing a single hydrogen storage tube as described in claim 8, wherein in step (1), the average thickness of the hydrogen storage structural material composition that coats the surface of each single fiber in the polymer fiber bundle by the impregnation is 25 to 30 μm.

13. Use of the hydrogen storage structure material composition according to claim 1, the hydrogen storage structure material according to claim 2, the hydrogen storage structure composite material according to claim 3, or the single hydrogen storage tube according to claim 4 in storing high-pressure hydrogen and / or liquid hydrogen.

Citation Information

Patent Citations

  • Oxidation resistance polyimide-Mg base composite hydrogen storage material and preparing method thereof

    CN110804705A

  • Special-shaped honeycomb type hydrogen high-pressure storage and transportation device and manufacturing method thereof

    CN110953477A

  • High pressure hydrogen storage bottle made of PBO fiber and carbon fiber mixed composite material and preparation method

    CN1948818A

  • Special-shaped honeycomb type hydrogen high-pressure storage and transportation device

    CN211146067U

  • Highly reductive base material compound of alumina, cerium oxide and zirconium oxide,production thereof and use thereofin catalyst manufacture

    JP1995315840A