Positive electrode active material for lithium-ion secondary batteries
The use of specific particle compositions in the positive electrode active material stabilizes the crystal structure and suppresses metal elution, enhancing both rate and cycle characteristics in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2020205252
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-10
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing lithium ion secondary batteries using layered lithium composite oxides face challenges in maintaining high rate characteristics and cycle characteristics due to the elution of transition metal components into the electrolyte, which affects crystal structure stability and safety, especially at elevated temperatures.
A positive electrode active material comprising specific particles represented by formulas (A), (B), and (C) in defined proportions, including Li Ni a Co b Mn c M 1 O 2, Li f Mn g Fe h M 2 P.O. 4, and LiM 3 y Mn j O 4, which stabilize the crystal structure and suppress metal component elution, enhancing both rate and cycle characteristics.
The proposed active material significantly improves both rate and cycle characteristics of lithium ion secondary batteries by preventing metal component elution and maintaining structural integrity, thereby ensuring better performance and safety.
Smart Images

Figure 0007594898000002 
Figure 0007594898000003 
Figure 0007594898000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery, for obtaining a lithium ion secondary battery having excellent rate characteristics and cycle characteristics. [Background technology]
[0002] Layered lithium composite oxides, such as layered lithium-nickel-cobalt-manganese composite oxide (NMC), have a layered crystal structure in which lithium atomic layers and transition metal atomic layers are alternately stacked with oxygen atomic layers in between. Such layered lithium composite oxides are used as positive electrode active materials in high-power and high-capacity lithium-ion secondary batteries.
[0003] In lithium-ion secondary batteries that use such layered lithium composite oxides as the positive electrode active material, charging and discharging are performed by the desorption and insertion of lithium ions into the layered lithium composite oxide. However, the capacity decreases with the number of charge-discharge cycles, and this decrease in battery capacity can become particularly severe over long-term use. This is thought to be due to the leaching of transition metal components of the lithium composite oxide into the electrolyte during charging, which makes the crystalline structure more susceptible to collapse. The amount of transition metal leaching increases particularly at higher temperatures, significantly affecting cycle performance. Furthermore, if the crystalline structure of the lithium composite oxide collapses, the transition metal components of the lithium composite oxide may leach into the surrounding electrolyte, reducing thermal stability and potentially compromising safety.
[0004] Under these circumstances, various developments have been made using highly useful layered lithium composite oxides. For example, Patent Document 1 discloses a positive electrode for a secondary battery containing a lithium-nickel-cobalt-manganese composite oxide with a specific number of cobalt atoms and a lithium iron manganese phosphate with a specific number of manganese atoms, in order to obtain a secondary battery with excellent energy density, thereby improving initial coulombic efficiency. Furthermore, Patent Document 2 discloses a positive electrode active material for a secondary battery containing a lithium-nickel-manganese-cobalt composite oxide, a lithium composite oxide, and a lithium-manganese composite oxide, in an attempt to improve safety, cycle characteristics, etc. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2011-159388 [Patent Document 2] International Publication No. 2016 / 163282 Summary of the Invention [Problem to be solved by the invention]
[0006] However, even with the technology described in Patent Document 1, it is not certain whether the rate characteristics and cycle characteristics can be sufficiently improved, and even with the technology described in Patent Document 2, sufficient consideration has not been given to improving the rate characteristics, and there is still room for improvement in order to achieve both high rate characteristics and excellent cycle characteristics.
[0007] Therefore, an object of the present invention is to provide a positive electrode active material for a lithium ion secondary battery that can sufficiently improve both the rate characteristics and the cycle characteristics. [Means for solving the problem]
[0008] Therefore, as a result of intensive studies to solve the above problems, the present inventors have found a positive electrode active material for a lithium ion secondary battery that can achieve both high rate characteristics and excellent cycle characteristics in the obtained lithium ion secondary battery by containing specific particles represented by a specific formula in specific amounts respectively.
[0009] That is, the present invention relates to the following components (A), (B), and (C): (A) 55% to 90% by mass of particles represented by the following formula (a) LiNi a Co b Mn c M 1 w O2···(a) (In formula (a), M 1 represents one or more elements selected from Mg, Ti, Nb, Fe, Cr, Si, Al, Ga, V, Zn, Cu, Sr, Mo, Zr, Sn, Ta, W, La, Ce, Pb, Bi, and Ge. a, b, c, w are numbers satisfying 0.3 ≤ a < 1, 0 < b ≤ 0.7, 0 < c ≤ 0.7, 0 ≤ w ≤ 0.3, and 3a + 3b + 3c + (valence of M 1 ) × w = 3. ) (B) 5% to 40% by mass of particles represented by the following formula (b) and having an average particle diameter of 12 μm to 25 μm Li f Mn g Fe h M 2 x PO4···(b) (In formula (b), M 2 represents one or more elements selected from Mg, Al, Ti, Cu, Zn, Nb, Co, Ni, Ca, Sr, Y, Zr, Mo, Ba, Pb, Bi, La, Ce, Nd, and Gd. f, g, h, and x are numbers satisfying 0 < f ≤ 1.2, 0.3 ≤ g ≤ 1.2, 0.2 ≤ h ≤ 1.2, 0 ≤ x ≤ 0.3, and 3 / 7 ≤ g / h ≤ 4, and f + (valence of Mn) × g + (valence of Fe) × h + (valence of M 2 ) × x = 3. ) (C) 1% to 10% by mass of particles represented by the following formula (c) LiM 3y Mn j O4···(c) (In formula (c), M 3 represents one or more elements selected from Ni, Co, Al, Mg, Ti, V, Cr, Fe, Zr, Ga, Cu, and Si. y and j are such that 0 ≦ y ≦ 0.1, 0 < j ≦ 2, and (valence of M 3 × y + (valence of Mn) × j = 7).) Disclosed is a positive electrode active material for a lithium ion secondary battery containing the same.)
Advantages of the Invention
[0010] According to the positive electrode active material for a lithium ion secondary battery of the present invention, a lithium ion secondary battery that exhibits excellent rate characteristics and also has excellent cycle characteristics can be realized.)
Brief Description of the Drawings
[0011] [Figure 1] SEM image showing a part of the particles (B1) obtained in Production Example 2.) [Figure 2] Distribution diagram obtained in the measurement of pore distribution of the particles (B1) obtained in Production Example 2 by mercury intrusion porosimetry.)
Modes for Carrying Out the Invention
[0012] Hereinafter, the present invention will be described in detail.) The positive electrode active material for a lithium ion secondary battery of the present invention comprises the following components (A), (B), and (C): (A) 55% to 90% by mass of particles represented by the following formula (a) LiNi a Co b Mn c M 1 w O2···(a) (In formula (a), M 1represents one or more elements selected from Mg, Ti, Nb, Fe, Cr, Si, Al, Ga, V, Zn, Cu, Sr, Mo, Zr, Sn, Ta, W, La, Ce, Pb, Bi, and Ge. a, b, c, and w are numbers satisfying 0.3 ≤ a < 1, 0 < b ≤ 0.7, 0 < c ≤ 0.7, 0 ≤ w ≤ 0.3, and 3a + 3b + 3c + (valence of M 1 × w = 3.) (B) 5% to 40% by mass of particles represented by the following formula (b) and having an average particle size of 12 μm to 25 μm Li f Mn g Fe h M 2 x PO4 ··· (b) (In formula (b), M 2 represents one or more elements selected from Mg, Al, Ti, Cu, Zn, Nb, Co, Ni, Ca, Sr, Y, Zr, Mo, Ba, Pb, Bi, La, Ce, Nd, and Gd. f, g, h, and x are numbers satisfying 0 < f ≤ 1.2, 0.3 ≤ g ≤ 1.2, 0.2 ≤ h ≤ 1.2, 0 ≤ x ≤ 0.3, and 3 / 7 ≤ g / h ≤ 4, and f + (valence of Mn) × g + (valence of Fe) × h + (valence of M 2 × x = 3.) (C) 1% to 10% by mass of particles represented by the following formula (c) LiM 3 y Mn j O4 ··· (c) (In formula (c), M 3 represents one or more elements selected from Ni, Co, Al, Mg, Ti, V, Cr, Fe, Zr, Ga, Cu, and Si. y and j are numbers satisfying 0 ≤ y ≤ 0.1, 0 < j ≤ 2, and (valence of M 3 × y + (valence of Mn) × j = 7.) contains.
