Dry films, cured products, and electronic components

The dry film with a specific polymer resin and inorganic filler composition addresses light-shielding and warpage issues, preventing burrs and chips during dicing, enhancing the quality of semiconductor chips and optical sensor modules.

JP7594998B2Active Publication Date: 2024-12-05TAIYO HOLDINGS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021509008
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-26
Filing Date
2020-03-11
Publication Date
2024-12-05
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

Conventional dry films used in electronic devices suffer from issues such as insufficient light-shielding properties, warpage, and the occurrence of burrs and chips during dicing, particularly in semiconductor chips and optical sensor modules.

Method used

A dry film composed of a light-shielding curable resin containing a polymer resin with a glass transition point of 20°C or less and a weight average molecular weight of 10,000 or more, combined with an inorganic filler and a coloring agent, where the maximum particle size of the filler aggregates is limited to half the thickness of the resin layer, enhancing dispersibility and light-shielding properties.

Benefits of technology

The solution provides excellent light-shielding, suppresses warpage, and effectively prevents burrs and chips during dicing, ensuring high-quality production of semiconductor chips and optical sensor modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594998000002
    Figure 0007594998000002
  • Figure 0007594998000003
    Figure 0007594998000003
  • Figure 0007594998000001
    Figure 0007594998000001
Patent Text Reader

Abstract

A dry film 11 includes a curable resin layer 12 made of a light-shielding curable resin composition containing: a polymer resin having a glass transition point of 20°C or less and a weight average molecular weight of 10,000 or greater; a coloring agent; and an inorganic filler. When the thickness of the curable resin layer 12 is X (μm), the largest particle diameter of aggregate particles of the inorganic filler is X / 2 (μm) or less. The dry film 11 has excellent light-shielding performance, and is configured such that warping is suppressed and burrs and chipping during dicing can also be suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dry film, a cured product, and an electronic component. [Background technology]

[0002] Conventionally, dry films (laminate films) have been used as one of the means for forming protective films and insulating layers such as solder resists and interlayer insulating layers provided on printed wiring boards used in electronic devices, etc. (for example, Patent Document 1). Dry films have a resin layer obtained by applying a resin composition having desired properties onto a carrier film and then carrying out a drying process, and are generally distributed on the market in a state in which a protective film for protecting the surface opposite to the carrier film is further laminated. After attaching the resin layer of the dry film to a substrate (hereinafter also referred to as "lamination"), patterning and curing treatment are carried out to manufacture printed wiring boards and the like having the above-mentioned protective films and insulating layers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-010179 A Summary of the Invention [Problem to be solved by the invention]

[0004] Dry films are also used as encapsulants for semiconductor chips. After the dry film laminated on the semiconductor wafer is cured to form an encapsulant, the semiconductor wafer is diced, for example, using a blade-type cutter to cut the wafer into individual semiconductor chips. During this dicing process, burrs may be formed on the cut edge of the encapsulant, or the encapsulant may be chipped. After the semiconductor chip is encapsulated, the encapsulant on the chip may become thinner, but even in this case, light-shielding properties are required to block light from the outside and protect the semiconductor chip. In addition, resins with high light-shielding properties are required for materials placed around the partitions in optical sensor modules and the RGB light-emitting elements in displays using micro LEDs, but the light-shielding properties of previous resins have not always been sufficient. In addition, dry films are sometimes required to have low light transmittance for other applications such as black solder resist. Furthermore, the dry film is required to have minimal warping when cured on the substrate so that the resin layer can adhere sufficiently to the substrate.

[0005] Therefore, an object of the present invention is to provide a dry film, a cured product, and an electronic component that have excellent light-shielding properties, are suppressed in warping, and are capable of suppressing burrs and chipping during dicing. [Means for solving the problem]

[0006] As a result of intensive research into solving the above-mentioned problems, the inventors have discovered that a dry film having a curable resin layer made of a light-blocking curable resin composition containing a polymer resin having a glass transition point of 20°C or less and a weight-average molecular weight of 10,000 or more, a colorant, and an inorganic filler, wherein the maximum particle diameter of the aggregated particles of the inorganic filler is half or less of the thickness of the curable resin layer, thereby achieving excellent dispersibility, sufficient light-blocking properties, suppression of warping, and suppression of burrs and chipping during dicing, and have arrived at the present invention.

[0007] That is, the dry film of the present invention includes a curable resin layer made of a light-blocking curable resin composition including a polymer resin having a glass transition point of 20° C. or lower and a weight average molecular weight of 10,000 or more, a colorant, and an inorganic filler; When the thickness of the curable resin layer is X (μm), the maximum particle size of the aggregate particles of the inorganic filler is X / 2 (μm) or less. In the present invention, the light-shielding property means that when the thickness of the curable resin layer is 40 μm, the transmittance is less than 0.5% over the entire light wavelength range of 380 to 780 nm.

[0008] In the dry film of the present invention, the maximum particle size of the inorganic filler aggregate particles is preferably 10 μm or less, the blending amount of the inorganic filler is preferably 0.1 to 70 mass % relative to the solid content of the light-shielding curable resin composition, the blending amount of the colorant is preferably 0.3 to 20 mass % relative to the solid content of the light-shielding curable resin composition, the blending amount of the polymer resin having a glass transition point of 20° C. or less and a weight-average molecular weight of 10,000 or more is preferably 1 to 35 mass % relative to the solid content of the light-shielding curable resin composition, and it is preferable that the curable resin layer further contains a liquid epoxy resin.

[0009] The cured product of the present invention is characterized by being obtained by curing the curable resin layer of the dry film.

[0010] The electronic part of the present invention is characterized by having the above-mentioned cured product. Effect of the Invention

[0011] According to the present invention, it is possible to provide a dry film, a cured product, and an electronic component that have excellent light-shielding properties, are suppressed from warping, and are further capable of suppressing burrs and chipping during dicing. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an embodiment of the dry film of the present invention. [Diagram 2] This is a diagram showing the color of a colorant on the coordinate axes representing the a* and b* values ​​in the L*a*b* color system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The dry film, the cured product, and the electronic component of the present invention will be described in more detail below. Fig. 1 is a schematic cross-sectional view of a dry film 11 according to one embodiment of the present invention. The dry film 11 shown in Fig. 1 has a three-layer structure in which a curable resin layer 12 is formed on a carrier film 13, and a protective film 14 is laminated on the carrier film 13. If necessary, the dry film 11 may have another resin layer between the protective film and the curable resin layer, or between the support film and the curable resin layer.

[0014] <Curable resin layer> The dry film of the present invention has a curable resin layer made of a light-blocking curable resin composition containing a polymer resin having a glass transition point of 20° C. or lower and a weight-average molecular weight of 10,000 or more, a colorant, and an inorganic filler, and when the thickness of the curable resin layer is X (μm), the maximum particle size of the agglomerated particles of the inorganic filler is X / 2 (μm) or less.

