Two-component solventless adhesive composition

JP7594856B2Active Publication Date: 2024-12-05ARKEMA FRANCE SA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019539942
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-01-27
Filing Date
2017-11-15
Publication Date
2024-12-05
Estimated Expiration
2037-11-15

Smart Images

  • Figure 0007594856000001
    Figure 0007594856000001
  • Figure 0007594856000002
    Figure 0007594856000002
  • Figure 0007594856000003
    Figure 0007594856000003
Patent Text Reader

Abstract

A two-component solventless polyurethane adhesive composition is disclosed. In some embodiments, the solventless adhesive composition includes an isocyanate component comprising an isocyanate. The solventless adhesive composition further includes an isocyanate-reactive component comprising a highly reactive amine-initiated polyol containing two or more primary hydroxyl groups and a backbone incorporating a tertiary amine. The isocyanate-reactive component further includes a phosphate ester polyol. The isocyanate-reactive component can further include one or more non-amine-initiated polyols. Also disclosed is a method for forming a laminate structure, including uniformly applying the isocyanate component to a first substrate, uniformly applying the isocyanate-reactive component to a second substrate, bringing the first and second substrates together, thereby mixing and reacting the isocyanate component and the isocyanate-reactive component to form an adhesive between the first and second substrates, and curing the adhesive to bond the first and second substrates. Also disclosed is a laminate including the adhesive composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 62 / 451,304, filed January 27, 2017.

[0002] The present disclosure relates to a solventless adhesive composition. More particularly, the present disclosure relates to a two-component solventless polyurethane adhesive composition for use in laminated structures. The disclosed adhesive composition includes an amine-initiated polyol and a phosphate ester polyol that have improved conversion efficiency and provide a laminated structure suitable for use in high performance food packaging applications (e.g., boil-in-bag applications).

[0003] In some embodiments, the adhesive composition is formulated to be highly reactive and thus applied to two substrates independently, and then the two substrates are brought together to mix and react the adhesive composition. In particular, one component of the adhesive composition is configured to be applied uniformly to the surface of the first substrate, and the other component of the adhesive composition is configured to be applied to the surface of the second substrate. The first and second substrates are then brought together, thereby mixing and reacting the two components to form an adhesive between the first substrate and the second substrate. In this manner, the adhesive can be cured, thereby bonding the first and second substrates. [Background technology]

[0004] Adhesive compositions are useful for a wide variety of purposes. For example, adhesive compositions are used to bond substrates such as polyethylene, polypropylene, polyester, polyamide, metal, paper, or cellophane together to form composite films, i.e., laminates. The use of adhesives in different end-use applications is commonly known. For example, adhesives can be used in the production of film / film and film / foil laminates used in the packaging industry, particularly for food packaging. Adhesives used in lamination applications, i.e., "lamination adhesives," can generally be classified into three categories: solvent-based, water-based, and solvent-free. The performance of the adhesives varies from category to category and from application to which the adhesive is applied.

[0005] Solventless lamination adhesives can be applied at up to 100 percent solids without either organic solvents or water-based carriers. Because no organic solvent or water needs to be dried from the adhesive during application, these adhesives can be run at high line speeds and are preferred in applications that require rapid adhesive application. Solvent- and water-based lamination adhesives are limited by the speed at which the solvent or water can be effectively dried and removed from the laminate structure after application of the adhesive. For environmental, health, and safety reasons, lamination adhesives are preferably water-based or solvent-free. However, solventless adhesives often encounter problems such as short pot life, poor initial adhesion, slow adhesion development, slow primary aromatic amine ("PAA") and isocyanate ("NCO") decay, poor adhesion to metal surfaces, and poor chemical and thermal resistance, especially in high performance applications such as boil-in-bag applications.