[0013] As described above, the positive electrode active material for a lithium ion secondary battery of the present invention contains specific amounts of each of the three specific types of particles represented by the above specific formulas, which promotes carbon contact within the electrode, makes it easier to ensure a conductive path, and effectively suppresses the elution of metal components from the particles, thereby effectively improving both the rate characteristics and cycle characteristics of the resulting lithium ion secondary battery.
[0014] The positive electrode active material for a lithium ion secondary battery of the present invention contains, as component (A), 55% by mass to 90% by mass of particles represented by the following formula (a): LiNi a Co b Mn c M 1 w O2 (a) (In formula (a), M 1 represents one or more elements selected from Mg, Ti, Nb, Fe, Cr, Si, Al, Ga, V, Zn, Cu, Sr, Mo, Zr, Sn, Ta, W, La, Ce, Pb, Bi, and Ge. a, b, c, and w are within the range of 0.3≦a<1, 0 <b≦0.7、0<c≦0.7、0≦w≦0.3、かつ3a+3b+3c+(M 1 The number satisfies (valence of x) × w = 3.
[0015] The particles of component (A) represented by the above formula (a) are lithium composite oxide particles (so-called Li-Ni-Co-Mn oxide particles (NCM particles), hereinafter also referred to as "particles (A)"), which have a layered rock salt structure and are secondary particles formed by aggregation of primary particles. By containing such component (A) in the above amount, good rate characteristics can be maintained, and in combination with component (B) described below, it can contribute to improving cycle characteristics.
[0016] M in formula (a) 1 represents one or more elements selected from Mg, Ti, Nb, Fe, Cr, Si, Al, Ga, V, Zn, Cu, Sr, Mo, Zr, Sn, Ta, W, La, Ce, Pb, Bi, and Ge. In addition, a, b, c, and w in the above formula (a) are 0.3≦a<1, 0 <b≦0.7、0<c≦0.7、0≦w≦0.3、かつ3a+3b+3c+(M 1 It is a number that satisfies (valence of x) × w = 3.
[0017] In the particles (A) represented by the formula (a), Ni, Co, and Mn are known to have excellent electronic conductivity and contribute to the battery capacity and output characteristics. From the viewpoint of cycle characteristics, it is also known that some of these transition elements are mixed with other metal elements M 1 It is preferable that these metal elements M 1 It is considered that the substitution by stabilizes the crystal structure of the particles (A) represented by formula (a), so that destruction of the crystal structure can be suppressed even when charge and discharge are repeated, and excellent cycle characteristics can be realized.
[0018] Specific examples of the NCM particles represented by the formula (a) include LiNi 0.33 Co 0.33 Mn 0.34 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.2 Co 0.4 Mn 0.4 O2, LiNi 0.33 Co 0.31 Mn 0.33 Mg 0.03 O2 or LiNi 0.33 Co 0.31 Mn 0.33 Zn 0.03 O2, etc. Among them, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.33 Co 0.33 Mn 0.34 O2, LiNi 0.33 Co 0.31 Mn 0.33 Mg 0.03Particles made of O2 are preferred.
[0019] Furthermore, two or more types of particles (A) represented by the above formula (a) having different compositions may form a core-shell structure having a core (interior) and a shell (surface). By forming particles (A) having this core-shell structure, NCM-based composite oxide particles with a high Ni concentration, which are likely to dissolve in the electrolyte, can be arranged in the core, while NCM-based composite oxide particles with a low Ni concentration can be arranged in the shell, which is in contact with the electrolyte. This can further suppress deterioration of cycle performance and ensure safety. In this case, the core may be composed of a single phase or two or more phases with different compositions. In an embodiment where the core is composed of two or more phases, the core may have a structure in which multiple phases are concentrically layered, or a structure in which the composition changes gradually from the surface to the center of the core. Furthermore, the shell portion may be formed on the outside of the core portion, and may be a single phase like the core portion, or may be composed of two or more phases with different compositions.
[0020] As the particle (A) having a core-shell structure formed by two or more kinds of NCM particles with different compositions, specifically, (core portion)-(shell portion) is, for example, (LiNi 0.8 Co 0.1 Mn 0.1 O2)-(LiNi 0.2 Co 0.4 Mn 0.4 O2), (LiNi 0.8 Co 0.1 Mn 0.1 O2)-(LiNi 0.33 Co 0.33 Mn 0.34 O2), or (LiNi 0.8 Co 0.1 Mn 0.1 O2)-(LiNi 0.33 Co 0.31 Mn 0.33 Mg 0.03 Examples include particles consisting of O2.
[0021] Furthermore, the particles (A) represented by the formula (a) may be coated with a metal oxide, a metal fluoride, or a metal phosphate. By coating the NCM particles with these metal oxides, metal fluorides, or metal phosphates, the metal components (Ni, Mn, Co, Mn) from the NCM particles can be easily transferred to the electrolyte. 1 As such a coating, one or more materials selected from CeO2, SiO2, MgO, Al2O3, ZrO2, TiO2, ZnO, RuO2, SnO2, CoO, Nb2O5, CuO, V2O5, MoO3, La2O3, WO3, AlF3, NiF2, MgF2, LiF, Li3PO4, Li4P2O7, LiPO3, Li2PO3F, and LiPO2F2, or a composite thereof, can be used.
[0022] The average particle size of the primary particles of the particles (A) represented by the formula (a) is preferably 50 nm to 500 nm, more preferably 50 nm to 300 nm, from the viewpoints of being able to suppress the amount of expansion and contraction of the primary particles accompanying the insertion and desorption of lithium ions, effectively preventing particle cracking, and handling. Here, the "average particle size as primary particles" of the particles (A) means the crystallite size measured by X-ray diffraction. Furthermore, the average particle size of the particles (A), which are secondary particles formed by aggregation of the primary particles (simply referred to as "average particle size of particles (A)") is preferably 5 μm to 15 μm, more preferably 8 μm to 12 μm, from the viewpoint of obtaining a battery with excellent cycle characteristics and from the viewpoint of handling. Here, the "average particle size" of the particles (A) is the D obtained from the volume-based particle size distribution based on the laser diffraction / scattering method. 50 The values are the particle diameters (median diameters) at 50% of the cumulative particle size.
[0023] From the viewpoint of effectively achieving both high rate characteristics and excellent cycle characteristics, the content of component (A) (particles (A)) in the positive electrode active material for a lithium ion secondary battery of the present invention is 55% by mass to 90% by mass, preferably 60% by mass to 80% by mass, and more preferably 65% by mass to 70% by mass.
[0024] The particles (A) can be obtained, for example, by the following production method. Specifically, the production method includes a step (Ia) of preparing slurry water a by adding a nickel compound, a cobalt compound, a manganese compound, and water, and then filtering and drying the slurry water a to obtain mixture A; and a step (IIa) of adding a lithium compound to the obtained mixture A, mixing them, and then firing them.
[0025] Examples of the nickel compound used in step (Ia) include nickel sulfate, nickel acetate, etc., which may be used alone or in combination of two or more. Among these, nickel sulfate is preferred from the viewpoint of improving battery characteristics. Examples of the cobalt compound include cobalt acetate, cobalt nitrate, and cobalt sulfate. These may be used alone or in combination of two or more. Among these, cobalt sulfate is preferred from the viewpoint of improving battery characteristics. Examples of manganese compounds include manganese acetate, manganese nitrate, and manganese sulfate. These may be used alone or in combination of two or more. Among these, manganese sulfate is preferred from the viewpoint of improving battery characteristics. In addition to these nickel compounds, cobalt compounds, and manganese compounds, metals other than these compounds (M 1 ) compounds may also be used. Examples of lithium compounds include hydroxides (e.g., LiOH·H2O, LiOH), carbonates, sulfates, and acetates. Of these, carbonates are preferred.