[0015] The inorganic filler can suppress the curing shrinkage of the obtained cured product, and improve various properties such as adhesion, hardness, and crack resistance by matching the coefficient of linear expansion (CTE) with that of a conductor layer such as copper surrounding the insulating layer. However, the inorganic filler aggregates when the light-shielding curable resin composition is prepared and made into an ink. The present inventors' research has revealed that if the aggregated particles of the aggregated inorganic filler are large, burrs and chipping are likely to occur during dicing. In addition, the light-shielding property (low transmittance) of the cured product is improved by including a colorant such as carbon black in the curable resin composition. The present inventors' research has revealed that if the aggregated particles of the aggregated inorganic filler are large, the inorganic filler is likely to scatter light in the cured product, which is disadvantageous to the light-shielding property. Therefore, when the thickness of the curable resin layer is X (μm), by setting the maximum particle diameter of the aggregated particles of the inorganic filler to X / 2 (μm) or less, burrs and chipping during dicing can be suppressed, and the light-shielding property can be improved even in a thin film on a semiconductor chip.

[0016] In addition, the curable resin layer contains a polymer resin having a glass transition point of 20° C. or less and a weight average molecular weight of 10,000 or more, which can suppress aggregation of the colorant and inorganic filler, improve the dispersibility of the colorant and inorganic filler, and suppress sedimentation, thereby improving both the light blocking property and the long-term stability of the curable resin composition. Furthermore, warping of the cured product can be suppressed. The curable resin layer of the dry film is generally in a state called a B-stage state, and is obtained from a light-blocking curable resin composition. Each component will be described below.

[0017] [Polymer resin with a glass transition temperature of 20°C or lower and a weight-average molecular weight of 10,000 or more] The glass transition point of a polymer resin having a glass transition point of 20° C. or less and a weight average molecular weight of 10,000 or more is preferably −40 to 20° C., more preferably −15 to 15° C., and particularly preferably −5 to 15° C. When it is −5 to 15° C., warping of the cured product can be effectively suppressed. In addition, since the higher the weight average molecular weight of the polymer resin, the greater the effect of preventing the colorant and inorganic filler from settling, the weight average molecular weight is preferably 100,000 or more, and more preferably 200,000 or more. The upper limit is, for example, 1,000,000 or less, and preferably 500,000 or less.

[0018] Examples of the polymer resin include polymer resins having one or more skeletons selected from a butadiene skeleton, an amide skeleton, an imide skeleton, an acetal skeleton, a carbonate skeleton, an ester skeleton, a urethane skeleton, an acrylic skeleton, and a siloxane skeleton. Examples of the resins include polymer resins having a butadiene skeleton ("G-1000", "G-3000", "GI-1000", "GI-3000" manufactured by Nippon Soda Co., Ltd., "R-45EPI" manufactured by Idemitsu Kosan Co., Ltd., "PB3600" and "Epofriend AT501" manufactured by Daicel Corporation, "Ricon130", "Ricon142", "Ricon150", "Ricon657", and "Ricon130MA" manufactured by Cray Valley Chemical Industries, Ltd.), polymer resins having a butadiene skeleton and a polyimide skeleton (those described in JP 2006-37083 A), and polymer resins having an acrylic skeleton ("SG-P3", "SG-600LB", "SG-280", "SG-790", and "SG-K2" manufactured by Nagase ChemteX Corporation, and "SN-50", "AS-3000E", and "ME-2000" manufactured by Negami Chemical Industries, Ltd.).

[0019] From the viewpoint of flatness of the cured product, the polymer resin is preferably an acrylic copolymer having a glass transition point of 20° C. or less and a weight average molecular weight of 10,000 or more. Also, from the viewpoint of dispersibility of the colorant and inorganic filler and suppression of sedimentation of the composition, the polymer resin is preferably an acrylic copolymer having a glass transition point of 20° C. or less and a weight average molecular weight of 100,000 to 1,000,000, and more preferably an acrylic copolymer having a glass transition point of −5 to 15° C. and a weight average molecular weight of 200,000 to 500,000.

[0020] The acrylic acid ester copolymer may have a functional group, and examples of the functional group include a carboxyl group, a hydroxyl group, an epoxy group, and an amide group.

[0021] The acrylic acid ester copolymer preferably contains an epoxy group, and more preferably contains an epoxy group and an amide group. By containing an epoxy group, warping of the cured product can be suppressed.

[0022] Examples of the acrylic acid ester copolymer include Teisan Resin SG-70L, SG-708-6, WS-023 EK30, SG-P3, SG-80H, SG-280 EK23, SG-600TEA, and SG-790 manufactured by Nagase Chemtex Corp. The acrylic acid ester copolymer may be obtained by synthesis, and examples of the synthesis method include the synthesis method described in JP 2016-102200 A.

[0023] The polymer resin can be used alone or in combination of two or more kinds. The blending amount of the polymer resin is preferably 1 to 35 mass% based on the total solid content of the composition, and more preferably 1 to 30 mass%. When it is within the above range, the dispersibility of inorganic fillers and the like and the long-term stability of the composition can be improved. In particular, when the blending amount of the polymer resin is 5 mass% or more, a cured film having low transmittance and suppressing warping of the substrate can be obtained.

[0024] In this specification, the value of the weight average molecular weight (Mw) can be measured by gel permeation chromatography (GPC) method (polystyrene standard) using, for example, the measurement device and measurement conditions described below. Measurement equipment: Waters 2695 Detector: Waters "Waters2414", RI (differential refractometer) Column: Waters "HSPgel Column, HR MB-L, 3 μm, 6 mm × 150 mm" × 2 + Waters "HSPgel Column, HR1, 3 μm, 6 mm × 150 mm" × 2 Measurement conditions: Column temperature: 40℃ RI detector temperature setting: 35℃ Developing solvent: Tetrahydrofuran Flow rate: 0.5mL / min Sample volume: 10μL Sample concentration: 0.7% by mass

[0025] [Coloring agent] The colorant is not particularly limited as long as it can provide a light-blocking curable resin composition, and a known and commonly used black colorant can be used. Specific examples include carbon black, titanium black, iron oxide, cobalt oxide, and perylene-based black colorants, and these colorants can be used alone or in combination. The colorant may be a perylene-based colorant or a combination of a colorant having a complementary color to the perylene-based colorant, provided that the combination exhibits light-blocking properties. Perylene colorants include those that exhibit colors such as green, yellow, orange, red, purple, and black, and are assigned the following Color Index (CI; published by The Society of Dyers and Colourists) numbers. -Green: Solvent Green 5 -Orange:Solvent Orange 55 -Red: Solvent Red 135, 179; Pigment Red 123, 149, 178, 179, 190, 194, 224 -Pigment Violet 29 -Black: Pigment Black 31, 32 Perylene colorants other than those mentioned above can also be used. For example, although they do not have a color index number, BASF's Lumogen (registered trademark) Black FK4280 and Lumogen Black FK4281, which are known as near-infrared transmitting black organic pigments, and Lumogen F Yellow 083, Lumogen F Orange 240, Lumogen F Red 305, and Lumogen F Green 850, which are known as light-collecting fluorescent dyes, can be suitably used because, like other perylene compounds, they have little absorption in the ultraviolet region and high coloring power.