[0006] There are many types in the category of solventless lamination adhesives. One particular type includes premixed two-component polyurethane-based lamination adhesives. Typically, two-component polyurethane-based lamination adhesives include a first component that includes an isocyanate-containing prepolymer and / or polyisocyanate and a second component that includes a polyol. The prepolymer can be obtained by reaction of a polyether and / or polyester containing two or more hydroxyl groups per molecule with an excess of isocyanate. The second component includes polyethers and / or polyesters initiated with two or more hydroxyl groups per molecule. The two components are combined or "premixed" in a predetermined ratio and then applied to a first substrate ("carrier web"). The first substrate is then combined with a second substrate to form a laminate structure.

[0007] Additional substrate layers can be added to the structure, with additional layers of adhesive composition disposed between each successive substrate. The adhesive is then cured at room temperature or at an elevated temperature, thereby bonding the substrates together.

[0008] Further processing of the laminated structure depends on the cure rate of the adhesive. The cure rate of the adhesive is indicated by the time it takes for the mechanical bond between the laminated substrates to be sufficient to allow further processing and for the lamination process to comply with applicable regulations (e.g., food contact regulations). A slow cure rate reduces conversion efficiency. Premixed two-component solventless lamination adhesives exhibit weak initial bonds and slow cure rates compared to traditional solvent-containing adhesives. A general trend in the conversion industry is to cure lamination adhesives faster. Faster cure improves the operating efficiency of converters. Specifically, the rapid movement of finished products from the warehouse increases production capacity and flexibility to handle last minute orders (e.g., retail promotional campaigns). To improve operating efficiency, laminates should be formed using adhesive compositions that have much higher reactivity than existing adhesive compositions. However, such adhesive compositions may present challenges for traditional adhesive application techniques.

[0009] Therefore, a two-component solventless polyurethane-based laminating adhesive composition having improved bond strength, faster cure speed, and high performance application capabilities is desirable. Summary of the Invention

[0010] A two-component solventless polyurethane adhesive composition is disclosed. In some embodiments, the solventless adhesive composition includes an isocyanate component that includes an isocyanate. The solventless adhesive composition further includes an isocyanate-reactive component that includes a highly reactive amine-initiated polyol that includes a backbone incorporating two or more primary hydroxyl groups and a tertiary amine. The isocyanate-reactive component further includes a phosphate ester polyol. In some embodiments, the isocyanate can be selected from the group consisting of an aliphatic polyisocyanate, a cycloaliphatic polyisocyanate, an aromatic polyisocyanate, and combinations of two or more thereof. In some embodiments, the amine-initiated polyol can include a functionality of about 2 to about 12, a hydroxyl number of about 5 to about 1,830, and a molecular weight of about 200 to about 20,000. In some embodiments, the phosphate ester polyol is a reaction product of a polyol and polyphosphoric acid. The isocyanate-reactive component can further include one or more non-amine-initiated polyols.

[0011] The disclosed adhesive composition exhibits fast cure speed and improved performance compared to existing two-component solventless adhesive compositions. As a result, laminate structures containing the adhesive composition can be slit within just 2 hours after lamination and delivered to customers within 2 days. Laminates containing existing general-purpose adhesive compositions typically require 2-3 days from lamination for slitting and 5-7 days for delivery. Thus, process efficiency is significantly improved using the disclosed adhesive composition. Furthermore, the operating window of the disclosed adhesive composition is unclear compared to the 20-30 minute pot life of existing general-purpose adhesives. This is because the pot life of the disclosed adhesive composition is completely decoupled from the curing process, as explained below.

[0012] Because the disclosed adhesive compositions are formulated to be more reactive and exhibit faster cure rates than existing adhesive compositions, they are not ideally suited for use with existing adhesive application equipment. This is because the two components react so quickly that the adhesive gels and is incompatible with application to a substrate. For this reason, the disclosed adhesive compositions are formulated such that the isocyanate and isocyanate reactive components are applied separately onto two different substrates instead of being premixed and applied onto a carrier web.

[0013] In particular, the disclosed adhesive compositions are formulated such that an isocyanate component can be uniformly applied to a surface of a first substrate and an isocyanate-reactive component can be applied to a surface of a second substrate. The surface of the first substrate is then contacted with the surface of the second substrate to allow the two components to mix and react, thereby forming a laminate. The adhesive composition is then allowed to cure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The two-component solventless adhesive composition according to the present disclosure includes an isocyanate component and an isocyanate-reactive component.