[0026] In the step (Ia), when obtaining the slurry water a, it is preferable to adjust the pH to 8 to 13, for example, by adding aqueous ammonia dropwise.
[0027] In step (IIa), when firing, first perform preliminary firing at 500°C to 1000°C, preferably 600°C to 900°C for 1 hour to 15 hours, preferably 1 hour to 6 hours, and then perform main firing at 500°C to 1000°C, preferably 600°C to 900°C for 1 hour to 15 hours, preferably 5 hours to 13 hours. It is also preferable to perform crushing after preliminary firing and then subject it to main firing.
[0028] The positive electrode active material for a lithium ion secondary battery of the present invention contains, as component (B), particles represented by the following formula (b) and having an average particle diameter of 12 μm to 25 μm in an amount of 5 mass% to 40 mass%. Li f Mn g Fe h M 2 x PO4···(b) (In formula (b), M 2 represents one or more elements selected from Mg, Al, Ti, Cu, Zn, Nb, Co, Ni, Ca, Sr, Y, Zr, Mo, Ba, Pb, Bi, La, Ce, Nd, and Gd. f, g, h, and x satisfy 0 < f ≤ 1.2, 0.3 ≤ g ≤ 1.2, 0.2 ≤ h ≤ 1.2, 0 ≤ x ≤ 0.3, and 3 / 7 ≤ g / h ≤ 4, and f + (valence of Mn) × g + (valence of Fe) × h + (valence of M 2 ) × x = 3. )
[0029] The particles represented by the above formula (b) of component (B) are olivine-type lithium transition metal phosphate compounds containing at least both manganese (Mn) and iron (Fe) as transition metals (so-called LMFP particles, hereinafter also referred to as "particles (B)"), and are secondary particles formed by aggregation of primary particles. Such component (B) is also a factor that the particles are relatively more likely to deform than other components, and by containing it in the above amount, while maintaining good rate characteristics, in combination with the above component (A), it contributes to the improvement of cycle characteristics, and in particular, can effectively suppress the elution of metal components from component (C) described later.
[0030] For the particles (B), from the viewpoint of the average discharge voltage, f is preferably 0.6≦f≦1.2, more preferably 0.65≦f≦1.15, and even more preferably 0.7≦f≦1.1. g is preferably 0.4≦g≦0.8, more preferably 0.5≦g≦0.8, and even more preferably 0.7≦g≦0.8. h is preferably 0.2≦h≦0.6, more preferably 0.2≦h≦0.5, and even more preferably 0.2≦h≦0.3. x is preferably 0≦x≦0.2, more preferably 0≦x≦0.15, and even more preferably 0≦x≦0.1. g / h is the molar ratio of Mn and Fe constituting the so-called particles (B), and is preferably 2 / 3≦g / h≦4, more preferably 1≦g / h≦4, and even more preferably 3 / 2≦g / h≦4.
[0031] Specifically, for example, LiMn 0.3 Fe 0.7 PO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.9 Fe 0.1 PO4, LiMn 0.8 Fe 0.2 PO4, LiMn 0.75 Fe 0.15 Mg 0.1 PO4, LiMn 0.75 Fe 0.19 Zr 0.03 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, Li 1.2 Mn 0.63 Fe 0.27 PO4, Li 0.6 Mn 0.84 Fe 0.36 PO4, etc. Among them, LiMn 0.3 Fe 0.7 PO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.8 Fe 0.2 PO4, LiMn 0.6 Fe 0.4 PO4, Li 1.2 Mn 0.63 Fe 0.27PO4 or Li 0.6 Mn 0.84 Fe 0.36 PO4 is preferred.
[0032] From the viewpoint of effectively improving both the rate characteristics and the cycle characteristics, the particles (B) represented by the above formula (b) are preferably particles that are easily deformed, i.e., particles that exhibit the physical property of being easily crushed. Specifically, the particles (B) are a particle aggregate including particles each having one to two depressions formed on the surface, and the particles (B) as a whole have a mode of depression diameter of 1.0 μm to 4.0 μm, a depression volume of 0.2 mL / g to 0.8 mL / g, and a compaction degree of 2.5 g / cm under a load of 20 kN, as measured by mercury intrusion porosimetry. 3 ~3.3g / cm 3 That is, it is desirable that the particles (B) contain, as some of the particles constituting the particles, particles having one to two large depressions on their surfaces, and that the particle aggregate as a whole exhibits the above-mentioned high mode of depression diameter and depression volume as measured by mercury intrusion porosimetry, and have an appropriate strength that allows for easy deformation to avoid collapse while also suppressing excessive pulverization.
[0033] The "depressions" formed on the surfaces of some particles included in particles (B) refer to depressions in the particle surface that deviate from the hypothetical surface, assuming that the entire particle is a sphere and the surface of the sphere is a hypothetical surface, and are recessed toward the interior of the particle. Such "depressions" are large enough to be recognized, for example, in an SEM photograph. Furthermore, the "indentation diameter" refers to the diameter of a perfect circle when the circle drawn by connecting the points where the deviation of the particle surface from the virtual surface begins is considered to be a perfect circle, and the "mode of indentation diameter" corresponds to the average value of the "indentation diameters" and is a value that serves as an index for recognizing the size of the "indentations." In the present invention, the so-called pore diameter measured by mercury intrusion porosimetry for the entire particle (B) is defined as the "indentation diameter," and the peak value obtained from a pore diameter distribution diagram is defined as the "mode of indentation diameter." Furthermore, the "cavity volume" is the volume occupied by the "cavities" and is synonymous with the value obtained by subtracting the volume of the particle having the cavities from the volume of the assumed sphere. In the present invention, the "cavity volume" is defined as the peak area in a pore size distribution diagram measured by mercury intrusion porosimetry for the entire particle (B).
[0034] By forming a positive electrode active material for a lithium ion secondary battery containing such particles (B) together with the above particles (A) and particles (C) described below under specified conditions, it is possible to promote carbon contact within the electrode and ensure the establishment of a conductive path, while suppressing the elution of metal components from the particles, making it even more possible to achieve both good rate characteristics and good cycle characteristics in the lithium ion secondary battery.
[0035] The mode of the pit diameter in the particles (B) measured by mercury intrusion porosimetry is 1.0 μm to 4.0 μm, preferably 1.0 μm to 3.0 μm, and more preferably 1.0 μm to 2.5 μm. The void volume of the particles (B) measured by mercury intrusion porosimetry (void volume per 1 g of particles (B)) is 0.2 mL / g to 0.8 mL / g, preferably 0.25 mL / g to 0.8 mL / g, and more preferably 0.3 mL / g to 0.8 mL / g.
[0036] The particles (B) can be easily compacted to exhibit a high degree of compaction, and therefore the degree of compaction under a load of 20 kN is 2.5 g / cm 3 ~3.3g / cm 3 and preferably 2.7 g / cm 3 ~3.3g / cm 3 and more preferably 2.9 g / cm 3 ~3.3g / cm 3 is.
[0037] The tap density of the particles (B) is preferably 0.7 g / cm3, from the viewpoint that some of the particles constituting the particles (B) are large particles having large depressions on the surface. 3 ~1.1g / cm 3 and more preferably 0.7 g / cm 3~1.0g / cm 3 and more preferably 0.7 g / cm 3 ~0.9g / cm 3 is. The tap density means the "tap bulk density" measured by the method specified in JIS R 1628 "Method for measuring bulk density of fine ceramic powders."
[0038] In particles (B), the proportion of particles having one to two depressions formed on the surface exhibits the mode of depression diameter and depression volume as described above, and from the viewpoint of imparting a high degree of compaction that allows for easy compaction, is preferably 30% to 100%, more preferably 55% to 100%, and even more preferably 70% to 100% of the total number of particles (B) of particles (B). The percentage of particles (B) having one to two depressions on their surface can be determined by observing the particles with an electron microscope and calculating the value (%) of {(number of particles having one to two depressions with a diameter of 1.0 μm or more on their surface) / (total number of particles with a diameter of 5.0 μm or more)}×100.