[0026] The complementary colorant used in combination with the perylene-based colorant in the present invention will be described below. First, the complementary color relationship in the present invention will be described. Since the colorant may not have a color according to the color index color, the external color tone of the cured coating film of the resin composition is measured and displayed by the method specified in JIS Z8729, and the a* and b* values ​​indicating the color in the L*a*b* color system are confirmed on the coordinate axes (see FIG. 2), and a colorant that brings the (a* value, b* value) of the cured coating film obtained in combination with the perylene colorant as close as possible to (0, 0) is selected as a colorant having a complementary color relationship. Here, the film thickness of the cured coating film is not particularly limited, but is, for example, 40 μm. Moreover, as for (a* value, b* value) that is infinitesimally close to (0, 0), the a value and the b value are each in the range of −5 to +5, and preferably in the range of −2 to +2. Moreover, the colorants having a complementary color relationship may be either perylene-based colorants or colorants other than perylene-based colorants.

[0027] The colorant that has a complementary color relationship with the perylene-based colorant may be any colorant that, when combined with the perylene-based colorant, causes the color system a* value and b* value of each of the colorants to approach 0, and examples of the colorants include the following colorants: More preferred combinations of perylene-based colorants and colorants that are complementary to each other are combinations of Pigment Red 149, 178, and 179 with green anthraquinone-based colorants (Solvent Green 3, Solvent Green 20, Solvent Green 28, etc.), and mixtures (combinations) of perylene-based colorants include combinations of a red perylene-based colorant (Pigment Red 149, 178, and 179) with a black perylene-based colorant (Pigment Black 31 and 32), and combinations of a black perylene-based colorant (Pigment Black 31 and 32) with the same black perylene-based colorant (Lumogen (registered trademark) Black FK4280 and 4281).

[0028] The colorant may be any combination selected from the group consisting of a yellow colorant and a purple colorant, a yellow colorant, a blue colorant, and a red colorant, a green colorant and a purple colorant, a green colorant and a red colorant, a yellow colorant, a purple colorant, and a blue colorant, and a green colorant, a red colorant, and a blue colorant, as long as the resin composition has a light-shielding property by the combination. In addition, a purple colorant, an orange colorant, a brown colorant, etc. may be combined.

[0029] Blue colorants include phthalocyanine and anthraquinone compounds, which are classified as pigments and solvents. In addition, metal-substituted or unsubstituted phthalocyanine compounds can also be used. Red colorants include monoazo-based, diazazol-based, azo lake-based, benzimidazolone-based, perylene-based, diketopyrrolopyrrole-based, condensed azo-based, anthraquinone-based, and quinacridone-based. Yellow colorants include monoazo-based, disazo-based, condensed azo-based, benzimidazolone-based, isoindolinone-based, and anthraquinone-based. Green colorants include phthalocyanine and anthraquinone types, and metal-substituted or unsubstituted phthalocyanine compounds can also be used.

[0030] Specific examples of purple, orange and brown colorants include Pigment Violet 19, 23, 29, 32, 36, 38 and 42; Solvent Violet 13 and 36; CI Pigment Orange 1, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 14, CI Pigment Orange 16, CI Pigment Orange 17, CI Pigment Orange 24, CI Pigment Orange 34, CI Pigment Orange 36, CI Pigment Orange 38, CI Pigment Orange 40, CI Pigment Orange 43, CI Pigment Orange 46, CI Pigment Orange 49, CI Pigment Orange 51, CI Pigment Orange 61, CI Pigment Orange 63, CI Pigment Orange 64, CI Pigment Orange 71, CI Pigment Orange 73; CI Pigment Brown 23, CI Pigment Brown 25; CI Pigment Black 1, CI Pigment Black 7, etc. The amount of the colorant is not particularly limited, but is preferably 0.3 to 20 parts by mass based on the total solid content of the composition. By making the amount 0.3 parts by mass or more, the light-shielding properties can be improved. On the other hand, by making the amount 20 parts by mass or less, a composition with excellent dispersibility can be obtained.

[0031] Carbon black can obtain light-shielding properties by dispersing it in a resin. Carbon black generally used as a black colorant can be used. As the carbon black, one or more types of known carbon black such as channel black, furnace black, thermal black, and lamp black can be used. Resin-coated carbon black may also be used. Furthermore, carbon nanofibers and carbon nanotubes may also be used. When carbon black is blended into the resin composition, carbon black powder or a carbon black dispersion may be added. The average particle size of carbon black is preferably from 10 to 500 nm, more preferably from 10 to 300 nm, and particularly preferably from 10 to 100 nm. The average particle size is an arithmetic mean diameter determined by observation with an electron microscope.

[0032] The blending amount of carbon black is preferably 0.1 to 20 mass% based on the total solid content of the light-shielding curable resin composition. When the blending amount of carbon black is 0.1 mass% or more, sufficient light-shielding properties can be obtained, and when it is 20 mass% or less, the occurrence of cracks can be suppressed. Furthermore, the greater the amount of carbon black blended, the more likely the carbon black is to settle, but the inclusion of the aforementioned polymer resin having a glass transition point of 20° C. or lower and a weight average molecular weight of 10,000 or more suppresses the settling of carbon black. Here, the amount of the polymer resin having a glass transition point of 20° C. or lower and a weight average molecular weight of 10,000 or more blended to the amount of carbon black blended is preferably 1:1 to 100:1 in mass ratio.

[0033] [Inorganic filler] The curable resin layer contains an inorganic filler. By blending an inorganic filler, the curing shrinkage of the obtained cured product can be suppressed, and thermal properties such as adhesion, hardness, and crack resistance can be improved by matching the CTE with a conductor layer such as copper around the insulating layer. As the inorganic filler, a conventionally known inorganic filler can be used, and is not limited to a specific one. For example, barium sulfate, barium titanate, amorphous silica, crystalline silica, fused silica, spherical silica, and other silica, talc, clay, Neuburg silica particles, boehmite, magnesium carbonate, calcium carbonate, titanium oxide, aluminum oxide, aluminum hydroxide, silicon nitride, aluminum nitride, calcium zirconate, and metal powders such as copper, tin, zinc, nickel, silver, palladium, aluminum, iron, cobalt, gold, and platinum can be mentioned. The inorganic filler is preferably a spherical particle. Among them, silica is preferable, as it suppresses the curing shrinkage of the cured product of the curable composition, has a lower CTE, and improves properties such as adhesion and hardness.