[0015] Isocyanate component In some embodiments, the isocyanate component comprises an isocyanate. The isocyanate may be selected from the group consisting of monomeric isocyanate, polymeric isocyanate, prepolymeric isocyanate, and combinations of two or more thereof. As used herein, a prepolymeric isocyanate is a reaction product of a reactant comprising an isocyanate and a polyol, such as a polyester polyol. A "prepolymeric isocyanate" may be a polyisocyanate itself.

[0016] In some embodiments, the isocyanate comprises a functionality of 1.5 to 10, or 1.8 to 5, or 2 to 3. When used with respect to the isocyanate component, "functionality" refers to the number of hydroxyl reactive sites per molecule. Compounds having isocyanate groups, such as the isocyanate component, can be characterized by the parameter "NCO%", which is the amount of isocyanate groups by weight based on the weight of the compound. The parameter NCO% is measured by the method of ASTM D2572-97(2010). In some embodiments, the isocyanate component has an NCO% of at least 3% by weight, or at least 6% by weight, or at least 10% by weight. In some embodiments, the isocyanate component has an NCO% of not more than 25%, or 18%, or 14%.

[0017] In some embodiments, the isocyanate component comprises a free monomer content of 0-50%, or 5-40%, or 10-30%. In some embodiments, the isocyanate component comprises a molecular weight of 200-3,000 g / mol, or 300-2,000 g / mol, or 500-1,000 g / mol. In some embodiments, the isocyanate component has a viscosity of 300-40,000 mPa-s, or 500-20,000 mPa-s, or 1,000-10,000 mPa-s at 25° C., as measured by the method of ASTM D2196.

[0018] In some embodiments, the isocyanate of the isocyanate component may be selected from the group consisting of aliphatic polyisocyanates, cycloaliphatic polyisocyanates, aromatic polyisocyanates, and combinations of two or more thereof. "Aromatic polyisocyanates" are isocyanates that contain one or more aromatic rings. "Aliphatic polyisocyanates" do not contain aromatic rings. "Cycloaliphatic polyisocyanates" are a subset of aliphatic polyisocyanates in which the chemical chain has a cyclic structure.

[0019] Examples of isocyanates suitable for use according to the present disclosure include, but are not limited to, isomers of hexamethylene diisocyanate ("HDI"), isophorone diisocyanate ("IPDI"), isomers of xylylene diisocyanate ("XDI"), isomers of methylene diphenyl diisocyanate ("MDI"), such as 4,4-MDI, 2,2-MDI, and 2,4-MDI, isomers of toluene diisocyanate ("TDI"), such as 2,4-TDI, 2,6-TDI, isomers of naphthalene diisocyanate ("NDI"), such as 1,5-NDI, isomers of norbornane diisocyanate ("NBDI"), isomers of tetramethylxylylene diisocyanate ("TMXDI"), and combinations of two or more thereof. Isomers of MDI are preferred, in particular mixtures of 4,4-MDI and 2,4-MDI (ie liquid MDI), or 4,4-MDI (ie solid MDI).

[0020] In some embodiments, the amount of isocyanate in the isocyanate component is at least 40%, or at least 70%, or at least 90% by weight, based on the weight of the isocyanate component. In some embodiments, the amount of isocyanate in the isocyanate component is not more than 100%, or not more than 95%, or not more than 90% by weight, based on the weight of the isocyanate component. In some embodiments, the amount of isocyanate in the isocyanate component is between 40 and 100% by weight, based on the weight of the isocyanate component.

[0021] The isocyanate component can further include other components generally known to those skilled in the art.