[0039] The average particle size of the primary particles of the particles (B) represented by the formula (b) is preferably 50 nm to 250 nm, more preferably 100 nm to 200 nm, from the viewpoints of suppressing the amount of expansion and contraction of the primary particles accompanying the insertion and desorption of lithium ions, effectively preventing particle cracking, and ease of handling. Here, the "average particle size as primary particles" of the particles (B) means the crystallite size measured by X-ray diffraction. Furthermore, the average particle size of particles (B), which are secondary particles formed by aggregation of the primary particles (simply referred to as "average particle size of particles (B)"), is 12 μm to 25 μm, preferably 12 μm to 20 μm, and more preferably 12 μm to 18 μm, from the viewpoint of obtaining a battery with excellent cycle characteristics and from the viewpoint of handling. Here, the "average particle size" of particles (B) is the D obtained from the volume-based particle size distribution based on the laser diffraction / scattering method. 50The values are the particle diameters (median diameters) at 50% of the cumulative particle size. It should be noted that particles having one or two depressions formed on the surface are also so-called secondary particles formed by aggregation of the above primary particles.
[0040] From the viewpoint of ensuring an excellent discharge capacity, the particles (B) may be particles having carbon derived from cellulose nanofibers and / or carbon derived from a water-soluble carbon material supported on the surface of the particles. Cellulose nanofibers are the skeletal component that accounts for approximately 50% of all plant cell walls. They are lightweight, high-strength fibers that can be obtained by defibrating the plant fibers that make up these cell walls to nano-size. The fiber diameter of these cellulose nanofibers is 1 nm to 1,000 nm, and they also have good dispersibility in water. Furthermore, the cellulose molecular chains that make up the cellulose nanofibers form a periodic structure of carbon. Therefore, when these cellulose nanofibers are carbonized to form carbon, and this carbon is firmly supported on the surface of the particles (B), the particles (B) exhibit crushable properties, yet have an appropriate strength that allows them to easily deform and avoid collapse while also suppressing excessive pulverization. This effectively suppresses the deterioration of the electronic conductive path, effectively increases the degree of compaction, and ensures that the resulting battery exhibits excellent discharge capacity.
[0041] When carbon derived from cellulose nanofibers is supported on the surface of particles (B), the atomic equivalent amount of carbon derived from the carbonized cellulose nanofibers, i.e., the amount of carbon derived from cellulose nanofibers supported, is preferably 0.1% by mass to 10.0% by mass, more preferably 0.1% by mass to 7.0% by mass, and even more preferably 0.1% by mass to 5.0% by mass, based on 100% by mass of particles (B).
[0042] Like cellulose nanofibers, water-soluble carbon materials are carbonized to form carbon, and when this is supported on the surface of particles (B), like cellulose nanofibers, it effectively suppresses the deterioration of the electronic conductive path and effectively increases the degree of compaction, thereby ensuring that the resulting battery exhibits excellent discharge capacity. Examples of such water-soluble carbonaceous materials include one or more selected from sugars, polyols, polyethers, and organic acids. More specifically, examples include monosaccharides such as glucose, fructose, galactose, and mannose; disaccharides such as maltose, sucrose, and cellobiose; polysaccharides such as starch and dextrin; polyols and polyethers such as ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, butanediol, propanediol, polyvinyl alcohol, and glycerin; and organic acids such as citric acid, tartaric acid, and ascorbic acid. Among these, from the viewpoint of increasing solubility and dispersibility in a solvent and effectively functioning as a carbonaceous material, glucose, fructose, sucrose, and dextrin are preferred, and glucose is more preferred.
[0043] When carbon derived from a water-soluble carbon material is supported on the surface of particles (B), the atomic amount of carbon derived from the water-soluble carbon material, i.e., the amount of carbon derived from the water-soluble carbon material supported, is preferably 0% by mass to 4.0% by mass, more preferably 0% by mass to 3.0% by mass, and even more preferably 0% by mass to 2.0% by mass, based on 100% by mass of particles (B).
[0044] The cellulose nanofiber-derived carbon and the water-soluble carbon material-derived carbon may be supported in the form of only the cellulose nanofiber-derived carbon, only the water-soluble carbon material-derived carbon, or both the cellulose nanofiber-derived carbon and the water-soluble carbon material-derived carbon. Of these, it is preferable to support the cellulose nanofiber-derived carbon from the viewpoint of covering only a portion of the surface of the particles (B) and not interfering with the deformation of the particles (B).
[0045] When carbon derived from cellulose nanofibers and carbon derived from a water-soluble carbon material are supported on the surface of particles (B), the sum of the atomic equivalent amount of carbon derived from cellulose nanofibers and the atomic equivalent amount of carbon derived from the water-soluble carbon material, i.e., the total amount of carbon derived from cellulose nanofibers and the total amount of carbon derived from the water-soluble carbon material, is preferably 1.0 mass% to 10.0 mass%, more preferably 1.5 mass% to 7.0 mass%, and even more preferably 2.0 mass% to 5.0 mass% based on 100 mass% of particles (B).
[0046] From the viewpoint of effectively achieving both high rate characteristics and excellent cycle characteristics, the content of component (B) (particles (B)) in the positive electrode active material for a lithium ion secondary battery of the present invention is 5% by mass to 40% by mass, preferably 10% by mass to 40% by mass, and more preferably 20% by mass to 30% by mass.
[0047] In addition, when component (B) (particles (B)) has carbon derived from cellulose nanofibers and / or carbon derived from a water-soluble carbon material supported on its surface, the content of component (B) (particles (B)) also includes the amount of carbon supported. Furthermore, the atomic equivalent amount (supported amount) of carbon derived from cellulose nanofibers present in particle (B) and the atomic equivalent amount (supported amount) of carbon derived from water-soluble carbon materials are values determined by measurements using a carbon / sulfur analyzer.
[0048] The particles (B) can be obtained, for example, by the following production method. Specifically, the particles (B) can be obtained by the following steps (Ib) to (IVb): (Ib) A step of adding a lithium compound, a manganese compound and / or an iron compound, a phosphate compound, cellulose nanofibers, and water to obtain a slurry water b, and then subjecting the slurry water b to a hydrothermal reaction to obtain a composite B. (IIb) A step of adding the obtained composite B, an acrylic acid (co)polymer or a salt thereof x, nano-resin particles y having an average particle size of 10 nm to 150 nm, and water to obtain a slurry water c. (IIIb) A step of subjecting the obtained slurry water c to spray drying to obtain granules Z (IVb) A step of firing the obtained granules Z Equipped with In this production method, the nano-resin particles y are one or more types selected from polystyrene particles, polymethyl methacrylate particles, and polylactic acid particles.
[0049] The above step (Ib) is a step in which a lithium compound, a manganese compound, an iron compound, a phosphate compound, and water are added to obtain a slurry water b, which is then subjected to a hydrothermal reaction to obtain a composite B.
[0050] As the lithium compound, the same compounds as those used for the particles (A) can be used, but hydroxides are preferred. As the manganese compound, the same ones as those used for the particles (A) can be used. Examples of iron compounds include iron acetate, iron nitrate, and iron sulfate. These may be used alone or in combination of two or more. Among these, iron sulfate is preferred from the viewpoint of improving battery characteristics. In addition to these manganese compounds and iron compounds, metals other than manganese compounds and iron compounds (M 2 ) compounds may also be used. Examples of phosphoric acid compounds include orthophosphoric acid (H3PO4, phosphoric acid), metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, tetraphosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, etc. Among these, phosphoric acid is preferably used, and is preferably used as an aqueous solution with a concentration of 70% by mass to 90% by mass. When supporting carbon derived from cellulose nanofibers, cellulose nanofibers can be added together with a lithium compound and the like in step (Ib) to obtain slurry water b.