[0034] The inorganic filler may be surface-treated. The surface treatment may be a surface treatment using a coupling agent or a surface treatment that does not introduce an organic group, such as an alumina treatment. The surface treatment method of the inorganic filler is not particularly limited, and a publicly known and commonly used method may be used, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.

[0035] The surface treatment of the inorganic filler is preferably a surface treatment with a coupling agent. As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents can be used. Among them, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane, which can be used alone or in combination. It is preferable that these silane-based coupling agents are fixed to the surface of the inorganic filler in advance by adsorption or reaction. Here, the treatment amount of the coupling agent relative to 100 parts by mass of the inorganic filler is, for example, 0.5 to 10 parts by mass.

[0036] The curable reactive group is preferably a thermosetting reactive group. Examples of the thermosetting reactive group include a hydroxyl group, a carboxyl group, an isocyanate group, an amino group, an imino group, an epoxy group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. Among them, at least one of an amino group and an epoxy group is preferable. The surface-treated inorganic filler may have a photocurable reactive group in addition to the thermosetting reactive group.

[0037] In addition, the surface-treated inorganic filler may be contained in the curable resin layer in a surface-treated state, and the inorganic filler and the surface treatment agent may be separately blended into the curable resin composition forming the curable resin layer to surface-treat the inorganic filler in the composition, but it is preferable to blend the inorganic filler that has been surface-treated in advance. By blending the inorganic filler that has been surface-treated in advance, it is possible to prevent a decrease in crack resistance, etc. due to the surface treatment agent that was not consumed in the surface treatment that may remain when blended separately. When performing surface treatment in advance, it is preferable to blend a preliminary dispersion in which the inorganic filler is pre-dispersed in a solvent or a curable resin, and the surface-treated inorganic filler is pre-dispersed in a solvent and the preliminary dispersion is blended into the composition, or it is more preferable to sufficiently surface-treat the inorganic filler when pre-dispersing it in a solvent, and then blend the preliminary dispersion into the composition. The inorganic filler may be blended in a powder or solid state with other components of the curable resin composition, or may be mixed with a solvent and a dispersant to form a slurry and then blended with other components.

[0038] The maximum particle diameter of the aggregated particles of the inorganic filler is X / 2 (μm) or less, where X (μm) is the thickness of the curable resin layer. By making the maximum particle diameter of the aggregated particles equal to or less than half the thickness of the curable resin layer, it is possible to suppress scattering of light by the inorganic filler in the curable resin layer and obtain sufficient light blocking properties. In addition, although the inclusion of the inorganic filler itself is advantageous in suppressing burrs during dicing, if the maximum particle diameter of the aggregated particles is large, burrs are more likely to occur and chipping is more likely to occur during dicing. The maximum particle size of the aggregated particles of the inorganic filler is preferably 10 μm or less while satisfying the relationship with the film thickness of the curable resin layer described above. By having the maximum particle size of the aggregated particles of the inorganic filler be 10 μm or less, burrs and chipping during dicing can be more effectively suppressed. The above-mentioned polymer resin having a glass transition point of 20° C. or less and a weight average molecular weight of 10,000 or more can improve the dispersibility of the inorganic filler. Therefore, a curable resin composition containing a polymer resin having a glass transition point of 20° C. or less and a weight average molecular weight of 10,000 or more has excellent dispersion stability in the ink state and can suppress the aggregation of the inorganic filler. Therefore, the maximum particle size of the aggregated particles of the inorganic filler can be maintained at 10 μm or less even after the ink, i.e., the curable resin composition, is stored for a long period of time.

[0039] The inorganic filler may be used alone or in a mixture of two or more kinds. The amount of the inorganic filler is preferably 0.1 to 70% by mass based on the total solid content of the curable resin layer of the dry film. When the amount of the inorganic filler is 0.1% by mass or more, thermal expansion is suppressed and heat resistance is improved, while when the amount is 70% by mass or less, the occurrence of cracks can be suppressed. In addition, when the amount of the inorganic filler is 20% by mass or more, dicing resistance is improved, so this is preferable.

[0040] [Epoxy resin] The light-shielding curable resin composition may contain an epoxy resin. The epoxy resin is a resin having an epoxy group, and any of the conventionally known epoxy resins may be used. Examples of the epoxy resin include a bifunctional epoxy resin having two epoxy groups in the molecule, and a multifunctional epoxy resin having three or more epoxy groups in the molecule. The epoxy resin may be a hydrogenated epoxy resin. The epoxy resin may be a solid epoxy resin, a liquid epoxy resin, a semi-solid epoxy resin, or a crystallized epoxy resin, and among these, it is preferable to include at least a liquid epoxy resin. The solid epoxy resin and the liquid epoxy resin may be used alone or in combination of two or more types. In this specification, the solid epoxy resin refers to an epoxy resin that is solid at 40°C, the semi-solid epoxy resin refers to an epoxy resin that is solid at 20°C and liquid at 40°C, and the liquid epoxy resin refers to an epoxy resin that is liquid at 20°C. The liquid state is determined in accordance with the "Method of Confirming Liquid State" in Appendix 2 of the Ministerial Ordinance on the Testing and Properties of Hazardous Materials (Ministry of Home Affairs Ordinance No. 1 of 1989). For example, the method described in paragraphs 23 to 25 of JP 2016-079384 A can be used. The crystalline epoxy resin refers to a highly crystalline epoxy resin, and is a thermosetting epoxy resin in which polymer chains are regularly arranged at temperatures below the melting point, and which, although being a solid resin, has a low viscosity comparable to that of a liquid resin when melted.

[0041] Examples of liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, glycidylamine type epoxy resins, aminophenol type epoxy resins, alicyclic epoxy resins, etc. By including a liquid epoxy resin, the flexibility of the dry film is excellent.

[0042] Examples of solid epoxy resins include naphthalene-type epoxy resins such as HP-4700 (naphthalene-type epoxy resin) manufactured by DIC Corporation and NC-7000 (naphthalene skeleton-containing multifunctional solid epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; epoxidized products (trisphenol-type epoxy resins) of condensates of phenols and aromatic aldehydes having a phenolic hydroxyl group, such as EPPN-502H (trisphenol epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; dicyclopentadiene aralkyl-type epoxy resins such as EPICLON HP-7200H (dicyclopentadiene skeleton-containing multifunctional solid epoxy resin) manufactured by DIC Corporation; biphenyl aralkyl-type epoxy resins such as NC-3000H (biphenyl skeleton-containing multifunctional solid epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; biphenyl / phenol novolac-type epoxy resins such as NC-3000L manufactured by Nippon Kayaku Co., Ltd.; EPICLON N660 and EPICLON Examples include novolac epoxy resins such as N690, N770, and EOCN-104S manufactured by Nippon Kayaku Co., Ltd.; phosphorus-containing epoxy resins such as TX0712 manufactured by Nippon Steel Chemical & Material Co., Ltd.; and tris(2,3-epoxypropyl)isocyanurate such as TEPIC manufactured by Nissan Chemical Co., Ltd. By including a solid epoxy resin, the glass transition temperature of the cured product becomes high, resulting in excellent heat resistance.