[0022] Isocyanate-Reactive Components The solventless adhesive composition further comprises an isocyanate-reactive component comprising a highly reactive amine-initiated polyol. In some embodiments, the amine-initiated polyol comprises a primary hydroxyl group and a backbone incorporating at least one tertiary amine. In some embodiments, the isocyanate-reactive component may also comprise other types of polyols that are non-amine-initiated polyols. For example, the isocyanate-reactive component may comprise at least one selected from the group consisting of polyester polyols, polyether polyols, polycarbonate polyols, polyacrylate polyols, polycaprolactone polyols, polyolefin polyols, natural oil polyols, and combinations of two or more thereof. Each polyol type may comprise one type of polyol. Alternatively, each polyol type may comprise a mixture of different types of polyols. In some embodiments, one polyol type may be one type of polyol and the other polyol type may be a mixture of different types of polyols.

[0023] In some embodiments, the amine-initiated polyol comprises a primary hydroxyl group and a backbone incorporating at least one tertiary amine. In some embodiments, the amine-initiated polyol has the chemical structure I:

[0024] [ka]

[0025] In the formula, R 1 , R 2 , and R 3 are each independently a straight or branched chain alkyl group. For example, each can be independently a C1-C6 straight or branched chain alkyl group. In some embodiments, the amine-initiated polyol comprises a tertiary amine and a secondary amine.

[0026] In some embodiments, the amine-initiated polyol comprises a functionality of 2 to 12, or 3 to 10, or 4 to 8. When used in reference to the isocyanate-reactive component, "functionality" refers to the number of isocyanate-reactive sites per molecule. In some embodiments, the amine-initiated polyol comprises a hydroxyl number of 5 to 1,830, or 20 to 100, or 31 to 40. When used in reference to the isocyanate-reactive component, "hydroxyl number" is a measure of the amount of reactive hydroxyl groups available for reaction. This number is determined by wet analytical methods and is reported as the number of milligrams of potassium hydroxide equivalent to the hydroxyl groups found in one gram of sample. The most commonly used method for determining hydroxyl number is described in ASTM D4274D. In some embodiments, the amine-initiated polyol comprises a viscosity of 500 to 30,000 mPa-s, or 1,000 to 15,000 mPa-s, or 1,500 to 10,000 mPa-s at 25°C.

[0027] Amine-initiated polyols suitable for use in accordance with the present disclosure are made by alkoxylating one or more amine initiators with one or more alkylene oxides.

[0028] In some embodiments, the amount of amine-initiated polyol in the isocyanate-reactive component is at least 0.2 weight percent, or at least 1 weight percent, or at least 5 weight percent, based on the weight of the isocyanate-reactive component. In some embodiments, the amount of amine-initiated polyol in the isocyanate-reactive component is no more than 30 weight percent, or no more than 15 weight percent, or no more than 10 weight percent, based on the weight of the isocyanate-reactive component. In some embodiments, the amount of amine-initiated polyol in the isocyanate-reactive component is 0.2 to 30 weight percent, based on the weight of the isocyanate-reactive component.

[0029] In some embodiments, a non-amine-initiated polyol may be optionally included in the isocyanate-reactive component. Examples of suitable non-amine-initiated polyols include, but are not limited to, polyester polyols, polyether polyols, polycarbonate polyols, polyacrylate polyols, polycaprolactone polyols, polyolefin polyols, natural oil polyols, and combinations of two or more thereof. Preferably, the non-amine-initiated polyol has a viscosity of 30 to 40,000 mPa-s, or 50 to 30,000 mPa-s, or 70 to 20,000 mPa-s at 25°C, as measured by the method of ASTM D2196. Preferably, the non-amine-initiated polyol has a viscosity of 100 to 10,000 mPa-s at 25°C, as measured by the method of ASTM D2196. In some embodiments, the non-amine-initiated polyol is a solid at 25°C.

[0030] In some embodiments, the amount of non-amine-initiated polyol in the isocyanate-reactive component is at least 0 wt%, or at least 5 wt%, or at least 10 wt%. In some embodiments, the amount of non-amine-initiated polyol in the isocyanate-reactive component is no more than 98 wt%, or no more than 90 wt%, or no more than 70 wt%.