[0051] More specifically, step (Ib) includes a step (ib-1) of mixing a phosphate compound with a slurry water b' containing a lithium compound to obtain a composite B'; A step (ib-2) of subjecting the obtained composite B' and a slurry water b containing metal compounds including at least a manganese compound and an iron compound to a hydrothermal reaction to obtain a composite B. It is preferable to have: When cellulose nanofibers are used, a slurry water b' containing a lithium compound and cellulose nanofibers may be prepared.
[0052] In the step (ib-1), the content of the lithium compound in the slurry water b' is preferably 5 to 50 parts by mass, more preferably 7 to 45 parts by mass, per 100 parts by mass of water. When cellulose nanofibers are used, the content thereof in the slurry water b' is preferably 0.2 to 10.6 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 0.8 to 5.3 parts by mass, calculated as the amount of carbonization residue per 100 parts by mass of water. Before adding the phosphoric acid compound to the slurry water b', it is preferable to stir the slurry water b' in advance. The stirring time of the slurry water b' is preferably 1 to 15 minutes, more preferably 3 to 10 minutes. The temperature of the slurry water b' is preferably 20 to 90°C, more preferably 20 to 70°C.
[0053] In step (Ib), when mixing phosphoric acid with the slurry water b', it is preferable to add the phosphoric acid dropwise while stirring the slurry water. The rate at which phosphoric acid is added dropwise to the slurry water b' is preferably 15 mL / min to 50 mL / min, more preferably 20 mL / min to 45 mL / min, and even more preferably 28 mL / min to 40 mL / min. The stirring time for the slurry water b while adding the phosphoric acid dropwise is preferably 0.5 hours to 24 hours, more preferably 3 hours to 12 hours. The stirring speed for the slurry water while adding the phosphoric acid dropwise is preferably 200 rpm to 700 rpm, more preferably 250 rpm to 600 rpm, and even more preferably 300 rpm to 500 rpm. When stirring the slurry water b', it is preferable to further cool it to the boiling point or lower of the slurry water b'. Specifically, it is preferable to cool it to 80°C or lower, and more preferably to 20 to 60°C.
[0054] The slurry water b' after mixing with the phosphoric acid compound preferably contains 2.0 to 4.0 moles, more preferably 2.0 to 3.1 moles, of lithium per mole of phosphoric acid, and the lithium compound and phosphoric acid compound may be used in such amounts. More specifically, the slurry water b' after mixing with the phosphoric acid compound preferably contains 2.7 to 3.3 moles, more preferably 2.8 to 3.1 moles, of lithium per mole of phosphoric acid.
[0055] Nitrogen is purged into the slurry water b' after mixing with the phosphoric acid compound to complete the reaction in the slurry water, obtaining a composite B', a precursor of particle (B), as a slurry. Purging nitrogen allows the reaction to proceed in a state where the dissolved oxygen concentration in the slurry water b' is reduced, and the dissolved oxygen concentration of the resulting slurry water containing composite B' is also effectively reduced, thereby suppressing the oxidation of the metal compound added in the next step. In the slurry water b' containing composite B', the precursor of particle (B) exists as fine dispersed particles. Composite B' is obtained as a composite of trilithium phosphate (Li3PO4) and cellulose nanofibers.
[0056] Next, in step (ib-2), composite B' obtained in step (ib-1) and slurry water b containing metal compounds including at least a manganese compound and an iron compound are subjected to a hydrothermal reaction to obtain composite B.
[0057] The molar ratio of the manganese compound to the iron compound (manganese compound:iron compound) used is preferably 20:80 to 90:10, more preferably 25:75 to 85:15, and even more preferably 30:70 to 80:20. The total amount of these metal compounds added is preferably 0.99 mol to 1.01 mol, more preferably 0.995 mol to 1.005 mol, per mol of phosphate ions contained in the slurry water A.
[0058] The amount of water used in the hydrothermal reaction is preferably 10 mol to 50 mol, and more preferably 12.5 mol to 45 mol, per mol of phosphate ions contained in the slurry water b, from the viewpoints of the solubility of the metal compound, ease of stirring, synthesis efficiency, etc.
[0059] Manganese compounds, iron compounds and metals (M 2 The order of adding the compounds is not particularly limited. In addition to adding these metal compounds, an antioxidant may be added if necessary. Examples of such antioxidants include sodium sulfite (Na2SO3), sodium hydrosulfite (Na2S2O4), and aqueous ammonia. The amount of antioxidant to be added is determined based on the amount of manganese compound, iron compound, and metal (M) compounds used as needed. 2 The amount is preferably 0.01 mol to 1 mol, and more preferably 0.03 mol to 0.5 mol, relative to 1 mol of the total amount of the salt.
[0060] Manganese compounds, iron compounds and metals (M 2 The content of complex B' in the slurry water b obtained by adding the hydroxybenzoate compound and, if necessary, adding an antioxidant, etc. is preferably 10 to 50 mass %, more preferably 15 to 45 mass %, and even more preferably 20 to 40 mass %.
[0061] The hydrothermal reaction may be carried out at a temperature of 100°C or higher, preferably 130°C to 200°C. The hydrothermal reaction is preferably carried out in a pressure-resistant vessel, and when the reaction is carried out at 130°C to 200°C, the pressure is preferably 0.3MPa to 1.6MPa, and when the reaction is carried out at 140°C to 160°C, the pressure is preferably 0.3MPa to 0.6MPa. The hydrothermal reaction time is preferably 0.1 hours to 48 hours, more preferably 0.2 hours to 24 hours. The obtained complex B is isolated by filtration, washing with water, and drying, which can be performed by freeze-drying or vacuum drying.
[0062] The above-mentioned step (IIb) is a step of obtaining a slurry water c by adding the composite B obtained in step (Ib), an acrylic acid (co)polymer or its salt x, nano-resin particles y having an average particle size of 10 nm to 150 nm, and water, and the nano-resin particles y are one or more selected from polystyrene particles, polymethyl methacrylate particles, and polylactic acid particles. In this way, by preparing a slurry water using the composite B obtained in step (Ib), the acrylic acid (co)polymer or its salt x, and the fine nano-resin particles y, physical and electrical effects can be exerted to separate the particles (B) while suppressing their aggregation, and it is also possible to produce particles with large depressions on their surfaces as part of the particles (B) obtained after steps (IIIb) to (IVb) described below.
[0063] The acrylic acid (co)polymer or its salt x adheres to the surface of the particles (B) and can effectively suppress aggregation of the particles (B) by physical and electrical actions. The mass average molecular weight of the acrylic acid (co)polymer or its salt x is preferably 1,000 to 200,000, more preferably 1,000 to 150,000, and even more preferably 1,000 to 100,000, from the viewpoint of effectively suppressing aggregation of the particles (B).
[0064] Specific examples of the acrylic acid (co)polymer or salt thereof x include one or more selected from sodium polyacrylate, ammonium polyacrylate, sodium salt of acrylic acid / maleic acid copolymer, and sodium salt of acrylic acid / acrylamide / sulfonic acid copolymer. Of these, sodium polyacrylate is preferred from the viewpoint of effectively increasing the dispersibility of the aqueous slurry b.
[0065] The amount of the acrylic acid (co)polymer or its salt x added is preferably 0.01 to 1.5 parts by mass, more preferably 0.05 to 1.5 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, relative to 100 parts by mass of composite B.
[0066] The nano-resin particles y enter the gaps between the particles (B), further separating the particles (B) from each other, and also increase the fluidity of the slurry water, facilitating the formation of depressions on the particle surfaces. The nano-resin particles y include one or two types selected from polystyrene particles, polymethyl methacrylate particles, and polylactic acid particles, with polystyrene particles being preferred from the viewpoint of efficiently producing particles having large depressions on their surfaces.
[0067] The amount of such nano resin particles y added is preferably 0.5 to 15 parts by mass, more preferably 1 to 12 parts by mass, and even more preferably 2 to 10 parts by mass, relative to 100 parts by mass of composite B.
[0068] The mass ratio (x / y) of the amount of acrylic acid (co)polymer or its salt x to the amount of nano resin particles y is preferably 0.002 to 3.0, more preferably 0.033 to 1.0, and even more preferably 0.05 to 0.2.