[0043] The semi-solid epoxy resin preferably contains at least one selected from the group consisting of bisphenol A type epoxy resin, naphthalene type epoxy resin, and phenol novolac type epoxy resin. By containing the semi-solid epoxy resin, the glass transition temperature (Tg) of the cured product becomes high, the CTE becomes low, and the crack resistance becomes excellent. Examples of semi-solid epoxy resins include bisphenol A type epoxy resins such as EPICLON 860, EPICLON 900-IM, EPICLON EXA-4816, and EPICLON EXA-4822 manufactured by DIC Corporation, Epotohto YD-134 manufactured by Nippon Steel Chemical & Materials Co., Ltd., jER834 and jER872 manufactured by Mitsubishi Chemical Corporation, and ELA-134 manufactured by Sumitomo Chemical Co., Ltd.; naphthalene type epoxy resins such as EPICLON HP-4032 manufactured by DIC Corporation; and phenol novolac type epoxy resins such as EPICLON N-740 manufactured by DIC Corporation.

[0044] As the crystalline epoxy resin, for example, a crystalline epoxy resin having a biphenyl structure, a sulfide structure, a phenylene structure, a naphthalene structure, or the like can be used. Examples of biphenyl type epoxy resins include jER YX4000, jER YX4000H, jER YL6121H, jER YL6640, and jER YL6677 manufactured by Mitsubishi Chemical Corporation. Examples of diphenyl sulfide type epoxy resins include Epotohto YSLV-120TE manufactured by Nippon Steel Chemical & Material Co., Ltd. Examples of phenylene type epoxy resins include Epotohto YDC-1312 manufactured by Nippon Steel Chemical & Material Co., Ltd. Examples of naphthalene type epoxy resins include EPICLON HP-4032, EPICLON HP-4032D, and EPICLON HP-4700 manufactured by DIC Corporation. In addition, as the crystalline epoxy resin, Epotohto YSLV-90C manufactured by Nippon Steel Chemical & Material Co., Ltd. and TEPIC-S (triglycidyl isocyanurate) manufactured by Nissan Chemical Industries, Ltd. can also be used.

[0045] The total amount of epoxy resin is preferably 1 to 70 mass% based on the total solid content of the composition. Within this range, the cured product has excellent heat resistance, flexibility, and crack resistance. The liquid epoxy resin is preferably 5 to 60 mass% based on the total solid content of the epoxy resin, curing agent, curing accelerator, and polymer resin. Within this range, the dry film has excellent flexibility.

[0046] The light-blocking curable resin composition may contain a curable resin component other than the epoxy resin, as long as the effect of the present invention is not impaired. For example, a known and commonly used thermosetting resin such as an isocyanate compound, a blocked isocyanate compound, an amino resin, a benzoxazine resin, a carbodiimide resin, a cyclocarbonate compound, a polyfunctional oxetane compound, or an episulfide resin can be used.

[0047] [Hardening agent] The light-shielding curable resin composition preferably contains a curing agent. Examples of the curing agent include a compound having a phenolic hydroxyl group, a polycarboxylic acid and its acid anhydride, a compound having a cyanate ester group, a compound having an active ester group, a compound having a maleimide group, and an alicyclic olefin polymer. The curing agent can be used alone or in combination of two or more.

[0048] Examples of the resin having a phenolic hydroxyl group that can be used include conventionally known resins such as phenol novolac resins, alkylphenol novolac resins, bisphenol A novolac resins, dicyclopentadiene-type phenol resins, Xylok-type phenol resins, terpene-modified phenol resins, cresol / naphthol resins, polyvinyl phenols, phenol / naphthol resins, α-naphthol skeleton-containing phenol resins, triazine skeleton-containing cresol novolac resins, biphenylaralkyl-type phenol resins, and Xylok-type phenol novolac resins. Examples of resins having a phenolic hydroxyl group include dicyclopentadiene skeleton phenol novolac resin (GDP series, manufactured by Gun-ei Chemical Industry Co., Ltd.), Zylok type phenol novolac resin (MEH-7800, manufactured by Meiwa Chemical Industry Co., Ltd.), biphenyl aralkyl type novolac resin (MEH-7851, manufactured by Meiwa Chemical Industry Co., Ltd.), naphthol aralkyl type hardener (SN series, manufactured by Nippon Steel Chemical & Material Co., Ltd.), triazine skeleton-containing cresol novolac resin (LA-3018-50P, manufactured by DIC Corporation), and triazine skeleton-containing phenol novolac resin (LA-705N, manufactured by DIC Corporation).

[0049] The compound having a cyanate ester group is preferably a compound having two or more cyanate ester groups (-OCN) in one molecule. Any of the conventionally known compounds having a cyanate ester group can be used. Examples of the compound having a cyanate ester group include phenol novolac type cyanate ester resin, alkylphenol novolac type cyanate ester resin, dicyclopentadiene type cyanate ester resin, bisphenol A type cyanate ester resin, bisphenol F type cyanate ester resin, and bisphenol S type cyanate ester resin. In addition, it may be a prepolymer partially converted to triazine.

[0050] Commercially available compounds having a cyanate ester group include phenol novolac type polyfunctional cyanate ester resin (PT30S, manufactured by Lonza Japan), a prepolymer in which a part or all of bisphenol A dicyanate is triazine-converted to a trimer (BA230S75, manufactured by Lonza Japan), and a dicyclopentadiene structure-containing cyanate ester resin (DT-4000, DT-7000, manufactured by Lonza Japan).

[0051] The compound having an active ester group is preferably a compound having two or more active ester groups in one molecule. The compound having an active ester group can generally be obtained by a condensation reaction between a carboxylic acid compound and a hydroxy compound. Among them, a compound having an active ester group obtained by using a phenol compound or a naphthol compound as a hydroxy compound is preferable. Examples of the phenol compound or naphthol compound include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadienyl diphenol, and phenol novolac. The compound having an active ester group may be a naphthalenediol alkyl / benzoic acid type compound.

[0052] Commercially available compounds having an active ester group include dicyclopentadiene-type diphenol compounds such as HPC8000-65T (manufactured by DIC Corporation), HPC8100-65T (manufactured by DIC Corporation), and HPC8150-65T (manufactured by DIC Corporation).