[0031] In some embodiments, the isocyanate-reactive component further comprises a phosphate ester polyol. In some embodiments, the phosphate ester polyol is made from a trifunctional propylene glycol, a polyphosphoric acid, and a polyisocyanate. Commercially available examples of trifunctional propylene glycols suitable for use according to the present disclosure include products sold under the trade names VORANOL™ CP-450, VORANOL™ CP-260, VORANOL™ CP-755, and VORANOL™ CP-1055, each available from Dow Chemical Company.

[0032] In some embodiments, the phosphate ester polyol has a phosphoric acid content of less than 4 weight percent based on the weight of the phosphate ester polyol, or a phosphoric acid content of 0 to 3 weight percent based on the weight of the phosphate ester polyol, or a phosphoric acid content of 1.5 to 2.5 weight percent based on the weight of the phosphate ester polyol. In some embodiments, the phosphate ester polyol has a viscosity of less than 40,000 cps at 25° C., or less than 30,000 cps at 25° C., as measured by the method of ASTM D2196. In some embodiments, the phosphate ester polyol has a hydroxyl equivalent weight of less than 330 g / mol. In some embodiments, the phosphate ester polyol has 0 to 100 weight percent of a trifunctional polyether polyol having an equivalent weight of less than 2,000 g / mol, based on the weight of the phosphate ester polyol.

[0033] The mix ratio by weight of the isocyanate component to the isocyanate-reactive component is controlled by adjusting the coating weight of each of the components on its respective substrate. In some embodiments, the mix ratio of the isocyanate component to the isocyanate-reactive component in the final adhesive composition can be 100:100, or 100:90, or 100:80. The disclosed adhesive composition is more forgiving than conventional adhesives and can accommodate some coating weight error (e.g., up to about 10% coating weight error).

[0034] In some embodiments, one or more additives may be optionally included in the adhesive composition. Examples of such additives include, but are not limited to, tackifiers, plasticizers, rheology modifiers, adhesion promoters, antioxidants, fillers, colorants, surfactants, defoamers, wetting agents, leveling agents, solvents, and combinations of two or more thereof.

[0035] The isocyanate-reactive component can further include other components commonly known to those skilled in the art, such as additional polyols, isocyanates, and the like.

[0036] Laminate formation It is contemplated that the isocyanate component and the isocyanate-reactive component of the disclosed solventless adhesive composition are compounded separately and desirably stored until it is time to form a laminate structure. Preferably, the isocyanate component and the isocyanate-reactive component are in a liquid state at 25° C. Even if the components are solid at 25° C., the components can be heated to a liquid state if necessary.

[0037] Laminates containing the disclosed adhesive compositions can be formed by applying the isocyanate and isocyanate-reactive components of the adhesive composition separately to two different substrates, such as two films. As used herein, a "film" is any structure with one dimension equal to or less than 0.5 mm and two other dimensions equal to or greater than 1 cm. A "polymer film" is a film made from a polymer or mixture of polymers. The composition of a polymer film is typically 80 weight percent or more of one or more polymers.

[0038] For example, a layer of an isocyanate component is applied to a surface of a first substrate. Preferably, the thickness of the layer of the isocyanate component on the first substrate is 0.5-2.5 μm. A layer of an isocyanate-reactive component is applied to a surface of a second substrate. Preferably, the thickness of the layer of the isocyanate-reactive component on the second substrate is 0.5-2.5 μm. By controlling the thickness of the layer applied to each substrate, the ratio of the components can be controlled.

[0039] The surfaces of the first and second substrates are then passed through a device for applying external pressure to the first and second substrates, such as a nip roller. When the isocyanate component and the isocyanate-reactive component are brought together, a curable adhesive mixture layer is formed. When the surfaces of the first and second substrates are brought together, the thickness of the curable adhesive mixture layer is 1-5 μm. When the first and second substrates are brought together and the components contact each other, the isocyanate component and the isocyanate-reactive component begin to mix and react. This marks the beginning of the curing process.

[0040] Further mixing and reaction is accomplished as the first and second substrates are passed through various other rollers and finally through an unwind roller. Further mixing and reaction occurs as the first and second substrates pass through the rollers, as each substrate takes a longer or shorter path across each roller than the other substrate. In this manner, the two substrates move relative to each other, mixing the components on the respective substrates. Such arrangements of rollers in coating devices are generally known in the art. The curable mixture is then cured or allowed to cure.