[0069] The solid content concentration of the slurry water c is preferably 5% by mass to 30% by mass, more preferably 5% by mass to 20% by mass, and even more preferably 5% by mass to 15% by mass.
[0070] After adding water, it is preferable to pre-stir the slurry water c before proceeding to step (IIIb). The stirring time of the slurry water c is preferably 3 to 60 minutes, more preferably 5 to 30 minutes. The temperature of the slurry water c is preferably 10 to 60°C, more preferably 20 to 40°C.
[0071] The step (IIIb) is a step of subjecting the slurry water c obtained in the step (IIb) to spray drying to obtain granules Z. In the spray drying, the operating conditions may be appropriately set depending on the apparatus used. For example, the treatment conditions for a micromist dryer (MDL-050M manufactured by Fujisaki Electric Co., Ltd.) equipped with a four-fluid nozzle are such that the hot air temperature is preferably 110°C to 300°C, and more preferably 150°C to 250°C. The volume ratio of the supply amount of hot air to the supply amount of slurry water (supply amount of hot air / supply amount of slurry water) is preferably 500 to 10,000, and more preferably 1,000 to 9,000.
[0072] By obtaining granules Z in step (IIIb), it becomes possible to effectively include particles having one to two large depressions on the surface as part of the particles obtained through the subsequent step (IVb). That is, when the slurry water c is subjected to spray drying, it is first atomized into droplets, and within these droplets, particles (B) are uniformly dispersed in the water. Next, when heat is applied to the droplets in this state, the water on the droplet surface evaporates, and the water present in the center of the droplet migrates to the droplet surface and subsequently evaporates. In this way, as the water migrates from the center to the surface within the droplet, particles (B) migrate along with the water to the droplet surface, resulting in a transition to a state in which particles (B) are distributed in large numbers on the surface. When this state is reached, the water still remaining in the center of the droplet has nowhere to go when it is subsequently dried, and evaporates, breaking down part of the layer of particles (B) on the droplet surface. Traces of the evaporation of the water in the center appear as depressions in the granules Z, and later, through step (IVb) described below, these depressions form larger depressions on the particle surface.
[0073] The step (IVb) is a step of calcining the granules Z obtained in the step (IIIb). The calcination conditions in the step (IVb) are preferably a reducing atmosphere or an inert atmosphere, the calcination temperature is preferably 500°C to 1000°C, more preferably 550°C to 900°C, and the calcination time is preferably 0.5 hours to 12 hours, more preferably 1 hour to 6 hours.
[0074] The positive electrode active material for a lithium ion secondary battery of the present invention contains, as component (C), particles represented by the following formula (c) in an amount of 1% to 10% by mass. LiM 3 y Mn h O4···(c) (In formula (c), M 3 represents one or more elements selected from Ni, Co, Al, Mg, Ti, V, Cr, Fe, Zr, Ga, Cu, and Si. y and h are numbers satisfying 0 ≦ y ≦ 0.1, 0 < h ≦ 2, and (valence of M 3 ) × y + (valence of Mn) × h = 7.)
[0075] The particles represented by the above formula (c) of component (C) (hereinafter also referred to as "particles (C)") are particles having a spinel structure and are secondary particles formed by aggregation of primary particles. By containing such particles (C) in the above amount, the rate characteristics can be remarkably improved.
[0076] Specific examples of the particles (C) represented by the above formula (c) include LiMn2O4, LiNi 0.5 Mn 1.5 O4, LiCoMnO4, LiCrMnO4, LiFeMnO4, LiAlMnO4, LiCu 0.5 Mn 1.5 O4 can be used. Among them, LiMn2O4 is preferable.
[0077] The average particle diameter of the primary particles of the particles (C) represented by the above formula (c) is preferably 50 nm to 1 μm, more preferably 50 nm to 800 nm, from the viewpoints of ensuring excellent rate characteristics and handling. Here, the "average particle diameter as primary particles" in the particles (B) means the crystallite diameter measured by the X-ray diffraction method. Furthermore, the average particle size of particles (C), which are secondary particles formed by aggregation of the primary particles (simply referred to as "average particle size of particles (C)"), is preferably 2 μm to 8 μm, more preferably 5 μm to 8 μm, from the viewpoint of effectively achieving both excellent rate characteristics and cycle characteristics, and from the viewpoint of handling. Here, the "average particle size" of the particles (C) is the D obtained from the volume-based particle size distribution based on the laser diffraction / scattering method. 50 The values are the particle diameters (median diameters) at 50% of the cumulative particle size.
[0078] The content of component (C) (particles (C)) in the positive electrode active material for a lithium ion secondary battery of the present invention is 1 mass % to 10 mass %, preferably 1 mass % to 8 mass %, and more preferably 1 mass % to 4 mass %, from the viewpoint of effectively achieving both excellent rate characteristics and cycle characteristics.
[0079] The particles (C) can be obtained, for example, by the production method described in the Examples. Specifically, the manufacturing method includes steps of adding a lithium compound and a manganese compound, pulverizing and mixing them in a ball mill, calcining the mixture, and then calcining the mixture. Examples of the lithium compound to be used include hydroxides (e.g., LiOH·H2O, LiOH), carbonates, acetates, and nitrates. Of these, carbonates are preferred. Examples of manganese compounds include manganese acetate, manganese nitrate, and manganese oxide. These may be used alone or in combination of two or more. Among these, manganese oxide is preferred from the viewpoint of improving battery characteristics. In addition to these lithium compounds and manganese compounds, metals other than these compounds (M 3 ) compounds may also be used. When firing, it is preferable to first calcinate at 250°C to 700°C, preferably 300°C to 600°C, for 1 to 15 hours, preferably 6 to 12 hours, and then calcinate at 500°C to 1000°C, preferably 600°C to 900°C, for 3 to 30 hours, preferably 12 to 24 hours. After calcination, it is also preferable to crush the material before firing.
[0080] The positive electrode active material for a lithium ion secondary battery of the present invention can be obtained by adjusting the amounts of the particles of the above-mentioned components (A), (B), and (C) to the above-mentioned contents and then mixing them by a conventional method. There is no particular limitation on the order in which the particles of the components (A), (B), and (C) are added.
[0081] The positive electrode active material for a lithium ion secondary battery of the present invention can be used as a positive electrode material to construct a lithium ion secondary battery essentially consisting of a positive electrode, a negative electrode, an electrolyte, and a separator, or a positive electrode, a negative electrode, and a solid electrolyte. Specifically, for example, the positive electrode active material for a lithium ion secondary battery of the present invention is mixed with acetylene black, ketjen black, polyvinylidene fluoride, N-methyl-2-pyrrolidone, or the like to prepare a positive electrode slurry, which is then coated on a current collector and press-molded to form a positive electrode. In the positive electrode active material for a lithium ion secondary battery of the present invention, the three specific types of particles (A) to (C) are closely associated with each other and are easily compacted during press molding, thereby increasing the electrode density and providing a highly useful positive electrode that can effectively improve the rate characteristics and cycle characteristics.
[0082] The negative electrode is not particularly limited in terms of material composition, and any known material composition can be used as long as it can absorb lithium ions during charging and release them during discharging. For example, lithium metal, graphite, silicon-based materials (Si, SiOx), lithium titanate, or carbon materials such as amorphous carbon can be used. It is preferable to use an electrode formed of an intercalating material capable of electrochemically absorbing and releasing lithium ions, particularly a carbon material. Furthermore, two or more of the above negative electrode materials may be used in combination, such as a combination of graphite and silicon-based materials.
[0083] The electrolyte solution is prepared by dissolving a supporting salt in an organic solvent. The organic solvent is not particularly limited as long as it is an organic solvent typically used in electrolyte solutions for lithium ion secondary batteries, and examples thereof include carbonates, halogenated hydrocarbons, ethers, ketones, nitriles, lactones, and oxolane compounds.