[0053] The compound having a maleimide group is a compound having a maleimide skeleton, and any of the conventionally known compounds can be used. The compound having a maleimide group preferably has two or more maleimide skeletons, and examples of the compound include N,N'-1,3-phenylene dimaleimide, N,N'-1,4-phenylene dimaleimide, N,N'-4,4-diphenylmethane bismaleimide, 1,2-bis(maleimide)ethane, 1,6-bismaleimide hexane, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 2,2'-bis-[4-(4-maleimide phenoxy)phenyl]propionate, and the like. More preferably, the oligomer is at least one of the following: bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, bisphenol A diphenyl ether bismaleimide, polyphenylmethane maleimide, and oligomers thereof, and diamine condensates having a maleimide skeleton. The oligomer is an oligomer obtained by condensing a compound having a maleimide group, which is a monomer among the above-mentioned compounds having a maleimide group.

[0054] Commercially available compounds having a maleimide group include BMI-1000 (4,4'-diphenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-2300 (phenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-3000 (m-phenylene bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-5100 (3,3'-dimethyl-5,5'-dimethyl-4,4'-diphenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-7000 (4-methyl-1,3,-phenylene bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), and BMI-TMH ((1,6-bismaleimide-2,2,4-trimethyl)hexane, manufactured by Daiwa Chemical Industry Co., Ltd.).

[0055] The amount of the curing agent to be added is preferably 20 to 500 parts by mass, and more preferably 25 to 500 parts by mass, based on 100 parts by mass of the epoxy resin.

[0056] In the following, as an example, components that may be contained in addition to the above components will be described for the case where the light-blocking curable resin composition is formed from a thermosetting resin composition that does not contain a photocurable component.

[0057] The light-shielding curable resin composition may further contain a thermoplastic resin in order to improve the mechanical strength of the resulting cured film. The thermoplastic resin is preferably soluble in a solvent. When soluble in a solvent, the flexibility of the dry film is improved, and the occurrence of cracks and powdering can be suppressed. Examples of the thermoplastic resin include thermoplastic polyhydroxypolyether resins, phenoxy resins which are condensates of epichlorohydrin and various bifunctional phenolic compounds, or phenoxy resins in which the hydroxyl group of the hydroxyether moiety present in the skeleton is esterified using various acid anhydrides or acid chlorides, polyvinyl acetal resins, polyamide resins, polyamideimide resins, block copolymers, and the like. The thermoplastic resins may be used alone or in combination of two or more.

[0058] The blending amount of the thermoplastic resin is preferably 0.5 to 20 mass %, more preferably 0.5 to 10 mass %, based on the total solid content of the light-blocking curable resin composition. When the blending amount of the thermoplastic resin is within the above range, a uniform roughened surface state is easily obtained.

[0059] Furthermore, the light-shielding curable resin composition may contain rubber particles as necessary. Examples of such rubber particles include polybutadiene rubber, polyisopropylene rubber, urethane-modified polybutadiene rubber, epoxy-modified polybutadiene rubber, acrylonitrile-modified polybutadiene rubber, carboxyl-modified polybutadiene rubber, acrylonitrile-butadiene rubber modified with carboxyl or hydroxyl groups, and crosslinked rubber particles thereof, core-shell type rubber particles, etc., and one type may be used alone or two or more types may be used in combination. These rubber particles are added to improve the flexibility of the obtained cured film, improve crack resistance, enable surface roughening treatment with an oxidizing agent, and improve adhesion strength with copper foil, etc.

[0060] The average particle size of the rubber-like particles is preferably in the range of 0.005 to 1 μm, more preferably in the range of 0.2 to 1 μm. The average particle size of the rubber-like particles can be determined by a laser diffraction particle size distribution measuring device and a measuring device using a dynamic light scattering method. An example of a measuring device using the laser diffraction method is Microtrac MT3300EXII manufactured by Microtrac-Bell, and an example of a measuring device using the dynamic light scattering method is Nanotrac Wave II UT151 manufactured by Microtrac-Bell.

[0061] The amount of the rubber particles is preferably 0.5 to 10 mass %, more preferably 1 to 5 mass %, based on the total solid content of the light-shielding curable resin composition. When it is 0.5 mass % or more, crack resistance is obtained and the adhesive strength with a conductor pattern, etc. can be improved. When it is 10 mass % or less, the coefficient of thermal expansion (CTE) decreases and the glass transition temperature (Tg) increases, improving the curing characteristics.

[0062] The light-blocking curable resin composition may contain a curing accelerator. The curing accelerator accelerates the thermosetting reaction and is used to further improve properties such as adhesion, chemical resistance, and heat resistance. Specific examples of such curing accelerators include imidazole and its derivatives; guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; amines such as trimethylamine, triethanolamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; polyvinylphenol, polyvinylphenol brominated products, and phenol novolac. Examples of the curing accelerator include polyphenols such as alkylphenol novolak and alkylphenol novolak; organic phosphines such as tributylphosphine, triphenylphosphine, and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the polybasic acid anhydrides; photocationic polymerization catalysts such as diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and 2,4,6-triphenylthiopyrylium hexafluorophosphate; styrene-maleic anhydride resins; equimolar reactants of phenylisocyanate and dimethylamine, equimolar reactants of organic polyisocyanates such as tolylene diisocyanate and isophorone diisocyanate and dimethylamine, and metal catalysts. Among the curing accelerators, phosphonium salts are preferred because they provide BHAST resistance.

[0063] The curing accelerator can be used alone or in combination of two or more. The use of a curing accelerator is not essential, but when it is particularly desired to accelerate curing, it can be used in an amount of preferably 0.01 to 5 parts by mass per 100 parts by mass of the epoxy resin. In the case of a metal catalyst, the amount is preferably 10 to 550 ppm, more preferably 25 to 200 ppm, calculated as the metal per 100 parts by mass of the compound having a cyanate ester group.

[0064] The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, petroleum-based solvents, etc. Specific examples of the organic solvent include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol diethyl ether, and triethylene glycol monoethyl ether; Examples of the solvent include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine. Also usable are organic solvents such as Swazol 1000 and Swazol 1500 manufactured by Maruzen Petrochemical Co., Ltd., Solvent #100 and Solvent #150 manufactured by Sankyo Chemical Co., Ltd., Shellsol A100 and Shellsol A150 manufactured by Shell Chemicals Japan Ltd., and Ipzol No. 100 and Ipzol No. 150 manufactured by Idemitsu Kosan Co., Ltd. One type of organic solvent may be used alone, or two or more types may be used in combination.

[0065] The amount of residual solvent in the light-shielding curable resin composition is preferably 0.5 to 7.0% by mass. When the amount of residual solvent is 7.0% by mass or less, bumping during thermal curing is suppressed, and the surface flatness is improved. In addition, the melt viscosity is prevented from dropping too much, causing the resin to flow, and the flatness is improved. When the amount of residual solvent is 0.5% by mass or more, the flowability during lamination is good, and the flatness and embeddability are improved.