[0041] Suitable substrates for the laminate structure include paper, woven and nonwoven fabrics, metal foils, polymeric films, and films such as metallized polymeric films. Some films optionally have a surface that is printed with an image with an ink that can contact the adhesive composition. The substrates are laminated to form a laminate structure, with the adhesive composition according to the present disclosure adhering one or more substrates together.

[0043] Thus, including the disclosed amine-initiated polyols in the isocyanate-reactive component of the adhesive composition provides an adhesive composition with a significantly faster reactivity profile that is particularly suitable for lamination by the methods disclosed herein. EXAMPLES

[0044] The present disclosure will now be described in further detail by describing examples (collectively, "Examples") that illustrate the disclosed and existing adhesive compositions, although the scope of the present disclosure is, of course, not limited to the Examples.

[0045] Example isocyanate-reactive components are prepared using the ingredients specified in Table 1 below.

[0046] [Table 1]

[0047] The examples are prepared according to the formulations of the ingredients listed in Table 2 below, in weight percent.

[0048] [Table 2]

[0049] Illustrative Example 1 ("IE1")

[0050] [Table 3]

[0051] VORANOL™ CP450, VORANOL™ CP755, and ISONATE™ 125M are reacted in a reactor at 80° C. for 2 hours under nitrogen purge to form an OH-terminated polyether-based polyurethane. The synthesized polyether-based polyurethane is blended with SPECFLE™ ACTIV2306 and MOR-FREE™ 88-138 to form co-reactant 2D ("CR2D"). Detailed composition information of CR2D is listed in Table 3.

[0052] A polyurethane adhesive containing approximately 52.2% by weight Polyisocyanate A and 47.8% by weight CR2D is used to bond the foil / polyethylene ("PE") and polyethylene terephthalate ("PET") / PE structures. The resulting laminate is cured at 25°C and 50% relative humidity. The resulting laminate samples are cut into 15 mm wide strips and their T-peel bond strength is evaluated on a Thwing-Albert peel tester at 4 inches / minute. If one of the substrates is stretched or torn, the maximum force or force at break is recorded. If the two substrates are separated, the average force during the test is recorded. The bond strength value is the average of at least three sample strips.

[0053] After the adhesive is fully cured, a boil-in-bag test is performed on the foil / PE laminate. The pouch for the boil-in-bag test has an internal size of 4 inches by 6 inches and is filled with 100 ml of 1:1:1 sauce (i.e., equal parts of vinegar, corn oil, and ketchup). The pouch is then placed in boiling water for 30 minutes. Once complete, at least three 25.4 mm wide strips are cut from the area in contact with the boiling water and the bond strength of each strip is measured on a Thwing-Albert peel tester at 10 inches / minute.

[0054] Illustrative Example 2 ("IE2")

[0055] [Table 4]

[0056] VORANOL™ CP755 and ISONATE™ 125M are reacted in a reactor under nitrogen purge at 80° C. for 2 hours to form OH-terminated polyether-based polyurethane. The synthesized polyether-based polyurethane is blended with VORANOL™ CP450, SPECFLE™ ACTIV2306 and MOR-FREE™ 88-138 to form CR2F. The detailed composition information of CR2F is listed in Table 4.

[0057] A polyurethane adhesive containing approximately 52.6% by weight Polyisocyanate A and 47.4% by weight CR2F is used to bond the foil / PE and PET / PE structures. The resulting laminate is cured at 25°C and 50% relative humidity. The laminate samples are cut into 15 mm wide strips and their T-peel bond strength is evaluated on a Thwing-Albert peel tester at 4 in / min. If one of the substrates is stretched or torn, the maximum force or force at break is recorded. If the two substrates are separated, the average force during the test is recorded. The bond strength value is the average of at least three sample strips.