[0084] The supporting salt is not particularly limited in type, but is preferably at least one of inorganic salts selected from LiPF6, LiBF4, LiClO4, and LiAsF6, derivatives of these inorganic salts, organic salts selected from LiSO3CF3, LiC(SO3CF3)2, LiN(SO3CF3)2, LiN(SO2C2F5)2, and LiN(SO2CF3)(SO2C4F9), and derivatives of these organic salts.
[0085] The separator serves to electrically insulate the positive and negative electrodes and retain the electrolyte solution, and may be, for example, a porous synthetic resin film, particularly a porous film of a polyolefin polymer (polyethylene, polypropylene).
[0086] The solid electrolyte electrically insulates the positive and negative electrodes and exhibits high lithium ion conductivity. 0.51 Li 0.34 TiO 2.94 , Li 1.3 Al 0.3 Ti 1.7(PO4)3, Li7La3Zr2O 12 , 50Li4SiO4·50Li3BO3, Li 2.9 PO 3.3 N 0.46 , Li 3.6 Si 0.6 P 0.4 O4, Li 1.07 Al 0.69 Ti 1.46 (PO4)3, Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, 30Li2S 26B2S3 44LiI, 63Li2S 36SiS2 1Li3PO4, 57Li2S 38SiS2 5Li4SiO4, 70Li2S 30P2S5, 50Li2S 50GeS2, Li7P3S 11 , Li 3.25 P 0.95 Just use S4.
[0087] The shape of the lithium ion secondary battery having the above configuration is not particularly limited, and may be various shapes such as coin-shaped, cylindrical, or rectangular, or may be an irregular shape enclosed in a laminate exterior. [Example]
[0088] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.
[0089] Particles of each component were produced according to the description of each production example. The physical properties of the particles (B) were measured according to the following methods.
[0090] <<Measurement of the most common cavity diameter and cavity volume>> Particle (B) was measured by mercury intrusion porosimetry using a measuring device (AutoPore IV9520, manufactured by Micromeritics). A Model 08 (manufactured by Micromeritics) sample cell was used, and measurements were made with the surface tension of mercury set at 485 dynes / cm and the contact angle of mercury set at 130°. The measurement pressure range was 0.1 to 60,000 psia. The peak value of the obtained pore size distribution diagram was taken as the mode of the pit diameter, and the peak area was calculated as the pit volume.
[0091] <<Measurement of the average particle size of primary particles>> Measurements were carried out using an X-ray diffractometer (D8 ADVANCE A-25, manufactured by BrukerAXS). The measurement conditions were CuKα target, tube voltage 50 kV, tube current 350 mA, scan range 10 to 80° (2θ), step width 0.0234°, and scan speed 0.13° / step. The XRD pattern was analyzed using the XRD / Lebert method to calculate the crystallite diameter, and this value was used as the average particle diameter of the primary particles.
[0092] <<Measurement of the average particle size of particles (secondary particles)>> The particle size distribution of the particles was measured using a laser diffraction device (Microtrac MT3000II, manufactured by MicrotracBEL). The measurement conditions were particle transmittance: transmission, particle shape: non-spherical, particle refractive index: 1.52. Ethanol was used as the solvent, and the solvent refractive index: 1.36.
[0093] <<Measurement of compaction density>> The density of the particles (B) was measured using a low resistivity meter (MCP-T610, manufactured by Mitsubishi Analytech Co., Ltd.) when a load of 20 kN was applied.
[0094] <<Measurement of the proportion of lithium-based polyanion particles with depressions>> Particles (B) were observed using an SEM, and 10 images were taken of different fields of view. A total of approximately 300 particles (B) were counted in each image. Particles with one to two depressions with a diameter of 1.0 μm or more on their surface were considered to be "particles (B) with one to two depressions formed on their surface," and the number of such particles was counted. The value (%) of {(number of particles with one to two depressions with a diameter of 1.0 μm or more on their surface) / (total number of particles (B) with a diameter of 5.0 μm or more)} × 100 was calculated, and this value was defined as the "particle number ratio of particles (B) with one to two depressions formed on their surface (particle number ratio of depression particles)."
[0095] [Production Example 1: Production of Particles (A) (NCM Particles)] 473 g of nickel sulfate hexahydrate, 169 g of cobalt sulfate heptahydrate, 145 g of manganese sulfate pentahydrate, and 3 L of water were mixed so that the molar ratio of Ni:Co:Mn was 6:2:2, and then 25% ammonia water was added dropwise to the mixture at a rate of 300 mL / min to obtain a slurry a1 containing a metal composite hydroxide with a pH of 11. Next, the slurry a1 was filtered and dried to obtain a metal composite hydroxide mixture b1, and then 37 g of lithium carbonate was mixed with this mixture b1 in a ball mill to obtain a powder mixture c1. The obtained powder mixture c1 was pre-fired in an air atmosphere at 800 °C for 4 hours and crushed, and then fired in an air atmosphere at 800 °C for 11 hours to obtain particles (A) (LiNi 0.6 Co 0.2 Mn 0.2 O2, average particle size of primary particles: 250 nm, average particle size of particles (A): 11.8 μm) were obtained.
[0096] [Production Example 2: Production of particles (B1) (LMFP particles)] Slurry x1 was obtained by mixing 1272 g of LiOH·H2O and 4 L of water. Next, 1153 g of 85% aqueous phosphoric acid solution was added dropwise at 35 mL / min to the resulting slurry x1 while stirring for 3 minutes at 25 °C. Subsequently, 5892 g of cellulose nanofibers (Wma-10002, manufactured by Sugino Machine, fiber diameter 4-20 nm) were added and stirred at 400 rpm for 12 hours to obtain slurry y1 containing Li3PO4. The resulting slurry y1 was purged with nitrogen to adjust the dissolved oxygen concentration of slurry y1 to 0.5 mg / L. Then, 1688 g of MnSO4·5H2O and 834 g of FeSO4·7H2O were added to the total amount of slurry y1 to obtain slurry z1. The molar ratio of added MnSO4 to FeSO4 (manganese compound:iron compound) was 70:30.
[0097] The resulting slurry Z1 was then placed in an autoclave and subjected to a hydrothermal reaction at 170°C for 1 hour. The pressure inside the autoclave was 0.8 MPa. After the hydrothermal reaction, the resulting crystals were filtered and washed with 12 parts by weight of water per part by weight of the crystals. The washed crystals were freeze-dried at -50°C for 12 hours to obtain complex Cz1. 100 g of the resulting complex Cz1 was taken and mixed with 1 L of water, 0.5 g of sodium polyacrylate (Aqualic YS-100, Nippon Shokubai Co., Ltd.), and 5.0 g of polystyrene nanoparticles (PS05V, Nano-Mill Co., Ltd., average particle size 50 nm) to obtain slurry Ez1. The obtained slurry Ez1 was dispersed for 1 minute using an ultrasonic agitator (T25, manufactured by IKA) to uniformly color the entire slurry, and then spray-dried using a spray dryer (MDL-050M, manufactured by Fujisaki Electric Co., Ltd.) (nozzle air flow rate 35 L / min, slurry flow rate 30 mL / min, inlet air temperature 200°C) to obtain granules Fz1. The obtained granules Fz1 were calcined at 700°C for 1 hour under an argon-hydrogen atmosphere (hydrogen concentration 3%) to obtain particles (B1) (LiMn 0.7 Fe 0.3 PO4, carbon loading: 2.0 mass %, average particle size of primary particles: 100 nm, average particle size of particles (B1): 15.8 μm) was obtained. The obtained particles (B1) had a mode of pit diameter measured by mercury intrusion porosimetry: 1.50 μm, pit volume: 0.44 mL / g, and compaction density: 3.1 g / cm. 3 The proportion of particles having one to two depressions on the surface was 72%. An SEM photograph of the obtained particles (B1) is shown in FIG.
[0098] [Production Example 3: Production of particles (B2) (LMFP particles)] In Production Example 2, cellulose nanofiber-derived carbon-supported particles (B2) (LiMn 0.3 Fe 0.7 PO4, carbon loading: 2.0 mass %, average particle size of primary particles: 100 nm, average particle size of particles (B2): 13.3 μm) was obtained. The obtained particles (B2) had a mode of pit diameter measured by mercury intrusion porosimetry: 1.67 μm, pit volume: 0.48 mL / g, and compaction density: 3.0 g / cm. 3 The proportion of particles having one to two depressions on the surface was 65%.