[0066] The light-blocking curable resin composition may further contain, as necessary, conventionally known colorants such as phthalocyanine blue, phthalocyanine green, iodine green, disazo yellow, crystal violet, titanium oxide, and naphthalene black; conventionally known thickeners such as asbestos, orben, bentone, and finely powdered silica; conventionally known antifoaming agents and / or leveling agents such as silicone-based, fluorine-based, and polymer-based agents; adhesion imparting agents such as thiazole-based, triazole-based, and silane coupling agents; conventionally known flame retardants, and titanate-based and aluminum-based additives.

[0067] The thickness of the curable resin layer of the dry fill made of the light-shielding curable resin composition may be, for example, 1 to 200 μm. Within this thickness range, the maximum diameter of the aggregated particles of the inorganic filler in the light-shielding curable resin composition is set to half or less of the thickness of the curable resin layer. Since the flatness is better when the thickness of the curable resin layer is large, for example, a thickness of 30 μm or more, further 50 μm or more, or even 100 μm or more can be suitably used. Note that a curable resin layer having a thickness of more than 200 μm may be formed by stacking a plurality of curable resin layers. In this case, a roll laminator or a vacuum laminator may be used.

[0068] [Carrier film] The carrier film supports the curable resin layer of the dry film, and is a film to which the light-shielding curable resin composition is applied when the curable resin layer is formed. Examples of the carrier film include polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, polystyrene films, and other thermoplastic resin films, and surface-treated paper. Among these, polyester films can be preferably used from the viewpoints of heat resistance, mechanical strength, and ease of handling. The thickness of the carrier film is not particularly limited, but is appropriately selected in the range of approximately 10 to 150 μm depending on the application. The surface of the carrier film on which the curable resin layer is provided may be subjected to a release treatment. In addition, sputtering or ultra-thin copper foil may be formed on the surface of the carrier film on which the curable resin layer is provided.

[0069] [Protective film] The protective film is provided on the side of the curable resin layer opposite to the carrier film in order to prevent dust and the like from adhering to the surface of the curable resin layer of the dry film and to improve handling. It is preferable to use a biaxially oriented polypropylene film (OPP) as the protective film. By using a biaxially oriented polypropylene film, it is possible to reduce cooling shrinkage after lamination to the curable resin layer. However, the protective film is not limited to a biaxially oriented polypropylene film. The thickness of the protective film is not particularly limited, but is appropriately selected in the range of about 10 to 100 μm depending on the application. It is preferable that the surface of the protective film on which the curable resin layer is provided is subjected to a treatment for improving adhesion, such as embossing, corona treatment, or slight adhesion treatment, or a release treatment.

[0070] The dry film of the present invention can be preferably used for forming a sealant or a permanent protective film for electronic components, particularly semiconductor devices, printed wiring boards, and optical sensor modules, by laminating the dry film on a semiconductor wafer or the like and curing the curable resin layer to form a cured product. In particular, it is suitable for use as a sealant for semiconductor chips. A wiring board may be formed by laminating wiring using the dry film of the present invention.

[0071] Examples of electronic components using the cured product of the light-blocking curable resin composition of the present invention or the cured product of the dry film of the present invention include semiconductor devices, printed wiring boards, and optical sensor modules. As a method for producing such electronic components, a conventionally known method may be used. EXAMPLES

[0072] The present invention will be specifically described below with reference to examples and comparative examples, but it goes without saying that the present invention is not limited to these examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0073] <Preparation of Light-Shielding Curable Resin Composition> The solvents described in the examples and comparative examples were placed in a container, and stirred while heating to 50°C so that the solvent would not volatilize, and then the resin components and coupling agents were added. After confirming that the resin components were dissolved, the inorganic filler and colorant described in the examples were added and thoroughly stirred. Then, the light-shielding curable resin composition was prepared by kneading with a bead mill filled with zirconia beads. As the bead mill, a conical type K-8 (manufactured by Buehler) was used, and kneading was performed under the conditions of a rotation speed of 1200 rpm, a discharge amount of 20%, a bead particle size of 0.65 mm, and a filling rate of 88%. The numerical values ​​in the table indicate parts by mass unless otherwise indicated by %, and indicate the solid content except for the solvent, polymer resin, and nanosilica.

[0074] <Dispersibility> The prepared light-shielding curable resin composition was checked for dispersibility using a 0-50 μm grind gauge in accordance with the JIS K5600-2-5 dispersibility method. The evaluation criteria are as follows. The maximum particle size of the aggregated particles obtained using the grind gauge is shown in the table. ○: Dispersion degree judged by 5 grain value is 20 μm or less △: Dispersion degree judged by 5 grain value is more than 20 μm and less than 30 μm ×: Dispersion degree judged based on 5 grain value is more than 30 μm

[0075] <Suppression of settling of composition (ink)> The prepared light-shielding curable resin composition was placed in a transparent glass screw tube and stored in a thermostatic chamber set at 23°C for 12 hours for aging treatment. The light-shielding curable resin composition was charged 50 mm from the bottom of the screw tube. After aging, the light-shielding curable resin composition was taken out and visually observed from the side to confirm the sedimentation state of the light-shielding curable resin composition. The evaluation criteria were as follows. ○: No settling is observed. Δ: A transparent supernatant liquid less than 1 mm in size was observed from the top of the composition. ×: A transparent supernatant liquid of 20 mm or more was observed above the composition.

[0076] <Preparation of dry film> The amount of the solvent was adjusted so that the viscosity of the prepared light-shielding curable resin composition was 0.5 to 20 dPa·s (rotational viscometer 5 rpm, 25°C), and each was applied to a carrier film (PET film; Toyobo Co., Ltd. TN-200, thickness 38 μm, size 30 cm × 30 cm) using a bar coater so that the film thickness of the curable resin layer after drying was 40 μm. Next, the curable resin layer was formed on the carrier film by drying for 5 to 10 minutes at 70 to 120 °C (average 100 °C) in a hot air circulation drying oven so that the residual solvent in the curable resin layer was 0.5 to 2.5 mass%. Next, a biaxially stretched polypropylene film (OPP, Alphan FG-201, Fish Eyeless, Oji F-Tech Co., Ltd.) was laminated to the surface of the prepared dry film using a roll laminator set at a temperature of 80 °C to prepare a three-layered dry film.