[0058] After the adhesive is fully cured, a boil-in-bag test is performed on the foil / PE laminate. The pouch for the boil-in-bag test has an internal size of 4 inches by 6 inches and is filled with 100 ml of 1:1:1 sauce (i.e., equal parts of vinegar, corn oil, and ketchup). The pouch is then placed in boiling water for 30 minutes. Once complete, at least three 25.4 mm wide strips are cut from the area in contact with the boiling water and the bond strength of each strip is measured on a Thwing-Albert peel tester at 10 inches / minute.

[0059] Comparative example 1 (“CE1”) A polyurethane adhesive containing approximately 52.6% by weight MOR-FREE™ L-PLUS and 47.4% by weight CR121-14 is used to bond the foil / PE and PET / PE structures. The produced laminate is cured at 25° C. and 50% relative humidity. The laminate samples are cut into 15 mm wide strips and their T-peel bond strength is evaluated on a Thwing-Albert peel tester at 4 in / min. If one of the substrates stretches or tears, the maximum force or force at break is recorded. If the two substrates are separated, the average force during the test is recorded. The bond strength value is the average of at least three sample strips.

[0060] After the adhesive is fully cured, a boil-in-bag test is performed on the foil / PE laminate. The pouch for the boil-in-bag test has an internal size of 4 inches by 6 inches and is filled with 100 ml of 1:1:1 sauce (i.e., equal parts of vinegar, corn oil, and ketchup). The pouch is then placed in boiling water for 30 minutes. Once complete, at least three 25.4 mm wide strips are cut from the area in contact with the boiling water and the bond strength of each strip is measured on a Thwing-Albert peel tester at 10 inches / minute.

[0061] Comparative Example 2

[0062] [Table 5]

[0063] VORANOL™ CP450, VORANOL™ CP755, and ISONATE™ 125M are reacted in a reactor under nitrogen purge at 80° C. for 2 hours to form an OH-terminated polyether-based polyurethane. The synthesized polyether-based polyurethane is blended with SPECFLE™ ACTIV2306 to form CR2E. The detailed composition information of CR2E is listed in Table 5.

[0064] A polyurethane adhesive containing approximately 50.5% by weight Polyisocyanate A and 49.5% by weight CR2E is used to bond the foil / PE and PET / PE structures. The resulting laminate is cured at 25°C and 50% relative humidity. The laminate samples are cut into 15 mm wide strips and their T-peel bond strength is evaluated on a Thwing-Albert peel tester at 4 in / min. If one of the substrates is stretched or torn, the maximum force or force at break is recorded. If the two substrates are separated, the average force during the test is recorded. The bond strength value is the average of at least three sample strips.

[0065] After the adhesive is fully cured, a boil-in-bag test is performed on the foil / PE laminate. The pouches for the boil-in-bag test have an internal size of 4 inches by 6 inches and are filled with 100 ml of 1:1:1 sauce (i.e., equal amounts of vinegar, corn oil, and ketchup). They are then placed in boiling water for 30 minutes. Once complete, at least three 25.4 mm wide strips are cut from the area in contact with the boiling water and the bond strength of each strip is measured on a Thwing-Albert peel tester at 10 inches / minute.

[0066] Comparative Example 3

[0067] [Table 6]

[0068] VORANOL™ CP450, VORANOL™ CP755, and ISONATE™ 125M are reacted in a reactor under nitrogen purge at 80° C. for 2 hours to form an OH-terminated polyether-based polyurethane. The synthesized polyether-based polyurethane is blended with SPECFLE™ ACTIV2306 to form CR2C. The detailed composition information of CR2C is listed in Table 6.

[0069] A polyurethane adhesive containing approximately 49.5% by weight Polyisocyanate A and 50.5% by weight CR2C is used to bond the foil / PE and PET / PE structures. The resulting laminate is cured at 25°C and 50% relative humidity. The laminate samples are cut into 15mm wide strips and their T-peel bond strength is evaluated on a Thwing-Albert peel tester at 4 inches / min. If one of the substrates is stretched or torn, the maximum force or force at break is recorded. If the two substrates are separated, the average force during the test is recorded. The bond strength value is the average of at least three sample strips.