[0099] [Production Example 4: Production of particles (B3) (LMFP particles)] In Production Example 2, particles (B3) (LiMn) supported on cellulose nanofiber-derived carbon were prepared in accordance with Production Example 2, except that the amount of MnSO 5H O was changed from 1688 g to 241 g and the amount of FeSO 7H O was changed from 834 g to 2502 g relative to the total amount of slurry y1. 0.1 Fe 0.9 PO4, carbon loading: 2.0 mass %, average particle size of primary particles: 100 nm, average particle size of particles (B3): 12.7 μm) was obtained. The obtained particles (B3) had a mode of pit diameter measured by mercury intrusion porosimetry: 1.41 μm, pit volume: 0.40 mL / g, and compaction degree: 3.0 g / cm. 3 The proportion of particles having one to two depressions on the surface was 69%.
[0100] [Production Example 5: Production of particles (B4) (LMFP particles)] In Production Example 2, in the granulation step using a spray dryer (MDL-050M, manufactured by Fujisaki Electric Co., Ltd.), the operating conditions of the spray dryer were changed from a nozzle air flow rate of 35 L / min, a slurry flow rate of 30 mL / min, and an inlet air temperature of 200°C to a nozzle air flow rate of 5 L / min, a slurry flow rate of 60 mL / min, and an inlet air temperature of 200°C. 0.7 Fe 0.3 PO4, carbon loading: 2.0 mass %, average particle size of primary particles: 100 nm, average particle size of particles (B4): 31.2 μm) was obtained. The obtained particles (B4) had a mode of pit diameter measured by mercury intrusion porosimetry: 6.81 μm, pit volume: 20.3 mL / g, and compaction degree: 2.2 g / cm. 3 The proportion of particles having one to two depressions on the surface was 54%.
[0101] [Production Example 6: Production of Particles (C) (LMO Particles)] 348 g of manganese oxide and 739 g of lithium carbonate were mixed and pulverized in a ball mill so that the molar ratio of Mn:Li was 2:1, and then the mixture was calcined at 400°C for 10 hours in an air atmosphere to disintegrate it. Then, the mixture was calcined at 800°C for 24 hours in an air atmosphere to obtain particles (C) (LiMn2O4, average particle size of primary particles: 500 nm, average particle size of particles (C): 6.8 μm).
[0102] [Examples 1 to 6, Comparative Examples 1 to 4] According to the formulation shown in Table 1, particles of each component were mixed using a pestle and mortar to obtain a positive electrode active material. Next, the obtained positive electrode active material was used to carry out various evaluations according to the following methods. The results are shown in Table 1.
[0103] <Evaluation of battery characteristics (rate characteristics and cycle characteristics)> The resulting positive electrode active materials were used as positive electrode materials to fabricate positive electrodes for lithium-ion secondary batteries. Specifically, the resulting positive electrode active materials, Ketjen black, and polyvinylidene fluoride were mixed in a mass ratio of 90:5:5, and N-methyl-2-pyrrolidone was added and thoroughly kneaded to prepare a positive electrode slurry. The positive electrode slurry was applied to a 20 μm-thick aluminum foil current collector using a coating machine and vacuum dried at 80 °C for 12 hours. The mixture was then pressed at 20 kN using a roll press and punched into a φ14 mm disk to form a positive electrode.
[0104] Next, a coin-type secondary battery was constructed using the above positive electrode. A lithium foil punched to a diameter of 15 mm was used as the negative electrode. The electrolyte was a 1 mol / L solution of LiPF6 in a mixed solvent of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7. A polymer porous film was used as the separator. These battery components were assembled and housed in an atmosphere with a dew point of -50°C or lower using standard methods to obtain a coin-type secondary battery (CR-2032).
[0105] Using the obtained coin-type secondary battery, the discharge capacities at 0.2 C (34 mAh / g) and 5 C (850 mAh / g) were measured in an environment of 30°C using a discharge capacity measuring device (HJ-1001SD8, manufactured by Hokuto Denko Corporation), and the value of the rate characteristic was calculated using the following formula (x). Rate characteristic = (discharge capacity at 5 C) / (discharge capacity at 0.2 C) (x) Furthermore, the cycle characteristics were calculated by repeating charge and discharge 50 times at 1C (170mAh / g) in an environment at a temperature of 30°C, using the following formula (y). Cycle characteristics = (discharge capacity after 50 cycles) / (maximum discharge capacity during 50 cycles) (y)
[0106] [Table 1]
Claims
1. The following components (A), (B), and (C): (A) Particles represented by the following formula (a) and having an average particle size of 8 μm to 15 μm: 55% by mass to 90% by mass L)) a Co b Mn c M 1 w O 2 ・・・(a) (In formula (a), M 1 represents one or more elements selected from Mg, Ti, Nb, Fe, Cr, Si, Al, Ga, V, Zn, Cu, Sr, Mo, Zr, Sn, Ta, W, La, Ce, Pb, Bi, and Ge. a, b, c, and w are within the range of 0.3≦a<1, 0<b≦0.7, 0<c≦0.7, and 0≦w≦0.3, and 3a+3b+3c+(M 1 (valence of x) × w = 3. (B) A particle aggregate containing particles represented by the following formula (b) and having an average particle size of 12 μm to 25 μm, with one to two depressions formed on the surface: 5% by mass to 40% by mass Li f Mn g Fe h M 2 x 2O 4 ・・・(b) (In formula (b), M 2 represents one or more elements selected from Mg, Al, Ti, Cu, Zn, Nb, Co, Ni, Ca, Sr, Y, Zr, Mo, Ba, Pb, Bi, La, Ce, Nd, and Gd. f, g, h, and x satisfy 0<f≦1.2, 0.3≦g≦1.2, 0.2≦h≦1.2, 0≦x≦0.3, and 3 / 7≦g / h≦4, and f+(valence of Mn)×g+(valence of Fe)×h+(valence of Mn)×g+(valence of Mn). 2 (valence of x) × x = 3. (C) Particles represented by the following formula (c) and having an average particle size of 5 μm to 8 μm: 1% by mass to 10% by mass LiM 3 y Mn j O 4 ・・・(c) (In formula (c), M 3 represents one or more elements selected from Ni, Co, Al, Mg, Ti, V, Cr, Fe, Zr, Ga, Cu, and Si. y and j are each 0≦y≦0.1, 0<j≦2, and (M 3 (valence of Mn) × y + (valence of Mn) × j = 7. A positive electrode active material for a lithium ion secondary battery, comprising components (A), (B), and (C) mixed together in an amount of: In component (B), the most frequent pit diameter as a whole is 1.0 μm to 2.5 μm, the pit volume is 0.3 mL / g to 0.8 mL / g, and the compaction degree under a load of 20 kN is 2.9 g / cm 3 to 3.3 g / cm 3 , as measured by mercury intrusion porosimetry; the ratio of particles having one or two depressions on their surfaces to the number of particles in component (B) is 55% to 100%; A positive electrode active material for a lithium ion secondary battery, comprising carbon derived from cellulose nanofibers and / or carbon derived from a water-soluble carbon material supported on the surface of particles of component (B).
2. A positive electrode active material for a lithium ion secondary battery as described in claim 1, wherein the total amount of carbon derived from cellulose nanofibers and carbon derived from the water-soluble carbon material supported on the surface of the particles of component (B) is 1.0 mass % to 10.0 mass % in 100 mass % of component (B).
Citation Information
Patent Citations
Positive electrode for lithium secondary battery, and lithium secondary battery
JP2011159388A
Lithium ion battery
JP2014192142A
Lithium ion secondary battery
JP2016076317A
Method for manufacturing positive electrode active material composite for lithium ion secondary battery
JP2019050104A
Lithium ion secondary battery
WO2016163282A1