[0077] <Transmittance> The protective film of the obtained three-layered dry film was peeled off, and the film was laminated on a 1 mm thick slide glass using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho). The lamination was performed under conditions of 80 to 110°C lamination temperature and 0.5 MPa pressure. Next, the carrier film was peeled off, and the resin layer was cured in a hot air circulation drying oven under conditions of 100°C x 30 min and 200°C x 60 min. The transmittance of the obtained cured product at 380 nm to 780 nm was measured using a UV-Visible Near-Infrared Spectrophotometer V-700 (manufactured by JASCO). The evaluation criteria are as follows: ◎: Transmittance less than 0.1% across the entire wavelength range ○: Transmittance of 0.1% or more and less than 0.5% in the entire wavelength range ×: Transmittance of 0.5% or more in all wavelength ranges

[0078] <Dicing resistance> The protective film of the obtained three-layered dry film was peeled off, and the film was laminated on an 8-inch silicon wafer with a thickness of 700 μm using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho). The lamination conditions were a lamination temperature of 80 to 110°C and a pressure of 0.5 MPa. Next, the carrier film was peeled off, and the resin layer was cured in a hot air circulation drying oven at 100°C x 30 min and 200°C x 60 min. Next, the dicing resistance of the cured film was evaluated using a dicing machine DFD6240 (manufactured by Disco, equipped with a ceramic blade). The dicing conditions were a rotation speed of 10,000 rpm and a feed speed of 1 mm / min. The evaluation criteria were as follows. ◎: No burrs on the cured film surface, no chipping of resin Good: Burrs on the cured film surface and resin chips are less than 1.0 mm long ×: Burrs on the cured film surface, or chipped resin length is 1.0 mm or more

[0079] <Warping of the board> A copper-clad laminated substrate (MCL-E-770G, Hitachi Chemical Co., Ltd., size 10 x 10 cm) with a copper thickness of 12 μm and a plate thickness of 0.1 mm was electrolytically plated with copper (Atotech Co., Ltd., surface roughness after plating 100 nm or less) to a total copper thickness of 20 μm. Then, CZ-8101 (1 μm etching, MEC Co., Ltd.) was used as a pretreatment. After that, the dry film from which the OPP had been peeled off was laminated on one side of the substrate using a two-chamber vacuum laminator CVP-600 (Nichigo Morton Co., Ltd.). The conditions for lamination and pressing were a temperature of 80 to 110 °C and a pressure of 0.5 MPa, respectively. Next, the carrier film was peeled off, and the resin layer was cured in a hot air circulation drying oven at 100 °C x 30 min and 200 °C x 60 min. Next, five cycles of reflow treatment were performed with the peak temperature set at 280°C and 275°C or higher for an exposure time of 10 seconds or more, and the warpage of the four corners of the board (all warpage shapes were smiles) was measured with a caliper. The evaluation criteria were as follows: ◎: No warping 〇: The amount of warping in the most warped part of the four corners is less than 10 mm △: The amount of warping at the most warped part of the four corners is 10 mm or more but less than 30 mm ×: The largest warpage in the four corners is 30 mm or more.

[0080] Table 1 shows the blending ratio of each component and the evaluation results.

[0081] [Table 1]

[0082] Notes *1 to *17 in Table 1 are as follows: *1: Mitsubishi Chemical jER828, bisphenol A type epoxy resin, epoxy equivalent 189g / eq, liquid *2: NC-3000H manufactured by Nippon Kayaku Co., Ltd., biphenyl novolac type epoxy compound, epoxy equivalent 290g / eq, *3: Primaset PT-30 manufactured by Lonza Japan, novolac type cyanate resin, cyanate equivalent 124g / eq, solid *4: DIC EPICLON HPC-8000, active ester resin, active equivalent weight 223g / eq, solid *5: HF-1M, phenol novolac resin, manufactured by Meiwa Kasei Co., Ltd. *6: Shikoku Kasei 2E4MZ, 2-ethyl-4-methylimidazole *7: Cobalt(II) acetylacetonate manufactured by Tokyo Chemical Industry Co., Ltd. *8: A polymer resin with a glass transition point of 20°C or less and a weight average molecular weight of 10,000 or more, Nagase ChemteX Teisan Resin SG-80H MEK cut product, solid content 18% by mass, acrylic ester copolymer resin (functional groups: epoxy groups, amide groups) *9: Mitsubishi Chemical carbon black powder MA77 (average particle size 23 nm) *10: Paliogen Red K 3580, Pigment Red 149, BASF, perylene colorant *11: Solvent Green 3, Tokyo Chemical Industry Co., Ltd., green anthraquinone colorant *12: Firstogen Blue 5380, DIC, Phthalocyanine Blue *13: Cromophtal (registered trademark) Red A2BN, manufactured by BASF, a red anthraquinone colorant *14: Silica fine particles FB-3SDC (D50 = 3.1 μm) manufactured by Denka *15: Admatechs silica fine particles SO-E1 (D50=0.2μm) *16: Nanosilica (D50 = 50 nm) manufactured by Admatechs, solid content 30% by mass *17: Epoxy silane coupling agent KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.

[0083] From the results shown in Table 1 above, it can be seen that the dry films having a curable resin layer made of the light-blocking curable resin composition shown in each Example have excellent dispersibility, ink settling suppression, light transmission suppression (in other words, light-blocking properties), dicing resistance, and substrate warpage suppression. [Explanation of symbols]

[0084] 11 Dry Film 12 Curable resin layer 13 Career Film 14 Protective film

Claims

1. a light-shielding thermosetting resin composition (excluding a case where the light-shielding thermosetting resin composition includes a resin having an ethylenically unsaturated group and a carboxyl group) including a polymer resin that is an acrylic acid ester copolymer having a glass transition point of 20° C. or lower and a weight average molecular weight of 10,000 or more, an epoxy resin including at least a liquid epoxy resin, a colorant, and an inorganic filler (excluding the colorant); the colorant is blended in an amount of 0.3 to 20% by mass based on the solid content of the light-blocking thermosetting resin composition, the inorganic filler is mixed in an amount of 0.1 to 70% by mass based on the solid content of the light-shielding thermosetting resin composition, The curable resin layer has a maximum particle size of the inorganic filler aggregate of 10 μm or less, A dry film characterized in that, when the thickness of the curable resin layer is X (μm), the maximum particle size of the aggregate particles of the inorganic filler is X / 2 (μm) or less.

2. 2. The dry film according to claim 1, wherein the amount of the polymer resin having a glass transition point of 20° C. or lower and a weight average molecular weight of 10,000 or more is 1 to 35 mass % relative to the solid content of the light-shielding thermosetting resin composition.

3. A cured product obtained by curing the curable resin layer of the dry film according to claim 1 or 2.

4. An electronic part comprising the cured product according to claim 3.

Citation Information

Patent Citations

  • laminate

    JP2005238469A

  • Dry film and printed wiring board

    JP2015010179A

  • Adhesive composition, adhesive sheet, adhesion method for adherend and composite material

    JP2016050224A

  • Circuit board with electromagnetic wave shield film, and production method of the same

    JP2016149388A

  • Resin composition and electronic component

    JP2017178990A