[0070] After the adhesive is fully cured, a boil-in-bag test is performed on the foil / PE laminate. The pouches for the boil-in-bag test have an internal size of 4 inches by 6 inches and are filled with 100 ml of 1:1:1 sauce (i.e., equal amounts of vinegar, corn oil, and ketchup). They are then placed in boiling water for 30 minutes. Once complete, at least three 25.4 mm wide strips are cut from the area in contact with the boiling water and the bond strength of each strip is measured on a Thwing-Albert peel tester at 10 inches / minute.

[0071] performance results

[0072] [Table 7]

[0073] [Table 8]

[0074] [Table 9]

[0075] Tables 7 and 8 show that IE1 and IE2 have ultra-fast cure and bond strength development. For example, both IE1 and IE2 have bond strengths of over 1N / 15mm after 2 hours cure. IE1 and IE2 show high dry bond after 24 hours cure compared to CE1-CE3. As shown in Table 9, after 1:1:1 boil-in-bag test, all laminates from CE1 to CE3 delaminated. In contrast, IE1 and IE2 still have bond strengths of about 383 and 386g / inch, respectively, indicating excellent temperature and chemical resistance.

Claims

1. 1. A two-component solventless adhesive composition comprising: an isocyanate component including an isocyanate; an isocyanate-reactive component, the isocyanate-reactive component comprising: an amine-initiated polyol comprising two or more primary hydroxyl groups and a backbone incorporating a tertiary amine; and a phosphate ester polyol.

2. 2. The two-component solventless adhesive composition of claim 1, wherein the amine-initiated polyol comprises a functionality of 2 to 12, a hydroxyl number of 5 to 1,830, and a viscosity of 500 to 30,000 mPa-s at 25°C.

3. The two-component solventless adhesive composition of claim 1, wherein the amine-initiated polyol comprises 0.5 to 30 weight percent of the isocyanate-reactive component, based on the total weight of the isocyanate-reactive component.

4. The amine-initiated polyol has structure I: 【Chemistry 1】 In the formula, R 1 , R 2 , and R 3 2. The two-component solventless adhesive composition of claim 1, wherein is independently a straight or branched chain alkyl group.

5. 2. The two-component solventless adhesive composition of claim 1, wherein the phosphate ester polyol comprises 0.2 to 30 weight percent of the isocyanate-reactive component, based on the total weight of the isocyanate-reactive component.

6. 2. The two-component solventless adhesive composition of claim 1, wherein the phosphate ester polyol is made from a trifunctional propylene glycol, a polyphosphoric acid, and a polyisocyanate, the phosphate ester polyol having a phosphoric acid content of less than 3 weight percent, based on the weight of the phosphate ester polyol, and a viscosity of less than 40,000 cps at 25°C.

7. The two-component solventless adhesive composition of claim 1 further comprising an adhesion promoter.

8. 8. The two-component solventless adhesive composition of claim 7, wherein the adhesion promoter is selected from the group consisting of coupling agents, epoxy resins, phosphoric acids, polyphosphoric acids, phosphate esters, and combinations of two or more thereof.

9. A laminate structure comprising the two-component solventless adhesive composition of claim 1.

10. 1. A method for forming a laminate structure, comprising: applying an isocyanate component uniformly to a first substrate, the isocyanate component comprising an isocyanate; uniformly applying an isocyanate-reactive component to a second substrate, the isocyanate-reactive component comprising: an amine-initiated polyol comprising primary hydroxyl groups and a backbone incorporating a tertiary amine; a phosphate ester polyol; contacting the first and second substrates, thereby causing the isocyanate component and the isocyanate-reactive component to mix and react to form an adhesive between the first and second substrates; and curing the adhesive to bond the first and second substrates.

Citation Information

Patent Citations

  • Production of compound vibration-damping material

    JP1988278988A

  • Adhesive composition and preparation of decorative sheet-covered material

    JP1999035917A

  • Adhesive composition for plastic film-laminated metallic plate

    JP2007169548A

  • Two-component polyurethane adhesive for bonding fiber-containing molded products.

    JP2011509316A

  • Phosphate adhesion promoters

    WO2015168670A1